Method for producing polyarylene sulfide resin
The method of adding PAS oligomers to the reaction mixture and heat-treating in an inert gas atmosphere addresses the issues of viscosity and recrystallization in PAS resin production, achieving high molecular weight and efficient oligomer reuse.
Patent Information
- Application Number
- JP2024032827
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-14
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-01
AI Technical Summary
Conventional methods for producing high molecular weight polyarylene sulfide (PAS) resin face issues such as viscosity dependence on shear rate due to branched polymer chains, low recrystallization temperature, and increased cycle time, while the reuse of PAS oligomers is hindered by by-products and gas generation.
A method involving the addition of PAS oligomers to a crude reaction mixture, followed by solid-liquid separation, washing, and heat-treatment in an inert gas atmosphere to maintain a linear structure and increase molecular weight, utilizing both chain and cyclic PAS oligomers.
This method produces a high molecular weight linear PAS resin with improved molecular weight distribution and reduced cycle time, while effectively reusing PAS oligomers and minimizing branched structure formation.
Smart Images

Figure 2024132932000001 
Figure 2024132932000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polyarylene sulfide resin. [Background technology]
[0002] Polyarylene sulfide (PAS) resins, such as polyphenylene sulfide (PPS), have excellent heat resistance, chemical resistance, etc., and are widely used in electrical and electronic components, automotive parts, water heater parts, fibers, films, etc. Among them, the demand for high molecular weight PAS resins has been increasing in recent years due to their excellent mechanical properties such as toughness.
[0003] As a conventional method for producing a high molecular weight PAS resin, for example, a method has been disclosed in which a linear PAS resin is heated to a temperature below the melting point in a gas-phase oxidizing atmosphere to be crosslinked by oxidation (Patent Document 1). However, the crosslinked high molecular weight PAS resin obtained in this manner tends to have a relatively high shear rate dependency of viscosity due to the branched structure of the polymer chain, which causes problems in processability during molding such as spinning and film formation. In addition, the recrystallization temperature is generally low and crystallization tends to take a long time, which leads to an increase in cycle time during melt molding.
[0004] On the other hand, oligoarylene sulfide (hereinafter referred to as PAS oligomer) produced as a by-product in the manufacturing process of PAS resin is generally removed in the purification process of PAS polymerization because it reduces the crystallization rate of PAS resin and increases the amount of gas generated, but the resulting unit loss has been an issue. As a method for utilizing PAS oligomer, for example, a method for producing a crosslinked polyarylene sulfide resin by reacting it under an oxidizing atmosphere has been proposed (Patent Document 2). However, in order to use PAS oligomer as a reaction raw material in this way, it was necessary to remove by-products other than PAS oligomer in order to suppress the polymerization inhibition reaction. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-84132 A [Patent Document 2] JP 2012-116918 A Summary of the Invention [Problem to be solved by the invention]
[0006] The problem to be solved by the present invention is to provide a method for producing a high molecular weight linear PAS resin by reusing a PAS oligomer. [Means for solving the problem]
[0007] As a result of extensive investigations, the inventors discovered that in the production process of PAS resin, a composition containing a PAS oligomer is added to the mixture after the polymerization reaction, and then the mixture is washed and then heat-treated under an inert gas atmosphere, thereby enabling the PAS resin to be increased in molecular weight while maintaining its linear structure, and thus completed the present invention.
[0008] That is, the present invention provides (1) reacting a polyhaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent to obtain a crude reaction mixture containing at least a PAS resin (a), a PAS oligomer (b), an alkali metal halide, and an organic polar solvent; (2) removing a liquid phase component from the crude reaction mixture by solid-liquid separation using a flash method to obtain a mixture (A) containing at least a PAS resin (a), a PAS oligomer (b), and an alkali metal halide; (3) washing the mixture (A) to remove the alkali metal halide to obtain a mixture (B) containing at least a PAS resin (a) and a PAS oligomer (b); and The method includes a step (4) of heat-treating the mixture (B) under an inert gas atmosphere, and In the step (2) and / or (3), adding a composition (C) containing 10% by mass or more of the PAS oligomer (c) to at least one of the crude reaction mixture and the mixture (A). The present invention relates to a method for producing a PAS resin, characterized in that the PAS oligomer (c) contains a chain-like PAS oligomer and a cyclic PAS oligomer.
[0009] In the present disclosure, a high molecular compound having repeating units 2 to 50 (a mixture of dimer to 50-mer) may be referred to as an "oligomer".
Advantages of the Invention
[0010] According to the present invention, it is possible to provide a method for producing a linear PAS resin having a high molecular weight by reusing a PAS oligomer.
Embodiments for Carrying Out the Invention
[0011] Hereinafter, an embodiment of the present invention will be described in detail. However, the scope of the present invention is not limited to the embodiment described here, and various modifications can be made without departing from the spirit of the present invention. Also, when a plurality of upper limit values and lower limit values are described for specific parameters, any upper limit value and lower limit value can be combined to form a suitable numerical range.
[0012] <Method for Producing PAS Resin> The method for producing a PAS resin according to this embodiment is to react a polyhaloaromatic compound with (i) an alkali metal sulfide or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent to obtain a crude reaction mixture containing at least a PAS resin (a), a PAS oligomer (b), an alkali metal halide, and an organic polar solvent in step (1). In step (2), removing the liquid phase component from the crude reaction mixture by solid-liquid separation by the flash method to obtain a mixture (A) containing at least a PAS resin (a), a PAS oligomer (b), and an alkali metal halide. (3) washing the mixture (A) to remove the alkali metal halide to obtain a mixture (B) containing at least a PAS resin (a) and a PAS oligomer (b); and The method includes a step (4) of heat-treating the mixture (B) under an inert gas atmosphere, and In the steps (2) and / or (3), adding a composition (C) containing 10% by mass or more of a PAS oligomer (c) to at least one of the crude reaction mixture and the mixture (A); The PAS oligomer (c) is characterized in that it contains a linear PAS oligomer and a cyclic PAS oligomer.
[0013] ·Process (1) Step (1) is a step of reacting a polyhaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide, in an organic polar solvent to obtain a crude reaction mixture containing at least a PAS resin (a), a PAS oligomer (b), an alkali metal halide, and an organic polar solvent.
[0014] Here, in the present invention, the polyhalo aromatic compound is, for example, a halogenated aromatic compound having two or more halogen atoms directly bonded to an aromatic ring, and specifically includes p-dichlorobenzene, o-dichlorobenzene, m-dichlorobenzene, trichlorobenzene, tetrachlorobenzene, dibromobenzene, diiodobenzene, tribromobenzene, dibromonaphthalene, triiodobenzene, dichlorodiphenylbenzene, dibromodiphenylbenzene, dichlorobenzophenone, dibromobenzophenone, dichlorodiphenylether, dibromodiphenylether, dichlorodiphenylsulfide, dibromodiphenylsulfide, dichlorobiphenyl, dibromobiphenyl and other dihalo aromatic compounds and their mixtures, and these compounds may be block copolymerized.Among these, dihalogenated benzenes are preferred, and those containing 80 mol% or more of p-dichlorobenzene are particularly preferred.
[0015] In the present embodiment, an alkali metal sulfide or an alkali hydrosulfide and an alkali metal hydroxide (hereinafter, sometimes referred to as a sulfidizing agent) are used as raw materials.
[0016] In this embodiment, the alkali metal sulfide includes lithium sulfide, sodium sulfide, rubidium sulfide, cesium sulfide, and mixtures thereof. Such alkali metal sulfides can be used as hydrates, aqueous mixtures, or anhydrides. The alkali metal sulfides can also be derived by reacting an alkali metal hydrosulfide with an alkali metal hydroxide. Note that a small amount of an alkali metal hydroxide may be added to react with the alkali metal hydrosulfide and alkali metal thiosulfate that are usually present in trace amounts in the alkali metal sulfide.
[0017] The alkali metal hydrosulfides include lithium hydrogen sulfide, sodium hydrogen sulfide, rubidium hydrogen sulfide, cesium hydrogen sulfide, and mixtures thereof. The alkali metal hydrosulfides can be used as hydrates, aqueous mixtures, or anhydrous forms.
[0018] The alkali metal hydrosulfide is used together with an alkali metal hydroxide. Examples of the alkali metal hydroxide include lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide, and these may be used alone or in combination of two or more. Among these, lithium hydroxide, sodium hydroxide, and potassium hydroxide are preferred because of their easy availability, and sodium hydroxide is particularly preferred.
[0019] In the method for producing the PAS resin according to the present embodiment, a hydrous sulfidizing agent can be used as a raw material, and in this case, it is preferable to dehydrate the hydrous sulfidizing agent in the presence of at least an aprotic polar solvent, and then subject the agent to polymerization reaction for the PAS resin. In addition, when the amount of the aprotic polar solvent is small, for example, less than 1 mole per mole of sulfur atom of the sulfidizing agent, it is preferable to dehydrate the hydrous sulfidizing agent and the aprotic polar solvent in the presence of a polyhalo aromatic compound.
[0020] The dehydration step of the hydrous sulfidizing agent is carried out by charging at least an aprotic polar solvent and a hydrous alkali metal sulfide or a hydrous alkali hydrosulfide and an alkali metal hydroxide as the hydrous sulfidizing agent into a reaction vessel equipped with a distillation apparatus, heating to a temperature at which water is removed by azeotropy, specifically, to a temperature in the range of 300° C. or less, preferably 80 to 220° C., more preferably 100 to 200° C., and discharging water by distillation out of the system. In the dehydration step, dehydration is preferably carried out until the amount of water in the polymerization system is 5 mol or less, more preferably 0.01 to 2.0 mol, per mol of sulfur atoms in the sulfidizing agent.
[0021] In addition, examples of the organic polar solvent in this embodiment include amides, ureas, and lactams such as formamide, acetamide, N-methylformamide, N,N-dimethylacetamide, tetramethylurea, N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid; sulfolanes such as sulfolane and dimethylsulfolane; nitriles such as benzonitrile; ketones such as methyl phenyl ketone, and mixtures thereof. Among these, amides having an aliphatic cyclic structure, such as N-methyl-2-pyrrolidone, 2-pyrrolidone, N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinoic acid, are preferred, and N-methyl-2-pyrrolidone is more preferred.
[0022] In the PAS polymerization step, the polymerization reaction of the PAS resin is carried out by reacting the above-mentioned alkali metal sulfide as a sulfidizing agent with a polyhalo aromatic compound in the presence of these organic polar solvents. Alternatively, the polymerization reaction of the PAS resin is carried out by reacting the above-mentioned alkali metal hydrosulfide and alkali metal hydroxide as sulfidizing agents with a polyhalo aromatic compound in the presence of these aprotic polar solvents. The polymerization conditions are generally a temperature range of 200 to 330°C, and a pressure range that should be such that the polymerization solvent and the polyhalo aromatic compound as the polymerization monomer are substantially kept in a liquid phase, and are generally selected from a range of 0.1 to 20 MPa, preferably a range of 0.1 to 2 MPa. The amount of the polyhalo aromatic compound charged is prepared to be in the range of 0.2 mol to 5.0 mol, preferably a range of 0.8 to 1.3 mol, and more preferably a range of 0.9 to 1.1 mol, relative to 1 mol of sulfur atom of the sulfidizing agent. The amount of the aprotic polar solvent is adjusted to be in the range of 1.0 to 6.0 mol, preferably 2.5 to 4.5 mol, per mol of sulfur atom of the sulfidizing agent. The polymerization reaction is preferably carried out in the presence of a small amount of water, and the ratio is preferably adjusted appropriately in consideration of the polymerization method, the molecular weight of the obtained polymer, and the productivity. Specifically, the dehydration operation is carried out so that the amount of water is in the range of 2.0 mol or less, preferably 1.6 mol or less, per mol of sulfur atom of the sulfidizing agent. In addition, when the dehydration operation is carried out in the presence of a polyhalo aromatic compound (for example, the method of "5)" in the specific embodiment below), the dehydration operation may be carried out so that the amount of water is in the range of 0.9 mol or less, preferably 0.05 to 0.3 mol, more preferably 0.01 to 0.02 mol.
[0023] Specific examples of the polymerization of a sulfidizing agent and a polyhalo aromatic compound in the presence of the above-mentioned organic polar solvent include, for example, 1) A method using a polymerization aid such as an alkali metal carboxylate or a lithium halide, 2) A method using a branching agent such as an aromatic polyhalogen compound, 3) A method in which the polymerization reaction is carried out in the presence of a small amount of water and then water is added to further polymerize; 4) A method in which the gas phase of a reaction vessel is cooled during the reaction of an alkali metal sulfide with an aromatic dihalogen compound, and a part of the gas phase in the reaction vessel is condensed and refluxed to the liquid phase; 5) A method for producing a PAS resin, which includes, as essential production steps, a step of reacting an alkali metal sulfide or a hydrous alkali metal hydrosulfide and an alkali metal hydroxide with an amide, urea or lactam having an aliphatic cyclic structure while dehydrating in the presence of a polyhalogenated aromatic compound to produce a slurry containing a solid alkali metal sulfide, a step of further adding a polar organic solvent such as NMP after producing the slurry and distilling off water to perform dehydration, and a step of reacting a polyhalogenated aromatic compound, an alkali metal hydrosulfide, and an alkali metal salt of a hydrolyzate of the amide, urea or lactam having an aliphatic cyclic structure in the slurry obtained through the dehydration step at a water content of 0.02 mol or less in the reaction system per 1 mol of the polar organic solvent such as NMP to polymerize.
[0024] In this way, by polymerizing a dihaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent, a PAS resin is obtained as a product, and cyclic or chain-like PAS oligomers are also produced as by-products. Substances remaining after the reaction may include by-products such as alkali metal-containing inorganic salts, carboxyalkylamino group-containing compounds, and terminal SH group-containing compounds, as well as unreacted raw materials and water.
[0025] ·Process (2) Step (2) is a step of removing liquid phase components from the crude reaction mixture by solid-liquid separation using a flash method to obtain a mixture (A) containing at least a PAS resin (a), a PAS oligomer (b), and an alkali metal halide.
[0026] The solid-liquid separation is roughly divided into two types, the flash method and the quench method, which will be described later. In this step, the flash method is used in order to incorporate the PAS oligomer (b) into the mixture (A) without removing it. The flash method is a method in which the solvent in the crude reaction mixture is evaporated to recover the solvent and at the same time recover the solid matter. In general, the crude reaction mixture is flashed from a high-temperature, high-pressure state into an atmosphere of normal pressure or reduced pressure to distill off and recover the solvent, and at the same time recover the solid matter containing the PAS resin in the form of powder or granules. A preferred embodiment of the flash method is a method in which the high-temperature, high-pressure (usually 240°C or higher, 0.3 MPa or higher) polymerization reaction product obtained in the polymerization step is ejected from a nozzle into an atmosphere of nitrogen or water vapor at normal pressure. In the flash method, the solvent can be efficiently recovered by utilizing the heat of vaporization of the solvent when the polymerization reaction product is flashed from a high-temperature, high-pressure state to a normal pressure state, and the higher the internal temperature during flashing, the more efficient the solvent recovery and the better the productivity. Therefore, the temperature and pressure in the polymerization system during flashing are usually set to 240° C. or higher, preferably in the range of 250 to 280° C., and 0.3 MPa or higher, preferably in the range of 0.4 to 5.0 MPa. From this state, the atmospheric temperature when flashing under reduced pressure or normal pressure is usually in the range of 150 to 250° C., and if the recovery of the solvent from the crude reaction mixture is insufficient, heating may be continued in an atmosphere of 150 to 250° C. after flashing.
[0027] ·Process (3) The step (3) is a step of washing the mixture (A) to remove the alkali metal halide, thereby obtaining a mixture (B) containing at least a PAS resin (a) and a PAS oligomer (b).
[0028] In this step, the mixture (A) is washed with water or hot water. Examples of a method for performing solid-liquid separation after washing with water include a method of adding water to the slurry, stirring the mixture, and then filtering the mixture using a filtering device, a method of adding water to the moisture-containing filtration residue (hereinafter abbreviated as "wet cake") obtained by the above-mentioned filtration to form a slurry and then filtering the slurry, and a method of adding water to the wet cake retained in a filter and filtering the slurry.
[0029] In the water washing, the amount of water added to the mixture (A) is preferably in the range of 2 to 20 times the theoretical yield of the PAS resin finally obtained, from the viewpoint of washing efficiency, and the above amount of water is preferably divided into 1 to 10 times, preferably 1 to 4 times, and used for water washing. The water washing is preferably carried out in a nitrogen or air atmosphere at a water temperature in the range of 20°C to 300°C, more preferably in the range of 50°C to 100°C, and most preferably in the range of 70°C to 90°C, from the viewpoint of good washing efficiency. The water washing can be carried out once or repeatedly a plurality of times. When the water washing is repeated a plurality of times, the atmospheric and temperature conditions may be the same or different.
[0030] Since the filtered solid phase component may contain trace amounts of alkali metal halide and sulfidizing agent that have not been washed out sufficiently, it is preferable to further contact the solid phase component with water in the range of 100° C. to 280° C. and then perform solid-liquid separation (hereinafter sometimes referred to as "hot water washing"). Furthermore, by washing with hot water, the affinity between the added PAS oligomer and the PAS resin can be increased, and the reaction can proceed effectively in the subsequent heat treatment step.
[0031] The temperature of the hot water washing is, for example, preferably in the range of 100 to 280° C., more preferably in the range of 120 to 275° C., from the viewpoint of improving the efficiency of extraction of the alkali metal halide and sulfidizing agent remaining in the resin. More specifically, it is preferable to carry out the extraction treatment with hot water at 140 to 260° C. under the condition that the pressure of the gas phase in the reactor is increased, more preferably 0.2 to 4.6 MPa (gauge pressure).
[0032] A specific method for performing such hot water washing includes a method in which the solid phase component filtered after the above-mentioned water washing is washed with water under agitation under predetermined pressure and temperature conditions in a pressure vessel. The amount of water during hot water washing is preferably 1.5 to 10 times the mass of the PAS resin from the viewpoint of improving the extraction efficiency of the alkali metal halide and the sulfidizing agent, and hot water washing may be performed by dividing this amount of hot water into two or more times. For example, when hot water washing is repeated twice, it is preferable to perform filtration between the first and second hot water washings, and to filter out the alkali metal halide and sulfidizing agent extracted in the first hot water washing and the PAS resin. Alternatively, filtration may be performed after one hot water washing, and the above-mentioned water washing may be performed. This operation can also further promote separation and removal of the alkali metal halide and the sulfidizing agent from the PAS resin. Although the conditions for the first and second hot water washing steps can be arbitrarily selected from the above conditions, it is preferable from the viewpoint of the chemical resistance of the apparatus used in the hot water washing to set the temperature for the first hot water washing step to a temperature in the range of, for example, 120° C. to 250° C., and to first filter and remove the highly alkaline filtrate, and then set the temperature for the second hot water washing step to a higher temperature than that of the first hot water washing step, for example, a temperature in the range of 150° C. to 275° C. In this step, hot water washing and solid-liquid separation can also be repeatedly performed.
[0033] In this step, a water washing tank having an agitator and a centrifuge for solid-liquid separation can be used, but it can also be carried out in a vessel having a mixing function with an agitator inside and a filtration filter at the bottom. In addition, even in the case of hot water washing at a temperature exceeding 100°C, it is possible to use a water washing tank having an agitator for hot water washing and a centrifuge for subsequent filtration at 20 to 100°C, but it is also possible to carry out the process in a sealed or sealable vessel having a mixing function with an agitator inside and a filtration filter at the bottom. In the present invention, water washing or hot water washing may be carried out continuously or batchwise.
[0034] The solid phase component separated by filtration can be used as it is in the next step as mixture (B), or it can be dried by heating to a temperature at which the solvent such as water evaporates. Drying can be performed under vacuum or in an inert atmosphere such as air or nitrogen.
[0035] ·Process (4) The step (4) is a step of heat-treating the mixture (B) under an inert gas atmosphere.
[0036] In this process, the inert gas refers to a stable gas that is unlikely to undergo chemical reactions, such as rare gas elements or nitrogen, and is preferably at least one selected from the group consisting of nitrogen, helium, and argon. The inert gas may also be a mixed inert gas obtained by mixing two or more inert gases. In addition, the term "inert gas atmosphere" as used herein refers to a mixed gas atmosphere containing an inert gas, in which the inert gas occupies 99% by volume or more of the total volume (100% by volume) of the mixed gas. A known method can be adopted for measuring the gas concentration. For example, the measurement can be performed using a detector such as various sensors, gas chromatography, or a gas detector tube, using a specified container or gas suction pump.
[0037] The heating means is not particularly limited, and known devices and methods can be used. For example, the mixture (B) is placed in a treatment vessel and heat-treated under inert gas. The heating conditions are preferably in the range of 180°C or higher to 20°C lower than the melting point of the PAS resin, from the viewpoints of the time required for the heat treatment and of improving the thermal stability of the PAS resin when melted after the heat treatment. However, the melting point here refers to the one measured using a differential scanning calorimeter in accordance with JIS K 7121.
[0038] The heating time is not particularly limited as long as it does not impair the effects of the present invention, but it is preferable to adjust the oligomer consumption to 20% by mass or more from the viewpoints of molecular weight elongation and weight loss reduction.
[0039] In this process, by performing heat treatment under an inert gas atmosphere, the formation of branched structures in the PAS resin can be suppressed, and the molecular weight can be increased while maintaining the linear structure. The reason why such an effect is obtained is not necessarily clear, but it is speculated to be due to the following mechanism. That is, in an inert gas atmosphere and a high temperature environment, the cyclic PAS oligomer contained in PAS oligomer (b) and PAS oligomer (c) opens the ring and exerts a molecular chain elongation effect at the end of the PAS resin. In addition, the linear PAS oligomer contained in PAS oligomer (c) suppresses the formation of branched structures by having the carboxylic acid in the structure react with the alkali metal at the end of the PAS resin to suppress the generation of radicals. It is considered that the synergistic effect of the cyclic and linear PAS oligomers causes the PAS resin to polymerize while maintaining the linear structure. Note that the above mechanism is merely speculation, and even if the effect of the present invention is achieved for other reasons, it is included in the technical scope of the present invention.
[0040] In addition, in this step, the reduction rate of the chemiluminescence intensity of the polyarylene sulfide resin before and after the heat treatment is preferably in the range of 45% or less, more preferably in the range of 30% or less, and further preferably in the range of 15% or less, where the chemiluminescence intensity in the present disclosure is a value obtained by measurement in an oxygen atmosphere at 150°C by the method described in the Examples.
[0041] PAS resin shows weak chemiluminescence, which is presumed to be derived from active groups (such as terminal SH groups) in the PAS molecule. Therefore, the content of active groups in the PAS molecule can be roughly calculated by measuring the chemiluminescence intensity of the PAS resin. For example, when heat treatment is performed under an oxidizing gas atmosphere, the PAS active groups are first converted to radicals by heating, and the radicals are incorporated into other PAS molecules by chemical reaction to form branched structures, and the radicals disappear. In other words, the active groups in the PAS resin after heat treatment are reduced, so the chemiluminescence intensity derived from the active groups is reduced. On the other hand, when heat treatment is performed under an inert gas atmosphere, there is no change in the active groups due to heating, so no branched structures are formed, and the PAS resin is polymerized while maintaining its linear structure. Since the state of the active groups does not change, the chemiluminescence intensity derived from the active groups in the PAS resin is maintained even after heat treatment. According to the above mechanism, if the change in the chemiluminescence intensity of the resin before and after heat treatment is small, it is considered that the polymerization while maintaining the linear structure is preferentially progressing. It should be noted that the above mechanism is merely speculation, and even if the chemiluminescence intensity contributes to the effect of the present invention for other reasons, it is still included in the technical scope of the present invention.
[0042] <Composition (C) Containing 10% by Mass or More of Oligoarylene Sulfide (c)> The method for producing a PAS resin according to this embodiment is characterized in that in steps (2) and / or (3), a composition (C) containing 10% by mass or more of a PAS oligomer (c) is added to at least one of the crude reaction mixture and the mixture (A), and the PAS oligomer (c) contains a linear PAS oligomer and a cyclic PAS oligomer.
[0043] When the composition (C) is added in the step (2), it can be added to the crude reaction mixture before solid-liquid separation and / or the mixture (A) obtained after solid-liquid separation. When the composition (C) is added in the step (3), it can be added to the mixture (A) before or during washing. The amount of the composition (C) added is not particularly limited as long as it does not impair the effects of the present invention, but it is preferable to adjust the amount of the PAS oligomer (c) contained in the composition (C) to 0.1 to 30 mass%, more preferably 0.5 to 25 mass%, of the content (theoretical yield) of the PAS resin (a) contained in the object to which it is added. Within this range, molecular weight elongation by heat treatment in the step (4) can be efficiently performed.
[0044] In this embodiment, the amount of the linear PAS oligomer and the cyclic PAS oligomer in the PAS oligomer (c) is not particularly limited, but the linear PAS oligomer is preferably contained at 10 to 90 mass%, more preferably at 20 to 70 mass%, in which case the reaction rate and molecular chain elongation effect in the subsequent heat treatment step are excellent.
[0045] The content of the PAS oligomer (c) in the composition (C) and the contents of the linear PAS oligomer and cyclic PAS oligomer in the PAS oligomer (c) can be measured by the method described in the Examples.
[0046] The carboxylic acid content of the linear PAS oligomer used in this embodiment is not particularly limited, but from the viewpoint of the radical suppression effect in the heat treatment step, it is preferably 50 μmol / g or more, preferably 500 μmol / g or less, and more preferably 200 μmol / g or less. The carboxylic acid content of the linear PAS oligomer in this disclosure is a value measured by the following method using a Fourier transform infrared spectrometer (hereinafter abbreviated as "FT-IR device"). That is, the linear PAS oligomer was separated, hot-pressed at 280°C, and then rapidly cooled to prepare a film showing amorphousness as a test piece, which was then measured with the FT-IR device. The 630.6 cm peak in the infrared absorption spectrum was -1 Absorption at 1705cm-1 The relative intensity of absorption was measured, and the carboxylic acid content in the measurement sample was calculated using a calibration curve prepared using p-chlorophenylacetic acid as a sample. The carboxylic acid content is expressed as the number of moles per gram of linear PAS oligomer, and its unit is μmol / g.
[0047] The method for producing the composition (C) is not particularly limited, and the composition can be produced, for example, by a production method having a step similar to the step (1) and the following step (5). That is, the composition can be produced by a production method having a step (1) of reacting a polyhalo aromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent to obtain a crude reaction mixture containing at least a PAS resin, a PAS oligomer (c), an alkali metal halide, and an organic polar solvent, and the following step (5).
[0048] ·Process (5) In step (5), solid phase components are removed from the crude reaction mixture by solid-liquid separation to obtain a liquid phase component containing at least the PAS oligomer (c). The quench method is preferred for the solid-liquid separation in this step, because it is less likely that impurities such as by-products and unreacted raw materials will be incorporated into the polymer particles during crystallization, and a larger amount of the PAS oligomer can be recovered in the liquid phase component.
[0049] The quench method is a method of crystallizing a particulate PAS resin by gradually cooling a crude reaction mixture. In general, the crude reaction mixture is gradually cooled from a high-temperature, high-pressure state to crystallize the PAS resin in the reaction system, and then the solid-liquid separation is performed by filtration or the like to recover the solid phase component and liquid phase component containing the PAS resin as granules. There is no particular limit to the cooling time, but the preferred range is usually 0.1°C / min to 3°C / min. In addition, it is not necessary to slowly cool at the same rate throughout the entire slow cooling process, and a method in which the rate is in the range of 0.1°C / min to 1°C / min until the granular PAS resin crystallizes, and then cooling at a rate of 1°C / min or more is also preferred. It is preferable to finally cool to 70°C or higher, preferably 100°C or higher and 200°C or lower, and then perform solid-liquid separation to separate the solid phase component containing the PAS resin and recover the liquid phase component. In the quench method, solid-liquid separation can be performed by filtration or using a centrifuge such as a screw decanter. Furthermore, the polymerization solvent can be added again to the obtained solid phase component to form a slurry, and solid-liquid separation can be repeated.
[0050] The liquid phase component thus obtained may contain, in addition to the PAS oligomer (c) and the organic polar solvent, by-products such as a carboxyalkylamino group-containing compound and a terminal SH group-containing compound, unreacted raw materials, and water. The liquid phase component can be used as is as composition (C), but can also be further purified. In that case, by subjecting the liquid phase component to a known purification operation, other by-products can be removed and the concentration of the PAS oligomer (c) can be increased.
[0051] By adding the composition (C) in step (2), components other than the PAS oligomer (c) contained in the composition (C) can be efficiently removed in the subsequent step (3), which eliminates the need for a step of purifying the composition (C) in advance to extract the PAS oligomer (c), thereby reducing production costs and improving the reuse rate of the PAS oligomer.
[0052] The PAS resin obtained by the above manufacturing method has Mw / Mtop in the range of 0.82 to 1.18, preferably 0.85 to 1.15. In the present disclosure, Mw indicates the weight average molecular weight measured by gel permeation chromatography, and Mtop indicates the average molecular weight (peak molecular weight) at the point where the detection intensity of the chromatogram obtained by the same measurement is maximum. Mw / Mtop is an index of the distribution of the molecular weight of the measurement target, and generally, the closer the value is to 1, the narrower the molecular weight distribution is, and the larger the value is, the wider the molecular weight distribution is. In addition, the more polymers having a branched structure, the larger Mw / Mtop tends to be. In the present disclosure, the values of Mw and Mtop are values measured by the method described in the Examples, but it is possible to change the measurement conditions within a range that does not substantially affect the values of Mw and Mw / Mtop.
[0053] The PAS resin obtained by the above manufacturing method has a melt viscosity (V6) measured at 300°C in the range of 5 to 5,000 [Pa·s], and more preferably in the range of 10 to 2,000 [Pa·s]. However, the melt viscosity (V6) measured at 300°C refers to the melt viscosity after being held for 6 minutes using a flow tester at a temperature of 300°C, a load of 1.96 MPa, and an orifice with an orifice length / orifice diameter ratio of 10 / 1.
[0054] The PAS resin obtained by the above-mentioned production method preferably has a chemiluminescence intensity per gram in the range of 1,000 to 10,000,000 counts / sec, more preferably in the range of 10,000 to 5,000,000 counts / sec, and even more preferably in the range of 10,000 to 1,000,000 counts / sec. The chemiluminescence intensity is a value measured by the method described in the Examples.
[0055] <Composition / Applications, etc.> The PAS resin obtained by the above-mentioned manufacturing method can contain additives such as a mold release agent, a colorant, a heat stabilizer, an ultraviolet stabilizer, a foaming agent, an anti-rust agent, a flame retardant, a lubricant, a coupling agent, and a filler, as long as the effects of the present invention are not impaired. As the filler, any known and commonly used material can be used as long as it does not impair the effects of the present invention, and examples of such fillers include inorganic fillers of various shapes, such as fibrous ones and non-fibrous ones such as granular and plate-shaped ones. Specifically, fibrous fillers such as fibers such as glass fiber, carbon fiber, silane glass fiber, ceramic fiber, aramid fiber, metal fiber, potassium titanate, silicon carbide, calcium silicate, and wollastonite, and natural fibers can be used, and non-fibrous fillers such as glass beads, glass flakes, barium sulfate, clay, pyrophyllite, bentonite, sericite, mica, talc, attapulgite, ferrite, calcium silicate, calcium carbonate, glass beads, zeolite, milled fiber, and calcium sulfate can also be used.
[0056] The PAS resin obtained by the above-mentioned manufacturing method can also be mixed with the following synthetic resins and elastomers to the extent that the effects of the present invention are not impaired. Examples of the synthetic resins include polyester, polyamide, polyimide, polyetherimide, polycarbonate, polyphenylene ether, polysulfone, polyethersulfone, polyetheretherketone, polyetherketone, polyarylene, polyethylene, polypropylene, polytetrafluoroethylene, polydifluoroethylene, polystyrene, ABS resin, epoxy resin, silicone resin, phenolic resin, urethane resin, liquid crystal polymer, etc., and examples of the elastomers include polyolefin rubber, fluororubber, silicone rubber, etc.
[0057] Furthermore, the PAS resin obtained by the manufacturing method according to this embodiment has excellent heat resistance, moldability, dimensional stability, etc., when used in various melt processing methods such as injection molding, extrusion molding, compression molding, blow molding, etc. Therefore, it can be widely used as injection-molded or compression-molded products such as electric or electronic parts, such as connectors, printed circuit boards, and encapsulated molded products, automobile parts, such as lamp reflectors and various electrical parts, interior materials for various buildings, aircraft, automobiles, etc., precision parts, such as office equipment parts, camera parts, and watch parts, or extrusion-molded or pultrusion-molded products, such as fibers, films, sheets, and pipes. EXAMPLES
[0058] The present invention will be specifically described below with reference to examples. These examples are illustrative and not limiting. In the following, unless otherwise specified, "%" and "parts" are based on mass.
[0059] <Production Example 1: Production and evaluation of a composition containing 10% by mass or more of PAS oligomer (c)> 129.42g of flake sodium sulfide (60.3% by weight Na2S) and 300.0g of N-methyl-2-pyrrolidone (NMP) were charged into a 1L autoclave equipped with a stirring blade connected to a pressure gauge, a thermometer, and a condenser. The temperature was raised to 209°C while stirring under a nitrogen stream, and 30.96g of water was distilled off (the remaining water content was 1.13 moles per mole of sodium sulfide). The autoclave was then sealed and cooled to 180°C, and 147.90g of p-dichlorobenzene (hereinafter abbreviated as DCB) and 120.0g of NMP were charged. At a liquid temperature of 150°C, the gauge pressure was increased to 0.1MPa using nitrogen gas, and the temperature was raised. The reaction was allowed to proceed with stirring for 3 hours at a liquid temperature of 260°C. The maximum pressure during the reaction was 0.85MPa. After the reaction, the mixture was cooled, and when the temperature reached 170°C, a solution containing 1.89g (0.015 mol) of oxalic acid dihydrate in 4.42g of NMP was pressure-injected, stirred for 30 minutes, and then cooled. The entire reaction slurry obtained was filtered at 120°C, and 320g of NMP was added to wash the cake, followed by filtration. The amount of NMP filtrate obtained was 536g.
[0060] 536 g of the NMP filtrate was placed in a 1 L eggplant flask, and NMP was removed by distillation at 150 ° C under reduced pressure using a rotary evaporator, to obtain 18.35 g of a composition containing a PPS oligomer. Water was added to the composition containing the PPS oligomer to form a water slurry, and solid-liquid separation and washing with water were repeated three times, and then dried to obtain a powder. 5.0000 g of the obtained powder was taken out, 75 mL of chloroform was added, and the mixture was refluxed for 1 hour while heating to 62 ° C. The residue after the reflux operation was taken as linear PPS oligomer, and the solid matter contained in the obtained chloroform extract when it was gradually cooled to room temperature was taken as cyclic PPS oligomer, and the weights were measured. The linear PPS oligomer content was 1.85 g, and the cyclic PPS oligomer content was 3.15 g. From the obtained values, the PPS oligomer content, linear PPS oligomer content, and cyclic PPS oligomer content in the composition containing PPS oligomer were calculated to be 27.8 mass%, 37 mass%, and 63 mass%, respectively. The carboxylic acid content in the linear PPS oligomer was 160 μmol / g.
[0061] <Examples 1 to 4 and Comparative Examples 1 to 5>
[0062] <Example 1> ·Process (1) A 1L autoclave with an agitator connected to a pressure gauge, a thermometer, a condenser, a decanter, and a rectification column was charged with 244.02g (1.66 moles) of DCB, 26.96g (0.16 moles) of NMP, 201.78g of 47.23% by mass NaSH aqueous solution (1.70 moles as NaSH), and 135.74g of 49.21% by mass NaOH aqueous solution (1.67 moles as NaOH), and the mixture was heated to 173°C over 5 hours under a nitrogen atmosphere while stirring, and 200.59g of water was distilled off, after which the kettle was sealed. The DCB distilled by azeotropy during dehydration was separated in a decanter and returned to the kettle as needed. After the dehydration was completed, the anhydrous sodium sulfide composition was dispersed in the DCB in the kettle. After the dehydration step, the inside temperature was cooled to 160°C, 340.92g (3.40 moles) of NMP was charged, and the temperature was raised to 185°C. When the pressure reached 0.00MPa, the valve connected to the distillation tower was opened, and the inside temperature was raised to 200°C over 1 hour. At this time, the cooling and valve opening were controlled so that the outlet temperature of the distillation tower was 110°C or less. The mixed vapor of distilled DCB and water was condensed in a condenser and separated in a decanter, and DCB was returned to the kettle. The amount of distilled water was 1.32g. The inside temperature was raised from 200°C to 230°C over 3 hours, stirred for 3 hours, and then raised to 250°C and stirred for 1 hour.
[0063] ·Process (2) After the reaction was completed, 26.4 g of the PPS oligomer contained in the composition obtained in Production Example 1 was added so that the amount was equivalent to 4 mass % relative to the PPS resin, and the bottom valve of the autoclave was opened to flush the autoclave into a 2 L vacuum stirring dryer equipped with a stirring blade to remove the NMP, and the autoclave was cooled to room temperature. A crude PPS mixture with a solid content of 55% was obtained.
[0064] ·Process (3) 600g of 70°C ion-exchanged water was added to the entire amount of the obtained crude PPS mixture, stirred for 30 minutes, and then filtered. 1L of 70°C ion-exchanged water was added to the cake after filtration to wash the cake. Furthermore, the obtained wet cake and 600g of ion-exchanged water were charged into a 1L autoclave equipped with a stirring blade, heated to 230°C over 2 hours while stirring, extracted by stirring for 30 minutes, and cooled to room temperature. The entire amount of the obtained mixture was filtered, and 1L of 70°C ion-exchanged water was added to the cake after filtration to wash the cake. It was dried at 120°C for 4 hours to obtain PPS resin with a melt viscosity (V6) of 130 Pa·s and a yield of 191.3g.
[0065] ·Process (4) 50 g of the above PPS resin was heat-treated for 15 hours in an inert gas oven at 240° C. under an inert gas atmosphere. The properties of the PPS resin obtained after the treatment are shown in Table 1.
[0066] <Example 2> The same procedure as in Example 1 was repeated, except that in step (2), 132.6 g of the PPS oligomer contained in the composition obtained in Production Example 1, which corresponds to 20 mass % based on the PPS resin, was added. The properties of the obtained PPS resin are shown in Table 1.
[0067] <Example 3> The same procedure as in Example 1 was repeated, except that in step (3), 26.4 g of the PPS oligomer contained in the composition obtained in Production Example 1, which corresponds to 4 mass % based on the PPS resin, was added. The properties of the obtained PPS resin are shown in Table 1.
[0068] <Example 4> The same procedure as in Example 1 was repeated, except that in step (3), 132.6 g of the PPS oligomer contained in the composition obtained in Production Example 1, which corresponds to 20 mass % based on the PPS resin, was added. The properties of the obtained PPS resin are shown in Table 1.
[0069] <Comparative Example 1> The same procedure as in Example 1 was repeated, except that step (2) was carried out without adding the composition obtained in Production Example 1. The properties of the obtained PPS resin are shown in Table 2.
[0070] <Comparative Example 2> The same procedure as in Example 1 was repeated, except that in step (2), 264 g of the PPS oligomer contained in the composition obtained in Production Example 1, which corresponds to 40 mass % based on the PPS resin, was added. The properties of the obtained PPS resin are shown in Table 2.
[0071] <Comparative Example 3> The same operations as in Example 1 were carried out except that in step (3), 264 g of the PPS oligomer contained in the composition obtained in Production Example 1, which corresponds to 40 mass % based on the PPS resin, was charged. The properties of the obtained PPS resin are shown in Table 2.
[0072] <Comparative Example 4> Except for carrying out the step (4) under an oxygen-containing gas atmosphere, the same procedure as in Example 1 was carried out. The properties of the obtained PPS resin are shown in Table 2.
[0073] <Comparative Example 5> Except for carrying out the step (4) under an oxygen-containing gas atmosphere, the same procedure as in Example 3 was carried out. The properties of the obtained PPS resin are shown in Table 2.
[0074] <Evaluation>
[0075] (1) Measurement of Mtop and Mw / Mtop The weight average molecular weight (Mw) and peak molecular weight (Mtop) of the PPS resin obtained in each of the Examples and Comparative Examples were measured by gel permeation chromatography under the following measurement conditions, and Mw / Mtop was calculated. The results are shown in Tables 1 and 2. Six types of monodisperse polystyrene were used for calibration. Equipment: Ultra-high temperature polymer molecular weight distribution measuring device (SSC-7000, manufactured by Senshu Scientific Co., Ltd.) Column: UT-805L (Showa Denko K.K.) Column temperature: 210℃ Solvent: 1-chloronaphthalene Measurement method: UV detector (360 nm)
[0076] (2) Measurement of weight loss The powder samples of PPS resin obtained in each Example and Comparative Example were weighed into 4.0000 g aluminum petri dishes using a precision balance. The samples were left to stand in a dryer set at 150°C for 1 hour, then the petri dishes were removed and allowed to cool to room temperature before being weighed. The same petri dishes were then left to stand in a dryer set at 370°C for 1 hour, then the petri dishes were removed and allowed to cool to room temperature before being weighed. The weight loss of each sample was calculated using the following formula. The results are shown in Tables 1 and 2. {(Weight value after heating to 150℃) - (Weight value after heating to 370℃)} ÷ (Weight value after heating to 150℃) × 100
[0077] (3) Measurement of recrystallization temperature (Tc2) The recrystallization temperature of the PPS resin obtained in each of the Examples and Comparative Examples was evaluated using a differential scanning calorimeter (Perkin Elmer's "DSC8500") by measuring the peak top temperature of the exothermic peak resulting from the crystallization of the resin when the temperature was increased from 40° C. to 350° C., held for 3 minutes, and then decreased at a rate of 20° C. / min to 120° C. The results are shown in Tables 1 and 2.
[0078] (4) Measurement of chemiluminescence intensity In step (4) in each example and comparative example, the chemiluminescence intensity of the PPS resin before and after the heat treatment was measured. The measurement was performed using a "Chemiluminescence Analyzer CLA-FS5" manufactured by Tohoku Electronics Industries Co., Ltd. Specifically, PPS resin (0.10 g of sample) was placed in the sample chamber of the device, and the room temperature was first raised to 150°C under nitrogen flow as preheating, and then maintained at 150°C for 5 minutes, and then cooled to 75°C. The temperature was then maintained at 75°C for 5 minutes, the gas in the chamber was switched from nitrogen to oxygen, and the temperature was raised again to 150°C and maintained at 150°C for 5 minutes. The chemiluminescence intensity shown by the sample at that time was divided by the sample weight (g) to obtain the chemiluminescence intensity per 1 g. Using this value, the reduction rate of chemiluminescence intensity due to heat treatment was calculated using the following formula. The results are shown in Tables 1 and 2. ·CL0: Chemiluminescence intensity per gram of PPS resin after steps (1) to (3) CL1: Chemiluminescence intensity per gram of PPS resin after steps (1) to (4) (Reduction rate of chemiluminescence intensity, %) = (CL0-CL1)÷CL0×100
[0079] [Table 1]
[0080] [Table 2]
[0081] From the results in Table 1, comparing the PPS resin obtained by the manufacturing method of the Example with the PPS resin of Comparative Example 1, it was shown that the addition of oligomers increased Mtop and increased the molecular weight. Comparing the Example with Comparative Examples 2 and 3, it was found that weight loss increased when too much oligomer was added. Comparing the Example with Comparative Examples 4 and 5, it was shown that when treated in an oxidizing atmosphere, Mw / Mtop increased, and thus a polymer having a crosslinked structure was formed during heat treatment, resulting in a broader molecular weight distribution.
Claims
1. (1) reacting a polyhaloaromatic compound with (i) an alkali metal sulfide, or (ii) an alkali metal hydrosulfide and an alkali metal hydroxide in an organic polar solvent to obtain a crude reaction mixture containing at least a polyarylene sulfide resin (a), an oligoarylene sulfide (b), an alkali metal halide, and an organic polar solvent; (2) removing a liquid phase component from the crude reaction mixture by solid-liquid separation using a flash method to obtain a mixture (A) containing at least a polyarylene sulfide resin (a), an oligoarylene sulfide (b), and an alkali metal halide; (3) a step of washing the mixture (A) to remove alkali metal halides to obtain a mixture (B) containing at least a polyarylene sulfide resin (a) and an oligoarylene sulfide (b); and The method includes a step (4) of heat-treating the mixture (B) under an inert gas atmosphere, and In the step (2) and / or (3), adding a composition (C) containing 10% by mass or more of an oligoarylene sulfide (c) to at least one of the crude reaction mixture and the mixture (A); A method for producing a polyarylene sulfide resin, wherein the oligoarylene sulfide (c) contains a chain oligoarylene sulfide and a cyclic oligoarylene sulfide.
2. The method for producing a polyarylene sulfide resin according to claim 1, wherein the amount of the oligoarylene sulfide (c) added in the steps (2) and / or (3) is in the range of 0.1 to 30 mass% based on the polyarylene sulfide resin (a).
3. The composition (C) The step (1), (5) removing a solid phase component from the crude reaction mixture by solid-liquid separation to obtain a liquid phase component containing at least an oligoarylene sulfide (c); The method for producing the polyarylene sulfide resin according to claim 1 or 2, which is obtained by a production method comprising the steps of:
4. 3. The method for producing a polyarylene sulfide resin according to claim 1, wherein the oligoarylene sulfide (c) contains 10 to 90 mass % of a chain oligoarylene sulfide.
5. The method for producing a polyarylene sulfide resin according to claim 1 or 2, wherein the melt viscosity (V6) of the polyarylene sulfide resin obtained by the steps (1) to (4) measured at 300°C is in the range of 10 to 2000 [Pa·s]. (Note that the melt viscosity (V6) represents the melt viscosity after holding for 6 minutes using a flow tester at a temperature of 300° C., a load of 1.96 MPa, and an orifice with an orifice length / orifice diameter ratio of 10 / 1.)
6. 3. The method for producing a polyarylene sulfide resin according to claim 1 or 2, wherein a decrease in chemiluminescence intensity of the polyarylene sulfide resin before and after the heat treatment in the step (4) is 45% or less. (Note that the chemiluminescence intensity was measured at 150°C in an oxygen atmosphere.)
Citation Information
Patent Citations
Method of manufacturing polyarylene sulfide