Olefinic resin packaging material

The olefin resin packaging material with a high olefin content and iron powder enhances oxygen barrier properties, ensuring recyclability and effective oxygen scavenging, addressing the challenge of monomaterials with insufficient oxygen barriers.

JP2024133047APending Publication Date: 2024-10-01TOYO SEIKAN KAISHA LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024042380
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2024-03-18
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Olefin resins used in packaging materials lack sufficient oxygen barrier properties, which is a major obstacle in creating monomaterials that are recyclable and require minimal use of different materials.

Method used

An olefin resin packaging material containing 80 parts by mass of olefin resin, less than 15 parts by mass of other resins, and less than 5 parts by mass of iron powder, with optional additives like metal halides and alkaline compounds, and a multilayer structure to enhance oxygen barrier properties.

Benefits of technology

The packaging material maintains recyclability and oxygen barrier properties while minimizing the use of additional materials, allowing easy separation and reuse of olefin resin, and providing effective oxygen scavenging without environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133047000001
    Figure 2024133047000001
Patent Text Reader

Abstract

To provide an olefinic resin packaging material which contains a large amount of olefinic resin, is suitable for recyclability of the olefinic resin, and simultaneously has excellent characteristics that are not seen in the olefinic resin.SOLUTION: An olefinic resin packaging material contains, based on 100 pts.mass of the packaging material, 80 pts.mass or more of an olefinic resin, less than 15 pts.mass of a resin other than the olefinic resin, and less than 5 pts.mass of iron powder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a packaging material such as a bag (pouch) made of an olefin-based resin. [Background technology]

[0002] Olefin-based resins are inexpensive, exhibit heat-sealing properties, and are easy to mold into bags and the like, and therefore are widely used for molding packaging materials such as pouches (see Patent Documents 1 and 2).

[0003] However, since olefin resins have low oxygen barrier properties, it is necessary to impart oxygen barrier properties to the packaging material in the final form in which the contents are packaged, and for this reason, as described in the above patent document, gas barrier resins such as ethylene-vinyl alcohol copolymers (EVOH) and aromatic polyamides are often used in combination with olefin resins. However, from the viewpoint of environmental protection in recent years, there is a demand for recyclability of various materials, and in the field of packaging materials, there is a demand for mono-materials that minimize the use of different materials as much as possible, and for example, a pouch containing olefin resins at a content of 80% by mass or more has been proposed (see Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-214352 A [Patent Document 2] JP 2020-97421 A [Patent Document 3] WO2022 / 054891 Summary of the Invention [Problem to be solved by the invention]

[0005] A major obstacle to the creation of mono-materials from the above-mentioned olefin-based resins is the oxygen barrier property. That is, when creating a mono-material, the use of different materials is greatly restricted, so the question is how to impart properties such as oxygen barrier property.

[0006] Therefore, an object of the present invention is to provide a packaging material made of an olefin-based resin that contains a large amount of olefin-based resin, is suitable for the recyclability of olefin-based resin, and at the same time, has excellent properties not found in olefin-based resins.

[0007] According to the present invention, there is provided an olefin-based resin packaging material, which is characterized in that it contains 80 parts by mass or more of olefin-based resin, the amount of resin other than olefin-based resin is suppressed to less than 15 parts by mass per 100 parts by mass of the packaging material, and contains iron powder in an amount of less than 5 parts by mass.

[0008] As the olefin-based resin packaging material of the present invention, the following embodiments are preferably adopted. (1) It must be in the form of a film or sheet. (2) It has the form of a bag. (3) Contains metal halides and alkaline compounds. (4) Contains white pigment. (5) Contains a gas barrier resin. (6) It has a multi-layer structure. Effect of the Invention

[0009] The olefin resin packaging material of the present invention is premised on containing 80 parts by mass of olefin resin per 100 parts by mass of the packaging material, and the content of resin components other than the olefin resin is suppressed to less than 15 parts by mass. This makes it easy to recover the olefin resin, and even if a different component is mixed in, it is possible to avoid a significant decrease in the properties of the olefin resin due to the mixing in of the different component, and it is possible to effectively reuse the olefin resin.

[0010] Furthermore, in the present invention, a small amount of iron powder, less than 5 parts by mass, is contained. That is, the incorporation of iron powder provides the mono-material properties of the olefin resin, and the incorporation of such a small amount of iron powder allows the iron powder to exhibit its deoxidizing properties (oxygen absorbing properties) and oxygen barrier properties. That is, oxygen barrier resins such as ethylene-vinyl alcohol copolymers (EVOH) require a fairly large amount to impart the oxygen barrier properties required for the packaging material, and it is not easy to separate them from the olefin resin after use. However, iron powder is a natural inorganic material, and not only does it not have a negative effect on the environment, it is also easy to separate from the olefin resin, and it can exhibit oxygen barrier properties with a small amount that maintains the mono-material properties, making it possible to satisfy both the recyclability and oxygen barrier properties of the olefin resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The packaging material of the present invention may have various forms, for example, it may be a packaging material in the form of a film or sheet that contains various substances, it may be a lid material that is attached to the mouth of a cup container by heat sealing, it may be a bag (pouch) obtained by making a film into a bag by heat sealing, or it may be a cup container obtained by vacuum forming or plug-assist molding a sheet. Furthermore, it may be a blown bottle obtained by blow molding a preform formed by extrusion molding or injection molding. However, it is most suitable to be a bag from the viewpoint of maximizing the properties of the iron powder blended, in which the content of resin components other than olefin resin is less than 15 parts by mass and the content of iron powder is less than 5 parts by mass per 100 parts by mass of the packaging material.

[0012] Furthermore, the packaging material may have a single layer structure made of an olefin-based resin containing iron powder, or may have a multi-layer structure including at least one layer of an olefin-based resin containing iron powder.

[0013] Olefin resins; The olefin-based resin used as the main material forming the packaging material of the present invention may be any olefin-based resin known per se. Representative examples of such olefin-based resins include well-known resins that have traditionally been used as packaging materials, such as ethylene-based resins such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; and propylene-based resins such as homopolypropylene, random polypropylene (random PP), and block polypropylene (block PP). Furthermore, olefin-based copolymers such as poly-1-butene, poly-4-methyl-1-pentene, or random or block copolymers of α-olefins such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, and cyclic olefin copolymers disclosed in, for example, JP 2007-284066 A can also be used.

[0014] In the present invention, ethylene-based resins and propylene-based resins are most suitable, as they have been widely used in various applications and are particularly required to have good recyclability and excellent heat sealability.

[0015] The above-mentioned olefin resins are used in a manner appropriate to the properties required for the packaging material. For example, in applications where heat sterilization such as retort sterilization is applied, propylene-based resins are particularly suitable, and block PP, which has excellent heat resistance and impact resistance, is particularly suitable. Also, when heat sealing is performed for bag manufacturing, such as for bags, the film is used in the form of an unstretched film. In this case, a stretched propylene film can be laminated on an unstretched olefin resin film to improve its strength. In this case, a dry lamination adhesive or the like is used, and it is naturally necessary to maintain the olefin resin content at 80 parts by mass or more per 100 parts by mass of the packaging material, preferably 85 parts by mass or more, and more preferably 90 to 99 parts by mass.

[0016] Iron powder; The iron powder used in the present invention is known as an inorganic material that exhibits deoxidizing properties (oxygen absorbing properties). That is, iron reacts with moisture to generate divalent iron hydroxide, which reacts with oxygen to produce ferric oxide (Fe 2 O 3 This property is used for deoxidation to impart oxygen barrier properties to the packaging material and prevent oxidation deterioration of the packaged substance. The amount of this iron powder is less than 5 parts by mass, preferably 0.1 to 4.0 parts by mass, and more preferably 0.2 to 1.1 parts by mass, per 100 parts by mass of the packaging material, and is used in an amount that does not violate the condition that the olefin resin content is 80 parts by mass or more.

[0017] Such iron powder usually has a BET specific surface area of ​​0.5 m, as disclosed in, for example, Japanese Patent No. 5378639. 2 / g or more. As such iron powder, known iron powders such as reduced iron powder, atomized iron powder, electrolytic iron powder, and carbonyl iron powder can be used, but reduced iron powder is preferably used because of its high oxygen absorption ability. That is, reduced iron powder is obtained by reducing iron ore and has a large specific surface area. Furthermore, among reduced iron powders, rotary reduced iron powder is particularly preferable because of its high purity. In particular, as described in the above patent, iron powder in which the half-width of the peak of the iron (110) plane measured by powder X-ray diffraction method (Co-Kα) is adjusted to 0.20° / 2θ or less by moderate heat treatment is preferable because it suppresses the generation of hydrogen as a by-product of the oxygen absorption reaction.

[0018] The iron powder is mixed with an olefin resin to form an olefin resin layer, but is basically blended into an unstretched layer, because blending of such iron powder impairs stretchability.

[0019] In addition, it is preferable to blend a metal halide and an alkaline substance as an auxiliary agent for promoting the oxygen absorption reaction of the iron powder in the olefin-based resin layer (unstretched layer) in which the iron powder is blended as described above.

[0020] Metal halides function as assistants that promote the oxygen absorption reaction, and are halides of various metals (e.g., alkali metals, alkaline earth metals, copper, zinc, iron, etc.), and examples of such halides include sodium chloride, sodium bromide, sodium iodide, potassium chloride, potassium bromide, potassium iodide, calcium chloride, magnesium chloride, barium chloride, etc. In particular, sodium chloride is most suitable in terms of performance as an assistant and cost.

[0021] Such metal halides may be used in small amounts compared to the iron powder, for example, in an amount of 0.1 to 10 parts by mass, particularly 1 to 5 parts by mass, per 100 parts by mass of iron powder.

[0022] The alkaline substance absorbs water and promotes the oxygen absorption reaction by the iron powder, and examples of the alkaline substance that can be used include magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, etc. In particular, non-carbonate compounds are preferred in terms of avoiding foaming, and slaked lime (calcium hydroxide) and quicklime (calcium oxide) are preferably used.

[0023] Such an alkaline substance may be used in a small amount compared to the iron powder, for example, in an amount of 0.5 to 2 parts by mass, particularly 1 to 2 parts by mass, per 100 parts by mass of iron powder.

[0024] Naturally, the auxiliary used together with the iron powder as described above is used in an amount that does not violate the condition that the olefin-based resin content is 80 parts by mass or more per 100 parts by mass of the packaging material. However, as described above, the amount is very small compared to the iron powder, so this condition is not violated.

[0025] Other materials; In the present invention, materials other than iron powder may be contained within a range that does not violate the condition that the olefin-based resin content is 80 parts by mass or more per 100 parts by mass of the packaging material.

[0026] For example, in order to reinforce the strength, a stretched film can be laminated onto an unstretched olefin resin film (iron powder-containing film), and typical examples of such stretched films include polyamide films such as nylon and polyester films such as polyethylene terephthalate (PET) in addition to stretched polypropylene films. That is, when a resin film other than an olefin resin film is used, it should be significantly thinner than the total thickness of the laminated film so as to satisfy the above conditions.

[0027] Furthermore, in order to laminate a stretched film onto an unstretched olefin-based resin film (iron powder-containing film), a dry lamination adhesive is used, and typical examples of such adhesives include epoxy adhesives and urethane adhesives. Of course, the layer formed by such an adhesive is also very thin in order to satisfy the above-mentioned olefin-based resin content.

[0028] Furthermore, conventionally known gas barrier resins, such as ethylene-vinyl alcohol copolymers (EVOH) and aromatic polyamides, can also be used on the condition that the above-mentioned olefin resin content is satisfied. However, when such a gas barrier resin layer is provided independently, it is necessary to make the layer considerably thick and to use an adhesive such as an acid-modified olefin resin. Therefore, when using a gas barrier resin, it is preferable to use a layer in which the olefin resin is mixed and to omit the adhesive layer. Furthermore, it is desirable to use an oriented olefin resin film with inorganic deposition such as alumina or silica as a barrier material other than EVOH or aromatic amide in terms of mono-materialization.

[0029] In addition, EVOH tends to deteriorate when heated in the presence of iron powder. Therefore, it is preferable to form a layer of olefin resin containing EVOH and a layer containing iron powder as separate layers, but when a mixture layer containing EVOH and iron powder is formed as in the examples described later, EVOH is contained in an amount of less than 15.0 parts by mass, preferably less than 10 parts by mass, more preferably less than 3.0 parts by mass, per 100 parts by mass of the mixture, depending on the content of iron powder.

[0030] In addition, the olefin resin layer containing iron powder has a color close to black, which may deteriorate the appearance characteristics of the packaging material and impair its commercial value. For this reason, in the packaging material of the present invention having a layer of olefin resin containing iron powder, it is preferable to provide a layer of olefin resin in which a white pigment is dispersed. That is, by providing a white pigment-dispersed olefin resin layer on the outer surface side of an olefin resin layer containing iron powder, it is possible to avoid deterioration of appearance characteristics due to the use of iron powder.

[0031] Examples of such white pigments include titanium oxide and zinc oxide. Of course, the amount of such white pigment used is set so that the olefin resin content is 80 parts by mass or more per 100 parts by mass of the packaging material.

[0032] In addition, the packaging material of the present invention described above can also be provided with a regrind layer formed using waste material (scrap) generated in the manufacturing process of the same product in a factory. Such a regrind layer is formed by co-extruding (or co-injecting) a resin composition in which the waste material is mixed with virgin olefin-based resin with a layer such as the iron powder-containing olefin-based resin layer. Even in packaging materials containing such a regrind layer, the content of the olefin-based resin is maintained at 80 parts by mass or more per 100 parts by mass of the packaging material. When scrap having an iron powder-containing olefin resin layer and an EVOH layer is used as a regrind layer, there is a concern that the deterioration of the EVOH may cause foaming or impair moldability. To suppress deterioration, the EVOH concentration in the layer where EVOH and iron powder coexist is important. It is preferable that the EVOH concentration is less than 10 parts by mass per 100 parts by mass of the coexisting layer.

[0033] The packaging material of the present invention is particularly suitable as a bag (pouch), and the layer structure of the film forming the pouch is shown below as an example, but is not limited to this. If necessary, the presence or absence of an adhesive layer and the structure of each layer can be changed. In addition, the black appearance caused by iron powder can be avoided by adding a white pigment such as titanium oxide to the iron powder-containing olefin layer or by forming a multilayer structure. In the following description, the following abbreviations are used: CPO: Unstretched olefin resin (no iron powder) FeCPO: Iron powder-containing olefin resin OPO: Oriented olefin resin VOPO: Vapor-deposition stretched olefin resin AD:Adhesive layer EV:EVOH EV+Fe+OL: A mixture layer of EVOH, iron powder, and olefin resin

[0034] FeCPO (single layer) (Internal) CPO / FeCPO (External) (Internal) CPO / FeCPO / CPO (External) (Internal) CPO / FeCPO / OPO (External) (inside) CPO / FeCPO / VOPO (outside) (Inside) CPO / EV+Fe+OL / VOPO (Outside) (inside) CPO / FeCPO / AD / VOPO (outside) (inside) CPO / EV+Fe+OL / AD / VOPO (outside) (inside) CPO / FeCPO / VOPO / AD / OPO (outside) (inside) CPO / EV+Fe+OL / VOPO / AD / OPO (outside) (Domestic) CPO / FeCPO / AD / EV / AD / CPO (External) (inside) CPO / FeCPO / AD / EV / AD / EV+Fe+OL / CPO (outside) (in) CPO / FeCPO / EV+Fe+OL / AD / EV / AD / EV+Fe+OL / CPO (outside) (inside) CPO / EV+Fe+OL / AD / EV / AD / CPO (outside) In addition, "inner" refers to the inside surface that comes into contact with the material being packaged, and "outer" refers to the outer surface that does not come into contact with the contents.

[0035] Recycling of olefin resins; The olefin-based resin packaging material of the present invention has an extremely high mono-material property when it contains 80 parts by mass or more of olefin-based resin per 100 parts by mass of the packaging material, and therefore has excellent recyclability of the olefin-based resin.

[0036] For example, this packaging waste is collected, appropriately separated from other molded products (e.g. polyester molded products), and foreign matter is removed as much as possible through crushing, washing, separation by specific gravity, etc. Then, it is dissolved using an appropriate solvent, and inorganic substances such as iron powder and white pigment are separated from olefin resin.

[0037] The olefin resin separated in this manner contains almost no other resins and is therefore reused as an olefin resin. It is usually mixed with virgin olefin resin and used to manufacture various plastic molded products. Instead of using a solvent to separate inorganic substances such as iron powder from the pulverized product from which foreign matter has been removed, the olefin resin can be decomposed (gasified) by heating and used as a heat source.

[0038] Furthermore, from the inorganic matter separated from the olefin resin, iron can be recovered using a magnet, and after appropriate alkaline washing, it can be used as iron powder for deoxidization.

[0039] In this way, the packaging material of the present invention contains 80 parts by mass or more of olefin-based resin per 100 parts by mass of the packaging material, which not only enables effective recycling of the olefin-based resin, but also allows oxygen barrier properties to be imparted with a small amount of iron powder, making it particularly ideal for use as a pouch. EXAMPLES

[0040] The present invention will be further described with reference to examples, but the present invention is not limited thereto. Using a 4-type, 6-layer multilayer sheet molding machine, each resin was melt-kneaded in a single-screw extruder, extruded into a sheet from a T-die at a T-die temperature of 230°C, solidified by contacting it with a cooling roll, and wound up to form a 500 μm-thick multilayer sheet. The layer structure is as follows: outermost PP layer 85μm / adhesive layer 10μm / EVOH layer 15μm / adhesive layer 10μm / mixture layer 130μm / inner PP layer 250μm. The resins used will be described later. The resulting multilayer sheet was heated to 145° C. and subjected to plug-assisted vacuum and pressure forming to form a flanged multilayer tray. The container dimensions are as follows: Flange outer diameter; Long axis: 155mm x short axis: 120mm Caliber; Long axis: 135mm x short axis: 100mm Bottom outer diameter; Long axis: 115mm x short axis: 90mm, height 35mm

[0041] Using the obtained container, the effect of the resin content of the mixture layer on the oxygen barrier property was evaluated. The evaluation method is as follows. After replacing the air in a glove box with nitrogen, 5 ml of distilled water was dropped into the container, which was covered with a barrier film made of a dry laminate of a silica deposition film and a non-oriented polypropylene film, and heat-sealed.The container was then stored at 30°C and 80% RH, and the oxygen concentration was measured by gas chromatography. The increase in oxygen concentration in the container after one month was 0% and was evaluated as ⊚, less than 0.5%, ◯, and 0.5% or more, respectively.

[0042] The resin materials used to mold the container are as follows: Outermost PP layer, inner PP layer; Ethylene-Propylene Block Copolymer MFR: 0.5g / 10min 230℃ Density: 0.90g / cm 3 adhesive layer; Maleic anhydride modified polypropylene MFR: 5.7g / 10min 230℃ Density: 0.89g / cm 3 EVOH layer; Ethylene-vinyl alcohol polymer Ethylene content: 32mol% MFR: 2.0g / 10min 190℃ Density: 1.17g / cm 3 mixture layer; A dry blend of PP resin, EVOH, and iron powder-containing olefin resin used in the outermost or inner layer. The iron powder-containing olefin resin used was a resin composition prepared by melt-kneading 29 parts by weight of an oxygen absorbent and 71 parts by weight of random polypropylene in a twin-screw extruder. The oxygen absorber has an apparent density of 1.86 g / cm 3 The reduced iron composition is composed of 100 parts by weight of reduced iron, 2 parts by weight of sodium chloride, and 1 part by weight of calcium hydroxide. The random polypropylene has an MFR of 1.2 g / 10 min (230°C) and a density of 0.91 g / cm 3 The following was used.

[0043] <Examples 1 to 4, Comparative Examples 1 and 2> The oxygen barrier properties of containers were evaluated by molding them while varying the ratio of each component in the mixture layer as shown in Table 1. The evaluation results are also shown in Table 1.

[0044]

Table 1

Claims

1. The olefin-based resin packaging material is characterized in that it contains 80 parts by mass or more of olefin-based resin per 100 parts by mass of the packaging material, resins other than the olefin-based resin are suppressed to less than 15 parts by mass, and iron powder is contained in an amount of less than 5 parts by mass.

2. 2. The olefin-based resin packaging material according to claim 1, which is in the form of a film or sheet.

3. 2. The packaging material according to claim 1, which is in the form of a bag.

4. 2. The packaging material according to claim 1, further comprising a metal halide and an alkaline compound.

5. 2. The packaging material according to claim 1, further comprising a white pigment.

6. The olefin-based resin packaging material according to claim 1, which contains a gas barrier resin.

7. 2. The packaging material according to claim 1, which has a multi-layer structure.

Citation Information

Patent Citations

  • Standing pouch and manufacturing method of the same

    JP2015214352A

  • Film and pouch

    JP2020097421A

  • Layered body for packaging

    WO2022054891A1