Methyl methacrylate composition

A balanced mixture of recycled and non-regenerated methyl methacrylate in a specific ratio addresses the heat resistance issue in recycled methyl methacrylate compositions, enhancing durability and storage stability.

JP2024133080APending Publication Date: 2024-10-01SUMITOMO CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024106822
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-07-29
Filing Date
2024-07-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Methyl methacrylate compositions derived from recycling methods may not provide sufficient heat resistance for molded articles.

Method used

A methyl methacrylate composition is formulated with a specific ratio of recycled and non-regenerated methyl methacrylate, ranging from 0.5 to 99.5% by mass each, to enhance heat resistance and glass transition temperature.

Benefits of technology

The composition achieves improved heat resistance and glass transition temperature, maintaining high quality and suppressing yellowing during long-term storage, suitable for applications requiring durability and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133080000001_ABST
    Figure 2024133080000001_ABST
Patent Text Reader

Abstract

To improve a heat resistance of a molded body.SOLUTION: A methyl methacrylate composition includes a recycled methyl methacrylate and a non-recycled methyl methacrylate. A content of the recycled methyl methacrylate is 0.5 to 99.5 mass%, and a content of the non-recycled methyl methacrylate is 0.5 to 99.5 mass%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a methyl methacrylate composition containing methyl methacrylate as a main component. [Background technology]

[0002] Polymethylmethacrylate (PMMA), a polymer of methyl methacrylate (MMA), has excellent transparency and weather resistance, and is therefore widely used as a material for components of automobile parts, signboards, display devices, etc.

[0003] In response to the recent rise in resource prices and growing awareness of environmental issues, efforts are being made to collect and recycle polymethyl methacrylate products (molded articles) that have been used for various applications as described above.

[0004] Methods for recycling polymethyl methacrylate include, for example, material recycling, in which the recovered molded bodies are subjected to a molding process again to produce new molded bodies; chemical recycling, in which the recovered molded bodies are heat-treated to thermally decompose (depolymerize) the polymethyl methacrylate to recover methyl methacrylate, and the recovered methyl methacrylate (sometimes referred to as recovered MMA) is used to produce new molded bodies; and thermal recycling, in which the recovered molded bodies are burned as fuel and the combustion energy is used directly as a heat source and further to generate electricity.

[0005] Polymethyl methacrylate is preferably recycled by chemical recycling, since methyl methacrylate can be recovered in high yield by heating at a relatively low temperature of about 300° C., and impurities can be reduced.

[0006] In chemical recycling of acrylic resin waste materials mainly composed of polymethyl methacrylate, a technology is known in which, when depolymerizing by heat treatment using a heating vessel having a stirring device, the tip speed of the stirring blade is focused on and adjusted to recover monomers such as methyl methacrylate generated by depolymerization as high-purity monomers without further decomposing them (see Patent Document 1). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2003-321571 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, depending on the methyl methacrylate obtained by the recovery method according to the above Patent Document 1, the heat resistance of a molded article obtained by molding a methyl methacrylate composition containing the methyl methacrylate may not be sufficient. [Means for solving the problem]

[0009] The present inventors have conducted intensive research to solve the above problems, and have found that the above problems can be solved by adjusting the composition of recycled methyl methacrylate and non-regenerated methyl methacrylate in the methyl methacrylate composition, thereby completing the present invention.

[0010] That is, the present invention provides the following [1] to

[12] . [1] Contains recycled methyl methacrylate and non-regenerated methyl methacrylate, A methyl methacrylate composition, comprising 0.5 to 99.5% by mass of recycled methyl methacrylate and 0.5 to 99.5% by mass of unregenerated methyl methacrylate. [2] The methyl methacrylate composition according to [1], wherein the recycled methyl methacrylate is chemically recycled methyl methacrylate. [3] The methyl methacrylate composition according to [1] or [2], wherein the content of the recycled methyl methacrylate is 5 to 40% by mass, and the content of the unregenerated methyl methacrylate is 60 to 95% by mass. [4] The methyl methacrylate composition according to any one of [1] to [3], further comprising an alkyl acrylate. [5] A method for producing a methyl methacrylate polymer, comprising a step of polymerizing the methyl methacrylate composition according to any one of [1] to [3]. [6] A methyl methacrylate polymer obtained by polymerizing the methyl methacrylate composition according to any one of [1] to [3]. [7] A methyl methacrylate polymer containing structural units derived from recycled methyl methacrylate and structural units derived from unregenerated methyl methacrylate, the content of the structural units derived from recycled methyl methacrylate being 0.5 to 99.5% by mass, and the content of the structural units derived from unregenerated methyl methacrylate being 0.5 to 99.5% by mass. [8] A heat resistance improver for methyl methacrylate polymers containing non-regenerated methyl methacrylate, the heat resistance improver comprising, as an active ingredient, a regenerated methyl methacrylate product derived from chemical recycling of polymethyl methacrylate. [9] The agent according to [8], wherein the polymer of the recycled methyl methacrylate product has a 5% weight loss temperature of 300°C or higher and / or a glass transition temperature of 90°C or higher.

[10] The agent according to [8] or [9], wherein the polymer of the non-regenerated methyl methacrylate product has a 5% weight loss temperature of 200°C or higher and / or a glass transition temperature of 105°C or higher.

[11] The agent according to any one of [8] to

[10] , wherein the 5% weight loss temperature of the polymer of the recycled methyl methacrylate product is higher than that of a non-recycled methyl methacrylate product, and / or the glass transition temperature is lower.

[12] Use of a regenerated methyl methacrylate product derived from chemical recycling of poly(methyl methacrylate) for producing a heat resistance improver for a methyl methacrylate polymer containing unregenerated methyl methacrylate. Effect of the Invention

[0011] According to the present invention, it is possible to improve the heat resistance of a methyl methacrylate-based polymer obtained by polymerizing a methyl methacrylate composition containing recycled methyl methacrylate, which may contain recovered MMA, and unregenerated methyl methacrylate, and further of a molded article thereof. [Brief description of the drawings]

[0012] [Figure 1] 1 is a graph showing the relationship between the proportion of recycled MMA and the 5% weight loss temperature in a molded product of a methyl methacrylate composition using the recovered MMA in Preparation Example 1. The dotted line in FIG. 1 is a straight line connecting the plots of Reference Example 1 and Comparative Example 1. [Diagram 2] 2 is a graph showing the relationship between the proportion of recycled MMA and the glass transition temperature in a molded product of a methyl methacrylate composition using the recovered MMA in Preparation Example 1. The dotted line in FIG. 2 is a straight line connecting the plots of Reference Example 1 and Comparative Example 1. [Diagram 3] Fig. 3 is a graph showing the relationship between the proportion of each recycled MMA and the 5% weight loss temperature in molded articles of methyl methacrylate compositions using recycled MMA (A) to (D). The dotted line in Fig. 3 is a straight line connecting the plots of Reference Example 1 and Comparative Example 2 of recycled MMA (A). [Figure 4] Fig. 4 is a graph showing the relationship between the proportion of each recycled MMA and the glass transition temperature in molded articles of methyl methacrylate compositions using recycled MMA (A) to (D). The dotted line in Fig. 3 is a straight line connecting the plots of Reference Example 1 and Comparative Example 5 using recycled MMA (D). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, the embodiments of the present invention will be described in detail. The present invention is not limited to the following description. Furthermore, each element of the embodiments of the present invention can be appropriately modified without departing from the gist of the present invention.

[0014] 1. Methyl methacrylate composition The methyl methacrylate composition of the present embodiment contains recycled methyl methacrylate and unregenerated methyl methacrylate, with the recycled methyl methacrylate content being 0.5 to 99.5 mass% and the unregenerated methyl methacrylate content being 0.5 to 99.5 mass%.

[0015] According to the methyl methacrylate composition of the present embodiment, the heat resistance, specifically the 5% weight loss temperature and the glass transition temperature, of the methyl methacrylate polymer obtained by polymerizing the methyl methacrylate composition and further of the molded product thereof can be improved, and the 5% weight loss temperature and the glass transition temperature can be made compatible to achieve a good balance between them. In addition, the methyl methacrylate composition can exhibit good storage stability, such as maintaining high quality even after long-term storage (for example, suppressing yellowing). Therefore, after the composition is prepared, it can maintain high quality even after long-term storage, and can be used for the manufacture of molded products at appropriate times.

[0016] The methyl methacrylate composition of the present embodiment is usually, but not limited to, a liquid. Hereinafter, components that may be contained in the methyl methacrylate composition of the present embodiment will be specifically described.

[0017] (1) Methyl methacrylate In this embodiment, "methyl methacrylate" refers to methyl methacrylate that is essentially free of impurities such as by-products such as methyl isobutyrate. However, it is not limited thereto, provided that the object of the present invention is not impaired. In other words, "methyl methacrylate" may contain impurities that cannot be completely removed by conventional purification methods, or may contain impurities at a content that cannot be detected by conventional detection methods.

[0018] In this embodiment, the method for producing methyl methacrylate is not particularly limited. Examples of the method for producing methyl methacrylate, which is the raw material of the methyl methacrylate composition of this embodiment, include the "ACH (acetone cyanohydrin) method" which is carried out using acetone and hydrogen cyanide (hydrogen cyanide) as raw materials, the "C4 direct oxidation method" which is carried out using isobutylene or tert-butyl alcohol as raw materials, and the "alpha method" which is carried out using ethylene as raw materials.

[0019] As a raw material for the methyl methacrylate composition of the present embodiment, a product (sometimes referred to as a methyl methacrylate product) that may contain components other than methyl methacrylate, such as methyl isobutyrate, methyl isobutyrate, and / or methyl acrylate, in amounts that are unavoidably mixed in depending on the production method described above can be used.

[0020] Methyl methacrylate (or a methyl methacrylate product) that can be used as a raw material for the methyl methacrylate composition of the present embodiment and is produced by the above-mentioned production method may be purified by any suitable purification method known in the art.

[0021] The content of methyl isobutyrate that may be contained in the methyl methacrylate product, which is a raw material for the methyl methacrylate composition of this embodiment, is preferably more than 0 ppm by mass and not more than 300 ppm by mass, and / or the content of methyl acrylate that may be contained in the methyl methacrylate product is preferably 0 ppm by mass to 20,000 ppm by mass, when the total amount of the methyl methacrylate product is 100 parts by mass.

[0022] In the methyl methacrylate composition of the present embodiment, the content of methyl methacrylate is usually 85% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, even more preferably 98% by mass or more, and particularly preferably 99% by mass or more, when the total amount of the methyl methacrylate composition is 100% by mass, from the viewpoint of improving heat resistance.

[0023] In the present embodiment, the methyl methacrylate composition contains, as methyl methacrylate, recycled methyl methacrylate and non-regenerated methyl methacrylate. Hereinafter, the recycled methyl methacrylate and the non-regenerated methyl methacrylate will be described.

[0024] (1-1) Regenerated methyl methacrylate In this embodiment, "recycled methyl methacrylate" refers to methyl methacrylate derived from chemical recycling, which is obtained by depolymerizing (chemical recycling) molded bodies obtained by molding polymethyl methacrylate, i.e., methyl methacrylate, or further methyl methacrylate compositions containing methyl methacrylate as the main component, into various shapes by any suitable injection molding process known in the art. Specifically, "recycled methyl methacrylate" refers to, for example, polymethyl methacrylate polymerized from methyl methacrylate, more specifically, methyl methacrylate (recycled MMA) recovered by thermally decomposing (depolymerizing) a molded body mainly composed of polymethyl methacrylate that has been distributed to the market and used for various purposes and then recovered, or that has not yet been distributed to the market (e.g., surplus production), by heat treatment under any suitable conditions known in the art.

[0025] In this embodiment, the embodiment of chemical recycling for obtaining regenerated methyl methacrylate is not particularly limited. In this embodiment, chemical recycling can be carried out using any suitable conventionally known device under any suitable conventionally known conditions (thermal decomposition conditions). For example, the thermal decomposition temperature can be, for example, about 300 to 600 ° C, preferably about 350 to 500 ° C, more preferably about 400 to 500 ° C. When an extruder is used for thermal decomposition, if it is within the above range, regenerated methyl methacrylate that can be used in the composition of this embodiment can be obtained.

[0026] Depolymerization of polymethyl methacrylate (e.g., chemical recycling) usually results in a regenerated methyl methacrylate product containing regenerated methyl methacrylate. Examples of components other than regenerated methyl methacrylate contained in the regenerated methyl methacrylate product include methyl isobutyrate, methyl propionate, methyl acrylate, and other components derived from the depolymerization of polymethyl methacrylate, i.e., chemical recycling.

[0027] Chemical recycling allows the recovery of regenerated methyl methacrylate in high yield. In addition, by carrying out any suitable conventional purification step after depolymerization, the content (concentration) of low-boiling compounds (impurities) that are by-products such as methyl propionate, methyl isobutyrate, and methyl acrylate, which may be inevitably contained in the regenerated methyl methacrylate product containing methyl methacrylate as a main component, can be effectively reduced. The purification step may be carried out at a temperature that can reduce impurities, for example, in the range of 30 to 130°C, preferably 30 to 120°C. The purification step may be carried out under reduced pressure conditions as long as the regenerated methyl methacrylate can be recovered. When the purification step is carried out under a reduced pressure environment, it may be carried out at a temperature lower than 100°C, preferably in the range of 30 to 80°C, more preferably 50 to 80°C.

[0028] The regenerated methyl methacrylate product contains regenerated methyl methacrylate in an amount of usually 80% by mass or more, preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 92% by mass or more, and even more preferably 95% by mass or more. The upper limit of the content of regenerated methyl methacrylate is not particularly limited, and may be 100% by mass, 99% by mass or less, or 98% by mass or less. That is, the regenerated methyl methacrylate product contains regenerated methyl methacrylate in an amount of usually 80 to 100% by mass, and preferably 85 to 99% by mass.

[0029] Although recycled methyl methacrylate is basically methyl methacrylate with the same chemical structure as unregenerated methyl methacrylate, it has been found that adding recycled methyl methacrylate to unregenerated methyl methacrylate changes the physical properties of the composition and polymer. The reason for this is unclear, but it is speculated that due to the thermal decomposition (depolymerization) during the manufacturing process of recycled methyl methacrylate, the reactivity of unregenerated methyl methacrylate has changed for some reason, and it is a separate component that behaves differently from unregenerated methyl methacrylate. Possible reasons for this include at least some disappearance of reaction sites, changes in purity, and changes in interactions between monomers.

[0030] (1-2) Unregenerated methyl methacrylate In this embodiment, "unregenerated methyl methacrylate" refers to methyl methacrylate that does not fall under the category of "regenerated methyl methacrylate" already explained, and specifically refers to, for example, methyl methacrylate that has been produced by a specified production method, and then has not been polymerized and applied to various uses (virgin methyl methacrylate).

[0031] As already explained, the non-regenerated methyl methacrylate may unavoidably contain other components (impurities) such as methyl isobutyrate, methyl propionate, and methyl acrylate. Such a composition containing non-regenerated methyl methacrylate and other components may be called a non-regenerated methyl methacrylate product. The non-regenerated methyl methacrylate content of the non-regenerated methyl methacrylate product is usually 95% by mass or more, preferably 96% by mass or more, more preferably 97% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. The upper limit is not particularly limited and may be 100% by mass. That is, the non-regenerated methyl methacrylate content of the non-regenerated methyl methacrylate product is usually in the range of 95 to 100% by mass, and preferably in the range of 96 to 99% by mass.

[0032] In this embodiment, the method for producing the non-regenerated methyl methacrylate that can be used as the raw material of the methyl methacrylate composition is not particularly limited. Examples of the method for producing the non-regenerated methyl methacrylate that is the raw material of the methyl methacrylate composition of this embodiment include the "ACH (acetone cyanohydrin) method", "C4 direct acid method", and "alpha method" already described. In this embodiment, the non-regenerated methyl methacrylate may be produced by any of these methods.

[0033] In the methyl methacrylate composition of the present embodiment, the non-regenerated methyl methacrylate includes methyl methacrylate produced using plant-derived raw materials (sometimes referred to as bio-MMA). Specifically, bio-MMA may include methyl methacrylate produced by the above-described production methods such as the ACH (acetone cyanohydrin) method, the C4 direct oxidation method, and the alpha method using butanol, isobutylene, ethanol, ethylene, methanol, propylene acetone, etc., which are produced by microbial decomposition, fermentation, etc., using plant-derived raw materials such as starch and polysaccharides derived from plants such as corn, wheat, and potato.

[0034] In this embodiment, as long as raw materials, reagents, and the like produced by the action of microbial decomposition, fermentation, and the like are used, for example, methyl methacrylate produced by the above-mentioned production method can be included in "bio-MMA".

[0035] Bio-MMA contains carbon-12( 12 Carbon-14 (C), a radioactive isotope 14 C), while methyl methacrylate derived from mineral resources such as petroleum contains carbon-14 ( 14 Therefore, whether non-regenerated methyl methacrylate, furthermore, recycled methyl methacrylate, methyl methacrylate composition, and furthermore, molded articles molded from said methyl methacrylate composition contain bio-MMA or are derived from bio-MMA can be determined by the carbon-14 ( 14 It can be confirmed by detecting whether or not the compound (C) is contained by any suitable method known in the art.

[0036] The non-regenerated methyl methacrylate produced by the above-mentioned manufacturing method can be subjected to any suitable purification process known in the art to effectively reduce the content (concentration) of impurities that may be inevitably contained in the non-regenerated methyl methacrylate product containing methyl methacrylate as the main component.

[0037] In the methyl methacrylate composition of this embodiment, from the viewpoint of achieving a good balance between the 5% weight loss temperature and the glass transition temperature, and from the viewpoint of suppressing the occurrence of yellowing, the content of recycled methyl methacrylate and the content of non-regenerated methyl methacrylate are preferably 0.5 to 99.5 mass% when the total amount of the methyl methacrylate composition is 100 mass%, with the content of recycled methyl methacrylate being 0.5 to 99.5 mass% and the content of non-regenerated methyl methacrylate being 0.5 to 99.5 mass%, respectively. The content of these is preferably 3 to 90% by mass for the recycled methyl methacrylate and 10 to 97% by mass for the non-regenerated methyl methacrylate, more preferably 5 to 80% by mass for the recycled methyl methacrylate and 20 to 95% by mass for the non-regenerated methyl methacrylate, even more preferably 10 to 70% by mass for the recycled methyl methacrylate and 30 to 90% by mass for the non-regenerated methyl methacrylate, and even more preferably 20 to 60% by mass for the recycled methyl methacrylate and 40 to 80% by mass for the non-regenerated methyl methacrylate. When the content of recycled methyl methacrylate and non-regenerated methyl methacrylate is within the above range, the heat resistance of the polymer of the methyl methacrylate composition and further the molded product thereof can be improved, and the yellowing of the methyl methacrylate composition can be suppressed, and the storage stability can be improved. In another embodiment, it is more preferable that the content of recycled methyl methacrylate is 3 to 40% by mass and the content of unregenerated methyl methacrylate is 60 to 97% by mass, and it is even more preferable that the content of recycled methyl methacrylate is 3 to 20% by mass and the content of unregenerated methyl methacrylate is 80 to 97% by mass.

[0038] (2) Alkyl acrylate The methyl methacrylate composition of the present embodiment may further contain an alkyl acrylate. The alkyl acrylate that may be contained in the methyl methacrylate composition of the present embodiment may be methyl acrylate that is generated and inevitably mixed in by the already described method for producing methyl methacrylate, or methyl acrylate that is inevitably generated by depolymerization in the above-mentioned chemical recycling. In addition, the alkyl acrylate that may be contained in the methyl methacrylate composition of the present embodiment may be an alkyl acrylate that is intentionally mixed into the above-mentioned methyl methacrylate product (regenerated methyl methacrylate product, non-regenerated methyl methacrylate product). Examples of such alkyl acrylate include methyl acrylate, ethyl acrylate, propyl acrylate, and butyl acrylate.

[0039] The content of alkyl acrylate that can be contained in the methyl methacrylate composition of the present embodiment is preferably 0% by mass to 10% by mass, and more preferably 0% by mass to 5% by mass.

[0040] The concentration of methyl acrylate that can be contained in the methyl methacrylate composition of the present embodiment is preferably 5 ppm by mass to 50,000 ppm by mass, and more preferably 5 ppm by mass to 30,000 ppm by mass.

[0041] (3) Other low content ingredients In addition to the "impurities" already described, the methyl methacrylate composition of this embodiment may contain other low content components, particularly those resulting from the recovery process of regenerated methyl methacrylate. Examples of other low content components include methanol, 2,4-dimethyl-4-methyl pentenoate, 1-butanol, and butyl acrylate, as well as 2-methyl-3-butenoate, methyl tiglate, 3-methyl-3-butenoate, 3-methyl-2-butenoate, dimethyl icosanoate, 2-methyl-5-methylenehexanedioate, toluene, and styrene.

[0042] When the methyl methacrylate composition of the present embodiment further contains one or more selected from the group consisting of methanol, methyl 2,4-dimethyl-4-pentenoate, 1-butanol, and butyl acrylate among the other low content components described above, the concentrations of each of the methanol, methyl 2,4-dimethyl-4-pentenoate, 1-butanol, and butyl acrylate are preferably 10 ppm by mass to 5000 ppm by mass, and more preferably 10 ppm by mass to 4000 ppm by mass, when the total amount of the methyl methacrylate composition is 100 parts by mass.

[0043] When the methyl methacrylate composition of the present embodiment further contains one or more selected from the group consisting of methyl 2-methyl-3-butenoate, methyl tiglate, methyl 3-methyl-3-butenoate, methyl 3-methyl-2-butenoate, dimethyl itanoate, dimethyl 2-methyl-5-methylenehexanedioate, toluene, and styrene among the other low content components described above, the concentration of each of methyl 2-methyl-3-butenoate, methyl tiglate, methyl 3-methyl-3-butenoate, methyl 3-methyl-2-butenoate, dimethyl itanoate, dimethyl 2-methyl-5-methylenehexanedioate, toluene, and styrene is preferably 10 ppm by mass to 1000 ppm by mass, and more preferably 10 ppm by mass to 800 ppm by mass, when the total amount of the methyl methacrylate composition is 100 parts by mass.

[0044] According to the methyl methacrylate composition of the present embodiment, even if the other low content components are further contained at the above concentrations, the 5% weight loss temperature and glass transition temperature of the methyl methacrylate-based polymer obtained by polymerizing the methyl methacrylate composition, and further the molded product thereof, can be improved, and the 5% weight loss temperature and the glass transition temperature can be made compatible to achieve a good balance. Specifically, for example, the 5% weight loss temperature and the glass transition temperature of the methyl methacrylate composition of the present embodiment can show values ​​much higher than those predicted from the 5% weight loss temperature and the glass transition temperature predicted from non-regenerated methyl methacrylate or regenerated methyl methacrylate alone. For example, when the relationship between the measured values ​​of the 5% weight loss temperature of the above-mentioned single molded product and the composition of the present embodiment and the content of the regenerated methyl methacrylate is plotted, and the measured values ​​of the single molded product are connected with a straight line, the methyl methacrylate composition of the present embodiment can show a measured value higher than the straight line. The same is true for the glass transition temperature.

[0045] In addition, the methyl methacrylate composition of this embodiment can exhibit good storage stability and inhibit deterioration such as yellowing during storage. Since unregenerated methyl methacrylate and regenerated methyl methacrylate are subject to deterioration during storage, this effect obtained by mixing the two in a predetermined ratio can be said to be an unexpected and surprising effect. Although the reason is unclear, it is believed that the addition of regenerated methyl methacrylate to unregenerated methyl methacrylate causes some kind of action (e.g., interaction between monomers) that is different from the case of unregenerated methyl methacrylate alone or the case of regenerated methyl methacrylate alone.

[0046] (4) Other ingredients In addition to the above components (1) to (3), the methyl methacrylate composition of the present embodiment may further contain other components such as a release agent, a polymerization regulator, a polymerization initiator, an ultraviolet absorber, and a colorant that can be added to produce a molded article having predetermined properties, provided that the object of the present invention is not impaired. Hereinafter, other components that can be contained in the methyl methacrylate composition of the present embodiment will be described.

[0047] (i) Release agent The methyl methacrylate composition of the present embodiment may contain a release agent for improving the releasability of a molded article, particularly, when producing a methyl methacrylate-based polymer obtained by polymerizing the methyl methacrylate composition and a molded article thereof.

[0048] Examples of release agents that may be contained in the methyl methacrylate composition of the present embodiment include higher fatty acid esters, higher aliphatic alcohols, higher fatty acids, higher fatty acid amides, higher fatty acid metal salts, and fatty acid derivatives.

[0049] Specific examples of the release agent that may be contained in the methyl methacrylate composition of this embodiment include sodium di-(2-ethylhexyl)sulfosuccinate, stearyl alcohol, methyl stearate, and stearic acid amide. In the methyl methacrylate composition of this embodiment, the above release agents may be used alone or in combination of two or more.

[0050] The content of the release agent in the methyl methacrylate composition of the present embodiment can be, for example, 0.01 part by mass to 1.0 part by mass when the total amount of the methyl methacrylate composition is taken as 100 parts by mass.

[0051] (ii) Polymerization regulator The methyl methacrylate composition of the present embodiment may contain a polymerization regulator capable of regulating the polymerization rate in the polymerization reaction of methyl methacrylate.

[0052] As the polymerization regulator that may be contained in the methyl methacrylate composition of the present embodiment, any suitable polymerization regulator known in the art can be used. As such a polymerization regulator, for example, a compound that can adjust the polymerization rate in the direction of decreasing the polymerization rate can be used.

[0053] Specific examples of suitable polymerization regulators include mercaptan compounds such as n-butyl mercaptan and n-octyl mercaptan, terpenoid compounds such as limonene, myrcene, α-terpinene, β-terpinene, γ-terpinene, terpinolene, β-pinene, and α-pinene, and α-methylstyrene dimer. In the present embodiment, it is preferable to use terpinolene, which is a terpenoid compound, as the polymerization regulator.

[0054] In the methyl methacrylate composition of the present embodiment, the above polymerization regulators may be used alone or in combination of two or more kinds.

[0055] The content of the polymerization regulator in the methyl methacrylate composition of the present embodiment can be, for example, 0.001 to 0.5 parts by mass when the total amount of the methyl methacrylate composition is taken as 100 parts by mass.

[0056] (iii) Polymerization initiator Examples of polymerization initiators that may be contained in the methyl methacrylate composition of the present embodiment include radical polymerization initiators, diacyl peroxide initiators, dialkyl peroxide initiators, peroxyester initiators, percarbonate initiators, and peroxyketal initiators.

[0057] Specific examples of radical polymerization initiators include azo compounds such as 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4,4-trimethylpentene), 2,2'-azobis(2-methylpropane), 2-cyano-2-propylazoformamide, 2,2'-azobis(2-hydroxymethylpropionate), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], and dimethyl 2,2'-azobis(2-methylpropionate).

[0058] Specific examples of diacyl and dialkyl peroxide initiators include dicumyl peroxide, tert-butylcumyl peroxide, di-tert-butyl peroxide, benzoyl peroxide, and lauroyl peroxide.

[0059] Specific examples of peroxyester initiators include tert-butylperoxy-3,3,5-trimethylhexanoate, tert-butylperoxylaurate, tert-butylperoxyisobutyrate, tert-butylperoxyacetate, di-tert-butylperoxyhexahydroterephthalate, di-tert-butylperoxyazelate, tert-butylperoxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, and tert-amylperoxy-2-ethylhexanoate.

[0060] Specific examples of percarbonate initiators include tert-butyl peroxy allyl carbonate, and tert-butyl peroxy isopropyl carbonate.

[0061] Specific examples of peroxyketal initiators include 1,1-di-tert-butylperoxycyclohexane, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, and 1,1-di-tert-hexylperoxy-3,3,5-trimethylcyclohexane.

[0062] In the methyl methacrylate composition of the present embodiment, the above polymerization initiators may be used alone or in combination of two or more kinds.

[0063] The content of the polymerization initiator in the methyl methacrylate composition of the present embodiment can be, for example, 0.01 parts by mass to 5 parts by mass when the total amount of the methyl methacrylate composition is taken as 100 parts by mass.

[0064] (iv) Ultraviolet absorber The methyl methacrylate composition of the present embodiment may contain an ultraviolet absorber in order to further improve the weather resistance of the produced polymethyl methacrylate and its molded article.

[0065] Examples of suitable UV absorbers that may be included in the methyl methacrylate composition of the present embodiment include benzophenone UV absorbers, cyanoacrylate UV absorbers, benzotriazole UV absorbers, malonic acid ester UV absorbers, and oxalanilide UV absorbers.

[0066] Specific examples of ultraviolet absorbers include 2(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-n-octylbenzophenone, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-pentylphenyl)benzotriazole, and 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate.

[0067] In the methyl methacrylate composition of the present embodiment, the above ultraviolet absorbents may be used alone or in combination of two or more kinds.

[0068] The content of the ultraviolet absorber in the methyl methacrylate composition of the present embodiment can be, for example, 0.001 part by mass to 1 part by mass when the total amount of the methyl methacrylate composition is taken as 100 parts by mass.

[0069] (v) Coloring agent The methyl methacrylate composition of the present embodiment may contain a colorant for imparting any suitable color to the produced methyl methacrylate polymer and its molded article.

[0070] Examples of suitable colorants that may be included in the methyl methacrylate compositions of the present embodiments include perylene dyes, perinone dyes, pyrazolone dyes, methine dyes, coumarin dyes, quinophthalone dyes, quinoline dyes, anthraquinone dyes (e.g., Sumiplast Violet B), anthraquinone dyes, asdolapyridone dyes, thioindigo dyes, coumarin dyes, isoindolinone pigments, sichetopyrrolopyrrole pigments, condensed azo pigments, benzimidazolone pigments, dioxazine pigments, copper phthalocyanine pigments, and quinacridone pigments.

[0071] The above colorants may be used alone or in combination of two or more.

[0072] The content of the colorant in the methyl methacrylate composition of the present embodiment is, for example, 1.0 × 10 -8 It can be between 0.5 parts by mass and 0.5 parts by mass.

[0073] 2. Method for producing methyl methacrylate composition The methyl methacrylate composition of the present embodiment can be produced by mixing the components already described using any suitable conventional method under any suitable conditions.

[0074] Specifically, the methyl methacrylate composition of the present embodiment can be produced by preparing the components already described in preset amounts and mixing them in, for example, a mixing tank whose temperature can be controlled to a constant temperature by a heat medium jacket or the like having any suitable conventional configuration.

[0075] The methyl methacrylate composition of the present embodiment may be a methyl methacrylate composition (mixture) produced by the above-mentioned production method, which is purified by any suitable conventionally known purification method.

[0076] As described above, according to the method for producing a methyl methacrylate composition of the present embodiment, a methyl methacrylate polymer having excellent properties as already described, and further a methyl methacrylate composition from which a molded article thereof can be produced, can be produced simply and at low cost.

[0077] 3. Method for producing methyl methacrylate polymer and molded product In this embodiment, the method for producing a methyl methacrylate polymer includes a step of polymerizing a methyl methacrylate composition. The method for converting the methyl methacrylate composition of this embodiment into a methyl methacrylate polymer is not particularly limited. Specifically, the methyl methacrylate composition can be polymerized into a methyl methacrylate polymer by any suitable method selected in consideration of the components contained in the methyl methacrylate composition of this embodiment and their contents.

[0078] In the present embodiment, examples of the method for polymerizing the methyl methacrylate composition include bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization.

[0079] Specifically, the methyl methacrylate composition of the present embodiment can be polymerized by, for example, bulk polymerization to obtain a molded article of a methyl methacrylate-based polymer, i.e., a molded article containing polymethyl methacrylate. In addition, in cell cast polymerization, the methyl methacrylate composition can be subjected to any suitable heat treatment under predetermined heating conditions to allow the polymerization reaction to proceed, thereby obtaining a molded article of a methyl methacrylate-based polymer in which the methyl methacrylate contained in the methyl methacrylate composition is polymerized and hardened.

[0080] In the method of polymerizing the methyl methacrylate composition (methyl methacrylate) of the present embodiment to form a methyl methacrylate-based polymer, and further in the method of producing a molded article obtained by polymerizing the methyl methacrylate composition, the heating temperature and heating time among the heating conditions can be appropriately set in consideration of, for example, the type and content of the selected polymerization regulator, polymerization initiator, and / or other components, the content of methyl methacrylate, and the concentrations of alkyl acrylate and other components that may be contained.

[0081] In the present embodiment, in the cell cast polymerization, when producing a methyl methacrylate polymer, that is, a molded article, the heating temperature can be, for example, 50° C. to 130° C., and the heating time can be, for example, 1 hour to 20 hours.

[0082] The heat treatment in the method for producing the polymer and the molded article of this embodiment may be a heat treatment including a plurality of steps with different heating temperatures and / or heating times.

[0083] The polymer and its molded product of this embodiment can be produced, for example, by carrying out a heat treatment under heating conditions including the following steps 1 to 7. Step 1: Raise the temperature from room temperature to 68°C over 20 minutes. Step 2: Hold at 68°C for 90 minutes. Step 3: Reduce the temperature from 68°C to 64°C over 20 minutes. Step 4: Hold at 64°C for 90 minutes. Step 5: Increase temperature from 64°C to 123°C over 10 minutes. Step 6: Hold at 123°C for 120 minutes. Step 7: The temperature is lowered from 123°C to room temperature over 90 minutes.

[0084] In the method for producing a methyl methacrylate polymer and a molded article according to this embodiment, by carrying out the above steps 1 to 7 in this order, heat generation during the polymerization reaction can be suppressed and the polymerization reaction can be stably completed.

[0085] When the methyl methacrylate composition of the present embodiment is subjected to a heat treatment, for example, a cell casting method (cell casting polymerization) using a cell capable of defining an enclosed space of a predetermined shape inside can be applied to form a molded body of a predetermined shape. Hereinafter, the manufacturing method of the molded body by the cell casting method will be specifically described.

[0086] In producing a molded body of a methyl methacrylate polymer by the cell casting method, a cell is first prepared. Here, an example of forming a molded body in the form of a plate (sometimes called a cast plate) will be described.

[0087] Such a cell can be composed of at least two flat plate-like members and a sealing material (gasket) that is arranged so as to be sandwiched between the two flat plate-like members and can seal the gap between the two opposing flat plate-like members as an enclosed space.

[0088] The flat plate member may be a sheet or a belt. The flat plate member may be made of a material that is not dissolved by the methyl methacrylate composition of the present embodiment, does not inhibit the polymerization reaction, and has sufficient heat resistance to the heating temperature in the heat treatment. Examples of suitable materials for the flat plate member include glass and metal.

[0089] As the sealing material, any suitable sealing material known in the art can be used. The sealing material may be made of a material that is not dissolved by the methyl methacrylate composition of the present embodiment, does not inhibit the polymerization reaction, and has sufficient heat resistance to the heating temperature in the heat treatment. A specific example of a suitable sealing material is a polyvinyl chloride resin gasket.

[0090] Next, the methyl methacrylate composition of the present embodiment is injected into the gap (void) defined by the cells prepared as described above by any suitable method known in the art.

[0091] Next, the cell is subjected to a heat treatment under the heating conditions already described. The method of heat treatment of the cell into which the methyl methacrylate composition of the present embodiment has been injected is not particularly limited. The method of heat treatment of the cell can be, for example, a method of directly heat treating the cell from the outside using a hot air circulating oven, an infrared heater, or the like, as in the conventionally known cell casting method, or a method of further providing any suitable conventionally known jacket on the outside of the cell and introducing a heat medium such as hot air, hot water, or water vapor into the jacket.

[0092] 4. Measurement of 5% weight loss temperature (heat weight loss rate) of molded body In this embodiment, the 5% weight loss temperature of the molded product of the methyl methacrylate polymer can be measured using a conventionally known thermogravimetry / differential thermal analyzer (for example, "TG / DTA7200" manufactured by Hitachi High-Tech Science Corporation).

[0093] Specifically, a test piece is prepared by crushing a molded body such as a cast plate so that the diameter or length of each side is 0.5 mm or less, and a heat treatment is carried out using a thermogravimetry / differential thermal analyzer to heat the test piece to a predetermined temperature under an inert gas flow at a predetermined gas flow rate and heating rate. The weight of the heat-treated test piece is then measured, and the 5% weight loss temperature can be calculated based on the measured weight and the initial weight.

[0094] In this embodiment, the molded body, ie, the 5% weight loss temperature of the methyl methacrylate polymer is preferably 260°C to 360°C, and more preferably 290°C to 330°C.

[0095] When the 5% weight loss temperature of the methyl methacrylate polymer is less than 260° C., the molded article obtained using the methyl methacrylate polymer may have poor appearance. On the other hand, when the 5% weight loss temperature of the methyl methacrylate polymer is more than 330° C., a large amount of energy may be required for thermal decomposition of the molded article obtained using the methyl methacrylate polymer. The 5% weight loss temperature of a molded article obtained using the homopolymer (regenerated methyl methacrylate polymer) of the recycled methyl methacrylate product as the raw material of the composition is usually 300°C or higher, preferably 310°C or higher, more preferably 320°C or higher. The upper limit is usually 400°C or lower, preferably 380°C or lower, more preferably 350°C or lower. The 5% weight loss temperature of a molded article obtained using the homopolymer (regenerated methyl methacrylate polymer) of the non-regenerated methyl methacrylate product as the raw material is usually 200°C or higher, preferably 250°C or higher. The upper limit is usually less than 300°C, preferably 290°C or lower. The 5% weight loss temperature of a molded article of the recycled methyl methacrylate polymer is preferably higher than that of a molded article of the non-regenerated methyl methacrylate polymer, and the difference is usually 10°C or higher, preferably 20°C or higher, more preferably 30°C or higher. The upper limit is usually 50°C or lower, preferably 40°C or lower.

[0096] 5. Measurement of Glass Transition Temperature In this embodiment, the glass transition temperature of the molded article of the methyl methacrylate polymer is the glass transition temperature (Tmg) (° C.) measured in accordance with JIS-K7121.

[0097] The glass transition temperature can be measured using any suitable conventional measuring device (for example, a differential scanning calorimeter "DSC7020" manufactured by Hitachi High-Tech Science Corporation).

[0098] Specifically, a test specimen is prepared by pulverizing a molded body such as a cast plate so that the diameter or the length of each side is 0.5 mm or less, and the test specimen is completely melted in an inert gas atmosphere, after which the measurement can be performed based on a DSC curve obtained according to a specified temperature profile.

[0099] In this embodiment, the molded product, ie, the glass transition temperature of the methyl methacrylate polymer is usually 100°C to 130°C, or 105°C to 125°C, preferably 110°C to 120°C, and more preferably 110°C to 115°C. The glass transition temperature of the polymer (molded product) of recycled methyl methacrylate is usually 90°C or higher, preferably 95°C or higher, more preferably 100°C or higher, and even more preferably 105°C or higher. The upper limit is usually 130°C or lower, preferably 120°C or lower, and more preferably 110°C or lower. The glass transition temperature of the polymer (molded product) of non-regenerated methyl methacrylate is usually 105°C or higher, preferably 110°C or higher. The upper limit is usually 150°C or lower, preferably 140°C or lower. It is preferable that the glass transition temperature of the recycled methyl methacrylate polymer (molded product) is lower than that of the non-regenerated methyl methacrylate polymer (molded product), and the difference is usually 2°C or higher, preferably 2.5°C or higher, and more preferably 3°C or higher. The upper limit is usually 10°C or lower, preferably 9°C or lower, and more preferably 8°C or lower.

[0100] 6. Yellowing measurement The yellowing index (YI value) of the molded product of the methyl methacrylate polymer in this embodiment can be calculated according to the method described in JIS K7373. In the examples described later, the composition to be measured is placed in a quartz glass cell with a length of 10 mm, width of 10 mm, and height of 45 mm, and the yellowing index (YI value) when the optical path length is set to 10 mm is calculated according to the method described in JIS K7373. A commercially available spectrophotometer can be used for the measurement, and the measurement may be performed, for example, under the following conditions. The smaller the calculated YI value, the more suppressed the yellowing. For example, the YI value measured under the measurement conditions of the examples is preferably 0.1 or less. (YI measurement conditions) Light source: C light source Field of view: 2 degrees Calculation formula: YI=(1.2769×X-1.0592×Z) / Y×100

[0101] 7. Uses of polymers and molded articles thereof The polymer of the methyl methacrylate composition of the present embodiment and its molded article are excellent in light transmittance, heat resistance, and weather resistance, and therefore can be suitably applied to various applications that may be exposed to the external environment and further to heat and light sources, such as lighting fixtures, automobile parts, signs, and building materials. EXAMPLES

[0102] Examples according to the embodiments of the present invention will be described below. The present invention is not limited to the examples described below.

[0103] <Preparation Example 1> Preparation of regenerated methyl methacrylate product (recovered MMA) Polymethyl methacrylate resin (SUMIPEX MH, manufactured by Sumitomo Chemical Co., Ltd.) was pyrolyzed (depolymerized) under the following pyrolysis conditions using a twin-screw extruder (TEX-44, manufactured by The Japan Steel Works, Ltd.).

[0104] The methyl methacrylate product containing pyrolyzed methyl methacrylate was condensed using a heat exchanger to obtain a crude regenerated methyl methacrylate product.

[0105] Next, the crude regenerated methyl methacrylate product was purified using a rotary evaporator (R-300, manufactured by BUCHI) under the following purification conditions to obtain a regenerated methyl methacrylate product.

[0106] The content of recycled methyl methacrylate in the obtained recycled methyl methacrylate product was 97.3 mass %.

[0107] (Pyrolysis conditions) Cylinder temperature: 450℃ Rotational speed: 500 rpm Screw L / D: 60 ·Resin supply amount: 40kg / hr

[0108] (Purification conditions) Bath temperature: 50℃ ·Circulating water temperature: 5℃ Pressure: 90mbar or more

[0109] <Preparation Example 2> Preparation of non-regenerated methyl methacrylate In the reactor, methacrylic acid and methanol were reacted to form methyl methacrylate.

[0110] From the obtained methyl methacrylate product containing methyl methacrylate, unreacted methanol was removed using an extraction column, and then the product was purified according to a conventional method using multiple distillation columns to obtain a non-regenerated methyl methacrylate product. The content of non-regenerated methyl methacrylate contained in the non-regenerated methyl methacrylate product was 99.99% by mass.

[0111] <Example 1> Preparation of Composition 1 5 parts by mass of the regenerated methyl methacrylate product obtained in Preparation Example 1 above and 95 parts by mass of the non-regenerated methyl methacrylate product obtained in Preparation Example 2 above were mixed to obtain a methyl methacrylate composition (hereinafter simply referred to as composition) 1. The obtained composition 1 was liquid.

[0112] Preparation of Composition 1' Composition 1 (99.83 parts by mass), a release agent, di-(2-ethylhexyl) sodium sulfosuccinate (0.05 parts by mass), a polymerization regulator, terpinolene (0.01 parts by mass), a polymerization initiator, 2,2'-azobisisobutyronitrile (0.08 parts by mass), and an ultraviolet absorber, 2(2'-hydroxy-5'-methylphenyl)benzotriazole (0.01 parts by mass), were mixed to obtain a composition 1' for forming a molded body (cast plate). The obtained composition 1' was liquid.

[0113] -Preparation of cast plate 1 A cell was prepared in which a 3.8 mm thick polyvinyl chloride resin gasket was sandwiched between two opposing glass plates, thereby defining a gap sealed by the polyvinyl chloride resin gasket and the two glass plates.

[0114] Composition 1' was poured into the gap in the cell. The cell with composition 1' poured therein was placed in an oven, and composition 1' was polymerized by carrying out a heat treatment under heating conditions including the following steps 1 to 7 in this order, to produce cast plate 1, which was a molded product of a methyl methacrylate polymer, having a thickness of 3 mm and a size of 250 mm square.

[0115] (Heating conditions) Step 1: Raise the temperature from room temperature to 68°C over 20 minutes. Step 2: Hold at 68°C for 90 minutes. Step 3: Reduce the temperature from 68°C to 64°C over 20 minutes. Step 4: Hold at 64°C for 90 minutes. Step 5: Increase temperature from 64°C to 123°C over 10 minutes. Step 6: Hold at 123°C for 120 minutes. Step 7: The temperature is lowered from 123°C to room temperature over 90 minutes.

[0116] Measurement of 5% weight loss temperature of cast plate 1 The cast plate 1 was crushed to a diameter or length of each side of 0.5 mm or less, and 9.3 mg of the crushed material was placed on an aluminum pan (Hitachi High-Tech Science Corp., "P / N SSC000E030 Open Sample Pan", diameter 5 mm). The weight change was measured using a thermogravimetric / differential thermal analyzer (Hitachi High-Tech Science Corp., "TG / DTA7200") while heating from 45°C to 520°C under conditions of a nitrogen gas flow rate of 200 mL / min and a heating rate of 10°C / min. The weight of the crushed material decreased as the temperature increased. The weight of the crushed material at the initial temperature of 45°C was taken as 100% by weight, and the temperature at which the weight of the crushed material decreased to 95% by weight (5% weight loss temperature) was calculated. The results are shown in Table 1.

[0117] Measurement of glass transition temperature (Tmg) of cast plate 1 A cast plate 1, which is a molded body of a methyl methacrylate polymer, was crushed to a diameter or each side length of 0.5 mm or less, and the crushed material obtained was used as a test piece to measure the glass transition temperature (°C) in accordance with JIS-K7121.

[0118] Specifically, a differential scanning calorimeter ("DSC7020" manufactured by Hitachi High-Tech Science Corporation) was used as the measuring device for measuring the glass transition temperature, and the nitrogen gas flow rate was set to 50 mL / min. The temperature was raised from room temperature (23°C) to 150°C at 20°C / min (first heating), and the test piece was kept at 150°C for 5 minutes to completely melt, and then the temperature was lowered from 150°C to -35°C at 10°C / min, and kept at -35°C for 1 minute, and further raised again to 210°C at 10°C / min (second heating).

[0119] Of the DSC curves obtained from the above temperature profile, the intersection point (midpoint glass transition temperature) between the stepwise change partial curve during the second heating and a straight line equidistant in the vertical direction from the two baseline extensions was taken as the glass transition temperature (°C). Measurements were performed at three points per test piece, and the average value was calculated and taken as the glass transition temperature. The results are shown in Table 1.

[0120] <Example 2> Preparation of Composition 2 Composition 2 was obtained by mixing 10 parts by mass of the regenerated methyl methacrylate product obtained in Preparation Example 1 and 90 parts by mass of the non-regenerated methyl methacrylate product obtained in Preparation Example 2. The obtained composition 2 was liquid.

[0121] Composition 2' was prepared in the same manner as in Example 1, except that composition 2 was used, and then cast plate 2 was produced, and the 5% weight loss temperature and glass transition temperature were measured. The results are shown in Table 1.

[0122] <Example 3> Preparation of composition 3 30 parts by mass of the regenerated methyl methacrylate product obtained in Preparation Example 1 and 70 parts by mass of the non-regenerated methyl methacrylate product obtained in Preparation Example 2 were mixed to obtain Composition 3. The obtained Composition 3 was liquid.

[0123] Composition 3' was prepared in the same manner as in Example 1, except that composition 3 was used, and then a cast plate 3 was produced, and the 5% weight loss temperature and the glass transition temperature were measured. The results are shown in Table 1.

[0124] <Example 4> Preparation of Composition 4 50 parts by mass of the regenerated methyl methacrylate product obtained in Preparation Example 1 and 50 parts by mass of the non-regenerated methyl methacrylate product obtained in Preparation Example 2 were mixed to obtain Composition 4. The obtained Composition 4 was liquid.

[0125] Composition 4' was prepared in the same manner as in Example 1, except that composition 4 was used, and then a cast plate 4 was produced, and the 5% weight loss temperature and the glass transition temperature were measured. The results are shown in Table 1.

[0126] <Example 5> Preparation of Composition 5 80 parts by mass of the regenerated methyl methacrylate product obtained in Preparation Example 1 above and 20 parts by mass of the non-regenerated methyl methacrylate product obtained in Preparation Example 2 above were mixed to obtain Composition 5. The obtained Composition 5 was in a liquid state.

[0127] Composition 5' was prepared in the same manner as in Example 1, except that composition 5 was used, and then a cast plate 5 was produced, and the 5% weight loss temperature and the glass transition temperature were measured. The results are shown in Table 1.

[0128] <Comparative Example 1> Preparation of composition C1 The liquid consisting only of the recycled methyl methacrylate product obtained in Preparation Example 1 above was designated as composition C1.

[0129] A composition C1' was prepared in the same manner as in Example 1, except that the composition C1 was used, and then a cast plate C1 was produced, and the 5% weight loss temperature and the glass transition temperature were measured. The results are shown in Table 1.

[0130] <Reference example 1> Preparation of composition R1 The liquid consisting only of the non-regenerated methyl methacrylate product obtained in Preparation Example 2 above was designated composition R1.

[0131] Except for using composition R1, composition R1' was prepared in the same manner as in Example 1, and then a cast plate R1 was produced, and the 5% weight loss temperature and the glass transition temperature were measured. The results are shown in Table 1.

[0132] [Table 1]

[0133] As is clear from Table 1 above, the molded articles of the methyl methacrylate polymers according to Examples 1 to 5, which satisfy the requirements of the present invention, were able to achieve excellent heat resistance.

[0134] Here, the relationship between the proportion of recycled methyl methacrylate and the 5% weight loss temperature or glass transition temperature will be described with reference to FIGS.

[0135] Fig. 1 is a graph showing the relationship between the proportion of recycled methyl methacrylate and the 5% weight loss temperature, and Fig. 2 is a graph showing the relationship between the proportion of recycled methyl methacrylate and the glass transition temperature. The straight lines (dashed lines) in each graph are lines connecting the values ​​when the proportion of recycled MMA is 0% (Reference Example 1) and 100% (Comparative Example 1).

[0136] As shown in FIG. 1, the molded bodies of the methyl methacrylate polymers according to Examples 1 to 5, which satisfy the requirements of the present invention, exhibited good 5% weight loss temperatures even when the methyl methacrylate compositions contained recycled methyl methacrylate (recycled methyl methacrylate products).

[0137] In addition, as shown in FIG. 2, the molded articles of the methyl methacrylate polymer according to Examples 1 to 5, which satisfy the requirements of the present invention, were able to realize excellent glass transition temperatures.

[0138] As is clear from Figs. 1 and 2, the molded bodies of the methyl methacrylate polymers of Examples 1 to 5, which satisfy the requirements of the present invention, were able to achieve a good balance between the 5% weight loss temperature and the glass transition temperature.

[0139] With regard to the 5% weight loss temperature, a person skilled in the art would predict that the values ​​when the proportion of recycled methyl methacrylate was 0% (Reference Example 1) and 100% (Comparative Example 1) would be connected by a straight line (dashed line in FIG. 1), but all of the measured values ​​in Examples 1 to 5 exceeded this prediction, achieving an improvement of more than 10°C at the maximum. In addition, a person skilled in the art would predict that the values ​​when the proportion of recycled methyl methacrylate was 0% (Reference Example 1) and 100% (Comparative Example 1) would be connected by a straight line (dashed line in FIG. 2) when the proportion of recycled methyl methacrylate was 0%, taking into account the predicted value calculated from the FOX formula, but all of the measured values ​​in Examples 1 to 5 significantly exceeded this prediction. Specifically, except for the cases where the proportion of recycled methyl methacrylate was 0% and 100%, the measured values ​​tended to be higher than the straight line in compositions containing non-regenerated methyl methacrylate and recycled methyl methacrylate. This tendency was such that the measured values ​​tended to be significantly higher than the straight line in compositions with a proportion of recycled MMA of 5 to 80%.

[0140] <Examples 6 to 7 and Comparative Example 2> A recycled methyl methacrylate product (recycled MMA (A), recycled methyl methacrylate content: 96.7% by mass) was prepared under the same conditions as in Preparation Example 1 (Comparative Example 2), except that the bath temperature during purification was changed to 60°C and the pressure to 170 mbar or more. Recycled MMA (A) and the non-recycled MMA obtained in Preparation Example 2 were mixed in the blending ratios shown in Table 2 to obtain each composition (liquid) (Examples 6 to 7). The 5% weight loss temperature (hereinafter referred to as T5) and glass transition temperature (hereinafter referred to as Tmg) of the molded bodies obtained by molding each composition by the above-mentioned method were measured under the above-mentioned conditions (Table 2).

[0141] [Table 2]

[0142] <Examples 8 to 10 and Comparative Example 3> A recycled methyl methacrylate product (recycled MMA (B): recycled methyl methacrylate content 97.9% by mass) was prepared under the same conditions as in Preparation Example 1, except that the raw material polymethyl methacrylate resin was changed to PMMA waste material (lighting cover) (Comparative Example 3). Recycled MMA (B) and the non-recycled methyl methacrylate product (non-recycled MMA) obtained in Preparation Example 2 were mixed in the blending ratios shown in Table 3 to obtain each composition (liquid) (Examples 8 to 10). The T5 and Tmg of the molded bodies obtained by molding each composition using the above-mentioned method were measured under the above-mentioned conditions (Table 3).

[0143] [Table 3]

[0144] <Examples 11 to 12 and Comparative Example 4> A recycled methyl methacrylate product (recycled MMA (C), recycled methyl methacrylate content 97.8% by mass) was prepared under the same conditions as in Preparation Example 1, except that the cylinder temperature during thermal decomposition was changed to 400°C (Comparative Example 4). Recycled MMA (C) and the non-recycled methyl methacrylate product (non-recycled MMA) obtained in Preparation Example 2 were mixed in the blending ratios shown in Table 4 to obtain each composition (liquid) (Examples 11-12). The T5 and Tmg of the molded bodies obtained by molding each composition using the above-mentioned method were measured under the above-mentioned conditions (Table 4).

[0145] [Table 4]

[0146] <Example 13 and Comparative Example 5> A recycled methyl methacrylate product (recycled MMA (D), recycled methyl methacrylate content 97.3% by mass) was prepared under the same conditions as in Preparation Example 1, except that the cylinder temperature during thermal decomposition was changed to 480°C (Comparative Example 5). Recycled MMA (D) and the non-recycled methyl methacrylate product (non-recycled MMA) obtained in Preparation Example 2 were mixed in the blending ratios shown in Table 4 to obtain each composition (liquid) (Example 13). The T5 and Tmg of the molded bodies obtained by molding each composition using the above-mentioned method were measured under the above-mentioned conditions (Table 5).

[0147] [Table 5]

[0148] When the results of T5 and Tg of each test example are plotted in Figures 3 and 4, the T5 and Tg of the PMMA molded body mixed with the recycled MMA of Examples 1 to 5 of the present application (● in the figure) and the PMMA molded body mixed with recycled MMA (A) to (D) (□, △, *, - in the figure, respectively) were all higher than the straight lines (dashed lines) connecting the T5 and Tmg of the molded body of Reference Example 1 (100% non-recycled MMA) and the T5 of Comparative Example 2 and the Tmg of Comparative Example 5 (the highest values ​​of T5 and Tmg of Comparative Examples 2 to 5). For both Tmg and T5 (especially Tmg), there was a tendency for measured values ​​to exceed the straight line in compositions containing non-recycled methyl methacrylate and recycled methyl methacrylate, except when the proportion of recycled methyl methacrylate was 0% or 100%. This tendency was such that measured values ​​significantly exceeded the straight line in compositions containing 5 to 80% recycled MMA.

[0149] (Evaluation of storage stability of composition) A storage test was carried out in the following order of steps 1 to 7 for compositions 1 to 3 and R1 prepared in Examples 1 to 3, Comparative Example 1 and Reference Example 1. The storage test was carried out under accelerated conditions (80°C) in order to evaluate the stability after long-term storage.

[0150] Step 1: 25 mL of the composition is poured into the lower part (container) of a pressure vessel ("TVS-N2 type" manufactured by Taiatsu Glass Industries Co., Ltd.). Step 2: Place a gasket between the top (top lid) and bottom of the pressure vessel to seal the pressure vessel. Step 3: Nitrogen is sent from the tip (piping) at the top of the pressure vessel, and sealed when the internal pressure is 0.2 MPa. Check that the internal pressure does not change for one minute. Step 4: Install the stopcock at the top of the pressure vessel. Step 5: Place the pressure vessel in an oil bath set at 80°C. Step 6: Keep in oil bath for 24 hours. Step 7: After 24 hours, remove the pressure vessel from the oil bath.

[0151] The composition (4 mL) after the storage test was placed in a quartz glass cell (T-1, manufactured by Taiko Seisakusho Co., Ltd.) with dimensions of 10 mm length x 10 mm width x 45 mm height. Using the composition placed in the quartz glass cell, the yellowness index (YI value) was determined according to the method described in JIS K7373 when the optical path length was set to 10 mm (Table 6). The measurement was performed using a spectrophotometer (Hitachi High-Tech Fielding Corporation's "Hitachi Spectrophotometer U-4000") under the following conditions. It can be determined that the smaller the YI value, the more the yellow discoloration is suppressed even after storage.

[0152] (YI measurement conditions) Light source: C light source Field of view: 2 degrees Calculation formula: YI=(1.2769×X-1.0592×Z) / Y×100

[0153] [Table 6]

[0154] Compared with compositions R1 and C1 of Reference Example 1 and Comparative Example 1, compositions 1 to 3 of Examples 1 to 3 had lower YI values ​​after the storage test, indicating that yellowing after storage was suppressed (Table 6).

Claims

1. Contains recycled methyl methacrylate and non-regenerated methyl methacrylate, A methyl methacrylate composition having a recycled methyl methacrylate content of 0.5 to 99.5% by mass and a non-recycled methyl methacrylate content of 0.5 to 99.5% by mass.

2. The methyl methacrylate composition according to claim 1, wherein the recycled methyl methacrylate is recycled methyl methacrylate derived from chemical recycling.

3. The methyl methacrylate composition according to claim 1 or 2, wherein the content of the regenerated methyl methacrylate is 5 to 40% by mass and the content of the non-regenerated methyl methacrylate is 60 to 95% by mass.

4. 3. The methyl methacrylate composition of claim 1 or 2, further comprising an alkyl acrylate.

5. A method for producing a methyl methacrylate polymer, comprising a step of polymerizing the methyl methacrylate composition according to claim 1 or 2.

6. A methyl methacrylate polymer obtained by polymerizing the methyl methacrylate composition according to claim 1 or 2.

7. A methyl methacrylate-based polymer containing structural units derived from recycled methyl methacrylate and structural units derived from unregenerated methyl methacrylate, the content of the structural units derived from recycled methyl methacrylate being 0.5 to 99.5% by mass, and the content of the structural units derived from unregenerated methyl methacrylate being 0.5 to 99.5% by mass.

Citation Information

Patent Citations

  • Method for recovering monomer from acrylic resin

    JP2003321571A