Thermosetting resin composition, cured product and laminate
The thermosetting resin composition with a polydimethylsiloxane structure and blocked isocyanate groups addresses issues of transparency and durability in cured films, providing long-lasting water sliding properties and improved scratch resistance for automotive components.
Patent Information
- Application Number
- JP2024112692
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-31
AI Technical Summary
Existing thermosetting resin compositions used for forming cured films on automotive components suffer from defects such as poor appearance and transparency, as well as reduced durability and water sliding properties after wet heat tests.
A thermosetting resin composition comprising a polymer with a polydimethylsiloxane structure and active hydrogen groups, combined with compounds having blocked isocyanate groups, and optionally inorganic fine particles, to form a cured film with improved transparency and long-lasting water sliding properties.
The composition achieves excellent transparency and maintains good water sliding properties over time, with enhanced durability and scratch resistance, making it suitable for automotive applications.
Smart Images

Figure 2024133245000001 
Figure 2024133245000002 
Figure 2024133245000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, in particular a thermosetting resin composition capable of forming a cured film having excellent water sliding properties, a cured product of the composition, and a laminate having a layer made of the cured product. [Background technology]
[0002] Resin molded products made from resins such as polymethyl methacrylate resin, polymethacrylimide resin, polycarbonate resin, polystyrene resin, and acrylonitrile-styrene resin are lightweight, have excellent impact resistance, and have good transparency, so they are used as materials for various automotive lamp lenses, glazing (plastic windows), exteriors, instrument covers, and other components. In recent years, radar devices using various electromagnetic waves such as millimeter waves are installed on the back of the emblem or front grille on the front of the vehicle to detect obstacles ahead and measure the distance between vehicles. Since these electromagnetic waves are significantly attenuated by water, the outermost surfaces of the emblem, front grille, etc. through which the electromagnetic waves pass are required to have a water-repellent function that makes it difficult for water droplets to adhere and allows water droplets to slide off easily. To satisfy these demands, a method is known in which the surface of a resin molded article is coated with a curable composition containing a resin having a polydimethylsiloxane structure to impart water-sliding properties.
[0003] For example, Patent Document 1 discloses a method for forming a cured film having water-sliding properties by applying a curable composition containing a monomer having a fluoroalkyl group, a monomer having a polydimethylsiloxane structure, and a copolymer of a polyfunctional unsaturated compound to a substrate and heating the composition. Furthermore, Patent Document 2 discloses a method for forming a cured film having water-sliding properties by curing a thermosetting resin composition containing a copolymer of a monomer having a polydimethylsiloxane structure and a monomer having a hydroxyl group, and a bifunctional isocyanate.
[0004] However, the method described in Patent Document 1 has the problem that defects such as repelling are generated in the cured film, which deteriorates the appearance of the cured film and reduces the transparency. In addition, the method described in Patent Document 2 has the problem that the durability of the cured film is low, and the water sliding property is significantly impaired after a wet heat test. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-185072 A [Patent Document 2] JP 2000-230060 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a thermosetting resin composition capable of forming a cured film having excellent transparency and capable of maintaining good water sliding property for a long period of time, a cured product of the composition, and a laminate having a layer made of the cured product. [Means for solving the problem]
[0007] The gist of the present invention resides in the following [1] to [9]. [1] A thermosetting resin composition comprising: a polymer (X1) having a polydimethylsiloxane structure and an active hydrogen group in the main chain or a side chain; a compound (Y1) having two or more optionally blocked isocyanate groups per molecule; and a compound (Z1) having two or more active hydrogen groups per molecule. [2] A thermosetting resin composition comprising: a polymer (X1) having a polydimethylsiloxane structure and an active hydrogen group in the main chain or a side chain; and a compound (Y2) having three or more optionally blocked isocyanate groups per molecule. [3] A polymer (X2-2) having a polydimethylsiloxane structure and an optionally blocked isocyanate group in its main chain or side chain, and further containing 30 mass% or more of a structural unit derived from an aromatic vinyl monomer in its main chain. [4] A thermosetting resin composition comprising a polymer (X2) having a polydimethylsiloxane structure and an optionally blocked isocyanate group in the main chain or a side chain, and a compound (Z1) having two or more active hydrogen groups per molecule. [5] The thermosetting resin composition according to [4], further comprising a compound (Y1) having two or more optionally blocked isocyanate groups per molecule. [6] The thermosetting resin composition according to any one of [1], [2], [4] and [5], further comprising inorganic fine particles. [7] The thermosetting resin composition according to [6], wherein the inorganic fine particles are surface-modified with a compound having any one of a mercapto group, a hydroxyl group, or an isocyanate group. [8] A cured product obtained by curing the thermosetting resin composition according to any one of [1], [2], [4], and [7]. [9] A laminate having a layer made of the cured product of [8] on a substrate. Effect of the Invention
[0008] The thermosetting resin composition of the present invention can form a cured film that has excellent transparency and can maintain good water sliding property for a long period of time. The cured product and laminate of the present invention have excellent transparency and can maintain good water sliding property for a long period of time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Composition (A1)] The thermosetting resin composition of the present invention is a thermosetting resin composition [hereinafter referred to as "composition (A1)"] comprising a polymer (X1) [hereinafter referred to as "polymer (X1)"] having a polydimethylsiloxane structure and an active hydrogen group in the main chain or side chain, a compound (Y1) [hereinafter referred to as "compound (Y1)"] having two or more optionally blocked isocyanate groups per molecule, and a compound (Z1) [hereinafter referred to as "compound (Z1)"] having two or more active hydrogen groups per molecule.
[0010] <Polymer (X1)> The polymer (X1) is a polymer having a polydimethylsiloxane structure and an active hydrogen group in the main chain or side chain. That is, the polymer (X1) needs to contain a polydimethylsiloxane structure in either or both of its main chain or side chain, and to contain an active hydrogen group in either or both of its main chain or side chain.
[0011] <Polydimethylsiloxane structure> The polydimethylsiloxane structure contributes to the water-repellent property of the cured film formed from the composition (A1) containing the polymer (X1).
[0012] Examples of methods for introducing a polydimethylsiloxane structure into the polymer (X1) include (1) copolymerizing a macromonomer having a polydimethylsiloxane structure and an unsaturated bond [hereinafter referred to as "macromonomer (M1)] with another monomer, (2) copolymerizing a polydimethylsiloxane having mercapto groups at the α,ω positions with another monomer as a chain transfer agent, (3) copolymerizing an azo compound having a polydimethylsiloxane structure with another monomer, and (4) adding a hydroxyl group of a polydimethylsiloxane having a hydroxyl group at its terminal to the isocyanate group of a polymer having an optionally blocked isocyanate group.
[0013] Examples of the macromonomer (M1) used in the method (1) include Silaplane (registered trademark) FM-0711 (number average molecular weight listed in the catalog: 1000), Silaplane FM-0721 (number average molecular weight listed in the catalog: 5000), and Silaplane FM-0725 (number average molecular weight listed in the catalog: 10000) manufactured by JNC; and X-22-174ASX (number average molecular weight listed in the catalog: 900), X-22-174BX (number average molecular weight listed in the catalog: 2300), KF-2012 (number average molecular weight listed in the catalog: 4600), and X-22-2426 (number average molecular weight listed in the catalog: 12000) manufactured by Shin-Etsu Chemical Co., Ltd. Among these, mono(meth)acryloyloxypropyl-modified polydimethylsiloxanes such as Silaplane FM-072, Silaplane FM-0721, Silaplane FM-0725, X-22-174ASX, X-22-174BX, KF-2012, and X-22-2426 are suitable because they are easily available industrially.
[0014] Examples of polydimethylsiloxanes having mercapto groups at the α- and ω-positions that can be used as chain transfer agents in the method (2) above include X-22-167B (number average molecular weight listed in the catalog: 3400) and X-22-167C (number average molecular weight listed in the catalog: 4600) manufactured by Shin-Etsu Chemical Co., Ltd.
[0015] Examples of the azo compound having a polydimethylsiloxane structure used in the method (3) include VPS-0501 (product name: polydimethylsiloxane-based polymeric azo initiator, polydimethylsiloxane chain length 5000) and VPS-1001 (product name: polydimethylsiloxane-based polymeric azo initiator, polydimethylsiloxane chain length 10000) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0016] As a method for introducing a polydimethylsiloxane structure into the polymer (X1), the above method (1) is preferred from the viewpoint of easy availability of raw materials.
[0017] <Active hydrogen group> The active hydrogen group reacts with the isocyanate group of the compound (Y1), and the polymer (X1) is firmly fixed to the cured film, contributing to water sliding durability and scratch resistance. The active hydrogen group of the polymer (X1) is, for example, a functional group such as a hydroxyl group, a mercapto group, or an amino group. The active hydrogen group can react with the isocyanate group of the compound (Y1) having an isocyanate group to form a bond such as a urethane bond.
[0018] The hydroxyl group may be primary, secondary or tertiary, but is preferably primary or secondary. The mercapto group and amino group may be primary, secondary or tertiary, but is preferably primary or secondary.
[0019] In order to introduce an active hydrogen group into the polymer (X1), a method is preferred in which a monomer having an active hydrogen group [hereinafter referred to as "monomer (M2)] is copolymerized with the macromonomer (M1) as another monomer in the above-mentioned method (1) for introducing a polydimethylsiloxane structure.
[0020] <Production of Polymer (X1)> Hereinafter, the method (1) for producing the polymer (X1) by copolymerization of the macromonomer (M1) with the monomer (M2) as another monomer will be described.
[0021] <Macromonomer (M1)> The polydimethylsiloxane structure of the macromonomer (M1) used in the production of the polymer (X1) may be either a straight-chain structure or a branched-chain structure. The polydimethylsiloxane structure may have an alkyl group at the end or an alkylene group inside. For example, when an unsaturated bond is introduced or a branched chain is formed, an alkylene group having 1 to 6 carbon atoms may be interposed between the polydimethylsiloxane structure.
[0022] Examples of the unsaturated bond in the macromonomer (M1) include a (meth)acryloyl group, a vinyl group, and a (meth)acrylamide group. Among these, a (meth)acryloyl group is preferred from the viewpoint of ease of copolymerization with other monomers.
[0023] The molecular weight of the macromonomer (M1) is preferably 500 to 40,000, more preferably 700 to 30,000, and even more preferably 800 to 20,000. The smaller the molecular weight, the easier the compatibility of the macromonomer (M1) with other monomers, and the easier it tends to be to produce the polymer (X1). Also, the larger the molecular weight, the better the water slipping property of the cured film tends to be.
[0024] The amount of the macromonomer (M1) introduced into the polymer (X1) is preferably 5% by mass or more and less than 70% by mass, more preferably 10% by mass or more and less than 60% by mass, and even more preferably 20% by mass or more and less than 50% by mass. The larger the amount of the macromonomer (M1) introduced, the better the water sliding property of the cured film becomes, and the smaller the amount of unpolymerized macromonomer (M1) can be reduced, so that the transparency of the cured film tends to be better.
[0025] <Monomer (M2)> The monomer (M2) is used to introduce an active hydrogen group into the polymer (X1). Examples of the monomer (M2) include (meth)acrylic acid esters, N-substituted (meth)acrylamides, and vinyl compounds having a hydroxyl group, a mercapto group, or an amino group. Examples of the monomer (M2) having a hydroxyl group include (meth)acrylic acid esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, propylene glycol mono(meth)acrylate, 1,6-hexanediol mono(meth)acrylate, and glycerin mono(meth)acrylate; N-(2-hydroxyethyl)acrylamide, N-(2-hydroxyethyl)methacrylamide, N-(2-hydroxypropyl) ... Examples of N-substituted (meth)acrylamides include N-(1-hydroxypropyl)methacrylamide, N-(1-hydroxypropyl)acrylamide, N-(3-hydroxypropyl)acrylamide, N-(3-hydroxypropyl)methacrylamide, N-(2-hydroxybutyl)acrylamide, N-(2-hydroxybutyl)methacrylamide, N-(3-hydroxybutyl)acrylamide, N-(3-hydroxybutyl)methacrylamide, N-(4-hydroxybutyl)acrylamide, and N-(4-hydroxybutyl)methacrylamide. Here, examples of the (meth)acrylic acid ester include 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 3-hydroxypropyl (meth)acrylate, and examples of the N-substituted (meth)acrylamide include N-(2-hydroxyethyl)acrylamide and N-(2-hydroxyethyl)methacrylamide. Particularly preferred examples of the monomer (M2) having a hydroxyl group include 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate. The monomer (M2) having a hydroxyl group may be used alone or in combination of two or more kinds.
[0026] The active hydrogen group can also be introduced by using a chain transfer agent during the production of the polymer (X1) by copolymerization. Examples of such a chain transfer agent include mercaptans having a hydroxyl group and mercaptans having an amino group.
[0027] Examples of mercaptans having a hydroxyl group include mercaptoethanol and thioglycerol. Examples of mercaptans having an amino group include 2-aminoethanethiol, 2-aminobenzenethiol, 4-aminobenzenethiol, and L-cysteine, as well as hydrochlorides thereof.
[0028] The amount of active hydrogen groups introduced into the polymer (X1) is preferably 0.1 mmol / g or more and less than 4.0 mmol / g, more preferably 0.2 mmol / g or more and less than 3.5 mmol / g, and even more preferably 0.3 mmol / g or more and less than 3.0 mmol / g. The greater the amount introduced, the more the durability of the cured film improves, and the smaller the amount introduced, the more the water slipping of the cured film improves.
[0029] <Other monomers> In the production of the polymer (X1), in addition to the macromonomer (M1) and the monomer (M2), other monomers can be copolymerized within the range that does not impair the performance. Examples of other monomers include aromatic vinyl compounds such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, vinylbiphenyl, vinylanthracene, and vinylxylene; alkyl (meth)acrylates or alkenyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, behenyl (meth)acrylate, and allyl (meth)acrylate; cyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopenta(meth)acrylate, and the like. (meth)acrylates having an alicyclic structure such as dicyclopentenyl (meth)acrylate and dicyclopentenyl (meth)acrylate; (meth)acrylates having an aromatic ring such as benzyl (meth)acrylate and phenyl (meth)acrylate; (meth)acrylates containing an oxygen atom such as phenoxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate and glycidyl methacrylate; carboxy group-containing methacrylic acid monomers such as (meth)acrylic acid and 2-(meth)acryloyloxyethyl phthalate; N-substituted (meth)acrylamides such as (meth)acrylamide, dimethyl (meth)acrylamide, (meth)acryloylmorpholine, isopropyl (meth)acrylamide and dimethylaminopropyl acrylamide; (meth)acrylates containing a halogen atom such as trifluoroethyl (meth)acrylate and heptadecafluorodecyl (meth)acrylate;Examples of the monomers include silicon atom-containing (meth)acrylates such as trimethylsilyl (meth)acrylate, 3-(trimethoxysilyl)propyl (meth)acrylate, 3-(methyldiethoxy)propyl (meth)acrylate, and 3-(triethoxy)propyl (meth)acrylate; (meth)acrylates having an ultraviolet absorbing group such as 2-(4-benzoxy-3-hydroxyphenoxy)ethyl methacrylate and 2-(2'-hydroxy-5-methacryloyloxyethylphenyl)-2H-benzotriazole; and nitrogen atom-containing (meth)acrylates such as tetramethylpiperidinyl (meth)acrylate and diethylaminoethyl (meth)acrylate. As other monomers, monomers such as vinyl alkanoate compounds and maleic acid monomers may be used.
[0030] As the other monomers, those having a homopolymer glass transition temperature of more than 30° C. are preferred from the viewpoint of improving the hardness of the cured film, and monomers having an aromatic ring or an alicyclic structure are preferred from the viewpoint of water slippage. Among them, aromatic vinyl compounds not containing a carbonyl group are preferred from the viewpoint of improving the water slippage of the cured film, since they have low hydrogen bonding with water molecules.
[0031] The copolymerization amount of the other monomer in the polymer (X1) is the remainder of the copolymerization amount of the macromonomer (M1) and the monomer (M2), and is preferably 20% by mass or more and less than 90% by mass, more preferably 25% by mass or more and less than 85% by mass, and even more preferably 30% by mass or more and less than 80% by mass. The higher the copolymerization amount, the better the copolymerization property during copolymerization, and the lower the copolymerization amount, the better the water sliding property tends to be.
[0032] <Initiator> In the production of the polymer (X1), it is preferable to use an initiator when copolymerizing the macromonomer (M1) and the monomer (M2). As the initiator, various initiators can be used. Examples of the oil-soluble radical polymerization initiator include azonitrile compounds such as 2,2-azobis(4-methoxy-2,4-dimethylvaleronitrile) (V-70, Fujifilm Wako Pure Chemical Industries, Ltd.), 2,2'-azobis(2,4-dimethylvaleronitrile) (V-65, Fujifilm Wako Pure Chemical Industries, Ltd.), 2,2'-azobisisobutyronitrile (V-60, Fujifilm Wako Pure Chemical Industries, Ltd.), and 2,2'-azobis(2-methylbutyronitrile) (V-59, Fujifilm Wako Pure Chemical Industries, Ltd.); octanoyl peroxide (Perloyl (registered trademark) O, NOF Corp., diacyl peroxides such as lauroyl peroxide (Perloyl L, manufactured by NOF Corp.), stearoyl peroxide (Perloyl S, manufactured by NOF Corp.), succinic acid peroxide (Perloyl SA, manufactured by NOF Corp.), benzoyl peroxide (Niper (registered trademark) BW, manufactured by NOF Corp.), isobutyryl peroxide (Perloyl IB, manufactured by NOF Corp.), 2,4-dichlorobenzoyl peroxide (Niper CS, manufactured by NOF Corp.), and 3,5,5-trimethylhexanoyl peroxide (Perloyl 355, manufactured by NOF Corp.); di-n-propyl peroxide Dicarbonate (Perloyl NPP-50M, NOF Corp.), diisopropyl peroxydicarbonate (Perloyl IPP-50, NOF Corp.), bis(4-t-butylcyclohexyl) peroxydicarbonate (Perloyl TCP, NOF Corp.), di-2-ethoxyethyl peroxydicarbonate (Perloyl EEP, NOF Corp.), di-2-ethoxyhexyl peroxydicarbonate (Perloyl OPP, NOF Corp.), di-2-methoxybutyl peroxydicarbonate (Perloyl MBP, NOF Corp.), di(3-methyl-3-meth peroxydicarbonates such as tert-butyl hydroperoxide (Perbutyl H-69, NOF Corp.), 1,1,3,3-tetramethylbutyl hydroperoxide (Perocta(R) H, NOF Corp.), etc. hydroperoxides such as di-t-butyl peroxide (Perbutyl(R) D, NOF Corp.), 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane (Perhexa(R) 25B, NOF Corp.), etc. dialkyl peroxides such as di-t-butyl peroxide (Perbutyl(R) D, NOF Corp.), 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane (Perhexa(R) 25B, NOF Corp.), etc.α,α'-Bis(neodecanoylperoxy)diisopropylbenzene (Diper(R) ND, manufactured by NOF Corp.), cumyl peroxy neodecanoate (Percumyl(R) ND, manufactured by NOF Corp.), 1,1,3,3-tetramethylbutyl peroxy neodecanoate (Perocta ND, manufactured by NOF Corp.), 1-cyclohexyl-1-methylethyl peroxy neodecanoate (Percyclo(R) ND, manufactured by NOF Corp.), t-hexyl peroxy neodecanoate (Perhexyl(R) ND, manufactured by NOF Corp.), t-butyl peroxy neodecanoate (Perbutyl ND, manufactured by NOF Corp.), t-hexyl peroxy pivalate (Perhexyl PV, manufactured by NOF Corp.), t-butyl peroxy pivalate (Perbutyl PV, manufactured by NOF Corp.), 1,1,3,3-tetramethylbutyl Examples of the peroxyester include organic peroxides such as peroxy esters such as peroxy esters, ...
[0033] The amount of initiator added when producing the polymer (X1) is preferably 0.1% by mass or more and less than 10% by mass, more preferably 0.3% by mass or more and less than 6% by mass, and even more preferably 0.5% by mass or more and less than 3% by mass, based on the total amount of the macromonomer (M1), the monomer (M2), and other monomers. The larger the amount of initiator added, the better the coatability becomes, and the smaller the amount of initiator added, the better the water slipping property tends to be.
[0034] The polymer (X1) can be produced by a polymerization method such as solution polymerization, bulk polymerization, suspension polymerization, emulsion polymerization, etc. An initiator may be used in an appropriate manner for each polymerization method.
[0035] <Molecular weight of polymer (X1)> The weight average molecular weight of the polymer (X1) is preferably 5000 to 400000, more preferably 5000 to 300000, and particularly preferably 10000 to 200000. The smaller the weight average molecular weight, the lower the viscosity of the thermosetting resin composition and the better the coatability, while the larger the weight average molecular weight, the more firmly the polymer (X1) is fixed to the cured film, which tends to improve the water sliding property and scratch resistance.
[0036] The molecular weight of the polymer (X1) is a weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) and converted into standard polystyrene.
[0037] <Content of polymer (X1)> The content of the polymer (X1) in the composition (A1) is preferably 5 to 95 mass%, more preferably 8 to 90 mass%, and even more preferably 10 to 75 mass%, based on the total mass of the polymer (X1), the compound (Y1), and the compound (Z1). The higher the content, the higher the water slipping property of the cured film tends to be, while the lower the content, the higher the scratch resistance and hardness of the cured film tends to be.
[0038] <Compound (Y1)> Compound (Y1) is a compound having two or more isocyanate groups, which may be blocked, in one molecule. When curing composition (A1), the isocyanate group of compound (Y1) reacts with the active hydrogen group of polymer (X1) and the active hydrogen group of compound (Z1), forming bonds such as urethane bonds between these compounds and polymers. This increases the crosslink density of the cured product, such as the cured film, and is therefore considered to improve weather resistance and contamination resistance.
[0039] Examples of the compound (Y1) include difunctional isocyanates such as hexamethylene diisocyanate (HDI), dicyclohexylmethane diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, and 4,4-dicyclohexyl diisocyanate, as well as trifunctional or higher isocyanates such as biuret compounds, trimethylolpropane adduct compounds, isocyanurate compounds, and allophanate compounds synthesized using these difunctional isocyanates as a starting material.
[0040] Examples of the compound (Y1) include a biuret of hexamethylene diisocyanate (trade name: Duranate (registered trademark) 22A-75P), an adduct of hexamethylene diisocyanate (trade name: Duranate P-301-75E), an isocyanurate of hexamethylene diisocyanate (trade name: Duranate TPA-100), a blocked isocyanate (trade name: Duranate MF-K60X), and a trimethylol propionate of 1,3-bis(isocyanatomethyl)cyclohexane (trade name: Duranate MF-K60X), all manufactured by Asahi Kasei. Examples of such isocyanates include tri- or higher functional isocyanates and blocked isocyanates, such as a trimethylolpropane adduct (trade name: Takenate (registered trademark) D-120N), an isocyanurate of 1,3-bis(isocyanatomethyl)cyclohexane (trade name: Takenate D-127N), a trimethylolpropane adduct of isophorone diisocyanate (trade name: Takenate D-140N), and an allophanate of hexamethylene diisocyanate manufactured by Sumika Covestro Urethane Co., Ltd. (trade name: Desmodur (registered trademark) XP2679).
[0041] As the compound (Y1), a trifunctional or higher isocyanate (hereinafter referred to as "compound (Y2)") is preferable from the viewpoint of improving the crosslink density of the cured film and improving the weather resistance and stain resistance. The compound (Y1) may be used alone or in combination of two or more kinds.
[0042] The content of compound (Y1) in composition (A1) is preferably 5 to 60 mass%, more preferably 7 to 50 mass%, and even more preferably 10 to 45 mass%, based on the total mass of polymer (X1), compound (Y1) and compound (Z1). The higher the content, the higher the scratch resistance and hardness of the cured film, and the lower the content, the higher the water sliding property.
[0043] <Compound (Z1)> The compound (Z1) is a compound having two or more active hydrogen groups in one molecule. The active hydrogen group is, for example, a functional group such as a hydroxyl group, a mercapto group, or an amino group. The active hydrogen group can react with the isocyanate group of the compound (Y1) having an isocyanate group to form a bond such as a urethane bond. The hydroxyl group may be primary, secondary, or tertiary, but is preferably primary or secondary. The mercapto group and the amino group may also be primary, secondary, or tertiary, but is preferably primary or secondary.
[0044] From the viewpoints of availability of raw materials and resistance to yellowing due to hardness of the cured film, the active hydrogen group of compound (Z1) is most preferably a hydroxyl group, followed by a mercapto group, and then an amino group.
[0045] When the active hydrogen group of the compound (Z1) is a hydroxyl group, any known polyol compound can be used without any particular limitation.
[0046] <Compound (Z1) having two hydroxyl groups per molecule> When the active hydrogen group of the compound (Z1) is a hydroxyl group, any known polyol compound can be used without any particular limitation. Specific examples of the polyol compounds having two hydroxyl groups per molecule include chain aliphatic glycols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, methylpentanediol, dimethylbutanediol, butylethylpropanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, tripropylene glycol, and bishydroxyethoxybenzene; Examples of the glycols include alicyclic glycols such as 4-cyclohexanediol and 1,4-cyclohexanedimethanol; bisphenols such as bisphenol A, bisphenol F, hydrogenated bisphenol A, and hydrogenated bisphenol F; polycarbonate diols; dimer acid diols; polyether polyols obtained by addition polymerization of the above-mentioned glycols with alkylene oxides such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide, epichlorohydrin, tetrahydrofuran, and cyclohexylene in the presence of a polymerization initiator; and polyester diols obtained by condensing the above-mentioned glycols with polyvalent carboxylic acids.
[0047] Among compounds having two hydroxyl groups in one molecule, polycarbonate diols having a large molecular weight are preferred because they increase the hardness of the cured film. Commercially available polycarbonate diols include, for example, Kuraray Polyol C-1015N, Kuraray Polyol C-1065N (Kuraray carbonate diol: 2-methyl-1,8-octanediol / 1,9-nonanediol, number average molecular weight of about 1000), Kuraray Polyol C-2015N, Kuraray Polyol C-2065N (Kuraray carbonate diol: 2-methyl-1,8-octanediol / 1,9-nonanediol, number average molecular weight of about 2000), Kuraray Polyol C-1050, Kuraray Polyol C-1090 (Kuraray carbonate diol: 3-methyl-1,5-pentanediol / 1,6-hexanediol, number average molecular weight of about 1000), Kuraray Polyol C-2050, Kuraray Polyol C-2090 (Kuraray carbonate diol: 3-methyl-1,5-pentanediol / 1,6-hexanediol, number average molecular weight about 2000), DURANOL (registered trademark)-T5650E (Asahi Kasei polycarbonate diol: 1,5-pentanediol / 1,6-hexanediol, number average molecular weight about 500), DURANOL-T5651 (Asahi Kasei polycarbonate diol: 1,5-pentanediol / 1,6-hexanediol, number average molecular weight about 1000), DURANOL-T5652 (Asahi Kasei polycarbonate diol: 1,5-pentanediol / 1,6-hexanediol, number average molecular weight about 2000).
[0048] Of the compounds (Z1), those having three or more hydroxyl groups per molecule are preferred because they are more likely to improve the hardness of the cured film than those having two hydroxyl groups per molecule. Specific examples of the compound having three or more hydroxyl groups per molecule include trifunctional or tetrafunctional aliphatic alcohols such as glycerin, trimethylolpropane, pentaerythritol, polycaprolactone triol, and polycaprolactone tetraol; polyether polyols obtained by addition polymerization of the trifunctional or tetrafunctional aliphatic alcohols or the like with alkylene oxides such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide, epichlorohydrin, tetrahydrofuran, and cyclohexylene in the presence of a polymerization initiator; and polyester polyols obtained by condensing the trifunctional or tetrafunctional aliphatic alcohols or the like with polyvalent carboxylic acids.
[0049] Among these compounds having three or more hydroxyl groups per molecule, the group of compounds having five or more hydroxyl groups per molecule and a dendritic branched structure is particularly preferred because it has the greatest effect of improving the hardness and scratch resistance of the cured film. The group of compounds having five or more hydroxyl groups per molecule and a dendritic branched structure is sometimes called a dendrimer or a hyperbranched polymer.
[0050] Examples of commercially available dendrimers having a hydroxyl group at an end include Boltorn (registered trademark) H20 (hydroxyl group concentration 8.73 to 9.27 mmol / g, molecular weight 2100 (catalog value)), Boltorn H311 (hydroxyl group concentration 4.10 to 4.63 mmol / g, molecular weight 5300 (catalog value)), Boltorn H2004 (hydroxyl group concentration 2.23 to 2.67 mmol / g, molecular weight 3100 (catalog value)), Boltorn P500 (hydroxyl group concentration 9.98 to 11.23 mmol / g, molecular weight 1800 (catalog value)), Boltorn P1000 (hydroxyl group concentration 7.66 to 11.23 mmol / g, molecular weight 1500 (catalog value)), Boltorn Examples include U3000 (hydroxyl group concentration 0.27 mmol / g, molecular weight 6500 (catalog value)) and Boltorn W3000 (hydroxyl group concentration 0.27 mmol / g, molecular weight 10000 (catalog value)).
[0051] Commercially available examples of the hyperbranched polymers having hydroxyl groups at their ends include BASF's Basonol (registered trademark) HPE 1170B (hydroxyl group concentration 4.99 mmol / g, molecular weight 1800 (catalog value)) and Basonol HPE 021 (hydroxyl group concentration 3.39 mmol / g, molecular weight 1400 (catalog value)).
[0052] Specific examples of the compound (Z1) having two mercapto groups per molecule include 1,3-propanedithiol, 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexaneedithiol, 1,7-heptanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 1,10-decanedithiol, bis(mercaptomethyl)sulfide, bis(mercaptoethyl)sulfide, bis(mercaptomethyl)ether, bis(mercaptoethyl)ether, bis(mercaptomethyl)amine, and bis(mercaptoethyl)amine.
[0053] Specific examples of the compound (Z1) having three or more mercapto groups per molecule include trimethylolpropane tris(3-mercaptopropionate), tris[(3-mercaptopropionyloxy)-ethyl]-isocyanurate, pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), 1,3,5-tris(2-(3-sulfanylbutanoyloxy)ethyl)-1,3,5-triazinane-2,4,6-trione, and trimethylolpropane tris(3-mercaptobutyrate).
[0054] Specific examples of the compound (Z1) having two amino groups per molecule include low molecular weight diamines in which the alcoholic hydroxyl groups of the low molecular weight diols described above are substituted with amino groups, such as ethylenediamine and propylenediamine; polyether diamines, such as polyoxypropylenediamine and polyoxyethylenediamine; menthene diamine, isophorone diamine, norbornene diamine, bis(4-amino-3-methyldicyclohexyl)methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro(5,5 alicyclic diamines such as m-xylylenediamine, α-(m / p-aminophenyl)ethylamine, m-phenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiethyldimethyldiphenylmethane, diaminodiethyldiphenylmethane, dimethylthiotoluenediamine, diethyltoluenediamine, α,α'-bis(4-aminophenyl)-p-diisopropylbenzene, and other aromatic diamines; hydrazine; and dicarboxylic acid dihydrazide compounds which are compounds of hydrazine and the dicarboxylic acids exemplified in the polyvalent carboxylic acids used in the polyester polyols described above.
[0055] Among the compounds (Z1), examples of the compounds having three or more amino groups in one molecule include aliphatic amines such as triethylenetetramine, tetraethylenepentamine, and pentaethylenehexamine.
[0056] As the compound (Z1), a single compound may be used, or two or more kinds may be used in combination.
[0057] The molecular weight of the compound (Z1) is preferably 150 to 30,000, more preferably 600 to 10,000, and even more preferably 800 to 5,000. The higher the molecular weight, the higher the hardness of the cured film, and the lower the molecular weight, the better the appearance of the cured film. The molecular weight here is the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) and converted into standard polystyrene.
[0058] The active hydrogen group concentration of the compound (Z1) is preferably 0.35 to 18.0 mmol / g, more preferably 0.90 to 12.0 mmol / g. The higher the hydroxyl group concentration, the higher the hardness of the cured film tends to be, and the lower the hydroxyl group concentration, the better the solubility of the compound (Z1) in the composition (A1).
[0059] The content of compound (Z1) in composition (A1) is preferably 3 to 60 mass%, more preferably 5 to 50 mass%, and even more preferably 10 to 45 mass%, based on the total mass of polymer (X1), compound (Y1), and compound (Z1). The higher the content, the higher the scratch resistance and hardness of the cured film, and the lower the content, the higher the water slipping property of the cured film.
[0060] <Compounds having only one isocyanate group, which may be blocked, in one molecule> The composition (A1) may contain a compound having only one isocyanate group which may be blocked in one molecule. Examples of the compound having only one isocyanate group which may be blocked in one molecule include 2-isocyanatopropane, 2-isocyanato-2-methylpropane, isocyanatocyclohexane, 1-isocyanato-4-isopropenyl-1-methyl-cyclohexane, 4-(1-isocyanato-1-methylethyl)-1-methyl-1-cyclohexene, 1,3-dimethyl-5-isocyanatoadamantane, and 1-(1-isocyanato-1-methylethyl)-3-isopropenylbenzene.
[0061] The content of the compound having only one optionally blocked isocyanate group per molecule in the composition (A1) is preferably less than 8 mass%, more preferably less than 4 mass%, particularly preferably less than 2 mass%.
[0062] <Compounds that have only one active hydrogen group per molecule> The composition (A1) may contain a compound having only one active hydrogen group per molecule. Examples of the compound having an active hydrogen group even if it is the only blocked group in one molecule include alcohols such as methanol, ethanol, propanol, butanol, pentanol, hexanol, heptanol, octanol, 2-ethylhexanol, nonanol, decanol, undecyl alcohol, lauryl alcohol, tridecyl alcohol, myristyl alcohol, pentadecyl alcohol, cetanol, palmitoleic alcohol, heptadecanol, and stearyl alcohol (including isomers), as well as monofunctional thiols and monoamines.
[0063] The content of the compound having only one optionally blocked active hydrogen group per molecule in composition (A1) is preferably less than 8 mass%, more preferably less than 4 mass%, particularly preferably less than 2 mass%.
[0064] <Inorganic fine particles> The composition (A1) may contain inorganic fine particles such as silica fine particles. The inorganic fine particles contribute to improving the scratch resistance of the cured film. Since the scratch resistance is further improved, it is preferable that the inorganic fine particles have a functional group on the surface that can react with the active hydrogen group of the polymer (X1) or the compound (Z1) or the isocyanate group of the compound (Y1) to form a bond such as a urethane bond. Examples of such functional groups include mercapto groups, isocyanate groups, epoxy groups, hydroxyl groups, amino groups, and carbamoyl groups. Mercapto groups, isocyanate groups, and epoxy groups are preferred because they have high reactivity with active hydrogen groups or isocyanate groups.
[0065] As the inorganic fine particles to which the functional group is introduced, silica fine particles are preferred from the viewpoint of ease of introduction. As the method of introducing the functional group onto the surface of silica fine particles, for example, the method of treating by reacting the silanol group on the surface of silica fine particles with a silane coupling agent having a desired functional group can be mentioned.
[0066] The inorganic fine particles are preferably mixed in a dispersion. Specific examples of commercially available silica fine particle dispersions include SIRMEK20WT%-M70, SIRMEK50WT%-E86, SIRMIBK15WT%-M96, and SIRMIBK30WT%-S39 manufactured by CIK Nanotech, and MEK-EC-2130Y, MEK-EC-6150P, and MEK-EC-7150P manufactured by Nissan Chemical Industries. The inorganic fine particles may be used alone or in combination of two or more kinds.
[0067] The average particle size of the inorganic fine particles is preferably 300 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less, from the viewpoint of transparency of the cured film. Also, the average particle size is preferably 2 nm or more, more preferably 4 nm or more, from the viewpoint of improving scratch resistance. The average particle size is a value converted from the specific surface area measured by the BET adsorption method (based on JIS Z8830).
[0068] The content of the inorganic fine particles is preferably 1 to 60 mass %, more preferably 3 to 50 mass %, and even more preferably 5 to 45 mass %. The greater the amount of the inorganic fine particles added, the better the hardness of the cured film.
[0069] <Curing accelerating catalyst> The composition (A1) can be cured at room temperature or by heating, and may contain a curing-accelerating catalyst as necessary. Examples of the curing-accelerating catalyst include triethylamine, tetra(2-ethylhexyl) titanate, di-n-butyltin dilaurate, and 1,4-diazabicyclo[2.2.2]octane. The curing-accelerating catalyst may be used alone or in combination of two or more. The content of the curing-accelerating catalyst in the composition (A1) is preferably 0.001 to 10 parts by mass, more preferably 0.01 to 5 parts by mass, and even more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of isocyanate.
[0070] <Organic solvent> Composition (A1) may contain an organic solvent as necessary. Examples of the organic solvent include alcohol-based solvents such as methanol, isopropyl alcohol, n-butanol, diacetone alcohol, 2-methoxyethanol (methyl cellosolve), 2-ethoxyethanol (ethyl cellosolve), 2-butoxyethanol (butyl cellosolve) and tertiary amyl alcohol; carboxylic acid ester-based solvents such as ethyl acetate, n-propyl acetate, butyl acetate and butyl formate; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, acetone and cyclohexanone; amide-based solvents such as dimethylformamide and dimethylacetamide; ether-based solvents such as diethyl ether, methoxytoluene, 1,2-dimethoxyethane, 1,2-dibutoxyethane, 1,1-dimethoxymethane, 1,1-dimethoxyethane, 1,4-dioxane and tetrahydrofuran; aliphatic and aromatic hydrocarbon-based solvents such as hexane, pentane, xylene, toluene and benzene. These may be used alone or in combination of two or more.
[0071] <UV absorbers, light stabilizers> Composition (A1) may contain a weather resistance imparting agent such as an ultraviolet absorber, a light stabilizer, etc., in order to impart weather resistance to the cured film. As the weather resistance imparting agent, an ultraviolet absorber having a maximum absorption spectrum in the ultraviolet wavelength region that accelerates substrate deterioration is preferred.
[0072] The ultraviolet absorbing agent is preferably a compound derived from a triazine-based, benzophenone-based, benzotriazole-based, phenyl salicylate-based, or phenyl benzoate-based compound, and is preferably a benzophenone-based compound because it can be contained in a large amount in the composition, and is preferably a triazine-based or benzotriazole-based compound because it can prevent yellowing of a substrate such as polycarbonate. More preferably, the ultraviolet absorbing agent has a maximum absorption wavelength in the range of 240 to 380 nm.
[0073] Examples of the ultraviolet absorber include a mixture of 2-[4-(2-hydroxy-3-dodecyloxy-propyl)oxy-2-hydroxyphenyl]-4,6-[bis(2,4-dimethylphenyl)-1,3,5-triazine] and 2-[4-(2-hydroxy-3-tridecyloxy-propyl)oxy-2-hydroxyphenyl]-4,6-[bis(2,4-dimethylphenyl)-1,3,5-triazine] manufactured by BASF {trade name "Tinuvin (registered trademark) 400"}, 2-[4-(octyl-2-methylethanoate)o Tris[2,4,6-[2-{4-(octyl-2-methylethanoate)oxy-2-hydroxyphenyl}]-1,3,5-triazine]{trade name: Tinuvin 777}, and other commercially available products such as 2-hydroxybenzophenone, 5-chloro-2-hydroxybenzophenone, 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, and 2-hydroxybenzophenone. -Hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-octadecyloxybenzophenone, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, phenyl salicylate, p-tert-butylphenyl salicylate, p-(1,1,3,3-tetramethylbutyl)phenyl salicylate, 3-hydroxyphenyl benzoate, phenylene-1,3-dibenzoate, 2- Examples of the benzotriazole include (2-hydroxy-5'-methylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-5-tert-butylphenyl)benzotriazole, 2-(2-hydroxy-4-octylphenyl)benzotriazole, and 2-(2'-hydroxy-5'-methacryloxyethylphenyl)-2H-benzotriazole. These may be used alone or in combination of two or more.
[0074] <Other components of composition (A1)> The composition (A1) may contain, if necessary, components such as antioxidants, anti-yellowing agents, bluing agents, pigments, leveling agents, defoamers, thickeners, anti-settling agents, antistatic agents and anti-fogging agents.
[0075] [Composition (A2)] The thermosetting resin composition of the present invention is a thermosetting resin composition [hereinafter referred to as "composition (A2)"] that contains a polymer (X1) having a polydimethylsiloxane structure and an active hydrogen group in the main chain or a side chain, and a compound (Y2) having three or more optionally blocked isocyanate groups per molecule.
[0076] <Polymer (X1)> The polymer (X1) having a polydimethylsiloxane structure and an active hydrogen group in the main chain or side chain, which is a component of the composition (A2), is the same as the polymer (X1) in the composition (A1).
[0077] The content of the polymer (X1) in the composition (A2) is preferably 5 to 95 mass%, more preferably 8 to 90 mass%, and even more preferably 10 to 75 mass%, based on the total mass of the polymer (X1) and the compound (Y2). The higher the content, the better the water slipping property of the cured film, and the lower the content, the higher the scratch resistance and hardness of the cured film.
[0078] <Compound (Y2)> The compound (Y2) is a compound having three or more isocyanate groups, which may be blocked, in one molecule. When the composition (A2) is cured, the isocyanate group of the compound (Y2) reacts with the active hydrogen group of the active hydrogen group of the polymer (X1), forming a bond such as a urethane bond between these compounds and the polymer. This increases the crosslink density of the cured product, such as the cured film, and is therefore considered to improve weather resistance and stain resistance. The compound (Y2) is a compound of the compound (Y1), which is a component of the composition (A1), having three or more isocyanate groups, which may be blocked, in one molecule, so a detailed description is omitted.
[0079] The content of compound (Y2) in composition (A2) is preferably 10 to 99 mass%, more preferably 20 to 97 mass%, and even more preferably 95 to 30 mass%, based on the total mass of polymer (X1) and compound (Y2). The higher the content, the higher the scratch resistance and hardness of the cured film, and the lower the content, the higher the water sliding property of the cured film.
[0080] <Inorganic fine particles> The composition (A2) may contain inorganic fine particles such as silica fine particles in the same amount as in the composition (A1) for the same purpose.
[0081] <Other components of composition (A2)> The composition (A2) may contain components other than the polymer (X1) and the compound (Y2). Examples of such components include a compound (Y1) other than the compound (Y2) described in the composition (A1), a compound (Z1), a compound having only one isocyanate group per molecule which may be blocked, a compound having only one active hydrogen group per molecule, a curing accelerator catalyst, an organic solvent, an ultraviolet absorber, a light stabilizer, an antioxidant, an anti-yellowing agent, a bluing agent, a pigment, a leveling agent, an antifoaming agent, a thickener, an anti-settling agent, an antistatic agent, and an anti-fogging agent.
[0082] [Composition (A3)] The thermosetting resin composition of the present invention is a thermosetting resin composition comprising a polymer (X2) [hereinafter referred to as "polymer (X2)] having a polydimethylsiloxane structure and an optionally blocked isocyanate group in the main chain or a side chain, and a compound (Z1) having two or more active hydrogen groups per molecule.
[0083] <Polymer (X2)> The polymer (X2) is a polymer having a polydimethylsiloxane structure and an optionally blocked isocyanate group in the main chain or side chain. In other words, the polymer (X2) needs to contain a polydimethylsiloxane structure in either or both of its main chain or side chain, and an isocyanate group in either or both of its main chain or side chain.
[0084] <Polydimethylsiloxane structure> The polydimethylsiloxane structure contributes to the water sliding property of the cured film formed by the composition (A3) containing the polymer (X2). The isocyanate group reacts with the active hydrogen group of the compound (Z1) to firmly fix the polymer (X2) to the cured film, thereby contributing to the durability of the water sliding property and scratch resistance.
[0085] Methods for introducing a polydimethylsiloxane structure into the polymer (X2) include, as explained for the polymer (X1), (1) a method of copolymerizing a macromonomer (M1) with another monomer, (2) a method of copolymerizing a polydimethylsiloxane having mercapto groups at the α,ω positions with another monomer as a chain transfer agent, (3) a method of copolymerizing an azo compound having a polydimethylsiloxane structure with another monomer, and (4) a method of adding a hydroxyl group of a polydimethylsiloxane having a hydroxyl group at its terminal to the isocyanate group of a polymer having an optionally blocked isocyanate group.
[0086] <Optionally blocked isocyanate group> The isocyanate group which may be blocked in the polymer (X2) can be appropriately deblocked to react with the active hydrogen group of the compound (Z1) having an active hydrogen group to form a bond such as a urethane bond.
[0087] To introduce an isocyanate group which may be blocked into the polymer (X2), a method is preferred in which a monomer having an isocyanate group which may be blocked [hereinafter referred to as "monomer (M3)] is copolymerized with the macromonomer (M1) as another monomer in the method (1) for introducing a polydimethylsiloxane structure. The blocked isocyanate group may be obtained by copolymerizing a monomer having an isocyanate group and blocking the isocyanate group of the resulting copolymer by a known method.
[0088] <Production of Polymer (X2)> Hereinafter, the method (1) for producing the polymer (X2) by copolymerizing the macromonomer (M1) with the monomer (M3) as another monomer will be described.
[0089] <Macromonomer (M1)> The macromonomer (M1) used in the production of the polymer (X2) is the same as that described in the polymer (X1). It is similar to the above.
[0090] The amount of the macromonomer (M1) introduced into the polymer (X2) is preferably 5% by mass or more and less than 70% by mass, more preferably 10% by mass or more and less than 60% by mass, and even more preferably 20% by mass or more and less than 50% by mass. The larger the amount of the macromonomer (M1) introduced, the better the water sliding property of the cured film becomes, and the smaller the amount of unpolymerized macromonomer (M1) can be reduced, so that the transparency of the cured film tends to be better.
[0091] <Monomer (M3)> Monomer (M3) is used to introduce an isocyanate group into polymer (X2). Examples of monomer (M3) include 2-isocyanatoethyl (meth)acrylate, 3-isocyanatopropyl (meth)acrylate, 2-isocyanato-1-methylethyl (meth)acrylate, and methacryloyloxyethoxyethyl isocyanate. The isocyanate group contained in these monomers may be blocked with a blocking agent such as alcohol, phenols, lactam, oxime, alkyl acetoacetate, alkyl malonate, phthalimide, imidazole, hydrogen chloride, hydrogen cyanide, and sodium hydrogen sulfite.
[0092] Specific examples of blocking agents include alcohols such as methanol, ethanol, and benzyl alcohol; phenols such as phenol and cresol; lactams such as caprolactam and butyrolactam; and oximes such as cyclohexanone, oxime, and methyl ethyl ketoxime.
[0093] The amount of isocyanate group introduced in the polymer (X2) is preferably 0.1 mmol / g or more and less than 4.0 mmol / g, more preferably 0.2 mmol / g or more and less than 3.5 mmol / g, and more preferably 0.3 mmol / g or more and less than 3.0 mmol / g. The greater the amount introduced, the more the durability of the cured film improves, and the smaller the amount introduced, the more the water slipping property improves. In the case of a blocked isocyanate, the amount introduced of the isocyanate group is the amount introduced after deblocking.
[0094] <Other monomers> In the production of the polymer (X2), other monomers can be copolymerized in addition to the macromonomer (M1) and the monomer (M3) to the extent that the performance is not impaired. Examples of the other monomers include the same ones as those other than the macromonomer (M1) and the monomer (M2) described in the polymer (X1). Among them, when aromatic vinyl monomers such as styrene, α-methylstyrene, vinyltoluene, vinylnaphthalene, vinylbiphenyl, vinylanthracene, and vinylxylene are contained as monomers constituting the polymer (X2), the polymer (X2) can exhibit particularly good water slipping properties. The aromatic vinyl monomer-derived structural unit is preferably contained in the polymer (X2) in an amount of 30% by mass or more [hereinafter referred to as "polymer (X2-2)"].
[0095] <Initiator> In the production of the polymer (X2), it is preferable to use an initiator when copolymerizing the macromonomer (M1) and the monomer (M3). Examples of the initiator include the same initiators as those described for the polymer (X1).
[0096] The amount of initiator added when producing the polymer (X2) is preferably 0.1% by mass or more and less than 10% by mass, more preferably 0.3% by mass or more and less than 6% by mass, and even more preferably 0.5% by mass or more and less than 3% by mass, based on the total amount of the macromonomer (M1), the monomer (M3), and other monomers. The higher the amount of initiator added, the better the coatability becomes, and the lower the amount, the better the water slipping property tends to be.
[0097] The polymer (X2) can be produced by, for example, a polymerization method such as solution polymerization, bulk polymerization, suspension polymerization, or emulsion polymerization. An initiator may be used in a manner appropriate for each polymerization method.
[0098] <Molecular weight of polymer (X2)> The weight average molecular weight of the polymer (X2) is preferably 5000 to 400000, more preferably 5000 to 300000, and particularly preferably 10000 to 200000. When the weight average molecular weight is less than 400000, the viscosity of the thermosetting resin composition decreases, resulting in good coatability, and when the weight average molecular weight is more than 1000, the polymer (X2) is firmly fixed to the cured film, resulting in improved water sliding properties and scratch resistance. The molecular weight of the polymer (X2) is the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) in terms of standard polystyrene.
[0099] <Content of polymer (X2)> The content of the polymer (X2) in the composition (A3) is preferably 5 to 95 mass%, more preferably 8 to 90 mass%, and even more preferably 10 to 75 mass%, based on the total mass of the polymer (X2) and the compound (Z1). The higher the content, the higher the water slipping property of the cured film tends to be, while the lower the content, the higher the scratch resistance and hardness of the cured film tends to be.
[0100] <Compound (Z1)> The compound (Z1) having two or more active hydrogen groups in one molecule is the same as the compound (Z1) in the composition (A1) described above, and therefore a detailed description thereof will be omitted.
[0101] The content of compound (Z1) in composition (A2) is preferably 3 to 60 mass%, more preferably 5 to 50 mass%, and even more preferably 10 to 45 mass%, based on the total mass of polymer (X1) and compound (Z1). The higher the content, the higher the scratch resistance and hardness of the cured film, and the lower the content, the higher the water sliding property of the cured film.
[0102] <Inorganic fine particles> The composition (A3) may contain inorganic fine particles such as silica fine particles in the same amount as in the composition (A1) for the same purpose.
[0103] <Other components of composition (A3)> The composition (A3) may contain components other than the polymer (X2) and the compound (Z1). Examples of such components include the compound (Y1) described in the composition (A1), a compound having only one isocyanate group per molecule which may be blocked, a compound having only one active hydrogen group per molecule, a curing accelerator catalyst, an organic solvent, an ultraviolet absorber, a light stabilizer, an antioxidant, an anti-yellowing agent, a bluing agent, a pigment, a leveling agent, an antifoaming agent, a thickener, an anti-settling agent, an antistatic agent, and an anti-fogging agent.
[0104] [Composition (A4)] The thermosetting resin composition of the present invention is a thermosetting resin composition comprising a polymer (X2) having a polydimethylsiloxane structure and an optionally blocked isocyanate group in the main chain or a side chain [hereinafter referred to as "polymer (X2)"], a compound (Z1) having two or more active hydrogen groups per molecule, and a compound (Y1) having two or more optionally blocked isocyanate groups per molecule.
[0105] <Polymer (X2)> The polymer (X2) having a polydimethylsiloxane structure and an active hydrogen group in the main chain or side chain, which is a component of the composition (A4), is the same as the polymer (X2) in the composition (A3). Therefore, a detailed description will be omitted.
[0106] The content of the polymer (X2) in the composition (A4) is preferably 5 to 95 mass%, more preferably 8 to 90 mass%, and even more preferably 10 to 75 mass%, based on the total mass of the polymer (X2), the compound (Z1) and the compound (Y1). The higher the content, the higher the water slipping property of the cured film tends to be, while the lower the content, the higher the scratch resistance and hardness of the cured film tends to be.
[0107] <Compound (Z1)> The compound (Z1) having two or more active hydrogen groups in one molecule is the same as the compound (Z1) in the composition (A1) described above, and therefore a detailed description thereof will be omitted.
[0108] The content of compound (Z1) in composition (A4) is preferably 5 to 95 mass%, more preferably 10 to 80 mass%, and even more preferably 15 to 50 mass%, based on the total mass of polymer (X2), compound (Z1) and compound (Y1). The higher the content, the higher the scratch resistance and hardness of the cured film, and the lower the content, the higher the water sliding property of the cured film.
[0109] <Compound (Y1)> The compound (Y1) having two or more optionally blocked isocyanate groups in one molecule is the same as the compound (Y1) in the composition (A1) described above, and therefore a detailed description thereof will be omitted.
[0110] The content of compound (Y1) in composition (A4) is preferably 5 to 95 mass%, more preferably 10 to 80 mass%, and even more preferably 15 to 50 mass%, based on the total mass of polymer (X2), compound (Z1) and compound (Y1). The higher the content, the higher the scratch resistance and hardness of the cured film, and the lower the content, the higher the water sliding property of the cured film.
[0111] <Inorganic fine particles> The composition (A4) may contain inorganic fine particles such as silica fine particles in the same amount as in the composition (A1) for the same purpose.
[0112] <Other components of composition (A4)> The composition (A4) may contain components other than the polymer (X2) and the compounds (Z1) and (Y1). Examples of such components include a compound having only one isocyanate group per molecule which may be blocked, a compound having only one active hydrogen group per molecule, a curing accelerator catalyst, an organic solvent, an ultraviolet absorber, a light stabilizer, an antioxidant, an anti-yellowing agent, a bluing agent, a pigment, a leveling agent, an antifoaming agent, a thickener, an anti-settling agent, an antistatic agent, and an anti-fogging agent.
[0113] [Cured product] The cured product obtained by curing the thermosetting resin composition of the present invention can be obtained, for example, by applying the thermosetting resin composition to a substrate by a known method.
[0114] <Base material> Examples of the substrate include metals such as zinc-plated steel sheet, zinc alloy-plated steel sheet, stainless steel sheet, and tin-plated steel sheet, polymethyl methacrylate resin, polycarbonate resin, polyester resin, polystyrene resin, ABS resin, AS resin, polyamide resin, polyarylate resin, polymethacrylimide resin, and polyallyl diglycol carbonate resin. It is particularly effective in improving the scratch resistance of the surfaces of polymethyl methacrylate resin, polycarbonate resin, polystyrene resin and polymethacrylimide resin.
[0115] <Coating method> The coating on the substrate can be carried out by a known method such as brush coating, gravure coating, die coating, bar coating, spray coating, dip coating, spin coating, curtain coating, etc. If necessary, the thermosetting resin composition can be coated multiple times.
[0116] <Curing method> The temperature for curing the coating composition of the present invention may be appropriately set taking into consideration the heat resistance and thermal deformation property of the substrate, and is preferably from 20° C. to 200° C., more preferably from 60° C. to 150° C. The curing time is preferably from several minutes to several hours.
[0117] <Thickness of the cured film> The thickness of the cured film obtained by curing the thermosetting resin composition of the present invention is preferably 1 to 50 μm, more preferably 1 μm or more from the viewpoint of obtaining the effects of the coating composition of the present invention, and preferably 50 μm or less from the viewpoint of reducing cracks.
[0118] [Laminate] The laminate of the present invention is a laminate having a layer of a cured film obtained by curing the thermosetting resin composition of the present invention on a substrate. The laminate of the present invention has excellent water sliding properties and transparency, and is therefore suitable for use in various lamp lenses and glazing for automobiles, as well as radome parts such as emblems and front grilles on the front surface of electromagnetic wave radar devices, and is particularly suitable for use in millimeter wave radar covers. EXAMPLES
[0119] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited thereto. In the explanation, "parts" refers to "parts by mass." Measurements and evaluations were performed by the following methods.
[0120] [Measurement and evaluation method] <Molecular weight> The molecular weight of the polymer produced in the present invention is a weight average molecular weight (Mw) calculated in terms of standard polystyrene, measured by gel permeation chromatography (GPC) under the following conditions. Equipment: Waters "e2695", Column: Tosoh "TSKgel Super H3000+H4000+H6000" Detector: Differential refractive index detector (RI detector / built-in), Solvent: tetrahydrofuran, Temperature: 40℃, Flow rate: 0.5mL / min, Injection volume: 10μL, Concentration: 0.2% by mass, Calibration sample: monodisperse polystyrene, Calibration method: Polystyrene equivalent
[0121] <Evaluation sample> The thermosetting resin composition was applied to the PMMA side of a two-layer laminate sheet of polymethyl methacrylate (PMMA) and polycarbonate (ShineTech (registered trademark) AW-10U, total thickness 1.0 mm, PMMA layer 60 μm) using a bar coater (#30) so that the coating after curing would be 7 μm thick. Then, the laminate was heated at 110° C. for 30 minutes to produce a laminate in which a cured film of the thermosetting resin composition was formed on the substrate, and the following evaluation was performed on this laminate as an evaluation sample.
[0122] <Transparency> The transparency of the evaluation sample was evaluated by measuring the total light transmittance and the diffuse transmittance (haze value) using a haze meter (SH 7000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS K7136: 2000. The criteria for judging transparency are as follows. ·Judgment criteria 3: Haze value is less than 1%. 2: Haze value is 1% or more and less than 5%. 1: Haze value is 5% or more.
[0123] <Initial hydrophobicity> The initial water sliding property of the evaluation sample was evaluated by measuring the sliding angle of 20 μL of water by the sliding method using a contact angle meter (DM-500, manufactured by Kyowa Interface Science Co., Ltd.). The criteria for judging the initial water sliding property are as follows. ·Judgment criteria 5: The sliding angle of 20 μL of water is greater than 1° and less than 20°. 4: The sliding angle of 20 μL of water is greater than 20° and less than 50°. 3: The sliding angle of 20 μL of water is greater than 50° and less than 70°. 2: The sliding angle of 20 μL of water is greater than 70° and less than 80°. 1: The sliding angle of 20 μL of water is greater than 80°.
[0124] <Water slippage after wet heat test> The evaluation sample was left to stand for 24 hours under conditions of 50°C and 99% humidity, and then the evaluation sample was taken out and water droplets adhering to the surface of the evaluation sample were removed. The water slippage after the wet heat test was evaluated by measuring the sliding angle of 20 μL of water in the same manner as in the evaluation of the initial water slippage. The judging criteria for the water slippage after the wet heat test are as follows. ·Judgment criteria 5: The sliding angle of 20 μL of water is greater than 1° and less than 20°. 4: The sliding angle of 20 μL of water is greater than 20° and less than 50°. 3: The sliding angle of 20 μL of water is greater than 50° and less than 70°. 2: The sliding angle of 20 μL of water is greater than 70° and less than 80°. 1: The sliding angle of 20 μL of water is greater than 80°.
[0125] <Scratch resistance> The evaluation sample was subjected to a flat surface abrasion test using a KASAI scratch tester. Steel wool #000 was placed on the evaluation sample, and 250g / 1.1cm 2 After 20 reciprocating abrasions with a rubbing tester under a load of 10000, the diffuse transmittance (haze value) was measured with a haze meter (SH 7000, manufactured by Nippon Denshoku Industries Co., Ltd.). The scratch resistance was judged based on the value obtained by subtracting the initial haze value from the measured haze value (increased haze value (Δ haze value)). The criteria for judging scratch resistance are as follows: ·Judgment criteria 3: Increased haze value is less than 25%. 2: Increased haze value is 25% or more but less than 40%. 1: Increased haze value is 40% or more.
[0126] <Pencil hardness> The pencil hardness of the evaluation sample was evaluated in accordance with ISO / DIS 15184. After the test, the highest hardness that did not cause any scratches was adopted as the pencil hardness of the cured film. The pencil hardness was evaluated according to the following criteria: ·Judgment criteria 3: F or higher. 2:B~HB. Less than 1:B.
[0127] [Polymer preparation] The preparation method of the polymers used in the examples and comparative examples of the present invention will be described. The polymers (1-1) to (1-4) prepared in the following examples correspond to the polymer (X1), the polymers (2-1) to (2-5) correspond to the polymer (X2), and among them, the polymers (2-1) to (2-4) correspond to the polymer (X2-2). The polymer (3-1) prepared in the following examples is a polymer that does not have a polydimethylsiloxane structure, and does not correspond to either the polymer (X1) or the polymer (X2).
[0128] <Preparation of Polymer (1-1)> Into a 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer, 18 g of toluene, 18.5 g of propylene glycol monomethyl ether acetate, 31.25 g of styrene, 0.75 g of acrylic acid, 3.0 g of 2-hydroxyethyl methacrylate, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were placed. In addition, 18 g of toluene, 18.5 g of propylene glycol monomethyl ether acetate, 31.25 g of styrene, 0.75 g of acrylic acid, 3.0 g of 2-hydroxyethyl methacrylate, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were placed in the dropping funnel. Next, the flask was placed in an oil bath, stirring was started under a nitrogen atmosphere, and the internal temperature was raised to 85°C. Thirty minutes after the internal temperature reached 85°C, the raw materials from the dropping funnel were dropped over 2 hours, and the mixture was held for 1 hour, after which 0.1 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (Perocta O, manufactured by NOF Corp.) was added, and 1 hour later, 0.1 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (Perocta O, manufactured by NOF Corp.) was added, and the mixture was allowed to react for 5 hours before being cooled to prepare a polymer (1-1) solution. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and active hydrogen group (hydroxyl group) concentration of the polymer (1-1) are shown in Table 1.
[0129] <Preparation of Polymer (1-2)> Into a 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer, 36.5 g of methyl isobutyl ketone, 28.25 g of styrene, 0.75 g of acrylic acid, 6.0 g of 2-hydroxyethyl methacrylate, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were placed. In addition, 36.5 g of methyl isobutyl ketone, 28.25 g of styrene, 0.75 g of acrylic acid, 6.0 g of 2-hydroxyethyl methacrylate, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added to the dropping funnel. The other operations were the same as those for preparing polymer (1-1), and polymer (1-2) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and active hydrogen group (hydroxyl group) concentration of polymer (1-2) are shown in Table 1.
[0130] <Preparation of Polymer (1-3)> Into a 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer, 36.5 g of methyl isobutyl ketone, 28.25 g of styrene, 0.75 g of acrylic acid, 6.0 g of 2-hydroxyethyl methacrylate, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0711), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were placed. In addition, 36.5 g of methyl isobutyl ketone, 28.25 g of styrene, 0.75 g of acrylic acid, 6.0 g of 2-hydroxyethyl methacrylate, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0711), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added to the dropping funnel. The other operations were the same as those for preparing polymer (1-1), and polymer (1-3) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and active hydrogen group (hydroxyl group) concentration of polymer (1-3) are shown in Table 1.
[0131] <Preparation of Polymer (1-4)> Into a 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer, 36.5 g of methyl isobutyl ketone, 28.25 g of styrene, 0.75 g of acrylic acid, 6.0 g of 4-hydroxybutyl acrylate, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were placed. In addition, 36.5 g of methyl isobutyl ketone, 28.25 g of styrene, 0.75 g of acrylic acid, 6.0 g of 4-hydroxybutyl acrylate, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added to the dropping funnel. The other operations were the same as those for preparing polymer (1-1), and polymer (1-4) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and active hydrogen group (hydroxyl group) concentration of polymer (1-4) are shown in Table 1.
[0132] <Preparation of Polymer (2-1)> A 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer was charged with 36.5 g of toluene, 29.0 g of styrene, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 6.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz (registered trademark) AOI), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxyate (manufactured by NOF Corp., Perocta O). In addition, 36.5 g of toluene, 29.0 g of styrene, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 6.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added to the dropping funnel. The other operations were the same as those for preparing polymer (1-1), and polymer (2-1) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and isocyanate group concentration of polymer (2-1) are shown in Table 1.
[0133] <Preparation of Polymer (2-2)> Into a 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer, 37.0 g of toluene, 29.0 g of styrene, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 6.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.5 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxyate (manufactured by NOF Corp., Perocta O) were placed. In addition, 37.0 g of toluene, 29.0 g of styrene, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 6.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.5 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added to the dropping funnel. The other operations were the same as those for preparing polymer (1-1), and polymer (2-2) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and isocyanate group concentration of polymer (2-2) are shown in Table 1.
[0134] <Preparation of Polymer (2-3)> Into a 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer, 36.5 g of toluene, 42.0 g of styrene, 7.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 6.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxyate (manufactured by NOF Corp., Perocta O) were placed. In addition, 36.5 g of toluene, 42.0 g of styrene, 3.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 6.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added to the dropping funnel. The other operations were the same as those for the preparation of polymer (1-1), and polymer (2-3) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and isocyanate group concentration of polymer (2-3) are shown in Table 1.
[0135] <Preparation of Polymer (2-4)> Into a 300 ml five-neck separable flask equipped with a stirrer, a dropping funnel, a cooling condenser, and a thermometer, 36.5 g of toluene, 34.0 g of styrene, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 1.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxyate (manufactured by NOF Corp., Perocta O) were placed. In addition, 36.5 g of toluene, 34.0 g of styrene, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 1.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added to the dropping funnel. The other operations were the same as those for the preparation of polymer (1-1), and polymer (2-4) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and isocyanate group concentration of polymer (2-4) are shown in Table 1.
[0136] <Preparation of Polymer (2-5)> In a 300 ml five-necked separable flask equipped with a stirrer, dropping funnel, cooling condenser, and thermometer, 36.5 g of toluene, 29.0 g of isobornyl methacrylate, 20.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 6.0 g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were added. In addition, 36.5 g of toluene, 29.0 g of isobornyl methacrylate, 10.0 g of polydimethylsiloxane having a methacryloyl group at one end (manufactured by JNC, Silaplane FM-0721), 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz A Into the reaction mixture were added 6.0 g of 2-ethylhexaneperoxy acid (OI) and 0.25 g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (Perocta O, manufactured by NOF Corp.). The other operations were the same as those for preparing polymer (1-1), and polymer (2-5) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and isocyanate group concentration of polymer (2-5) are shown in Table 1.
[0137] <Preparation of Polymer (3-1)> 36.5g of toluene, 49.0g of styrene, 6.0g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were placed in a 300ml five-neck separable flask equipped with a stirrer, dropping funnel, cooling condenser, and thermometer. In addition, 36.5g of toluene, 39.0g of styrene, 6.0g of 2-(acryloyloxy)ethyl isocyanate (manufactured by Showa Denko, Karenz AOI), and 0.25g of 1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid (manufactured by NOF Corp., Perocta O) were placed in the dropping funnel. The other operations were the same as in the preparation of polymer (1-1), and polymer (3-1) was prepared. The solid content and solid content ratio of the obtained solution, as well as the weight average molecular weight (Mw) and isocyanate group concentration of the polymer (3-1) are shown in Table 1.
[0138] [Table 1]
[0139] The abbreviations in Table 1 are as follows. FM-0721: JNC Silaplane FM-0721 (catalog number average molecular weight 5000) FM-0711: JNC Silaplane FM-0711 (catalog number average molecular weight 1000) HEMA: 2-hydroxyethyl methacrylate 4-HBA: 4-hydroxybutyl acrylate AOI: Showa Denko Karenz AOI (2-isocyanatoethyl acrylate) St: styrene IBXMA: Isobornyl methacrylate AA: Acrylic acid Perocta O: NOF Corp. Perocta O (1,1,3,3-tetramethylbutyl 2-ethylhexaneperoxy acid)
[0140] [Preparation of inorganic particles] <Preparation of inorganic fine particles having mercapto groups (C-1)> A flask equipped with a stirrer was charged with 12 g of 3-mercaptopropyltrimethoxysilane manufactured by Tokyo Chemical Industry Co., Ltd., 6 g of distilled water, and 21 g of tetrahydrofuran, and the mixture was stirred at 30° C. for 3 hours to carry out a hydrolysis reaction. Next, this reaction liquid (silanol solution) was transferred to a dropping funnel. Next, the dropping funnel was attached to a 2000 ml five-necked separable flask equipped with a stirrer, a cooling condenser, and a thermometer, and 1000 g of methyl isobutyl ketone-dispersed silica sol (product name: "MIBK-ST", solvent: methyl isobutyl ketone, solid content concentration 30 mass%, average particle size: 15 nm) manufactured by Nissan Chemical Industries was charged into the flask, and the temperature was raised to 70° C. The reaction liquid (silanol solution) in the dropping funnel was dropped over 2 hours, and after the end of the dropping, the reaction was carried out for another hour to obtain a dispersion liquid of inorganic fine particles (C-1) having mercapto groups.
[0141] [Example 1] As the polymer (X1), 158.6 g (solid content 92.0 g) of the polymer (1-1), 10.67 g (solid content 8.0 g) of Duranate 22A-75P (manufactured by Asahi Kasei) as a compound (Y2) having three or more blocked isocyanate groups in one molecule, 0.05 g of dibutyltin dilaurate as a catalyst, and 330.9 g of a mixture of cyclohexanone and methyl isobutyl ketone in a mass ratio of 60:40 as an organic solvent were mixed to prepare a thermosetting resin composition with a solid content concentration of 20% by mass. Using the obtained thermosetting resin composition, an evaluation sample (laminate) was prepared by the above-mentioned method, and the evaluation results are shown in Table 2.
[0142] [Examples 2 to 14, Comparative Examples 1 to 3] Thermosetting resin compositions were prepared and evaluated in the same manner as in Example 1, except that the raw materials were mixed so as to obtain the solid content mass ratios shown in Tables 2 to 4. The evaluation results are shown in Tables 2 to 4.
[0143] [Table 2]
[0144] The abbreviations in Table 2 are as follows: Functional group concentration: Concentration of hydroxyl or isocyanate groups Amount: Solid content if solvent is included 22A-75P: Asahi Kasei Duranate 22A-75P HDI: Hexamethylene diisocyanate DBTDL: Dibutyltin dilaurate Overall evaluation: Total value of the evaluations of transparency, initial water slippage, water slippage after wet heat test, pencil hardness and scratch resistance
[0145] [Table 3]
[0146] The abbreviations in Table 3 are as follows: Functional group concentration: Concentration of hydroxyl or isocyanate groups Amount: Solid content if solvent is included C-1090: Kuraray Polyol C-1090 made by Kuraray HPE 1170B:Basonol HPE 1170B manufactured by BASF DBTDL: Dibutyltin dilaurate Overall evaluation: Total value of the evaluations of transparency, initial water slippage, water slippage after wet heat test, pencil hardness and scratch resistance
[0147] [Table 4]
[0148] The abbreviations in Table 4 are as follows: Functional group concentration: Concentration of hydroxyl or isocyanate groups Amount: Solid content if solvent is included C-1090: Kuraray Polyol C-1090 made by Kuraray HPE 1170B:Basonol HPE 1170B manufactured by BASF 22A-75P: Asahi Kasei Duranate 22A-75P DBTDL: Dibutyltin dilaurate Tinuvin 400: BASF Tinuvin 400 Tinuvin 123: BASF Tinuvin 123
[0149] As can be seen from the evaluation results in Tables 2 to 4, the cured films obtained from the thermosetting resin compositions of the Examples had excellent transparency, and both the initial water slippage and the water slippage after the wet heat test were good. In contrast, the cured film obtained from the thermosetting resin composition of Comparative Example 1 had good initial water sliding property, but the water sliding property after the wet heat test was low. The cured film obtained from the thermosetting resin composition of Comparative Example 2 did not exhibit water sliding property because a polymer not containing a polydimethylsiloxane structure was used. The cured film of the thermosetting resin composition of Comparative Example 3 did not exhibit water sliding property because it did not contain the polymer (X2). [Industrial Applicability]
[0150] Since the thermosetting resin composition of the present invention has excellent water sliding properties and transparency, it is suitable for use as a hard coat on the surface of various lamp lenses and glazing for automobiles, as well as radome parts such as emblems and front grilles on the front surface of electromagnetic wave radar devices, and is particularly suitable for use as a hard coat on millimeter wave radar covers.
Claims
1. A thermosetting resin composition comprising: a polymer (X1) having a polydimethylsiloxane structure and an active hydrogen group in the main chain or a side chain; a compound (Y1) having two or more optionally blocked isocyanate groups per molecule; and a compound (Z) having five or more hydroxyl groups per molecule and having a dendritic branched structure.
2. A thermosetting resin composition comprising: a polymer (X1) having a polydimethylsiloxane structure and an active hydrogen group in a side chain; and a compound (Y2) having three or more optionally blocked isocyanate groups per molecule.
3. The thermosetting resin composition according to claim 1 or 2, further comprising inorganic fine particles.
4. 4. The thermosetting resin composition according to claim 3, wherein the inorganic fine particles are surface-modified with a compound having any one of a mercapto group, a hydroxyl group, and an isocyanate group.
5. A cured product obtained by curing the thermosetting resin composition according to any one of claims 1 to 4.
6. A laminate comprising a substrate and a layer comprising the cured product according to claim 5.
Citation Information
Patent Citations
Polishing agent
JP2001172576A
Plastic member readily removing living pollutant
JP2002293969A
Sheet
JP2003072012A
Leveling agent for filling flaw on coated film surface and method for lustering coated film surface using the same
JP2005082772A
Multi-branched polyether polyol and urethane resin composition
JP2006282698A