Packaging material
A gas barrier laminate with a polypropylene base, polyvinyl alcohol resin, and metal oxide layers addresses the need for recyclable and gas-tight monomaterial packaging by ensuring heat resistance and smooth adhesion, enhancing recyclability and barrier properties.
Patent Information
- Application Number
- JP2024118533
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-07-29
AI Technical Summary
There is a demand for monomaterial packaging solutions with improved recyclability and gas barrier properties, particularly in flexible packaging materials, to address environmental concerns and enhance recycling efficiency.
A gas barrier laminate structure comprising a polypropylene base layer, a first polyvinyl alcohol resin layer, and a metal oxide layer, with optional second polyvinyl alcohol resin layer, is developed to achieve excellent gas barrier properties and recyclability, using propylene homopolymer film for heat resistance and incorporating specific surface roughness and mass ratios to ensure adhesion and smoothness.
The laminate provides a monomaterial packaging solution with enhanced gas barrier properties and recyclability, capable of withstanding heat sterilization treatments while maintaining structural integrity and reducing material costs.
Smart Images

Figure 2024133400000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a gas barrier laminate and a packaging material using the same. [Background technology]
[0002] 2. Description of the Related Art Laminates (soft packaging materials) that include a biaxially oriented PET (polyethylene terephthalate) film having excellent heat resistance and toughness as a base film and a polyolefin film such as polyethylene or polypropylene as a sealant layer are known (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-178357 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, due to the growing environmental awareness triggered by the problem of marine plastic waste, there is a demand for further efficient sorting and recovery of plastic materials and recycling. In other words, even for soft packaging materials, which have traditionally been made high-performance by combining various different materials, there is a demand for mono-materialization.
[0005] The present disclosure provides a gas barrier laminate that is useful for realizing excellent recyclability of a packaging material and has excellent gas barrier properties. The present disclosure also provides a packaging material using the gas barrier laminate. [Means for solving the problem]
[0006] A gas barrier laminate according to one aspect of the present disclosure has a laminate structure including a polypropylene-based base layer, a first polyvinyl alcohol-based resin layer, and a metal oxide layer in this order, and the mass per unit area of the first polyvinyl alcohol-based resin layer is 0.5 to 2.5 g / m. 2 According to this gas barrier laminate, since the first polyvinyl alcohol-based resin layer is interposed between the polypropylene-based base layer and the metal oxide layer, excellent gas barrier properties can be achieved even if the surface of the polypropylene-based base layer is not necessarily highly smooth. From the viewpoint of achieving better gas barrier properties, the surface roughness Sa of the first polyvinyl alcohol-based resin layer is preferably 0.2 μm or less, more preferably 0.1 μm or less.
[0007] The present inventors have developed a gas barrier laminate that is used in combination with a sealant layer to form a packaging material and can realize a mono-material packaging material with excellent recyclability. In order to realize a mono-material packaging material including a non-oriented polypropylene film (CPP film) that is widely used as a sealant film, it is necessary to use a polypropylene-based film (PP-based film) as the base layer of the gas barrier laminate. However, in consideration of the heat resistance of the packaging material, it is not the case that any type of PP-based film can be used, and it is useful to use a propylene monopolymer film that has excellent heat resistance compared to other PP-based films. The packaging material may be subjected to heat sterilization treatment such as boiling treatment or retort treatment while containing food, etc., and heat resistance may be required in some cases.
[0008] However, according to the evaluation tests conducted by the present inventors, a propylene monopolymer film has a drawback in that its surface is easily vein-like, and sufficient barrier properties cannot be achieved even when a metal oxide layer (gas barrier layer) is directly formed on the surface of the propylene monopolymer film. Therefore, by interposing a polyvinyl alcohol-based resin layer between the propylene monopolymer film as a base layer and the metal oxide layer, the inventors have developed a gas barrier laminate that has excellent gas barrier properties and is useful for obtaining a mono-material packaging material.
[0009] From the viewpoint of achieving excellent heat resistance of the gas barrier laminate, as described above, the polypropylene-based base layer is preferably a propylene monopolymer layer.
[0010] The gas barrier laminate according to the present disclosure may further include a second polyvinyl alcohol-based resin layer sandwiching a metal oxide layer with the first polyvinyl alcohol-based resin layer. By adopting a configuration in which the metal oxide layer is sandwiched between the first and second polyvinyl alcohol-based resin layers, even more excellent gas barrier properties can be achieved. From the viewpoint of adhesion to the metal oxide layer and maintaining gas barrier properties, the second polyvinyl alcohol-based resin layer may contain a silane compound. The mass ratio of the silane compound to the mass of the second polyvinyl alcohol-based resin layer is, for example, 0.05 to 0.95.
[0011] A packaging material according to one aspect of the present disclosure includes the gas barrier laminate and a polypropylene-based sealant layer provided on the surface of the gas barrier laminate, and the total mass ratio of the polypropylene-based base layer and the polypropylene-based sealant layer is 85% by mass or more based on the total mass of the packaging material, and may be 90% by mass or more or 95% by mass or more depending on the thickness of the polypropylene-based sealant layer. According to this packaging material, the gas barrier laminate and the polypropylene-based sealant layer can be used in combination to realize a mono-material packaging material. In the present disclosure, a mono-material packaging material refers to a packaging material in which the mass ratio of a specific material (polypropylene-based material) is 85% by mass or more (preferably 90% by mass or more or 95% by mass or more). Effect of the Invention
[0012] According to the present disclosure, there is provided a gas barrier laminate that is useful for realizing excellent recyclability of a packaging material and has excellent gas barrier properties. According to the present disclosure, there is provided a packaging material using the gas barrier laminate. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a gas barrier laminate according to the present disclosure. [Diagram 2] 2(a) and 2(b) are cross-sectional views each showing a schematic diagram of a modified example of the gas barrier laminate shown in FIG. [Diagram 3] FIG. 3 is a cross-sectional view that typically shows a packaging material using the gas barrier laminate shown in FIG. [Figure 4] FIG. 4 is a cross-sectional view that illustrates a schematic diagram of another embodiment of the gas barrier laminate according to the present disclosure. [Diagram 5] FIG. 5 is a cross-sectional view that illustrates a schematic diagram of another embodiment of a packaging material according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the present disclosure will be described in detail with reference to the drawings as needed. In the drawings, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0015] <Gas barrier laminate> Fig. 1 is a schematic cross-sectional view showing a gas barrier laminate according to this embodiment. The gas barrier laminate 10 shown in Fig. 1 has a laminate structure including a base layer 1, a first polyvinyl alcohol-based resin layer 3a, a metal oxide layer 5, and a second polyvinyl alcohol-based resin layer 3b, in this order.
[0016] (base material layer) The base layer 1 is made of a polypropylene-based resin. Examples of polypropylene-based resins include propylene homopolymers, random copolymers, and block copolymers. When heat resistance is required for the base layer 1, the polypropylene-based resin is preferably a propylene homopolymer. However, as described above, a propylene homopolymer film has a drawback in that its surface is likely to become vein-like. The surface roughness Sa of the vein-like film surface is, for example, more than 0.2 μm and may be 0.21 to 0.5 μm.
[0017] In this disclosure, the surface roughness Sa of each layer refers to a value measured under the following conditions using a three-dimensional non-contact surface shape measurement system (Vertscan R3300h Lite, manufactured by Ryoka Systems Co., Ltd.). Measurement mode: Phase Scan speed: 4μm / sec Scan range: 10 / -20μm Scan count: 1 Interpolation: Fully Interpolated Surface correction: 4th order -Tube lens: 1x Objective lens: 5x
[0018] By using a propylene homopolymer film as the base layer 1, the gas barrier laminate 10 can be made to withstand heat sterilization treatments such as boiling and retort treatment. The temperature for boiling is about 60 to 100°C, and the temperature for retort treatment is about 105 to 140°C.
[0019] The film constituting the base layer 1 may be a stretched film or a non-stretched film. However, from the viewpoints of impact resistance, heat resistance, water resistance, dimensional stability, etc., the film constituting the base layer 1 may be a stretched film. The stretching method is not particularly limited, and any method may be used as long as it can provide a dimensionally stable film, such as stretching by inflation, uniaxial stretching, or biaxial stretching.
[0020] The thickness of the base layer 1 is not particularly limited, but from the viewpoint of obtaining excellent impact resistance and excellent gas barrier properties, it can be 10 to 100 μm, and may be 15 to 30 μm. The film constituting the base layer 1 may be subjected to various pretreatments such as corona treatment, plasma treatment, and frame treatment on the lamination surface F1 of the film constituting the base layer 1, as long as the barrier performance is not impaired, or may be provided with a coating layer 1a (adhesion layer) for improving adhesion (see FIG. 2(a)). In addition, a copolymer layer 1b may be provided on the outer surface F2 of the base layer 1. A specific example of the resin constituting the polymer layer 1c is a copolymer of propylene and another monomer. The other monomer is, for example, at least one of ethylene and butene.
[0021] The polypropylene-based resin constituting the base layer 1 may contain additives such as antistatic agents, UV absorbers, plasticizers, slipping agents, etc., as necessary. From the viewpoint of achieving a high degree of mono-materiality in the gas barrier laminate 10 and the packaging material 50 using the same, the mass ratio of the polypropylene-based resin in the base layer 1 is preferably 90 mass% or more, and more preferably 95 mass% or more.
[0022] (First polyvinyl alcohol-based resin layer) The resin constituting the first polyvinyl alcohol-based resin layer 3a may be any resin having a vinyl alcohol unit obtained by saponifying a vinyl ester unit, such as polyvinyl alcohol (PVA) or ethylene-vinyl alcohol copolymer (EVOH). From the viewpoints of heat resistance and gas barrier properties, EVOH is preferably used.
[0023] Examples of PVA include resins obtained by homopolymerizing vinyl esters such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, and vinyl versatate, followed by saponification.
[0024] The PVA may be a copolymerized or post-modified modified PVA. The copolymerized modified PVA can be obtained, for example, by copolymerizing a vinyl ester with an unsaturated monomer copolymerizable with the vinyl ester, followed by saponification. The post-modified PVA can be obtained by copolymerizing an unsaturated monomer with the PVA obtained by saponifying the vinyl ester in the presence of a polymerization catalyst. The amount of modification in the modified PVA can be less than 50 mol% from the viewpoint of exhibiting sufficient gas barrier properties, and can be 10 mol% or more from the viewpoint of obtaining the effect of modification.
[0025] Examples of the unsaturated monomer include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxyl group-containing α-olefins such as 3-buten-1-ol, 4-pentyn-1-ol, and 5-hexen-1-ol; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, and undecylenic acid; nitriles such as acrylonitrile and methacrylonitrile; amides such as diacetone acrylamide, acrylamide, and methacrylamide; and ethylene. Examples of suitable unsaturated monomers include olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid; vinyl compounds such as alkyl vinyl ether, dimethyl allyl vinyl ketone, N-vinyl pyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxane, glycerin monoallyl ether, and 3,4-diacetoxy-1-butene; vinylidene chloride, 1,4-diacetoxy-2-butene, vinylene carbonate, polyoxypropylene, and polyoxypropylene vinylamine. From the viewpoint of gas barrier properties, the unsaturated monomer may be an olefin, and may in particular be ethylene.
[0026] Examples of the polymerization catalyst include radical polymerization catalysts such as azobisisobutyronitrile, benzoyl peroxide, lauryl peroxide, etc. The polymerization method is not particularly limited, and bulk polymerization, emulsion polymerization, solvent polymerization, etc. can be adopted.
[0027] The polymerization degree of PVA is preferably 300 to 3000. If the polymerization degree is less than 300, the barrier property is likely to decrease, and if it exceeds 3000, the viscosity is too high and the coating suitability is likely to decrease. The saponification degree of PVA is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 99 mol% or more. The saponification degree of PVA may be 100 mol% or less, or 99.9 mol% or less. The polymerization degree and saponification degree of PVA can be measured according to the method described in JIS K 6726 (1994).
[0028] EVOH is generally obtained by saponifying a copolymer of ethylene and an acid vinyl ester such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, or vinyl versatate.
[0029] The degree of polymerization of EVOH is preferably 300 to 3000. If the degree of polymerization is less than 300, the barrier property is likely to decrease, and if it exceeds 3000, the viscosity is too high and the coating suitability is likely to decrease. The degree of saponification of the vinyl ester component of EVOH is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 99 mol% or more. The degree of saponification of EVOH may be 100 mol% or less, or 99.9 mol% or less. The degree of saponification of EVOH is determined by nuclear magnetic resonance (1H-NMR) measurement, from the peak area of hydrogen atoms contained in the vinyl ester structure and the peak area of hydrogen atoms contained in the vinyl alcohol structure.
[0030] The ethylene unit content of EVOH is, for example, 10 mol% or more, more preferably 15 mol% or more, even more preferably 20 mol% or more, and particularly preferably 25 mol% or more. The ethylene unit content of EVOH is preferably 65 mol% or less, more preferably 55 mol% or less, and even more preferably 50 mol% or less. When the ethylene unit content is 10 mol% or more, the gas barrier property or dimensional stability can be maintained well under high humidity. On the other hand, when the ethylene unit content is 65 mol% or less, the gas barrier property can be improved. The ethylene unit content of EVOH can be determined by NMR method.
[0031] The saponification can be carried out with an alkali or an acid, but from the viewpoint of the saponification rate, an alkali can be used. Examples of the alkali include alkali metal oxides such as sodium hydroxide and potassium hydroxide, and alkali metal alkoxides such as sodium ethylate, potassium ethylate, and lithium methylate.
[0032] The mass per unit area of the first polyvinyl alcohol-based resin layer 3a is 0.5 to 2.5 g / m 2 and 0.5 to 2.0 g / m 2 Or 0.5 to 1.5 g / m 2 This mass may be 0.5 g / m 2 If the mass is 2.5 g / m or more, even if the lamination surface F1 of the base layer 1 is insufficiently smooth, the surface F3 of the first polyvinyl alcohol-based resin layer 3a can be formed sufficiently smooth, and the metal oxide layer 5 having excellent gas barrier properties can be formed on the surface F3. 2 It is advantageous in terms of realizing a monomaterial of polypropylene resin and reducing material costs to be equal to or less than this. From the same viewpoint as the mass per unit area, the thickness of the first polyvinyl alcohol resin layer 3a is, for example, 0.4 to 2.0 μm, and may be 0.4 to 1.7 μm or 0.4 to 1.3 μm. The thickness of the resin layer can be calculated based on the mass per unit area of the resin layer and the density of the resin.
[0033] The surface roughness Sa of the surface F3 of the first polyvinyl alcohol-based resin layer 3a is, for example, 0.2 μm or less, and may be 0.01 to 0.1 μm or 0.02 to 0.1 μm. When the surface roughness Sa of the surface F3 is 0.2 μm or less, a metal oxide layer 5 having excellent gas barrier properties can be formed on the surface F3. On the other hand, when the surface roughness Sa of the surface F3 is 0.01 μm or more, the adhesion between the first polyvinyl alcohol-based resin layer 3a and the metal oxide layer 5 can be improved due to the anchor effect, compared to when the surface roughness Sa is less than 0.01 μm.
[0034] (Metal oxide layer) The metal oxide layer 5 has gas barrier properties. Examples of metal oxides include silicon oxide (SiOx) and aluminum oxide (AlOx). By using these metal oxides, high gas barrier properties can be obtained while keeping the thickness low. From the viewpoint of excellent tensile elongation during processing, the metal oxide layer 5 may be composed of silicon oxide.
[0035] The thickness of the metal oxide layer 5 is, for example, 5 to 100 nm, and may be 10 to 50 nm or 20 to 40 nm. When the thickness of the metal oxide layer 5 is 5 nm or more, sufficient gas barrier properties can be obtained, while when the thickness is 100 nm or less, the occurrence of cracks due to deformation caused by internal stress of the metal oxide layer 5 is suppressed, and excellent gas barrier properties can be maintained.
[0036] (Second polyvinyl alcohol-based resin layer) With regard to the polyvinyl alcohol-based resin constituting the second polyvinyl alcohol-based resin layer 3b, the description of the first polyvinyl alcohol-based resin layer 3a can be referred to.
[0037] The second polyvinyl alcohol-based resin layer 3b may contain a silane compound. Examples of the silane compound include tetraalkoxysilanes such as tetramethoxysilane and tetraethoxysilane, reactive group-containing trialkoxysilanes such as glycidoxypropyltrimethoxysilane and acryloxypropyltrimethoxysilane, and silazanes such as hexamethyldisilazane. Examples of the silane compound include compounds generally used as silane coupling agents and polysiloxane compounds having siloxane bonds.
[0038] The mass ratio of the silane compound to the mass of the second polyvinyl alcohol resin layer 3b is, for example, 0.05 to 0.95, and may be 0.1 to 0.8 or 0.3 to 0.7, from the viewpoint of maintaining adhesion to the metal oxide layer and gas barrier properties.
[0039] The thickness of the second polyvinyl alcohol-based resin layer 3b is, for example, 0.1 to 1.0 μm, and may be 0.1 to 0.8 μm or 0.2 to 0.7 μm. When the thickness is 0.1 μm or more, excellent gas barrier properties can be achieved and the gas barrier properties are sufficiently maintained for a long period of time. On the other hand, when the thickness is 1.0 μm or less, it is advantageous in terms of realizing a monomaterial of polypropylene-based resin and reducing material costs.
[0040] <Method of manufacturing gas barrier laminate> The gas barrier laminate 10 is produced, for example, through a step of forming a first polyvinyl alcohol-based resin layer 3a on a base layer 1, a step of forming a metal oxide layer 5 on the first polyvinyl alcohol-based resin layer 3a, and a step of forming a second polyvinyl alcohol-based resin layer 3b on the metal oxide layer 5.
[0041] (Step of forming first polyvinyl alcohol-based resin layer) In this step, a coating liquid containing a polyvinyl alcohol-based resin and a liquid medium can be used. The coating liquid can be obtained, for example, by dissolving a powder of a polyvinyl alcohol-based resin obtained by synthesis in a liquid medium. Examples of the liquid medium include water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyhydric alcohols such as trimethylolpropane, and amines such as ethylenediamine and diethylenetriamine. These may be used alone or in combination of two or more. From the viewpoint of reducing environmental load, water can be used as the liquid medium. In this case, the coating liquid can be obtained by dissolving a powder of a polyvinyl alcohol-based resin in water at a high temperature (for example, 80°C).
[0042] The content of polyvinyl alcohol resin (solid content) in the coating liquid can be 3 to 20% by mass in order to maintain good coating properties. The coating liquid may contain additives such as isocyanate and polyethyleneimine to improve adhesion. The coating liquid may also contain additives such as preservatives, plasticizers (alcohol, etc.), and surfactants.
[0043] The coating liquid can be applied to the base layer 1 by any appropriate method. The coating liquid can be applied by a wet film formation method using, for example, a gravure coater, a dip coater, a reverse coater, a wire bar coater, a die coater, etc. The application temperature and drying temperature of the coating liquid are not particularly limited and can be, for example, 50°C or higher.
[0044] The first polyvinyl alcohol-based resin layer 3a may be formed on the substrate layer 1 by an extrusion method. In this case, multi-layer extrusion using a T-die may be adopted. Examples of adhesives that can be used during extrusion include two-liquid curing polyurethane adhesives in which a base material such as polyester polyol, polyether polyol, or acrylic polyol is reacted with a difunctional or higher aromatic or aliphatic isocyanate compound as a curing agent. The adhesive component may be applied to the substrate layer 1 and then dried to form an adhesive layer on the substrate layer 1 in advance. When a polyurethane adhesive is used, the reaction between the hydroxyl group of the base material and the isocyanate group of the curing agent proceeds by aging for 4 days or more at 40°C after application, thereby enabling strong adhesion. The thickness of the adhesive layer may be 1 to 50 μm, and may be 3 to 20 μm, from the viewpoints of adhesion, followability, processability, and the like.
[0045] (Step of forming a metal oxide layer) The metal oxide layer 5 can be formed, for example, by vacuum deposition. In the vacuum deposition, physical vapor deposition or chemical vapor deposition can be used. Examples of physical vapor deposition include, but are not limited to, vacuum deposition, sputtering, and ion plating. Examples of chemical vapor deposition include, but are not limited to, thermal CVD, plasma CVD, and photo CVD.
[0046] In the vacuum film formation, the resistance heating vacuum deposition method, the EB (Electron Beam) heating vacuum deposition method, the induction heating vacuum deposition method, the sputtering method, the reactive sputtering method, the dual magnetron sputtering method, the plasma enhanced chemical vapor deposition method (PECVD method), and the like are particularly preferably used. However, in terms of productivity, the vacuum deposition method is currently the most excellent. As the heating means for the vacuum deposition method, it is preferable to use any one of the electron beam heating method, the resistance heating method, and the induction heating method.
[0047] In the case of the sputtering method, a negative potential gradient is generated in the target, which is the cathode, and Ar + The ions receive potential energy and collide with the target. Here, even if plasma is generated, sputtering cannot be performed unless a negative self-bias potential is generated. Therefore, MW (Micro Wave) plasma is not suitable for sputtering because it does not generate a self-bias. However, in the PECVD method, chemical reactions and deposition processes proceed by utilizing gas phase reactions in the plasma, making it possible to generate films even without a self-bias, so MW plasma can be used.
[0048] (Step of forming second polyvinyl alcohol-based resin layer) In this step, a coating liquid can be used in the same manner as in the step of forming the first polyvinyl alcohol-based resin layer 3a. For the coating liquid, the contents described in the section on the step of forming the first polyvinyl alcohol-based resin layer 3a can be referred to.
[0049] The coating liquid for forming the second polyvinyl alcohol-based resin layer 3b may contain a silane compound. The content of the silane compound in the coating liquid may be adjusted so that the second polyvinyl alcohol-based resin layer 3b contains a desired amount of the silane compound. When the coating liquid contains a silane compound, the coating liquid may further contain an acid catalyst, an alkali catalyst, a photopolymerization initiator, etc.
[0050] <Packaging material> 3 includes a gas barrier laminate 10 and a polypropylene-based sealant layer 20 provided on the inner surface 10F of the gas barrier laminate 10. Based on the total mass of the packaging material 50, the combined mass ratio of the base layer 1 and the polypropylene-based sealant layer 20 is 85 mass% or more (preferably 90 mass% or more or 95 mass% or more), and the packaging material 50 is a mono-material.
[0051] The gas barrier laminate 10 may be bonded to the polypropylene-based sealant layer 20 using, for example, an adhesive (not shown). The adhesive may contain, for example, linear low-density polyethylene (LLDPE), polyurethane, polypropylene, ethylene-unsaturated ester copolymer resin, or polyester-based copolymer resin. The thickness of the adhesive layer may be, for example, about 1 to 5 μm. A specific example of the polypropylene-based sealant layer 20 is, for example, an unstretched polypropylene film (CPP film). The thickness of the polypropylene-based sealant layer 20 is, for example, 10 to 100 μm.
[0052] Although the embodiment of the present disclosure has been described in detail above, the present invention is not limited to the above embodiment. For example, in the above embodiment, the gas barrier laminate 10 including the second polyvinyl alcohol-based resin layer 3b is illustrated, but depending on the application of the gas barrier laminate, the second polyvinyl alcohol-based resin layer 3b may not be included (see FIG. 4).
[0053] In the above embodiment, the packaging material 50 in which the polypropylene-based sealant layer 20 is laminated to the barrier side surface of the gas barrier laminate 10 has been exemplified, but the polypropylene-based sealant layer 20 may be laminated to the base layer 1 side surface of the gas barrier laminate 10 (see FIG. 5). The packaging material 60 shown in FIG. 5 has a configuration in which the barrier side of the gas barrier laminate 10 faces a general OPP film 8 (printing base material, etc.), and the polypropylene-based sealant layer 20 is laminated to the base layer 1 side of the gas barrier laminate 10. EXAMPLES
[0054] The present disclosure will now be described more specifically with reference to examples, but the present invention is not limited to these examples.
[0055] In the examples and comparative examples, the following materials were prepared. (base material layer) Polypropylene resin: Propylene monopolymer (mono PP) (Polyvinyl alcohol resin layer) EVOH: EVAL L171B (Kuraray Co., Ltd.) PVA: Poval 60-98 (Kuraray Co., Ltd.) TEOS: KBE04 (Shin-Etsu Chemical Co., Ltd.) (Sealant layer) Polypropylene sealant film: Torayfan ZK207#60 (CPP, thickness 60μm, Toray Industries, Inc.)
[0056] Example 1 The mono PP was used to form an OPP film (base layer), and at the same time, an EVOH layer (first polyvinyl alcohol-based resin layer) was formed on the surface of the OPP film by extrusion. The mass per unit area of the EVOH layer was 0.97 g / m 2 The thickness of the EVOH layer was 0.8 μm, and the surface roughness Sa was 0.08 μm. When the EVOH layer was peeled off and the surface roughness Sa of the OPP film was measured, the value was 0.23 μm. The surface roughness Sa was measured under the above-mentioned conditions using a three-dimensional non-contact surface shape measurement system (Vertscan R3300h Lite, manufactured by Ryoka Systems Co., Ltd.).
[0057] Using an electron beam heating vacuum deposition apparatus, a SiOx film (metal oxide layer) was formed on the surface of the EVOH layer. That is, the SiO deposition material was evaporated by electron beam heating to form a SiOx film (50 nm thick). Next, a layer containing PVA and TEOS (a second polyvinyl alcohol resin layer) was formed on the surface of the SiOx film. That is, TEOS, methanol, and hydrochloric acid (0.1N) were mixed to a mass ratio of 18 / 10 / 72 to obtain a hydrolyzed solution (TEOS-containing solution). A coating solution was prepared by mixing a 5% aqueous solution of PVA and a TEOS-containing solution so that the mass ratio of PVA and TEOS was 50 / 50. This coating solution was applied to the surface of the SiOx film, and then dried to form a layer containing PVA and TEOS (PVA / TEOS=50 / 50).
[0058] A packaging material was produced by bonding a polypropylene sealant film to the inner surface of the gas barrier laminate obtained through the above process using an adhesive (A-525, manufactured by Mitsui Chemicals, Inc.). The mass ratio of the polypropylene resin in the packaging material was 94 mass%. The oxygen permeability of this packaging material was measured. The oxygen permeability was measured using OX-TRAN2 / 20 (manufactured by MOCON) under conditions of a temperature of 30°C and a relative humidity of 70% in accordance with JIS K7126-2. The oxygen permeability of the packaging material after boiling was also measured in the same manner. That is, a three-sided pouch was produced using the packaging material, and city water was sealed in it. This sealed body was boiled for 30 minutes under a temperature condition of 90°C, and the oxygen permeability of the packaging material was measured. The results are shown in Table 1.
[0059] Example 2 A gas barrier laminate and a packaging material were produced and evaluated in the same manner as in Example 1, except that an AlOx film (50 nm) was formed as the metal oxide layer instead of a SiOx film (50 nm). The AlOx film was formed by evaporating an aluminum ingot by electron beam heating and introducing oxygen. The results are shown in Table 1.
[0060] Example 3 A gas barrier laminate and a packaging material were produced in the same manner as in Example 1, except that a layer with a mass ratio of PVA and TEOS of 97 / 3 was formed instead of a layer with a mass ratio of PVA and TEOS of 50 / 50, and each evaluation was carried out. The results are shown in Table 1.
[0061] Comparative Example 1 A gas barrier laminate and a packaging material were produced in the same manner as in Example 1, except that an EVOH layer (first polyvinyl alcohol-based resin layer) was not formed and a SiOx film (50 nm) was directly formed on the surface of the OPP film, and each evaluation was performed. The results are shown in Table 2.
[0062] Comparative Example 2 As the first polyvinyl alcohol-based resin layer, a layer of EVOH (mass per unit area: 0.97 g / m 2 Instead of forming a layer of PVA (mass per unit area 2.8 g / m, thickness 0.8 μm), 2 Except for forming a thin film (2.3 μm thick), a gas barrier laminate and a packaging material were produced in the same manner as in Example 1, and each evaluation was carried out. The results are shown in Table 2.
[0063] Comparative Example 3 As the first polyvinyl alcohol-based resin layer, a layer of EVOH (mass per unit area: 0.97 g / m 2 Instead of forming a layer of EVOH (mass per unit area 0.40 g / m, thickness 0.8 μm), 2 A gas barrier laminate and a packaging material were produced in the same manner as in Example 1, except that a 0.33 μm thick film was formed, and the respective evaluations were carried out. The results are shown in Table 2.
[0064] [Table 1]
[0065] [Table 2] [Explanation of symbols]
[0066] 1...base layer, 1a...coat layer (adhesive layer), 1b...copolymer layer, 3a...first polyvinyl alcohol-based resin layer, 3b...second polyvinyl alcohol-based resin layer, 5...metal oxide layer, 10...gas barrier laminate, 10F...inner surface, 20...polypropylene-based sealant layer, 50, 60...packaging material, F1...lamination surface of polypropylene-based base layer, F2...outer surface of polypropylene-based base layer, F3...surface of first polyvinyl alcohol-based resin layer
Claims
1. A gas barrier laminate; A polypropylene-based sealant layer; an adhesive layer provided between the gas barrier laminate and the polypropylene-based sealant layer, bonding the gas barrier laminate and the polypropylene-based sealant layer together; A packaging material comprising: The gas barrier laminate is A polypropylene-based base layer; A first polyvinyl alcohol-based resin layer; A gas barrier layer; A second polyvinyl alcohol-based resin layer; in this order, and has a laminated structure consisting of the polypropylene-based base layer, the first polyvinyl alcohol-based resin layer, the gas barrier layer, and the second polyvinyl alcohol-based resin layer, The first polyvinyl alcohol-based resin layer has a thickness of 0.4 to 2.0 μm, the gas barrier layer is a metal oxide layer having a thickness of 5 to 100 nm, The second polyvinyl alcohol-based resin layer has a thickness of 0.1 to 1.0 μm, A packaging material, wherein the combined mass ratio of the polypropylene-based base layer and the polypropylene-based sealant layer is 85 mass% or more based on the total mass of the packaging material.
2. 10. The packaging material of claim 1, wherein the metal oxide layer comprises silicon oxide.
3. 3. The packaging material according to claim 1, wherein the ethylene-vinyl alcohol copolymer has an ethylene unit content of 10 to 65 mol %.
4. The packaging material according to any one of claims 1 to 3, wherein the surface roughness Sa of the first polyvinyl alcohol-based resin layer on the side in contact with the gas barrier layer is 0.2 µm or less.
5. The packaging material according to any one of claims 1 to 3, wherein the surface roughness Sa of the first polyvinyl alcohol-based resin layer on the side in contact with the gas barrier layer is 0.1 µm or less.
6. The packaging material according to any one of claims 1 to 5, wherein the polypropylene-based base layer is a propylene monopolymer layer.
7. The packaging material according to any one of claims 1 to 6, wherein the second polyvinyl alcohol-based resin layer contains a silane compound.
8. The packaging material according to claim 7, wherein a mass ratio of the silane compound to the mass of the second polyvinyl alcohol-based resin layer is 0.05 to 0.
95.
9. The polypropylene-based base material layer further includes a copolymer layer of propylene and another monomer on a surface opposite to the side on which the first polyvinyl alcohol-based resin layer is provided, The packaging material according to any one of claims 1 to 8, wherein the other monomer is at least one of ethylene and butene.
10. The packaging material according to any one of claims 1 to 9, further comprising a printed substrate, and the gas barrier laminate is disposed between the printed substrate and the polypropylene-based sealant layer.
Citation Information
Patent Citations
Polypropylene composite film
JP1996238730A
Gas barrier olefin resin laminate
JP1997201897A
Packing laminated film and laminated film for deposition packing
JP2000071395A
Laminated film and its manufacturing method
JP2005088415A
Coating agent
JP2006056927A