Silicon-carbon composite materials and methods

The creation of core-shell composite particles with a porous carbon skeleton and low-temperature carbon coating addresses the capacity and stability issues of silicon-based anodes, achieving high specific capacities and improved cycle life in lithium ion batteries.

JP2024133480AActive Publication Date: 2024-10-02NEXEON LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024091986
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-09-10
Filing Date
2024-06-06
Publication Date
2024-10-02
Estimated Expiration
2040-09-10

AI Technical Summary

Technical Problem

Conventional lithium ion batteries using graphite as anode material face limitations in gravimetric and volumetric capacities, and silicon-based anodes suffer from mechanical stress and irreversible capacity loss due to volume changes during charging and discharging, leading to poor cycle life and efficiency.

Method used

Development of core-shell composite particles with a porous carbon skeleton and nanoscale silicon domains, where a pyrolytic carbon coating is applied at low temperatures below 700°C to maintain the microstructure and enhance conductivity, reducing surface area and SEI formation.

Benefits of technology

The method results in improved conductivity, reduced SEI formation, and enhanced capacity retention, with specific capacities up to 2340 mAh/g, suitable for high-energy density batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133480000008
    Figure 2024133480000008
  • Figure 2024133480000009
    Figure 2024133480000009
  • Figure 2024133480000010
    Figure 2024133480000010
Patent Text Reader

Abstract

To provide electroactive materials with a conductive carbon coating.SOLUTION: The invention provides methods for providing composite particles with a carbon coating, and core-shell particulate material obtained thereby. The methods comprise subjecting a plurality of precursor composite particles to a heat treatment by contact with a pyrolytic carbon precursor, so that an outer shell of a pyrolytic conductive carbon material is formed on the precursor composite particles, where the heat treatment is carried out at a temperature of 700°C or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for preparing core-shell composite particles comprising electroactive materials such as carbon and silicon The present invention also relates to particulate materials comprising silicon and carbon and having a core-shell structure. [Background technology]

[0002] Rechargeable metal-ion batteries are widely used in portable electronic devices such as mobile phones and laptops. Also, the rapid development of electric and hybrid vehicle technology is creating a large new market for high performance secondary batteries. Typically, the anode of a metal-ion battery has a metallic current collector provided with a layer of electroactive material (defined here as a material capable of inserting and releasing metal ions during charging and discharging of the battery). When the metal-ion battery is charged, metal ions are transported from the metal-ion-containing cathode layer through the electrolyte and inserted into the anode material.

[0003] Conventional lithium-ion batteries use graphite as the electroactive material in the anode. When a graphite-containing anode is charged, lithium is intercalated between the graphite layers, with the empirical formula Li x C 6 (where x is greater than 0 and less than or equal to 1). This means that in lithium ion batteries, graphite has a maximum theoretical capacity of 372 mAh / g, but the practical capacity is somewhat lower (about 340 to 360 mAh / g). The development of portable electronic devices and electric vehicles with high energy demands means that there is a need for electroactive materials that offer an improvement over graphite's gravimetric and volumetric capacities.

[0004] Materials such as silicon, tin, and germanium have significantly higher intercalation lithium atom capacities than graphite. In particular, silicon, due to its extremely high lithium capacity, has been identified as a promising alternative to graphite for the manufacture of rechargeable metal-ion batteries with high gravimetric and volumetric capacities (see, for example, Winter, M. et al., "Intercalation Electrode Materials for Rechargeable Lithium Batteries," Adv. Mater. 1998, 10, No. 10). Silicon has a theoretical maximum specific capacity of about 3,600 mAh / g at room temperature in lithium-ion batteries (Li 15 S 4 (Based on.

[0005] The high specific capacity of silicon is accompanied by large volume changes upon charging and discharging. Intercalation of lithium into bulk silicon increases the volume of the silicon material by up to 400% of its original volume. Repeated charge-discharge cycles therefore create large mechanical stresses in the silicon material, resulting in fracture and delamination of the silicon anode material, as well as deformation of other battery components. Contraction of silicon particles upon delithiation can lead to loss of electrical contact between the anode material and the current collector. Another problem is the formation of a solid electrolyte interface (SEI) layer on the nascent silicon surface during the initial charge cycle as a result of electrolyte deposition. This SEI layer does not have sufficient mechanical durability to accommodate the expansion and contraction of silicon and delaminates from the silicon surface. The newly exposed silicon surface then leads to further electrolyte decomposition, increasing the thickness of the SEI layer and irreversible consumption of lithium. The totality of these failure mechanisms results in an unacceptable loss of electrochemical capacity over successive charge and discharge cycles.

[0006] Many approaches have been proposed to overcome the problems associated with the volume changes observed during charging of silicon-containing anodes. One approach is to use some form of microstructured silicon as the electroactive material. Microstructured silicon structures with cross sections less than about 150 nm, such as silicon films and silicon nanoparticles, are more resistant to volume changes during charging and discharging than silicon particles in the micron size range. However, in their unaltered forms, none of them are particularly suitable for commercial-scale applications. Nanoscale particles are difficult to prepare and handle, and silicon films do not provide sufficient bulk capacitance. Also, the relatively high surface area of ​​microstructured silicon results in unacceptable capacity loss during the first charging cycle due to excessive SEI formation.

[0007] To address the lack of available silicon-containing electroactive materials, the present inventors have developed a class of composite particles in which silicon is deposited within the pores of a porous conductive material (e.g., a carbon-containing porous material such as an activated carbon material). The median pore diameter is about 5 to 10 nm or less. It has been determined that by carefully controlling the total pore volume, the pore size distribution of the conductive material, and the weight ratio of silicon to the conductive material, it is possible to obtain materials with controlled expansion characteristics, limited SEI formation, and high reversible capacity retention. However, further improvements in the properties of these materials can be obtained by suppressing the surface area. The suppression of the surface area has several advantages, including further reduction of SEI formation and a reduction in the amount of binder required to form the electrode active layer. Excess binder can contribute to reduced rate characteristics. Summary of the Invention [Problem to be solved by the invention]

[0008] Thus, there is a need for an electroactive material having a composite particle of the aforementioned type, while at the same time having a conductive carbon coating that helps to reduce the surface area of ​​the particle, improve the kinetic properties of the composite, and provide improved electrical conductivity of the electrode active layer having core-shell particles. However, the aforementioned composite particles are characterized by an extremely fine microstructure, with fine domains of silicon and fine pore walls. The fine microstructure of the composite particles is crucial to their function as electroactive materials in the anode, but is not compatible with conventional techniques of applying a conductive carbon coating. [Means for solving the problem]

[0009] According to a first aspect of the present invention there is provided a method for preparing core-shell composite particles comprising the steps of: (a) Below: (i) a porous carbon skeleton having micropores and / or mesopores, the total pore volume of the micropores and mesopores being at least 0.4 cm as measured by gas adsorption techniques; 3 / g, and the PD of the porous carbon skeleton 50 A porous carbon skeleton having a pore diameter of 10 nm or less, and (ii) a plurality of nanoscale electroactive material domains disposed with said porous carbon scaffold; providing a plurality of precursor composite particles comprising: (b) heat treating the plurality of precursor composite particles by contacting them with a pyrolyzable carbon precursor, wherein an outer shell of pyrolyzable conductive carbon material is formed on the precursor composite particles, the heat treating being at a temperature of 700° C. or less; A method is provided comprising:

[0010] It is important for the method of the present invention that the pyrolysis of the pyrolytic carbon precursor is carried out at a temperature of 700°C or less. Generally, conventional processes for forming pyrolytic carbon coatings require temperatures above 700°C, for example, in the range of 800°C to 1200°C. However, it has been found that the fine microstructure of the precursor composite particles is not compatible with such high temperatures and undergoes various thermally induced changes, including heat treatment and crystallization processes. Heat treatment of the particle microstructure can lead to the elimination of void spaces that accommodate the expansion of electroactive materials, such as silicon. Also, crystallization of silicon is problematic, since amorphous silicon exhibits good properties as an electroactive material. Excessive temperatures during the formation of the pyrolytic carbon coating can also lead to the formation of undesirable compounds that have no or low electrochemical activity, such as silicon carbide and silicon nitride. Taken together, these processes are detrimental to the properties of the carbon-coated particles as electroactive materials in the anodes of lithium-ion batteries.

[0011] Surprisingly, it has been found that low temperature carbon coating processes are effective in providing carbon coatings with sufficient graphitic properties to provide the necessary electrical conductivity for the coating, but do not adversely affect the structure underlying the precursor composite particle core. Thus, the method of the present invention provides an effective method for preparing core-shell composite particles with enhanced properties as electroactive materials.

[0012] Another advantage of the method of the present invention is that the surface area and pore volume are each 100 m 2 / g and above 0.1 mL / g of material. In the open void system, the carbon partially penetrates into the pore structure, allowing conductive tendrils to extend from the pyrolytic carbon coating into the interior of the particle. The coating combined with these conductive tendrils has the effect of shortening the average electron transport length in the core-shell composite particles. Instead, electrons can be transported to or from the current collector through the highly conductive carbon matrix during lithium insertion and release.

[0013] The heat treatment temperature in step (b) is preferably below 700° C. The heat treatment may for example be carried out at a temperature of 680° C. or less, 660° C. or less, 650° C. or less, 640° C. or less, 620° C. or less, or 600° C. or less.

[0014] The lower limit of the heat treatment temperature in step (b) is not limited. However, in general, the deposition of the carbon coating increases with increasing temperature. The required minimum temperature also depends on the type of carbon precursor used in the deposition step. The heat treatment temperature in step (b) is preferably at least 300°C or higher, for example, at least 500°C or higher, at least 520°C or higher, at least 540°C or higher, at least 560°C or higher, or at least 580°C or higher.

[0015] The carbon precursor may be contacted with the precursor composite particles in one of two ways: 1 Steam contact, 2 Contact from liquid or solution.

[0016] Some carbon precursors are suitable for only one of these two contacting methods.

[0017] Certain alternative carbon precursors are suitable for both contacting methods, depending on the temperature at which the contacting occurs. These carbon precursors may be in liquid form at low temperatures and sublime into vapor precursors above a set temperature before pyrolyzing at higher temperatures. They may be placed on the precursor composite particles as liquids, if desired. Examples of such compounds include camphor, anthracene, pentacene, and metal phthalocene complexes.

[0018] The pyrolytic carbon precursor may be contacted with the precursor composite particles as a vapor, preferably as a hydrocarbon vapor, during the heat treatment step. Suitable hydrocarbons include polycyclic hydrocarbons containing 10 to 25 carbon atoms and optionally 1 to 3 heteroatoms, where the polycyclic hydrocarbons are selected from naphthalene, substituted naphthalenes such as di-hydroxynaphthalene, anthracene, tetracene, pentacene, fluorene, acenaphthene, phenanthrene, fluorene, pyrene, chrysene, perylene, coronene, fluorenone, anthraquinone, anthrone, and alkyl-substituted derivatives thereof. Suitable pyrolytic carbon precursors also include bicyclic monoterpenoids, where the bicyclic monoterpenoids are selected from camphor, borneol, eucalyptol, camphene, carene, sabinene, thujene, and pinene. Suitable pyrolytic carbon precursors also include C 1 ~C 10 or C 2 ~C 10 where the hydrocarbon is selected from alkanes, alkenes, alkynes, cycloalkanes, cycloalkenes, and arenes, such as methane, ethylene, propylene, acetylene, and cyclohexane. Other suitable pyrolytic carbon precursors include phthalocyanine, sucrose, starch, graphene oxide, reduced graphene oxide, pyrene, perhydropyrene, triphenylene, tetracene, benzopyrene, perylene, coronene, and chrysene. Preferably, the carbon precursor comprises acetylene, and more preferably, the carbon precursor is acetylene.

[0019] The hydrocarbon vapor may be contacted with a transition metal catalyst at a temperature of at least 500° C. prior to contact with the precursor composite particles. The transition metal catalyst may be selected from nickel, iron, cobalt, copper and mixtures thereof, most preferably nickel. The transition metal catalyst may be in the form of a mesh, which is disposed in the flow path of the vapor prior to contact with the precursor composite particles.

[0020] Alternatively, the transition metal catalyst may be disposed on the surface of the precursor composite particles. For example, prior to step (b), the gaseous nickel carbonyl may be thermally decomposed to deposit nickel on the surface of the precursor composite particles. If necessary, the deposition of nickel may be carried out in the same reactor as for the heat treatment described above. A suitable temperature for the decomposition of nickel carbonyl is about 220 to 250° C. If necessary, after the deposition of the carbon coating, the nickel may be converted back to nickel carbonyl vapor by contacting the coated particles with carbon monoxide gas, for example at a temperature of 50° C. to 60° C. The nickel carbonyl gas may thus be recycled.

[0021] Transition metal catalyzed processing offers further improvements in the formation of pyrolytic carbon coatings at low temperatures, and the recovery and recycling of nickel in the form of nickel carbonyl gas makes the process more cost-effective.

[0022] Alternatively, the pyrolytic carbon precursor may be contacted with the precursor composite particles in liquid form. In particular, the precursor composite particles may be contacted with a dispersion or solution of the pyrolytic carbon precursor in a solvent, after which the solvent is removed to provide the precursor composite particles coated with the pyrolytic carbon precursor prior to heat treatment. Suitable pyrolytic carbon precursors for contacting the precursor composite particles in liquid form include polymers and oligomers that include a carbon-containing backbone, such as polyvinylpyrrolidone (PVP), or copolymers of vinylpyrrolidone with one or more other ethylenically unsaturated monomers.

[0023] Carbon precursor compounds that can be deposited from solution include polydopamine, poly(diallyldimethylammonium chloride) (PDDA), citric acid, mixtures containing citric acid and ethanol, polyacrylonitrile (PAN), PAN derivatives, polymerized polypyrrole (PPy) composites, melamine resins such as melamine-formaldehyde resin, pitch, glucose, sucrose, phenolic resins, polyvinyl alcohol (PVA), polyacrylic acid (PAA), resorcinol-formaldehyde resin, poly(methyl methacrylate) (PMMA), camphor, anthracene, pentacene, and metal phthalocene complexes.

[0024] If necessary, a dopant material may be introduced into the carbon coating. The dopant material may be introduced into the coating by incorporating a dopant precursor. Preferably, the dopant is boron or phosphorus. Doping the pyrolytic carbon coating further increases the electrical conductivity of the coating. Also, by incorporating a dopant material into the carbon coating, the electroactive material domains are preferably doped, further increasing their electrical conductivity.

[0025] When the pyrolytic carbon precursor is provided as a vapor, it may be used in conjunction with a gaseous precursor of the dopant material. When the dopant is boron, a suitable gaseous dopant precursor includes borane (BH 3 ), diborane (B 2 H 6 ), triisopropyl borate ([(CH 3 ) 2 CH] 3 B), triphenylborane ((C 6 H 5 ) 3 B), and tris(pentafluorophenyl)borane (C 6 F 5 ) 3 B, preferably diborane. When the dopant is phosphorus, the preferred gaseous dopant precursor is phosphine (PH 3 ).

[0026] Also, if the pyrolytic carbon precursor is a volatile liquid, the dopant may be introduced as a volatile liquid. In the case of boron, the preferred dopant precursor is triethylborane. In the case of phosphorus, the preferred dopant precursor is triethylphosphine.

[0027] When the pyrolytic carbon precursor is provided as a solution or suspension, suitable boron dopant precursors include boric acid (H 3 BO 3 ), Sodium Tetraborate (Na 2 [B 4 O 5 (OH) 4 ].8H 2 O, borazine (B 3 H 6 N 3 ), and ammonia borane (BH 6 N), the preferred source being boric acid. When the dopant is phosphorus, the preferred precursors are phosphoric acid (H 3 PO 4 ), or phosphonates and phosphonic acids.

[0028] Another option when using liquid, solution phase, or suspended pyrolytic carbon precursors is to For example, the dopant is introduced into the reactor as a gas in a stream of inert gas that is fed to the headspace of the reactor. Suitable gaseous dopant precursors include those previously described.

[0029] The outer shell of the conductive carbon material deposited by the method of the present invention preferably has a thickness after pyrolysis of 10 nm or less, 5 nm or less, 4 nm or less, 2 nm or less, or 1 nm or less.

[0030] The outer shell of the conductive carbon material deposited by the method of the present invention may be amorphous, crystalline, or have both amorphous and crystalline domains. Preferably, the carbon coating is amorphous carbon. Preferred types of crystalline carbon coatings are graphite and graphene.

[0031] The porous carbon framework has a three-dimensionally interconnected open pore network, which has micropores and / or mesopores, and optionally contains a small amount of macropores. In accordance with conventional IUPAC terminology, the term "macropores" is used herein to describe pores with a diameter of less than 2 nm, the term "mesopores" is used to describe pores with a diameter of 2 to 50 nm, and the term "macropores" is used to describe pores with a diameter of more than 50 nm.

[0032] References to the volumes of micropores, mesopores, and macropores in a porous carbon scaffold, as well as the distribution of pore volumes in a porous carbon scaffold, are intended to define the pore structure of the porous carbon scaffold when separation is taken into account. Pore occupation by nanoscale electroactive material domains results in a measurable reduction in pore volume; however, this is not taken into account for purposes of defining the pore structure of the porous carbon scaffold.

[0033] Using the quenched solid density functional theory (QSDFT) according to the standard methods specified in ISO15901-2 and ISO15901-3, -6Nitrogen gas adsorption at a relative pressure of p / p0 (or less) was used to determine the total volume of micropores and mesopores and the pore size distribution of micropores and mesopores. Nitrogen gas adsorption is a technique that characterizes the porosity and pore diameter distribution of a material by condensing a gas into the pores of a solid. As the pressure is increased, the gas condenses first in the smallest diameter pores until a saturation point is reached where all pores are filled with liquid. The nitrogen gas pressure is then gradually reduced, allowing the liquid to evaporate from the system. Analysis of the adsorption and desorption isotherms, and the hysteresis between them, determines the pore volume and pore diameter distribution. Apparatus suitable for measuring the pore volume and pore diameter distribution by nitrogen gas adsorption includes the TriStar II and TriStar II Plus porosity analyzers available from Micromeritics Instrument, Inc., USA, and the Autosorb IQ porosity analyzer available from Quantachrome Instruments, Inc.

[0034] Nitrogen gas adsorption is effective for measuring pore volume and pore size distribution for pores with diameters up to 50 nm, but is unreliable for larger diameter pores. Therefore, for the purposes of this invention, the nitrogen adsorption method is used to measure pore volume and pore size distribution only for pores with diameters up to 50 nm (i.e., only micropores and mesopores). Similarly, PD 50 is defined only for the total volume of micropores and mesopores.

[0035] The porous conductive particles have a thickness of at least 0.4 cm when measured by gas adsorption. 3 The porous carbon skeleton is characterized by the total volume of micropores and mesopores (i.e., the total pore volume in the range of 0 to 50 nm) in nanometers per gram. Typically, the porous carbon skeleton contains both micropores and mesopores. However, it is not excluded to use a porous carbon skeleton that contains micropores but no mesopores, or that contains mesopores but no micropores.

[0036] More preferably, the total volume of the micropores and mesopores in the porous conductive particles is at least 0.45 cm 3 / g, at least 0.5 cm 3 / g, at least 0.55 cm 3 / g, at least 0.6 cm 3 / g, at least 0.65 cm 3 / g, at least 0.7 cm 3 / g, at least 0.75 cm 3 / g, at least 0.8 cm 3 / g, at least 0.85 cm 3 / g, at least 0.9 cm 3 / g, at least 0.95 cm 3 / g, or at least 1 cm 3 The use of conductive particles with high porosity is advantageous since it allows a greater amount of silicon to be accommodated within the pore structure.

[0037] The internal pore volume of the porous conductive particles is suitably capped at a value where the increased embrittlement of the porous conductive particles outweighs the benefit of the increased pore volume accommodating a greater amount of silicon. Preferably, the total volume of micropores and mesopores in the porous conductive particles is less than 2.2 cm 3 / g or less, 2cm 3 / g or less, 1.8cm 3 / g or less, 1.6cm 3 / g or less, 1.5cm 3 / g or less, 1.45cm 3 / g or less, 1.4cm 3 / g or less, 1.35cm 3 / g or less, 1.3cm 3 / g or less, 1.25cm 3 / g or less, or 1.2cm 3 / g or less.

[0038] In one example, the total volume of micropores and mesopores in the porous conductive particle is between 0.7 and 2.2 cm 3 / g range, 0.7 to 2 cm 3 / g range, 0.8 to 2 cm 3 / g range, 0.8 to 1.8 cm 3 / g range, 0.9 to 1.8 cm 3 / g range, 0.9 to 1.6 cm 3 / g range, 1 to 1.6 cm 3 / g range, or 1.1 to 1.6 cm 3 / g.

[0039] In another example, the total volume of micropores and mesopores in the porous conductive particle is between 0.4 and 0.75 cm 3 / g, 0.4 to 0.7 cm 3 / g, 0.4 to 0.65 cm 3 / g, 0.45 to 0.75 cm 3 / g, 0.45 to 0.7 cm 3 / g, 0.45 to 0.65 cm 3 / g, or 0.45 to 0.6 cm 3 / g.

[0040] In another example, the total volume of micropores and mesopores in the porous conductive particles is between 0.6 and 2 cm. 3 / g, 0.6 to 1.8 cm 3 / g, 0.7 to 1.8 cm 3 / g, 0.7 to 1.6 cm 3 / g, 0.8 to 1.6 cm 3 / g, 0.8 to 1.5 cm 3 / g, 0.8 to 1.4 cm 3 / g, 0.9 to 1.5 cm 3 / g, 0.9 to 1.4 cm 3 / g, or 1 to 1.4 cm 3 / g.

[0041] The pore size distribution of the porous conductive particles may be monomodal, bimodal or multimodal. The term "pore size distribution" as used herein refers to the distribution of pore sizes relative to the cumulative total internal pore volume of the porous conductive particles. Bimodal or multimodal pore size distributions are preferred, as the close proximity between micropores and larger diameter pores offers the advantage of efficient ion transport through the porous network to the nanoscale electroactive material domains.

[0042] Given the limitations of available analytical techniques, it is difficult to measure the pore volume and pore size distribution over the full range of micropores, mesopores and macropores using a single technique. When the porous carbon skeleton has macropores, the volume of pores with diameters in the range of more than 50 nm and less than or equal to 100 nm can be measured by mercury porosimetry, which is preferably performed on a 0.3 cm 3 / g or less, or 0.20 cm 3 / g or less, or 0.1cm 3 / g or less, or 0.05 cm 3 / g or less. Although a small proportion of macropores is beneficial for facilitating electrolyte access to the pore network, the advantages of the present invention are obtained by substantially containing the silicon in the micropores and smaller mesopores.

[0043] Pore ​​volumes measured by mercury porosimetry at pore sizes below 50 nm are ignored (as previously described, when using nitrogen adsorption techniques, mesopores and micropores are characterized). Pore volumes measured by mercury porosimetry above 100 nm are assumed to be interparticle porosity for purposes of this invention and are ignored.

[0044] Mercury porosimetry is a technique for characterizing the porosity and pore diameter distribution of a material by applying various levels of pressure to a sample of the material immersed in mercury. The pressure required to force mercury into the pores of the sample is inversely proportional to the size of the pores. The values ​​obtained by the mercury porosimetry method described in this application were obtained according to ASTM UOP578-11, with a surface tension γ of 480 mN / m and a contact angle φ of 140° for mercury at room temperature. The density of mercury is 13.5462 g / cm at room temperature. 3 A number of high precision mercury porosimeters are commercially available, such as the AutoPore IV series of automated mercury porosimeters available from Micromeritics Instrument Corporation, USA. For a complete review of mercury porosimetry methods, see PA Webb and C. Orr, "Analytical Methods in Fine Particle Technology, 1997, Micromeritics Instrument Corporation, ISBN 0-9656783-0".

[0045] It is understood that intrusion techniques such as gas adsorption and mercury porosimetry are only effective in determining the pore volume of pores accessible to nitrogen or mercury from the outside of the porous conductive particle. It is understood that the porosity values ​​specified herein represent the volume of open pores, i.e., pores accessible to fluids from the outside of the porous carbon skeleton. In determining the porosity value, pores that are completely surrounded and cannot be identified by nitrogen adsorption or mercury porosimetry are not taken into account. Similarly, any pore volume located in pores small enough to be below the detection limit by nitrogen adsorption is not taken into account.

[0046] The general term "PD n "Pore diameter" refers to the pore diameter of n percent by volume, based on the total volume of micropores and mesopores. For example, the term "PD 90 The pore diameter is less than P 1represents the pore diameter at which 90% of the total micropore and mesopore volume is found, and PD 50 The pore diameter is the median pore diameter below which 50% of the total micropore and mesopore volume is found.

[0047] PD of porous carbon frameworks 90 The pore diameter may be 20 nm or less, or 15 nm or less. 90 The pore diameter of the porous carbon skeleton is 12 nm or less, 10 nm or less, 8 nm or less, or 6 nm or less. 90 The pore diameter is at least 3 nm, at least 3.2 nm, at least 3.5 nm, at least 3.8 nm, or at least 4 nm.

[0048] PD of porous carbon frameworks 30 The pore diameter is preferably 1.6 nm or less, 1.5 nm or less, 1.4 nm or less, 1.3 nm or less, 1.2 nm or less, 1.1 nm or less, or 1 nm or less. 30 The pore diameter is preferably at least 0.45 nm, at least 0.5 nm, at least 0.6 nm, or at least 0.7 nm.

[0049] Photodischarge of conductive multiporous particle scaffolds 50 The pore diameter is preferably 8 nm or less, 6 nm or less, 5 nm or less, 4 nm or less, 3 nm or less, 2.5 nm or less, 2 nm or less, 1.5 nm or less. 50 The pore diameter is at least 1 nm, at least 1.1 nm, or at least 1.2 nm. Thus, in the present invention, it is preferred that at least 50% of the total volume of micropores and mesopores within the conductive porous particle scaffold is in the form of pores with a diameter of less than 8 nm.

[0050] For the avoidance of doubt, macropore volume (pore diameters greater than 50 nm) is defined as PD 50 are not taken into account for purposes of determining value.

[0051] Typically, the precursor composite particles have a D in the range of 1 to 50 μm. 50 Optionally, the precursor composite particles may have a particle diameter D 50 The particle diameter may be at least 1.5 μm, at least 2 μm, at least 3 μm, at least 4 μm, or at least 5 μm. If desired, the D of the precursor composite particles 50 The particle diameter may be 40 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, 18 μm or less, 15 μm or less, 12 μm or less, 10 μm or less.

[0052] For example, the precursor composite particles may have a D in the range of 1 to 25 μm, 1 to 20 μm, 2 to 25 μm, 2 to 20 μm, 2 to 18 μm, 3 to 20 μm, 3 to 18 μm, 3 to 15 μm, 4 to 18 μm, 4 to 15 μm, 4 to 12 μm, 5 to 15 μm, 5 to 12 μm, or 5 to 10 μm. 50 The precursor composite particles may have particle diameters within these size ranges and with the porosity and pore diameter distributions described herein are ideally suited for the preparation of composite particles for use in metal ion battery anodes. These particles provide core-shell composite particles with good dispersibility in slurries, structural robustness, high capacity retention over repeated charge-discharge cycles, and suitability for forming dense electrode layers of uniform thickness in the conventional thickness range of 20 to 50 μm.

[0053] For the avoidance of doubt, the term "particle diameter" as used herein refers to the equivalent spherical diameter (esd), i.e., the diameter of a sphere having the same volume as a given particle, and it is understood that particle volume includes the volume of any intraparticle pores. 50 " and "D 50 "Particle diameter" refers to the volume-based median particle diameter, i.e., the diameter below which less than 50% by volume of the particle population is found. 10 " and "D 10 "Particle diameter" refers to the 10 percent volumetric median particle diameter, i.e., the diameter below which less than 10 volume percent of the particle population is found. 90" and "D 90 "Particle diameter" refers to the 90 percent volume-based median particle diameter, ie, the diameter below which less than 90% by volume of the particle population are found.

[0054] Particle diameter and particle size distribution can be measured by standard laser diffraction methods according to ISO 13320:2009. Laser diffraction relies on the principle that particles scatter light at angles that vary with the size of the particle, and that a collection of particles produces a pattern of scattered light defined by intensity and angle that correlates to particle size distribution. Many laser diffraction instruments are commercially available for rapid and reliable particle size distribution measurement. Unless otherwise stated, particle size distribution measurements described or reported in this application were measured using a conventional Malvern Instruments Malvern Mastersizer™ 3000 particle size analyzer. The Malvern Mastersizer™ 3000 particle size analyzer works by shining a helium-neon gas laser beam through a transparent cell containing particles of interest suspended in an aqueous solution. The light beam that strikes the particles is scattered at angles that are inversely proportional to the particle size, a photodetector array measures the light intensity at several predetermined angles, and the measured intensities at different angles are processed by a computer using standard theoretical principles to determine the particle size distribution. The laser diffraction values ​​reported herein are obtained using a wet dispersion of particles in distilled water. The particle refractive index is 3.50 and a dispersant index of 1.330 is used. The particle size distribution is calculated using the Mie scattering model.

[0055] D of precursor composite particles 10 The particle diameter is preferably at least 0.2 μm, at least 0.5 μm, at least 0.8 μm, at least 1 μm, at least 1.5 μm, or at least 2 μm. 10 Maintaining particle diameters of 0.2 μm or greater reduces the likelihood of undesirable agglomeration of submicron sized particles, resulting in improved flow behavior and improved dispersibility of the composite particles formed.

[0056] D of precursor composite particles 90 The particle diameter is preferably 40 μm or less, or 30 μm or less, or 25 μm or less, or 20 μm or less. The use of larger precursor composite particles results in non-uniform packing of the core-shell composite particle products in the electrode active layer, thus preventing the formation of a dense electrode layer, especially an electrode layer having a thickness in the range of 20 to 50 μm.

[0057] The precursor composite particles preferably have a narrow size distribution span. For example, the particle size distribution span (D 90 -D 10 ) / D 50 (defined as) is preferably 5 or less, more preferably 4 or less, more preferably 3 or less, more preferably 2 or less, and most preferably 1.5 or less. By maintaining a narrow size distribution span, efficient packing of the core-shell composite particle product into a dense electrode layer can be easily achieved.

[0058] The porous carbon skeleton preferably comprises at least 80% by weight carbon, more preferably at least 90% by weight carbon, more preferably at least 95% by weight carbon, and where necessary at least 98% or at least 99% by weight carbon. The carbon may be crystalline carbon, or amorphous carbon, or a mixture of amorphous and crystalline carbon. The porous carbon particles may be either hard or soft carbon particles and may be suitably obtained by known procedures including pyrolysis of polymers. Porous carbon particles of various different specifications are available from commercial suppliers.

[0059] The precursor composite particles may have a range of different electroactive material loadings. For example, the amount of electroactive material in the precursor composite particles may be selected such that at least 25% and up to 80% or more of the internal pore volume of the porous carbon scaffold is occupied by the electroactive material. For example, the electroactive material may occupy 25% to 60%, 25% to 55%, 25% to 50%, 25% to 45%, 25% to 40% of the internal pore volume of the porous carbon scaffold. Within these preferred ranges, the pore volume of the porous carbon scaffold effectively accommodates the expansion of the electroactive material during charging and discharging and avoids excess pore volume that does not contribute to the volumetric capacity of the core-shell composite particles. However, the amount of electroactive material is not so high that inadequate metal ion diffusion rates prevent effective lithiation or inadequate expansion volume creates mechanical resistance to lithiation.

[0060] The electroactive material in the precursor composite particles is preferably selected from silicon, tin, germanium, aluminium and mixtures thereof. A preferred electroactive material is silicon.

[0061] When the electroactive material is silicon, the preferred mass ratio of silicon to the porous carbon scaffold is [0.5×P 1 From 1.3 x P 1 ]:1, where P 1 is a dimensionless quantity having the size of the total pore volume of micropores and mesopores in the porous conductive particle, cm 3 / g (for example, a porous carbon particle is 1.2 cm 3 / g, P 1 = 1.2), which takes into account the density of the silicon and the pore volume of the porous conductive particles, and determines the weight ratio of silicon that will occupy approximately 20% to 55% of the pore volume, assuming that the silicon is located completely within the internal pore volume.

[0062] In practice, it is preferred that at least 90% by weight, more preferably at least 95% by weight, and even more preferably at least 98% by weight of the electroactive material in the precursor composite particles is located within the internal pore volume of the porous carbon skeleton, with very little or no silicon located on the external surface of the precursor composite particles. Preparation of the precursor composite particles by chemical vapor infiltration (CVI) is an effective method to ensure that only very small amounts of the electroactive material are located on the external surface. This is because the kinetics of the CVI process favors the deposition of silicon into small pores, thus resulting in preferential deposition of silicon on the internal surfaces of the porous conductive particles.

[0063] The heat treatment in step (b) may suitably be carried out for a period of from 1 to 3 hours.

[0064] The step (a) of providing a plurality of precursor composite particles may comprise contacting the electroactive material precursor with a plurality of porous carbon particles at a temperature of from 200 to 800° C., thereby depositing the electroactive material within the pores of the carbon particles. The electroactive material may be selected from silicon, tin, germanium, aluminum and mixtures thereof. A preferred electroactive material is silicon.

[0065] The preferred gas precursor for silicon deposition is silane (SiH 4 ) and trichlorosilane (SiHCl 3 The CVI method is particularly useful in preparing the electroactive materials disclosed herein because it causes minimal damage to the geometry of the porous substrate.

[0066] Suitable silicon-containing precursors include silane (SiH 4 ), disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ), tetrasilane (Si 4 H 10 ), or trichlorosilane (HSiCl 3), or methyltrichlorosilane (CH 3 SiCl 3 ) or dimethyldichlorosilane ((CH 3 ) 2 SiCl 2 ) and methylchlorosilanes. Preferably, the silicon-containing precursor is a silane. Suitable tin-containing precursors include bis[bis(trimethylsilyl)amino]tin(II) ([(CH 3 ) 3 Si] 2 N) 2 Sn), tetraaryltin (((H 2 C=CHCH 2 ) 4 Sn), tetrakis(diethylamido)tin(IV) ([(C 2 H 5 ) 2 N] 4 Sn), tetrakis(dimethylamido)tin(IV) ([(CH 3 ) 2 N] 4 Sn, tetramethyltin (Sn(CH 3 ) 4 ), tetravinyltin (Sn(CH=CH 2 ) 4 ), tin(II) acetylacetonate (C 10 H 14 O 4 Sn), trimethyl(phenylene)tin (C 6 H 5 C≡CSn(CH 3 ) 3 ), and trimethyl(phenyl)tin (C 6 H 5 Sn(CH 3 ) 3 Preferably, the tin-containing precursor is tetramethyltin.

[0067] Suitable aluminum-containing precursors include aluminum tris(2,2,6,6-tetramethyl-3,5-heptanedionate) (Al(OCC(CH 3 ) 3 CHCOC(CH 3 ) 3) 3 ), trimethylaluminum ((CH 3 ) 3 Al), and tris(dimethylamido)aluminum(III) (Al(N(CH 3 ) 2 ) 3 Preferably, the aluminum-containing precursor is trimethylaluminum.

[0068] Suitable germanium-containing precursors include germane (GeH 4 ), hexamethyldigermanium ((CH 3 ) 3 GeGe(CH 3 ) 3 ), tetramethylgermanium ((CH 3 ) 4 Ge), tributylgermanium hydride ([CH 3 (CH 2 ) 3 ] 3 GeH), triethylgermanium hydride ((C 2 H 5 ) 3 GeH), and triphenylgermanium hydride ((C 6 H 5 ) 3 GeH). Preferably, the germanium-containing precursor is germane.

[0069] The CVI process may also utilize gaseous precursors of the dopant material to deposit the doped electroactive material into the micropores and / or mesopores of the porous carbon skeleton. When the dopant is boron, suitable precursors include borane (BH 3 ), diborane (B 2 H 6 ), triisopropyl borate ([(CH 3 ) 2 CH] 3 B), triphenylborane ((C 6 H 5 ) 3 B), and tris(pentafluorophenyl)borane (C 6 F 5 )3 B, preferably borane. When the dopant is phosphorus, the preferred precursor is phosphine (PH 3 ).

[0070] The precursors may be used in pure form or, more commonly, as a mixture diluted with an inert carrier gas such as nitrogen or argon. For example, the precursors may be used in an amount ranging from 0.5 to 20 vol%, or 1 to 10 vol%, or 1 to 5 vol%, based on the total volume of the precursors and the inert carrier gas. The CVI process is preferably carried out at low partial pressures of the gaseous precursors, with the total pressure being at or near 101.3 kPa (i.e., atmospheric pressure, 1 atm), with the remaining partial pressure being brought to atmospheric pressure using an inert padding gas such as hydrogen, nitrogen or argon. The presence of oxygen should be minimized according to conventional procedures operating in an inert atmosphere to prevent undesired oxidation of the deposited electroactive material. Preferably, the oxygen content is less than 0.01 vol%, more preferably less than 0.001 vol%, based on the total volume of the gas used in step (b).

[0071] The temperature of the CVI process is suitably selected to pyrolyse the precursor into the electroactive material. The CVI process is suitably carried out at a temperature in the range of 200 to 800° C., 400 to 700° C., 400 to 600° C., 400 to 550° C., 450 to 550° C., 450 to 500° C. Preferably, the CVI process is carried out at a temperature in the range of 400 to 500° C., preferably 450 to 500° C.

[0072] The surface of the electroactive material deposited by the CVI method is reactive to oxygen and forms a native oxide layer when exposed to atmospheric oxygen. In the case of silicon, an amorphous silicon dioxide film forms quickly when the silicon surface is exposed to oxygen. The formation of the native oxide layer is reactive and therefore requires careful process control to prevent overheating or burning of the particulate material during manufacture. The presence of the native oxide layer can lead to irreversible capacity loss and reduced cycle life and therefore be detrimental to the performance of the electroactive material in lithium-ion batteries. Therefore, it is preferred that the electroactive material is not exposed to oxygen prior to deposition of the lithium-ion permeable filler material.

[0073] More preferably, step (b) of the method of the present invention further comprises the step (b2) of contacting the surface of the deposited electroactive material with a passivating agent, wherein the electroactive material is not exposed to oxygen prior to contacting with the passivating agent, where a passivating agent is defined as a compound capable of modifying the surface of the electroactive material in such a way as to inhibit or prevent the formation of surface oxides.

[0074] Suitable passivating agents include compounds that contain an alkene, alkyne or carbonyl functionality, more preferably compounds that contain a terminal alkene, terminal alkyne, or aldehyde group.

[0075] Suitable passivating agents include one or more of the following formulas: (i) R-CH=CH-R; (ii) RC ≡ CR; (iii) O=CH-R; wherein R represents H or an unsubstituted or substituted aliphatic or aromatic hydrocarbyl group having from 1 to 20 carbon atoms, preferably from 2 to 10 carbon atoms, or the two R groups in formula (i) form an unsubstituted or substituted hydrocarbyl ring structure containing from 3 to 8 carbon atoms. Particularly preferred passivators include compounds of one or more of the following formulae: (i)CH 2 =CH-R; (ii) HC ≡ CR; wherein R is defined as above. Preferably, R is unsubstituted.

[0076] Examples of suitable compounds include ethylene, propylene, 1-butene, butadiene, 1-pentene, 1,4-pentadiene, 1-hexene, 1-octene, styrene, divinylbenzene, acetylene, phenylacetylene, norbornene, norbornadiene, and bicyclo[2.2.2]oct-2-ene. Mixtures of different passivators may also be used.

[0077] It is understood that the alkene, alkyne, or carbonyl groups of the passivating agent undergo an insertion reaction with M-H groups at the surface of the electroactive material, where M represents an atom of the electroactive material, to form a covalently passivated surface that is resistant to oxidation by air. When silicon is the electroactive material, the passivation reaction between the silicon surface and the passivating agent may be understood as a form of hydrosilylation, as shown diagrammatically below:

[0078] [ka] Other suitable passivation agents include compounds that contain an active hydrogen atom combined with oxygen, nitrogen, sulfur, or phosphorus. For example, the passivation agent may be an alcohol, an amine, a thiol, or a phosphine. The reaction of -XH groups with hydroxyl groups on the surface of the electroactive material results in H 2 It will be appreciated that this results in the removal of X and the formation of a direct bond between X and the surface of the electroactive material.

[0079] Suitable passivators in this category include compounds of formula HX-R, where X represents O, S, NR or PR, and each R is independently defined as above. The two R groups in formula (iv) may form an unsubstituted or substituted hydrocarbyl ring structure containing 3 to 8 carbon atoms. Preferably, X represents O or NH, and optionally, R represents a substituted aliphatic or aromatic group having 2 to 10 carbon atoms. The amine group may also be incorporated into a 4 to 10 membered aliphatic or aromatic ring structure, such as pyrrolidine, pyrrole, imidazole, piperazine, indole, or purine. The contacting step of the electroactive material with the passivator in step (b2) may be carried out at a temperature in the range of 25 to 700° C. For example, step (b2) may be suitably carried out within the suitable temperature range of step (b) and / or step (c) described herein. Preferably, step (c) is carried out at the same temperature as step (b2) or at a higher temperature than step (b2). For example, step (b2) may be carried out at a temperature in the range of from 25° C. to less than 500° C. and step (c) may be carried out at a temperature in the range of from 500° C. to 700° C.

[0080] After passivation of the electroactive material surface, a lithium ion permeable filler material may be deposited in step (c) as described above. The R group of the passivating agent may be incorporated into the lithium ion permeable filler such that a covalent bond is formed between the lithium ion permeable filler and the surface of the electroactive material via the passivating agent.

[0081] When the lithium ion permeable filler material is a conductive pyrolytic carbon material, the same compound may function as both the passivator and the pyrolytic carbon precursor. For example, if styrene is selected as the pyrolytic carbon precursor, it will also function as the passivator, provided that the electroactive material is not exposed to oxygen before contacting the styrene. Thus, step (c) may comprise depositing a conductive pyrolytic carbon material by a CVI process. The pyrolytic carbon precursor is the same as the passivator used in step (b2). In this case, the passivation in step (b2) and the deposition of the conductive carbon material in step (c) may be carried out simultaneously, for example at a temperature in the range of 500 to 700° C. Alternatively, the passivation in step (b2) and the deposition of the conductive carbon material in step (c) may be carried out sequentially using the same material as the passivator and the pyrolytic carbon precursor, except that step (c) is carried out at a higher temperature than step (b2). For example, step (b2) may be carried out at a temperature in the range of from 25°C to less than 500°C and step (c) may be carried out at a temperature in the range of from 500°C to 700°C.

[0082] Alternatively, different compounds may be used as the passivation agent in step (b2) and the pyrolytic carbon precursor in step (c). For example, the electroactive material may first be contacted with the passivation agent in step (b2), and then the deposition of the conductive pyrolytic carbon material may be performed in step (c), and the pyrolytic carbon precursor used in step (c) is different from the passivation agent used in step (b2). For example, the passivation agent in step (b2) may be styrene, and the pyrolytic carbon precursor in step (c) may be a compound such as cyclohexane. Cyclohexane is a compound that can form a pyrolytic carbon material but cannot passivate the electroactive material surface. When the passivation agent and the pyrolytic carbon precursor are different materials, steps (b2) and (c) may be performed at the same temperature, for example, in the range of 500 to 700° C. Alternatively, step (c) may be performed at a higher temperature than step (b2). For example, step (b2) may be carried out at a temperature in the range of from 25°C to less than 500°C and step (c) may be carried out at a temperature in the range of from 500°C to 700°C.

[0083] Another suitable passivation agent is ammonia. Step (b2) may thus comprise contacting the surface of the deposited electroactive material with ammonia at a temperature in the range of 200 to 800° C., preferably in the range of 400 to 700° C. For example, when the passivation agent is ammonia, step (b2) may be carried out at the same temperature as that used in depositing the electroactive material in step (b). Thereafter, if necessary, the temperature is increased to the range of 500 to 1,000° C. to form a crystalline nitride surface (e.g. of formula SiN x (where x≦4 / 3) of silicon nitride surface is formed. Thus, ammonia passivation provides another means of inhibiting oxidation of the electroactive material. Because sub-stoichiometric silicon nitride is conductive, this step also results in the formation of a conductive network that allows for more rapid charging and discharging of the electroactive material.

[0084] When the electroactive material is silicon, it is preferred that the silicon is amorphous. The amorphous nature of silicon can be measured by X-ray diffraction (XRD), which is shown for Example 4 in FIG.

[0085] One advantage of the present invention is that the temperature of the carbon coating process inhibits or substantially avoids annealing the microstructure of the composite particles. The microstructure of the composite particles can be evaluated by TGA analysis, which is a method for determining the oxidation of elemental silicon to silicon dioxide (SiO ) at high temperatures in air. 2 ), a weight gain is observed. The mechanism by which Si is oxidized is temperature dependent. Silicon atoms at the surface of silicon nanostructures are oxidized at lower temperatures than silicon atoms in the bulk of the silicon nanostructure (Reference: Bardet et al., Phys. Chem. Chem. Phys. (2016), 18, 18201). TGA analysis shows that silicon is oxidized to silicon dioxide (SiO 2 The relative amount of surface silicon can be quantified based on the weight gain observed as the silicon becomes finer (fine) and coarse (coarse) silicon in the sample. By plotting the weight gain versus temperature, the fine and coarse silicon in the sample can be distinguished and quantified.

[0086] A determination of the amount of unoxidized surface silicon is obtained from the characteristic TGA traces of these materials, as shown in Figure 1. After an initial mass loss up to about 300 °C (shown in Figure 1 as a mass loss from (a) to (b)), a large mass increase begins to be observed at about 400 °C, with a peak being obtained between 550 and 650 °C (shown in Figure 1 as a mass increase from (b) to (c)). The porous carbon skeleton is then oxidized to CO 2 When it becomes a gas, a mass loss is observed (mass loss from (c)). Then, at temperatures above about 800°C, the silicon SiO 2A mass increase is again observed, corresponding to a continuing change to . This increases towards an asymptotic value above 1000°C as the oxidation of the silicon approaches completion (mass increase from (d) to (e)). The temperature at which the weight increase occurs is related to the structure of the silicon; at the surface of the silicon structure, silicon is oxidized at lower temperatures, and in the bulk of the silicon, it is oxidized at higher temperatures. Thus, at higher temperatures, the silicon domains become coarser and more oxidation is observed.

[0087] Coarse silicon is defined herein as silicon that is oxidized above 800° C. as measured by TGA, where the TGA is performed under air at a ramping temperature of 10° C. / min. This is shown in FIG. 1 as increasing in mass from (d) to (e). The content of coarse bulk silicon is therefore defined according to the following formula: Z = 1.875 × [(M f -M 800 ) / M f ]×100% where Z is the percentage of unoxidized silicon at 800°C, and M 800 is the mass of the sample at 800°C (mass (d) in Figure 1), and M f is the mass of the ash at the completion of oxidation at 1400°C (mass (e) in Figure 1). In this analysis, any mass increase at temperatures above 800°C is due to the addition of silicon SiO 2 The total mass at the end of oxidation is SiO 2 For completeness, 1.875 is assumed to be O 2 SiO 2 The molar mass ratio of SiO formed to the mass increase due to the addition of oxygen (i.e. 2 It is understood that the mass ratio is

[0088] In a second aspect of the present invention, there is provided a particulate material comprising a plurality of core-shell composite particles obtainable by the method described above.

[0089] In a third aspect of the present invention, A particulate material comprised of a plurality of core-shell composite particles, The core-shell composite particles are (a) a core, (i) a porous carbon skeleton having micropores and / or mesopores, the micropores and / or mesopores having a size of at least 0.4 cm as measured by gas adsorption techniques; 3 / g total pore volume, and the PD of said porous carbon skeleton 50 A porous carbon skeleton having a pore diameter of 10 nm or less, preferably 5 nm or less; (ii) a plurality of electroactive material domains disposed within the micropores and / or mesopores of the porous carbon framework; and A core having (b) an outer shell of a pyrolyzable conductive carbon material surrounding at least a portion of the core; and A particulate material is provided having the following structure:

[0090] If desired, the pyrolyzable conductive carbon coating may also infiltrate into the pores of the porous carbon skeleton.

[0091] The core-shell composite particles may have different electroactive material loading ranges. For example, the amount of electroactive material in the precursor composite particles may be selected such that at least 25% and up to 80% or more of the internal pore volume of the porous carbon scaffold is occupied by the electroactive material. For example, the electroactive material may occupy 25% to 60%, 25% to 55%, 25% to 50%, 25% to 45%, or 25% to 40% of the internal pore volume of the porous carbon scaffold. Within these preferred ranges, the pore volume of the porous carbon scaffold effectively accommodates the expansion of the electroactive material during charging and discharging, and excess pore volume that does not contribute to the volumetric capacity of the core-shell composite particles is avoided. However, the amount of electroactive material is not so high that inadequate metal ion diffusion rates or inadequate expansion volume create mechanical resistance to lithiation and prevent effective lithiation.

[0092] The electroactive material in the precursor composite particles is preferably selected from silicon, tin, germanium, aluminum and mixtures thereof. A preferred electroactive material is silicon.

[0093] The core-shell composite particles are preferably substantially free of silicon carbide. The core-shell composite particles are preferably substantially free of silicon nitride. The presence or absence of silicon carbide and silicon nitride can be determined by X-ray diffraction (XRD) analysis. Suitable apparatus and methods for this purpose are well known to those skilled in the art.

[0094] The core-shell composite particles have a D range of 1.5 to 60 μm. 50 It is preferred to have a particle diameter.

[0095] If necessary, the D of the core-shell composite particles 50 The particle diameter may be at least 2 μm, at least 3 μm, at least 4 μm, or at least 5 μm. If desired, the D of the core-shell composite particles 50 The particle diameter may be 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, 18 μm or less, or 15 μm or less.

[0096] For example, the core-shell composite particles may have a D in the range of 2 to 50 μm, 2 to 40 μm, 2 to 30 μm, 3 to 30 μm, 3 to 25 μm, 3 to 20 μm, 4 to 25 μm, 4 to 20 μm, 4 to 18 μm, 5 to 20 μm, 5 to 18 μm, 5 to 15 μm. 50 The core-shell composite particles may have a particle diameter of 0.1 to 1.0 mm. Core-shell composite particles within these size ranges and having the porosity and pore diameter distributions described herein are ideally suited for the preparation of composite particles for use in metal ion battery anodes due to their good dispersibility in slurries, structural robustness, high capacity retention over repeated charge-discharge cycles, and suitability for forming dense electrode layers of uniform thickness in the conventional thickness range of 20 to 50 μm.

[0097] The core-shell composite particles are 50m 2 It is preferred that the BET surface area is less than or equal to 30 m 2 / g or less, more preferably 15m 2 / g or less, or 12m 2 / g or less, or 10m 2 / g or less, or 8m 2 / g or less, or 6m 2 / g or less, or 5m 2 The composite particles have a particle size of at least 0.1 m 2 / g, or at least 0.5m 2 / g, at least 1m 2 / g, or at least 2m 2 / g, or at least 3m 2 / g BET surface area.

[0098] The particulate material of the present invention may have a specific capacity upon lithiation of from 1200 to 2340 mAh / g, measured per gram of particulate material.

[0099] In a fourth aspect of the invention there is provided a composition comprising a particulate material according to the second or third aspect of the invention and at least one other component. The at least one other component may suitably be selected from one or more of: (i) a binder, (ii) a conductive additive, and (iii) an additional particulate electroactive material. The composition of the fourth aspect of the invention may in particular be used as an active layer in the anode of a metal ion battery.

[0100] The composition may have from 1 to 95%, or from 2 to 90%, or from 5 to 85%, or from 10 to 80% by weight of the particulate material of the invention, based on the total dry weight of the composition.

[0101] The binder may be present in an amount of from 0.5 to 20 wt%, or from 1 to 15 wt%, or from 2 to 10 wt%, based on the total dry weight of the electrode composition.

[0102] The one or more conductive additives may be present in a total amount of from 0.5 to 20 wt %, or from 1 to 15 wt %, or from 2 to 10 wt %, based on the total dry weight of the electrode composition.

[0103] The optional at least one additional particulate electroactive material may be selected from graphite, hard carbon, silicon, tin, germanium, gallium, aluminum and lead.

[0104] In a fifth aspect, the present invention provides an electrode having a particulate material according to the second or third aspect of the present invention in electrical contact with a current collector. If desired, the particulate material may be in the form of a composition according to the fourth aspect of the present invention.

[0105] In a sixth aspect, the present invention provides a rechargeable metal-ion battery comprising: (i) an anode, the anode comprising an electrode according to the fifth aspect of the present invention; (ii) a cathode having a cathode active material capable of releasing and resorbing metal ions; (iii) an electrolyte between the anode and the cathode; A rechargeable metal ion battery is provided having the following structure:

[0106] In a seventh aspect, the present invention provides the use of a particulate material according to the second or third aspect of the present invention as an anode active material, in which the particulate material may be in the form of a composition of the present invention.

[0107] The present invention will now be described with reference to examples and the accompanying drawings. [Brief description of the drawings]

[0108] [Figure 1] FIG. 2 shows a characteristic TGA trace of a particulate material according to the present invention having low levels of coarse silicon. [Diagram 2] FIG. 1 shows thermogravimetric analysis (TGA) data for Example 4. [Diagram 3]FIG. 1 shows X-ray diffraction (XRD) data for Example 4. [Figure 4] FIG. 13 shows cell data of Example 5. [Diagram 5] FIG. 13 shows the effect of temperature on the coarse silicon content in Example 4. [Figure 6] FIG. 1 shows XRD data of Example 6. [Figure 7] FIG. 13 is a graph showing the effect of temperature on the amount of coarse silicon in Example 7. [Figure 8] FIG. 1 shows the effect of temperature on capacity retention over 100 cycles. The numbers for each data point indicate the level of roughened silicon. [Figure 9] FIG. 1 shows the effect of temperature on capacity retention over 200 cycles. The numbers for each data point indicate the level of roughened silicon. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0109] (example) The porous carbon skeletons C1 to C3 used in the following examples have the characteristics shown in Table 1.

[0110] [Table 1] (Example 1: Preparation of particulate material in a fluidized bed reactor) Silicon-carbon composite particles were prepared in a vertical bubbling fluidized bed reactor with a stainless steel cylindrical vessel with an internal diameter of 83 mm. A quantity of powder of carbon skeleton particles with the properties listed in Table 1 is placed in the reactor. The reactor is injecting a slow flow rate of inert gas (nitrogen) to remove oxygen. The reactor is then heated to a reaction temperature between 430 and 500° C., and 4% by volume monosilane gas diluted in nitrogen is fed to the bottom of the reactor at a flow rate sufficient to fluidize the carbon skeleton particles for a sufficient length of time to deposit the target mass of silicon. The reactor is purged under nitrogen for 30 minutes and then cooled to room temperature over several hours. The atmosphere is then gradually switched to air over a period of 2 hours by switching the gas flow from nitrogen to air from a compressed air supply.

[0111] (Example 2: Preparation of granular materials in a static furnace) Silicon-carbon composite particles were prepared by placing 1.8 g of particulate porous scaffolds with the properties listed in Table 1 on a stainless steel plate with a constant thickness of 1 mm along its length. The plate was then placed in a stainless steel tube with an outer diameter of 60 mm, which had gas inlet and outlet lines located in the hot zone of a retort furnace. After purging the furnace tube with nitrogen gas for 30 minutes at room temperature, the sample temperature was increased from 450 to 475°C. The nitrogen gas flow rate was adjusted to ensure a gas residence time of at least 90 seconds in the furnace tube and to maintain this flow rate for 30 minutes. The gas supply was then switched from nitrogen to a gas mixture containing monosilane at a concentration of 1.25 vol% in nitrogen. Dosing of monosilane is carried out for a period of up to 5 hours. The reactor pressure is maintained at 101.3 kPa (1 atm). After dosing is completed, the gas flow rate is held constant while silane is purged from the furnace with nitrogen. The furnace is purged under nitrogen for 30 minutes and then allowed to cool to room temperature over several hours.The atmosphere is then gradually switched to air over a period of 2 hours by switching the gas flow from nitrogen to air from a compressed air supply.

[0112] (Example 3: Measurement of weight percent of coarse silicon) The procedure used in calculating the coarse silicon for the example composites was as follows: 10-20 mg of the sample to be tested was loaded into a 70 μL crucible. The sample was loaded into a Mettler Toledo TGA / DSC3+ instrument. 100 mL / min of Ar purge gas, N 2 Padding gas and air reactant gas were used. The TGA furnace chamber was heated from 25° C. to 1400° C. at a rate of 10° C. / min. Data were collected at 1 second intervals.

[0113] The amount of coarse silicon was determined by determining the final mass of the ash at the end of the TGA test and the mass at 800° C. The formula above is used to calculate the coarse silicon (Z) value.

[0114] Example 4 - Heat Treatment of Uncoated Particles Silicon-carbon composite particles were prepared using 125 g of carbon C1 and the method of Example 1. The silicon-carbon composite particles were separated into five samples. Each sample was then individually jet milled for 25 minutes using a Hosokawa Alpine 50 AS Spiral Jet Mill at 8 bar feed gas pressure and a feed rate of 8 rpm. After jet milling and prior to any heat treatment steps, the resulting volumetric particle size distributions were measured using laser diffraction as previously described, resulting in Table 2.

[0115] The first sample was used as a reference sample and was not subjected to any further treatment. The remaining four samples were flushed in argon flow at a flow rate of 1 L / min for 30 min, then ramped at 5°C / min to the corresponding heat treatment temperature of 600°C, 700°C, 800°C, or 900°C, and then held at the heat treatment temperature for 1 h. The properties of the silicon-carbon composite precursor particles were measured after heat treatment and compared with the reference sample.

[0116] (result) The reference sample and the heat-treated samples were subjected to various analyses to compare the effect of each temperature on the material properties.

[0117] Thermogravimetric analysis (TGA) in air (Figure 2) confirmed that samples exposed to heat treatment at 800°C and 900°C suffered from the formation of larger silicon domains via thermal treatment of the fine micropore structure and fusion of nanoscale silicon domains within the pore structure. The sample heat treated at 600°C showed a nearly identical TGA profile to the reference sample, indicating that the carbon coating process on these silicon-carbon composite precursor particles is highly unlikely to damage the fine micropore structure, which is highly desirable for the use of particulate materials in anodes.

[0118] Figure 5 shows the amount of coarse silicon in each sample, as measured by the method of Example 3. The reference sample is designated as 430 and the other samples are designated by the temperature of the heat treatment step to which they were subjected. Fine silicon is more desirable than coarse silicon in the final product. Figure 5 shows that any treatment steps carried out at temperatures above 700°C tend to result in a final particulate product with a higher proportion of coarse silicon compared to products (e.g., carbon coated) treated at temperatures below 700°C.

[0119] Total pore volume and BET surface area were evaluated using the methods previously described.

[0120] [Table 2] These data show that the total pore volume decreases with increasing treatment temperature. The total pore volumes obtained for the 800°C and 900°C samples are reduced to unfavourable levels, which can be explained by the thermal treatment of the pores at these high temperatures.

[0121] The total pore volume and BET surface area depend on the particle size of the sample. The increase in the BET surface area and total pore volume of the sample heat treated at 600°C compared to the reference sample is explained by the fact that the sample heat treated at 600°C has a larger particle size than all the other samples since the samples were jet milled individually.

[0122] The chemical composition of five samples was further analyzed using X-ray diffraction (XRD), and the results are shown in Figure 3.

[0123] Up to 700°C, and especially up to 600°C, the characteristics of amorphous silicon, i.e. broad peaks, are evident. In the 700°C, 800°C, and 900°C samples, a degree of crystalline silicon variation is evident, especially in the 800°C and 900°C samples.

[0124] Evidence of silicon carbide is also evident in the 900°C samples. The formation of silicon carbide is undesirable in silicon-carbon composite particles because silicon carbide is not electrochemically active and is a poor electrical conductor. Thus, the formation of this compound reduces the overall effectiveness of the product in conjunction with the anode.

[0125] Further testing of the electrodes was carried out, with one of the test samples of particulate material being introduced into each of the electrodes.

[0126] Example 5 - Electrochemical Testing A test coin cell was fabricated using a negative electrode with the composite material prepared as described in Example 4. Carbon Super P (conductive carbon) was dispersed in the CMC binder and mixed in a Thinky™ mixer. Silicone-based material was added to the mixture and mixed in the Thinky™ mixer for 30 minutes. SBR binder was then added to obtain a 1:1 CMC:SBR ratio to obtain a slurry with 70%:16%:14% silicon-based material:CMC / SBR:conductive carbon by weight. The slurry was further mixed in the Thinky™ mixer for 30 minutes. It was then coated on a 10 μm thick copper substrate (current collector) and dried at 50° C. for 10 minutes. It was further dried at 110° C. for 12 hours to form an electrode with an active layer on the copper substrate.

[0127] Using a ring-shaped electrode with a radius of 0.8 cm cut from the electrode, a porous polyethylene separator, lithium foil as a counter electrode, and a 7:3 solution of EC / FEC (ethylene carbonate / fluoroethylene carbonate) containing 3 wt% vinylene carbonate were mixed with 1 M LiPF 6 A coin half-cell was fabricated having an electrolyte containing

[0128] Using these half cells, the initial volumetric energy density (VED2, mAh / cm 3), first cycle loss (FCL), and first delithiation capacity (DC1) of the active layer were measured. The half-cell was evaluated by applying a constant current of C / 25 (where "C" represents the specific capacity of the electrode in mAh and "25" represents 25 hours) to lithiate the electrode with the porous particles with a cutoff voltage of 10 mV. Once the cutoff is reached, a constant voltage of 10 mV is applied. The cutoff current is C / 100. The cell is then rested for 10 minutes in the lithiation state. The electrode is then delithiated with a constant current of C / 25 with a cutoff voltage of 1 V, after which the cell is rested for 10 minutes. The cell is then subjected to a second lithiation with a constant current of C / 25 and a cutoff voltage of 10 mV. A constant voltage of 10 mV with a cutoff current of C / 100 is then applied and rested for 5 minutes.

[0129] The effect of silicon carbide formation on cell performance is shown in Figure 4. The delithiation capacity, measured as described above, is significantly reduced for the 900°C heat treated samples, indicating a detrimental effect of silicon carbide formation on the anode performance.

[0130] Also shown in Figure 4 is the thickness change of the electrode coating (excluding the current collector) for electrodes prepared and evaluated using half cells as described above. The thickness change was measured ex situ in the charged state as a percentage after removing the anode after lithiation, delithiation, and second lithiation cycles in the lithium-ion half cells. In other words, the thickness change was measured for the anode in the lithiated state.

[0131] The anode incorporating the particulate material subjected to a 900°C heat treatment showed the greatest increase in thickness, suggesting that a carbon coating step at the same temperature would have an unfavorable effect on the utility of the particulate material in the anode. Typically, the degree of electrode expansion would be expected to correlate positively with the amount of active silicon. However, the opposite was observed for the electrode containing the 900°C sample. Without wishing to be bound by theory, it is believed that the fact that this electrode showed the highest degree of expansion of all the samples indicates that the structural and chemical relationships within the particulate material have deteriorated so adversely that particle expansion is no longer controlled. This excessive expansion is expected to lead to isolated particles and poor cycle retention.

[0132] Further electrode property data was measured for anodes each incorporating one of the samples, and the results of these tests are shown in Table 3 and FIG.

[0133] These data show that the first lithiation capacity and the first delithiation capacity of the samples incorporated in the electrodes both decrease with increasing heat treatment temperature. The percentage of active silicon relative to the total particle mass also decreased with increasing heat treatment temperature. The active silicon content of the composite particles was calculated by dividing the first delithiation capacity of the half-cell (per mAh of composite particles) by the theoretical capacity of silicon (3579 mAh / g), and the result is expressed as a percentage. The first cycle loss increases with increasing heat treatment temperature, especially for the 900°C treated sample. The anode thickness increased for all samples after 1.5 cycles. However, the thickness increase was nearly constant for the reference sample, the 600°C treated sample, and the 700°C treated sample, whereas the 800°C and 900°C treated samples showed a large increase in electrode thickness. For batteries, it is desirable to keep the electrode thickness as constant as possible.

[0134] Overall, the volumetric capacity of the anodes was similar for the 600° C. treated and reference samples, decreased slightly for the 700° C. treated samples, and decreased significantly for the 800° C. and 900° C. treated samples.

[0135] These tests were performed in a half-cell with silicon-carbon composite precursor particles without a carbon coating, however the results are expected to be reproduced with a carbon coating, suggesting that the high temperature carbon coating process adversely affects the properties of the carbon-coated particulate silicon-carbon composite product.

[0136] [Table 3-1] (Example 6 - Uncoated sample) Evaluation Procedure Silicon-carbon composite particles were prepared using 125 g of carbon C1 and the method of Example 2. The heat treatment test procedure of Example 4 was repeated, except that there was no jet milling step prior to the heat treatment step, and the heat treatment step was carried out in a nitrogen atmosphere instead of an argon atmosphere.

[0137] (result) The heat treated and reference samples were analyzed using XRD, and the results are shown in Figure 6. The heat treatment temperature for each sample is on the right side of the XRD plot, with the XRD trace for the 600°C sample shown on the front side and the XRD trace for the 900°C sample shown on the back side.

[0138] An important effect observed depending on the heat treatment temperature was the formation of compounds. In particular, in the 800 and 900 °C samples, Si 3 N 4and SiC. This is an undesirable result since it reduces the overall capacity of the material, thereby making it less valuable as an anode material. Furthermore, SiC is a poor conductor of electricity, and its presence in the final product may interfere with the lithiation of silicon within the granular material, making it even more undesirable.

[0139] The absence of silicon nitride formation after heat treatment at temperatures below 700° C. is an important advantage since it means that the method of the present invention can be carried out in a nitrogen atmosphere instead of an argon atmosphere.

[0140] Similarly, in the 800° C. and 900° C. samples, crystallization of silicon was observed, which is undesirable: the preferred form of silicon for these materials is amorphous silicon.

[0141] For the 700 °C sample, a mixture of amorphous and crystalline silicon was observed in the XRD data: at this temperature, a small crystalline silicon peak overlaps a broad amorphous peak, and if silicon crystallization occurs, this is thought to be an indication of an increase in the average length scale of silicon domains within the particulate material caused by the heat treatment.

[0142] The deposition of the carbon coating in the method of the present invention takes approximately the same time that the samples were held at their respective temperatures in these tests. By evaluating uncoated particles, the effect of temperature on the microstructure of the composite particles can be more easily observed than when they are coated. It is expected that similar effects will be observed when carbon deposition is performed at the same temperatures.

[0143] Thus, the method of the present invention, in which carbon deposition is performed at temperatures below 700° C., is expected to avoid or mitigate the deleterious effects observed in this experiment at 800° C. and 900° C., and thus provide the benefits of the conductive coating and pore capping while preserving the significant microstructure previously developed by the inventors. At temperatures below 600° C., the material properties of the particles are more suitable for use in the anode.

[0144] (Example 7: Carbon coating) A series of composite particle samples were prepared using carbon skeletons C2 and C3 by the method of Example 1. The precursor particles had the properties listed in Table 3. The amount of coarse silicon was determined using the TGA method described in Example 3. All composite particle samples contained less than 4 wt% coarse silicon.

[0145] [Table 3-2] The composite particulate samples listed in Table 3 were carbon coated by the following method: The mixed particles (60 g) were placed in a stainless steel tube (57 mm diameter, 500 mm length) packed (sealed) in the heating zone of a rotary furnace. The reactor space was purged with nitrogen at 0.2 L / min for 30 minutes. In the presence of nitrogen flow, the furnace temperature was increased to the temperature listed in Table 4. An excess amount of styrene was placed in a Drescher bottle and heated up to 75° C. in a water bath. After stabilizing the furnace temperature for 10 minutes, styrene was flowed into the reactor tube for up to 90 minutes by bubbling nitrogen at 2 L / min into the Drescher bottle (as shown in Table 4). The reactor was then purged with nitrogen and cooled to ambient temperature under nitrogen to obtain the carbon coated material.

[0146] The carbon coated particles from Example 7 were analyzed for elemental composition and coarse silicon content, again using the TGA method described in Example 3. The results are shown in Table 4 and FIG. S1(58m 2 / g) and S10(22m 2 / g), all carbon-coated particles showed a range of 6 to 12 m2 BET surface areas in the range of / g were obtained.

[0147] [Table 4] *Comparative example The data in Table 4 show that when carbon coating is performed at temperatures below 700°C, the relative increase in coarse silicon is less than 190% in all cases. However, when temperatures exceed 700°C, the amount of coarse silicon increases significantly. This suggests that particles coated at temperatures above 700°C form large silicon domains due to heat treatment of the fine micropore structure and nanoscale silicon domains within the pore structure. This therefore supports the hypothesis in Example 4 that the changes in silicon domains observed upon heating of uncoated particles are also observed during the carbon coating process.

[0148] (Example 8 - Electrochemical evaluation of coated particles) The Si-C composites in Table 4 were used to prepare negative electrode coatings (anodes) and tested in full coin cells. To make the electrodes, a dispersion of carbon black was mixed in a CMC binder in a Thinky™ mixer. The Si-C composites were added to the mixture and mixed in a Thinky™ mixer for 30 minutes. SBR binder was then added to achieve a 1:1 CMC:SBR ratio to form a slurry with a weight ratio of 70%:16%:14% Si-C composite:CMC / SBR:carbon black. The slurry was mixed in the Thinky™ mixer for an additional 30 minutes and then coated on a 10 μm thick copper substrate (current collector) and dried at 50° C. for 10 minutes. It was then further dried at 110° C. for 12 hours, resulting in a coating density of 0.7±0.5 g / cm. 3 A negative electrode was formed.

[0149] A full coin cell was fabricated with a porous polyethylene separator and a nickel manganese cobalt oxide (NMC532) cathode using a ring-shaped anode cut from the anode with a radius of 0.8 cm. The cathode and anode were designed to form a balanced set such that the capacity ratio of the cathode to the anode was 0.9. Next, 1 M LiPF was dissolved in a solution of fluoroethylene carbonate, ethylene carbonate, and ethyl methyl carbonate containing 3 wt% vinylene carbonate. 6 An electrolyte having a pH of 10 was added to the cell before sealing.

[0150] The coin cells were cycled as follows: A constant current was applied at a rate of C / 25 to lithiate the anode. The cutoff voltage was 4.3V. Once the cutoff was reached, a constant voltage of 4.3V was applied until a cutoff current of C / 100 was reached. The cell was then left to rest for 10 minutes in the lithiated state. The anode was then delithiated at a constant current of C / 25 with a cutoff voltage of 2.75V. The cell was then left to rest for 10 minutes. After this first cycle, a constant current of C / 2 was applied to lithiate the anode with a cutoff voltage of 4.3V, followed by a constant voltage of 4.3V with a cutoff current of C / 40 with a rest time of 5 minutes. The anode was then delithiated at a constant current of C / 2 with a cutoff of 2.75V. This was then repeated for the desired number of cycles. The capacity retention at 100 cycles (CR100) and 200 cycles (CR200) ​​was calculated. This is shown in Table 5 along with the first lithiation capacity, first delithiation capacity, and first cycle loss (FCL).

[0151] The charge (lithiation) and discharge (delithiation) capacities for each cycle are calculated per unit mass of silicon-carbon composite, and the capacity retention is calculated for each discharge capacity as a percentage of the discharge capacity at the second cycle. The first cycle loss (FCL) is (1-(1st delithiation capacity / 1st lithiation capacity)) x 100%. The values ​​in Table 5 are averaged over three coin cells of each material.

[0152] The active silicon levels are determined from half-cell experiments as described in Example 5.

[0153] The data in Table 5 show that the increase in coarse Si weight percent with increasing carbon coating temperature is reflected in a degradation of the electrochemical properties. As the level of coarse silicon increases, the amount of active silicon in the material (determined from half cells) decreases, the initial lithiation and delithiation capacity of the material decreases, and the normalized capacity retention over multiple charge-discharge cycles decreases. Figures 8 and 9 show the normalized capacity retention of these materials.

[0154] [Table 5] *Comparative example **To facilitate comparison between samples with different initial capacities, the capacity retention values ​​in Table 5 have been normalized to 45 wt. % active silicon by multiplying the capacity retention percentage by the active Si value and dividing by 45.

Claims

1. 1. A method for preparing core-shell composite particles, comprising: (a) Below: i. A porous carbon skeleton having micropores and / or mesopores, the total pore volume of the micropores and mesopores being at least 0.6 cm as measured by gas adsorption techniques. 3 / g and 1.2 cm 3 / g or less, and the PD of the porous carbon skeleton is 50 The pore diameter is 2.5 nm or less, and the PD of the porous carbon skeleton is 90 A porous carbon scaffold having a pore diameter of at least 3 nm and no greater than 10 nm; and ii. a plurality of nanoscale electroactive material domains disposed within the porous carbon skeleton, the electroactive material being silicon. providing a plurality of precursor composite particles comprising: (b) heat treating the plurality of precursor composite particles by contacting them with a pyrolyzable carbon precursor, wherein an outer shell of pyrolyzable conductive carbon material is formed on the precursor composite particles, the heat treating being at a temperature of 680° C. or less; The method comprising:

2. 2. The method of claim 1, wherein the heat treatment is carried out at 660°C or less, or 650°C or less, or 640°C or less, or 620°C or less, or 600°C or less.

3. 3. The method of claim 1 or claim 2, wherein the heat treatment is carried out at a temperature of at least 500°C, or at least 520°C, or at least 540°C, or at least 560°C, or at least 580°C.

4. 4. The method of claim 1, wherein the pyrolytic carbon precursor is contacted with the composite particles as a vapor.

5. The method of claim 4 , wherein the vapor is a hydrocarbon vapor.

6. 6. The method of claim 5, wherein the hydrocarbon is selected from polycyclic hydrocarbons having from 10 to 25 carbon atoms and optionally from 1 to 3 heteroatoms.

7. 7. The method of claim 6, wherein the polycyclic hydrocarbon is selected from naphthalene, anthracene, tetracene, pentacene, fluorene, acenaphthene, phenanthrene, fluoranthrene, pyrene, chrysene, perylene, coronene, fluorenone, anthraquinone, anthrone, and alkyl substituted derivatives thereof.

8. 6. The method of claim 5, wherein the hydrocarbon is selected from bicyclic monoterpenoids.

9. 9. The method of claim 8, wherein the bicyclic monoterpenoid is selected from camphor, borneol, eucalyptol, camphene, careen, sabinene, thujene, and pinene.

10. The hydrocarbon is C 2 From C 10 is selected from the group consisting of 6. The method of claim 5, wherein the hydrocarbon is selected from an alkane, an alkene, an alkyne, a cycloalkane, a cycloalkene, and an arene.

11. 11. The method of claim 10, wherein the hydrocarbon is selected from methane, ethylene, propylene, and acetylene.

12. 12. The method of claim 4, wherein the pyrolytic carbon precursor vapor is contacted with a transition metal catalyst at a temperature of at least 500°C prior to contacting the composite particles.

13. 13. The method of claim 12, wherein the transition metal catalyst comprises nickel, iron, cobalt, copper and mixtures thereof.

14. the transition metal catalyst is in the form of a mesh; 14. The method of claim 12 or 13, wherein the mesh is disposed in the flow path of the hydrocarbon vapor prior to contacting the composite particles.

15. 14. The method of claim 12 or 13, wherein the transition metal catalyst is disposed on a surface of the composite particles.

16. 12. The method of claim 1, wherein prior to step (b), gaseous nickel carbonyl is pyrolyzed to deposit nickel on the surfaces of the composite particles.

17. 17. The method of claim 16, wherein after step (b), the carbon coated particulate material is contacted with carbon monoxide gas to form gaseous nickel carbonyl, thereby removing nickel from the carbon coated composite particles.

18. Step (b) contacting the composite particles with a dispersion or solution of a pyrolytic carbon precursor in a solvent; removing the solvent prior to the heat treatment to provide composite particles coated with the pyrolytic carbon precursor; 4. The method according to claim 1 , further comprising:

19. 20. The method of claim 18, wherein the pyrolyzable carbon precursor is a polymer or oligomer that includes a carbon-containing backbone.

20. 20. The method of claim 18 or claim 19, wherein the pyrolyzable carbon precursor is polyvinylpyrrolidone (PVP) or a copolymer of vinylpyrrolidone and one or more other ethylenically unsaturated monomers.

21. 21. A method according to any preceding claim, wherein the outer shell of pyrolytic conductive carbon material has a thickness of 10 nm or less, or 5 nm or less, or 4 nm or less, or 2 nm or less, or 1 nm or less.

22. The total pore volume of micropores and mesopores, as measured by gas adsorption, is at least 0.65 cm 3 / g or at least 0.7 cm 3 / g and at least 0.75 cm 3 / g or at least 0.8 cm 3 / g or at least 0.85 cm 3 / g or at least 0.9 cm 3 / g or at least 0.95 cm 3 / g or at least 1 cm 3 / g or at least 1.05 cm 3 / g or at least 1.1 cm 3 22. The method according to claim 1, wherein the molecular weight is 1 / g.

23. The PD of the porous carbon framework 50 23. The method of any one of claims 1 to 22, wherein the pore diameter is 2 nm or less, or 1.5 nm or less, or 1 nm or less.

24. 24. The method of claim 1, wherein the step (a) of providing a plurality of precursor composite particles comprises contacting a plurality of porous carbon particles with a silicon precursor gas at a temperature between 400° C. and 650° C., thereby depositing silicon in pores of the carbon particles.

25. 25. The method of claim 24, wherein the temperature is between 400°C and 500°C.

26. The silicon precursor gas is silane (SiH 4 ), disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ) Tetrasilane (Si 4 H 10 26. The method according to claim 24 or 25, wherein the silane is selected from the group consisting of chlorosilanes, methylchlorosilanes, and preferably silanes.

27. The precursor composite particles have a D of at least 1 μm, or at least 2 μm, or at least 3 μm, or at least 4 μm, or at least 5 μm. 50 27. The method of claim 1, having a particle diameter.

28. The precursor composite particles have a D of 50 μm or less, or 40 μm or less, or 30 μm or less, or 25 μm or less, or 20 μm or less, or 15 μm or less, or 12 μm or less, or 10 μm or less. 50 28. The method of claim 1, having a particle diameter.

29. 29. The method of claim 1, wherein the volumetric fill factor of the electroactive material within the porous carbon skeleton, based on the volume of the micropores and / or mesopores, is 85% or less, or 75% or less, or 65% or less, or 55% or less, or 45% or less.

30. 30. The method of claim 1, wherein the volumetric filling of the electroactive material within the porous carbon skeleton, based on the volume of the micropores and / or mesopores, is at least 20%, or at least 25%.

31. 31. The method of claim 1, wherein the porous carbon skeleton comprises at least 80% by weight carbon, or at least 85% by weight carbon, or at least 90% by weight carbon, or at least 95% by weight carbon.

32. 32. The method of claim 1, wherein the electroactive material is selected from silicon, tin, germanium, aluminium and mixtures thereof.

33. The method of claim 32 , wherein the electroactive material is silicon.

34. 34. The method of any one of claims 1 to 33, wherein the duration of the heat treatment in step (b) is from 1 to 3 hours.

35. The step (a) further comprises: (a2) contacting the surface of the deposited silicon with a passivation agent; having 35. The method of claim 1, wherein the silicon is not exposed to oxygen prior to contact with the passivation agent.

36. The passivator has the general formula (i) R−CH=CH−R, (ii) R-CH≡CH-R, (iii) O=CH-R is selected from one or more compounds of where R represents H or an unsubstituted or substituted aliphatic or aromatic hydrocarbyl group having 1 to 20 carbon atoms, preferably 2 to 10 carbon atoms, or 36. The method of claim 35, wherein the two R groups in formula (i) form an unsubstituted or substituted hydrocarbyl ring structure having from 3 to 8 carbon atoms.

37. 37. The method of claim 35 or 36, wherein step (b) is carried out at the same temperature as step (a2) or at a higher temperature than step (a2).

Citation Information

Patent Citations

  • Composite and method for producing the same

    JP2016132608A

  • NANO silicon composite negative electrode material for lithium ion battery, production method and lithium ion battery

    JP2016134382A

  • Novel material having highly durable lithium insertion and method for manufacturing the same

    JP2018534720A

  • Manufacturing method of Si / C composite particles

    JP2019511444A