Ion conductive solid electrolyte and all-solid battery
A low-temperature process using specific metal element substitutions in the Li6+a-c-2dYb1-a-b-c-dM1aM2bM3cM4dB3O9 formula enhances ionic conductivity in all-solid-state batteries, addressing the high-temperature issues of conventional oxide-based electrolytes and improving battery performance.
Patent Information
- Application Number
- JP2024107128
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-03-14
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-02
AI Technical Summary
Conventional oxide-based solid electrolytes for all-solid-state batteries require high-temperature heat treatment, which can lead to the formation of high-resistance phases, reducing ionic conductivity and battery performance.
A low-temperature process for producing an ion-conductive solid with the formula Li6+a-c-2dYb1-a-b-c-dM1aM2bM3cM4dB3O9, where M1-M4 are specific metal elements, enhancing ionic conductivity by adjusting charge balance and lattice structure through element substitution.
The process enables the production of an ion-conductive solid with high ionic conductivity at lower temperatures, reducing the formation of high-resistance phases and improving battery performance.
Smart Images

Figure 2024133564000001 
Figure 2024133564000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to ion-conducting solid states and all-solid-state batteries. [Background technology]
[0002] 2. Description of the Related Art Lightweight, high-capacity lithium-ion secondary batteries have conventionally been mounted in mobile devices such as smartphones and notebook computers, and in transportation equipment such as electric vehicles and hybrid electric vehicles. However, because conventional lithium-ion secondary batteries use a liquid containing a flammable solvent as an electrolyte, there are concerns about the leakage of the flammable solvent and ignition in the event of a short circuit in the battery. In recent years, therefore, in order to ensure safety, secondary batteries that use an ion-conductive solid as an electrolyte, which is different from liquid electrolytes, have been attracting attention, and such secondary batteries are called all-solid-state batteries.
[0003] Solid electrolytes such as oxide-based solid electrolytes and sulfide-based solid electrolytes are widely known as electrolytes used in all-solid-state batteries. Among them, oxide-based solid electrolytes do not react with moisture in the air to generate hydrogen sulfide, and are therefore safer than sulfide-based solid electrolytes.
[0004] Incidentally, an all-solid-state battery has a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, an electrolyte containing an ion-conductive solid disposed between the positive electrode and the negative electrode, and a current collector as necessary (the positive electrode active material and the negative electrode active material are also collectively referred to as "electrode active material"). When an all-solid-state battery is produced using an oxide-based solid electrolyte, a heat treatment is performed to reduce the contact resistance between particles of an oxide-based material contained in the solid electrolyte. However, since a high temperature of 900°C or more is required for the heat treatment in the conventional oxide-based solid electrolyte, there is a risk that the solid electrolyte and the electrode active material will react to form a high-resistance phase. The high-resistance phase may lead to a decrease in the ion conductivity of the ion-conductive solid, and thus to a decrease in the output of the all-solid-state battery. Li is an oxide-based solid electrolyte that can be prepared by heat treatment at temperatures below 900°C. 2+x C1-x B x O3 is an example (Non-Patent Document 1). In addition, the above Li 2+x C 1-x B x It has been disclosed that the characteristics can be improved by adding specific elements to O3 in specific ratios (Patent Document 1). [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] Solid State Ionic 288 (2016) 248-252 [Patent documents]
[0006] [Patent Document 1] Patent No. 6948676 Summary of the Invention [Problem to be solved by the invention]
[0007] The present disclosure provides an ion-conductive solid that can be produced by heat treatment at a low temperature and has high ion conductivity, and an all-solid-state battery having the same. [Means for solving the problem]
[0008] The ionically conductive solids of the present disclosure have the general formula Li 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 d It is an ionically conductive solid characterized by containing an oxide represented by the formula B3O9. (In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr, and Ba, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, In and Fe; M3 is at least one metal element selected from the group consisting of Zr, Ce, Hf, Sn, and Ti; M4 is at least one metal element selected from the group consisting of Nb and Ta; a is a real number that satisfies 0.000≦a≦0.800, b is 0.000≦b≦0.900, c is 0.000≦c≦0.800, d is 0.000≦d≦0.800, and a, b, c, and d are real numbers that satisfy 0.000≦a+b+c+d<1.000.)
[0009] In addition, the all-solid-state battery of the present disclosure has A positive electrode and A negative electrode; An electrolyte; An all-solid-state battery having at least The all-solid-state battery is characterized in that at least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte contains the ion-conducting solid of the present disclosure. Effect of the Invention
[0010] According to one embodiment of the present disclosure, it is possible to obtain an ion-conductive solid that can be produced by a heat treatment at a low temperature and has high ion conductivity, and an all-solid-state battery having the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In the present disclosure, the description of a numerical range such as "XX or more and YY or less" or "XX to YY" means a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. When a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. In addition, in the present disclosure, the term "solid" refers to one of the three states of a substance that has a definite shape and volume, and the powder state is included in the category of "solid."
[0012] The ionically conductive solids of the present disclosure have the general formula Li6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 d It is an ionically conductive solid that contains the oxide represented by the formula B3O9. In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr, and Ba; M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, In and Fe; M3 is at least one metal element selected from the group consisting of Zr, Ce, Hf, Sn, and Ti; M4 is at least one metal element selected from the group consisting of Nb and Ta; a is a real number that satisfies 0.000≦a≦0.800, b is 0.000≦b≦0.900, c is 0.000≦c≦0.800, d is 0.000≦d≦0.800, and a, b, c, and d are real numbers that satisfy 0.000≦a+b+c+d<1.000.
[0013] The present inventors speculate as follows as to the reason why the ion conductivity is improved in the ion-conductive solid containing the oxide represented by the above general formula. In Comparative Example 1 of Patent Document 1, Y in Li6YB3O9 is replaced with Yb, which has a small ionic radius, and the lattice constant and lattice volume become small, resulting in Li + This makes it easier for ions to move, improving ionic conductivity. In addition, in Patent Document 1, a part of the trivalent metal element Y is replaced with a tetravalent or pentavalent metal element. By using Yb instead of Y, the lattice constant and lattice volume are reduced, and the ionic conductivity is improved. + Since the ions are more easily mobile, the ionic conductivity is further improved.
[0014] The ionically conductive solids of the present disclosure preferably have a monoclinic crystal structure.
[0015] The ion conductive solid of the present disclosure has a volume average particle size of preferably 0.1 μm to 28.0 μm, more preferably 0.2 μm to 26.0 μm, even more preferably 0.3 μm to 20.0 μm, even more preferably 0.3 μm to 15.0 μm, and even more preferably 0.5 μm to 10.0 μm. By being in the above range, the grain boundary resistance in the ion conductive solid is reduced, and the ion conductivity is further improved. The volume average particle size of the ion-conductive solid can be controlled by pulverization or classification.
[0016] In the above general formula, a is a real number that satisfies 0.000≦a≦0.800. a is 0.000≦a≦0.800, preferably 0.000≦a≦0.600, more preferably 0.000≦a≦0.400, even more preferably 0.000≦a≦0.100, particularly preferably 0.000≦a≦0.050, and extremely preferably 0.000≦a≦0.030.
[0017] In the above general formula, b is a real number that satisfies 0.000≦b≦0.900. b is 0.000≦b≦0.900, preferably 0.000≦b≦0.600, more preferably 0.000≦b≦0.500, even more preferably 0.000≦b≦0.400, still more preferably 0.000≦b≦0.100, particularly preferably 0.000≦b≦0.050, and extremely preferably 0.000≦b≦0.030.
[0018] In the above general formula, c is a real number that satisfies 0.000≦c≦0.800. c is 0.000≦c≦0.800, preferably 0.000≦c≦0.600, more preferably 0.000≦c≦0.400, even more preferably 0.000≦c≦0.150, even more preferably 0.000≦c≦0.100, particularly preferably 0.000≦c≦0.050, and extremely preferably 0.000≦c≦0.030. C may also be preferably 0.050≦c≦0.200, more preferably 0.080≦c≦0.150.
[0019] In the above general formula, d is a real number that satisfies 0.000≦d≦0.800. d is 0.000≦d≦0.800, preferably 0.000≦d≦0.600, more preferably 0.000≦d≦0.400, even more preferably 0.000≦d≦0.100, particularly preferably 0.000≦d≦0.050, and extremely preferably 0.010≦d≦0.030.
[0020] In the above formula, a+b+c+d is a real number that satisfies 0.000≦a+b+c+d<1.000. a+b+c+d is 0.000≦a+b+c+d<1.000, preferably 0.000≦a+b+c+d<0.900, more preferably 0.000≦a+b+c+d<0.800, even more preferably 0.000≦a+b+c+d<0.700, even more preferably 0.000≦a+b+c+d≦0.600, especially preferably 0.010≦a+b+c+d<0.500, particularly preferably 0.050≦a+b+c+d<0.300, and extremely preferably 0.080≦a+b+c+d<0.250.
[0021] Yb 1-a-b-c-d In this case, 1-abcd is 0.300≦1-abc -d is preferable, 0.500≦1-abcd is more preferable, 0.700≦1-abcd is even more preferable, and 0.750≦1-abcd is even more preferable. The upper limit is not particularly limited, but is preferably less than 1.000, 0.950 or less, or 0.900 or less.
[0022] The ion-conducting solid of the present disclosure may have the following embodiments, for example, but is not limited to these embodiments. (1) It is preferable that a satisfies 0.010≦a≦0.100, b satisfies 0.000≦b≦0.200, c satisfies 0.000≦c≦0.200, d satisfies 0.010≦d≦0.100, and a, b, c, and d satisfies 0.010≦a+b+c+d<0.300. (2) It is preferable that a satisfies 0.010≦a≦0.030, b satisfies 0.030≦b≦0.100, c satisfies 0.010≦c≦0.030, d satisfies 0.010≦d≦0.030, and a, b, c, and d satisfies 0.050≦a+b+c+d<0.160. (3) It is preferable that a satisfies 0.000≦a≦0.010, b satisfies 0.000≦b≦0.100, c satisfies 0.050≦c≦0.150, d satisfies 0.000≦d≦0.030, and a, b, c, and d satisfies 0.050≦a+b+c+d<0.250. In the above general formula, M1, M2, M3, and M4 may or may not be included in the formula. That is, at least one of a, b, c, and d may be 0.
[0023] In the above general formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba. M1 is at least one selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr and Ba, preferably at least one selected from the group consisting of Mg, Zn, Ca, Sr and Ba, more preferably at least one selected from the group consisting of Mg, Ca and Sr.
[0024] In the above general formula, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, In and Fe. M2 is at least one selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, In and Fe, preferably at least one selected from the group consisting of La, Eu, Gd, Tb, Dy, Lu, In and Fe, more preferably at least one selected from the group consisting of Gd, Dy, Lu, In and Fe.
[0025] In the above general formula, M3 is at least one metal element selected from the group consisting of Zr, Ce, Hf, Sn and Ti. M3 is at least one selected from the group consisting of Zr, Ce, Hf, Sn and Ti, preferably at least one selected from the group consisting of Zr, Ce, Hf and Sn, more preferably at least one selected from the group consisting of Zr, Ce and Hf.
[0026] In the above general formula, M4 is at least one metal element selected from the group consisting of Nb and Ta. M4 is at least one selected from the group consisting of Nb and Ta, and is preferably Nb.
[0027] Furthermore, a part of the trivalent metal element Yb is replaced with specific elements M1, M2, M3, and M4. When substituted within a fixed ratio, the charge balance is adjusted by the substitution of elements with different valences. Therefore, the Li + The Li + In an attempt to fill the deficiency of + The ionic conductivity is improved due to the movement of
[0028] Next, a method for producing the ion-conductive solid of the present disclosure will be described. The method for producing an ion-conductive solid according to the present disclosure can be, but is not limited to, the following aspects. General formula Li 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 dA method for producing an ionically conductive solid containing an oxide represented by B3O9, comprising the steps of: The method may include a primary firing step in which raw materials mixed to obtain an oxide represented by the general formula are heat-treated at a temperature below the melting point of the oxide. In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr, and Ba, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, In, and Fe, M3 is at least one metal element selected from the group consisting of Zr, Ce, Hf, Sn, and Ti, M4 is at least one metal element selected from the group consisting of Nb and Ta, a is 0.000≦a≦0.800, b is 0.000≦b≦0.900, c is 0.000≦c≦0.800, d is 0.000≦d≦0.800, and a, b, c, and d are real numbers that satisfy 0.000≦a+b+c+d<1.000.
[0029] The method for producing an ion-conductive solid according to the present disclosure may include a primary firing step of weighing and mixing raw materials so as to obtain an oxide represented by the above general formula, and heat-treating the raw materials at a temperature below the melting point of the oxide to produce an ion-conductive solid containing the oxide. The ion-conductive solid can be obtained by the primary firing step. Furthermore, the production method may include, as necessary, a secondary firing step of heat-treating the obtained ion-conductive solid containing an oxide at a temperature below the melting point of the oxide to produce a sintered body of the ion-conductive solid containing the oxide. Hereinafter, the method for producing an ion-conductive solid according to the present disclosure, which includes the above-mentioned primary firing step and secondary firing step, will be described in detail, but the present disclosure is not limited to the following production method.
[0030] Primary firing process In the first firing process, the general formula Li 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 dB3O9 (wherein M1 is one or more metal elements selected from Mg, Mn, Zn, Ni, Ca, Sr, or Ba, M2 is one or more metal elements selected from La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, In, or Fe, M3 is one or more metal elements selected from Zr, Ce, Hf, Sn, or Ti, and M4 is one or more metal elements selected from Nb or Ta). Raw materials such as chemical reagent grade Li3BO3, H3BO3, Yb2O3, ZrO2, CeO2, and HfO2 are weighed out in stoichiometric amounts and mixed so that the composition satisfies the following criteria: a is 0.000≦a≦0.800, b is 0.000≦b≦0.900, c is 0.000≦c≦0.800, d is 0.000≦d≦0.800, and a, b, c, and d are real numbers that satisfy 0.000≦a+b+c+d<1.000).
[0031] The device used for mixing is not particularly limited, but for example, a grinding type mixer such as a planetary ball mill can be used. The material and capacity of the container used during mixing, and the material and diameter of the ball are not particularly limited, and can be appropriately selected according to the type and amount of raw material used. As an example, a 45 mL container made of zirconia and a 5 mm diameter ball made of zirconia can be used. In addition, the conditions of the mixing process are not particularly limited, but for example, the rotation speed can be 50 rpm to 2000 rpm, and the time can be 10 minutes to 60 minutes. After obtaining a mixed powder of the above-mentioned raw materials by the mixing process, the obtained mixed powder is pressed and molded. The mixture is pelletized. As the pressure molding method, known pressure molding methods such as cold uniaxial molding and cold isostatic pressing can be used. The conditions for pressure molding in the primary firing step are not particularly limited, but can be, for example, a pressure of 100 MPa to 200 MPa. The pellets obtained are sintered using a sintering device such as an air sintering device. The temperature at which the primary sintering is performed to synthesize the solid phase is set at 100°C, which is the temperature at which the solid phase synthesis is performed. 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 dThere is no particular limitation as long as it is below the melting point of the ion-conductive solid represented by B3O9. The temperature during primary firing can be, for example, less than 700°C, 680°C or less, 670°C or less, 660°C or less, or 650°C or less, and can be, for example, 500°C or more. The numerical ranges can be combined arbitrarily. If the temperature is within the above range, solid-phase synthesis can be performed sufficiently. The time of the primary firing step is not particularly limited, but can be, for example, about 700 to 750 minutes. By the above primary firing step, the above general formula Li 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 d It is possible to prepare an ionically conductive solid containing an oxide represented by B3O9. It is also possible to obtain a powder of the ionically conductive solid containing the oxide by grinding the ionically conductive solid containing the oxide using a mortar and pestle or a planetary mill.
[0032] Secondary firing process In the secondary firing step, at least one selected from the group consisting of the ion-conductive solid containing an oxide obtained in the primary firing step and a powder of the ion-conductive solid containing an oxide is pressure-molded as necessary and fired to obtain a sintered body of the ion-conductive solid containing an oxide. The pressure molding and secondary firing may be performed simultaneously using spark plasma sintering (hereinafter also simply referred to as "SPS") or hot pressing, or pellets may be produced by cold uniaxial molding and then secondary firing may be performed in air, an oxidizing atmosphere, or a reducing atmosphere. Under the above conditions, an ion-conductive solid with high ion conductivity can be obtained without melting due to heat treatment. The conditions for pressure molding in the secondary firing step are not particularly limited, but may be, for example, a pressure of 10 MPa to 100 MPa. The secondary firing temperature is the general formula Li 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 dThe temperature is lower than the melting point of the ion-conductive solid represented by B3O9. The temperature during the secondary firing is preferably lower than 700°C, more preferably 680°C or less, even more preferably 670°C or less, and particularly preferably 660°C or less. The lower limit of the temperature is not particularly limited, and the lower the better, but it is, for example, 500°C or more. The numerical ranges can be arbitrarily combined, and can be, for example, a range of 500°C or more and less than 700°C. Within the above range, the ion-conductive solid containing the oxide of the present disclosure can be prevented from melting or decomposing in the secondary firing step, and a sintered body of the ion-conductive solid containing the oxide of the present disclosure that is sufficiently sintered can be obtained. The time for the secondary firing step can be appropriately changed depending on the temperature, pressure, etc. of the secondary firing step, but is preferably 24 hours or less, and may be 14 hours or less. The time for the secondary firing step may be, for example, 5 minutes or more, 1 hour or more, or 6 hours or more.
[0033] The method for cooling the sintered body of the ion-conductive solid containing the oxide of the present disclosure obtained by the secondary firing step is not particularly limited, and the body may be allowed to cool naturally (cool in a furnace), may be cooled rapidly, may be cooled more gradually than by natural cooling, or may be maintained at a certain temperature during cooling.
[0034] Next, the all-solid-state battery of the present disclosure will be described. An all-solid-state battery generally includes a positive electrode, a negative electrode, an electrolyte including an ion-conducting solid disposed between the positive electrode and the negative electrode, and optionally a current collector.
[0035] The all-solid-state battery of the present disclosure is A positive electrode and A negative electrode; An electrolyte; An all-solid-state battery having at least At least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte comprises an ionically conductive solid of the present disclosure.
[0036] The all-solid-state battery of the present disclosure may be a bulk type battery or a thin-film battery. The specific shape of the all-solid-state battery of the present disclosure is not particularly limited, and examples thereof include a coin type, a button type, a sheet type, and a laminate type.
[0037] The all-solid-state battery of the present disclosure has an electrolyte. In the all-solid-state battery of the present disclosure, it is preferable that at least the electrolyte contains the ion-conducting solid of the present disclosure. The solid electrolyte in the all-solid-state battery of the present disclosure may be made of the ion-conductive solid of the present disclosure, or may contain other ion-conductive solids, or may contain ionic liquids or gel polymers. The other ion-conductive solids are not particularly limited, and may be ion-conductive solids that are commonly used in all-solid-state batteries, such as LiI, Li3PO4, Li7La3Zr2O 12 The content of the ion-conductive solid of the present disclosure in the electrolyte of the all-solid-state battery of the present disclosure is not particularly limited, and is preferably 25 mass % or more, more preferably 50 mass % or more, even more preferably 75 mass % or more, and particularly preferably 100 mass %.
[0038] The all-solid-state battery of the present disclosure has a positive electrode. The positive electrode may contain a positive electrode active material, or may contain the positive electrode active material and the ion-conductive solid of the present disclosure. As the positive electrode active material, any known positive electrode active material such as a sulfide containing a transition metal element or an oxide containing lithium and a transition metal element can be used without any particular limitation. For example, LiNiVO4, LiCoPO4, LiCoVO4, LiMn 1.6 Ni 0.4 O4, LiMn2O4, LiCoO2, Fe2(SO4)3, LiFePO4, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2, LiNi 1 / 2 Mn 1 / 2 O2, LiNiO2, Li 1+x (Fe, Mn, Co) 1-x O2, LiNi 0.8 Co 0.15 Al 0.05 Examples include O2. Furthermore, the positive electrode may contain a binder, a conductive agent, etc. Examples of the binder include polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, etc. Examples of the conductive agent include natural graphite, artificial graphite, acetylene black, ethylene black, etc.
[0039] The all-solid-state battery of the present disclosure has a negative electrode. The negative electrode may contain a negative electrode active material, or may contain the negative electrode active material and the ion-conductive solid of the present disclosure. As the negative electrode active material, known negative electrode active materials such as inorganic compounds such as lithium, lithium alloys, and tin compounds, carbonaceous materials capable of absorbing and releasing lithium ions, and conductive polymers can be used without any particular restrictions. For example, Li4Ti5O 12 etc. Furthermore, the negative electrode may contain a binder, a conductive agent, etc. As the binder and the conductive agent, the same materials as those exemplified for the positive electrode can be used.
[0040] Here, the term "including" an electrode active material means that the electrode has the electrode active material as a component, element, or property. For example, both cases where the electrode contains an electrode active material within the electrode and where the electrode active material is applied to the surface of the electrode are considered to be "including" above.
[0041] The positive electrode and the negative electrode can be obtained by a known method such as mixing, molding, and heat treatment of raw materials. It is considered that the ion conductive solid enters the gaps between the electrode active materials, and it is easy to secure the conduction path of lithium ions. Since the ion conductive solid of the present disclosure can be produced by a heat treatment at a lower temperature than the conventional technology, it is considered that the formation of a high resistance phase caused by the reaction between the ion conductive solid and the electrode active material can be suppressed.
[0042] The positive electrode and the negative electrode may have a current collector. As the current collector, known current collectors such as aluminum, titanium, stainless steel, nickel, iron, baked carbon, conductive polymer, conductive glass, etc. can be used. In addition, for the purpose of improving adhesion, conductivity, oxidation resistance, etc., aluminum, copper, etc., the surface of which is treated with carbon, nickel, titanium, silver, etc. can be used as the current collector.
[0043] The all-solid-state battery of the present disclosure can be obtained by a known method, for example, by stacking a positive electrode, a solid electrolyte, and a negative electrode, molding, heat treatment, etc. The ion-conductive solid of the present disclosure can be produced by a heat treatment at a lower temperature than in the conventional technology, and therefore it is considered that the formation of a high-resistance phase caused by the reaction between the ion-conductive solid and the electrode active material can be suppressed, and it is considered that an all-solid-state battery with excellent output characteristics can be obtained.
[0044] Next, the composition and the method for measuring each physical property according to the present disclosure will be described. -Methods for identifying and analyzing contained metals The composition of the ion-conductive solid is analyzed by wavelength-dispersive X-ray fluorescence analysis (hereinafter, also referred to as XRF) using a sample solidified by pressure molding. However, if analysis is difficult due to particle size effects, etc., it is advisable to vitrify the ion-conductive solid by the glass bead method and then perform composition analysis by XRF. In addition, if the yttrium peak and the contained metal peak overlap in XRF, it is advisable to perform composition analysis by inductively coupled plasma atomic emission spectrometry (ICP-AES). For XRF, the analytical equipment used is the ZSX Primus II manufactured by Rigaku Corporation. The analytical conditions are as follows: Rh is used for the anode of the X-ray tube, vacuum atmosphere, analysis diameter is 10 mm, analysis range is 17 deg to 81 deg, step is 0.01 deg, and scan speed is 5 sec / step. In addition, a proportional counter is used to measure light elements, and a scintillation counter is used to measure heavy elements. The elements are identified based on the peak positions of the spectrum obtained by XRF, and the molar concentration ratios are calculated from the counting rate (unit: cps), which is the number of X-ray photons per unit time, to obtain a, b, c, and d. EXAMPLES
[0045] Hereinafter, specific examples of the preparation and evaluation of the ion-conductive solid of the present disclosure will be described as examples, but the present disclosure is not limited to the following examples.
[0046] [Example 1] · Primary firing process Li3BO3 (Toshima Manufacturing, purity 99.9% by mass), H3BO3 (Kanto Chemical, purity 99.5%), Yb2O3 (Shin-Etsu Chemical, purity 99.9% by mass), and Nb2O5 (Mitsui Mining & Smelting, purity 99.9%) were used as raw materials, and each raw material was weighed out in stoichiometric amounts so that d was the value listed in Table 1, and mixed for 30 minutes at a disk rotation speed of 300 rpm in a Fritsch planetary mill P-7. A zirconia φ5 mm ball and a 45 mL container were used for the planetary mill. After mixing, the mixed powder was cold uniaxially molded at 147 MPa using a 100 kN electric press P3052-10 manufactured by NPA Systems, and sintered in air at a heating temperature of 650°C and a holding time of 720 minutes. The obtained ionically conductive solid containing an oxide was ground in a planetary mill P-7 manufactured by Fritsch at a disk rotation speed of 230 rpm for 180 minutes to prepare a powder of an ionically conductive solid containing an oxide. Secondary firing process The powder of the ion-conductive solid containing the oxide obtained above was molded and secondarily sintered to obtain Example 1. A sintered body of an ion-conductive solid containing the oxide was produced. The powder was cold uniaxially molded at 147 MPa using a 100 kN electric press P3052-10 manufactured by NPA Systems. The secondary sintering was carried out in an air atmosphere at a heating temperature of 650°C and a holding time of 720 minutes.
[0047] [Example 2] A sintered body of an ion-conductive solid containing the oxide of Example 2 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), and CeO2 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9%) were used as raw materials, and each raw material was weighed out in stoichiometric amounts so that c was the value shown in Table 1.
[0048] [Example 3] A sintered body of an ion-conductive solid containing the oxide of Example 3 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), ZrO2 (manufactured by Nippon Denko, purity 99.9%), CeO2 (manufactured by Shin-Etsu Chemical, purity 99.9%) and Nb2O5 (manufactured by Mitsui Mining and Smelting, purity 99.9%) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that c and d were the values shown in Table 1.
[0049] [Example 4] A sintered body of an ion-conductive solid containing the oxide of Example 4 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so as to obtain the values shown in Table 1.
[0050] [Example 5] A sintered body of an ion-conductive solid containing the oxide of Example 5 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), and HfO2 (manufactured by New Metals, purity 99.9%) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that c was the value shown in Table 1.
[0051] [Example 6] A sintered body of an ion-conductive solid containing the oxide of Example 6 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that c was the value shown in Table 1.
[0052] [Example 7] A sintered body of an ion-conductive solid containing the oxide of Example 7 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that c and d were the values shown in Table 1.
[0053] [Example 8] A sintered body of an ion-conductive solid containing the oxide of Example 8 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical Co., Ltd., purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), In2O3 (manufactured by Shinko Chemical Co., Ltd., purity 99% by mass), SnO2 (manufactured by Mitsuwa Chemical Co., Ltd., purity 99.9%) and CeO2 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9%) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that b and c were the values shown in Table 1.
[0054] [Example 9] A sintered body of an ion-conductive solid containing the oxide of Example 9 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and c were the values shown in Table 1.
[0055] [Example 10] A sintered body of an ion-conductive solid containing the oxide of Example 10 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), Fe2O3 (manufactured by Wako Pure Chemical Industries, Ltd., purity 95.0% by mass) and TiO2 (manufactured by Toho Titanium, purity 99%) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that b and c were the values shown in Table 1.
[0056] [Example 11] A sintered body of an ion-conductive solid containing the oxide of Example 11 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and c were the values shown in Table 1.
[0057] [Example 12] A sintered body of an ion-conductive solid containing the oxide of Example 12 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), and Lu2O3 (manufactured by Kojundo Chemical Laboratory, purity 99.9% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that b was the value shown in Table 1.
[0058] [Example 13] A sintered body of an ion-conductive solid containing the oxide of Example 13 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), MgO (manufactured by Ube Material Industries, Ltd., purity 99.0% by mass) and CeO2 (manufactured by Shin-Etsu Chemical, purity 99.9%) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and c were the values shown in Table 1.
[0059] [Example 14] A sintered body of an ion-conductive solid containing the oxide of Example 14 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that a and b were the values shown in Table 1.
[0060] [Example 15] A sintered body of an ion-conductive solid containing the oxide of Example 15 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), La2O3 (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.9% by mass), MgO (manufactured by Ube Material Industries, Ltd., purity 99.0% by mass) and CaO (manufactured by Kanto Chemical, purity 97.0% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 1.
[0061] [Example 16] The raw materials were Li3BO3 (Toshima Manufacturing, purity 99.9% by mass), H3BO3 (Kanto Chemical, purity 99.5%), Yb2O3 (Shin-Etsu Chemical, purity 99.9% by mass), La2O3 (Wako Pure Chemical Industries, purity 99.9% by mass), and MnO (Kanto Chemical, purity 80.0% by mass). A sintered body of an ion-conductive solid containing the oxide of Example 16 was produced in the same manner as in Example 1, except that the raw materials were weighed out in stoichiometric amounts so that a and b were the values shown in Table 1.
[0062] [Example 17] A sintered body of an ion-conductive solid containing the oxide of Example 17 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), Tb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass) and MnO (manufactured by Kanto Chemical, purity 80.0% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 1.
[0063] [Example 18] A sintered body of an ion-conductive solid containing the oxide of Example 18 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), Tm2O3 (manufactured by High Purity Chemical Laboratory, purity 99.9% by mass) and CaO (manufactured by Kanto Chemical, purity 97.0% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 1.
[0064] [Example 19] A sintered body of an ion-conductive solid containing the oxide of Example 19 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that c and d were the values shown in Table 1.
[0065] [Example 20] A sintered body of an ion-conductive solid containing the oxide of Example 20 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), In2O3 (manufactured by Shinko Chemical, purity 99% by mass), Nb2O5 (manufactured by Mitsui Mining and Smelting, purity 99.9%) and Ta2O5 (manufactured by Kanto Chemical, purity 99% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that b and d were the values shown in Table 1.
[0066] [Example 21] A sintered body of an ion-conductive solid containing the oxide of Example 21 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), and Pr2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass) were used as raw materials, and each raw material was weighed out in stoichiometric amounts so that b was the value shown in Table 1.
[0067] [Example 22] A sintered body of an ion-conductive solid containing the oxide of Example 22 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and d were the values shown in Table 1.
[0068] [Example 23] Li3BO3 (Toshima Manufacturing, purity 99.9% by mass), H3BO3 (Kanto Chemical, purity 99.5%), Yb2O3 (Shin-Etsu Chemical, purity 99.9% by mass), Sm2O3 (Wako Pure Chemical Industries, purity 99.9% by mass), HfO2 (New Metals, purity 99.9%) and Ta2O5 (Kanto Chemical, purity 99% by mass) were used as raw materials. A sintered body of an ion-conductive solid containing an oxide of Example 23 was produced in the same manner as in Example 1, except that each raw material was weighed out in stoichiometric amounts so as to obtain the values shown.
[0069] [Example 24] Li3BO3 (Toshima Manufacturing, purity 99.9% by mass), H3BO3 (Kanto Chemical, purity 99.5%), Yb2O3 (Shin-Etsu Chemical, purity 99.9% by mass), Nd2O3 (Shin-Etsu Chemical, purity 99.9% by mass), Sm2O3 (Wako Pure Chemical Industries, Ltd., purity 99.9% by mass), HfO2 (New Metals, purity 99.9%) and ZnO (Wako Pure Chemical Industries, Ltd., purity 99% by mass) were used as raw materials, and a sintered body containing the oxide of Example 24 was produced in the same process as Example 1, except that each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2.
[0070] [Example 25] A sintered body of an ion-conductive solid containing the oxide of Example 25 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and c were the values shown in Table 2.
[0071] [Example 26] A sintered body of an ion-conductive solid containing the oxide of Example 26 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), and Eu2O3 (manufactured by Shin-Etsu Chemical, purity 95% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that b was the value shown in Table 2.
[0072] [Example 27] A sintered body of an ion-conductive solid containing the oxide of Example 27 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), Eu2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 95% by mass) and NiO (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.0% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2.
[0073] [Example 28] A sintered body of an ion-conductive solid containing the oxide of Example 28 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and c were the values shown in Table 2.
[0074] [Example 29] A sintered body of an ion-conductive solid containing the oxide of Example 29 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), Gd2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), Dy2O3 (manufactured by Shin-Etsu Chemical, purity 95% by mass) and CaO (manufactured by Kanto Chemical, purity 99.0% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2.
[0075] [Example 30] A sintered body of an ion-conductive solid containing the oxide of Example 30 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and c were the values shown in Table 2.
[0076] [Example 31] A sintered body of an ion-conductive solid containing the oxide of Example 31 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and c were the values shown in Table 2.
[0077] [Example 32] A sintered body of an ion-conductive solid containing the oxide of Example 32 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b was the value shown in Table 2.
[0078] [Example 33] A sintered body of an ion-conductive solid containing the oxide of Example 33 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), Tb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), NiO (manufactured by Wako Pure Chemical Industries, Ltd., purity 99.0% by mass), and BaO (manufactured by Wako Pure Chemical Industries, Ltd., purity 90.0% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2.
[0079] [Example 34] A sintered body of an ion-conductive solid containing the oxide of Example 34 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing Co., Ltd., purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), Tb2O3 (manufactured by Shin-Etsu Chemical Co., Ltd., purity 99.9% by mass), Ho2O3 (manufactured by High Purity Chemical Laboratory, purity 99.9% by mass) and BaO (manufactured by Wako Pure Chemical Industries, Ltd., purity 90.0% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2.
[0080] [Example 35] A sintered body of an ion-conductive solid containing the oxide of Example 35 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b, c, and d were the values shown in Table 2.
[0081] [Example 36] A sintered body of an ion-conductive solid containing the oxide of Example 36 was produced in the same manner as in Example 1, except that Li3BO3 (manufactured by Toshima Manufacturing, purity 99.9% by mass), H3BO3 (manufactured by Kanto Chemical, purity 99.5%), Yb2O3 (manufactured by Shin-Etsu Chemical, purity 99.9% by mass), Er2O3 (manufactured by Shin-Etsu Chemical, purity 95% by mass), Tm2O3 (manufactured by High Purity Chemical Laboratory, purity 99.9% by mass) and SrO (manufactured by High Purity Chemical Laboratory, purity 98% by mass) were used as raw materials and each raw material was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2.
[0082] [Example 37] A sintered body of an ion-conductive solid containing the oxide of Example 37 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and c were the values shown in Table 2.
[0083] [Example 38] A sintered body of an ion-conductive solid containing the oxide of Example 38 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that a, b, and c were the values shown in Table 2.
[0084] [Example 39] A sintered body of an ion-conductive solid containing the oxide of Example 39 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and d were the values shown in Table 2.
[0085] [Example 40] A sintered body of an ion-conductive solid containing the oxide of Example 40 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b, c, and d were the values shown in Table 2.
[0086] [Example 41] A sintered body of an ion-conductive solid containing the oxide of Example 41 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that a, b, and c were the values shown in Table 2.
[0087] [Example 42] A sintered body of an ion-conductive solid containing the oxide of Example 42 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and d were the values shown in Table 2.
[0088] [Example 43] A sintered body of an ion-conductive solid containing the oxide of Example 43 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that b and d were the values shown in Table 2.
[0089] [Example 44] A sintered body of an ion-conductive solid containing the oxide of Example 44 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2, and the disk rotation speed during grinding was set to 300 rpm.
[0090] [Example 45] A sintered body of an ion-conductive solid containing the oxide of Example 45 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2, and the disk rotation speed during grinding was set to 300 rpm.
[0091] [Example 46] A sintered body of an ion-conductive solid containing the oxide of Example 46 was produced in the same manner as in Example 1, except that each of the raw materials used in the above examples was weighed out in stoichiometric amounts so that a and b were the values shown in Table 2, and the disk rotation speed during grinding was set to 300 rpm.
[0092] [Comparative Example 1] A sintered body of an ion-conductive solid containing the oxide of Comparative Example 1 was produced in the same manner as in Example 1, except that the raw material Yb2O3 in Example 1 was changed to Y2O3 and each raw material was weighed out in a stoichiometric amount so that d was the value shown in Table 1.
[0093] [Comparative Example 2] A sintered body of an ion-conductive solid containing the oxide of Comparative Example 2 was produced in the same manner as in Example 2, except that the raw material Yb2O3 in Example 2 was changed to Y2O3 and each raw material was weighed out in a stoichiometric amount so that c was the value shown in Table 1.
[0094] [Comparative Example 3] A sintered body of an ion-conductive solid containing the oxide of Comparative Example 3 was produced in the same manner as in Example 3, except that the raw material Yb2O3 in Example 3 was changed to Y2O3 and each raw material was weighed out in stoichiometric amounts so that c and d were the values shown in Table 1.
[0095] The composition analysis was carried out by the above-mentioned method for the sintered bodies of the ion-conductive solids containing oxides in Examples 1 to 46. In addition, the volume average particle size of the powders of the ion-conductive solids obtained in Examples 1 to 46 and Comparative Examples 1 to 3 and the ionic conductivity of the sintered bodies of the ion-conductive solids were measured by the following method. The methods for measuring the ionic conductivity and the volume average particle size are described below. The evaluation results are shown in Tables 1 and 2.
[0096] -Ionic conductivity measurement In the sintered body of the ion-conductive solid containing oxide in the shape of a plate obtained by the secondary firing, two faces that face each other in parallel and have a large area were polished with sandpaper. The dimensions of the sintered body of the ion-conductive solid containing oxide in the shape of a plate can be, for example, 0.9 cm x 0.9 cm x 0.05 cm, but are not limited thereto. The polishing was first performed with #500 for 15 to 30 minutes, then with #1000 for 10 to 20 minutes, and finally with #2000 for 5 to 10 minutes, and the polishing was completed if there were no noticeable unevenness or scratches on the polished surface when visually inspected. After polishing, a gold film was formed on the polished surface of the sintered body of ion-conductive solid containing oxide using a Sanyu Electronics SC-701MkII ADVANCE sputtering device. The film formation conditions were Ar process gas, vacuum level of 2 Pa to 5 Pa, and film formation time of 5 minutes for the measurement sample. After film formation, the AC impedance of the measurement sample was measured. An impedance / gain phase analyzer SI1260 and a dielectric interface system 1296 (both manufactured by Solartron) were used for the impedance measurement, and the measurement conditions were a temperature of 27° C., an amplitude of 20 mV, and a frequency of 0.1 Hz to 1 MHz. The resistance of the sintered body of ion-conductive solid containing oxide was calculated using the Nyquist plot obtained by impedance measurement and Scribner's AC analysis software ZVIEW. An equivalent circuit equivalent to the measurement sample was set in ZVIEW, and the resistance of the sintered body of ion-conductive solid containing oxide was calculated by fitting and analyzing the equivalent circuit and Nyquist plot. The ionic conductivity was calculated from the following formula using the calculated resistance, the thickness of the sintered body of ion-conductive solid containing oxide, and the electrode area. Ionic conductivity (S / cm) = thickness of sintered body of ion-conducting solid containing oxide (cm) / (resistance of sintered body of ion-conducting solid containing oxide (Ω) × electrode area (cm 2 ))
[0097] The ionic conductivity (S / cm) of the sintered body of the ion-conductive solid is preferably, for example, 8.00×10 -9 More preferably, it is 1.00×10 -8 More preferably, it is 1.00×10 -7 More preferably, it is 1.00×10 or more. -6 More preferably, it is 1.00×10 -5 The higher the conductivity, the more preferable it is. There is no particular upper limit to the conductivity. For example, the conductivity is 1.00×10 -2 Below, 1.00 x 10 -3 Below, 1.00 x 10 -4 The following is the result.
[0098] -Evaluation of volume average particle size The ion-conductive solid powder containing oxide obtained by ball milling (Fritsch Planetary Mill P-7) after the primary firing was subjected to particle size distribution measurement using a Horiba Laser Diffraction / Scattering Particle Size Distribution Analyzer LA-960V2. The refractive index was set to 1.8, and ethanol was used as the measurement solvent. The concentration of the sample was adjusted so that the transmittance was 90-70%. The volume average particle size was calculated from the obtained frequency distribution.
[0099] ·result Table 1 shows the sintered bodies of ion-conductive solids containing each oxide in Examples 1 to 46 and Comparative Examples 1 to 3. The stoichiometric amount of raw material (general formula Li 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 d The values of a, b, c and d in B3O9, the volume average particle size and the ionic conductivity are summarized. As a result of the above composition analysis, it was confirmed that all of the sintered bodies of ion-conductive solids containing oxides in Examples 1 to 46 and Comparative Examples 1 to 3 had compositions in accordance with the stoichiometric amounts of the raw materials listed in Table 1. Furthermore, the sintered bodies of ion-conductive solids containing oxides in Examples 1 to 46 were ion-conductive solids that exhibited high ion conductivity even when fired at a temperature of less than 700°C.
[0100] [Table 1]
[0101] [Table 2]
[0102] In Tables 1 and 2, the ionic conductivity of the ion-conductive solids produced in Examples 1 to 3 is improved compared to Comparative Examples 1 to 3, and it is shown that higher ionic conductivity can be obtained by substituting Yb for Y. It can be seen that higher ionic conductivity can be obtained by substituting Yb, which has a smaller ionic radius, for Y in the compositions disclosed in the prior art.
[0103] In Tables 1 and 2, the ion conductivity of the ion-conductive solids produced in Examples 44 to 46 was improved compared to Examples 17, 27, and 33. Since the compositions and substitution elements differ from those disclosed in the prior art, the density after firing is affected by differences in melting points, etc., which may result in a difference in the appropriate range of particle size.
Claims
1. General formula Li 6+a-c-2d Yb 1-a-b-c-d M1 a M2 b M3 c M4 d B 3 O 9 An ion-conductive solid electrolyte comprising an oxide represented by the formula: The volume average particle size of the oxide is 0.1 μm or more and 10 μm or less. (In the formula, M1 is at least one metal element selected from the group consisting of Mg, Mn, Zn, Ni, Ca, Sr, and Ba, M2 is at least one metal element selected from the group consisting of La, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Lu, In and Fe; M3 is at least one metal element selected from the group consisting of Zr, Hf, Sn, and Ti; M4 is at least one metal element selected from the group consisting of Nb and Ta; a is a real number that satisfies 0.000≦a≦0.800, b is 0.000≦b≦0.900, c is 0.000≦c≦0.800, d is 0.000≦d≦0.800, and a, b, c, and d are real numbers that satisfy 0.000≦a+b+c+d<0.900.)
2. 2. The ion-conducting solid electrolyte according to claim 1, wherein 1-ab-cd satisfies 0.300≦1-ab-cd.
3. 2. The ion-conducting solid electrolyte according to claim 1, wherein 1-ab-cd satisfies 0.500≦1-ab-cd.
4. 2. The ion-conducting solid electrolyte according to claim 1, wherein a satisfies 0.000≦a≦0.
400.
5. 2. The ion-conducting solid electrolyte according to claim 1, wherein b satisfies 0.000≦b≦0.
500.
6. 2. The ion-conducting solid electrolyte according to claim 1, wherein c satisfies 0.000≦c≦0.
400.
7. 2. The ion-conducting solid electrolyte according to claim 1, wherein d satisfies the condition 0.000≦d≦0.
400.
8. A positive electrode and A negative electrode; An electrolyte; An all-solid-state battery having at least At least one selected from the group consisting of the positive electrode, the negative electrode, and the electrolyte comprises the ion-conducting solid electrolyte according to any one of claims 1 to 7.
9. 9. The all-solid-state battery according to claim 8, wherein at least the electrolyte comprises the ion-conducting solid electrolyte.
Citation Information
Patent Citations
Ion-conducting solid and all-solid-state batteries
JP6948676B2