Coated paper

The coated paper with a balanced PHBH and inorganic pigment ratio and optional second coating layer addresses adhesion and heat-sealing issues, ensuring strong adhesion and resistance, suitable for diverse applications.

JP2024133593APending Publication Date: 2024-10-02NIPPON PAPER IND CO LTD
3 Cites 0 Cited by

Patent Information

Application Number
JP2024107857
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-06
Filing Date
2024-07-04
Publication Date
2024-10-02

Smart Images

  • Figure 2024133593000001
    Figure 2024133593000001
  • Figure 2024133593000002
    Figure 2024133593000002
  • Figure 2024133593000003
    Figure 2024133593000003
Patent Text Reader

Abstract

To provide coated paper with excellent heat sealability.SOLUTION: Coated paper comprises a coating layer containing PHBH (poly(3-hydroxybutyrate-co-3-hydroxyhexanoate)), inorganic pigments and an adhesive on at least one surface of a paper substrate, and it comprises a second coating layer containing PHBH on the coating layer. The solid content weight ratio between PHBH and inorganic pigment (PHBH:inorganic pigment) of the coating layer is 90:10 to 0.01:99.99, and the ratio of the adhesive to the total solid content is 0.1 to 40 wt.%, and the inorganic pigment has a volume 50% average particle diameter (D50) of 0.1 μm or more (excluding the aforementioned inorganic pigments that are coloring pigments).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coated paper coated with a coating liquid containing PHBH. [Background technology]

[0002] In recent years, efforts have begun to prevent environmental destruction caused by plastic waste, and there is a demand to replace disposable plastic products with materials that have a smaller impact on the environment. Alternative materials to plastic include biodegradable plastics, wood, paper, etc. Aliphatic polyesters such as polylactic acid and polycaprolactone are known as biodegradable plastics. However, aliphatic polyesters have the problem that they take a long time to biodegrade at low temperatures and decompose slowly in natural environments such as the ocean.

[0003] Poly(3-hydroxybutyrate) resins are thermoplastics produced by microorganisms that are highly degradable under both aerobic and anaerobic conditions, and have the remarkable ability to be decomposed by microorganisms in a short period of time even in water, such as the ocean. Patent Document 1 describes that a biodegradable polyester aqueous dispersion containing poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter, also referred to as PHBH), which is a copolymer of 3-hydroxybutyrate and 3-hydroxyhexanoate, has excellent film-forming properties and gives a resin coating film that is flexible, has good stretchability, and is strong against bending when applied to paints, adhesives, fiber processing, sheet / film processing, paper processing, etc. Patent Documents 2 and 3 describe that when PHBH is applied to the surface of a paper substrate, the fixation of PHBH to the surface of the paper substrate is improved by adding an adhesive to the coating liquid. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2004 / 041936 [Patent Document 2] Patent Publication No. 2021-195716 [Patent Document 3] Patent Publication No. 2021-195717 Summary of the Invention [Problem to be solved by the invention]

[0005] The inventors were developing coated paper with reference to these conventional techniques, and found that when producing coated paper with a coating solution containing PHBH and an adhesive, the adhesion of the coating layer to the paper substrate surface deteriorates if the drying conditions are weak. For example, if the drying temperature of the dryer fluctuates and becomes low, the adhesion of the coating layer decreases, resulting in defective products with peeling of the coating layer. For this reason, there was a demand for a technology that improves the adhesion of the coating layer even when the drying conditions are weak. It is also known that when the content of the adhesive in the coating solution is high, the adhesion of the coating layer to the surface of the paper substrate is improved, but the heat sealability is deteriorated due to the influence of the adhesive content (see the examples in Patent Documents 2 and 3). This is thought to be because the adhesive in the coating layer (PVA or starch) does not have thermal fusion properties and therefore inhibits heat sealing. However, there has been a demand for technology that can achieve good heat sealability even in such cases. The present invention has been developed against this background, and its first object is to provide a coated paper having a coating layer that has excellent adhesion to a paper substrate even when the drying conditions are weak. A second object of the present invention is to provide a coated paper that has good heat sealability even when the coating layer contains an adhesive. [Means for solving the problem]

[0006] The means for solving the problems of the present invention are as follows. 1. A paper substrate having a coating layer containing PHBH (poly(3-hydroxybutyrate-co-3-hydroxyhexanoate)), an inorganic pigment, and an adhesive on at least one surface thereof; 2. A coated paper, wherein the coating layer has a solids weight ratio of PHBH to inorganic pigment (PHBH:inorganic pigment) of 90:10 to 0.01:99.99. 2. The coated paper according to 1, wherein the inorganic pigment has a 50% volume average particle size (D50) of 6.0 μm or less. 3. The coated paper according to 1 or 2, wherein the solids weight ratio of PHBH to inorganic pigment in the coating layer is 70:30 to 20:80. 4. The coated paper according to 1, further comprising a second coating layer on the first coating layer, the second coating layer comprising PHBH. 5. The coated paper according to 4, wherein the inorganic pigment has a 50% volume average particle size (D50) of 8.0 μm or less. 6. The coated paper according to 4. or 5., wherein the solids weight ratio of PHBH to inorganic pigment in the coating layer is 90:10 to 5:95. 7. The coated paper according to any one of 4. to 6., wherein the weight average molecular weight of PHBH in the second coating layer is greater than the weight average molecular weight of PHBH in the first coating layer. 8. The coated paper according to any one of 4. to 7., characterized in that the heat seal strength is 5.0 N / 15 mm or more. 9. The coated paper according to any one of 4. to 8., characterized in that the average kit number according to JAPAN TAPPI Paper Pulp Test Method No. 41:2000 is 4 or more. Effect of the Invention

[0007] The coated paper of the present invention has excellent adhesion of the coating layer, and the coating layer is less likely to peel off. The coated paper of the present invention having a second coating layer has excellent heat seal strength and can be suitably used as a heat seal paper. Furthermore, when the coating layer contains an inorganic pigment having a volume 50% average particle size (D50) of 8.0 μm or less, it has excellent oil resistance and water resistance and can be suitably used as an oil-resistant heat seal paper, a water-resistant heat seal paper, or a water-resistant and oil-resistant heat seal paper. The coated paper of the present invention has a high ratio of biodegradable materials to the entire coated paper, and therefore, even if it is leaked into the environment, it will decompose quickly. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The coated paper of the present invention has a coating layer containing PHBH (poly(3-hydroxybutyrate-co-3-hydroxyhexanoate)), an inorganic pigment, and an adhesive on at least one surface of a paper substrate, In this coating layer, the solids weight ratio of PHBH to inorganic pigment (PHBH:inorganic pigment) is 90:10 to 0.01:99.99. In this specification, the expression "A to B" (A and B are numerical values ​​or ratios) means a numerical range including A and B.

[0009] (Paper base material) The paper base material is a sheet (hereinafter also referred to as "base paper") mainly made of pulp, and is obtained by papermaking a paper stock that further contains fillers, various auxiliaries, and the like. Examples of pulp include chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), unbleached softwood pulp (NUKP), sulfite pulp, and other such pulps, mechanical pulps such as stone-ground pulp and thermomechanical pulp, deinked pulp, wood fibers such as waste paper pulp, and non-wood fibers obtained from kenaf, bamboo, hemp, and the like, and one or more of these can be used in appropriate combination. Among these, preferred pulps are those which are less likely to be contaminated by foreign matter in the paper base material, and those which are made from waste paper. It is preferable to use chemical pulp of wood fiber or mechanical pulp of wood fiber, and more preferable to use chemical pulp of wood fiber, because it is less likely to discolor over time when recycled as a raw material, has a high whiteness so that the surface texture during printing is good, and has high utility value especially when used as a packaging material. Specifically, the blending amount of chemical pulp of wood fiber such as LBKP or NBKP to the total pulp is preferably 80% by weight or more, more preferably 90% by weight or more, even more preferably 95% by weight or more, and most preferably 100% by weight.

[0010] Examples of fillers that can be used include inorganic fillers such as talc, kaolin, calcined kaolin, clay, heavy calcium carbonate, light calcium carbonate, white carbon, zeolite, magnesium carbonate, barium carbonate, titanium dioxide, zinc oxide, silicon oxide, amorphous silica, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, zinc hydroxide, barium sulfate, and calcium sulfate, and organic fillers such as urea-formalin resin, polystyrene resin, phenolic resin, and hollow microparticles. Note that fillers are not essential materials and may not be used.

[0011] Examples of various auxiliary agents include sizing agents such as rosin, alkyl ketene dimer (AKD), alkenyl succinic anhydride (ASA), polyacrylamide polymers, polyvinyl alcohol polymers, cationic starch, various modified starches, urea-formaldehyde resin, melamine-formaldehyde resin, and other dry strength agents, wet strength agents, retention agents, drainage improvers, coagulants, aluminum sulfate, bulking agents, dyes, fluorescent brighteners, pH adjusters, defoamers, UV inhibitors, anti-fading agents, pitch control agents, slime control agents, and the like, and can be selected and used as appropriate as needed.

[0012] The surface of the paper substrate may be treated with various chemicals. Examples of chemicals include oxidized starch, hydroxyethyl etherified starch, enzyme-modified starch, polyacrylamide, polyvinyl alcohol, surface sizing agents, water-resistant agents, water retention agents, thickeners, and lubricants, and these may be used alone or in combination of two or more. Furthermore, these various chemicals may be used in combination with pigments. Examples of pigments include inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, and satin white, and organic pigments such as solid, hollow, and core-shell types may be used alone or in combination of two or more.

[0013] The basis weight of the paper base material can be selected appropriately depending on the desired quality and its application, but is usually 20 g / m 2 More than 600g / m 2 Less than 25 g / m is preferred. 2 More than 600g / m 2 The following is more preferred: For example, when used for wrapping paper, paper bags, lids, lining paper, packaging materials for liquid paper containers such as milk cartons, and posters to be used outdoors, the basis weight of the paper base material is 20 g / m 2 More than 350g / m 2 When used as a flexible packaging material, the paper base material preferably has a basis weight of 20 g / m 2 More than 100g / m 2 Less than 20 g / m is preferable. 2 More than 80g / m 2 The following is more preferable. The soft packaging material is, among the packaging materials, particularly, a material having a mass of 20 g / m 2 From 100g / m 2 It is a flexible packaging material made of thin paper of about 150 g / m2. When used for paper cups, paper containers, paper boxes, paper plates, paper trays, etc., the basis weight of the paper base material is 150 g / m2. 2 More than 300g / m 2 The following is preferred: The density of the paper base material can be appropriately selected depending on the desired qualities and ease of handling, but is usually 0.5 g / cm 3 More than 1.0g / cm 3 The following are preferred:

[0014] The method of manufacturing the paper base material (papermaking) is not particularly limited, and may be a fourdrinier papermaking machine, a cylinder papermaking machine, a short wire papermaking machine, a gap former type, a hybrid former type (on-top former Known manufacturing (papermaking) methods and papermaking machines can be selected, such as twin-wire papermaking machines (such as 100-200 mm-type papermaking machines). The pH during papermaking may be in the acidic range (acidic papermaking), pseudo-neutral range (pseudo-neutral papermaking), neutral range (neutral papermaking), or alkaline range (alkaline papermaking). After papermaking in the acidic range, an alkaline agent may be applied to the surface of the paper layer. The paper base material may be one layer, or may be composed of two or more layers. Furthermore, when treating the surface of a paper substrate with a chemical, the method of surface treatment is not particularly limited, and known coating devices such as a rod metering size press, a pond type size press, a gate roll coater, a spray coater, a blade coater, or a curtain coater can be used.

[0015] (Coating layer) The coating layer contains PHBH, an inorganic pigment, and an adhesive. In addition to PHBH, an inorganic pigment, and an adhesive, the coating layer may contain various auxiliaries that are blended in coating solutions in the papermaking field, such as other biodegradable resins (e.g., polybutylene succinate, polycaprolactone, polylactic acid, etc.), dispersants, viscosity modifiers, water retention agents, defoamers, water resistance agents, fluorescent dyes, coloring dyes, coloring pigments, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, and metal salts, as necessary.

[0016] <phbh> PHBH is a copolymer of 3-hydroxybutyrate (hereinafter also referred to as 3HB) and 3-hydroxyhexanoate (hereinafter also referred to as 3HH), and is a biodegradable resin known to be produced by microorganisms. In the present invention, the PHBH used may be derived from microorganisms or petroleum resources, but it is preferable to use the PHBH derived from microorganisms in terms of reducing the environmental load.

[0017] Microorganisms that produce PHBH are not particularly limited as long as they accumulate PHBH intracellularly, but examples include bacteria of the genus Alcaligenes, such as A. lipolytica, A. eutrophus, and A. latus, as well as bacteria of the genus Pseudomonas, Bacillus, Azotobacter, Nocardia, and Aeromonas. Among them, in terms of productivity of PHBH, strains such as Aeromonas caviae, and Alcaligenes eutrophus AC32 into which genes of PHA synthase group have been introduced (Accession No. FERM BP-6038, Date of deposit on August 7, 1997, National Institute of Advanced Industrial Science and Technology, International Patent Organism Depositary, Address: Central 6, 1-1-1 Higashi, Tsukuba-shi, Ibaraki-ken, Japan) (J. Bacteriol., 179, pp. 4821-4830 (1997)) are particularly preferred. A method for obtaining PHBH from Aeromonas caviae, a microorganism of the Aeromonas genus, is disclosed, for example, in Japanese Patent Application Laid-Open No. 05-093049. These microorganisms are used by culturing them under appropriate conditions to accumulate PHBH in the cells. The carbon source and culture conditions used in the culture can be obtained according to the methods described in JP-A-05-093049, JP-A-2001-340078, etc., but are not limited thereto.

[0018] The composition ratio (mol%) of PHBH is preferably 3HB:3HH=97:3 to 75:25, more preferably 95:5 to 85:15. If the composition of 3HH is less than 3 mol%, the properties of PHBH become similar to those of 3HB homopolymer, resulting in loss of flexibility and an excessively high film-forming processing temperature, which is undesirable. If the composition of 3HH exceeds 25 mol%, the crystallization rate becomes too slow to be suitable for film-forming processing, and the degree of crystallization decreases, making the resin flexible and decreasing the bending modulus. The composition ratio of PHBH can be measured by centrifuging the aqueous dispersion and then drying the powder obtained by NMR analysis. Microbial PHBH is a random copolymer. To adjust the molar ratio of the copolymer, there are several methods, such as selecting the bacterial cells, selecting the carbon source as the raw material, blending with PHBH of different molar ratios, and blending with 3HB homopolymer.

[0019] The weight-average molecular weight of PHBH is preferably 50,000 to 1,500,000. When the weight-average molecular weight of PHBH is within this range, it is possible to form a film at a low temperature when drying after coating. The weight-average molecular weight of PHBH is more preferably 100,000 to 500,000, and even more preferably 150,000 to 450,000. The weight-average molecular weight of PHBH can be determined by gel permeation chromatography (GPC, such as "Shodex GPC-101" manufactured by Showa Denko K.K.) using polystyrene gel (such as "Shodex K-804" manufactured by Showa Denko K.K.) in a column, using chloroform as the mobile phase, and converting it into a polystyrene-equivalent molecular weight. The measurement sample is a powder obtained by centrifuging an aqueous dispersion containing PHBH and then drying it.

[0020] The average particle size of PHBH is preferably 0.1 to 50 μm. PHBH with an average particle size of less than 0.1 μm is difficult to produce by microbial production, and even when obtained by chemical synthesis, a microparticulation operation is required. If the average particle size exceeds 50 μm, uneven coating may occur on the surface when a coating liquid containing PHBH is applied. The average particle size of PHBH is more preferably 0.5 to 10 μm. The average particle size of PHBH refers to the particle size corresponding to 50% accumulation of all particles in a normal distribution when a water suspension of PHBH is adjusted to a predetermined concentration using a general-purpose particle sizer such as a Microtrack particle sizer (manufactured by Nikkiso, FRA). The solid content of PHBH in the coating liquid is not particularly limited and can be adjusted to a viscosity suitable for the coating method, but is preferably 5 to 70% by weight. If the solid content is less than 5% by weight, the coating film tends not to be formed well, and if it exceeds 70% by weight, the viscosity of the coating liquid becomes too high, making coating difficult. The solid content of PHBH in the coating liquid is more preferably 10 to 55% by weight.

[0021] <Inorganic pigments> As the inorganic pigment, those used for coating on paper can be used without any particular limitation, and examples thereof include kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, bentonite, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, satin white, etc., and one or more of these can be used. Among these, one or more of kaolin, heavy calcium carbonate, light calcium carbonate, mica, talc, and bentonite are preferred.

[0022] From the viewpoint of the fixation of the coating layer, the inorganic pigment preferably has a volume 50% average particle size (D50) (hereinafter also referred to as "average particle size") of 6.0 μm or less, as measured by a laser diffraction / scattering method. Examples of measuring devices for the laser diffraction / scattering method include a particle size distribution measuring device "Partica" manufactured by Horiba Ltd. and a particle size distribution measuring device "MASTER Examples include "SIZER S". From the viewpoint of the fixation of the coating layer, the average particle size of the inorganic pigment is more preferably 5.0 μm or less, even more preferably 4.0 μm or less, even more preferably 3.0 μm or less, and even more preferably 2.0 μm or less. There is no particular lower limit to the average particle size of the inorganic pigment, but from the viewpoint of dispersibility, for example, it is preferably 0.1 μm or more, and more preferably 0.2 μm or more. When two or more inorganic pigments are contained, it is preferable that the average particle size of at least one of them is within the above-mentioned numerical range, and the proportion of the inorganic pigments satisfying this average particle size relative to the total inorganic pigments is preferably 50% by weight or more, and more preferably 70% by weight or more.

[0023] In addition, from the viewpoint of oil resistance and water resistance when a second coating layer is provided on the coating layer, the average particle size of the inorganic pigment is preferably 8.0 μm or less. From the viewpoint of aqueous nature, the average particle size of the inorganic pigment is more preferably 7.0 μm or less, even more preferably 6.0 μm or less, even more preferably 5.0 μm or less, even more preferably 4.0 μm or less, even more preferably 3.0 μm or less, and even more preferably 2.0 μm or less. There is no particular lower limit to the average particle size of the inorganic pigment, but from the viewpoint of dispersibility, for example, it is preferably 0.1 μm or more, more preferably 0.2 μm or more. When two or more inorganic pigments are included, it is preferable that the average particle size of at least one of them is within the above-mentioned numerical range, and the ratio of the inorganic pigments satisfying this average particle size to the total inorganic pigments is preferably 50% by weight or more, more preferably 70% by weight or more.

[0024] The aspect ratio of the inorganic pigment is preferably 60 or less in terms of oil resistance and water resistance when a second coating layer is provided on the coating layer. The aspect ratio can be calculated using measurements from a particle size measuring device by the calculation method described in "Basic Research on the Relationship between Coating Pigment Properties and Coated Paper Quality" in Vol. 65, No. 12 of the Paper and Pulp Technical Association. The aspect ratio of the inorganic pigment is more preferably 40 or less, even more preferably 30 or less, even more preferably 25 or less, and even more preferably 20 or less. There is no particular lower limit for the aspect ratio of the inorganic pigment. When two or more inorganic pigments are included, it is preferable that the aspect ratio of at least one of them is within the above-mentioned numerical range, and the proportion of the inorganic pigments satisfying this aspect ratio to the total inorganic pigments is preferably 50% by weight or more, and more preferably 70% by weight or more.

[0025] The solids weight ratio of PHBH to inorganic pigment in the coating layer (PHBH:inorganic pigment, total 100) is 90:10 to 0.01:99.99. By further blending inorganic pigment into a coating liquid containing PHBH and an adhesive, the fixation of the resulting coating layer is improved. Although the mechanism is unclear, the present inventors speculate that this is because inorganic pigments have better thermal conductivity than organic PHBH and adhesive, so that the inorganic pigments quickly rise in temperature when heated, and this heat is transferred from the inorganic pigment to PHBH, thereby heating the PHBH sufficiently.

[0026] The solids weight ratio of PHBH to inorganic pigment (PHBH:inorganic pigment, total 100) is preferably 70:30 to 1:99, more preferably 60:40 to 2:98, and even more preferably 50:50 to 3:97, from the viewpoint of fixation of the coating layer. From the viewpoint of heat seal strength when a second coating layer is provided on the coating layer, the solids weight ratio of PHBH to inorganic pigment (PHBH: inorganic pigment, total 100) is preferably 90:10 to 5:95, more preferably 80:20 to 10:90, even more preferably 70:30 to 10:90, even more preferably 65:35 to 10:90, even more preferably 60:40 to 15:85, and even more preferably 50:50 to 20:80. In particular, when the average particle size of the inorganic pigment exceeds 8.0 μm, from the viewpoint of oil resistance and water resistance, the solids weight ratio of PHBH to inorganic pigment (PHBH: inorganic pigment) is preferably 90:10 to 40:60, and more preferably 90:10 to 50:50. The total ratio of PHBH and the inorganic pigment to the total solid content of the coating layer is preferably 60% by weight or more, more preferably 70% by weight or more, and even more preferably 80% by weight or more.

[0027] <Adhesive> The adhesive bonds the PHBH, inorganic pigment, paper base material, etc. In the coated paper of the present invention, since the coating layer contains an adhesive, it is possible to obtain a uniform coating layer in which coating defects such as cracks and pinholes are suppressed. The adhesive can be used without any particular limitation as long as it can be dissolved or dispersed in water and can bond PHBH, inorganic pigments, paper substrates, etc. For example, fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, acetoacetylated polyvinyl alcohol, carboxy-modified polyvinyl alcohol, amide-modified polyvinyl alcohol, sulfonic acid-modified polyvinyl alcohol, butyral-modified polyvinyl alcohol, olefin-modified polyvinyl alcohol, etc. Examples of the polyvinyl alcohol include polyvinyl alcohol, nitrile-modified polyvinyl alcohol, pyrrolidone-modified polyvinyl alcohol, silicone-modified polyvinyl alcohol, other modified polyvinyl alcohols, polyvinyl alcohols such as ethylene-vinyl alcohol copolymers, starches such as oxidized starch, etherified starch, and esterified starch, cellulose derivatives such as hydroxymethyl cellulose, hydroxyethyl cellulose, methyl cellulose, ethyl cellulose, carboxymethyl cellulose, acetyl cellulose, and nanocellulose, partially saponified ethylene-vinyl acetate copolymers, styrene-butadiene copolymer latex, conjugated diene polymer latex of methyl methacrylate-butadiene copolymer, acrylic polymer latex, styrene-maleic anhydride copolymer latex, polyvinyl chloride latex, and polyvinyl acetate latex. One or more of these can be appropriately selected and used.

[0028] Among these, it is preferable to include at least one selected from the group consisting of polyvinyl alcohols, starches, cellulose derivatives, partially saponified ethylene-vinyl acetate copolymers, styrene-butadiene copolymer latexes, conjugated diene polymer latexes of methyl methacrylate-butadiene copolymers, and acrylic polymer latexes, and more preferably to include at least one selected from this group. In addition, since it is biodegradable, it is more preferable to include at least one selected from the group consisting of polyvinyl alcohols, starches, cellulose derivatives, and partially saponified ethylene-vinyl acetate copolymers, and even more preferable to include at least one selected from the group consisting of fully saponified polyvinyl alcohols, partially saponified polyvinyl alcohols, and partially saponified ethylene-vinyl acetate copolymers.

[0029] In terms of adhesion to a paper substrate, the adhesive preferably contains at least one of fully saponified polyvinyl alcohol and partially saponified polyvinyl alcohol, and more preferably consists of at least one of fully saponified polyvinyl alcohol and partially saponified polyvinyl alcohol. From the viewpoint of water resistance of the coating layer, the adhesive preferably contains a partially saponified ethylene-vinyl acetate copolymer, and more preferably consists of a partially saponified ethylene-vinyl acetate copolymer.

[0030] The ratio of the adhesive to the total solid content of the coating layer is preferably 0.1 to 40% by weight. If the adhesive is less than 0.1% by weight, the adhesive cannot be expected to have any effect on improving fixation, and if it exceeds 40% by weight, the adhesive becomes too much and the performance derived from PHBH may not be fully exhibited, and water resistance decreases, which is not preferable depending on the application of the coated paper. The ratio of the adhesive to the total solid content of the coating layer is more preferably 1% by weight or more, more preferably 3% by weight or more, even more preferably 5% by weight or more, and more preferably 30% by weight or less, even more preferably 25% by weight or less, and even more preferably 20% by weight or less.

[0031] (Second coating layer) In the coated paper of the present invention, a second coating layer containing PHBH can be formed on the coating layer. By forming the second coating layer on the coating layer containing an inorganic pigment, the heat seal strength is improved. Although the mechanism is unclear, the inventors speculate that this is because the coating layer containing an inorganic pigment reaches a high temperature in a short time, and the second coating layer is exposed to a high temperature for a longer time during heat fusion processing.

[0032] The second coating layer may contain the same PHBH as above except for the range of the weight average molecular weight, and the PHBH of the second coating layer preferably has a weight average molecular weight of 50,000 to 1,500,000. The PHBH of the second coating layer is preferably higher in weight average molecular weight than the PHBH of the coating layer. The higher the molecular weight of PHBH, the lower the MFR and the higher temperature is required for heat sealing. However, the second coating layer of the present invention has excellent heat sealing properties, so the PHBH of high molecular weight is Also, H can be suitably used. When the second coating layer contains PHBH having a large weight average molecular weight, the properties such as oil resistance and water resistance derived from PHBH can be more effectively exhibited.

[0033] The second coating layer preferably contains 50% by weight or more of PHBH, more preferably 70% by weight or more, even more preferably 90% by weight or more, even more preferably 95% by weight or more, even more preferably 98% by weight or more, and even more preferably 99% by weight or more. In addition to PHBH, the second coating layer may contain, as necessary, various auxiliaries that are blended in coating solutions in the papermaking field, such as other biodegradable resins such as polybutylene succinate, polycaprolactone, and polylactic acid, the above-mentioned adhesives, inorganic pigments, dispersants, viscosity improvers, water retention agents, defoamers, water resistance agents, fluorescent dyes, coloring dyes, coloring pigments, surfactants, pH adjusters, cationic resins, anionic resins, ultraviolet absorbers, and metal salts.

[0034] (Coating layer, coating of second coating layer) In the present invention, the coating method of the coating layer and the optional second coating layer is not particularly limited, and they can be coated using a known coating device and coating system. For example, the coating device may be a blade coater, a bar coater, a roll coater, an air knife coater, a reverse roll coater, a curtain coater, a spray coater, a size press coater, a gate roll coater, etc. In addition, the coating system may be an aqueous coating using a solvent such as water, a solvent-based coating using a solvent such as an organic solvent, etc., and the aqueous coating is preferable. The coating layer and the second coating layer can be dried by a conventional method such as using a steam heater, a gas heater, an infrared heater, an electric heater, a hot air heater, a microwave, or a cylinder dryer. The second coating layer can be applied simultaneously with the coating layer, before the coating layer is dried, or after the coating layer is dried.

[0035] The coating weight of the coating layer is 1g / m2 in dry weight. 2 More than 50g / m 2 The coating weight of the coating layer is preferably 1 g / m or less. 2 If the thickness is less than 50 g / m, the effect of the coating layer may be almost nonexistent. 2 If the amount is more than this, the drying load during coating will be large. The coating amount of the coating layer is 3g / m 2 More preferably, 5 g / m 2 More preferably, 40 g / m 2 Less than 30 g / m is more preferable. 2 The following is even more preferred:

[0036] When the second coating layer is formed, the coating amount of the second coating layer is 0.5 g / m 2 More than 20g / m 2 The coating weight of the second coating layer is preferably 0.5 g / m or less. 2 If the thickness is less than 20 g / m, the effect of the second coating layer may be almost nonexistent. 2 If the amount is more than this, the drying load during coating will be large. The coating amount of the second coating layer is 1g / m 2 More preferably, 3 g / m 2 More preferably, 17 g / m 2 Less than 14 g / m is more preferable. 2 The following is even more preferred:

[0037] Coated paper Since the coating layer and the optional second coating layer contain PHBH, the functionality of PHBH can be exhibited, and the layer can be used as a heat seal layer, an oil-resistant layer, a water-resistant layer, etc. The coating layer can be provided on only one side or both sides of the paper substrate. When the coating layer is provided on both sides, the second coating layer can be provided on one coating layer or on both coating layers.

[0038] The heat seal layer is a layer that has heat sealability, specifically, a layer that can be bonded to an object by heating and pressing. When imparting heat sealability to the coated paper of the present invention, the pressing temperature is 130° C. and the pressing pressure is 2 kgf / cm. 2 Heat with pressure for 0.5 seconds The heat seal strength when sealed and peeled off with a T-shaped strip at a tensile speed of 200 mm / min is preferably 5.0 N / 15 mm or more. This heat seal strength is more preferably 5.2 N / 15 mm or more, even more preferably 5.5 N / 15 mm or more, even more preferably 5.9 N / 15 mm or more, and even more preferably 6.2 N / 15 mm or more. The upper limit of this heat seal strength is not particularly limited, but is, for example, about 8.5 N / 15 mm.

[0039] The oil-resistant layer is a layer whose kit number, measured at any five points on the layer surface in accordance with "Paper and paperboard - Oil repellency test method - Kit method" specified in J.TAPPI No. 41: 2000, is an average of 4 or more. When imparting oil resistance to the coated paper of the present invention, the average kit number is preferably 6 or more, more preferably 8 or more, even more preferably 10 or more, even more preferably 11 or more, and most preferably 12. The water-resistant layer is a layer that has a water absorption (Cobb value) of 20 g / m2 or more, measured with a contact time of 120 seconds in accordance with JIS P 8140:1998 "Paper and paperboard - Water absorption test method - Cobb method". 2 In order to impart water resistance to the coated paper of the present invention, the water absorption is 10 g / m 2 Less than 5 g / m is preferable. 2 Less than 3 g / m is more preferable. 2 More preferably, 2 g / m 2 Even more preferably, 1 g / m 2 Even more preferred is the following:

[0040] The coated paper of the present invention is easy to mold, maintain its shape, and ensure airtightness, and can therefore be suitably used for paper bags, paper containers, paper boxes, paper cups, (soft) packaging materials, lid materials, and the like. The coated paper of the present invention, in which the coating layer is a heat seal layer, can be suitably used as wrapping paper, paper containers, paper boxes, paper cups, (soft) packaging materials, paper plates, paper trays, etc. The coated paper of the present invention, in which the coating layer is both a heat-sealing layer and an oil-resistant layer, can be suitably used as (soft) packaging materials or wrapping paper for foods that contain a lot of oil, such as hamburgers, hot dogs, French fries, fried chicken, potato chips, etc., paper linings for fried foods such as tempura, paper plates, paper trays, paper cups, etc. EXAMPLES

[0041] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, parts and % are by weight, respectively, unless otherwise specified.

[0042] ·PHBH An aqueous PHBH dispersion having a solid content of 50% by weight was obtained by the method described in Patent Document 1. Next, this aqueous PHBH dispersion was hydrolyzed at 60° C. to adjust the molecular weight, thereby obtaining the following aqueous PHBH dispersion having a solid content of 50%. PHBH1: Weight average molecular weight 200,000 PHBH2: Weight average molecular weight 600,000

[0043] Inorganic pigments Inorganic pigment 1: Kaolin (Shiraishi Kogyosha, KCS) Average particle size: 3.6 μm, aspect ratio: 10 to 15 Inorganic pigment 2: Kaolin (CADAM, Amazon Plus) Average particle size 0.4μm, aspect ratio 9 Inorganic pigment 3: Kaolin (Rio Kapim, Kapim DG) Average particle size 1.2μm, aspect ratio 13 Inorganic pigment 4: Kaolin (Shiraishi Kogyosha, Varisurf HX) Average particle size: 8.7 μm, aspect ratio: 80-100 Inorganic pigment 5: Heavy calcium carbonate (Bihoku Powder Industry Co., Ltd., Hydrocarb 90) Average particle size<2μm Inorganic pigment 6: Delaminated kaolin (Engelhard, New Surf) Average particle size 6.3μm, aspect ratio 16 ·glue PVA1: Kuraray Co., Ltd.: 28-98, saponification degree 98 mol%, polymerization degree 1700

[0044] (Evaluation method) ·Ceropic After drying for 24 hours, cellophane tape (25 mm wide) was applied to the surface of the coating layer, and a rubber roller 130 mm wide and weighing 1.8 kg was rolled back and forth 10 times under its own weight on the cellophane tape to adhere the cellophane tape to the surface of the coating layer. Immediately afterwards, the cellophane tape was vigorously peeled off, and the ratio of the area where the coating layer was attached to the cellophane tape and peeled off from the paper substrate surface (area of ​​interface failure) or the ratio of the area where the paper substrate was destroyed by a part of the paper substrate attached to the cellophane tape together with the coating layer (area of ​​internal failure of the paper substrate) was calculated to evaluate the adhesion to the paper substrate according to the following criteria. If the evaluation is ◎, 〇, or △, there is no problem in practical use. If the evaluation differs between the percentage of the area where the coating layer peeled off and the percentage of the area where the paper base material was destroyed, the more severe evaluation was adopted. [Evaluation criteria] ◎: The percentage of the area where the coating layer peeled off is less than 5%. Or, the percentage of area where the paper base material is destroyed is 95% or more. ○: The percentage of the area where the coating layer peeled off was 5% or more and less than 10%. Or, the percentage of the area where the paper base material is destroyed is between 90% and 95%. △: The percentage of the area where the coating layer peeled off was 10% or more and less than 30%. Or, the percentage of the area where the paper base material is destroyed is between 70% and 90%. ×: The percentage of the area where the coating layer peeled off was 30% or more. Or the percentage of area where the paper base is destroyed is less than 70%.

[0045] Heat seal strength The test was conducted in accordance with JIS Z1707:2019 7.4 "Heat seal strength test". Two square test pieces with sides of 100 mm were cut out from the obtained coated paper, and the coating layers were brought into contact with each other and pressed at a pressure of 130°C and 2 kgf / cm. 2 The test piece was heat-sealed with pressure for 0.5 seconds, and a measurement sample was cut out from the heat-sealed 100 mm square test piece so that the long side was 100 mm and the short side was 15 mm. The peeled long edge was then clamped between the upper and lower jigs of a vertical tensile testing machine (Tensilon, manufactured by A&D Corporation), and the peel strength, i.e., HS strength, was measured while peeling the measurement sample (T-type) from the long edge side at a speed of 200 mm / min.

[0046] ·Oil resistance The kit number was measured at any five points on the coating layer surface in accordance with "Paper and paperboard - Oil repellency test method - Kit method" specified in JAPAN TAPPI No. 41:2000. The average value of the five kit numbers measured was used as the value of oil resistance, and the oil resistance was evaluated according to the following criteria: If the evaluation was ◯ or △, there was no problem in practical use. [Evaluation Criteria] ○: Average kit number is 8 or higher. △: Average kit number is 4 or more but less than 8. ×: Average kit number is less than 4. ·water resistance In accordance with JIS P 8140:1998 "Paper and paperboard - Water absorption test method - Cobb method", the water absorbency (Cobb value) was measured on the coating layer surface with a contact time of 120 seconds, and this was used as the water resistance value.

[0047] [Examples 1 to 9, Reference Example 1, Comparative Examples 1 to 3] PHBH 1, inorganic pigment 1, and PVA 1 were added so as to obtain the solid content weight ratio shown in Table 1, and water was further added and stirred to obtain a coating liquid with a solid content concentration of 40 wt %. Paper base material (basis weight 50g / m 2 ) on one side of the sheet, this coating solution was applied at a dry weight of 10 g / m 2 The coating was then dried at 105°C for 1 minute to obtain a coated paper. The resulting coated papers were subjected to a cellophane test. Furthermore, the heat seal strength was measured for the coated papers obtained in Examples 1 and 3 and Comparative Example 1. The results are shown in Table 1. [Table 1]

[0048] The coated papers obtained in Examples 1 to 9 of the present invention and Comparative Example 3 not containing PHBH had cellophane ratings of ◯ or Δ, and the coating layer had sufficient strength for practical use. In contrast, the coated papers obtained in Reference Example 1 and Comparative Examples 1 and 2, which contained small amounts of inorganic pigment, had cellophane evaluations of ×, and the coating layer was brittle and easily peeled off. Furthermore, the results of the HS strength of the coated papers obtained in Examples 1 and 3 and Comparative Example 1 showed that, in the case of a single coating layer, the HS strength tended to decrease as the inorganic pigment content increased.

[0049] [Examples 1-2 to 9-2, Reference Example 1-2a, Comparative Examples 1-2 to 3-2] PHBH2 and PVA1 were mixed so as to obtain the solid content weight ratio shown in Table 2, and water was further added and stirred to prepare a coating solution for the second coating layer having a solid content concentration of 40 wt % in total of PHBH and PVA. On the coating layer of the coated paper obtained in Examples 1 to 9, Reference Example 1, and Comparative Examples 1 to 3, the coating solution for the second coating layer was applied in a coating amount of 10.0 g / m2 in terms of dry weight. 2 The coated paper was then dried at 160° C. for 3 minutes to obtain a coated paper having a second coating layer. The resulting coated papers were subjected to a cellophane test and a heat seal strength test. In addition, some of the coated papers were subjected to a water resistance test. The results are shown in Table 2.

[0050] [Table 2]

[0051] The second coating layer had excellent coating strength and only slight peeling occurred when using cellophane. Moreover, the samples (Examples 1-2 to 9-2) in which a second coating layer was further provided on the coating layer of the coated paper obtained in Examples 1 to 9 were excellent in heat seal strength. In particular, the results of Examples 4-2 to 8-2 confirmed that the heat seal strength was further increased at this range of blending ratio of PHBH and inorganic pigment in the coating layer. From this, it was confirmed that the formation of a coating layer containing PHBH on a coating layer having an inorganic pigment facilitates the progress of heat fusion. Furthermore, it was confirmed from Reference Example 1-2a that the inclusion of an adhesive in the coating layer resulted in a coated paper with excellent water resistance.

[0052] [Examples 10 to 14, 21] PHBH1, any one of inorganic pigments 1 to 5, and PVA1 were added so as to obtain the solid content weight ratio shown in Table 3, and water was further added and stirred to obtain a coating liquid with a solid content concentration of 40% by weight. Note that the pigment was used in a relatively high amount of 70 parts in order to confirm the effect of the pigment. Paper base material (basis weight 50g / m 2 ) on one side of the sheet, the coating liquid was applied at a dry weight of 10 g / m 2 The coating was then dried at 105°C for 1 minute to obtain a coated paper. The resulting coated paper was subjected to a cellophane test. The results are shown in Table 3 together with those of Reference Example 1.

[0053] [Table 3]

[0054] The coated papers obtained in Examples 13 and 21 were clearly inferior in cellotropic properties to the coated papers obtained in Examples 10 to 12 and 14. This suggests that the average particle size of the pigment in the coating layer affects cellotropic properties.

[0055] [Examples 10-2 to 14-2, 21-2, Reference Example 1-2b] Water was added to the aqueous dispersion of PHBH1 so as to obtain the solid content weight ratio shown in Table 4, and the mixture was stirred to prepare Coating Solution 2 for the second coating layer, in which the solid content concentration of PHBH was 40% by weight. On the coating layer of the coated paper obtained in Examples 10 to 14, 21 and Reference Example 1, Coating Solution 2 for the second coating layer was applied in a coating amount of 10.0 g / m2 (dry weight). 2 The coated paper was then dried at 160° C. for 3 minutes to obtain a coated paper having a second coating layer. The coated paper thus obtained was subjected to a cellophane test, and measurements of oil resistance and water resistance were carried out. The results are shown in Table 4.

[0056] [Table 4]

[0057] The second coating layer had excellent coating strength and only slight peeling with cellophane. On the other hand, the HS strength of the coated paper obtained in Example 13-2 was 3.8 N / 15 mm, which was equivalent to the other coated papers in Table 4. The samples obtained in Examples 10 to 12, 14, and 21, in which a second coating layer was further provided on the coating layer of the coated paper, had an average kit number of 8 or more, and were extremely excellent in oil resistance. The sample obtained in Example 13, in which a second coating layer was further provided on the coating layer of the coated paper, had an average kit number of 4 or more and less than 8, and was somewhat excellent in oil resistance. It is presumed that the oil resistance of the coated paper obtained in Example 13 was inferior to that of the other examples because the inorganic pigment used was larger than that of the other examples, and the gaps between the pigments in the coating layer could not be filled by the PHBH and adhesive.

[0058] [Examples 15 to 20, Comparative Examples 4 to 6] PHBH 1, inorganic pigment 1 or 4, and PVA 1 were added so as to obtain the solid content weight ratio shown in Table 5, and water was further added and stirred to obtain a coating liquid with a solid content concentration of 40 wt %. Paper base material (basis weight 50g / m 2 ) on one side of the sheet, the coating liquid was applied at a dry weight of 10 g / m 2 The coating was then dried at 105°C for 1 minute to obtain a coated paper. Further, water was added to the aqueous dispersion of PHBH2 and stirred to prepare Coating Solution 3 for the second coating layer having a solid content of 40% by weight. Coating Solution 3 for the second coating layer was applied to the coating layer of the obtained coated paper in a coating amount of 10.0 g / m2 in terms of dry weight. 2 The coated paper was then dried at 160° C. for 3 minutes to obtain a coated paper having a second coating layer. The oil resistance of the resulting coated paper was measured, and the results are shown in Table 5 together with those of Reference Example 1-2a.

[0059] [Table 5]

[0060] It was confirmed from Reference Example 1-2a that PHBH alone was inferior in oil resistance, while Comparative Examples 4 to 6 confirmed that oil resistance could be exhibited by combining PHBH with an adhesive, or by combining an inorganic pigment having a small particle size with an adhesive. In Examples 15 to 19 according to the present invention, the particle size of the inorganic pigment was small, and therefore the oil resistance was excellent. Example 20 used an inorganic pigment with a large particle size, and was inferior in oil resistance to other examples. Combined with the results of Example 13-2, it was suggested that when the inorganic pigment in the coating layer becomes large, the gaps between the pigments in the coating layer cannot be filled with PHBH and adhesive. However, as shown by Examples 13 and 13-2, even if the inorganic pigment is large, the heat sealability is sufficient, and it can be used sufficiently for applications that do not require excellent oil resistance.

[0061] [Examples 22 to 46] PHBH1, inorganic pigments 2 to 6, and PVA1 were added so as to obtain the solid content weight ratios shown in Table 6, and water was further added and stirred to obtain a coating liquid with a solid content concentration of 40% by weight. Paper base material (basis weight 50g / m 2 ) on one side of the sheet, the coating liquid was applied at a dry weight of 10 g / m 2 The coating was then dried at 105°C for 1 minute to obtain a coated paper. The coated papers obtained were subjected to a cellophane test, and some of the coated papers were subjected to a heat seal strength test. The results are shown in Table 6.

[0062] [Table 6]

[0063] Examples 32 to 36, in which the average particle size of the inorganic pigment contained in the coating layer was 8.7 μm, and Examples 42 to 46, in which the average particle size was 6.3 μm, were inferior in cellotropic properties, confirming that the cellotropic properties decrease as the average particle size of the inorganic pigment increases. As shown in Examples 24, 29, and 39, when an inorganic pigment with a small average particle size was used, the heat seal strength of the coating layer was almost unchanged.

[0064] [Examples 23-2 to 45-2] For some of the coated papers obtained in Examples 22 to 46, the coating solution for the second coating layer used in Examples 1-2, etc. was applied on the coating layer in a coating amount of 10.0 g / m2 in terms of dry weight. 2 The coated paper was then dried at 160° C. for 3 minutes to obtain a coated paper having a second coating layer. The resulting coated paper with the second coating layer was subjected to a cellophane test and heat seal strength measurement. The water resistance was then measured, and the results are shown in Table 7. [Table 7]

[0065] Examples 23-2 to 25-2, 28-2 to 30-2, 38-2 to 40-2, 43-2 to 4 The coated paper obtained in 5-2 had excellent strength of the second coating layer, and only slight peeling with cellophane. It also had excellent heat seal strength and water resistance. This confirmed that the provision of a second coating layer on top of the coating layer facilitates the thermal fusion of the coated paper. Example 35-2 was inferior in cellopic and also significantly inferior in water resistance. Example 35-2 is a sample containing a large amount of inorganic pigment with an average particle size of 8.7 μm, PHBH:inorganic pigment=25:75. Therefore, it is presumed that there are many gaps in the coating layer, and even if the second coating layer is formed, the gaps in the lower coating layer cannot be filled. Since the coated papers obtained in Examples 34-2 and 45-2 have good cellopic and water resistance, it was suggested that the cellopic and water resistance would be improved if the coating amount of the second coating layer is increased and the gaps in the lower coating layer are sufficiently filled. The coated paper obtained in Example 35-2 has sufficient heat seal strength and can be used for applications that do not require water resistance, oil resistance, etc.< / phbh>

Claims

1. A coating layer containing PHBH (poly(3-hydroxybutyrate-co-3-hydroxyhexanoate)), an inorganic pigment, and an adhesive on at least one surface of a paper substrate; A second coating layer containing PHBH is provided on the coating layer, the coating layer has a solids weight ratio of PHBH to inorganic pigment (PHBH:inorganic pigment) of 90:10 to 0.01:99.99, and a ratio of the adhesive to the total solids is 0.1 to 40% by weight; A coated paper (excluding those in which the inorganic pigment is a coloring pigment) characterized in that the inorganic pigment has a volume 50% average particle size (D50) of 0.1 μm or more.

2. The coating amount of the coating layer is 3 g / m 2 30g / m or more 2 is as follows: The coating amount of the second coating layer is 0.5 g / m 2 20g / m or more 2 2. The coated paper of claim 1, wherein:

3. 3. The coated paper according to claim 1 or 2, characterized in that the inorganic pigment is one or more selected from the group consisting of kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, bentonite, titanium dioxide, barium sulfate, calcium sulfate and satin white.

4. 3. The coated paper according to claim 1, wherein the weight average molecular weight of PHBH in the coating layer and the second coating layer is from 50,000 to 1,500,000.

5. 5. The coated paper of claim 4, wherein the weight average molecular weight of the PHBH in the second coating layer is the same as or greater than the weight average molecular weight of the PHBH in the first coating layer.

6. 3. The coated paper according to claim 1, wherein the second coating layer contains 50% by weight or more of PHBH.

Citation Information

Patent Citations

  • Coated paper

    JP2021195716A

  • Coated paper

    JP2021195717A

  • Aqueous dispersion of biodegradable polyester and method for production thereof

    WO2004041936A1