Method of manufacturing toner binder

The method of transesterifying crystalline polyesters with different solubility parameters addresses the dispersibility issue in toner binders, resulting in improved low-temperature fixability and heat-resistant storage stability, suitable for high-image-quality toners.

JP2024133754AInactive Publication Date: 2024-10-03SANYO CHEM IND LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023043705
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing toner binders face a trade-off between low-temperature fixability and heat-resistant storage stability, with crystalline polyester resins having insufficient dispersibility in amorphous polyester resins, especially when toner particles are made smaller for higher image quality.

Method used

A method involving the transesterification of two types of crystalline polyesters with different solubility parameters to produce a crystalline polyester resin, followed by melt-mixing with an amorphous polyester resin, ensuring excellent dispersibility and compatibility.

Benefits of technology

The resulting toner binder achieves improved dispersibility of crystalline polyester resin in amorphous polyester resin, enhancing both low-temperature fixability and heat-resistant storage stability, with better particle size distribution and charging characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133754000001
    Figure 2024133754000001
  • Figure 2024133754000002
    Figure 2024133754000002
  • Figure 2024133754000003
    Figure 2024133754000003
Patent Text Reader

Abstract

To provide a crystalline polyester resin which provides superior dispersibility in toner when the toner particle size is reduced to meet the demand for higher image quality.SOLUTION: A toner binder manufacturing method is provided, comprising a step 1 of obtaining a crystalline polyester resin (A) by transesterifying two types of crystalline polyesters with different solubility parameters, where a difference in the solubility parameters of the crystalline polyesters is 0.10-0.50 (cal / cm3)1 / 2 in absolute terms.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a toner binder. [Background technology]

[0002] In recent years, along with the promotion of miniaturization, speedup, and high image quality of electrophotographic devices, from the viewpoint of energy saving, such as reducing energy consumption in the fixing process, there is a strong demand for improving the low-temperature fixability of toners. However, in general, when low-temperature fixability is improved, heat-resistant storage stability is reduced, and when heat-resistant storage stability is improved, low-temperature fixability is reduced. Therefore, there is a trade-off between low-temperature fixability and heat-resistant storage stability, and there is a demand for the development of a toner binder that can achieve both low-temperature fixability and heat-resistant storage stability. The toner binder has a significant effect on the toner characteristics as described above. Known examples of the toner binder include polystyrene resin, styrene-acrylic resin, polyester resin, epoxy resin, polyurethane resin, and polyamide resin. Recently, polyester resin has been attracting particular attention because it is easy to balance storage stability and fixability. For example, a toner using a crystalline polyester resin with excellent melting properties and an amorphous resin has been proposed for the purpose of low-temperature fixing properties (see Patent Document 1). Also, a toner composition containing a hybrid polyester of a crystalline polyester and an amorphous polyester has been proposed for the purpose of improving low-temperature fixing properties and chargeability (see Patent Document 2). However, when the particle size of the toner is reduced to meet the demand for even higher image quality, the dispersibility of the crystalline polyester resin in the toner using the above-mentioned crystalline polyester resin is not sufficient, and improvements in this respect are desired. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2002-287426 A [Patent Document 2] Patent No. 6485155 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a toner binder that exhibits excellent dispersibility of a crystalline polyester resin in an amorphous polyester resin. [Means for solving the problem]

[0005] The present inventors conducted extensive research to solve these problems and arrived at the present invention. That is, the present invention is a method for producing a toner binder, comprising a step 1 of obtaining a crystalline polyester resin (A) by subjecting two kinds of crystalline polyesters (a) having different solubility parameters to an ester exchange reaction, and wherein the absolute value of the difference in solubility parameter between the crystalline polyester (a1) having the smaller solubility parameter and the crystalline polyester (a2) having the larger solubility parameter of the crystalline polyester (a) is 0.10 to 0.50 (cal / cm 3 ) 1 / 2 The present invention relates to a method for producing a toner binder. Effect of the Invention

[0006] The toner binder produced by the production method of the present invention has an effect of providing excellent dispersibility of the crystalline polyester resin in the amorphous polyester resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The present invention will be described in detail below.

[0008] The method for producing a toner binder of the present invention includes a step 1 of obtaining a crystalline polyester resin (A) by transesterification of two kinds of crystalline polyesters (a) having different solubility parameters, and a step 2 of melt-mixing a composition preferably containing the crystalline polyester resin (A) and the amorphous polyester resin (B). The method for producing the toner binder of the present invention will be described below in detail.

[0009] [Process 1] Step 1 is a step in which two kinds of crystalline polyesters (a) having different solubility parameters are subjected to an ester exchange reaction to obtain a crystalline polyester resin (A).

[0010] In step 1, two types of crystalline polyesters (a) having different solubility parameters are subjected to an ester exchange reaction to obtain a crystalline polyester resin (A). This makes it possible to obtain a crystalline polyester resin having a block structure in which a crystalline polyester segment having a low solubility parameter that exhibits excellent precipitation properties in a toner binder and a crystalline polyester segment having a high solubility parameter that exhibits excellent compatibility with an amorphous polyester resin are chemically bonded, thereby making it possible to obtain a toner binder that exhibits excellent dispersibility of the crystalline polyester resin in the amorphous polyester resin. In the present invention, "crystalline" means that in differential scanning calorimetry (also referred to as DSC measurement), a DSC curve has a peak top temperature (Tm) of an endothermic peak. The method for measuring the peak top temperature (Tm) of the endothermic peak is described below. The measurement is performed using a differential scanning calorimeter (e.g., DSC Q20, manufactured by TA Instruments, Inc.). The sample is first heated from 30°C to 180°C at 10°C / min, then cooled from 180°C to 0°C at 10°C / min, and then heated a second time from 0°C to 180°C at 10°C / min. The top temperature of the endothermic peak during the second heating process is taken as the peak top temperature (Tm) of the endothermic peak.

[0011] [Crystalline polyester (a)] The crystalline polyester (a) is not particularly limited as long as it is a polyester having crystallinity and a hydroxyl group, but from the viewpoint of reactivity, it is preferable that it is a polyester having two or more hydroxyl groups in one molecule. In addition, the crystalline polyester (a) is preferably a polycondensate of an alcohol component (x) and a carboxylic acid component (y).

[0012] Examples of the alcohol component (x) of the crystalline polyester (a) in the present invention include aliphatic diols (x1) having 2 to 36 carbon atoms, diols other than the aliphatic diols (x1) having 2 to 36 carbon atoms, and polyols having a valence of 3 or more.

[0013] Examples of the aliphatic diol (x1) having 2 to 36 carbon atoms include linear aliphatic diols having 2 to 36 carbon atoms (ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,9-nonanediol, 1,10-decanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,15-pentadecanediol, 1,18-octadecanediol, 1,19-nonadecanediol, and the like. diol and 1,20-eicosanediol, etc.), branched aliphatic diols having 3 to 36 carbon atoms (propylene glycol, 1,2-butanediol, 1,2-pentanediol, 1,2-hexanediol, 1,2-heptanediol, 1,2-octanediol, 1,2-nonanediol, 1,2-decanediol, etc.), and alicyclic diols having 4 to 36 carbon atoms (for example, 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.).

[0014] Examples of diols other than the aliphatic diol (x1) having 2 to 36 carbon atoms include alkylene ether glycols having 4 to 36 carbon atoms (for example, diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc.), alkylene oxide (hereinafter, "alkylene oxide" may be abbreviated as AO) adducts of the above-mentioned alicyclic diols (preferably the number of moles added is 1 to 30), alkylene oxide adducts of bisphenols (bisphenol A, bisphenol F, bisphenol S, etc.) (preferably the number of moles added is 2 to 30), polylactone diols (poly ε-caprolactone diol, etc.), and polybutadiene diols.

[0015] In the alkylene oxide adducts of alicyclic diols or bisphenols, examples of the alkylene oxide include ethylene oxide adducts, propylene oxide adducts, and butylene oxide adducts.

[0016] Examples of polyols having a valence of three or more include alkane polyols and their intramolecular or intermolecular dehydration products (for example, glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, sorbitan, polyglycerin, etc.), sugars and derivatives thereof (for example, sucrose and methyl glucoside, etc.), alkylene oxide adducts of trisphenols (trisphenol PA, etc.) (the number of moles added is preferably 2 to 30), alkylene oxide adducts of novolak resins (including phenol novolak and cresol novolak, etc., the average degree of polymerization being preferably 3 to 60) (the number of moles added is preferably 2 to 30), and acrylic polyols [copolymers of hydroxyethyl (meth)acrylate and other vinyl monomers, etc.].

[0017] Examples of the carboxylic acid component (y) of the crystalline polyester (a) in the present invention include aliphatic dicarboxylic acids (y1) having 4 to 36 carbon atoms, aromatic dicarboxylic acids, and polycarboxylic acids having a valence of 3 or more, as well as anhydrides and lower alkyl (having 1 to 4 carbon atoms) esters (methyl esters, ethyl esters, isopropyl esters, etc.) of these acids.

[0018] Examples of the aliphatic dicarboxylic acid (y1) having 4 to 36 carbon atoms include linear aliphatic dicarboxylic acids having 4 to 36 carbon atoms (adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, 1,18-octadecanedicarboxylic acid, etc.), and branched aliphatic dicarboxylic acids having 4 to 36 carbon atoms (decylsuccinic acid, dodecenylsuccinic acid, pentadecenylsuccinic acid, octadecenylsuccinic acid, etc.).

[0019] The aromatic dicarboxylic acid is not particularly limited as long as it is a carboxylic acid having two carboxyl groups bonded to a conjugated unsaturated ring structure such as a benzene ring or a naphthalene ring, and examples thereof include aromatic dicarboxylic acids having 8 to 36 carbon atoms (such as phthalic acid, isophthalic acid, terephthalic acid, t-butylisophthalic acid, 2,6-naphthalenedicarboxylic acid, and 4,4'-biphenyldicarboxylic acid).

[0020] Examples of polycarboxylic acids having a valence of three or more include aromatic polycarboxylic acids having 9 to 20 carbon atoms (such as trimellitic acid and pyromellitic acid), aliphatic tricarboxylic acids having 6 to 36 carbon atoms (such as hexanetricarboxylic acid), and vinyl polymers of unsaturated carboxylic acids [number average molecular weight (Mn): 450 to 10,000] (such as styrene / maleic acid copolymers, styrene / acrylic acid copolymers, and styrene / fumaric acid copolymers).

[0021] In the present invention, from the viewpoints of low-temperature fixability and heat-resistant storage stability, it is preferred that the crystalline polyester (a) is a polycondensate of an alcohol component (x) and a carboxylic acid component (y), the alcohol component (x) contains an aliphatic diol (x1) having 2 to 36 carbon atoms, and the carboxylic acid component (y) contains an aliphatic dicarboxylic acid (y1) having 4 to 36 carbon atoms, and it is more preferred that the alcohol component (x) is a linear aliphatic diol having 2 to 24 carbon atoms, and the carboxylic acid component (y) is a linear aliphatic dicarboxylic acid having 4 to 36 carbon atoms.

[0022] The reaction ratio of the alcohol component (x) and the carboxylic acid component (y) is preferably 1 / 2 to 2 / 1, more preferably 1 / 1 to 1.5 / 1, and even more preferably 1.004 / 1 to 1.040 / 1, in terms of the molar ratio of hydroxyl groups to carboxyl groups {[OH] / [COOH]}. The hydroxyl groups are those derived from the alcohol component.

[0023] The crystalline polyester (a) in the present invention can be produced in the same manner as in the production of known polyesters. For example, the reaction can be carried out by reacting the components in an inert gas (nitrogen gas, etc.) atmosphere at a reaction temperature of preferably 150 to 280° C., more preferably 160 to 250° C., and even more preferably 170 to 235° C. The reaction time is preferably 30 minutes or more, more preferably 2 to 40 hours, from the viewpoint of ensuring that the polycondensation reaction is carried out. In order to improve the reaction rate, it is preferable to have a step of reducing pressure in addition to the step at normal pressure (pressure of 80 to 120 kPa), and the degree of reduced pressure is preferably 20 kPa or less, more preferably 15 kPa or less, even more preferably 10 kPa or less, and particularly preferably 5 kPa or less.

[0024] In this case, an esterification catalyst can be used as necessary. Examples of the esterification catalyst include tin-containing catalysts (e.g., dibutyltin oxide, etc.), antimony trioxide, titanium-containing catalysts [e.g., titanium alkoxide, potassium oxalate titanate, titanium terephthalate, titanium alkoxide terephthalate, catalysts described in JP-A-2006-243715 (titanium diisopropoxybistriethanolaminate, titanium dihydroxybistriethanolaminate, titanium monohydroxytriethanolaminate, titanyl bistriethanolaminate, and intramolecular polycondensates thereof, etc.), and catalysts described in JP-A-2007-11307 (titanium tributoxyterephthalate, titanium triisopropoxyterephthalate, titanium diisopropoxyditerephthalate, etc.)], zirconium-containing catalysts (e.g., zirconyl acetate, etc.), and zinc acetate. Of the esterification catalysts, titanium-containing catalysts are preferred from the viewpoint of low-temperature fixability, and the catalysts described in JP-A-2006-243715 and JP-A-2007-11307 are more preferred.

[0025] The absolute value of the difference in solubility parameter between the crystalline polyester (a1) having a smaller solubility parameter and the crystalline polyester (a2) having a larger solubility parameter, among the crystalline polyesters (a), is 0.10 to 0.50 (cal / cm) from the viewpoints of low-temperature fixability, heat-resistant storage stability, and dispersibility.3 ) 1 / 2 and preferably 0.12 to 0.41 (cal / cm 3 ) 1 / 2 The absolute value of the difference in solubility parameters is 0.10 (cal / cm 3 ) 1 / 2 If it is more than 0.50 (cal / cm 3 ) 1 / 2 If it is less than this, the crystallinity will be good. The solubility parameter (SP value) is calculated by the method proposed by Fedors et al. in the following document. The SP value of the crystalline polyester (a) in the present invention can be calculated by determining the SP value of the structure obtained by removing the hydroxyl group from the alcohol component used and the hydrogen of the carboxyl group from the carboxylic acid component used, and taking the arithmetic average based on the molar fraction. "POLYMER ENGINEERING AND SCIENCE, FEBRUARY, 1974, Vol. 14, No. 2, ROBERT F. FEDORS. (pages 147-154)" In the present invention, the SP value of the crystalline polyester (a) refers to the SP value of the structure excluding the terminal functional groups.

[0026] The crystalline polyester (a) has an endothermic peak top temperature (Tm) of 50 to 85°C, preferably 60 to 85°C, and more preferably 70 to 85°C, as measured by a differential scanning calorimeter (DSC). When Tm is 50° C. or higher, the crystallinity is good, and when it is 85° C. or lower, the dispersibility is good. Tm can be adjusted by the content and carbon number of the aliphatic diol (x1) having 2 to 36 carbon atoms and the content and carbon number of the aliphatic dicarboxylic acid (y1) having 4 to 36 carbon atoms. For example, as the content and carbon number of the aliphatic diol (x1) and the aliphatic dicarboxylic acid (y1) increase, the peak top temperature (Tm) becomes higher.

[0027] From the viewpoint of crystallinity, the crystalline polyester (a) preferably has an endothermic value based on an endothermic peak measured by a differential scanning calorimeter (DSC) of 20 to 120 J / g.

[0028] The acid value of the crystalline polyester (a) is preferably from 0 to 10 mgKOH / g, more preferably from 0 to 1 mgKOH / g, from the viewpoints of crystallinity and reactivity.

[0029] The hydroxyl value of the crystalline polyester (a) is preferably from 1 to 100 mgKOH / g, more preferably from 5 to 50 mgKOH / g, from the viewpoints of crystallinity and reactivity.

[0030] The weight average molecular weight (hereinafter sometimes abbreviated as Mw) of the crystalline polyester (a) is preferably from 2,000 to 2,000,000, and more preferably from 10,000 to 50,000, from the viewpoints of crystallinity and reactivity.

[0031] [Transesterification] The transesterification reaction in step 1 is not particularly limited as long as it is a reaction in which an ester group portion of one of two crystalline polyesters (a) having different solubility parameters is exchanged with a hydroxyl group portion of the other crystalline polyester, and can be carried out in an inert gas (nitrogen gas, etc.) atmosphere at a reaction temperature of preferably 120 to 280° C., more preferably 130 to 230° C., and even more preferably 150 to 180° C. From the viewpoint of ensuring that the transesterification reaction is carried out, the reaction time is preferably 30 minutes or more, more preferably 2 to 40 hours. From the viewpoint of reactivity, it is preferable to have a step of reducing the pressure in the reaction system during the ester exchange reaction in step 1, and the degree of reduced pressure is preferably 20 kPa or less, more preferably 15 kPa or less, even more preferably 10 kPa or less, and particularly preferably 5 kPa or less.

[0032] In this case, an esterification catalyst can be used as necessary. Examples of the esterification catalyst include those similar to those used in the production of the crystalline polyester (a). From the viewpoint of reactivity, it is preferable to carry out the transesterification reaction in step 1 in the presence of a titanium-containing catalyst, and more preferable examples thereof include titanium diisopropoxybistriethanolaminate, titanium dihydroxybistriethanolaminate, titanium monohydroxytriethanolaminate, titanylbistriethanolaminate, and intramolecular polycondensates thereof.

[0033] In step 1, the method for mixing the two crystalline polyesters (a) having different solubility parameters is not particularly limited. From the viewpoints of low-temperature fixability, heat-resistant storage stability, and dispersibility, the weight ratio [(a1):(a2)] of the crystalline polyester (a1) having the smaller solubility parameter to the crystalline polyester (a2) having the larger solubility parameter is preferably 30:70 to 90:10, and more preferably 30:70 to 50:50.

[0034] [Process 2] Step 2 is a step of melt-mixing a composition containing a crystalline polyester resin (A) and an amorphous polyester resin (B). By melt-mixing the composition containing the crystalline polyester resin (A) and the amorphous polyester resin (B) obtained in step 1 in step 2, it is possible to provide a toner binder with excellent dispersibility.

[0035] [Crystalline polyester resin (A)] As described above, the crystalline polyester resin (A) can be obtained by subjecting two kinds of crystalline polyesters (a) having different solubility parameters to an ester exchange reaction in step 1. It is preferable that the resulting crystalline polyester resin (A) has an endothermic peak top temperature (Tm) of 50°C to 90°C and an endothermic amount based on the endothermic peak of 70 to 110 J / g, as measured by a differential scanning calorimeter (DSC).

[0036] From the viewpoints of crystallinity and dispersibility, it is preferable that the peak top temperature (Tm) of the endothermic peak of the crystalline polyester resin (A) measured by a differential scanning calorimeter (DSC) satisfies the relation (1). Relationship formula (1): {(Tma1)×(aw1) / ((aw1)+(aw2))+(Tma2)×(aw2) / ((aw1)+(aw2))}×0.97≦(Tm)≦{(Tma1)×(aw1) / ((aw1)+(aw2))+(Tma2)×(aw2) / ((aw1)+(aw2))}×1.03

[0037] In the relational formula (1), Tma1 is the peak top temperature of the endothermic peak of the crystalline polyester (a1) having the smaller solubility parameter, Tma2 is the peak top temperature of the endothermic peak of the crystalline polyester (a2) having the larger solubility parameter, aw1 is the weight ratio of (a1) based on the total weight of (a1) and (a2), and aw2 is the weight ratio of (a2) based on the total weight of (a1) and (a2). {(Tma1)×(aw1) / ((aw1)+(aw2))+(Tma2)×(aw2) / ((aw1)+(aw2))} is the calculated weighted average of the endothermic peak top temperatures of two crystalline polyesters (a) with different solubility parameters. When two crystalline polyesters (a) with different solubility parameters are simply mixed, the weighted average is not obtained, and the endothermic peak top temperature of either (a1) or (a2) approaches the value. In addition, when the constituent monomers used in the two crystalline polyesters (a) with different solubility parameters are esterified at once, the weighted average is not obtained, and the endothermic peak top temperature of either (a1) or (a2) approaches the value. In other words, it is estimated that the relational formula (1) indicates the presence or absence of a block structure in which (a1) and (a2) are bonded while maintaining their respective segments to a certain extent or more. The relationship (1) can be easily adjusted, for example, by setting the reaction time of the ester exchange reaction of two types of crystalline polyesters (a) having different solubility parameters to 20 hours or more and by setting the hydroxyl value of the crystalline polyester (a) to 5 mgKOH / g or more.

[0038] The acid value of the crystalline polyester resin (A) is preferably from 0 to 10 mgKOH / g, more preferably from 0 to 2 mgKOH / g, from the viewpoint of crystallinity.

[0039] The hydroxyl value of the crystalline polyester resin (A) is preferably from 1 to 100 mgKOH / g, more preferably from 3 to 10 mgKOH / g, from the viewpoint of crystallinity.

[0040] The weight average molecular weight of the crystalline polyester resin (A) is preferably from 2,000 to 2,000,000, and more preferably from 20,000 to 40,000, from the viewpoint of crystallinity.

[0041] [Amorphous polyester resin (B)] The composition of the amorphous polyester resin (B) in the present invention is not particularly limited as long as it is an amorphous polyester which is a polycondensation product of an alcohol component (X) and a carboxylic acid component (Y). In the present invention, the term "amorphous" means that when the transition temperature of a sample is measured using a differential scanning calorimeter, there is no peak top temperature of the endothermic peak.

[0042] The alcohol component (X) of the amorphous polyester resin (B) includes a diol (g) and a trihydric or higher polyol (h). Examples of the carboxylic acid component (Y) include dicarboxylic acids (i), tri- or higher carboxylic acids (j), and acid anhydrides or lower alkyl esters thereof.

[0043] Examples of the diol (g) include alkylene glycols having 2 to 36 carbon atoms, alkylene ether glycols having 4 to 36 carbon atoms, alicyclic diols having 4 to 36 carbon atoms, alkylene oxide adducts of alkylene glycols or alicyclic diols, alkylene oxide adducts of bisphenols, polylactone diols, and polybutadiene diols. Specific examples of alkylene glycols having 2 to 36 carbon atoms include ethylene glycol, 1,2-propanediol (propylene glycol), 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, octanediol, decanediol, dodecanediol, tetradecanediol, neopentyl glycol, and 2,2-diethyl-1,3-propanediol. Specific examples of alkylene ether glycols having 4 to 36 carbon atoms include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol. Specific examples of the alicyclic diol having 4 to 36 carbon atoms include 1,4-cyclohexanedimethanol and hydrogenated bisphenol A. In the alkylene oxide adduct of an alkylene glycol or an alicyclic diol, examples of the alkylene glycol or alicyclic diol include those mentioned above, and examples of the alkylene oxide include an ethylene oxide (hereinafter abbreviated as EO) adduct, a propylene oxide (hereinafter abbreviated as PO) adduct, and a butylene oxide (hereinafter abbreviated as BO) adduct, etc. Examples of the alkylene oxide adducts of bisphenol include AO (EO, PO, BO, etc.) adducts (molar number of addition: 2 to 30) of bisphenol A, bisphenol F, bisphenol S, etc. An example of the polylactone diol is poly-ε-caprolactone diol.

[0044] Examples of the trihydric or higher polyol (h) include trihydric or higher polyhydric aliphatic alcohols having 3 to 36 carbon atoms, AO adducts of polyhydric aliphatic alcohols (number of moles added: 2 to 120), AO adducts of trisphenols (trisphenol PA, etc.) (number of moles added: 2 to 30), AO adducts of novolak resins (phenol novolak, cresol novolak, etc.) (number of moles added: 2 to 30), and acrylic polyols [copolymers of hydroxyethyl (meth)acrylate and other vinyl monomers, etc.]. Examples of the polyhydric aliphatic alcohol having 3 to 36 carbon atoms and at least three valences include alkane polyols and their intramolecular or intermolecular dehydration products, as well as sugars (such as sucrose) and compounds in which part of the alcohol of the sugars is alkyl etherified. Specific examples of alkane polyols and their intramolecular or intermolecular dehydration products include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, sorbitan, and polyglycerin.

[0045] Of the above alcohol components (X), from the viewpoints of low-temperature fixability and heat-resistant storage stability, alkylene glycols having 2 to 36 carbon atoms and alkylene oxide adducts of bisphenol are preferred, and AO adducts of bisphenol A are more preferred.

[0046] Examples of the dicarboxylic acid (i) include alkane dicarboxylic acids having 4 to 36 carbon atoms, alkenyl succinic acids, alicyclic dicarboxylic acids having 6 to 40 carbon atoms, alkene dicarboxylic acids having 4 to 36 carbon atoms, and aromatic dicarboxylic acids having 8 to 36 carbon atoms. Examples of the alkanedicarboxylic acid having 4 to 36 carbon atoms include succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedicarboxylic acid, octadecanedicarboxylic acid, and decylsuccinic acid. Examples of the alkenylsuccinic acid include dodecenylsuccinic acid, pentadecenylsuccinic acid, and octadecenylsuccinic acid. Examples of the alicyclic dicarboxylic acid having 6 to 40 carbon atoms include dimer acid (dimerized linoleic acid). Examples of the alkene dicarboxylic acid having 4 to 36 carbon atoms include maleic acid, fumaric acid, and citraconic acid. Examples of the aromatic dicarboxylic acid having 8 to 36 carbon atoms include phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid.

[0047] Examples of the trivalent or higher polycarboxylic acid (j) include aromatic polycarboxylic acids having 9 to 20 carbon atoms (such as trimellitic acid and pyromellitic acid) and aliphatic (including alicyclic) tricarboxylic acids having 6 to 36 carbon atoms (such as hexanetricarboxylic acid and decanetricarboxylic acid).

[0048] As the dicarboxylic acid (i) or the tri- or higher carboxylic acid (j), acid anhydrides or lower alkyl esters having 1 to 4 carbon atoms (methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned compounds may be used.

[0049] Of the carboxylic acid components (Y), from the viewpoints of low-temperature fixability and heat-resistant storage stability, preferred are alkanedicarboxylic acids having 4 to 36 carbon atoms, aromatic dicarboxylic acids having 8 to 36 carbon atoms, and aromatic polycarboxylic acids having 9 to 20 carbon atoms, and more preferred are alkanedicarboxylic acids having 4 to 20 carbon atoms, aromatic dicarboxylic acids having 8 to 20 carbon atoms, and trimellitic acid.

[0050] The reaction ratio of the alcohol component (X) and the carboxylic acid component (Y) is preferably 1 / 2 to 2 / 1, more preferably 1 / 1.3 to 1.5 / 1, and even more preferably 1 / 1.2 to 1.4 / 1, in terms of the molar ratio of hydroxyl groups to carboxyl groups {[OH] / [COOH]}. The hydroxyl groups are those derived from the alcohol component.

[0051] In the present invention, the amorphous polyester resin (B) can be produced in the same manner as the above-mentioned crystalline polyester (a) by a known polyester production method.

[0052] The glass transition temperature (Tg) of the amorphous polyester resin (B) is preferably 20 to 90° C., and more preferably 40 to 80° C. If it is 20° C. or higher, the heat resistance storage property is excellent, and if it is 90° C. or lower, the inhibition of low-temperature fixability is small.

[0053] The acid value of the amorphous polyester resin (B) is preferably from 0 to 75 mgKOH / g, and more preferably from 7 to 24 mgKOH / g.

[0054] The hydroxyl value of the amorphous polyester resin (B) is preferably from 0 to 120 mgKOH / g, and more preferably from 1 to 70 mgKOH / g.

[0055] The weight average molecular weight (hereinafter sometimes abbreviated as Mw) of the amorphous polyester resin (B) is preferably from 2,000 to 200,000, and more preferably from 4,000 to 150,000.

[0056] The 1 / 2 drop temperature of the amorphous polyester resin (B) is preferably 80 to 170°C, more preferably 97 to 150°C, from the viewpoints of heat-resistant storage stability and low-temperature fixability.

[0057] [Mixing method] In step 2, the equipment used to mix the crystalline polyester resin (A) and the amorphous polyester resin (B) may be a general equipment capable of mixing resins while controlling the temperature, such as a twin-screw kneader. The temperature when mixing the crystalline polyester resin (A) and the amorphous polyester resin (B) is preferably from 80°C to 180°C, more preferably from 100°C to 160°C. The mixing time (resin residence time) is preferably 30 seconds or more, more preferably 60 seconds or more, and is preferably 600 seconds or less, more preferably 300 seconds or less.

[0058] The mixing ratio of the crystalline polyester resin (A) to 100 parts by weight of the amorphous polyester resin (B) is not particularly limited, but is preferably 1 part by weight or more, more preferably 5 parts by weight or more, and is preferably 30 parts by weight or less, more preferably 20 parts by weight or less. By making the mixing ratio equal to or more than the lower limit, the low temperature fixability can be improved, and by making the mixing ratio equal to or less than the upper limit, the dispersibility can be improved.

[0059] Two or more kinds of amorphous polyester resins (B) may be used in step 2. When two or more kinds of (B) are used, two or more kinds having different 1 / 2 drop temperatures may be used in combination, and a combination of one having a 1 / 2 drop temperature of 80° C. or more and less than 110° C. and one having a 1 / 2 drop temperature of 110° C. or more and 170° C. or less is preferred from the viewpoint of low-temperature fixability, and a combination of one having a 1 / 2 drop temperature of 85° C. to 105° C. and one having a 1 / 2 drop temperature of 115° C. to 160° C. is more preferred.

[0060] [Resin particles] The toner binder obtained by the production method of the present invention may be used to obtain resin particles for toner. The content of the toner binder in the resin particles is preferably 30 to 97% by weight, more preferably 42 to 96% by weight, and further preferably 50 to 95% by weight, based on the weight of the resin particles.

[0061] The resin particles may be mixed with various known additives such as a colorant, a release agent, a charge control agent, a fluidizing agent, etc., if necessary.

[0062] The colorant preferably contains at least one selected from the group consisting of black colorants, blue colorants, red colorants and yellow colorants. As the colorant, any dye, pigment, etc. used as a toner colorant can be used. Specific examples of the pigment include carbon black, iron black, Sudan Black SM, Fast Yellow G, Benzidine Yellow, Solvent Yellow (21, 77, 114, etc.), Pigment Yellow (12, 14, 17, 83, etc.), India Fast Orange, Irgasin Red, Paranitoaniline Red, Toluidine Red, Solvent Red (17, 49, 128, 5, 13, 22, 48·2, etc.), Disperse Red, Carmine FB, Pigment Orange R, Lake Red 2G, Rhodamine FB, Rhodamine B Lake, Methyl Violet B Lake, Phthalocyanine Blue, Solvent Blue (25, 94, 60, 15·3, etc.), Pigment Blue, Brilliant Green, Phthalocyanine Green, Oil Yellow GG, Kayaset YG, Orasol Brown B, and Oil Pink OP. If necessary, magnetic powder (powders of ferromagnetic metals such as iron, cobalt and nickel, and compounds such as magnetite, hematite and ferrite) may be contained to function as a colorant. The content of the colorant is preferably 1 to 40 parts by weight, more preferably 2 to 15 parts by weight, based on 100 parts by weight of the total of the binder resin for the toner of the present invention. When a magnetic powder is used, the content of the magnetic powder is preferably 20 to 150 parts by weight, more preferably 30 to 120 parts by weight, based on 100 parts by weight of the total of the binder resin for the toner.

[0063] Examples of the release agent include natural waxes (beeswax, carnauba wax, montan wax, etc.), petroleum waxes (paraffin wax, microcrystalline wax, petrolatum, etc.), synthetic waxes (Fischer-Tropsch wax, polyethylene wax, polypropylene wax, oxidized polyethylene wax, oxidized polypropylene wax, etc.), and synthetic ester waxes (fatty acid esters synthesized from fatty acids having 10 to 30 carbon atoms and alcohols having 10 to 30 carbon atoms, etc.), and it is preferable to contain one or more types selected from the group consisting of these release agents. The content of the release agent is preferably 0 to 30% by weight, more preferably 0.5 to 20% by weight, and even more preferably 1 to 10% by weight, based on 100 parts by weight of the total of the binder resin for toner of the present invention.

[0064] When using the above-mentioned release agent, modified wax may be used in combination, if necessary. The modified wax is a release agent to which a vinyl polymer chain is grafted. The release agent used in the modified wax may be the same as the above-mentioned release agent, and the preferred ones are also the same. Examples of the vinyl monomer constituting the vinyl polymer chain of the modified wax include styrene and methacrylic acid ester. The vinyl polymer chain may be a homopolymer or copolymer of a vinyl monomer. The content of the modified wax is preferably 0 to 15% by weight, more preferably 0.5 to 10% by weight, and even more preferably 1 to 5% by weight, based on 100 parts by weight of the total of the binder resin for the toner of the present invention.

[0065] The charge control agent may be either a positively charged charge control agent or a negatively charged charge control agent. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes having a tertiary amine as a side chain, quaternary ammonium salts, polyamine resins, imidazole derivatives, and quaternary ammonium salts. Examples of the charge control agent include um base-containing polymers, metal-containing azo dyes, copper phthalocyanine dyes, metal salicylic acid salts, boron complexes of benzilic acid, sulfonic acid group-containing polymers, fluorine-containing polymers, halogen-substituted aromatic ring-containing polymers, etc. The content of the charge control agent may be 0 to 20% by weight, preferably 0.1 to 10% by weight, and more preferably 0.5 to 7.5% by weight, based on 100 parts by weight of the total of the binder resin for the toner of the present invention.

[0066] Examples of the fluidizing agent include silica, titania, alumina, fatty acid metal salt, silicone resin particles, and fluororesin particles, and two or more of them may be used in combination. From the viewpoint of the chargeability of the toner, silica is preferred. From the viewpoint of the transferability of the toner, the silica is preferably hydrophobic. The content of the fluidizing agent may be 0 to 10% by weight, preferably 0 to 5% by weight, and more preferably 0.1 to 4% by weight, based on 100 parts by weight of the total of the binder resin for the toner of the present invention.

[0067] The total weight of additives such as colorants, release agents, charge control agents, and fluidizing agents may be 3 to 70% by weight, preferably 4 to 58% by weight, and more preferably 5 to 50% by weight, based on the weight of the resin particles.

[0068] The volume average particle diameter (D50) of the resin particles is preferably from 1 to 15 μm, more preferably from 2 to 10 μm, and particularly preferably from 3 to 7 μm. By keeping it within the above range, low-temperature fixability is improved.

[0069] The method for producing the resin particles is not particularly limited, and may be a known kneading and grinding method, a suspension polymerization method described in JP-B-10231 / 1961, JP-A-53856 / 1984, and JP-A-61842 / 1984, an emulsion polymerization method represented by a soap-free polymerization method in which a toner is produced by directly polymerizing a monomer in the presence of a water-soluble polymerization initiator that is soluble in the monomer, an interfacial polymerization method such as a microcapsule production method, an in situ polymerization method, a coacervation method in which at least one type of fine particles are aggregated to obtain particles of a desired particle size as disclosed in JP-A-106473 / 1987 and JP-A-186253 / 1988, a dispersion polymerization method characterized by monodispersion, a dissolution suspension method in which a required resin is dissolved in a water-insoluble organic solvent and then resin particles are formed in water, or an ester elongation polymerization method, or a method in which the resin particles are dispersed in carbon dioxide in a supercritical state.

[0070] When resin particles are used as a toner, they are mixed with carrier particles such as iron powder, glass beads, nickel powder, ferrite, magnetite, and ferrite coated with resin (acrylic resin, silicone resin, etc.) as necessary, and used as a developer for an electric latent image. When carrier particles are used, the weight ratio of the toner to the carrier particles is preferably 1 / 99 to 99 / 1. Also, instead of the carrier particles, the toner can be rubbed against a member such as a charging blade to form an electric latent image. The toner does not necessarily need to contain carrier particles.

[0071] The toner is fixed to a support (paper, polyester film, etc.) to form a recording material by a copier, printer, etc. As a method for fixing to a support, a known heat roll fixing method, flash fixing method, etc. can be used.

[0072] The toner is used for developing electrostatic images or magnetic latent images in electrophotography, electrostatic recording, electrostatic printing, etc. More specifically, it is used for developing electrostatic images or magnetic latent images that are particularly suitable for full color use. EXAMPLES

[0073] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited thereto. In the following, "parts" refers to parts by weight unless otherwise specified.

[0074] The physical properties of the crystalline polyester resin, the amorphous polyester resin, the toner, etc. were measured by the following methods.

[0075] <Method for measuring the peak top temperature of the endothermic peak of the crystalline polyester resin (A)> The measurement was performed using a differential scanning calorimeter {"DSCQ20" [manufactured by TA Instruments, Inc.]}. The crystalline polyester resin (A) was heated for the first time from 30°C to 180°C at 10°C / min, then cooled from 180°C to 0°C at 10°C / min, and then heated for the second time from 0°C to 180°C at 10°C / min. The temperature showing the top of the endothermic peak during the second heating process was determined as the peak top temperature of the endothermic peak of the crystalline polyester resin (A).

[0076] <Amount of heat absorbed at the endothermic peak of crystalline polyester resin (A)> In the DSC curve during the second heating process observed under the same measurement conditions as in the measurement of the peak top temperature of the endothermic peak, a straight line was drawn connecting the point closest to the peak on the baseline below the endothermic peak endothermic onset temperature (T0) and the point closest to the peak on the baseline above the endothermic peak end point temperature, thereby calculating the amount of endotherm in the endothermic peak having the peak top temperature of the endothermic peak.

[0077] <Weight average molecular weight (Mw)> The weight average molecular weight (Mw) was measured under the following conditions using a sample solution obtained by dissolving the polyester resin in tetrahydrofuran (THF) and filtering off the insoluble matter with a glass filter. Equipment: Tosoh Corporation HLC-8120 Column: TSK GEL GMH6 x 2 (Tosoh Corporation) Measurement temperature: 40℃ Sample solution: 0.25% by weight in THF Solution injection volume: 100μl Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) manufactured by Tosoh Corporation (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000)

[0078] <Acid value and hydroxyl value> The measurement was performed according to the method specified in JIS K0070, except that the measurement solvent for the acid value was a mixed solvent of acetone, methanol, and toluene (weight ratio of acetone:methanol:toluene=12.5:12.5:75), and the measurement solvent for the hydroxyl value was toluene.

[0079] <1 / 2 temperature drop> Using a constant test force extrusion-type capillary rheometer flow tester {Shimadzu Corporation, CFT-500D}, 1 g of the measurement sample was heated at a heating rate of 6°C / min while applying a load of 1.96 MPa with the plunger and extruding it from a nozzle of 1 mm diameter and 1 mm length. A graph was drawn of "plunger drop amount (flow value)" vs. "temperature," and the temperature corresponding to 1 / 2 of the maximum plunger drop amount was read from the graph. This value (the temperature when half of the measurement sample had flowed out) was determined as the 1 / 2 drop temperature.

[0080] <Method of measuring glass transition temperature (Tg)> The measurement was performed using a differential scanning calorimeter (DSC Q20, manufactured by TA Instruments) according to the method (DSC method) specified in ASTM D3418-82 under the following conditions. (1) Heat from 30°C to 150°C at 20°C / min (2) Hold at 150°C for 10 minutes (3) Cool to -35°C at 20°C / min (4) Keep at -35℃ for 10 minutes (5) Heat up to 150°C at 20°C / min. (6) The differential scanning calorimetric curve measured in the process of (5) was analyzed to determine the glass transition temperature.

[0081] <Toner volume average particle size (D50) (μm), number average particle size (μm), particle size distribution (volume average particle size / number average particle size)> Measurements were performed using a Coulter counter [product name: Multisizer III (manufactured by Beckman Coulter, Inc.)]. First, 0.1 to 5 mL of a surfactant (alkylbenzene sulfonate) was added as a dispersant to 100 to 150 mL of an electrolyte solution, ISOTON-II (manufactured by Beckman Coulter). 2 to 20 mg of a measurement sample was then added, and the electrolyte solution in which the sample was suspended was dispersed for approximately 1 to 3 minutes using an ultrasonic disperser. The toner volume and number were measured using a 50 μm aperture with the above-mentioned measuring device, and the volume distribution and number distribution were calculated. From the distribution obtained, the volume average particle diameter (D50) (μm), number average particle diameter (μm), and particle size distribution (volume average particle diameter / number average particle diameter) of the toner were obtained.

[0082] <Production Example 1> [Synthesis of Crystalline Polyester Resin (A-1)] <Synthesis of crystalline polyester (a1)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 235 parts (50.3 mol%) of 1,12-dodecanediol, 265 parts (49.7 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a1). The crystalline polyester (a1) had an endothermic peak top temperature (Tm) of 84.4° C., an endothermic amount at the endothermic peak of 116.4 J / g, a weight average molecular weight (Mw) of 39,000, an acid value of 1 mg KOH / g, and a hydroxyl value of 6 mg KOH / g.

[0083] <Synthesis of crystalline polyester (a2)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 170 parts (50.2 mol%) of 1,6-hexanediol, 330 parts (49.8 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a2). The crystalline polyester (a2) had an endothermic peak top temperature (Tm) of 73.8° C., an endothermic amount at the endothermic peak of 98.8 J / g, a weight average molecular weight (Mw) of 38,000, an acid value of 1 mgKOH / g, and a hydroxyl value of 6 mgKOH / g.

[0084] <Synthesis of crystalline polyester resin (A-1)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 500 parts of crystalline polyester (a1), 500 parts of crystalline polyester (a2) and 1.5 parts of titanium dihydroxybis(triethanolamine) as an ester exchange reaction catalyst were placed, and dehydration was performed under reduced pressure of 0.5 to 2.5 kPa at 150°C. Then, the ester exchange reaction was performed for 20 hours at 150°C under a nitrogen stream. The extracted resin was cooled to room temperature, and then crushed into particles to obtain a crystalline polyester resin (A-1). The peak top temperature (Tm) of the endothermic peak of the crystalline polyester resin (A-1) was 79.9°C, the endothermic amount at the endothermic peak was 105.9 J / g, the weight average molecular weight (Mw) was 38,000, the acid value was 1 mgKOH / g, and the hydroxyl value was 6 mgKOH / g.

[0085] <Production Example 2> [Synthesis of Crystalline Polyester Resin (A-2)] <Synthesis of crystalline polyester (a1)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 209 parts (50.8 mol%) of 1,9-nonanediol, 291 parts (49.2 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a1). The crystalline polyester (a1) had an endothermic peak top temperature (Tm) of 74.9° C., an endothermic amount at the endothermic peak of 106.0 J / g, a weight average molecular weight (Mw) of 20,000, an acid value of 1 mgKOH / g, and a hydroxyl value of 13 mgKOH / g.

[0086] <Synthesis of crystalline polyester (a2)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 170 parts (50.2 mol%) of 1,6-hexanediol, 330 parts (49.8 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a2). The crystalline polyester (a2) had an endothermic peak top temperature (Tm) of 73.8° C., an endothermic amount at the endothermic peak of 98.8 J / g, a weight average molecular weight (Mw) of 38,000, an acid value of 1 mgKOH / g, and a hydroxyl value of 6 mgKOH / g.

[0087] <Synthesis of crystalline polyester resin (A-2)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 500 parts of crystalline polyester (a1), 500 parts of crystalline polyester (a2) and 1.5 parts of titanium dihydroxybis(triethanolamine) as an ester exchange reaction catalyst were placed, and dehydration was performed under reduced pressure of 0.5 to 2.5 kPa at 150°C. Then, the ester exchange reaction was performed for 20 hours under a nitrogen stream at 150°C. The extracted resin was cooled to room temperature, then crushed and granulated to obtain a crystalline polyester resin (A-2). The peak top temperature (Tm) of the endothermic peak, the endothermic amount at the endothermic peak, the weight average molecular weight (Mw), the acid value and the hydroxyl value of the obtained crystalline polyester resin are shown in Table 1.

[0088] <Production Example 3> [Synthesis of Crystalline Polyester Resin (A-3)] <Synthesis of crystalline polyester (a1)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 235 parts (50.3 mol%) of 1,12-dodecanediol, 265 parts (49.7 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a1). The crystalline polyester (a1) had an endothermic peak top temperature (Tm) of 84.4° C., an endothermic amount at the endothermic peak of 116.4 J / g, a weight average molecular weight (Mw) of 39,000, an acid value of 1 mg KOH / g, and a hydroxyl value of 6 mg KOH / g.

[0089] <Synthesis of crystalline polyester (a2)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 185 parts (50.1 mol%) of 1,6-hexanediol, 315 parts (49.9 mol%) of sebacic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. Next, the temperature was gradually raised to 210°C, and the reaction was carried out for 4 hours under a nitrogen stream while distilling off the water produced, and the reaction was further carried out under a reduced pressure of 0.5 to 2.5 kPa, and the resin was taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a2). The crystalline polyester (a2) had an endothermic peak top temperature (Tm) of 68.7° C., an endothermic amount at the endothermic peak of 95.2 J / g, a weight average molecular weight (Mw) of 38,000, an acid value of 1 mgKOH / g, and a hydroxyl value of 6 mgKOH / g.

[0090] <Synthesis of crystalline polyester resin (A-3)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 500 parts of crystalline polyester (a1), 500 parts of crystalline polyester (a2) and 1.5 parts of titanium dihydroxybis(triethanolamine) as an ester exchange reaction catalyst were placed, and dehydration was performed under reduced pressure of 0.5 to 2.5 kPa at 150°C. Then, the ester exchange reaction was performed for 40 hours under a nitrogen stream at 150°C. The extracted resin was cooled to room temperature, then crushed and granulated to obtain a crystalline polyester resin (A-3). The peak top temperature (Tm) of the endothermic peak, the endothermic amount at the endothermic peak, the weight average molecular weight (Mw), the acid value and the hydroxyl value of the obtained crystalline polyester resin are shown in Table 1.

[0091] <Production Example 4> [Synthesis of Crystalline Polyester Resin (A-4)] <Synthesis of crystalline polyester (a1)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 141 parts (50.3 mol%) of 1,12-dodecanediol, 159 parts (49.7 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a1). The crystalline polyester (a1) had an endothermic peak top temperature (Tm) of 84.4° C., an endothermic amount at the endothermic peak of 116.4 J / g, a weight average molecular weight (Mw) of 39,000, an acid value of 1 mg KOH / g, and a hydroxyl value of 6 mg KOH / g.

[0092] <Synthesis of crystalline polyester (a2)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 238 parts (50.2 mol%) of 1,6-hexanediol, 462 parts (49.8 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a2). The crystalline polyester (a2) had an endothermic peak top temperature (Tm) of 73.8° C., an endothermic amount at the endothermic peak of 98.8 J / g, a weight average molecular weight (Mw) of 38,000, an acid value of 1 mgKOH / g, and a hydroxyl value of 6 mgKOH / g.

[0093] <Synthesis of crystalline polyester resin (A-4)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 300 parts of crystalline polyester (a1), 700 parts of crystalline polyester (a2) and 1.5 parts of titanium dihydroxybis(triethanolamine) as an ester exchange reaction catalyst were placed, and dehydration was carried out under reduced pressure of 0.5 to 2.5 kPa at 150°C. Then, the ester exchange reaction was carried out for 20 hours under a nitrogen stream at 150°C. The extracted resin was cooled to room temperature, then crushed and granulated to obtain a crystalline polyester resin (A-4). The peak top temperature (Tm) of the endothermic peak, the endothermic amount at the endothermic peak, the weight average molecular weight (Mw), the acid value and the hydroxyl value of the obtained crystalline polyester resin are shown in Table 1.

[0094] <Comparative Production Example 1> [Synthesis of Crystalline Polyester Resin (AR-1)] In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 471 parts (50.3 mol%) of 1,12-dodecanediol, 529 parts (49.7 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The temperature was then gradually raised to 210°C, and the reaction was continued for 4 hours under a nitrogen stream while distilling off the water produced, and the reaction was continued under a reduced pressure of 0.5 to 2.5 kPa, and the resin was taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester diol (AR-1). The peak top temperature (Tm) of the endothermic peak of the crystalline polyester diol (AR-1) was 84.4°C, the endothermic amount at the endothermic peak was 116.4 J / g, the weight average molecular weight (Mw) was 39,000, the acid value was 1 mg KOH / g, and the hydroxyl value was 6 mg KOH / g.

[0095] <Comparative Production Examples 2 and 3> [Synthesis of Crystalline Polyester Resins (AR-2 and AR-3)] Crystalline polyester resins (AR-2) and (AR-3) were obtained in the same manner as in Comparative Production Example 1, except that the raw materials shown in Comparative Production Examples 2 and 3 in Table 1 were used. The peak top temperature (Tm) of the endothermic peak, the endothermic amount at the endothermic peak, the weight average molecular weight (Mw), the acid value, and the hydroxyl value of the obtained crystalline polyester resins are shown in Table 1.

[0096] Comparative Production Example 4 [Synthesis of Crystalline Polyester Resin (AR-4)] <Synthesis of crystalline polyester (a1)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 235 parts (50.3 mol%) of 1,12-dodecanediol, 265 parts (49.7 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a1). The crystalline polyester (a1) had an endothermic peak top temperature (Tm) of 84.4° C., an endothermic amount at the endothermic peak of 116.4 J / g, a weight average molecular weight (Mw) of 39,000, an acid value of 1 mg KOH / g, and a hydroxyl value of 6 mg KOH / g.

[0097] <Synthesis of crystalline polyester (a2)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 170 parts (50.2 mol%) of 1,6-hexanediol, 330 parts (49.8 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a2). The crystalline polyester (a2) had an endothermic peak top temperature (Tm) of 73.8° C., an endothermic amount at the endothermic peak of 98.8 J / g, a weight average molecular weight (Mw) of 38,000, an acid value of 1 mgKOH / g, and a hydroxyl value of 6 mgKOH / g.

[0098] <Synthesis of crystalline polyester resin (AR-4)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 500 parts of crystalline polyester (a1) and 500 parts of crystalline polyester (a2) were dissolved in 1000 parts of tetrahydrofuran. The solvent was then removed, and the extracted resin was cooled to room temperature, then crushed into particles to obtain a crystalline polyester resin (AR-4). The peak top temperature (Tm) of the endothermic peak, the endothermic amount at the endothermic peak, the weight average molecular weight (Mw), the acid value and the hydroxyl value of the obtained crystalline polyester resin are shown in Table 1.

[0099] Comparative Production Example 5 [Synthesis of Crystalline Polyester Resin (AR-5)] <Synthesis of crystalline polyester (a1)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 236 parts (50.3 mol%) of 1,12-dodecanediol, 264 parts (49.7 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a1). The crystalline polyester (a1) had an endothermic peak top temperature (Tm) of 84.4° C., an endothermic amount at the endothermic peak of 116.4 J / g, a weight average molecular weight (Mw) of 39,000, an acid value of 1 mg KOH / g, and a hydroxyl value of 6 mg KOH / g.

[0100] <Synthesis of crystalline polyester (a2)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 217 parts (50.3 mol%) of 1,10-decanediol, 283 parts (49.7 mol%) of dodecanedioic acid, and 1.5 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted for 8 hours under a nitrogen stream at 160°C while distilling off the water produced. The mixture was then gradually heated to 210°C, and reacted for 4 hours under a nitrogen stream while distilling off the water produced, and further reacted under a reduced pressure of 0.5 to 2.5 kPa, and taken out when the acid value reached 1 mgKOH / g. The resin taken out was cooled to room temperature, pulverized and granulated to obtain a crystalline polyester (a2). The peak top temperature (Tm) of the endothermic peak of the crystalline polyester (a2) was 80.7° C., the endothermic amount at the endothermic peak was 103.5 J / g, the weight average molecular weight (Mw) was 38,000, the acid value was 1 mgKOH / g, and the hydroxyl value was 6 mgKOH / g.

[0101] <Synthesis of crystalline polyester resin (AR-5)> In a reaction vessel equipped with a cooling tube, a heating / cooling device, a thermometer, a stirrer and a nitrogen inlet tube, 500 parts of crystalline polyester (a1), 500 parts of crystalline polyester (a2) and 1.5 parts of titanium dihydroxybis(triethanolamine) as an ester exchange reaction catalyst were placed, and dehydration was performed under reduced pressure of 0.5 to 2.5 kPa at 150°C. Then, the ester exchange reaction was performed for 20 hours under a nitrogen stream at 150°C. The extracted resin was cooled to room temperature, then crushed and granulated to obtain a crystalline polyester resin (A-5). The peak top temperature (Tm) of the endothermic peak, the endothermic amount at the endothermic peak, the weight average molecular weight (Mw), the acid value and the hydroxyl value of the obtained crystalline polyester resin are shown in Table 1.

[0102] The compositions and physical properties of the crystalline polyester resins (A) obtained in Production Examples 1 to 4 and the polyester resins (AR) obtained in Comparative Production Examples 1 to 5 are shown in Table 1.

[0103] [Table 1]

[0104] <Production Example 5> [Synthesis of amorphous polyester resin (B-1)] In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 193 parts (14.6 mol%) of bisphenol A·PO 2-mol adduct (manufactured by Sanyo Chemical Industries, Ltd., "Hymer BP-2P"), 539 parts (35.4 mol%) of bisphenol A·PO 3-mol adduct (manufactured by Sanyo Chemical Industries, Ltd., "Hymer BP-3P"), 173 parts (26.7 mol%) of terephthalic acid, 67 parts (11.8 mol%) of adipic acid, 86 parts (11.5 mol%) of trimellitic anhydride, and 3.6 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed and reacted at 220°C for 20 hours while distilling off the water produced. The reaction was further carried out under a reduced pressure of 0.5 to 2.5 kPa, and when the half drop in temperature reached 150°C, the resin was taken out using a steel belt cooler. The resin taken out was pulverized and granulated to obtain amorphous polyester resin (B-1). The amorphous polyester resin (B-1) had a 1 / 2 drop temperature of 150° C., a glass transition temperature Tg of 60° C., an acid value of 23 mgKOH / g, a hydroxyl value of 1 mgKOH / g, and a weight average molecular weight Mw of 130,000.

[0105] <Production Example 6> [Synthesis of amorphous polyester resin (B-2)] In another reaction vessel equipped with a cooling tube, a stirrer and a nitrogen inlet tube, 324 parts (20.0 mol%) of bisphenol A·PO 2-mol adduct (manufactured by Sanyo Chemical Industries, Ltd., "Hymer BP-2P"), 443 parts (30.0 mol%) of bisphenol A·EO 2-mol adduct (manufactured by Sanyo Chemical Industries, Ltd., "Hymer BPE-20"), 280 parts (47.7 mol%) of terephthalic acid, and 3.0 parts of titanium dihydroxybis(triethanolamine) as a condensation catalyst were placed, and the mixture was reacted while distilling off the water produced while heating to 230°C under a reduced pressure of 0.5 to 2.5 kPa until the acid value was less than 2 mgKOH / g. The mixture was then cooled to 180°C, and 14 parts (2.3 mol%) of trimellitic anhydride was added, reacted under normal pressure for 1 hour and taken out. The resin taken out was cooled to room temperature, pulverized and granulated to obtain amorphous polyester resin (B-2). The amorphous polyester resin (B-2) had a 1 / 2 drop temperature of 97°C, a glass transition temperature (Tg) of 58°C, an acid value of 8 mgKOH / g, a hydroxyl value of 55 mgKOH / g, and a weight average molecular weight (Mw) of 5,000.

[0106] The compositions and physical properties of the amorphous polyester resins (B) obtained in Production Examples 5 and 6 are shown in Table 2.

[0107] [Table 2]

[0108] <Examples 1 to 4 and Comparative Examples 1 to 5> <Evaluation of Dispersibility of Crystalline Polyester Resin (A) in Amorphous Polyester Resin (B)> (1) Toner binder manufacturing 10 parts of each of the crystalline polyester resins (A-1) to (A-4) and (AR-1) to (AR-5) were premixed with 27 parts of the amorphous polyester resin (B-1) and 63 parts of the amorphous polyester resin (B-2) using a Henschel mixer [FM10B, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.], and then melt-mixed in a twin-screw kneader [IMC-9B20, manufactured by Imoto Machinery Co., Ltd.] at the temperature and residence time shown in Table 3 to obtain a toner binder. (2) Creation and evaluation of evaluation samples The obtained toner binder was embedded in a visible light curable embedding resin (D-800, manufactured by Nissin EM Co., Ltd.), cut to a thickness of 60 nm using an ultrasonic ultramicrotome (EM5, manufactured by Leica), and stained with ruthenium using a vacuum staining device (manufactured by Filgen Co., Ltd.). Then, using a transmission electron microscope (H7500, manufactured by Hitachi High-Technologies Corporation), the dispersion state of the crystalline polyester in the amorphous polyester was observed from the cross section of the obtained mixture at an acceleration voltage of 120 kV. The long diameter of the crystalline polyester with the largest long diameter in the entire observed image was taken as the maximum particle size. In addition, image processing was performed on randomly selected enlarged images (×1000) using the free software “image J” according to the following procedure, and the calculated “mean feret” was taken as the average particle size of the crystalline polyester. In addition, in the toner binder of Comparative Example 2, the dispersion of the crystalline polyester resin could not be confirmed. 1. image type → 8bit 2.line → analyze → set scale → known distance 5.0 3.process → binary → median filter 10 4.image → adjust → threshold 5.process → binary → fill holl 6.Analyze particles (set mesearements → feret diameter)

[0109] <Evaluation of low-temperature fixing property, charge property, storage stability and fixing strength of toner> (3) Toner manufacturing 10 parts of each of the crystalline polyester resins (A-1) to (A-4), (AR-1) to (AR-5), 27 parts of the amorphous polyester resin (B-1) and 63 parts of the amorphous polyester resin (B-2), 8 parts of the pigment carbon black "MA-100" [manufactured by Mitsubishi Chemical Corporation] as a colorant, 4 parts of the paraffin wax "HNP-9" [manufactured by Nippon Seiro Co., Ltd.] as a release agent, and 1 part by weight of the charge control agent "T-77" [manufactured by Hodogaya Chemical Co., Ltd.] were added, and the mixture was premixed using a Henschel mixer [manufactured by Mitsui Miike Chemical Engineering Co., Ltd., FM10B], and then kneaded in a twin-screw kneader [manufactured by Imoto Manufacturing Co., Ltd., IMC-9B20] at the temperature and residence time listed in Table 3. The resin particles were then finely pulverized using a supersonic jet mill, Labojet (manufactured by Nippon Pneumatic Mfg. Co., Ltd.), and classified using an air classifier (MDS-I, manufactured by Nippon Pneumatic Mfg. Co., Ltd.) to obtain resin particles with a volume average particle size of 5 μm and a particle size distribution of 1.2. The obtained resin particles (99 parts) were mixed with 1 part of a hydrophobic silica fluidizing agent, Aerosil R972 (manufactured by Nippon Aerosil), in a sample mill to obtain a toner.

[0110] (4) Toner evaluation <Low temperature fixability> (MFT) Toner is applied on the paper at 0.6mg / cm 2 The powder was evenly applied so that the density was 10 kg / cm. The powder was applied to the paper surface using a printer without a heat fixing unit. Other methods may be used as long as the powder can be evenly applied at the above weight density. The paper was then placed on the pressure roller at a fixing speed (heat roller peripheral speed) of 213 mm / sec and a fixing pressure (pressure roller pressure) of 10 kg / cm. 2 Under these conditions, the heating roller temperature was changed in the range of 90 to 230°C in 5°C increments to create fixed images at each temperature. Next, the presence or absence of cold offset in each fixed image was visually confirmed in ascending order of heating roller temperature, and the temperature at which cold offset no longer occurred is shown in Table 3 as MFT (°C). The lower the temperature at which cold offset does not occur, the better the low-temperature fixing ability. Under these evaluation conditions, it is generally preferable that the MFT is 125° C. or less.

[0111] <Chargeability> (charge amount) 0.5g of toner and 10g of ferrite carrier (F-150, Powder Tech Co., Ltd.) were placed in a 50ml glass bottle, which was then conditioned for 8 hours at 23°C and 50% relative humidity. The glass bottle containing the conditioned toner was sealed and set in a Turbula shaker mixer and stirred by friction at 90 rpm for 2 minutes. 0.2g of the mixed powder after stirring was loaded into a blow-off powder charge measurement device equipped with a stainless steel mesh with a mesh size of 20μm. The charge of the remaining ferrite carrier was measured under conditions of a blow pressure of 10KPa and a suction pressure of 5KPa, and the charge of the toner (μC / g) was calculated by a standard method. For toner, the higher the negative charge amount, the better the charging characteristics are, and it is preferable that the negative charge amount is -15 μC / g or less. The charge amount was measured using a blow-off charge amount measuring device (manufactured by Toshiba Chemical Co., Ltd.).

[0112] <Heat-resistant storage stability> (degree of agglomeration) 1 g of toner and 0.013 g of Aerosil R8200 (manufactured by Evonik Japan Co., Ltd.) were mixed in a shaker for 1 hour, the mixture was placed in a sealed container, and left to stand for 48 hours in an atmosphere at a temperature of 45°C and a humidity of 80%. The degree of cohesion was then measured using a powder tester, and the heat resistance storage stability was evaluated. The lower the value in the cohesion test determined by the following method, the more excellent the heat-resistant storage stability. Under these evaluation conditions, a value of 3% or less is preferable. Equipment: POWDER TESTER model PT-X (manufactured by Hosokawa Micron) Sieve openings: 355μm, 250μm, 150μm Vibration width: 1mm Vibration duration: 30 seconds Operation method: Set the sieves on the vibration table of the powder tester in the following order: top 355μm, middle 250μm, bottom 150μm. Place 1g of toner on the top sieve and vibrate with a vibration amplitude of 1mm for 30 seconds. Measure the weight of toner remaining on each sieve. Cohesion: Calculated from the weight of toner used for measurement and the weight of toner remaining after sieving. Cohesion degree (%)=(U / N+M / N×3 / 5+L / N×1 / 5)×100 U: weight of top row, M: weight of middle row, L: weight of bottom row, N: weight of sample (1g)

[0113] <Fixing strength> (Tape peeling) The fixing strength of the fixed image in the MFT prepared for the evaluation of low-temperature low-adhesion was evaluated by a tape peeling test. After attaching tape (3M's "Scotch Mending Tape") to the fixed image, the tape was peeled off and the image density (ID) of the image attached to the tape was measured with a reflection densitometer (product name "X-Rite model 404", X-Rite). The smaller the image density (number) of the attached image, the higher the fixing strength. Under these evaluation conditions, it is preferable that it is 0.2 or less.

[0114] <Fixing strength> (pencil hardness) The MFT-fixed image prepared in the above evaluation of low-temperature adhesion was subjected to a scratch hardness test in accordance with JIS K5600-5-4 (1999) by applying a load of 10 g from directly above a pencil fixed at a 45-degree angle by hand scratching, and the image strength was evaluated based on the pencil hardness at which the image was not scratched. The higher the pencil hardness, the better the image strength. Generally, it is preferable that the pencil hardness is HB or higher.

[0115] [Table 3]

[0116] As is clear from the results in Table 3, the toner binders of Examples 1 to 4 have smaller maximum particle diameters of the crystalline polyester in the amorphous polyester, smaller average particle diameters, and better dispersibility than the toner binders of Comparative Examples 1 to 5, and further have higher charge amounts, heat-resistant storage stability, and fixing strength. [Industrial Applicability]

[0117] The toner binder of the present invention can be suitably used as an electrophotographic toner used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing and the like. Further, it is suitable for use as an additive for paints, an additive for adhesives, particles for electronic paper, and the like.

Claims

1. A method for producing a toner binder, comprising the step 1 of obtaining a crystalline polyester resin (A) by transesterification of two kinds of crystalline polyesters (a) having different solubility parameters, wherein the absolute value of the difference in solubility parameter between the crystalline polyester (a1) having the smaller solubility parameter and the crystalline polyester (a2) having the larger solubility parameter of the crystalline polyesters (a) is 0.10 to 0.50 (cal / cm 3 ) 1/2 A method for producing a toner binder comprising the steps of:

2. 2. The method for producing a toner binder according to claim 1, wherein the hydroxyl value of the crystalline polyester (a) is from 1 to 100 mgKOH / g.

3. 3. The method for producing a toner binder according to claim 1, wherein the crystalline polyester (a) is a polycondensate of an alcohol component (x) and a carboxylic acid component (y), the alcohol component (x) being a linear aliphatic diol having 2 to 24 carbon atoms, and the carboxylic acid component (y) being a linear aliphatic dicarboxylic acid having 4 to 36 carbon atoms.

4. 3. The method for producing a toner binder according to claim 1, wherein the crystalline polyester resin (A) has an endothermic peak top temperature (Tm) of 50° C. to 90° C. as measured by a differential scanning calorimeter (DSC), and an endothermic amount based on the endothermic peak of 70 to 110 J / g.

5. 3. The method for producing a toner binder according to claim 1, wherein the weight ratio [(a1):(a2)] of the crystalline polyester (a1) having a smaller solubility parameter to the crystalline polyester (a2) having a larger solubility parameter is 30:70 to 90:

10.

6. 3. The method for producing a toner binder according to claim 1, wherein the peak top temperature (Tm) of an endothermic peak of the crystalline polyester resin (A) measured by a differential scanning calorimeter (DSC) satisfies relational expression (1). Relational formula (1): {(Tma1) x (aw1) / ((aw1) + (aw2)) + (Tma2) x (aw2) / ((aw1) + (aw2))} x 0.97 ≤ (Tm) ≤ {(Tma1) x (aw1) / ((aw1) + (aw2)) + (Tma2) x (aw2) / ((aw1) + (aw2))} x 1.03 [In the relational formula (1), Tma1 is the peak top temperature of the endothermic peak of the crystalline polyester (a1) having the smaller solubility parameter, Tma2 is the peak top temperature of the endothermic peak of the crystalline polyester (a2) having the larger solubility parameter, aw1 is the weight ratio of (a1) based on the total weight of (a1) and (a2), and aw2 is the weight ratio of (a2) based on the total weight of (a1) and (a2)]

7. 3. The method for producing a toner binder according to claim 1, wherein the transesterification reaction in step 1 is carried out in the presence of a titanium-containing catalyst.

8. 3. The method for producing a toner binder according to claim 1, wherein the pressure in the reaction system is reduced during the ester exchange reaction in step 1.

9. 3. The method for producing a toner binder according to claim 1, further comprising a step 2 of melt-mixing a composition containing the crystalline polyester resin (A) and the amorphous polyester resin (B).

Citation Information

Patent Citations

  • Polyester sheet

    JP2002363271A

  • Electrophotographic toner

    JP2015084076A

  • Toner and manufacturing method thereof

    JP2019045662A

  • Toner binder and resin particle

    JP2019061239A

  • Toner for electrostatic charge image development