Method for producing polyvinyl ester-based polymer

By performing RAFT polymerization at lower temperatures with specific agents and conditions, the method achieves high molecular weight polyvinyl ester polymers with narrow molecular weight distribution, addressing the limitations of existing methods and enhancing polymer properties.

JP2024133755AInactive Publication Date: 2024-10-03MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023043707
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing RAFT polymerization methods for producing polyvinyl ester polymers struggle with controlling molecular weight distribution, particularly when aiming for high molecular weight polymers, leading to broader distributions due to side reactions and inefficient use of RAFT agents.

Method used

The method involves conducting RAFT polymerization at lower temperatures (0 to 55°C) using a specific compound as a chain transfer agent and a polymerization initiator, with controlled bulk polymerization to achieve polyvinyl ester polymers with a narrow molecular weight distribution.

Benefits of technology

This approach results in high molecular weight polyvinyl ester polymers with a narrow molecular weight distribution, enabling stable production and improved properties such as enhanced coating stability and optical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133755000001
    Figure 2024133755000001
  • Figure 2024133755000002
    Figure 2024133755000002
  • Figure 2024133755000003
    Figure 2024133755000003
Patent Text Reader

Abstract

To provide a new production method that yields a polyvinyl ester-based polymer with a narrow molecular weight distribution even when producing a high-molecular-weight vinyl ester polymer by RAFT polymerization.SOLUTION: The present invention provides a method for producing a polyvinyl ester-based polymer through a polymerization process using a vinyl ester monomer. This method induces the polymerization process with a polymerization initiator in the presence of a compound represented by the general formula (A) at a polymerization temperature of 0-55°C. (In the formula (A), R is a C1-5 alkyl group).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a polyvinyl ester polymer, and more particularly to a method for producing a polyvinyl ester polymer, Polyvinyl ester polymers obtained by polymerizing vinyl ester monomers in the presence of a polymerization initiator It concerns the manufacturing method. [Background technology]

[0002] Polyvinyl ester polymers have traditionally been used as polyvinyl alcohol (hereinafter referred to as "PVA"). PVA is a polyvinyl ester polymer that is widely used as a raw material for It is a crystalline water-soluble polymer material obtained by saponifying a copolymer of ethylenediaminetetraacetate and propylene glycol. It has excellent water solubility and Taking advantage of the film properties (strength, oil resistance, film-forming ability, oxygen gas barrier properties, etc.), it is used as an emulsifier, suspending agent, Used in surfactants, textile processing agents, various binders, paper processing agents, adhesives, films, etc. There are.

[0003] Polyvinyl ester polymers are obtained by polymerizing vinyl ester monomers. However, the polymerization method can be applied to the polymerization of various vinyl compounds, and the handling of the reaction system is easy. Radical polymerization, which is easy to carry out, is widely used industrially. The reaction includes initiation, propagation and termination reactions, and chain transfer reactions may occur as side reactions. In radical polymerization, when an initiating radical is generated, it reacts with the monomers one after another to produce The reaction is terminated by the inactivation of the propagating radical. This occurs due to the polymerization termination reaction, disproportionation termination reaction, and side reaction, chain transfer reaction, etc., so the length of the molecule As a result, polymers with inconsistent sizes are produced.

[0004] Therefore, as a method for controlling the molecular weight of the resulting polymer, living radical polymerization Living radical polymerization is a process in which the polymer is synthesized. This is a polymerization method that consists only of initiation and propagation reactions, and does not involve propagation reactions such as termination reactions and chain transfer reactions. Since no reaction that inactivates radicals is involved, polymers with uniform molecular length can be obtained. In addition, sudden temperature rises during the polymerization reaction are less likely to occur, making it easier to control the reaction. The molecular weight of vinyl ester polymers can be easily controlled in production to be uniform. As a living radical polymerization, R AFT (Reversible Addition-Fragmentation Chain Transfer) polymerization was also known ( (See Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-24966 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the RAFT polymerization disclosed in Patent Document 1, a high molecular weight polyvinyl ester There is still room for improvement in controlling the molecular weight distribution when producing polymers. there were. Generally, when trying to obtain a high molecular weight polymer by RAFT polymerization, The amount of RAFT agent added must be reduced, but the RAFT polymerization of vinyl ester monomers The main causes are the generation of low molecular weight polymers through chain transfer reactions and head-to-head bonds. The formation of terminals that do not function as RAFT agents due to the bonding of the secondary carbon with the RAFT agent, However, side reactions such as the elimination of the RAFT agent from the terminal of R Under conditions where the amount of AFT agent added is small, that is, under conditions where a polymer having a high molecular weight is to be obtained, the above It was thought that the effects of side reactions could no longer be ignored, resulting in a broad molecular weight distribution.

[0007] In this invention, we aim to develop a method for the synthesis of high molecular weight vinyl ethers using RAFT polymerization. When preparing vinyl ester polymers, it is necessary to produce polyvinyl esters having a narrow molecular weight distribution. The object of the present invention is to provide a new production method by which a polymer based on the above-mentioned copolymer can be obtained. [Means for solving the problem]

[0008] However, the present inventors focused on the polymerization temperature during RAFT polymerization and discovered that the polymerization reaction can be carried out at a lower temperature than usual. In the case where a high molecular weight vinyl ester polymer is to be produced by carrying out the steps It has been found that a polyvinyl ester polymer having a narrow molecular weight distribution can be obtained even in the presence of the Completed Ming.

[0009] That is, the gist of the present invention is the following [1] to [6]. [1] A method for producing polyvinyl ester polymers by polymerization using vinyl ester monomers. The polymerization is carried out using a polymerization initiator in the presence of a compound represented by the following general formula (A), A method for producing a polyvinyl ester polymer, comprising carrying out polymerization at 0 to 55°C. [ka] (In the above formula (A), R is an alkyl group having 1 to 5 carbon atoms.) [2] The polymerization initiator according to [1], characterized in that the 10-hour half-life temperature of the polymerization initiator is 50°C or less. A method for producing the polyvinyl ester polymer described above. [3] The amount of the compound represented by the general formula (A) added is [1] or [2], characterized in that the amount of 2. A method for producing the polyvinyl ester polymer according to claim 1 . [4] The process according to [1] to [3] is characterized in that the process is carried out by bulk polymerization substantially free of polymerization solvent. ] A method for producing a polyvinyl ester polymer according to any one of the preceding claims. [5] The vinyl ester monomer is preferably vinyl acetate. ] A method for producing a polyvinyl ester polymer according to any one of the preceding claims. [6] The number average molecular weight of the polyvinyl ester polymer is 100,000 or more. The method for producing a polyvinyl ester polymer according to any one of [1] to [5], . Effect of the Invention

[0010] According to the production method of the present invention, it is possible to obtain a polyvinyl ester polymer having a high molecular weight and a narrow molecular weight distribution. A combination can be produced. In addition, since the production method of the present invention can stably carry out the reaction during polymerization, the reaction control This makes it possible to stably produce a polyvinyl ester polymer. The resulting polyvinyl ester polymer is then saponified to obtain a high molecular weight copolymer having a narrow molecular weight distribution. The molecular weight distribution of the high molecular weight polyvinyl alcohol is narrow. Alcohol improves coating stability by lowering the viscosity of the aqueous solution and improves optical properties when processed into optical films. Improved performance can be expected. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below, but these are merely examples of preferred embodiments. However, the present invention is not limited to these contents. In the present specification, (meth)allyl means allyl, methallyl, or (meth)acrylic. means acrylic or methacrylic, (meth)acrylate means acrylate or methacrylate Each of these terms means

[0012] The method for producing a polyvinyl ester polymer of the present invention comprises the steps of: The polymerization was carried out at a temperature of 0 to 55°C using a polymerization initiator in the presence of a certain chain transfer agent (RAFT agent). Living Radical Polymerization (RAFT) of Nyl Ester Monomers n-Fragmentation Chain Transfer Polymerization).

[0013] [ka]

[0014] (In the above formula (A), R is an alkyl group having 1 to 5 carbon atoms.)

[0015] The vinyl ester monomer used in the production method of the present invention is, for example, vinyl acetate. , vinyl propionate, vinyl butyrate, vinyl caproate, vinyl caprylate, capric acid Vinyl, vinyl laurate, vinyl myristate, vinyl palmitate, vinyl stearate Vinyl, cyclohexane carboxylate, vinyl pivalate, vinyl octylate, monoc Vinyl peracetate, vinyl adipate, vinyl methacrylate, vinyl crotonate, sorbic acid Examples of vinyl acrylate include vinyl acetate, vinyl benzoate, vinyl cinnamate, and vinyl trifluoroacetate. These may be used alone or in combination of two or more. From the viewpoints of cost and availability, vinyl acetate is preferably used.

[0016] The polyvinyl ester polymer produced in the present invention is preferably Alternatively, the vinyl ester monomer may be copolymerized with another monomer copolymerizable with the vinyl ester monomer. Examples of the monomer include ethylene, propylene, isobutylene, α-octene, α-dodecane, and the like. Olefins such as decene and α-octadecene; acrylic acid, methacrylic acid, crotonic acid, Unsaturated acids such as maleic acid, maleic anhydride, itaconic acid, etc., or their salts, mono- or Dialkyl esters, etc.; nitriles such as acrylonitrile and methacrylonitrile; acrylonitrile amides such as acrylamides and methacrylamides; ethylenesulfonic acid, allylsulfonic acid, methylsulfonic acid, Olefin sulfonic acids such as terarylsulfonic acid or their salts; alkyl vinyl ethers N-Acrylamidomethyltrimethylammonium chloride;Allyltrimethyla Ammonium chloride;Dimethylallyl vinyl ketone;N-Vinylpyrrolidone;Vinyl chloride vinylidene chloride; polyoxyethylene (meth)allyl ether, polyoxypropylene polyoxyalkylene (meth)allyl ethers such as polyoxyalkylene (meth)allyl ethers; Polyethylene (meth)acrylate, polyoxypropylene (meth)acrylate, etc. Oxyalkylene (meth)acrylate; Polyoxyethylene (meth)acrylamide, Polyoxyalkylene (meth)acrylamide, etc. Polyoxyethylene [1-(meth)acrylamide-1,1-dimethylpropionate esters; polyoxyethylene vinyl ether, polyoxypropylene vinyl ether polyoxyalkylene vinyl ethers such as polyoxyethylene allylamine, polyoxyethylene polyoxyalkylene allylamines such as propylene allylamine; polyoxyethylene Polyoxyalkylene vinylamines such as polyoxyalkylene vinylamine and polyoxypropylene vinylamine 3-Buten-1-ol, 4-Penten-1-ol, 5-Hexen-1-ol Hydroxy group-containing α-olefins such as α-olefins containing hydroxy groups or their acylated derivatives. can be done.

[0017] Also, 3,4-dihydroxy-1-butene, 3,4-diacyloxy-1-butene, 3- Acyloxy-4-hydroxy-1-butene, 4-acyloxy-3-hydroxy-1-butene 3,4-diacyloxy-2-methyl-1-butene, 4,5-dihydroxy-1-pentene 4,5-Diacyloxy-1-pentene, 4,5-Dihydroxy-3-methyl-1- Pentene, 4,5-diacyloxy-3-methyl-1-pentene, 5,6-dihydroxy- 1-Hexene, 5,6-diacyloxy-1-hexene, glycerin monoallyl ether, 2,3-Diacetoxy-1-allyloxypropane, 2-acetoxy-1-allyloxy -3-hydroxypropane, 3-acetoxy-1-allyloxy-2-hydroxypropane Glycerol monovinyl ether, glycerol monoisopropenyl ether, vinyl ether Dioxanes such as ethylene carbonate and 2,2-dimethyl-4-vinyl-1,3-dioxolane Examples of the compound include compounds having a ring structure.

[0018] The compound represented by the above general formula (A) is a compound for controlling radical polymerization. It reacts with the end of a growing polymer chain to terminate the polymer growth and simultaneously initiate new polymerization. It is a so-called chain transfer agent (RAFT agent) that generates radicals. The polymerization mechanism of living radical polymerization was examined using vinyl acetate as a vinyl ester monomer. The following scheme I will be used to explain the production of polyvinyl acetate. The dithiocarbonyl compound 1 (dormant species) was added as a dithiocarbamate, and polyvinyl acetate was The radical Y of the aryl group is added to generate intermediate radical 2. Another polyvinyl acetate radical Y'· is eliminated from the carboxyl group, forming a new dormant species (dithiocarbamate). In this way, a carbonyl compound 1') and another polyvinyl acetate radical Y'· are produced. Polymerization proceeds by repeating addition and elimination. In the following scheme I, X is OR (R is , an alkyl group having 1 to 5 carbon atoms).

[0019] [ka]

[0020] In the general formula (A), R is an alkyl group having 1 to 5 carbon atoms. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, Examples include an isobutyl group, a sec-butyl group, a tert-butyl group, and a pentyl group.

[0021] From the viewpoint of ease of production, the compound represented by the general formula (A) is preferably a compound in which R has 1 to 4 carbon atoms. Compounds in which R is an alkyl group having 2 to 4 carbon atoms are preferred. More preferably, specifically, an isopropyl group and an ethyl group are preferred, and particularly preferably an isopropyl group. The compound represented by formula (A) may be used alone or in combination of two or more. They may also be used in combination.

[0022] Specific examples of the compound represented by formula (A) include S-1-isobuto xyethyl O-isopropyl xanthate (R is an isopropyl group) Compound (S-1-isobutoxyethyl O-ethyl xanthate) e (a compound in which R is an ethyl group) and the like.

[0023] The method for producing a polyvinyl ester polymer of the present invention is carried out in the presence of a polymerization initiator. Examples of initiators include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-Azobisisobutyronitrile (AIBN), 2,2'-azobis-(4-meth 2,2'-azobis-(2-methylpropionyl) azo compounds such as tert-butyl peroxyneodecanoate, peroxypivalate, alkyl peresters such as t-butyl peroxypivalate, bis-(4-t- Butylcyclohexyl)peroxydicarbonate, dicyclohexylperoxy -dicarbonate, bis(2-ethylhexyl)peroxy-dicarbonate, di sec-Butyl peroxy dicarbonate, diisopropyl peroxy dicarbonate Peroxydicarbonates such as carbonates, acetyl peroxide, diacetyl peroxide Oxide, dilauroyl peroxide, didecanoyl peroxide, dioctanoyl peroxide, dipropyl peroxide, dibenzoyl peroxide, etc. The polymerization initiators may be any of the known polymerization initiators such as azides. Alternatively, two or more of them may be used simultaneously. Among these, it is preferable to use a polymerization initiator having a low 10-hour half-life temperature. t-Butyl peroxypivalate, t-Butyl peroxyneodecanoate, bis (2-Ethylhexyl)peroxydicarbonate, di-sec-butylperoxy -dicarbonate, 2,2'-azobis-(2,4-dimethylvaleronitrile), 2, 2'-azobis-(4-methoxy-2,4-dimethylvaleronitrile) is preferred, 2,2'-azobis( 4-Methoxy-2,4-dimethylvaleronitrile). The 10-hour half-life temperature of the polymerization initiator is preferably 50° C. or lower. If the temperature is too high, the number of free polymer end radicals will be too low, and the polymerization may not proceed. The 10-hour half-life temperature of the polymerization initiator is more preferably 40° C. or lower.

[0024] Other components may be added to the polymerization reaction solution within the range that does not impair the effects of the present invention. Other additives include, for example, colorants, dyes, defoamers, preservatives, fungicides, and oxidants. In addition, saturated fats such as stearic acid amides can be used. Aliphatic amides, unsaturated fatty acid amides such as oleic acid amide, ethylene bis(stearic acid amide) and bis-fatty acid amides such as ethylene glycol, low molecular weight polyolefins and other known lubricants, release agents, and Polyhydric alcohols such as glycerin, hexanediol, etc., especially aliphatic polyhydric alcohols known plasticizers such as alcohol, acids such as acetic acid and phosphoric acid, and their alkali metals and alkaline earth metals metal salts of metals such as boric acid, metal oxides and hydroxides, and other metal compounds; Known heat stabilizers, such as boron compounds such as salts, may also be included.

[0025] Next, a specific method for producing the polyvinyl ester polymer of the present invention will be described. In the production method of the present invention, a vinyl ester monomer, a copolymer represented by general formula (A), The compound and polymerization initiator are added to start the polymerization reaction. They may be added in any order.

[0026] In the polymerization reaction in the production method of the present invention, a polymerization solvent may be used. Although bulk polymerization may be carried out without using a polymerization solvent, it is difficult to control the molecular weight and molecular weight distribution. In this respect, it is preferred to carry out bulk polymerization substantially without using a polymerization solvent. The term "substantially free of polymerization solvent" means that the content of the polymerization solvent is usually 1% by mass or less. , preferably 0.1 mass % or less.

[0027] The polymerization reaction in the production method of the present invention is carried out using an inactive solvent that is inactive to vinyl ester monomers. The reaction is preferably carried out under an inert gas atmosphere. Examples of the inert gas include nitrogen and argon. Examples include:

[0028] The amount of the compound represented by the general formula (A) to be added is determined based on the initial amount of the vinyl ester monomer. It is preferable that the content of the compound represented by formula (A) is 0.0001 to 1 mol %. If there is too much, the number of free polymer end radicals will be too few, and the polymerization will not proceed. If the amount is too small, the polymerization control may not be performed, and polyvinyl esters with a uniform molecular weight may not be obtained. It is difficult to obtain a vinyl polymer. The amount of the compound represented by formula (A) to be added is 0.0005 to 0. It is more preferably 1 mol %, and further preferably 0.001 to 0.01 mol %. .

[0029] The amount of polymerization initiator added is 0.0000 relative to the initial amount of vinyl ester monomer. The amount of the polymerization initiator is preferably 1 to 0.2 mol %. If the amount of the polymerization initiator is too large, it becomes difficult to control the polymerization. If the amount of the polymerization initiator is too small, productivity may be impaired. is 0.00005 to 0.01 mol% of the initial charge of vinyl ester monomer. It is more preferable that the content is 0.0001 to 0.001 mol %, and further more preferable that the content is 0.0001 to 0.001 mol %.

[0030] In the production method of the present invention, the polymerization temperature is 0 to 55° C. in order to exhibit the effects of the present invention. The temperature of the reaction solution is preferably 5 to 50° C. The temperature is more preferably 15 to 45°C, and particularly preferably 20 to 35°C. If the temperature of the reaction solution is too high, it becomes difficult to control the molecular weight or polymerization. If the temperature is too low, the polymerization rate will be slow, which may cause problems in productivity. be. In this specification, the polymerization temperature refers to the temperature during the period in which the monomer is converted into a polymer. The temperature of the reaction solution, more specifically, the temperature at which the polymerization reaction is started by adding the polymerization initiator. When the polymerization reaction is stopped by adding a polymerization terminator or when the temperature of the reaction solution is suddenly lowered, This refers to the temperature up to the point at which the polymerization reaction is substantially stopped by, for example,

[0031] The reaction time may be appropriately set so as to obtain a polymer having a desired molecular weight. In consideration of the above, the reaction is preferably carried out for a period of 0.1 to 48 hours, more preferably for a period of 0.3 to 36 hours. The reaction time is preferably from 0.5 to 24 hours, and more preferably from 0.5 to 24 hours. If the reaction time is too long, problems will arise in productivity. If the length is too short, the molecular weight will not be uniform, and a polyvinyl ester polymer with a homogeneous molecular weight will not be obtained. Coalescence may not be achieved.

[0032] In the present invention, when the desired polymerization rate is reached, a polymerization terminator is added to terminate the polymerization. Perform the stop reaction.

[0033] Examples of the polymerization terminator include hydroquinone, hydroquinone monomethyl ether, Quinone compounds such as parabenzoquinone, o-dinitrobenzene, m-dinitrobenzene, Nitrobenzene compounds such as p-dinitrobenzene are examples of these. Among these, those having problems such as coloring and toxicity may be used. From this viewpoint, it is preferable to use hydroquinone monomethyl ether.

[0034] The amount of the polymerization terminator to be added is not particularly limited as long as it is an amount that can terminate the polymerization. The content of the initial charge of ester monomer is 0.001 to 10,000 ppm. If the amount of the polymerization terminator is too small, the radicals at the polymer terminals cannot be sufficiently captured, and the polymerization Insufficient termination may result in a broad molecular weight distribution, and too much When the PVA produced using the obtained polyvinyl ester polymer is easily discolored, The amount of polymerization terminator added is 0.1 times the initial amount of vinyl ester monomer. The concentration is more preferably from 1 to 5000 ppm, and further preferably from 1 to 1000 ppm.

[0035] In the termination step, the temperature of the reaction solution is adjusted so that the polymerization terminator can capture the radicals at the polymer terminals. The temperature may be set to any value within the range of 0 to 100°C, preferably 3 to 60°C, and more preferably 5 to 100°C. 50°C is more preferable. If the temperature of the reaction solution is too high, polymerization will proceed while the termination reaction will proceed. If the temperature is too low, the viscosity of the polymerization solution may increase. This makes it difficult for the polymerization terminator to be mixed uniformly in the polymerization solution.

[0036] The reaction time in the termination step should be within the range of 0.01 to 24 hours, taking productivity into consideration. is preferable, 0.03 to 6 hours is more preferable, and 0.05 to 2 hours is even more preferable.

[0037] After the stopping step, the solution containing the polyvinyl ester polymer is heated, vacuum dried, etc. By this, the solvent and the unreacted monomers are distilled off to obtain a polyvinyl ester polymer. .

[0038] The number average molecular weight (Mn) of the polyvinyl ester polymer of the present invention is 100,000 to 1 When the number average molecular weight (Mn) is in the above range, the poly When vinyl ester polymers are used to produce PVA, they can be produced stably. If the number average molecular weight (Mn) of the ester polymer is too high, the viscosity of the solution becomes too high and it becomes difficult to separate. It may be difficult to handle, the dissolution rate may decrease, and if it is too low, particle formation may be difficult. It may be difficult to obtain a number average molecular weight (Mn) of 150,000 to 900,000. It is more preferable that the molecular weight is 180,000 to 800,000, and further more preferable that the molecular weight is 180,000 to 800,000. In the present invention, the number average molecular weight (Mn) and the weight average molecular weight (Mw) of the polyvinyl ester polymer are The weight average molecular weight (Mw) was measured using gel permeation chromatography (GPC). This can be determined using polystyrene as a standard.

[0039] The molecular weight distribution (dispersity) of the polyvinyl ester polymer obtained by the production method of the present invention The molecular weight distribution (Mw / Mn) is preferably 1 to 2. It is a value expressed as the ratio of weight average molecular weight (Mw) to molecular weight (Mn), and the molecular weight distribution ( When the Mw / Mn ratio is within the above range, the molecular weight distribution of the polyvinyl ester polymer is narrow. In this way, it can be said that the generation of low molecular weight polymers is small. It is possible to stably produce polyvinyl ester polymers having a narrow molecular weight distribution. The fabric (Mw / Mn) is more preferably more than 1 and not more than 1.8, and more preferably more than 1 and not more than 1.5. Even more preferred.

[0040] The polyvinyl ester polymer obtained by the production method of the present invention is saponified. This allows the production of polyvinyl alcohol (PVA). The resulting polyvinyl ester polymer can be saponified by a conventionally known saponification method. That is, the polyvinyl ester polymer is dissolved in alcohol or This can be done by dissolving in a water / alcohol solvent and using an alkaline or acid catalyst. Cut. Examples of the alkali catalyst include potassium hydroxide, sodium hydroxide, and sodium Al methylate, sodium ethylate, potassium methylate, lithium methylate, etc. Potassium metal hydroxides and alcoholates can be used. Generally, transesterification using an alkali catalyst in an absolute alcohol solvent has a high reaction rate. It is preferably used in that impurities such as fatty acid salts can be reduced.

[0041] The reaction temperature for the saponification reaction is usually 20 to 60°C. If the reaction temperature is too low, the reaction rate If the temperature is too high, it may exceed the boiling point of the reaction solvent. This tends to reduce safety in terms of production. When saponification is performed under high pressure using a saponification tower, the saponification is performed at a higher temperature, for example, 80 to 150°C. It is possible to obtain a high degree of saponification in a short time with a small amount of saponification catalyst. is possible.

[0042] The polyvinyl ester polymer obtained in the present invention is obtained by removing the solvent and unreacted monomers. Alternatively, the saponification step may be carried out directly after the termination step without carrying out the above-mentioned step to obtain PVA.

[0043] The polyvinyl ester polymer obtained by the production method of the present invention has a narrow molecular weight distribution. The crystallinity of PVA obtained by using the polyvinyl ester polymer is increased, and the molding The product has excellent gas barrier properties. In addition, the content of low molecular weight is small, so it can be used as a filler for molding. This prevents impurities from being mixed into the film when it is made, resulting in high-quality film. It can be achieved. EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the following examples. In the following examples and comparative examples, the units "parts" and "components" are used. "%" is by weight unless otherwise specified.

[0045] <Measurement of polymerization rate> Weigh out about 1 to 2 g of the sample into an aluminum cup and dry it in a dryer at 140°C for 30 minutes. After that, the resin content was calculated from the amount of sample remaining in the aluminum cup.

[0046] <Measurement of number average molecular weight, weight average molecular weight, and dispersity (molecular weight distribution)> The number average molecular weight (Mn) and weight average molecular weight (Mw) of the polyvinyl ester polymer were measured using a high performance liquid chromatograph "Prominence" (product name) manufactured by Shimadzu Corporation, with Shodex KF-806L (8.0 mm ID × 300 mm ) × 3 columns and RI (Shodex RI-501) as the detector. The polyvinyl ester polymer was dissolved in tetrahydrofuran to obtain a polymer sample solution with a polymer concentration of 0.25% by mass, and using tetrahydrofuran as the eluent, the flow rate was 1.0 ml / min, and the column temperature was measured under the condition of 35 °C. A calibration curve was prepared using monodisperse molecular weight polystyrene as the standard substance, and the number average molecular weight (M n) and weight average molecular weight (Mw) of the polyvinyl ester polymer in terms of polystyrene were measured. From the obtained values of number average molecular weight (Mn) and weight average molecular weight (Mw), the dispersity (Mw / M n) was calculated.

[0047] <RAFT agent> The RAFT agent, S-1-isobutoxyethyl O-is opropyl xanthate (hereinafter referred to as iPrBEX. R in formula (A) = isopropyl group) used in the examples of the present application was synthesized according to a known method as in the following synthesis example. <Synthesis Example 1> "Production of S-1-isobutoxyethyl O-isopropyl xa n thate (iPrBEX)" 100 mL (0.1 mo l in Et2O) of 1.0 M HCl·Et2O (hydrogen chloride·diethyl ether) was placed in a 200 mL eggplant flask cooled to 0 °C. 13 mL (0.1 mol) of isobutyl vinyl ether (IBVE) was added while stirring the HCl·Et2O Add the solution dropwise to the flask containing the IBVE-HCl solution, and continue stirring at 0°C for about 1 hour. The unused HCl was released as a gas and purified. Put 11.6 g (0.067 mol) of sodium into a recovery flask cooled to 0°C, and add the mixture from above. 76 mL (0.076 mol) of the IBVE-HCl adduct solution was added. The mixture was stirred for 4 hours at 0°C to room temperature using a stirrer. Then, the mixture was filtered using a glass funnel. The filtrate was transferred to a separatory funnel and washed three times with 0.2M NaHCO3 and twice with pure water. This was transferred to a dry Erlenmeyer flask and pre-dried overnight over anhydrous sodium sulfate. The sodium chloride was removed and the solution was decanted into a dry recovery flask. The solvent was distilled off. After that, vacuum distillation (bp78℃ / 0.6kPa) was performed twice over CaH2 under dry nitrogen. The yellow liquid was purified by filtration. The synthesis yield was 51%. .

[0048] <Polymerization initiator> The following polymerization initiators were prepared: 2,2'-Azobis(4-methoxy-2,4-dimethylvaleronitrile): 10.5 hours Decrease temperature 30℃ 2,2'-Azobisisobutyronitrile: 10 hours half-life temperature 65℃

[0049] <Example 1> A reactor equipped with a stirrer, a thermometer, a reflux condenser, and a sample inlet was charged with 200 parts by mass of vinyl acetate, Add 0.0384 parts by mass of iPrBEX (0.00699 mol% relative to vinyl acetate) The inside of the reactor was replaced with nitrogen by bubbling nitrogen for 30 minutes. The reactor was immersed in the bath and heating and stirring were started so that the internal temperature (polymerization temperature) of the reactor became 40°C. When the temperature of the liquid in the vessel reached 40°C, 2,2'-azobis(4-methionine) was added as a polymerization initiator. 0.005 parts by mass of 2,4-dimethylvaleronitrile (based on vinyl acetate) After polymerization for 3 hours, heating was stopped. As a polymerization terminator, 0.002 parts by mass of m-dinitrobenzene and 100 parts by mass of methanol were used. The polymerization was terminated by adding 1,000 ml of the mixture. The polymerization rate at this time was 19%. The resulting polymerization reaction solution was vacuum dried to remove unreacted monomers, and polyvinyl chloride was obtained. The number average molecular weight (Mn) of the obtained polyvinyl acetate was 182,000. The weight average molecular weight (Mw) was 265,000 and the dispersity (Mw / Mn) was 1.46.

[0050] <Example 2> The polymerization was carried out in the same manner as in Example 1, except that the polymerization temperature was 30° C. and the polymerization time was 6 hours. The conversion rate at the time of termination of the polymerization was 14%. The number average molecular weight (Mn) of the obtained polyvinyl acetate was 152,000, weight average molecular weight (Mw) is 200,000, and molecular weight distribution Mw / Mn is 1 The result was .32.

[0051] <Comparative Example 1> A reactor equipped with a stirrer, a thermometer, a reflux condenser, and a sample inlet was charged with 195 parts by mass of vinyl acetate, 0.086 parts by mass of iPrBEX (0.0157 mol% relative to vinyl acetate) was added. The reactor was immersed in a water bath and the water bath was heated until the liquid inside boiled. The temperature of the liquid in the vessel was 72°C. 15 minutes after the start of boiling, 2,2'-azo Bisisobutyronitrile 0.006 parts by mass (0.00157 mol% relative to vinyl acetate) ) was dissolved in 5 parts by mass of vinyl acetate and added to start polymerization. Polymerization was continued for 3.25 hours. After that, the heating was stopped and 0.002 parts by mass of m-dinitrobenzene and meta were added as a polymerization terminator. The polymerization was terminated by adding 100 parts by mass of alcohol. At this time, the polymerization rate was 56%. The number average molecular weight (Mn) of the obtained polyvinyl acetate was 167,000, and the weight average molecular weight ( The molecular weight (Mw) was 304,000 and the polydispersity (Mw / Mn) was 1.82.

[0052] The above examples and comparative examples are summarized in Table 1.

[0053] [Table 1]

[0054] Compared to Comparative Example 1, in Example 1, the polymerization temperature was set to 40° C., so that the number average molecular weight was high. Nevertheless, polyvinyl acetate with a narrow molecular weight distribution (small Mw / Mn) was obtained. In Example 2, the polymerization temperature was set at 30° C., and polyvinyl acetate with a narrower molecular weight distribution was obtained. I was able to do it.

Claims

1. A method for producing a polyvinyl ester polymer by polymerization using a vinyl ester monomer. The polymerization is carried out at a temperature of 0 to 400° C. using a polymerization initiator in the presence of a compound represented by the following general formula (A): A method for producing a polyvinyl ester polymer, comprising polymerizing at 55°C. 【Chemistry 1】 (In the above formula (A), R is an alkyl group having 1 to 5 carbon atoms.)

2. 2. The polymerization initiator according to claim 1, wherein the 10-hour half-life temperature of the polymerization initiator is 50° C. or less. A method for producing a polyvinyl ester polymer.

3. The amount of the compound represented by the general formula (A) added is the same as the amount of the vinyl ester monomer added. The polyvinyl chloride according to claim 1, characterized in that the content of the polyvinyl chloride is 0.0001 to 1 mol %. A method for producing a diester polymer.

4. The polymer according to claim 1, characterized in that the polymerization is carried out by bulk polymerization substantially free of polymerization solvent. A method for producing vinyl ester polymers.

5. 2. The polymer according to claim 1, wherein the vinyl ester monomer is vinyl acetate. A method for producing vinyl ester polymers.

6. The polyvinyl ester polymer has a number average molecular weight of 100,000 or more. The method for producing a polyvinyl ester polymer according to claim 1,

Citation Information

Patent Citations

  • Method of producing polyvinyl ester-based polymer

    JP2021024966A