Visible light responsive semiconductor photoelectrode
A protective film of Ti oxide and/or Al oxide on sulfide-based semiconductor photocatalyst materials addresses the stability issue, enhancing both efficiency and durability in semiconductor photoelectrodes.
Patent Information
- Application Number
- JP2023043745
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Sulfide-based semiconductor photocatalyst materials exhibit high light energy conversion efficiency but lack sufficient stability.
A protective film of Ti oxide and/or Al oxide is applied to the surface of a sulfide-based semiconductor photocatalyst material, with a thickness ranging from 2 to 5 nm, to enhance stability while maintaining conversion efficiency.
The protective film achieves both high light energy conversion efficiency and improved stability in semiconductor photocatalyst materials, ensuring consistent performance over time.
Smart Images

Figure 2024133782000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a visible light responsive semiconductor photoelectrode. [Background technology]
[0002] In recent years, artificial photosynthesis using sunlight has attracted attention as a way to achieve carbon neutrality. One example of a semiconductor photocatalyst material for artificial photosynthesis is a semiconductor photoelectrode, which has a visible-light-responsive semiconductor photocatalyst film made of metal oxides such as bismuth, vanadium, and tungsten formed on the surface of a conductive glass electrode.
[0003] Semiconductor photocatalysts made of metal oxides have the advantage of being inexpensive and easy to form into large-area films, but these semiconductor photocatalysts made of metal oxides lack sufficient light energy conversion efficiency and stability.
[0004] For example, Patent Document 1 describes a stabilized visible-light-responsive semiconductor photoelectrode, which is a stabilized material that improves the stability of semiconductor materials during photoreaction and does not reduce efficiency, and is characterized in that a semiconductor layer made of a visible-light-responsive semiconductor containing Bi, V, W, and oxygen as constituent elements is coated with a protective film made of a compound containing one or more elements selected from the group consisting of Nb, Sn, Zr, La, Ti, Bi, and Ta. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 2014-15642 Summary of the Invention [Problem to be solved by the invention]
[0006] Sulfide-based materials are known as highly efficient semiconductor photocatalyst materials that can be used in semiconductor photoelectrodes. Although sulfide-based materials have high light energy conversion efficiency, improving their stability remains an issue.
[0007] Therefore, an object of the present invention is to provide a means for achieving both high light energy conversion efficiency and stability in a semiconductor photocatalytic material used in a semiconductor photoelectrode. [Means for solving the problem]
[0008] The present inventors have investigated various means for solving the above problems. They have found that by disposing a protective film of Ti oxide and / or Al oxide on the upper surface of a sulfide-based semiconductor photocatalytic material and setting the thickness of the protective film within a predetermined range, it is possible to improve stability while maintaining high light energy conversion efficiency. Based on this finding, the present inventors have completed the present invention.
[0009] That is, the present invention includes the following aspects and embodiments. (Embodiment 1) A visible-light-responsive semiconductor photoelectrode comprising a semiconductor layer made of a visible-light-responsive semiconductor made of MoS2, and a protective film made of one or more metal oxides selected from the group consisting of Ti oxides and Al oxides, disposed on the upper surface of the semiconductor layer, the protective film having a thickness in the range of 2 to 5 nm. (Embodiment 2) The visible light responsive semiconductor photoelectrode according to embodiment 1, wherein the protective film is made of either Ti oxide or Al oxide. (Embodiment 3) The visible light responsive semiconductor photoelectrode according to embodiment 1 or 2, wherein the protective film is made of either TiO2 or Al2O3. (Embodiment 4) The visible light responsive semiconductor photoelectrode according to any one of embodiments 1 to 3, wherein the semiconductor layer has a film thickness of 2 to 3 nm. (Embodiment 5) The visible light responsive semiconductor photoelectrode according to any one of embodiments 1 to 4, wherein the semiconductor layer has a thickness of 2 to 3 nm, and the protective film is made of either TiO2 or Al2O3. [Effects of the Invention]
[0010] The present invention makes it possible to provide a means for achieving both high light energy conversion efficiency and stability in a semiconductor photocatalytic material used in a semiconductor photoelectrode. [Brief explanation of the drawings]
[0011] [Figure 1] This is a TEM image of a glass substrate having a semiconductor (MoS2) photoelectrode on which a TiO2 nanosheet film is formed. [Figure 2] Graphs showing the relationship between the thickness of protective films of semiconductor photoelectrodes having various protective film thicknesses and the initial photocurrent density and characteristic retention rate of a photoelectrochemical cell having the semiconductor photoelectrode as the working electrode (anode). In the graph, the horizontal axis represents the thickness (nm) of the protective film of the semiconductor photoelectrode, the left vertical axis and the black square plot represent the initial photocurrent density (μA / cm), and the right vertical axis and the black circle plot represent the characteristic retention rate (%). The characteristic retention rate (%) is the percentage of the photocurrent density after a 2-hour durability test relative to the initial photocurrent density. (a) represents a combination of black square and black circle plots measured using a photoelectrochemical cell having a glass substrate with a semiconductor photoelectrode on which an AlO nanosheet film is formed as the working electrode (anode). (b) represents a combination of black square and black circle plots measured using a photoelectrochemical cell having a glass substrate with a semiconductor photoelectrode on which a TiO nanosheet film is formed as the working electrode (anode). DETAILED DESCRIPTION OF THE INVENTION
[0012] Preferred embodiments of the present invention will now be described in detail.
[0013] One aspect of the present invention relates to a visible-light-responsive semiconductor photoelectrode (hereinafter also simply referred to as "semiconductor photoelectrode"). The semiconductor photoelectrode of this aspect has a semiconductor layer and a protective film made of a metal oxide disposed on the upper surface of the semiconductor layer. By disposing the protective film on the upper surface of the semiconductor layer, the semiconductor photoelectrode of this aspect can exhibit high stability.
[0014] In the semiconductor photoelectrode of this embodiment, the semiconductor layer is made of a visible-light-responsive semiconductor made of MoS2. Sulfide-based semiconductor photocatalytic materials are known to have high light energy conversion efficiency. The present inventors have found that when a semiconductor photoelectrode having a semiconductor layer made of a visible-light-responsive semiconductor made of MoS2 is applied to a photoelectrochemical cell, it exhibits a high photocurrent density. Therefore, the semiconductor photoelectrode of this embodiment having a semiconductor layer made of a visible-light-responsive semiconductor made of MoS2 can exhibit high light energy conversion efficiency.
[0015] In the semiconductor photoelectrode of this embodiment, the atomic composition of the semiconductor in the semiconductor layer can be confirmed by analyzing the semiconductor layer using, for example, X-ray photoelectron spectroscopy (XPS).
[0016] The semiconductor layer preferably has a film thickness of 2 to 3 nm. The semiconductor photoelectrode of this embodiment, which has a semiconductor layer in the form of a nanosheet film with a film thickness in this range, can exhibit high light energy conversion efficiency.
[0017] In the semiconductor photoelectrode of this embodiment, the film thickness of the semiconductor layer can be confirmed, for example, by observing the semiconductor layer using a transmission electron microscope (TEM).
[0018] In the semiconductor photoelectrode of this embodiment, the protective film is made of one or more metal oxides selected from the group consisting of Ti oxide and Al oxide. The protective film is preferably made of either Ti oxide or Al oxide, and more preferably made of either TiO2 or Al2O3. The inventors have found that when a semiconductor photoelectrode of this embodiment, in which a protective film having the characteristics described above is disposed on the upper surface of a semiconductor layer having the characteristics described above, is applied to a photoelectrochemical cell, the semiconductor photoelectrode exhibits consistent photoelectrochemical characteristics even after durability treatment. Therefore, the semiconductor photoelectrode of this embodiment, which has a protective film on the upper surface of the semiconductor layer, can exhibit high stability.
[0019] In the semiconductor photoelectrode of this embodiment, the atomic composition of the metal oxide of the protective film can be confirmed by analyzing the semiconductor layer using, for example, XPS.
[0020] In the semiconductor photoelectrode of this embodiment, the protective film has a thickness in the range of 2 to 5 nm. The inventors have found that when a semiconductor photoelectrode of this embodiment having a protective film with a thickness in this range is applied to a photoelectrochemical cell, it exhibits a high photocurrent density not only initially but also after durability treatment. If the thickness of the protective film exceeds the upper limit, carrier movement of the semiconductor photocatalyst in the semiconductor layer may be suppressed. Furthermore, if the thickness of the protective film is less than the lower limit, deterioration of the semiconductor layer may be accelerated, resulting in a decrease in stability. Therefore, the semiconductor photoelectrode of this embodiment having a protective film with a thickness in the above range on the upper surface of the semiconductor layer can exhibit both high light energy conversion efficiency and high stability.
[0021] In the semiconductor photoelectrode of this embodiment, the thickness of the protective film can be confirmed, for example, by observing the protective film using a TEM.
[0022] Particularly preferably, in the semiconductor photoelectrode of this embodiment, the semiconductor layer has a thickness of 2 to 3 nm, and the protective film is made of TiO2 or Al2O3. By having the above characteristics, the semiconductor photoelectrode of this embodiment can exhibit both high light energy conversion efficiency and high stability.
[0023] The light energy conversion efficiency and stability of the semiconductor photoelectrode of this embodiment can be evaluated, for example, by the following procedure. The semiconductor photoelectrode of this embodiment is fabricated on the outermost surface of a glass substrate having an ITO electrode formed on its surface. A photoelectrochemical cell is fabricated having this glass substrate as a working electrode and a Pt electrode as a counter electrode. A predetermined constant voltage (e.g., 1.2 V (RHE)) is applied to this cell, and durability treatment is performed for a predetermined time (e.g., 2 hours) from the start of application. The initial photocurrent density and the photocurrent density after the durability treatment are measured. The percentage of the photocurrent density after the durability treatment relative to the initial photocurrent density is calculated as the characteristic maintenance rate (%). The initial photocurrent density represents the light energy conversion efficiency of the semiconductor photoelectrode of this embodiment. Furthermore, the characteristic maintenance rate represents the stability of the semiconductor photoelectrode of this embodiment.
[0024] The semiconductor photoelectrode of this embodiment can be produced, for example, by a method including a semiconductor layer preparation step of obtaining a semiconductor layer made of a visible light responsive semiconductor made of MoS2, and a protective film formation step of forming a protective film made of one or more metal oxides selected from the group consisting of Ti oxides and Al oxides on the upper surface of the semiconductor layer obtained in the semiconductor layer preparation step.
[0025] In the method for producing a semiconductor photoelectrode of this embodiment, the semiconductor layer preparation step can be carried out, for example, by peeling off a nanosheet-shaped MoS2 layer from a MoS2 layered compound, or by depositing a MoS2 layer on the upper surface of a substrate by means of chemical vapor deposition (CVD) or the like. The nanosheet-shaped MoS2 layer can be peeled off, for example, by the following procedure: A MoS2 layered compound is placed on the negative electrode, and a cationic material is electrochemically intercalated between the layers. The expanded MoS2 layer is then subjected to ultrasonic treatment to peel off the nanosheet-shaped MoS2 layer, yielding a semiconductor photocatalyst material made of MoS2.
[0026] In the method for manufacturing the semiconductor photoelectrode of the present aspect, the protective film formation step can be carried out, for example, by using an atomic layer deposition (ALD) film formation method, a dipping film formation method, a dip coating method, a spin coating method, a sputtering method, CVD, PVD, or the like, to form a protective film made of one or more metal oxides selected from the group consisting of titanium oxide and aluminum oxide on the upper surface of the semiconductor layer obtained in the semiconductor layer manufacturing step.
[0027] As described above, the semiconductor photoelectrode of the present aspect can exhibit both high photoenergy conversion efficiency and high stability. Therefore, by applying the semiconductor photoelectrode of the present aspect to a photocatalytic reaction device, an optical sensor, or the like, it is possible to provide a device or the like that achieves both high photoenergy conversion efficiency and stability.
Example
[0028] Hereinafter, the present invention will be described more specifically using examples. However, the technical scope of the present invention is not limited to these examples.
[0029] <I: Fabrication of Semiconductor Photoelectrode> [I-1: Fabrication of Semiconductor Photocatalyst Material] The MoS2 layered compound was placed on the negative electrode, and a cationic material was electrochemically intercalated between the layers. A semiconductor photocatalyst material (hereinafter, also referred to as "MoS2 nanosheet") composed of MoS2 exfoliated into nanosheet form by ultrasonic treatment of the expanded MoS2 layers was obtained. The obtained MoS2 nanosheet was formed on the outermost surface of a glass substrate having an ITO electrode formed on its surface to obtain a glass substrate for evaluating the photoelectrochemical characteristics having a MoS2 nanosheet film with a film thickness of about 2 to 3 nm on its surface.
[0030] [I-2: Fabrication of Protective Film for Deterioration Suppression] On the surface of the MoS2 nanosheet film of the substrate fabricated in I-1, titanium oxide (TiO2) or aluminum oxide (Al2O3) was formed using the atomic layer deposition (ALD) method. In the ALD method, tetrakis(dimethylamino)titanium (TDMA Ti) and trimethylaluminum (TMA) were used as the film-forming raw materials, and water (H2O) was used as the oxidizing agent.
[0031] Also, on the surface of the MoS2 nanosheet film of another substrate fabricated in I-1, TiO2 (Ti 0.87 O2) nanosheets were formed using the dip coating method.
[0032] The film thickness of the protective film on the surface of the substrate fabricated by the above procedure was measured by observation with a transmission electron microscope (TEM) and analysis by X-ray photoelectron spectroscopy (XPS). A TEM image of a glass substrate having a semiconductor (MoS2) photoelectrode on which a TiO2 (Ti 0.87 O2) nanosheet film was formed is shown in FIG. 1. As shown in FIG. 1, this semiconductor (MoS2) photoelectrode has a TiO2 (Ti 0.87 O2) nanosheet film on the surface of the MoS2 nanosheet film.
[0033] <II: Evaluation of Photoelectrochemical Characteristics of Semiconductor Photoelectrodes> A photoelectrochemical cell was fabricated with a glass substrate having the semiconductor photoelectrode fabricated in I as the working electrode (anode) and a Pt electrode as the counter electrode (cathode). A constant voltage of 1.2 V (RHE) was applied to this cell, and durability treatment was performed for 2 hours from the start of application. The initial photocurrent density and the photocurrent density after 2-hour durability treatment were measured. The percentage of the photocurrent density after 2-hour durability treatment with respect to the initial photocurrent density was calculated as the characteristic retention rate (%). FIG. 2 shows a graph showing the relationship between the film thickness of the protective film and the initial photocurrent density and the characteristic retention rate of a photoelectrochemical cell having the semiconductor photoelectrode with the protective film of various film thicknesses as the working electrode (anode). In the figure, the horizontal axis is the film thickness (nm) of the protective film of the semiconductor photoelectrode, and the left vertical axis and the black-filled square plots are the initial photocurrent density (μA / cm 2), and the right vertical axis and the black circle plots represent the characteristic retention rate (%). (a) shows a combination of black squares and black circles plotted, measured using a photoelectrochemical cell having a glass substrate with a semiconductor photoelectrode on which an Al2O3 nanosheet film was formed as the working electrode (anode). (b) shows a combination of black squares and black circles plotted, measured using a photoelectrochemical cell having a glass substrate with a semiconductor photoelectrode on which a TiO2 nanosheet film was formed as the working electrode (anode).
[0034] As shown in Figure 2, as the thickness of the protective film on the semiconductor photoelectrode became thinner, the initial photocurrent density increased but the characteristic retention rate decreased. On the other hand, as the thickness of the protective film on the semiconductor photoelectrode became thicker, the characteristic retention rate increased but the initial photocurrent density decreased. When the thickness of the protective film on the semiconductor photoelectrode was in the range of 2 to 5 nm, both the initial photocurrent density and the characteristic retention rate showed good values.
[0035] From the above results, it became clear that when the thickness of the protective film of the semiconductor photoelectrode is in the range of 2 to 5 nm, high light energy conversion efficiency and stability can be achieved.
[0036] The present invention is not limited to the above-described embodiments, but includes various modifications. For example, the above-described embodiments have been described in detail to clearly explain the present invention, and the present invention is not necessarily limited to those including all of the described configurations. Furthermore, it is possible to add, delete, and / or replace part of the configuration of each embodiment with other configurations.
Claims
1. MoS 2 and a protective film disposed on an upper surface of the semiconductor layer and made of one or more metal oxides selected from the group consisting of Ti oxides and Al oxides, wherein the protective film has a thickness in the range of 2 to 5 nm.
2. 2. The visible light responsive semiconductor photoelectrode according to claim 1, wherein the protective film is made of either a Ti oxide or an Al oxide.
3. The protective film is TiO 2 Or Al 2 O 3 2. The visible light responsive semiconductor photoelectrode according to claim 1, comprising any one of the following:
4. 2. The visible light responsive semiconductor photoelectrode according to claim 1, wherein the semiconductor layer has a thickness of 2 to 3 nm.
5. The semiconductor layer has a thickness of 2 to 3 nm, and the protective film is TiO 2 Or Al 2 O 3 2. The visible light responsive semiconductor photoelectrode according to claim 1, comprising any one of the following:
Citation Information
Patent Citations
Light energy conversion apparatus and semiconductor photoelectrode
JP2007239048A
Visible light responsive semiconductor photoelectrode
JP2014015642A
Photoelectrode for water decomposition and water decomposition apparatus
JP2015200016A
Thin film laminate, manufacturing method thereof, and water decomposition system
JP2017130634A
Semiconductor electrode, device therewith, and production method of semiconductor electrode
JP2018204094A