Polyvinyl chloride-based paste resin particle and modifier including the same

Polyvinyl chloride paste resin particles with sulfosuccinate and controlled particle size enhance polyurethane foam hardness and stability, addressing monomer-related issues in existing polymer polyols.

JP2024133806APending Publication Date: 2024-10-03TOSOH CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023043775
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing polymer polyols used in polyurethane foam production leave monomers in the polyol composition, leading to decreased physical properties and odor issues.

Method used

Polyvinyl chloride paste resin particles containing a specific amount of sulfosuccinate and having a defined average particle size are used as a modifier, enhancing polyurethane foam hardness and stability.

Benefits of technology

The polyvinyl chloride paste resin particles improve the hardness and processability of polyurethane foams, providing excellent compression properties and suitability as a modifier.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133806000001
    Figure 2024133806000001
Patent Text Reader

Abstract

To provide a polyvinyl chloride-based paste resin particle that enables the provision of urethane foam with superior compression hardness and has suitability as a polyurethane foam modifier.SOLUTION: A polyvinyl chloride-based paste resin particle contains a polyvinyl chloride resin and a surfactant. The polyvinyl chloride-based paste resin particle is a ground particle of dried material. Relative to 100 pts.mass of the polyvinyl chloride resin, the polyvinyl chloride-based paste resin particle contains 0.01-1.0 pt.mass of sulfosuccinate as the surfactant. The polyvinyl chloride-based paste resin particle has an average particle size of 0.1-15 μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polyvinyl chloride paste resin particles and a modifier comprising the same, and more particularly to polyvinyl chloride paste resin particles useful as a modifier for polyurethane, particularly for polyurethane foam having excellent hardness, and uses thereof. [Background technology]

[0002] Polyurethane foam is mainly produced by the reaction of isocyanate and polyol, and is used for a wide range of applications such as cushioning materials for vehicles and furniture, and insulation and structural materials for buildings, storage tanks, ships, etc. Polymer polyols have been proposed to improve the hardness properties of polyurethane foam.

[0003] As such polymer polyols, there have been proposed polymer polyols obtained by polymerizing an ethylenically unsaturated compound in a polyol containing a specific ratio of multiple polyols having specific functional groups, hydroxyl values, and terminal polyoxyethylene contents (see, for example, Patent Document 1), and polymer polyols obtained by polymerizing an ethylenically unsaturated compound in a polyol having a specific hydroxyl value (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 3-81314 [Patent Document 2] JP 2003-226734 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the polymer polyols proposed in Patent Documents 1 and 2, since monomers are polymerized in the polyol, the monomers remain in the polyol composition, which is one of the causes of deterioration in the physical properties and odor of polyurethane foams.

[0006] Therefore, there has been a demand for the development of polyurethane foams that can improve hardness properties without causing problems such as deterioration in physical properties and odor. [Means for solving the problem]

[0007] Means for Solving the Problems The present inventors have conducted intensive research into the above-mentioned problems and have found that polyvinyl chloride paste resin particles containing a specific amount of sulfosuccinate and having a specific average particle size are highly suitable as a modifier for polyurethane foams having excellent compression hardness, thereby completing the present invention.

[0008] That is, the present invention relates to polyvinyl chloride paste resin particles comprising a polyvinyl chloride resin and a surfactant, which are ground particles of a dried material, contain 0.01 to 1.0 part by mass of a sulfosuccinate salt as a surfactant per 100 parts by mass of the polyvinyl chloride resin, and have an average particle size of 0.1 to 15 μm.

[0009] The present invention will be described in detail below.

[0010] The polyvinyl chloride paste resin particles of the present invention contain 0.01 to 1.0 parts by mass of a sulfosuccinate salt as a surfactant relative to 100 parts by mass of polyvinyl chloride resin, and are, for example, pulverized particles of a dried product during recovery, and have an average particle size of 0.1 to 15 μm. The dried product before being made into pulverized particles can be obtained, for example, by subjecting a polymerization reaction solution or polymerization slurry after polymerization of a polyvinyl chloride resin to a drying process such as spray drying.

[0011] The sulfosuccinate constituting the polyvinyl chloride paste resin particles of the present invention acts, for example, as a surfactant during polymerization, and may be any salt as long as it belongs to the category of sulfosuccinates, and examples thereof include dipotassium sulfosuccinates such as polyoxyethylene alkyl dipotassium sulfosuccinates and polyoxyethylene alkyl ether dipotassium sulfosuccinates; potassium dialkyl sulfosuccinates, potassium polyoxyethylene lauryl ether sulfosuccinates, potassium dioctyl sulfosuccinates, and dioctyl sulfosuccinates. disodium salts of sulfosuccinic acid such as polyoxyethylene alkyl sulfosuccinic acid disodium salt and polyoxyethylene alkyl ether sulfosuccinic acid disodium salt; sodium salts of sulfosuccinic acid such as dialkyl sulfosuccinic acid sodium salt, polyoxyethylene lauryl ether sulfosuccinic acid sodium salt, dioctyl sulfosuccinic acid sodium salt, dioctyl sulfosuccinic acid sodium salt and dihexyl sulfosuccinic acid sodium salt; diammonium salts of sulfosuccinic acid, such as polyoxyethylene alkyl sulfosuccinic acid diammonium salt, polyoxyethylene alkyl ether sulfosuccinic acid diammonium salt; ammonium salts of sulfosuccinic acid, such as dialkyl ammonium salts of sulfosuccinic acid, polyoxyethylene lauryl ether sulfosuccinic acid ammonium salt, dioctyl ammonium salts of sulfosuccinic acid, dioctyl ammonium salts of sulfosuccinic acid, and dihexyl ammonium salts of sulfosuccinic acid; ditriethanol ammonium salts of sulfosuccinic acid, such as polyoxyethylene alkyl sulfosuccinic acid ditriethanol ammonium salt, and polyoxyethylene alkyl ether sulfosuccinic acid ditriethanol ammonium salt; triethanol ammonium salts of sulfosuccinic acid, such as dialkyl triethanol ammonium salts of sulfosuccinic acid, polyoxyethylene lauryl ether sulfosuccinic acid triethanol ammonium salt, dioctyl triethanol ammonium salts of sulfosuccinic acid, dioctyl triethanol ammonium salts of sulfosuccinic acid, and dihexyl triethanol ammonium salts of sulfosuccinic acid;Two or more of these may be mentioned, and among them, it is preferable to use one or more selected from dipotassium sulfosuccinate, disodium sulfosuccinate, diammonium sulfosuccinate, and ditriethanolammonium sulfosuccinate. The content is 0.01 to 1.0 parts by mass, and preferably 0.1 to 0.9 parts by mass, relative to 100 parts by mass of the polyvinyl chloride resin. Here, if the content of the sulfosuccinate is less than 0.01 parts by mass, the dispersion stability during polymerization becomes unstable, making it difficult to prepare particles. On the other hand, if the content exceeds 1.0 part by mass, the viscosity of the urethane-forming composition when preparing polyurethane foam becomes high, the processability becomes poor, and the suitability as a modifier for polyurethane foam decreases.

[0012] The vinyl chloride paste resin particles of the present invention are particles obtained by pulverizing a dried product obtained when a vinyl chloride resin is prepared as a vinyl chloride paste resin, and have an average particle size of 0.1 to 15 μm. Here, if the average particle size is less than 0.1 μm, the stability during preparation of polyurethane foam is poor, and the suitability as a modifier for polyurethane foam is reduced. On the other hand, if it is more than 15 μm or is an unpulverized product, the particle size is too large, which causes problems in foaming properties during foaming as polyurethane foam, and the suitability as a modifier for polyurethane foam is reduced. The average particle size in this case can be measured using any device, for example, a particle size distribution measuring device based on the principle of a commonly known laser diffraction method and a dynamic light scattering method, and can be measured using a particle size distribution measuring device such as a disk centrifugal particle size distribution measuring device (manufactured by CPS Instruments, (product name) CPS Disc Centrifuge).

[0013] The polyvinyl chloride paste resin particles of the present invention can impart excellent hardness properties when blended with polyurethane foam, and therefore can be used as a modifier for polyurethane foam.

[0014] As the method for producing the polyvinyl chloride paste resin particles of the present invention, any method may be used as long as it is possible to produce polyvinyl chloride paste resin particles that fall within the scope of the present invention, and for example, a method in which a polyvinyl chloride paste resin latex obtained by a polymerization method such as emulsion polymerization of vinyl chloride monomer, microsuspension polymerization, seed emulsion polymerization, seed microsuspension polymerization, etc., which are generally known as methods for producing polyvinyl chloride paste resins, is dried into a powder or granular polyvinyl chloride paste resin by a drying method such as spray drying, and then pulverized by a pulverizer, etc., can be mentioned. In this case, the sulfosuccinate is used as a surfactant, and may be added at any stage before the start of polymerization, during polymerization, or after the end of polymerization, and a polyvinyl chloride paste resin latex containing the sulfosuccinate can be obtained.

[0015] Examples of the vinyl chloride monomer include vinyl chloride monomer alone or a mixture of vinyl chloride monomer and a monomer copolymerizable with vinyl chloride monomer. Examples of the monomer copolymerizable with vinyl chloride monomer include vinyl esters such as vinyl acetate, vinyl propionate, vinyl myristate, vinyl benzoate, etc.; unsaturated carboxylic acids or anhydrides thereof such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, etc.; acrylic acid esters such as methyl acrylate, ethyl acrylate, butyl acrylate, etc.; methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, butyl methacrylate, etc.; unsaturated carboxylic acid esters such as maleic acid esters, fumaric acid esters, cinnamic acid esters, etc.; vinyl methyl ether, vinyl amyl ether, vinyl phenyl ethers; monoolefins such as ethylene, propylene, butene, pentene, etc.; vinylidene chloride, styrene and derivatives thereof, acrylonitrile, methacrylonitrile, etc.

[0016] As a method for recovering the polyvinyl chloride paste resin as a dry product from the polyvinyl chloride paste resin latex containing sulfosuccinate obtained by polymerization reaction, any method may be used as long as the polyvinyl chloride paste resin can be recovered. Among them, the method using spray drying is preferred because it can remove water from the latex efficiently and recover the polyvinyl chloride paste resin as a dry product. The dryer used for spray drying in this case may be a commonly used one, for example, various spray dryers described in Figure 4.10 on page 121 of "SPRAY DAYING HANDBOOK" (K.Masters, 3rd Edition, 1979, published by George Godwin Limited). As the drying temperature, which is a drying condition, for example, the dryer inlet temperature is 80 to 200°C, and the dryer outlet temperature is 40 to 70°C, preferably 45 to 65°C.

[0017] The polyvinyl chloride paste resin particles of the present invention can be obtained by pulverizing the dried polyvinyl chloride paste resin using a pulverizer such as a general mechanical pulverizer.

[0018] The polyvinyl chloride paste resin particles of the present invention can be blended as a modifier into a polyurethane foam-forming composition containing, for example, an isocyanate component (A), a polyol component (B), a catalyst (C), a blowing agent (D), a foam stabilizer (E), etc., to produce a polyurethane foam that can be used for various applications such as shock-absorbing materials for vehicles and furniture. The polyurethane foam-forming composition can provide a polyurethane foam, particularly an open-cell polyurethane foam, having excellent mechanical properties such as hardness.

[0019] The method for producing the polyurethane foam can be a method known for producing polyurethane foam, for example, a method of preparing a polyurethane foam-forming composition containing an isocyanate component (A), a polyol component (B), a catalyst (C), a blowing agent (D), a foam stabilizer (E), etc., and polyadding the isocyanate component (A) and the polyol component (B) to form a polyurethane while foaming, thereby producing a polyurethane foam, further a soft polyurethane foam, and an open-cell polyurethane foam, can be mentioned. When the polyvinyl chloride paste resin particles of the present invention are used as a polyurethane foam modifier, they may be used by any of the following methods: a method of blending the polyvinyl chloride paste resin particles with the isocyanate component (A) to produce an isocyanate component (A) composition, a method of blending the polyol component (B) to produce a polyol component (B) composition, and a method of blending the polyvinyl chloride paste resin particles with the polyurethane foam-forming composition.

[0020] Examples of the isocyanate constituting the isocyanate component (A) include compounds having at least two isocyanate groups, such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, tolidine diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, lysine diisocyanate, triphenylmethane triisocyanate, tetramethylxylene diisocyanate, 1, Examples of the isocyanate-containing prepolymers include 6-hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, isophorone diisocyanate, 1,4-cyclohexane diisocyanate, norbornane diisocyanate, lysine ester triisocyanate, 1,6,11-undecane triisocyanate, 1,8-diisocyanate-4-isocyanate methyloctane, 1,3,6-hexamethylene triisocyanate, bicycloheptane triisocyanate, trimethylhexamethylene diisocyanate, isocyanate-containing prepolymers obtained by reacting these with polyols, and mixtures of two or more of these. Further examples include modified products of these isocyanates (modified products containing a urethane group, a carbodiimide group, an allophanate group, a urea group, a biuret group, an isocyanurate group, an amide group, an imide group, a uretonimine group, a uretdione group, or an oxazolidone group) and condensates (sometimes called polynuclear products) such as polymethylene polyphenylene polyisocyanate (polymeric MDI). Among these, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, and modified products thereof are preferred, as they give flexible polyurethane foams with excellent flexibility and compression hardness.

[0021] The polyol constituting the polyol component (B) may be any polyol that can form polyurethane by polyaddition with isocyanate, and it belongs to the category called polyol. For example, conventionally known polyether polyol, polyester polyol, polycarbonate polyol, polymer polyol, etc. can be mentioned. Among them, at least one selected from the group consisting of polyether polyol and polyester polyol is preferable because it is a soft polyurethane foam with excellent flexibility and compression hardness. Furthermore, it is more preferable that the number average molecular weight is 1000 to 10000 and the nominal functionality is 2 or more because it is a foam with excellent compression set, which is an index of hardness and durability. The nominal functionality indicates the theoretical average functionality (the number of active hydrogen atoms per molecule) when it is assumed that no side reaction occurs during the polymerization reaction of the polyol.

[0022] The polyether polyol is not particularly limited, and examples thereof include those produced by an addition reaction of a compound having at least two active hydrogen groups (examples include polyhydric alcohols such as ethylene glycol, propylene glycol, glycerin, trimethylolpropane, and pentaerythritol; amines such as ethylenediamine; and alkanolamines such as ethanolamine and diethanolamine) as a starting material with an alkylene oxide (examples include ethylene oxide and propylene oxide) (see, for example, the method described in Gunter Oertel, "Polyurethane Handbook" (1985) Hanser Publishers (Germany), pp. 42-53).

[0023] The polyester polyol is not particularly limited, and examples thereof include those obtained by reacting a dibasic acid with a glycol, such as a polyester polyol made of adipic acid and ethylene glycol, which is a polycondensation type polyester polyol, polycaprolactone polyol, which is a lactone type polyester polyol, and polyester polyols derived from the processing of waste materials during nylon production, waste trimethylolpropane, waste pentaerythritol, waste phthalic acid polyesters, and waste products (see, for example, the description in "Polyurethane Resin Handbook" by Iwata Keiji (1987), published by the Nikkan Kogyo Shimbun, p. 117).

[0024] The polymer polyol is not particularly limited, and examples thereof include polymer polyols obtained by reacting the above-mentioned polyether polyol with an ethylenically unsaturated monomer (e.g., butadiene, acrylonitrile, styrene, etc.) in the presence of a radical polymerization catalyst.

[0025] Commercially available examples of these polyols include Sannix (trade name, manufactured by Sanyo Chemical Industries, Ltd.), Exenol (trade name, manufactured by Asahi Glass Co., Ltd.), Actcoal (trade name, manufactured by Mitsui Chemicals Polyurethanes, Inc.), and VORANOL (trade name, manufactured by Dow).

[0026] In addition, since the polyvinyl chloride paste resin particles of the present invention are easy to handle when preparing polyurethane foam, they are preferably handled as a polyol composition in which they are dispersed in a polyol component (B), and may also be a polyol composition in which a catalyst (C), a blowing agent (D), a foam stabilizer (E), etc. are further dispersed.

[0027] Examples of the catalyst (C) include various types of urethane catalysts, such as triethylamine, tripropylamine, tributylamine, N-methylmorpholine, N-ethylmorpholine, dimethylbenzylamine, N,N,N',N'-tetramethylhexamethylenediamine, N,N,N',N',N''-pentamethyldiethylenetriamine, bis-(2-dimethylaminoethyl)ether, triethylenediamine, 1,8-diaza-bicyclo[5.4.0]undecene-7, 1,2-dimethylimidazole, 1-isobutyl-2-methylimidazole, and further. Examples of the catalyst (C) include organic acid salts of these compounds; organometallic compounds such as stannous octoate and zinc naphthenate; and amine catalysts having active hydrogen such as dimethylethanolamine, N,N-dimethyl-N-hexanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, hydroxymethyltriethylenediamine, and N,N,N'-trimethyl-N'-hydroxyethyl-bisaminoethylether; and among these, triethylamine, tripropylamine, tributylamine, and triethylenediamine are preferred because they are excellent in urethane-forming reactivity and foaming properties. The amount of the catalyst (C) is preferably 0.01 to 10 parts by mass relative to 100 parts by mass of the polyol component (B) because it is possible to efficiently obtain a flexible polyurethane foam with excellent foaming properties.

[0028] As the blowing agent (D), various known blowing agents can be used, and among them, water can be used as a blowing agent for polyurethane foam, because it generates carbon dioxide gas by reacting with isocyanate groups and enables carbon dioxide gas foaming by the carbon dioxide gas. Any blowing agent may be used in addition to water, and examples of such blowing agents include low-boiling organic compounds such as cyclopentane and isopentane. Furthermore, air, nitrogen gas, or liquefied carbon dioxide can be mixed and dissolved in the raw solution using a gas loading device to foam the mixture. When water is used as the blowing agent (D), the amount of water is preferably 0.5 to 10 parts by mass, particularly 1.0 to 8.0 parts by mass, and more preferably 2.0 to 8.0 parts by mass, relative to 100 parts by mass of the polyol component (B), because it is easy to provide a stable foam with a low apparent density.

[0029] As the foam stabilizer (E) which may be used in some cases, a normal surfactant is used, and an organosilicon-based surfactant can be preferably used, for example, (trade names) SRX-280A, SZ-1327, SZ-1325, SZ-1336, SZ-3601 (manufactured by Toray Dow Corning Co., Ltd.); (trade names) Y-10366, L-3620 (manufactured by Momentive Corporation), (trade names) B-8724LF2, B-8715LF2 (manufactured by Evonik Co., Ltd.); (trade name) F-122 (manufactured by Shin-Etsu Chemical Co., Ltd.), and the like. The blending amount of these foam stabilizers (F) is preferably 0.1 to 3 parts by mass per 100 parts by mass of the polyol component (B).

[0030] Furthermore, anti-settling agents and, if necessary, various known additives such as foam breakers, antioxidants, ultraviolet absorbers, plasticizers, pigments, dyes, antibacterial agents, antifungal agents, etc. can be used.

[0031] The ratio of the isocyanate component (A) to the polyol component (B) when preparing the polyurethane foam-forming composition may be any ratio, and in particular, the molar ratio of all isocyanate groups to all active hydrogen groups including water (NCO / active hydrogen) is preferably 0.7 to 1.4 (isocyanate index (NCOINDEX)=70 to 140) in order to efficiently obtain a flexible polyurethane foam having interconnected cells, and more preferably 0.7 to 1.2 (NCOINDEX=70 to 120) in order to obtain a good range for foam durability and molding cycle.

[0032] Examples of methods for producing polyurethane foams include those which involve subjecting the polyurethane foam-forming composition, particularly the flexible polyurethane foam-forming composition, to known foaming methods such as slab foaming, injection mold foaming, spray foaming, and continuous production panel foaming. The polyurethane foam-forming composition can be used in a variety of general applications, such as insulating materials and structural materials in architecture and civil engineering; insulating materials for freezers, refrigerators, freezer showcases, and the like in electrical equipment; insulating materials for LPG, LNG tankers, and pipelines in plants and ships; insulating materials for refrigerators and refrigerated cars in vehicles; and also as seats, cushioning materials, sound absorbing materials, vibration damping materials, construction flooring materials, and the like for bedding, automobiles, and the like, and particularly as seats and cushioning materials for bedding, automobiles, and the like. Effect of the Invention

[0033] The present invention provides vinyl chloride paste resin particles which have a specific particle size and contain a sulfosuccinate, thereby making it possible to provide a polyurethane foam having excellent compression hardness. The polyurethane foam, particularly a flexible polyurethane foam, is used in applications such as automobile seats, bedding, and cushioning materials. EXAMPLES

[0034] The present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.

[0035] The raw materials used in the examples and comparative examples are as follows: Polyol A: polyether polyol (manufactured by AGC Corporation, (product name) EL-840: functionality 3, hydroxyl value 26 mgKOH / g). Blowing agent A: Water. Foam stabilizer A: Silicone-based surfactant (manufactured by Momentive, (product name) L-3620). Catalyst A: a dipropylene glycol solution of triethylenediamine (manufactured by Tosoh Corporation, product name TEDA-L33). Catalyst B: a dipropylene glycol solution of bis(2-dimethylaminoethyl)ether (manufactured by Tosoh Corporation, product name: TOYOCAT-ET). Isocyanate: diphenylmethane diisocyanate (manufactured by Tosoh Corporation, (trade name) C-1331, NCO content = 31.5%). Modifier: Polyvinyl chloride paste resin particles.

[0036] The methods for evaluating the polyvinyl chloride paste resin particles and polyurethane foams obtained in the examples are described below.

[0037] <Average particle size> The measurement was performed using a disk centrifugal particle size distribution measuring device (manufactured by CPS Instruments, product name: CPS Disc Centrifuge).

[0038] <Method for preparing polyurethane foam-forming composition> At room temperature (20 to 25°C), 0.40 parts by mass of catalyst A, 0.12 parts by mass of catalyst B, 1 part by mass of foam stabilizer A, 3.2 parts by mass of blowing agent A, and 10.5 parts by mass of modifier A were mixed with 100 parts by mass of polyol A to prepare a polyol composition, and the temperature was adjusted to 20°C. Then, 55.6 parts by mass of isocyanate adjusted to 20°C was added with respect to 100 parts by mass of polyol A, and the mixture was stirred and mixed at a stirring speed of 7000 rpm for 7 seconds to prepare a polyurethane foam-forming composition, which was then poured into a mold to foam a flexible polyurethane foam, and then removed from the mold, and the physical properties of the resulting flexible polyurethane foam were measured.

[0039] <Moldability evaluation> In the table, a moldability rating of "○" means that a flexible polyurethane foam could be molded without any collapse (the polyurethane foam sinking significantly after reaching its maximum height) or shrinkage of the produced polyurethane foam immediately after foaming or after curing.

[0040] <Apparent density> It was determined according to the method described in JIS K6400.

[0041] <25% Compressive Hardness (25% ILD) of Skinned Specimen Form> It was determined according to JIS K6400 Method B.

[0042] <Compressive residual strain> The measurement was performed according to the method described in JIS K6400.

[0043] Synthesis Example 1 (Production Example of Seed Latex Containing Polymerization Initiator, etc.) 1m 3 In an autoclave, 360 kg of deionized water, 300 kg of vinyl chloride monomer, 6 kg of lauroyl peroxide, and 30 kg of 15% by mass aqueous solution of sodium dodecylbenzenesulfonate were charged, and the mixture was circulated for 2 hours using a homogenizer. After homogenization, the temperature was raised to 45° C. to proceed with polymerization. After the pressure had dropped by 0.2 MPa from the saturated vapor pressure of vinyl chloride at 45° C., the unreacted vinyl chloride monomer was recovered to prepare a seed latex containing a polymerization initiator, etc.

[0044] Example 1 1m 3After 400 kg of deionized water was put into the autoclave, the space in the autoclave was replaced with nitrogen, the pressure was reduced, and 400 kg of vinyl chloride monomer, 4.5 kg of 7.5 mass% polyoxyethylene alkyl sulfosuccinic acid disodium salt aqueous solution, 0.002 kg of copper sulfate were added, and 50 kg of the seed latex containing the polymerization initiator and the like obtained in Synthesis Example 1 was added. The temperature of this reaction mixture was raised to 49.6°C, and 16 kg of 0.1 mass% ascorbic acid aqueous solution was continuously added throughout the entire polymerization time. Furthermore, from the start of polymerization to the end of polymerization, 0.4 parts by mass of 7.5 mass% polyoxyethylene alkyl sulfosuccinic acid disodium salt aqueous solution per 100 parts by mass of vinyl chloride monomer was continuously added in total. The polymerization was stopped when the polymerization pressure dropped by 0.1 MPa from the saturated vapor pressure of the vinyl chloride monomer at 49.6°C, and the unreacted vinyl chloride monomer was recovered. The obtained polyvinyl chloride paste resin latex was spray-dried in a spray dryer with hot air inlet at 160°C and outlet at 55°C, and then pulverized to obtain polyvinyl chloride paste resin particles.

[0045] The polyvinyl chloride paste resin particles obtained had an average particle diameter of 3.1 μm and contained 0.8 parts by mass of polyoxyethylene alkyl sulfosuccinic acid disodium salt per 100 parts by mass of polyvinyl chloride resin. The above-mentioned polyurethane foam-forming composition was prepared using the obtained polyvinyl chloride paste resin particles, and a flexible polyurethane foam having open cells was obtained and its physical properties were evaluated. The results are shown in Table 1.

[0046] Example 2 1m 3After 400 kg of deionized water was put into the autoclave, the space in the autoclave was replaced with nitrogen, the pressure was reduced, and 400 kg of vinyl chloride monomer, 4.5 kg of 7.5 mass% polyoxyethylene alkyl sulfosuccinic acid disodium salt aqueous solution, 0.002 kg of copper sulfate were added, and 73.1 kg of the seed latex containing the polymerization initiator obtained in Synthesis Example 1 was added. The temperature of this reaction mixture was raised to 49.6°C, and 16 kg of 0.1 mass% ascorbic acid aqueous solution was continuously added throughout the entire polymerization time. Furthermore, from the start of polymerization to the end of polymerization, 0.4 parts by mass of 7.5 mass% polyoxyethylene alkyl sulfosuccinic acid disodium salt aqueous solution per 100 parts by mass of vinyl chloride monomer was continuously added in total. The polymerization was stopped when the polymerization pressure dropped by 0.1 MPa from the saturated vapor pressure of the vinyl chloride monomer at 49.6°C, and the unreacted vinyl chloride monomer was recovered. The obtained polyvinyl chloride paste resin latex was spray-dried in a spray dryer with hot air inlet at 160°C and outlet at 55°C, and then pulverized to obtain polyvinyl chloride paste resin particles.

[0047] The polyvinyl chloride paste resin particles obtained had an average particle diameter of 3.0 μm and contained 0.8 parts by mass of polyoxyethylene alkyl sulfosuccinic acid disodium salt per 100 parts by mass of polyvinyl chloride resin. The above-mentioned polyurethane foam-forming composition was prepared using the obtained polyvinyl chloride paste resin particles, and a flexible polyurethane foam having open cells was obtained and its physical properties were evaluated. The results are shown in Table 1.

[0048] Comparative Example 1 1m 3After 300 kg of deionized water was put into the autoclave, the space in the autoclave was replaced with nitrogen, the pressure was reduced, and 400 kg of vinyl chloride monomer, 10 kg of 15% by mass sodium dodecylbenzenesulfonate aqueous solution, 0.002 kg of copper sulfate, and 54 kg of the seed latex containing the polymerization initiator and the like obtained in Synthesis Example 1 were added, and the temperature of this reaction mixture was raised to 53°C, while 16 kg of 0.1% by mass aqueous ascorbic acid solution was continuously added throughout the entire polymerization time. Furthermore, from the start of polymerization to the end of polymerization, 0.6 parts by mass of a 15% by mass sodium dodecylbenzenesulfonate aqueous solution per 100 parts by mass of vinyl chloride monomer was continuously added in total. When the polymerization pressure dropped by 0.1 MPa from the saturated vapor pressure of the vinyl chloride monomer at 53°C, the polymerization was stopped, and the unreacted vinyl chloride monomer was recovered. The obtained polyvinyl chloride paste resin latex was spray-dried in a spray dryer with hot air inlet at 160°C and outlet at 55°C, and then pulverized to obtain a polyvinyl chloride paste resin.

[0049] The polyvinyl chloride paste resin obtained had an average particle size of 8.4 μm and contained 0.8 parts by mass of sodium dodecylbenzenesulfonate per 100 parts by mass of polyvinyl chloride resin. The above-mentioned polyurethane foam-forming composition was prepared using the obtained polyvinyl chloride paste resin, a polyurethane foam was obtained, and the physical properties were evaluated. The results are shown in Table 1. The obtained polyurethane foam was inferior in compression hardness and compression set compared to Examples 1 and 2.

[0050] Comparative Example 2 1m 3After 300 kg of deionized water was put into the autoclave, the space in the autoclave was replaced with nitrogen, the pressure was reduced, and 400 kg of vinyl chloride monomer, 10 kg of 15% by mass sodium lauryl sulfate aqueous solution, 0.002 kg of copper sulfate, and 54 kg of the polymerization initiator-containing seed obtained in Synthesis Example 1 were added. The temperature of this reaction mixture was raised to 48°C, and 16 kg of 0.1% by mass aqueous ascorbic acid solution was continuously added throughout the entire polymerization time. Furthermore, from the start of polymerization to the end of polymerization, a total of 0.6 parts by mass of 15% by mass sodium lauryl sulfate aqueous solution was continuously added per 100 parts by mass of vinyl chloride monomer. When the polymerization pressure dropped by 0.1 MPa from the saturated vapor pressure of vinyl chloride monomer at 48°C, the polymerization was stopped, and unreacted vinyl chloride monomer was recovered. The obtained polyvinyl chloride paste resin latex was spray-dried in a spray dryer at a hot air inlet temperature of 160°C and an outlet temperature of 55°C, and then pulverized to obtain a polyvinyl chloride paste resin.

[0051] The obtained polyvinyl chloride paste resin had an average particle size of 3.3 μm and contained 0.8 parts by mass of sodium lauryl sulfate per 100 parts by mass of polyvinyl chloride resin. The above-mentioned polyurethane foam-forming composition was prepared using the obtained polyvinyl chloride paste resin, a polyurethane foam was obtained, and the physical properties were evaluated. The results are shown in Table 1. The obtained polyurethane foam was inferior in compression hardness and compression set compared to Examples 1 and 2.

[0052] Comparative Example 3 1m 3After 300 kg of deionized water was put into the autoclave, the space in the autoclave was replaced with nitrogen, the pressure was reduced, and 400 kg of vinyl chloride monomer, 10 kg of 15% by mass sodium lauryl sulfate aqueous solution, 0.002 kg of copper sulfate, and 54 kg of the polymerization initiator-containing seed obtained in Synthesis Example 1 were added. The temperature of this reaction mixture was raised to 54°C, and 16 kg of 0.1% by mass ascorbic acid aqueous solution was continuously added throughout the entire polymerization time. Furthermore, from the start of polymerization to the end of polymerization, a total of 0.6 parts by mass of 15% by mass sodium lauryl sulfate aqueous solution was continuously added per 100 parts by mass of vinyl chloride monomer. When the polymerization pressure dropped by 0.1 MPa from the saturated vapor pressure of vinyl chloride monomer at 54°C, the polymerization was stopped, and unreacted vinyl chloride monomer was recovered. The obtained polyvinyl chloride paste resin latex was spray-dried with a spray dryer at a hot air inlet temperature of 110°C and an outlet temperature of 50°C to obtain a polyvinyl chloride paste resin.

[0053] The polyvinyl chloride paste resin thus obtained had an average particle size of 62 μm and an average degree of polymerization of 1200, and contained 0.8 parts by mass of sodium lauryl sulfate per 100 parts by mass of polyvinyl chloride resin. The above-mentioned polyurethane foam-forming composition was prepared using the polyvinyl chloride paste resin thus obtained, but the foam collapsed during foaming, making it impossible to evaluate its physical properties.

[0054] Comparative Example 4 A polyurethane foam-forming composition was prepared in the same manner except that no polyvinyl chloride paste resin particles were added, a polyurethane foam was obtained, and its physical properties were evaluated. The results are shown in Table 1. The obtained polyurethane foam was inferior to Examples 1 and 2 in compression hardness and compression set.

[0055] [Table 1] [Industrial Applicability]

[0056] The present invention provides polyvinyl chloride paste resin particles which can be used as a modifier to provide polyurethane foam, particularly soft polyurethane foam, having excellent compression hardness. The polyvinyl chloride paste resin particles are expected to be suitably used in the polyurethane and polyurethane foam manufacturing industry, and further as products thereof.

Claims

1. The polyvinyl chloride paste resin particles contain a polyvinyl chloride resin and a surfactant, the polyvinyl chloride paste resin particles being ground particles of a dried material, the polyvinyl chloride paste resin particles containing 0.01 to 1.0 part by mass of a sulfosuccinate salt as a surfactant relative to 100 parts by mass of the polyvinyl chloride resin, and having an average particle size of 0.1 to 15 μm.

2. 2. The polyvinyl chloride paste resin particle according to claim 1, characterized in that the sulfosuccinate is at least one selected from the group consisting of dipotassium sulfosuccinate, disodium sulfosuccinate, diammonium sulfosuccinate, and ditriethanolammonium sulfosuccinate.

3. 3. The polyvinyl chloride paste resin particles according to claim 1, wherein the dried product is a spray-dried product.

4. A modifier for polyurethane foam, comprising the polyvinyl chloride paste resin particles according to claim 1.

5. 2. A polyurethane foam, which is a foam of a polyurethane foam-forming composition comprising at least an isocyanate component, a polyol component, a blowing agent, and the polyvinyl chloride paste resin particles according to claim 1.

Citation Information

Patent Citations

  • Production of highly resilient polyurethane foam