Silane cross-linkable resin composition, silane cross-linked resin molding and method for manufacturing them, and molded article
A silane crosslinking method using organic peroxide and inorganic fillers achieves a silane crosslinked resin with enhanced heat resistance, tensile strength, and flexibility, addressing the needs of outdoor molded products for long-term insulation and tracking resistance.
Patent Information
- Application Number
- JP2023043805
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Molded products used outdoors, such as coating layers on outdoor wiring materials, require high heat resistance, mechanical properties, long-term insulation, tracking resistance, deliquescence resistance, and flexibility, which existing silane crosslinking methods fail to adequately address.
A specific silane crosslinking method using a combination of organic peroxide, inorganic fillers, and a silane coupling agent in a controlled ratio, along with a silanol condensation catalyst, to create a silane crosslinked resin composition that maintains excellent heat resistance, tensile strength, and flexibility while providing long-term insulation and tracking resistance.
The method produces a silane crosslinked resin molded article with balanced properties of heat resistance, tensile strength, long-term insulation, tracking resistance, and deliquescence resistance, suitable for outdoor applications.
Smart Images

Figure 2024133824000001 
Figure 2024133824000002 
Figure 2024133824000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a silane-crosslinkable resin composition, a silane-crosslinked resin molded article, a method for producing the same, and a molded article. [Background technology]
[0002] Various resin or rubber molded products are used as coating layers (insulators, sheaths, etc.) provided on wiring materials such as insulated wires, cables, cords, optical fiber cores, and optical fiber cords (optical fiber cables) used in the fields of electric and electronic equipment and industry, and as various molded products such as packings, sheets, etc. Various properties are required for such molded products depending on the application and mode of use, such as appearance properties, strength (e.g. tensile strength), and further, for coating layers for wiring materials, heat resistance, etc. are required from the viewpoint of safety and reliability. For such molded products, compositions (molded bodies) containing inorganic fillers and chemically crosslinked resins or rubbers are used. Electron beam crosslinking, chemical crosslinking, etc. are used as methods for crosslinking resins or rubbers. Among chemical crosslinking methods, the silane crosslinking method is advantageous in terms of production compared to other crosslinking methods because it does not require special equipment in the crosslinking process.
[0003] Various molded articles containing inorganic fillers and silane-crosslinked with resins and the like (silane crosslinking method of resins and the like) and methods for producing the same have been studied, and examples of such molded articles and methods for producing the same are described in Patent Documents 1 to 3. Specifically, Patent Documents 1 and 2 describe a silane crosslinking method and a silane-crosslinked resin molded article using hydroxides such as aluminum hydroxide and magnesium hydroxide, calcium carbonate, and the like, either alone or in combination, as suitable inorganic fillers that can also function as flame retardants. Meanwhile, Patent Document 3 describes a silane crosslinking method and a silane-crosslinked resin molded article using boehmite alone as an inorganic filler that can solve the problems of aluminum hydroxide. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2015 / 046477 [Patent Document 2] International Publication No. 2015 / 046478 [Patent Document 3] JP 2017-179235 A Summary of the Invention [Problem to be solved by the invention]
[0005] Among molded products, in particular, molded products used outdoors, for example, coating layers provided on outdoor wiring materials, are required to have, in addition to heat resistance and mechanical properties (tensile strength), a property of maintaining high insulation resistance for a long period of time (sometimes referred to as long-term insulation properties), a property of suppressing the occurrence of tracking phenomenon (sometimes referred to as tracking resistance), deliquescence resistance (also referred to as acid resistance), flexibility, etc. However, Patent Documents 1 to 3 do not consider the above points of view.
[0006] An object of the present invention is to provide a silane-crosslinked resin molded article that maintains excellent heat resistance and tensile strength while also having long-term insulating properties, tracking resistance, deliquescence resistance and flexibility, and a method for producing the same. Another object of the present invention is to provide a silane-crosslinkable resin composition capable of forming a silane-crosslinked resin molded article having all of the above-mentioned excellent properties, and a method for producing the same. A further object of the present invention is to provide a molded article containing a silane-crosslinked resin molded article having all of the above-mentioned excellent properties. [Means for solving the problem]
[0007] The present inventors have found that, in a specific silane crosslinking method using an organic peroxide in a specific ratio, a silane coupling agent in a specific ratio and an inorganic filler in a specific ratio of a combination of metal carbonate, boehmite, silica, etc. in a total mixture amount of 100 to 150 parts by mass per 100 parts by mass of a base resin having a specific composition containing at least one of a polyolefin resin and an ethylene rubber can be used to realize a silane crosslinked resin molded body that maintains excellent heat resistance and tensile strength while also having long-term insulation properties, tracking resistance, deliquescence resistance, and flexibility. Based on this finding, the present inventors have further studied and have come up with the present invention.
[0008] That is, the object of the present invention has been achieved by the following means. <1> A method for producing a silane-crosslinkable resin composition, comprising: (1) melt-mixing 0.01 to 0.3 parts by mass of an organic peroxide, 100 to 150 parts by mass of an inorganic filler, 2 to 10 parts by mass of a silane coupling agent, and a silanol condensation catalyst relative to 100 parts by mass of a base resin to obtain a mixture, the base resin contains at least one of a polyolefin resin and an ethylene rubber, and contains the polyolefin resin in an amount of 100% by mass or less, the ethylene rubber in an amount of 100% by mass or less, a styrene-based elastomer in an amount of 35% by mass or less, and an oil in an amount of 40% by mass or less; The inorganic filler contains 10 to 35 parts by mass of metal carbonate, 20 to 55 parts by mass of boehmite, and 45 to 90 parts by mass of silica and / or calcined clay, within the range of the mixing amount of the inorganic filler, A method for producing a silane-crosslinkable resin composition, wherein, in carrying out the step (1), when the whole of the base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), and (c) below, while, in the case where only a part of the base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), (b), and (c) below. Step (a-1): Mixing the inorganic filler and the silane coupling agent. A process for preparing a product Step (a-2): The mixture and all or a part of the base resin are mixed with the organic peroxide. In the presence of the organic peroxide, at a temperature equal to or higher than the decomposition temperature of the organic peroxide, Melt mixing to prepare a silane master batch. Step (b): Melt-mixing the remainder of the base resin and the silanol condensation catalyst to form a catalyst. A process for preparing a catalyst master batch Step (c): The silane master batch and the silanol condensation catalyst or the catalyst master batch are mixed. A process of melt mixing with the star batch. <2> A method for producing a silane-crosslinked resin molded product, comprising the following steps (1), (2) and (3): Step (1): 0.01 to 0.3 parts by mass of an organic peroxide relative to 100 parts by mass of a base resin 100 to 150 parts by mass of inorganic filler, and 2 parts by mass of silane coupling agent. and a silanol condensation catalyst to obtain a mixture. Process Step (2): A step of molding the mixture obtained in step (1) to obtain a molded body. Step (3): The molded body obtained in step (2) is contacted with water to form a silane-crosslinked resin compound. The process of obtaining a shape the base resin contains at least one of a polyolefin resin and an ethylene rubber, and contains the polyolefin resin in an amount of 100% by mass or less, the ethylene rubber in an amount of 100% by mass or less, a styrene-based elastomer in an amount of 35% by mass or less, and an oil in an amount of 40% by mass or less; The inorganic filler contains 10 to 35 parts by mass of metal carbonate, 20 to 55 parts by mass of boehmite, and 45 to 90 parts by mass of silica and / or calcined clay, within the range of the mixing amount of the inorganic filler, A method for producing a silane-crosslinked resin molded product, wherein, in carrying out the step (1), when the entire base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), and (c) below, while, in the case where only a part of the base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), (b), and (c) below. Step (a-1): Mixing the inorganic filler and the silane coupling agent. A process for preparing a product Step (a-2): The mixture and all or a part of the base resin are mixed with the organic peroxide. In the presence of the organic peroxide, at a temperature equal to or higher than the decomposition temperature of the organic peroxide, Melt mixing to prepare a silane master batch. Step (b): Melt-mixing the remainder of the base resin and the silanol condensation catalyst to form a catalyst. A process for preparing a catalyst master batch Step (c): The silane master batch and the silanol condensation catalyst or the catalyst master batch are mixed. A process of melt mixing with the star batch. <3> The base resin contains 50% by mass or less of a polyolefin resin, 10 to 100% by mass of an ethylene rubber, 35% by mass or less of a styrene-based elastomer, and 40% by mass or less of an oil. <1> The manufacturing method described in <4> The base resin contains 50% by mass or less of a polyolefin resin, 10 to 100% by mass of an ethylene rubber, 35% by mass or less of a styrene-based elastomer, and 40% by mass or less of an oil. <2> The manufacturing method described in <5> The base resin contains 20 to 40 mass% of a polyolefin resin, 10 to 45 mass% of an ethylene rubber, 10 to 35 mass% of a styrene-based elastomer, and 20 to 40 mass% of an oil. <1> or <3> The manufacturing method described in <6> The base resin contains 20 to 40 mass% of a polyolefin resin, 10 to 45 mass% of an ethylene rubber, 10 to 35 mass% of a styrene-based elastomer, and 20 to 40 mass% of an oil. <2> or <4> The manufacturing method described in <7> the above <1> , <3> and <5> 13. A silane-crosslinkable resin composition produced by the method according to any one of claims 1 to 12. <8> the above <2> , <4> and <6> 13. A silane-crosslinked resin molded article produced by the method according to any one of claims 1 to 12. <9> the above <8> A molded article comprising the silane-crosslinked resin molded article according to claim 1. Effect of the Invention
[0009] The present invention can provide a silane-crosslinked resin molded article that maintains excellent heat resistance and tensile strength while also exhibiting long-term insulating properties, tracking resistance, deliquescence resistance and flexibility, and a method for producing the same. The present invention also provides a silane-crosslinkable resin composition capable of forming a silane-crosslinked resin molded article having all of the above-mentioned excellent properties, and a method for producing the same. Furthermore, the present invention can provide a molded article containing a silane-crosslinked resin molded article having all of the above-mentioned excellent properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] In the present invention, when the content, physical properties, etc. of a component are described by showing a numerical range, and when the upper limit and lower limit of the numerical range are described separately, any of the upper limit and lower limit can be appropriately combined to form a specific numerical range. On the other hand, when multiple numerical ranges expressed using "~" are set and described, the upper limit and lower limit forming the numerical range are not limited to the specific combination described before and after "~" as a specific numerical range, and can be a numerical range obtained by appropriately combining the upper limit and lower limit of each numerical range. In addition, in the present invention, a numerical range expressed using "~" means a range including the numerical values described before and after "~" as the upper limit and lower limit. In the present invention, "(meth)acrylic acid" refers to either or both of acrylic acid and methacrylic acid, and "(meth)acrylic acid ester" refers to either or both of acrylic acid ester and methacrylic acid ester.
[0011] [Silane-crosslinkable resin composition] The silane crosslinkable resin composition (sometimes referred to as the silane crosslinkable resin composition of the present invention for convenience) preferably produced by the method for producing the silane crosslinkable resin composition of the present invention contains at least one of polyolefin resin and ethylene rubber, and contains 100 mass parts of a base resin containing 100 mass % or less of polyolefin resin, 100 mass % or less of ethylene rubber, 35 mass % or less of styrene-based elastomer, and 40 mass % or less of oil, and contains 2 to 10 mass parts of a silane coupling agent grafted to the base resin, 100 to 150 mass parts of an inorganic filler, and a silanol condensation catalyst. Here, the inorganic filler contains 10 to 35 mass parts of a metal carbonate, 20 to 55 mass parts of boehmite, and 45 to 90 mass parts of silica and / or calcined clay, within the range of 100 to 150 mass parts, which is the mixed amount (also referred to as the total mixed amount or total content) of the inorganic filler. This silane-crosslinkable resin composition can also be prepared by appropriately mixing the above-mentioned components, other than by the method for producing the silane-crosslinkable resin composition of the invention.
[0012] Although details will be described later, the silane crosslinkable resin composition of the present invention contains, together with an inorganic filler, a silane crosslinkable resin in which a silane coupling agent bonded or dissociated with an inorganic filler and a base resin are graft-bonded (grafting reaction).
[0013] This silane crosslinkable resin composition can induce a silanol condensation reaction under mild conditions without the need for special crosslinking equipment such as a chemical crosslinking tube or an electron beam crosslinking machine, and can produce a silane crosslinked resin molded article excellent in heat resistance, tensile strength, long-term insulation properties, tracking resistance, deliquescence resistance, and flexibility with excellent manufacturability. In addition, a silane crosslinked resin molded article excellent in appearance can be produced while maintaining the above-mentioned excellent properties. Therefore, the silane crosslinkable resin composition is suitably used in the method for producing a silane crosslinked resin molded article of the present invention or the silane crosslinked resin molded article of the present invention.
[0014] [Silane cross-linked resin molded body] The silane-crosslinked resin molded article (which may be conveniently referred to as the silane-crosslinked resin molded article of the present invention) that is suitably produced by the method for producing a silane-crosslinked resin molded article of the present invention is a crosslinked resin molded article (a molded article made of a silanol condensate of the silane-crosslinkable resin composition) obtained by subjecting the silane-crosslinkable resin composition of the present invention to silane crosslinking (silanol condensation reaction) after molding.
[0015] Although the details will be described later, the silane-crosslinked resin molded article of the present invention has a crosslinked structure in which the base resin is silane-crosslinked (a crosslinked structure via a silane coupling agent or a silanol condensate thereof). It is considered that an inorganic filler is incorporated into a part of this crosslinked structure, as described later. Therefore, the silane-crosslinked resin molded article of the present invention has a well-balanced structure between the base resins (not via the inorganic filler) and the crosslinked structure involving the inorganic filler, as described later, and exhibits a well-balanced heat resistance, tensile strength, long-term insulation properties, tracking resistance, deliquescence resistance, and flexibility. The silane-crosslinked resin molded article of the present invention is molded into an appropriate shape and size depending on the application, for example, the application of the molded article of the present invention described below.
[0016] Each component used in the present invention will now be described. Each of the components may be used alone or in combination of two or more.
[0017] <Base resin> The base resin used in the present invention contains at least one of polyolefin resin and ethylene rubber as essential components, contains styrene-based elastomer and / or oil as preferred components, and may further contain other resins or various rubbers as optional components. In the present invention, even when the molded body and composition contain ethylene rubber, they are referred to as resin molded body, resin composition, etc. for convenience, but this does not exclude rubber molded body and rubber composition from the technical scope of the present invention. The base resin contains at least one of polyolefin resin and ethylene rubber, and contains 100% by mass or less of polyolefin resin, 100% by mass or less of ethylene rubber, 35% by mass or less of styrene-based elastomer, and 40% by mass or less of oil. By using the base resin with the above composition in combination with an inorganic filler described below, it is possible to realize a silane crosslinked resin molded product that maintains excellent heat resistance and tensile strength while also having long-term insulation properties, tracking resistance, deliquescence resistance, and flexibility (hereinafter, sometimes simply referred to as "having all six of the above properties").
[0018] (Polymer component) At least one of the polymer components that can be contained in the base resin has a site in the main chain or at its end that can undergo grafting reaction with a grafting reaction site of a silane coupling agent described later in the presence of an organic peroxide. Examples of the site that can undergo grafting reaction include an unsaturated bond site in a carbon chain and a carbon atom having a hydrogen atom. Examples of such polymer components include polyolefin resin, ethylene rubber, and styrene-based elastomer. In the present invention, the base resin contains at least one of polyolefin resin and ethylene rubber, and preferably contains any two of polyolefin resin, ethylene rubber, and styrene-based elastomer, and more preferably contains all of them.
[0019] - Polyolefin resin - The polyolefin resin is not particularly limited as long as it is a resin made of a polymer obtained by polymerizing or copolymerizing a compound having an ethylenically unsaturated bond (olefin compound), and known resins used in various resin compositions can be used. For example, polyethylene, polypropylene, ethylene-α-olefin copolymer, block copolymer of polypropylene and ethylene-α-olefin resin, polyolefin copolymer having an acid copolymer component or an acid ester copolymer component can be mentioned. In addition, rubber or elastomer of these copolymers (excluding ethylene rubber and styrene-based elastomer) can be mentioned, for example, acrylic rubber.
[0020] The polyethylene resin (PE) is not particularly limited as long as it is a polymer resin mainly composed of ethylene. For example, high density polyethylene (HDPE), low density polyethylene (LDPE), ultra-high molecular weight polyethylene (UHMW-PE), linear low density polyethylene (LLDPE), and very low density polyethylene (VLDPE) resins can be mentioned. Among them, linear low density polyethylene and low density polyethylene resins are preferable.
[0021] The polypropylene resin (PP) is not particularly limited as long as it is a polymer resin mainly composed of propylene, and examples thereof include propylene homopolymers, random polypropylenes, and block polypropylenes.
[0022] As the ethylene-α-olefin copolymer, preferably, a copolymer of ethylene and an α-olefin having 3 to 12 carbon atoms (excluding those included in the above polyethylene and polypropylene) is used.
[0023] In the polyolefin copolymer having an acid copolymerization component or an acid ester copolymerization component, the compound leading to the acid copolymerization component or the acid ester copolymerization component is not particularly limited, and examples thereof include carboxylic acid compounds such as (meth)acrylic acid, and acid ester compounds such as vinyl acetate and (meth)acrylic acid ester. The (meth)acrylic acid ester is not particularly limited, and examples thereof include alkyl (meth)acrylate. The alkyl group of the alkyl (meth)acrylate is preferably one having 1 to 12 carbon atoms. Examples of polyolefin copolymer resins having an acid copolymerization component or an acid ester copolymerization component (excluding those contained in polyethylene resins) include, for example, ethylene-vinyl acetate copolymer (EVA), ethylene-(meth)acrylic acid copolymer, ethylene-alkyl (meth)acrylate copolymer, and other resins. Specific examples of ethylene-alkyl (meth)acrylate copolymer resins include ethylene-methyl acrylate copolymer (EMA), ethylene-ethyl acrylate copolymer (EEA), and ethylene-butyl acrylate copolymer (EBA).
[0024] The acrylic rubber (ACM) is not particularly limited, but is preferably a rubber elastic body made of a copolymer obtained by copolymerizing an alkyl acrylate such as ethyl acrylate or butyl acrylate as a constituent component with an unsaturated hydrocarbon or a monomer having various functional groups. The monomer to be copolymerized with the alkyl acrylate is not particularly limited, but examples thereof include ethylene, 2-chloroethyl vinyl ether, methyl vinyl ketone, acrylic acid, acrylonitrile, butadiene, etc.
[0025] As the polyolefin resin, the above-mentioned resins can be used alone or in combination of two or more depending on the application or required properties.
[0026] - Ethylene rubber - The ethylene rubber is not particularly limited as long as it is a rubber (including elastomers) made of a copolymer obtained by copolymerizing a compound having an ethylenically unsaturated bond, and known rubbers can be used. Preferred examples of the ethylene rubber include a copolymer of ethylene and an α-olefin, and a terpolymer of ethylene, an α-olefin, and a diene. Examples of the terpolymer include a terpolymer of ethylene, an α-olefin, and a conjugated diene, and a terpolymer of ethylene, an α-olefin, and a non-conjugated diene. The α-olefin is preferably an α-olefin having a carbon number of 3 to 12. The diene compound constituting the terpolymer is not particularly limited, and examples thereof include conjugated diene compounds such as butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene, and non-conjugated diene compounds such as dicyclopentadiene (DCPD), ethylidenenorbornene (ENB), and 1,4-hexadiene, with non-conjugated diene compounds being preferred. As the binary copolymer rubber, ethylene-propylene rubber (EPM) is preferred, and as the ternary copolymer rubber, ethylene-propylene-diene rubber (EPDM) is preferred. The amount of ethylene constituents in the copolymer of ethylene rubber (referred to as ethylene content) is preferably 45 to 75 mass%. The ethylene content is a value measured in accordance with the method described in ASTM D3900. When the content of ethylene rubber in the base resin is 60 parts by mass or more, the amount of diene constituents in the ethylene rubber (referred to as diene content) is preferably 0 to 7 mass%. The diene content can be measured, for example, by infrared absorption spectroscopy (FT-IR), proton NMR ( 1 It can be measured by H-NMR, etc.
[0027] - Styrene-based elastomer - The styrene-based elastomer refers to an elastomer made of a polymer having a component derived from an aromatic vinyl compound in the molecule. Such styrene-based elastomers include block copolymers and random copolymers of conjugated diene compounds and aromatic vinyl compounds, or hydrogenated products thereof. Examples of aromatic vinyl compounds include styrene, p-(t-butyl)styrene, α-methylstyrene, p-methylstyrene, divinylbenzene, 1,1-diphenylstyrene, N,N-diethyl-p-aminoethylstyrene, vinyltoluene, p-(t-butyl)styrene, etc. Examples of conjugated diene compounds include butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, etc. Examples of styrene-based elastomers include styrene-ethylene-butylene-styrene block copolymer (SEBS), styrene-isoprene-styrene block copolymer (SIS), hydrogenated SIS, styrene-butadiene-styrene block copolymer (SBS), hydrogenated SBS, styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), styrene-ethylene-propylene-styrene block copolymer (SEPS), styrene-butadiene rubber (SBR), hydrogenated styrene-butadiene rubber (HSBR), and the like.
[0028] - Oil - The oil that the base resin may contain is not particularly limited, and may be an organic oil or a mineral oil. When the base resin contains oil, the generation of bumps (granular objects protruding from the surface) is suppressed, and a silane-crosslinked resin molded product having excellent appearance can be produced. Examples of the organic oil or mineral oil include soybean oil, paraffin oil, naphthenic oil, and aromatic oil. Paraffin oil or naphthenic oil is preferred, and paraffin oil is more preferred in terms of mechanical strength.
[0029] (Base Resin Composition) The base resin contains up to 100% by mass of polyolefin resin, up to 100% by mass of ethylene rubber, up to 35% by mass of styrene-based elastomer, and up to 40% by mass of oil, when the total content of each component in the base resin is 100% by mass. The content of the polyolefin resin in the base resin is preferably 50% by mass or less, more preferably 20 to 40% by mass, and even more preferably 22 to 32% by mass. The content of the polyethylene resin in the base resin is not particularly limited and is appropriately set in consideration of the content of the polyolefin resin, and is, for example, preferably 0 to 25% by mass, and more preferably 12 to 22% by mass. Similarly, the content of the polypropylene resin in the base resin is not particularly limited and is appropriately set in consideration of the content of the polyolefin resin, and is, for example, preferably 25% by mass or less, and more preferably 5 to 15% by mass. The content of the ethylene rubber in the base resin is preferably from 10 to 100% by mass, more preferably from 10 to 45% by mass, and further preferably from 15 to 30% by mass. The content of the styrene-based elastomer in the base resin is preferably 35% by mass or less, more preferably 10 to 35% by mass, and even more preferably 15 to 30% by mass, particularly from the viewpoint of tensile strength. The content of oil in the base resin is preferably 40% by mass or less, more preferably 20 to 40% by mass, and even more preferably 22 to 32% by mass, particularly from the viewpoint of tensile strength. The composition of the base resin (combination of the content of each component) can be determined by combining appropriate contents (numerical ranges) of each of the above-mentioned components. For example, the composition of the base resin is preferably 50 mass% or less of polyolefin resin, 10 to 100 mass% of ethylene rubber, 35 mass% or less of styrene-based elastomer, and 40 mass% or less of oil, and more preferably 20 to 40 mass% of polyolefin resin, 10 to 45 mass% of ethylene rubber, 10 to 35 mass% of styrene-based elastomer, and 20 to 40 mass% of oil. By using the above-mentioned base resin composition, the above six properties can be provided in a well-balanced manner.
[0030] The base resin may contain other components, such as various additives and solvents, which will be described later.
[0031] <Organic peroxide> The organic peroxide generates radicals by thermal decomposition, and thereby has the function of initiating and promoting the grafting reaction between the silane coupling agent and the base resin (a covalent bond forming reaction between the grafting reaction site of the silane coupling agent and the grafting reaction site of the base resin, also called a (radical) addition reaction). There are no particular limitations on the organic peroxide, and examples thereof include those represented by the general formula: R 1 -O-O-R 2 , R 3 -OO-C(=O)R 4 , R 5 C(=O)-OO(C=O)R 6 Preferred are compounds represented by the formula: 1 ~R 6 Each independently represents an alkyl group, an aryl group, or an acyl group. R 1 ~R 6 Among these, it is preferable that all of them are alkyl groups, or that one of them is an alkyl group and the remaining is an acyl group.
[0032] The decomposition temperature of the organic peroxide is preferably 80 to 195°C, particularly preferably 125 to 180°C, as measured by the method described in JP-A-2016-121203. Examples of such organic peroxides include those described in paragraph
[0036] of JP 2016-121203 A, the contents of which are incorporated herein by reference as part of the present specification. Among these, dicumyl peroxide, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane (Perhexa 25B), and 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3 are preferred.
[0033] <Inorganic filler> The inorganic filler used in the present invention includes metal carbonate, boehmite, silica and / or calcined clay, and may further include other inorganic fillers. By using the above-mentioned three or four types of inorganic fillers in combination with the above-mentioned base resin, it is possible to realize a silane crosslinked resin molded product that maintains excellent heat resistance and tensile strength while also having long-term insulation properties, tracking resistance, deliquescence resistance, and flexibility. As the inorganic filler, it is preferable to use silica in combination with a metal carbonate and boehmite, since this makes it possible to highly enhance flexibility while maintaining heat resistance, tensile strength, long-term insulating properties, tracking resistance and deliquescence resistance.
[0034] - Metal carbonate - The metal carbonate can be used without any particular limitation as long as it is a metal carbonate, and examples thereof include alkali metal carbonates and alkaline earth metal carbonates, with alkaline earth metal carbonates being preferred. Examples of alkaline earth metal carbonates include magnesium carbonate and calcium carbonate, with calcium carbonate being preferred. The metal carbonates may be used alone or in combination of two or more. The average particle size of the metal carbonate is preferably 0.2 to 10 μm, more preferably 0.3 to 8 μm, even more preferably 0.4 to 5 μm, and particularly preferably 0.4 to 3 μm. If the average particle size is too small, secondary aggregation may occur when mixed with the silane coupling agent, resulting in a deterioration in the appearance of the molded product or the generation of lumps. On the other hand, if the average particle size is too large, the appearance may deteriorate, the retention effect of the silane coupling agent may decrease, and problems may occur in crosslinking. The average particle size is determined by dispersing the metal carbonate in alcohol or water and using an optical particle size measuring device such as a laser diffraction / scattering type particle size distribution measuring device.
[0035] - Boehmite - Boehmite is a hydrated aluminum oxide (Al 2 O 3 H 2Boehmite has a site on its surface that can be chemically bonded to a silanol condensable reactive site of a silane coupling agent by hydrogen bond, covalent bond, or intermolecular bond. Such sites that can be chemically bonded include, but are not limited to, OH groups (hydroxyl groups, water molecules of water of water or crystallization, OH groups such as carboxyl groups), amino groups, and SH groups. In the present invention, the boehmite holds the silane coupling agent and acts as a filler or a flame retardant. It is preferable to use the boehmite without surface treatment. The average secondary particle size of the boehmite is not particularly limited, but is preferably 0.3 to 5 μm, and more preferably 0.4 to 2 μm. When the average secondary particle size is 0.3 to 5 μm, for example, flame retardancy can be imparted without impairing elongation and strength. In addition, the appearance is excellent. The average secondary particle size is determined by dispersing the boehmite in alcohol or water and using an optical particle size measuring device such as a laser diffraction / scattering type particle size distribution measuring device. The shape of the boehmite is not particularly limited, and granular, plate-like, needle-like, etc. can be used, with plate-like being preferred. In the case of a plate-like shape, the aspect ratio is preferably 1 to 60, and from the viewpoint of the balance between strength and flexibility, preferably 1 to 3. The BET specific surface area of the boehmite is not particularly limited, but is preferably 0.8 to 30 m in terms of tensile strength or flexibility. 2 / g is preferable, and 1.2 to 25m 2 / g is more preferable. The BET specific surface area is a value measured using nitrogen gas as an adsorbate in accordance with the "carrier gas method" of JIS Z 8830:2013. For example, it is a value measured using a specific surface area / pore distribution measuring device "Flowsorb" (manufactured by Shimadzu Corporation).
[0036] - Silica - Silica is not particularly limited, and can be crystalline silica, non-crystalline silica, silica produced by fusion method, silica produced by wet method, silica produced by dry method, and silica powder produced by crushing high purity natural quartz.As silica, crystalline silica and silica powder produced by crushing high purity natural quartz are preferred.Silica has a site on its surface that can chemically bond with the reactive site that can condense silanol of silane coupling agent. The average particle size of silica (measured by the same method as for metal carbonates, the same applies below) is preferably 5 μm or less. When the average particle size of silica is 5 μm or less, the mechanical properties and extrusion appearance are particularly excellent. It is more preferably 3 μm or less, and even more preferably 2 μm or less. On the other hand, the lower limit of the average particle size of silica is not particularly limited, but from the viewpoint of excellent mechanical properties and tracking resistance, it is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1.0 μm or more. BET specific surface area of silica (m 2 / g) is not particularly limited, and may be, for example, 2 to 400 m 2 / g is preferable, and 2 to 300m 2 / g is more preferable, and 3 to 100m 2 / g is more preferable, and 5 to 50m 2 / g is more preferable. The BET specific surface area (m 2 / g) is a value measured using nitrogen gas as the adsorbate in accordance with the "carrier gas method" of JIS Z 8830:2013. For example, it is a value measured using a specific surface area / pore distribution measuring device "Flowsorb" (manufactured by Shimadzu Corporation).
[0037] - Calcined clay - The calcined clay is not particularly limited, and any known calcined clay can be used. The average particle size of the calcined clay is preferably 5 μm or less for the same reasons as those for the average particle size of silica.
[0038] - Other inorganic fillers - The inorganic filler used in the present invention may include inorganic fillers that do not fall under any of metal carbonates, boehmite, silica, and calcined clay (referred to as other inorganic fillers). Other inorganic fillers include those that are commonly used in resin compositions, such as metal hydrates such as compounds having hydroxyl groups or crystal water, such as aluminum hydroxide, magnesium hydroxide, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, aluminum borate whiskers, hydrated aluminum silicate, hydrated magnesium silicate, basic magnesium carbonate, hydrotalcite, talc, etc. Further examples include boron nitride, carbon black, zinc oxide, tin oxide, titanium oxide, molybdenum oxide, silicone compounds, quartz, zinc borate, white carbon, zinc borate, zinc hydroxystannate, zinc stannate, etc.
[0039] (Composition of inorganic filler) The inorganic filler contains 10 to 35 parts by mass of metal carbonate, 20 to 55 parts by mass of boehmite, and 45 to 90 parts by mass of silica and / or calcined clay within the range of the total content of the inorganic filler described below. The content of the metal carbonate is preferably 10 to 35 parts by mass, more preferably 12 to 32% by mass, and even more preferably 15 to 30% by mass, relative to 100 parts by mass of the base resin, in order to achieve, for example, both flexibility and long-term insulation resistance, and thus to achieve a good balance between the above six properties. The content of boehmite is preferably 20 to 55 parts by mass, more preferably 25 to 45% by mass, and even more preferably 28 to 40% by mass, relative to 100 parts by mass of the base resin, in order to achieve, for example, both tracking resistance and long-term insulation resistance and flexibility, and thus to have a good balance between the above six properties. The total content of silica and calcined clay is preferably 45 to 90 parts by mass, more preferably 50 to 80% by mass, and even more preferably 55 to 70% by mass, relative to 100 parts by mass of the base resin, in order to achieve, for example, insulation resistance (short-term or long-term insulation resistance), flexibility, and heat resistance, and thus to have a good balance between the above-mentioned six properties. The content of silica alone can be appropriately set in consideration of the total content, and is preferably 45 to 90 parts by mass, and more preferably 55 to 70% by mass, relative to 100 parts by mass of the base resin. The content of calcined clay alone can be appropriately set in consideration of the total content, and is preferably 45 to 75 parts by mass, and more preferably 50 to 65% by mass, relative to 100 parts by mass of the base resin. The content of the other inorganic fillers is appropriately set within the range of the total content of the inorganic fillers described below, and can be, for example, 1 to 20 parts by mass per 100 parts by mass of the base resin.
[0040] In the present invention, the mass ratio of the metal carbonate content, the boehmite content, and the total content of silica and calcined clay is appropriately set depending on the application and form of use. For example, the mass ratio of the content of boehmite to the content of metal carbonate [boehmite content / metal carbonate content] is preferably 0.5 to 6, and more preferably 0.7 to 4. Furthermore, the mass ratio of the total content of silica and calcined clay to the content of metal carbonate [total content of silica and calcined clay / metal carbonate content] is preferably 1.2 to 9, and more preferably 1.5 to 6. Furthermore, the mass ratio of the total content of silica and calcined clay to the content of boehmite [total content of silica and calcined clay / boehmite content] is preferably 0.8 to 5, and more preferably 1 to 4.
[0041] In order to produce a silane-crosslinked resin molded product having the above six properties in a well-balanced manner, it is preferable that the inorganic filler does not contain other inorganic fillers, that is, it is made up of three or four types of inorganic fillers, namely, metal carbonate, boehmite, and silica and / or calcined clay. In the present invention, "not containing other inorganic fillers" includes not only an embodiment in which the content of other inorganic fillers is 0 parts by mass relative to 100 parts by mass of the base resin, but also an embodiment in which other inorganic fillers are inevitably mixed in (for example, an embodiment in which the content of other inorganic fillers is 8 parts by mass or less relative to 100 parts by mass of the base resin).
[0042] <Silane coupling agent> The silane crosslinkable resin composition contains a silane coupling agent grafted to a base resin. The base resin to which the silane coupling agent is grafted is preferably prepared by a grafting reaction between the silane coupling agent and the base resin in step (1) described below. The silane coupling agent (before grafting reaction) used in the present invention has a grafting reaction site (functional group such as a group or an ethylenically unsaturated group) that can undergo grafting reaction with the grafting reaction site of the base resin in the presence of radicals generated by decomposition of organic peroxide.In addition, it has a hydrolyzable silyl group as a reaction site that can undergo silanol condensation, and is preferably capable of reacting with the site that can be chemically bonded to the inorganic filler.As such a silane coupling agent, there can be mentioned a silane coupling agent used in the conventional silane crosslinking method. Suitable examples of the silane coupling agent include silane coupling agents having an ethylenically unsaturated group and a hydrolyzable silyl group, and specifically include vinyl alkoxylanes such as vinyl trimethoxylane, vinyl triethoxylane, vinyl tributoxylane, vinyl dimethoxyethoxylane, vinyl dimethoxybutoxylane, vinyl diethoxybutoxylane, allyl trimethoxylane, allyl triethoxylane, and vinyl triacetoxylane, and (meth)acryloxyalkoxylanes such as methacryloxypropyl trimethoxylane, methacryloxypropyl triethoxylane, and methacryloxypropyl methyl dimethoxylane. Among these, vinyl trimethoxylane or vinyl triethoxylane is particularly preferred. The silane coupling agent may be used alone or in combination of two or more kinds. In addition, the silane coupling agent may be used as it is or after diluting with a solvent or the like.
[0043] <Silanol condensation catalyst> The silanol condensation catalyst works to promote the condensation reaction (promotion) of the silanol condensable reactive sites of the silane coupling agent grafted to the base resin in the presence of water (moisture). Based on the action of this silanol condensation catalyst, the base resin is crosslinked via the silane coupling agent. Such silanol condensation catalysts are not particularly limited, and examples thereof include organotin compounds, metal soaps, platinum compounds, etc. Examples of organotin compounds include dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin dioctiate, dibutyltin diacetate, and other organotin compounds.
[0044] <Carrier resin> The silanol condensation catalyst is mixed with a resin or rubber as desired and used. Such a resin or rubber (also called a carrier resin) is not particularly limited, but the components described in the base resin can be used. In terms of compatibility with the base resin, the carrier resin is preferably at least one of the components constituting the base resin, and preferably contains the same components as the base resin.
[0045] <Additives> In the present invention, various additives generally used in various wiring materials such as electric wires, electric cables, and electric cords, and various resin molded products such as sheets, foams, tubes, and pipes may be contained within a range that does not impair the effects of the present invention. Examples of such additives include crosslinking assistants, antioxidants, lubricants, metal deactivators, plasticizers, flame retardants, and flame retardant assistants.
[0046] The antioxidant is not particularly limited, but examples thereof include amine antioxidants, phenol antioxidants, and sulfur antioxidants. Examples of amine antioxidants include 4,4'-dioctyldiphenylamine, N,N'-diphenyl-p-phenylenediamine, and polymers of 2,2,4-trimethyl-1,2-dihydroquinoline. Examples of phenol antioxidants include pentaerythritol-tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene. Examples of sulfur antioxidants include bis(2-methyl-4-(3-n-alkylthiopropionyloxy)-5-tert-butylphenyl)sulfide, 2-mercaptobenzimidazole and its zinc salt, pentaerythritol-tetrakis(3-lauryl-thiopropionate), etc. The antioxidant can be added in an amount of preferably 0.1 to 15.0 parts by mass, more preferably 0.1 to 10 parts by mass, per 100 parts by mass of the base resin. The flame retardant is not particularly limited, but examples thereof include bromine-based flame retardants, chlorine-based flame retardants, antimony trioxide, etc. The content of the flame retardant is appropriately set within a range that does not impair the effects of the present invention.
[0047] (Composition of silane crosslinkable resin composition) The content of the silane coupling agent grafted to the base resin in the silane crosslinkable resin composition (converted into the mass before the graft reaction with the base resin) is 2 to 10 parts by mass relative to 100 parts by mass of the base resin, in order to suppress the generation of protruding aggregates (gel particles) caused by crosslinked gels, etc., and the volatilization of the silane coupling agent, thereby forming a sufficient crosslinked structure with excellent appearance, and further, to produce a silane crosslinked resin molded product having the above six characteristics in a well-balanced manner. The content of the silane coupling agent is preferably 2.2 to 6 parts by mass, more preferably 2.5 to 4.5 parts by mass, in order to produce a silane crosslinked resin molded product having the above six characteristics in a well-balanced manner at a high level.
[0048] The content (total content) of the inorganic filler in the silane crosslinkable resin composition is 100 to 150 parts by mass relative to 100 parts by mass of the base resin, in order to achieve both tracking resistance and flexibility, tensile strength, and long-term insulation resistance, and thus to produce a silane crosslinked resin molded product having the above six properties in a well-balanced manner. The total content of the inorganic filler is preferably 105 to 140 parts by mass, more preferably 108 to 135 parts by mass, in order to produce a silane crosslinked resin molded product having the above six properties in a well-balanced manner at high levels.
[0049] The content of the silanol condensation catalyst in the silane crosslinkable resin composition is not particularly limited and can be appropriately set. For example, in order to improve the appearance, heat resistance, and tensile strength of the silane crosslinked resin molded article in a well-balanced manner, the content is preferably 0.01 to 0.5 parts by mass, more preferably 0.03 to 0.3 parts by mass, and even more preferably 0.05 to 0.15 parts by mass, relative to 100 parts by mass of the base resin.
[0050] In the silane-crosslinkable resin composition, the composition of the base resin and the composition of the inorganic filler are as described above. Note that the organic peroxide is usually decomposed during the grafting reaction between the silane coupling agent and the base resin. The total content of the additives in the silane-crosslinkable resin composition is not particularly limited, and can be appropriately set within a range that does not impair the effects of the present invention.
[0051] (Composition of silane crosslinked resin molded body) Since the silane crosslinked resin molded product is formed by molding the silane crosslinkable resin composition and then contacting it with water to cause a silanol condensation reaction, the contents of the above-mentioned components in the molded product are usually the same as those in the silane crosslinkable resin composition, except that in the silane crosslinked resin molded product, the contents of the silane coupling agent and the base resin are those before the grafting reaction and the silanol condensation reaction, respectively.
[0052] [Method of manufacturing silane-crosslinkable resin composition and silane-crosslinked resin molded article] The method for producing the silane-crosslinkable resin composition of the present invention and the method for producing a silane-crosslinked resin molded article of the present invention will be described below. The silane-crosslinkable resin composition of the present invention is produced by carrying out the following step (1), and the silane-crosslinked resin molded product of the present invention is produced by carrying out the following steps (1) to (3). The method for producing a silane-crosslinked resin molded article and the method for producing a silane-crosslinkable resin composition of the present invention may be collectively referred to as the production method of the present invention.
[0053] Step (1): 100 parts by mass of a base resin, 0.01 to 0.3 parts by mass of an organic peroxide, 100 to 150 parts by mass of inorganic filler and 2 to 10 parts by mass of silane coupling agent and a silanol condensation catalyst to obtain a mixture. Step (2): A step of molding the mixture obtained in step (1) to obtain a molded body. Step (3): The molded product obtained in step (2) is contacted with water to obtain a silane-crosslinked resin molded product. Process The above-mentioned step (1) comprises the following steps (a-1), (a-2) and (c) when the entire base resin is melt-mixed in the following step (a-2), whereas it comprises the following steps (a-1), (a-2), (b) and (c) when only a part of the base resin is melt-mixed in the following step (a-2). Step (a-1): Mixing an inorganic filler and a silane coupling agent to prepare a mixture The process Step (a-2): The obtained mixture and all or a part of the base resin are reacted with an organic peroxide. In the presence of organic peroxide, the mixture is melted and mixed at a temperature equal to or higher than the decomposition temperature of the organic peroxide. and preparing a silane master batch. Step (b): Melt-mix the remainder of the base resin and the silanol condensation catalyst to form a catalyst masterbatch. - Preparation of the batch Step (c): A silane masterbatch and a silanol condensation catalyst or catalyst masterbatch and a step of melt-mixing the
[0054] In the manufacturing method of the present invention, the mixing amount of each component used as the base resin is the same as the above-mentioned content ratio explained as the composition of the base resin. Also, the mixing amount of the silane coupling agent, inorganic filler, silanol condensation catalyst, and additives is the same as the content of the corresponding component in the above-mentioned silane crosslinkable resin composition.
[0055] In step (1), the amount of organic peroxide to be mixed is 0.01 to 0.3 parts by mass relative to 100 parts by mass of the base resin. By mixing the organic peroxide in the above content, the silane coupling agent and the base resin can be effectively grafted, and a silane-crosslinked resin molded article having all the above six properties can be produced. In addition, the condensation of the unreacted silane coupling agent is suppressed, and no gel-like particles (aggregates) are generated, so that a composition with excellent extrudability and a molded article with excellent appearance can be obtained. The amount of organic peroxide to be mixed is preferably 0.05 to 0.2 parts by mass.
[0056] In the manufacturing method of the present invention, the base resin is a resin for forming a silane crosslinked resin molded product or a silane crosslinkable resin composition. Therefore, in the manufacturing method of the present invention, the mixture obtained in step (1) may contain 100 parts by mass of the base resin. For example, in step (a-2), the method includes an embodiment in which the entire amount (100 parts by mass) of the base resin is mixed and an embodiment in which only a part of the base resin is mixed.
[0057] When a part of the base resin is mixed in the step (a-2), the component to be mixed may be one type or two or more types. In the manufacturing method of the present invention, the base resin mixed in step (a-2) preferably contains a polyolefin resin, more preferably contains a polyolefin resin and an ethylene rubber, and even more preferably contains a polyolefin resin, an ethylene rubber, a styrene-based elastomer, and an oil, from the viewpoint of having a good balance of the six properties among the above-mentioned components. The remainder of the base resin (carrier resin) mixed in step (b) is as described above, and more preferably contains a polyolefin resin, an ethylene rubber, a styrene-based elastomer, and an oil.
[0058] The ratio of the base resin mixed in step (a-2) is preferably 60 to 95% by mass out of 100% by mass of the base resin mixed in steps (a-2) and (b), and more preferably 70 to 95% by mass in order to achieve a high level of both heat resistance and mechanical properties by constructing a sufficient crosslinked structure. The remainder of the base resin mixed in step (b) (carrier resin) is appropriately determined depending on the part of the base resin mixed in step (a-2).
[0059] Although a part of the inorganic filler can be used in a step other than the step (a-1), for example, in the step (b), it is preferable to mix the above three or four inorganic fillers in the step (a-1), and more preferable to mix the entire amount of the above three or four inorganic fillers in the step (a-1), in order to construct a well-balanced crosslinked structure between the base resins (without the inorganic filler) and a crosslinked structure involving the inorganic filler, thereby expressing the six characteristics at a high level. When the inorganic filler is used in a step other than the step (a-1), the amount of use is not particularly limited and is appropriately determined.
[0060] The antioxidant may be contained when carrying out step (c), and may be mixed in any step. It is preferable to mix the antioxidant in step (b) in order to efficiently generate and progress the grafting reaction between the silane coupling agent and the base resin without inhibiting it. When mixing in step (a-1) or step (a-2), the amount of the antioxidant mixed is preferably 0.5 parts by mass or less per 100 parts by mass of the base resin.
[0061] The various additives may be mixed in any of the steps (a-1), (a-2) and (b).
[0062] <Process (1)> The manufacturing method of the present invention involves a step (1) of grafting a base resin with a silane coupling agent in the presence of an inorganic filler to prepare a silane master batch (Silane MB) containing a silane crosslinkable resin in which the silane coupling agent is grafted and bonded to the base resin. In this process, the base resin is melt-mixed with the inorganic filler and the silane coupling agent in the presence of the organic peroxide at a temperature equal to or higher than the decomposition temperature of the organic peroxide, thereby obtaining the silane MB as a molten mixture. Step (1), that is, melt mixing of all or a part of the base resin, the organic peroxide, the inorganic filler, the silane coupling agent, and the silanol condensation catalyst, is carried out in the following order of steps.
[0063] (Process (a-1)) In the present invention, first, an inorganic filler and a silane coupling agent are mixed to prepare a mixture (step (a-1)). By premixing the inorganic filler and the silane coupling agent, a silane coupling agent bonded or adsorbed to the inorganic filler by a weak bond and a silane coupling agent bonded or adsorbed to the inorganic filler by a strong bond can be formed in a well-balanced manner. This effectively prevents the volatilization of the silane coupling agent and the condensation reaction between the unadsorbed silane coupling agents during the melt mixing in step (a-2). As a result, a silane crosslinked resin molded product can be produced that has a better appearance and also has the above six characteristics. Here, examples of the weak bond with the inorganic filler include interactions due to hydrogen bonds, interactions between ions, partial charges or dipoles, and actions due to adsorption. Examples of the strong bond with the inorganic filler include chemical bonds with sites on the surface of the inorganic filler that can be chemically bonded.
[0064] The mixing method and conditions in step (a-1) are not particularly limited, but examples of the method and conditions include a method and method of mixing by a dry or wet method using a known mixer, kneader, etc., usually at a temperature below the decomposition temperature of the organic peroxide, preferably 10 to 60°C, more preferably around room temperature (20 to 25°C), for several minutes to several hours. Among them, dry mixing (dry blending) at a temperature below the decomposition temperature of the organic peroxide is preferred. Other conditions for dry mixing are appropriately determined.
[0065] In step (a-1), a base resin can also be mixed as long as the temperature is maintained below the decomposition temperature. The organic peroxide may be present during the melt mixing in step (a-2), and may be mixed in step (a-2), but is preferably mixed in step (a-1). In this case, the organic peroxide may be mixed with the inorganic filler after being mixed with the silane coupling agent, or may be mixed with the inorganic filler separately from the silane coupling agent.
[0066] (Process (a-2)) In the manufacturing method of the present invention, the mixture obtained in step (a-1), all or a part of the base resin, and the remaining components not mixed in step (a-1) are melt-mixed in the presence of an organic peroxide by heating to a temperature equal to or higher than the decomposition temperature of the organic peroxide to prepare silane MB (step (a-2)). In the melt-mixing in this step, the volatilization and self-condensation of the above-mentioned silane coupling agent can be suppressed, while excessive crosslinking reaction (generation of gel particles) between the base resins can be prevented.
[0067] In step (a-2), the temperature (also called mixing temperature) at which the above components are melt-mixed (also called melt-kneading or kneading) is equal to or higher than the decomposition temperature of the organic peroxide, preferably a temperature of the decomposition temperature of the organic peroxide + (25 to 110)°C, more preferably 150 to 230°C, and even more preferably 175 to 210°C. At the above mixing temperature, the above components melt, and the organic peroxide decomposes and acts to proceed with the necessary grafting reaction. Other conditions, such as the mixing time, can be set appropriately. For example, the mixing time can be 1 to 25 minutes, and is preferably 3 to 20 minutes.
[0068] The mixing method is not particularly limited as long as it is a method commonly used for rubber, plastics, etc. As a mixing device, for example, a single screw extruder, a twin screw extruder, a roll, a Banbury mixer, various kneaders, etc. are used. A closed type mixer such as a Banbury mixer or various kneaders is preferred. The method of mixing the base resin is not particularly limited. For example, the base resin may be prepared in advance and used, or each component may be used separately.
[0069] In steps (a-1) and (a-2), especially in step (a-2), it is preferable to melt-mix the above-mentioned components substantially without mixing a silanol condensation catalyst. This can suppress the condensation reaction of the silane coupling agent, facilitate melt mixing, and obtain a desired shape during extrusion molding. Here, "substantially without mixing a silanol condensation catalyst" does not mean to exclude the silanol condensation catalyst that is inevitably present, but means that it may be present to the extent that the above-mentioned problems caused by the silanol condensation of the silane coupling agent do not occur. For example, in step (a-2), the silanol condensation catalyst may be present in an amount of 0.01 parts by mass or less relative to 100 parts by mass of the base resin.
[0070] In step (1), particularly in steps (a-1) and (a-2), it is preferable that the crosslinking aid is not substantially mixed in. If the crosslinking aid is not substantially mixed in, crosslinking between the base resins is unlikely to occur during melt mixing, and the appearance and heat resistance of the silane-crosslinked resin molded article are excellent.
[0071] In this way, the steps (a-1) and (a-2) are carried out to prepare Silane MB. This Silane MB contains a reaction mixture of a base resin, an inorganic filler, and a silane coupling agent, and contains a silane crosslinkable resin (silane graft polymer) in which the silane coupling agent and the base resin have undergone a graft reaction to such an extent that it can be molded in the step (2) described below. The silane coupling agent grafted to the base resin includes those that are bonded or adsorbed to the inorganic filler at their silanol condensable reaction sites.
[0072] In step (a-2), the silane coupling agent and the base resin may undergo a graft reaction in at least the following manner. That is, the silane coupling agent bonded or adsorbed to the inorganic filler by a weak bond is released from the inorganic filler and undergoes a graft reaction with the base resin. The crosslinked structure formed in step (3) described later from this manner does not incorporate the inorganic filler, and is usually a crosslinked structure via a silanol condensate between the silane coupling agents. In addition, the silane coupling agent bonded or adsorbed to the inorganic filler by a strong bond undergoes a graft reaction with the base resin while maintaining the bond or adsorption to the inorganic filler. The crosslinked structure formed in step (3) described later from this manner incorporates the inorganic filler, and is a crosslinked structure via the silane coupling agent bonded to the inorganic filler as the starting point. By mixing the crosslinked structures in both of the above manners, a highly developed crosslinked structure including a crosslinked structure involving the inorganic filler in the silane crosslinked resin molded body can be constructed.
[0073] (Step (b)) In the manufacturing method of the present invention, when a part of the base resin is melt-mixed in step (a-2) independently of step (a-2) or subsequent to step (a-2), the remaining part of the base resin (carrier resin) and the silanol condensation catalyst are melt-mixed to prepare a catalyst master batch (also called catalyst MB) (step (b)). Therefore, when the whole of the base resin is melt-mixed in step (a-2), step (b) does not need to be performed, and the silanol condensation catalyst may be mixed with another resin.
[0074] The mixing ratio of the carrier resin and the silanol condensation catalyst is not particularly limited, but is preferably set so as to satisfy the above-mentioned mixing amounts in step (1). The melt mixing method and conditions in step (b) are not particularly limited, and the melt mixing method and conditions in step (a-2) above can be applied. For example, the mixing temperature can be 120 to 200°C, and preferably 130 to 180°C. Other conditions, such as the mixing time, can be appropriately set. For example, the mixing time can be 1 to 25 minutes, and preferably 3 to 20 minutes.
[0075] In step (b), other resins can be used as carrier resins in place of or in addition to the remainder of the base resin. When the carrier resin is other resins, the grafting reaction in step (a-2) can be accelerated, and lumps are less likely to occur during molding. The amount of other resins mixed is preferably 1 to 60 parts by mass, more preferably 2 to 50 parts by mass, and even more preferably 2 to 40 parts by mass, based on 100 parts by mass of the base resin.
[0076] (Process (c)) In the production method of the present invention, the silane MB and the silanol condensation catalyst or catalyst MB are then mixed to obtain a mixture (step (c)). The mixing method may be any method as long as a uniform mixture can be obtained as described above. The mixing in step (c) is basically the same as the melt mixing in step (a-2), and mixing is performed at least at a temperature at which the base resin melts. The mixing conditions in step (c) are not particularly limited, and the mixing conditions in step (a-2) above can be applied. The melting temperature is appropriately selected according to the melting temperature of the base resin or carrier resin, and is, for example, preferably 80 to 250°C, more preferably 100 to 240°C. Other conditions, such as the mixing time, can be appropriately set. However, in step (c), in order to avoid the silanol condensation reaction, it is preferable that the silane MB and the silanol condensation catalyst are not kept in a high temperature state for a long time in a mixed state. In step (c), it is preferable to dry blend the silane MB and the silanol condensation catalyst or the catalyst master batch before melt mixing. The method and conditions of dry blending are not particularly limited, and examples thereof include the dry blending and its conditions in step (a-1).
[0077] In this manner, steps (a-1) to (c) (step (1)) are carried out to produce the silane crosslinkable resin composition of the present invention as a molten mixture of the silane MB and the silanol condensation catalyst or catalyst MB. The silane crosslinkable resin composition contains the above-mentioned silane crosslinkable resin, inorganic filler, silanol condensation catalyst, etc. In this silane crosslinkable resin, the silane coupling agent's reactive site capable of silanol condensation may be bonded or adsorbed to inorganic filler, but as described below, it is not silanol condensed. Therefore, the silane crosslinkable resin contains at least a silane crosslinkable resin in which the silane coupling agent bonded or adsorbed to inorganic filler is grafted to a base resin, and a silane crosslinkable resin in which the silane coupling agent not bonded or adsorbed to inorganic filler is grafted to a base resin. As described above, the silane crosslinkable resin is an uncrosslinked body in which the silane coupling agent is not condensed with silanol. In practice, when melt-mixed in step (c), partial crosslinking is unavoidable, but the obtained silane crosslinkable resin composition is one that maintains at least the moldability in the molding in step (2).
[0078] <Process (2)> The method for producing a silane-crosslinked resin molded article of the present invention then carries out step (2) of molding the mixture (silane-crosslinkable resin composition) obtained in step (1) to obtain a molded article. In step (2), the mixture may be molded, and the molding method and molding conditions are appropriately selected according to the form of the molded product of the present invention. For example, the molding method may be press molding, extrusion molding using an extruder, extrusion molding using an injection molding machine, or molding using other molding machines. When producing a wiring material, the extrusion molding method is preferred in terms of productivity and the ability to co-extrude with a conductor.
[0079] This step (2) can be carried out simultaneously with or consecutively to step (c). For example, a series of steps can be adopted in which the silane MB and the silanol condensation catalyst or catalyst MB are mixed by dry blending or the like just before the coating device (extruder) and then melt-mixed in the coating device (step (c)), or the silane MB and the silanol condensation catalyst or catalyst MB are separately charged into the coating device and then melt-mixed (step (c)), followed by molding (step (2)).
[0080] The molding conditions (melt mixing conditions) are not particularly limited as long as the silane crosslinkable resin composition of the present invention can be molded and the silanol condensation reaction does not occur under the conditions. For example, the melt mixing method and conditions of step (a-2) can be applied. When an extrusion molding machine is used, the temperature of the extrusion molding machine is preferably set to about 120 to 180°C in the cylinder section and about 160 to 200°C in the crosshead section, although it depends on various conditions such as the type of base resin and the take-up speed of the conductor, etc. The molding speed (linear speed) in the extrusion molding is not particularly limited and can be appropriately set depending on the characteristics or performance of the extruder, the extrusion amount (coating amount), etc. The linear speed can usually be set to 1 to 20 m / min.
[0081] In this way, a molded product (uncrosslinked molded product) of the silane crosslinkable resin composition is obtained. Although partial crosslinking of the silane crosslinkable resin is inevitable in this molded product, as in the case of the silane crosslinkable resin composition, the molded product is in a partially crosslinked state that retains moldability in step (2). Therefore, the silane crosslinked resin molded product of this invention is made into a crosslinked or final crosslinked molded product by carrying out step (3).
[0082] <Process (3)> In the method for producing a silane-crosslinked resin molded article of the present invention, the molded article obtained in step (2) is then brought into contact with water to produce a silane-crosslinked resin molded article in step (3). Since the molded article obtained in step (2) is an uncrosslinked silane-crosslinked resin, this step initiates and advances (promotes) a silanol condensation reaction (dehydration condensation reaction) at the silanol condensable reactive sites of the silane coupling agent grafted to the base resin, and finally results in silane crosslinking. In this way, a silane-crosslinked resin molded article in which the silane coupling agent is crosslinked by silanol condensation can be obtained. The contact of the uncrosslinked molded body with water can be carried out by a normal method. The silanol condensation reaction proceeds simply by leaving the molded body at room temperature, for example, at a temperature of about 20 to 25° C., in the presence of moisture, so there is no need to actively contact the molded body with water. From the viewpoint of promoting the silanol condensation reaction (crosslinking reaction), it is preferable to actively contact the uncrosslinked molded body with water. Examples of the contact method include a method of contacting the molded body with water under a normal pressure environment, and specifically, examples of the contact method include exposure to a saturated water vapor atmosphere, exposure to a high humidity environment, immersion in room temperature water or hot water (for example, 50 to 90° C.), insertion into a moist heat bath, exposure to high temperature water vapor, etc. In addition, pressure may be applied during contact to allow moisture to penetrate into the inside.
[0083] In this manner, the silane-crosslinked resin molded article of the present invention is produced. The silane crosslinked resin molded body contains a crosslinked resin in which a base resin (silane crosslinkable resin) is condensed through a siloxane bond. The silane crosslinked resin molded body also contains an inorganic filler, and the inorganic filler may be bonded to the silane coupling agent of the crosslinked base resin. Therefore, the silane crosslinked resin includes at least a crosslinked resin in which a plurality of base resins are bonded or adsorbed to the inorganic filler by the silane coupling agent, and bonded (crosslinked) through the inorganic filler and the silane coupling agent, and a crosslinked resin in which the silanol condensable reactive sites of the silane coupling agent grafted to the base resin are hydrolyzed and undergo a silanol condensation reaction with each other (without going through an inorganic filler) through the silane coupling agent (siloxane bond).
[0084] As described above, in the manufacturing method of the present invention, in step (1), a base resin having a specific composition, a specific amount of inorganic filler containing metal carbonate, boehmite, and silica and / or calcined clay in specific ratios, and a specific amount of silane coupling agent are melt-mixed. Therefore, it is believed that at least boehmite, silica and / or calcined clay can be incorporated into the crosslinked structure, and a crosslinked structure involving these inorganic fillers and a crosslinked structure not involving inorganic fillers can be constructed in a balanced manner, and as a result, a silane-crosslinked resin formed body can be produced which combines the above six properties and preferably also has excellent appearance.
[0085] [Molded products] The molded article of the present invention is a product (including semi-finished products, parts, and members) containing the silane-crosslinked resin molded article of the present invention, and can be used as various resin molded articles, and can preferably be used as a replacement for conventional resin molded articles. The molded article of the present invention may be a molded article containing the silane-crosslinked resin molded article of the present invention in a part thereof (resin molded part), or may be a molded article consisting only of the silane-crosslinked resin molded article of the present invention. Applications of the molded article of the present invention include, for example, covering materials for wiring materials such as insulated electric wires, cables, and optical fiber cables, materials for electric wires and cables as a rubber substitute, as well as heat-resistant parts for microwave ovens or gas ranges, heat-resistant electric wire parts, heat-resistant sheets, heat-resistant films, etc. Further applications include power plugs, connectors, sleeves, boxes, tape substrates, tubes, sheets, heat-resistant packings, cushioning materials, vibration-proofing materials, wiring materials used for internal wiring and external wiring of electric and electronic devices, particularly electric wires and optical fiber cables. The silane-crosslinked resin molded article of the present invention has the above-mentioned excellent properties, and even when exposed to wind and rain and subjected to repeated vibration, it can prevent damage due to its excellent flexibility. Moreover, in addition to heat resistance and tensile strength, it also has properties required for outdoor molded articles, such as long-term insulation properties, tracking resistance, and deliquescence resistance. Therefore, the molded article of the present invention is suitable as a molded article (outdoor molded article) that can be used for outdoor applications exposed to wind and rain for a long period of time by utilizing the above-mentioned excellent properties, and shows stable properties for a long period of time. Specific examples of outdoor molded articles include outdoor wiring materials, outdoor industrial electric wires (e.g., jumper wires, cab-tire cables), charging cables, insulator materials, etc.
[0086] When the molded article of the present invention is used as a wiring material, the molded article of the present invention is usually used as a covering material (insulator, sheath) for a conductor. The wiring material may be a wiring material having a coating layer (sheath) on the outer periphery of a conductor, the coating layer being formed of the silane-crosslinked resin shaped product of the present invention by molding the silane-crosslinkable resin composition of the present invention into a tubular layer and crosslinking it. When the coating layer of the wiring material is composed of a plurality of layers, it is sufficient that at least one of the layers is formed of the silane-crosslinked resin shaped product of the present invention. The wiring material is the same as a conventional one used in various electric and electronic equipment fields and industrial fields, except that the coating layer is formed of the silane crosslinked resin molded product of the present invention. The coating layer formed of the silane crosslinked resin molded product of the present invention is provided directly or via another layer on the outer peripheral surface of the conductor, and the presence or absence of other layers, materials, etc. are appropriately determined according to the type, use, required characteristics, etc. of the wiring material. A conventional conductor can be used, for example, a single wire or a twisted wire (a wire in which tensile strength fibers are vertically attached or twisted) of soft copper, copper alloy, or aluminum. In addition to bare wires, tin-plated wires and wires having an enamel-coated insulating layer can also be used. Generally, wiring materials having aluminum conductors are easily broken (easily broken) due to bending or curvature, but the wiring material as the molded product of the present invention has a coating layer made of a silane crosslinked resin molded product that exhibits the above six characteristics, especially excellent flexibility, so that aluminum can be suitably applied as a conductor. The thickness of the coating layer formed of the silane crosslinked resin molded product of the present invention is not particularly limited, but is usually about 0.15 to 5 mm.
[0087] The wiring material as the molded article of the present invention can be produced by various molding methods in the above step (2), for example, by molding with an extruder or injection molding machine, followed by contacting with water. Preferably, it can be produced by molding (arranging) the silane crosslinkable resin composition of the present invention into a tubular shape around the outer periphery of a conductor, followed by crosslinking reaction (silanol condensation reaction). For example, in the above-mentioned method for producing a silane crosslinked resin molded article of the present invention, the wiring material can be produced by co-extrusion molding the silane crosslinkable resin composition around the outer periphery of a conductor using a general-purpose coating device (extruder) in step (2). EXAMPLES
[0088] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0089] The compounds used in the examples and comparative examples are shown below. <Base resin> LLDPE: Evolu SP0540 (product name, manufactured by Prime Polymer, linear low-density polyethylene resin) PP: PB222A (product name, Sanallomer Co., Ltd., random polypropylene resin) EPDM: EPT3092PM (product name, manufactured by Mitsui Chemicals, ethylene-propylene-ethylidene norbornene rubber, ethylene content 65% by mass, diene content 4.6% by mass) Styrene-based elastomer: Tuftec N504 (product name, manufactured by Asahi Kasei Corporation, SEBS) Oil: Cosmo Neutral 500 (product name, Cosmo Oil Lubricants, paraffin oil) <Inorganic filler> Calcium carbonate: Softon 2200 (product name, manufactured by Bihoku Funka Kogyo Co., Ltd., average particle size 1 μm) Boehmite: Boehmite FKB-104 (product name, manufactured by Konoshima Chemical Co., Ltd., average secondary particle size 1.2 μm, BET surface area ratio 6 m 2 / g) Silica: Crystallite 5X (product name, manufactured by Takimori Co., Ltd., BET surface area ratio 12 m 2 / g, average particle size 1.2μm) Calcined clay: SATINTONE SP33 (product name, manufactured by BASF, average particle size 1.3 μm) Talc: Microace K-1 (product name, manufactured by Nippon Talc Co., Ltd.) Magnesium hydroxide: Magseeds FK621 (product name, manufactured by Konoshima Chemical Co., Ltd.) <Silane coupling agent> Silane coupling agent: KBM-1003 (product name, manufactured by Shin-Etsu Chemical Co., Ltd., vinyltrimethoxysilane) <Organic peroxide> Organic peroxide: Perhexa 25B (trade name, NOF Corp., 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, decomposition temperature 179°C) <Silanol condensation catalyst> Silanol condensation catalyst: Adeka STAB OT-1 (trade name, manufactured by ADEKA Corporation, dioctyltin dilaurate) <Antioxidants> Antioxidant: Irganox 1076 (product name, manufactured by BASF, hindered phenol antioxidant)
[0090] (Examples 1 to 13 and Comparative Examples 1 to 13) Examples 1 to 13 and Comparative Examples 1 to 13 were carried out using the components shown in Tables 1 to 4, respectively. In each of the Examples and Comparative Examples, a portion of the base resin (specifically, the component shown in the "Base Resin" column of the "Catalyst MB" column in Tables 1 to 4) was used as a carrier resin for catalyst MB in the mass ratio shown in the same column. In Tables 1 to 4, the numerical values for the mixed amount (content) of each example are in parts by mass unless otherwise specified. Furthermore, a blank for each component means that the mixed amount of the corresponding component is 0 parts by mass. Furthermore, the content of each component shown in the "Silane crosslinkable resin composition" column in Tables 1 to 4 indicates the total content of each component in the silane crosslinkable resin composition (molten mixture of silane MB and catalyst MB).
[0091] First, the inorganic filler, the silane coupling agent, and the organic peroxide were charged into a rotary blade mixer (Mazera PM: product name, manufactured by Mazera Co., Ltd.) in the mass ratio shown in the Silane MB column of Tables 1 to 4, and stirred (premixed) at room temperature (25°C) and a rotation speed of 10 rpm for 1 minute (step (a-1)). In this way, the above components were dry-mixed to obtain a powder mixture. Next, the powder mixture and the base resin and antioxidant shown in the "Silane MB" column of Tables 1 to 4 were added to a kneader (volume 75 L) preheated to 100°C in the mass ratio shown in the same column, and mixed at 40 rpm for 5 minutes, and then finish kneaded (melt mixed) at 30 rpm for an additional 3 minutes. After confirming that the temperature of the mixture had reached 180 to 200°C, which is higher than the decomposition temperature of the organic peroxide, a feeder-ruder was used to obtain Silane MB (step (a-2)).
[0092] On the other hand, the base resin, silanol condensation catalyst, and antioxidant shown in the "Catalyst MB" column of Tables 1 to 4 were sequentially charged in the mass ratios shown in the same column into a kneader (volume 75 L) preheated to 80°C, mixed at a rotation speed of 30 rpm for 5 minutes, and then finish kneaded (melt mixed) at a rotation speed of 25 rpm for 3 minutes. After confirming that the temperature of the mixture reached about 180°C and the carrier resin was sufficiently melted, catalyst MB was obtained using a feeder-ruder (step (b)).
[0093] Next, Silane MB and Catalyst MB were dry-blended in a tumbler mixer at room temperature (25°C) for 2 minutes immediately before extrusion in the mass ratios shown in the "Silane MB" and "Catalyst MB" columns of Tables 1 to 4 to obtain a dry blend (dry blending step (c)). The obtained dry blend was then introduced into an extruder (cylinder temperature 130°C, crosshead temperature 180°C) equipped with a screw having a screw diameter of 25 mm and L / D=25. While the dry blend was being melt-mixed in the extruder (step (c)), the silane crosslinkable resin composition was extrusion-coated at a thickness of 0.8 mm onto the outer circumferential surface of a copper conductor having a diameter of 0.8 mm at a linear speed of 10 m / min to obtain a coated conductor having an outer diameter of 2.4 mm (coating thickness of 0.8 mm) (step (2)). This coated conductor was left in an atmosphere having a temperature of 60° C. and a humidity of 95% for 24 hours to come into contact with water (step (3)). In this manner, an insulated wire having a coating layer made of a silane crosslinked resin molded product on the outer peripheral surface of the conductor was produced.
[0094] The following tests were carried out on each of the produced insulated wires, and the results are shown in Tables 1 to 4.
[0095] <Test 1: Extrusion appearance test> The appearance of each insulated wire produced was observed. This test was a reference test. As an insulated wire, a wire with a clean surface, no visible gel particles, and excellent appearance was rated as "A (good)". A wire with 1 to 5 gel particles per meter on the surface but no problem with the appearance as an insulated wire was rated as "B (good)". A wire with a large number of gel particles or roughness on the surface and a poor appearance as an insulated wire was rated as "D" (fail).
[0096] <Test 2: Mechanical property test> A tensile test was carried out on the covering layer (tubular piece) obtained by removing the conductor from each of the produced insulated wires. This tensile test was conducted in accordance with JIS C 3005, with a gauge length of 25 mm and a tensile speed of 200 mm / min, and the tensile strength (MPa), 100% modulus (MPa) and tensile elongation (%) were measured. In this test, a tensile strength of 14 MPa or more was rated as "A (excellent)", 12 MPa or more but less than 14 MPa was rated as "B (good)", 10 MPa or more but less than 12 MPa was rated as "C (acceptable)", and less than 10 MPa was rated as "D (fail)". The 100% modulus is one of the indices used to evaluate flexibility. In this test, a value of 5 MPa or less was rated as "A (excellent)", a value between 5 MPa and 6 MPa was rated as "B (good)", a value between 6 MPa and 7 MPa was rated as "C (acceptable)", and a value over 7 MPa was rated as "D (fail)". In this test, tensile elongation of 400% or more was rated as "A (excellent)", 350% or more but less than 400% was rated as "B (good)", 300% or more but less than 350% was rated as "C (acceptable)", and less than 300 was rated as "D (fail)".
[0097] <Test 3: Heat deformation test> A heat deformation test was performed on the coating layer (tubular piece) obtained by removing the conductor from each of the manufactured insulated wires in accordance with JIS C 3005, and the heat deformation rate (reduction rate) was calculated from the thickness of the coating layer after heating and the thickness before heating. The heating temperature was 120°C, and the applied load was 5N. The results of this test (heat deformation rate) are used as an index to evaluate heat resistance, with a result of less than 20% being rated as "A (excellent)", a result between 20% and 30% being rated as "B (good)", a result between 30% and 40% being rated as "C (acceptable)", and a result of 40% or more being rated as "D (fail)".
[0098] <Test 4: Tracking resistance test> The test specimens were round bars (φ10 mm) made from the same material as each insulated wire. In accordance with JIS C 3005, the distance between the electrodes was 100 mm, a voltage of 4 kV was applied, and 0.2% saline solution (conductivity 3,000 μS / cm) was sprayed periodically in a cycle of 10 seconds spray followed by a 20 second break. In this test, the spray cycle was changed from the set value of 101 times in the above standard to 500 times, and if a current of 0.5A or more did not flow or there were no abnormalities such as combustion, it was rated as "A (pass)", and if an abnormality was found, it was rated as "D (fail)".
[0099] <Test 5: Acid resistance test> The test specimens used were the coating layers (tubular pieces) obtained by removing the conductors from the respective insulated wires produced. 5 g of the test piece was weighed out and immersed in 50 mL of each of the four types of acid solutions listed below at 50° C. for 168 hours. The test piece was then removed and its mass WA (g) was measured. For each acid solution, the mass change rate (%) of the test piece before and after immersion was calculated using the following formula. Acid solution: 10% by mass sulfuric acid, 10% by mass nitric acid, 10% by mass hydrochloric acid, and 10% by mass acetic acid Formula: Mass change rate (%) = [WA(g)-5(g)] / 5(g) x 100 In this test, samples whose mass change rate before and after immersion in all acids was within 5% were rated as "A (pass)", and samples whose mass change rate exceeded 5% in one or more acids were rated as "D (fail)".
[0100] <Test 6: Insulation resistance test> In accordance with JIS C 3005, 10 m of each manufactured insulated electric wire was used as a test specimen, which was immersed in a water tank at 20°C for 24 hours to measure the insulation resistance value. The measurement voltage, charging time, and measurement time were 500 V, 10 seconds, and 50 seconds, respectively. The measurements were performed 1 hour and 28 days after immersion in water. The insulation resistance value after one hour of immersion serves as an index for evaluating short-term insulation resistance, and the insulation resistance value after 28 days of immersion serves as an index for evaluating long-term insulation resistance. In this test, insulation resistance values after one hour of immersion and after 28 days of immersion were classified as "A (excellent)" if they were 10,000 MΩ·km or more, "B (good)" if they were 6,000 MΩ·km or more and less than 10,000 MΩ·km, "C (acceptable)" if they were 3,000 MΩ·km or more and less than 6,000 MΩ·km, and "D (fail)" if they were less than 3,000 MΩ·km.
[0101] [Table 1]
[0102] [Table 2]
[0103] [Table 3]
[0104] [Table 4]
[0105] The results in Tables 1 to 4 reveal the following: In step (1), Comparative Examples 1 to 13, which do not satisfy the mixing amount of any of the base resin, organic peroxide, silane coupling agent, and inorganic filler, are all inferior in any of the properties of heat resistance, tensile strength, long-term insulation properties, tracking resistance, deliquescence resistance, and flexibility, and a silane-crosslinked resin molded article having all of these properties cannot be realized. In contrast, in a specific silane crosslinking method using 0.01 to 0.3 parts by mass of an organic peroxide, Examples 1 to 13, in which a specific proportion of a silane coupling agent and a specific proportion of an inorganic filler combining metal carbonate, boehmite, silica, etc. in a total content of 100 to 150 parts by mass are mixed with 100 parts by mass of a base resin containing at least one of a polyolefin resin and an ethylene rubber, all of which are excellent in heat resistance, tensile strength, long-term insulation properties, tracking resistance, deliquescence resistance and flexibility, and can realize a silane crosslinked resin molded product that combines all of these properties.
Claims
1. A method for producing a silane-crosslinkable resin composition, comprising: (1) melt-mixing 0.01 to 0.3 parts by mass of an organic peroxide, 100 to 150 parts by mass of an inorganic filler, 2 to 10 parts by mass of a silane coupling agent, and a silanol condensation catalyst relative to 100 parts by mass of a base resin to obtain a mixture, the base resin contains at least one of a polyolefin resin and an ethylene rubber, and contains the polyolefin resin in an amount of 100% by mass or less, the ethylene rubber in an amount of 100% by mass or less, a styrene-based elastomer in an amount of 35% by mass or less, and an oil in an amount of 40% by mass or less; The inorganic filler contains 10 to 35 parts by mass of metal carbonate, 20 to 55 parts by mass of boehmite, and 45 to 90 parts by mass of silica and / or calcined clay, within the range of the mixing amount of the inorganic filler, A method for producing a silane-crosslinkable resin composition, wherein, in carrying out the step (1), when the whole of the base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), and (c) below, and, on the other hand, when a part of the base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), (b), and (c) below. Step (a-1): Mixing the inorganic filler and the silane coupling agent. A process for preparing a product Step (a-2): The mixture and all or a part of the base resin are mixed with the organic peroxide. In the presence of the organic peroxide, at a temperature equal to or higher than the decomposition temperature of the organic peroxide, Melt mixing to prepare a silane master batch. Step (b): The remainder of the base resin and the silanol condensation catalyst are melt-mixed to form a catalyst. A process for preparing a catalyst master batch Step (c): The silane master batch and the silanol condensation catalyst or the catalyst master batch are mixed. A process of melt mixing with the star batch.
2. A method for producing a silane-crosslinked resin molded product, comprising the following steps (1), (2) and (3): Step (1): 0.01 to 0.3 parts by mass of an organic peroxide based on 100 parts by mass of a base resin parts by mass, 100 to 150 parts by mass of inorganic filler, and 2 parts by mass of silane coupling agent and a silanol condensation catalyst to obtain a mixture. Process Step (2): A step of molding the mixture obtained in the step (1) to obtain a molded body. Step (3): The molded body obtained in step (2) is contacted with water to form a silane-crosslinked resin compound. The process of obtaining a shape the base resin contains at least one of a polyolefin resin and an ethylene rubber, and contains the polyolefin resin in an amount of 100% by mass or less, the ethylene rubber in an amount of 100% by mass or less, a styrene-based elastomer in an amount of 35% by mass or less, and an oil in an amount of 40% by mass or less; The inorganic filler contains 10 to 35 parts by mass of metal carbonate, 20 to 55 parts by mass of boehmite, and 45 to 90 parts by mass of silica and / or calcined clay, within the range of the mixing amount of the inorganic filler, A method for producing a silane-crosslinked resin molded product, wherein, in carrying out the step (1), when the entire base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), and (c) below, and, on the other hand, when a part of the base resin is melt-mixed in the step (a-2) below, the step (1) comprises the steps (a-1), (a-2), (b), and (c) below. Step (a-1): Mixing the inorganic filler and the silane coupling agent. A process for preparing a product Step (a-2): The mixture and all or a part of the base resin are mixed with the organic peroxide. In the presence of the organic peroxide, at a temperature equal to or higher than the decomposition temperature of the organic peroxide, Melt mixing to prepare a silane master batch. Step (b): The remainder of the base resin and the silanol condensation catalyst are melt-mixed to form a catalyst. A process for preparing a catalyst master batch Step (c): The silane master batch and the silanol condensation catalyst or the catalyst master batch are mixed. A process of melt mixing with the star batch.
3. The method according to claim 1, wherein the base resin contains 50% by mass or less of a polyolefin resin, 10 to 100% by mass of an ethylene rubber, 35% by mass or less of a styrene-based elastomer, and 40% by mass or less of an oil.
4. The method according to claim 2, wherein the base resin contains 50% by mass or less of a polyolefin resin, 10 to 100% by mass of an ethylene rubber, 35% by mass or less of a styrene-based elastomer, and 40% by mass or less of an oil.
5. The manufacturing method according to claim 1, wherein the base resin contains 20 to 40% by mass of a polyolefin resin, 10 to 45% by mass of an ethylene rubber, 10 to 35% by mass of a styrene-based elastomer, and 20 to 40% by mass of an oil.
6. The manufacturing method according to claim 2, wherein the base resin contains 20 to 40% by mass of a polyolefin resin, 10 to 45% by mass of an ethylene rubber, 10 to 35% by mass of a styrene-based elastomer, and 20 to 40% by mass of an oil.
7. A silane-crosslinkable resin composition produced by the process according to any one of claims 1, 3 and 5.
8. A silane-crosslinked resin molded article produced by the method according to any one of claims 2, 4 and 6.
9. A molded article comprising the silane-crosslinked resin molded article according to claim 8.
Citation Information
Patent Citations
Production of crosslinked polyolefin-based rubber molded product
JP1999124438A
Crosslinked resin molded body, crosslinkable resin composition and manufacturing method of them, silane masterbatch and molded article
JP2016074853A
Crosslinked resin molded body, crosslinkable resin composition and manufacturing method therefor, silane master batch and molded article
JP2018111834A
Crosslinked resin molded body, crosslinkable resin composition, manufacturing method therefor, silane masterbatch, and molded article
WO2016056635A1
Flame-retardant crosslinked resin molded article, production method therefor, silane masterbatch, masterbatch mixture, molded article thereof, and flame-retardant product
WO2018180689A1