Method for producing fine cellulose fiber dried material
The method improves efficiency and maintains thixotropic properties of dried cellulose fibers by stirring and vacuum drum drying with a ceramic-coated drum, addressing the inefficiencies of existing methods.
Patent Information
- Application Number
- JP2023043837
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Existing methods for producing dried fine cellulose fibers, such as vacuum drum drying, face challenges in improving raw material input efficiency and production efficiency, and the dried fibers often lose their thixotropic properties due to hydrogen bonding and heat denaturation.
A method involving a stirring step followed by vacuum drum drying at controlled temperatures and pressures, using a ceramic-coated drum, with a specific concentration of fine cellulose fibers, dispersant, and solvent, to maintain fiber integrity and redispersibility.
The method enhances raw material input efficiency and production efficiency while preserving the thixotropic properties of the dried cellulose fibers, reducing heat-induced denaturation and improving redispersibility.
Smart Images

Figure 2024133846000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a dried fine cellulose fiber material. [Background technology]
[0002] Cellulose nanofibers and microfibrillated cellulose (hereinafter collectively referred to as "fine cellulose fibers") obtained by micronizing cellulose are fine fibers with diameters on the nano to micro order. As new materials with properties not found in ordinary pulp, such as high strength, high elasticity, and thixotropy, they are expected to be used in a variety of fields.
[0003] Generally, cellulose nanofibers are produced in a state where they are stably dispersed in water, and are usually used for various purposes as industrial materials or additives to foods and cosmetics in the state of a cellulose nanofiber dispersion of a specified concentration. In order to keep the state of cellulose nanofibers stable, moisture about several tens of times the amount of cellulose nanofiber is required, and this high moisture content leads to increased costs for packaging, storage, transportation, etc. of cellulose nanofibers, so reducing (concentrating) and removing (drying) the moisture has been considered an essential technology for promoting the spread of cellulose nanofibers.
[0004] Freeze-drying and critical point drying have been proposed as methods for drying cellulose nanofibers in a state dispersed in water (wet state) (Patent Document 1). However, freeze-drying and critical point drying have a problem in that they require a large amount of energy.
[0005] Furthermore, when fine cellulose fibers dispersed in water (wet state) are dried to form a dry body, hydrogen bonds are formed between the fibers of the fine cellulose fibers. Therefore, even if water is added to this dry body again to redisperse it, the viscosity characteristics, etc. cannot be restored to the same level as before drying, and the excellent properties of the fine cellulose fibers cannot be exhibited.
[0006] As a technique for obtaining a dried product of fine cellulose fibers that is easily redispersible, a method of drying a mixture of fine cellulose fibers and a solvent using a vacuum drum dryer (Patent Document 2) has been proposed.
[0007] The vacuum drum dryer has the advantage of being able to dry at low temperatures below 100°C, which prevents the denaturation of fine cellulose fibers due to heat. In addition, the heat of the drum directly touches the sample, which has the advantage of high thermal efficiency and making the device compact. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 6-233691 [Patent Document 2] International Publication No. 2019 / 189318 Summary of the Invention [Problem to be solved by the invention]
[0009] However, even when a vacuum drum dryer is used, there is a demand for further improvement in raw material input efficiency and production efficiency.
[0010] Therefore, an object of the present invention is to provide a method for producing a dried material of fine cellulose fibers, which has excellent raw material input efficiency and production efficiency when a vacuum drum dryer is used. [Means for solving the problem]
[0011] As a result of extensive research into achieving this object, the present inventors have discovered that it is extremely effective to carry out stirring of the raw material before feeding it into a vacuum drum dryer, and have completed the present invention.
[0012] The present invention provides the following: (1) A method for producing a dried fine cellulose fiber product, comprising: a stirring step of stirring a mixture containing fine cellulose fibers, a dispersant, and an aqueous solvent and having a solid content concentration of 1 to 10 mass %, and a drying step of drying the mixture after the stirring step at a temperature of 40 to 100°C under reduced pressure using a vacuum drum dryer. (2) The method for producing a dried fine cellulose fiber material according to (1), wherein the vacuum drum dryer is provided with a drum having a ceramic spray coating formed on its surface by thermal spraying. (3) The method for producing a dried fine cellulose fiber material according to (1) or (2), wherein the fine cellulose fiber is a carboxylated cellulose nanofiber, and the dispersant is carboxymethyl cellulose. (4) The method for producing a dried fine cellulose fiber material according to (1) or (2), wherein in the mixture, a compounding ratio (parts by mass) of the fine cellulose fiber (bone dry solid content) to the dispersant is in the range of 5:5 to 8:2. Effect of the Invention
[0013] According to the present invention, a method for producing a dried material of fine cellulose fibers having excellent raw material input efficiency and production efficiency when a vacuum drum dryer is used can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below. In the present invention, "to" includes the end values. That is, "X to Y" includes the values X and Y at both ends.
[0015] The present invention includes a stirring step of stirring a mixture containing fine cellulose fibers, a dispersant, and an aqueous solvent and having a solid content concentration of 1 to 10 mass %, and a drying step of drying the mixture that has undergone the stirring step at a temperature of 40 to 100°C under reduced pressure using a vacuum drum dryer.
[0016] (Microfine cellulose fiber) The fine cellulose fibers used in the present invention are fine fibers made from cellulose, and are a general term for cellulose nanofibers (hereinafter sometimes referred to as "CNF") having an average fiber diameter of less than 500 nm and microfibrillated cellulose (hereinafter sometimes referred to as "MFC") having an average fiber diameter of 500 nm or more. The average fiber diameter is a length-weighted average fiber diameter, and can be measured by observing the fine cellulose fibers using, for example, a fractionator manufactured by Valmet Co., Ltd. or an atomic force microscope (AFM). The average fiber diameter of the fine cellulose fibers is not particularly limited, but is about 1 nm to 60 μm. The fine cellulose fibers can be produced by defibrating cellulose.
[0017] (Cellulose nanofiber (CNF)) The average fiber diameter of the CNF that can be used in the present invention is preferably 100 nm or less, more preferably 50 nm or less. The average fiber length is preferably 5 μm or less, more preferably 3 μm or less. The lower limit of the average fiber length is about 0.1 μm or more. The average fiber length can be measured by analyzing 200 randomly selected fibers using an atomic force microscope (AFM) when the diameter is less than 20 nm, or a field emission scanning electron microscope (FE-SEM) when the diameter is 20 nm or more, and calculating the average. The average aspect ratio of the CNF that can be used in the present invention is preferably 50 or more. The upper limit is not particularly limited, but is usually 1000 or less. The average aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter
[0018] (Microfibrillated Cellulose (MFC)) The average fiber length of the MFC that can be used in the present invention is preferably 5 μm or more, more preferably 200 μm or more. The upper limit of the average fiber length is preferably 2.0 mm or less, more preferably about 1.5 mm or less. The average fiber length (length-weighted average fiber length) can be determined by measurement using a fractionator manufactured by Valmet Co., Ltd.
[0019] The cellulose raw material is not particularly limited as long as it contains cellulose, and examples thereof include plants (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), bleached kraft pulp (BKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc.), animals (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), microbial products, and the like. The cellulose raw material may be any one of these or a combination of two or more types, but is preferably a cellulose raw material derived from a plant or a microorganism (e.g., cellulose fiber), and more preferably a cellulose raw material derived from a plant (e.g., cellulose fiber).
[0020] The number average fiber diameter of the cellulose raw material is not particularly limited, but in the case of softwood kraft pulp, which is a common pulp, it is about 30 to 60 μm, and in the case of hardwood kraft pulp, it is about 10 to 30 μm. In the case of other pulps, those that have undergone general refining have a diameter of about 50 μm. For example, in the case of refining chips or the like that are several centimeters in size, it is preferable to adjust the diameter to about 50 μm by mechanical processing using a disintegrator such as a refiner or beater.
[0021] Cellulose has three hydroxyl groups per glucose unit and can be chemically modified in various ways. In the present invention, from the viewpoint of promoting the progress of defibration, it is preferable to use chemically modified fine cellulose fibers produced by defibrating a cellulose raw material (chemically modified cellulose) obtained by chemical modification.
[0022] Examples of chemical modification include carboxylation (oxidation), carboxymethylation, cationization, esterification, etc. Among these, carboxylation (oxidation) is more preferable.
[0023] (chemical modification) (Carboxylation) In the present invention, when using carboxylated fine cellulose fibers obtained by defibrating carboxylated (oxidized) cellulose, the carboxylated cellulose (also called oxidized cellulose) can be obtained by carboxylating (oxidizing) the above-mentioned cellulose raw material by a known method. Although not particularly limited, during carboxylation, it is preferable to adjust the amount of carboxyl groups to 0.6 to 2.0 mmol / g, and more preferably to adjust to 1.0 mmol / g to 2.0 mmol / g, based on the bone dry mass of the chemically modified fine cellulose fibers.
[0024] One example of a carboxylation (oxidation) method is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound and a compound selected from the group consisting of bromides, iodides, or a mixture thereof. This carboxylation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the glucopyranose ring on the cellulose surface, resulting in the formation of aldehyde groups and carboxyl groups (-COOH) or carboxylate groups (-COO - The concentration of cellulose during the reaction is not particularly limited, but is preferably 5% by mass or less.
[0025] The term "N-oxyl compound" refers to a compound capable of generating a nitroxy radical. Any compound that can promote the desired oxidation reaction can be used as the N-oxyl compound. For example, 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO) can be mentioned.
[0026] The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the raw cellulose. For example, the amount is preferably 0.01 to 10 mmol, more preferably 0.01 to 1 mmol, and even more preferably 0.05 to 0.5 mmol per 1 g of bone dry cellulose. Also, the amount is preferably about 0.1 to 4 mmol / L relative to the reaction system.
[0027] Bromides are compounds containing bromine, examples of which include alkali metal bromides that can dissociate and ionize in water. Also, iodides are compounds containing iodine, examples of which include alkali metal iodides. The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is, for example, preferably 0.1 to 100 mmol, more preferably 0.1 to 10 mmol, and even more preferably 0.5 to 5 mmol, per 1 g of bone-dry cellulose.
[0028] The oxidizing agent may be a known one, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxide, peroxide, etc. Among them, sodium hypochlorite is preferable because it is inexpensive and has a low environmental impact. The amount of the oxidizing agent used is preferably 0.5 to 500 mmol, more preferably 0.5 to 50 mmol, even more preferably 1 to 25 mmol, and most preferably 3 to 10 mmol, per 1 g of bone-dry cellulose. Also, for example, the amount is preferably 1 to 40 mol per 1 mol of the N-oxyl compound.
[0029] The carboxylation of cellulose can be efficiently carried out even under relatively mild conditions. Therefore, the reaction temperature is preferably 4 to 40°C, and may be room temperature of about 15 to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, and a decrease in the pH of the reaction solution is observed. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution to maintain the pH of the reaction solution at about 8 to 12, preferably 10 to 11. The reaction medium is preferably water, because it is easy to handle and does not easily cause side reactions.
[0030] The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually from 0.5 to 6 hours, for example, about 0.5 to 4 hours.
[0031] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtration after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first-stage reaction.
[0032] Another example of the carboxylation (oxidation) method is a method in which the cellulose raw material is oxidized by contacting it with an ozone-containing gas. This oxidation reaction oxidizes at least the hydroxyl groups at positions 2 and 6 of the glucopyranose ring, and decomposes the cellulose chain. The ozone concentration in the ozone-containing gas is 50 to 250 g / m 3 It is preferable that the thickness is 50 to 220 g / m 3 It is more preferable that the ozone is added to the cellulose raw material in an amount of 0.1 to 30 parts by mass, and more preferably 5 to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material. The ozone treatment temperature is preferably 0 to 50°C, and more preferably 20 to 50°C. The ozone treatment time is not particularly limited, but is about 1 to 360 minutes, and is preferably about 30 to 360 minutes. When the ozone treatment conditions are within these ranges, it is possible to prevent cellulose from being excessively oxidized and decomposed, and the yield of oxidized cellulose is good. After the ozone treatment, an oxidizing agent may be used to perform a post-oxidation treatment. The oxidizing agent used in the post-oxidation treatment is not particularly limited, but examples thereof include chlorine-based compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, these oxidizing agents are dissolved in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and the cellulose raw material is immersed in the solution to perform the post-oxidation treatment.
[0033] The amount of carboxyl groups in the carboxylated cellulose can be adjusted by controlling the reaction conditions such as the amount of the oxidizing agent added and the reaction time.
[0034] (Carboxymethylation) In the present invention, when using carboxymethylated fine cellulose fibers obtained by fibrillating carboxymethylated cellulose, the carboxymethylated cellulose may be obtained by carboxymethylating the above-mentioned cellulose raw material by a known method, or a commercially available product may be used. In either case, it is preferable that the degree of carboxymethyl group substitution per anhydrous glucose unit of cellulose is 0.01 to 0.50. An example of a method for producing such carboxymethylated cellulose can be mentioned as follows. Cellulose is used as a starting material, and 3 to 20 times by mass of water and / or lower alcohol, specifically water, methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc., are used as a solvent, or a mixture of two or more of them are used. In addition, when a lower alcohol is mixed, the mixing ratio of the lower alcohol is 60 to 95% by mass. As a mercerizing agent, 0.5 to 20 times mol of an alkali metal hydroxide, specifically sodium hydroxide or potassium hydroxide, is used per anhydrous glucose residue of the starting material. The starting material, solvent, and mercerizing agent are mixed, and a mercerization treatment is carried out at a reaction temperature of 0 to 70° C., preferably 10 to 60° C., for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Then, 0.05 to 10.0 times the moles of a carboxymethylating agent per glucose residue is added, and an etherification reaction is carried out at a reaction temperature of 30 to 90° C., preferably 40 to 80° C., for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours.
[0035] In this specification, "carboxymethylated cellulose", which is a type of chemically modified cellulose used in the preparation of fine cellulose fibers, refers to cellulose that maintains at least a part of its fibrous shape even when dispersed in water. Therefore, it is distinguished from carboxymethyl cellulose, which is a type of water-soluble polymer. When an aqueous dispersion of "carboxymethylated cellulose" is observed with an electron microscope, a fibrous substance can be observed. On the other hand, when an aqueous dispersion of carboxymethyl cellulose, which is a type of water-soluble polymer, is observed, no fibrous substance is observed. In addition, when "carboxymethylated cellulose" is measured by X-ray diffraction, a peak of cellulose type I crystals can be observed, but cellulose type I crystals are not observed in carboxymethyl cellulose, a water-soluble polymer.
[0036] (cationization) In the present invention, the cationized fine cellulose fibers obtained by defibrating the carboxylated cellulose can be used. The cationized cellulose can be obtained by reacting the carboxylated cellulose raw material with a cationizing agent such as glycidyl trimethylammonium chloride, 3-chloro-2-hydroxypropyl trialkylammonium hydrite or its halohydrin type, and an alkali metal hydroxide (sodium hydroxide, potassium hydroxide, etc.) as a catalyst in the presence of water or an alcohol having 1 to 4 carbon atoms.
[0037] The degree of cationic substitution per glucose unit is preferably 0.02 to 0.50. By introducing cationic substituents into cellulose, the cellulose particles repel each other electrically. Therefore, cellulose into which cationic substituents have been introduced can be easily defibrated. If the degree of cationic substitution per glucose unit is less than 0.02, it cannot be defibrated sufficiently. On the other hand, if the degree of cationic substitution per glucose unit is more than 0.50, it may swell or dissolve, and may not be possible to obtain fine fibers. In order to perform defibration efficiently, it is preferable to wash the cationically modified cellulose raw material obtained above. The degree of cationic substitution can be adjusted by the amount of the cationizing agent to be reacted and the composition ratio of water or alcohol having 1 to 4 carbon atoms.
[0038] (Esterification) In the present invention, esterified fine cellulose fibers obtained by defibrating esterified cellulose can be used. The esterified cellulose can be obtained by mixing a powder or an aqueous solution of phosphoric acid compound A with the above-mentioned cellulose raw material, or by adding an aqueous solution of phosphoric acid compound A to a slurry of the cellulose raw material.
[0039] Examples of the phosphoric acid compound A include phosphoric acid, polyphosphoric acid, phosphorous acid, hypophosphorous acid, phosphonic acid, polyphosphonic acid, and esters thereof. These may be in the form of a salt. Among these, compounds having a phosphoric acid group are preferred because they are low cost, easy to handle, and can be introduced into the cellulose of the pulp fiber to improve the defibration efficiency. Examples of compounds having a phosphoric acid group include phosphoric acid, sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, sodium phosphite, potassium phosphite, sodium hypophosphite, potassium hypophosphite, sodium pyrophosphate, sodium metaphosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, potassium pyrophosphate, potassium metaphosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, triammonium phosphate, ammonium pyrophosphate, and ammonium metaphosphate. These can be used alone or in combination of two or more. Among these, phosphoric acid, sodium salts of phosphoric acid, potassium salts of phosphoric acid, and ammonium salts of phosphoric acid are more preferred from the viewpoints of high efficiency of phosphoric acid group introduction, ease of defibration in the defibration step described below, and ease of industrial application. Sodium dihydrogen phosphate and disodium hydrogen phosphate are particularly preferred. In addition, it is preferable to use the phosphoric acid compound A as an aqueous solution, since this increases the uniformity of the reaction and the efficiency of introducing the phosphoric acid group. The pH of the aqueous solution of the phosphoric acid compound A is preferably 7 or less, since this increases the efficiency of introducing the phosphoric acid group, but from the viewpoint of suppressing hydrolysis of the pulp fiber, a pH of 3 to 7 is preferable.
[0040] The following method can be given as an example of a method for producing cellulose phosphate. A phosphoric acid compound A is added to a dispersion of a cellulose raw material having a solid content concentration of 0.1 to 10% by mass while stirring to introduce a phosphoric acid group into the cellulose. When the cellulose raw material is taken as 100 parts by mass, the amount of phosphoric acid compound A added is preferably 0.2 to 500 parts by mass, more preferably 1 to 400 parts by mass, in terms of the amount of phosphorus element. If the proportion of phosphoric acid compound A is equal to or greater than the lower limit, the yield of fine cellulose fibers can be further improved. However, if the upper limit is exceeded, the effect of improving the yield reaches a plateau, which is not preferable from the viewpoint of cost.
[0041] In this case, in addition to the cellulose raw material and the phosphoric acid compound A, a powder or an aqueous solution of the other compound B may be mixed. The compound B is not particularly limited, but is preferably a nitrogen-containing compound exhibiting basicity. Here, "basicity" is defined as an aqueous solution exhibiting pink to red color in the presence of a phenolphthalein indicator, or an aqueous solution having a pH of more than 7. The nitrogen-containing compound exhibiting basicity used in the present invention is not particularly limited as long as it exhibits the effects of the present invention, but is preferably a compound having an amino group. Examples include, but are not limited to, urea, methylamine, ethylamine, trimethylamine, triethylamine, monoethanolamine, diethanolamine, triethanolamine, pyridine, ethylenediamine, and hexamethylenediamine. Among these, urea, which is low-cost and easy to handle, is preferred. The amount of compound B added is preferably 2 to 1000 parts by mass, more preferably 100 to 700 parts by mass, relative to 100 parts by mass of the solid content of the cellulose raw material. The reaction temperature is preferably 0 to 95°C, more preferably 30 to 90°C. The reaction time is not particularly limited, but is about 1 to 600 minutes, and more preferably 30 to 480 minutes. When the esterification reaction conditions are within these ranges, it is possible to prevent cellulose from being excessively esterified and becoming easily soluble, and the yield of phosphated cellulose is good. After the obtained phosphated cellulose suspension is dehydrated, it is preferable to heat treat it at 100 to 170°C from the viewpoint of suppressing hydrolysis of cellulose. Furthermore, it is preferable to heat it at 130°C or less, preferably 110°C or less while water is contained during the heat treatment, and after removing the water, heat treat it at 100 to 170°C.
[0042] The degree of phosphate substitution per glucose unit of the phosphoric acid esterified cellulose is preferably 0.001 to 0.40. By introducing a phosphoric acid group substituent into cellulose, the cellulose particles are electrically repelled from each other. Therefore, the cellulose into which the phosphoric acid group has been introduced can be easily defibrated. If the degree of phosphate substitution per glucose unit is less than 0.001, the cellulose cannot be defibrated sufficiently. On the other hand, if the degree of phosphate substitution per glucose unit is more than 0.40, the cellulose may swell or dissolve, and may not be obtained as fine cellulose fibers. In order to perform defibration efficiently, the phosphoric acid esterified cellulose raw material obtained above is preferably washed by boiling and then washing with cold water.
[0043] (Defibrilization) In the present invention, the device for defibrating the chemically modified cellulose is not particularly limited, but it is preferable to apply a strong shear force to the aqueous dispersion using a device such as a high-speed rotation type, a colloid mill type, a high-pressure type, a roll mill type, or an ultrasonic type. In particular, for efficient defibration, it is preferable to use a wet-type high-pressure or ultra-high-pressure homogenizer that can apply a pressure of 50 MPa or more to the aqueous dispersion and a strong shear force. The pressure is more preferably 100 MPa or more, and further preferably 140 MPa or more. Furthermore, prior to the defibration and dispersion treatment with the high-pressure homogenizer, it is also possible to subject the fine cellulose fibers to a pretreatment using a known mixing, stirring, emulsifying, and dispersing device such as a high-speed shear mixer, if necessary. The number of treatments (passes) in the defibration device may be one or more than two, and is preferably more than two.
[0044] In the dispersion treatment, the chemically modified cellulose is usually dispersed in a solvent. The solvent is not particularly limited as long as it can disperse the chemically modified cellulose, and examples thereof include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixtures thereof. Since the cellulose raw material is hydrophilic, the solvent is preferably water.
[0045] The solid content concentration of the chemically modified cellulose in the dispersion is usually 0.1% by mass or more, preferably 0.2% by mass or more, and more preferably 0.3% by mass or more. This allows the amount of liquid to be appropriate relative to the amount of cellulose fiber raw material, which is efficient. The upper limit is usually 10% by mass or less, and preferably 6% by mass or less. This allows fluidity to be maintained.
[0046] Prior to the defibration or dispersion treatment, a pretreatment may be carried out as necessary. The pretreatment may be carried out using a mixing, stirring, emulsifying or dispersing device such as a high-speed shear mixer.
[0047] When the chemically modified fine cellulose fibers obtained through the defibration step are in a salt form, they may be used as they are, or may be converted into an acid form by an acid treatment using a mineral acid, a method using a cation exchange resin, etc. Also, they may be used after being imparted with hydrophobicity by a method using a cationic additive.
[0048] (Dispersant) In the production method of the present invention, the mixture containing fine cellulose fibers to be subjected to the stirring step contains a dispersant from the viewpoint of improving the redispersibility of the dried body obtained after drying. Examples of the dispersant include water-soluble polymers, surfactants, etc., and it is preferable to use a water-soluble polymer because the water-soluble polymer covers the low charge density part on the surface of the chemically modified fine cellulose fibers, suppresses the formation of hydrogen bonds, and prevents the aggregation of the fine cellulose fibers during drying.
[0049] (Water-soluble polymer) Examples of water-soluble polymers that can be used in the production method of the present invention include cellulose derivatives (carboxymethylcellulose, methylcellulose, hydroxypropylcellulose, ethylcellulose), xanthan gum, xyloglucan, dextrin, dextran, carrageenan, locust bean gum, alginic acid, alginates, pullulan, starch, potato starch, kudzu starch, modified starch (cationized starch, phosphorylated starch, phosphate crosslinked starch, phosphate monoesterified phosphate crosslinked starch, hydroxypropyl starch, hydroxypropylated phosphate crosslinked starch, acetylated adipic acid crosslinked starch, acetylated phosphate crosslinked starch, acetylated oxidized starch, sodium octenylsuccinate starch, acetate starch, oxidized starch), corn starch, gum arabic, locust bean gum, alginic acid, alginates, pullulan, starch, potato starch, kudzu starch, modified starch (cationized starch, phosphorylated starch, phosphate crosslinked starch, phosphate monoesterified phosphate crosslinked starch, hydroxypropyl starch, hydroxypropylated phosphate crosslinked starch, acetylated adipic acid crosslinked starch, acetylated phosphate crosslinked starch, sodium octenylsuccinate starch, acetate starch, oxidized starch), corn starch, gum arabic, Examples of the suitable cellulose gum include tobean gum, gellan gum, polydextrose, pectin, chitin, water-soluble chitin, chitosan, casein, albumin, soy protein lysate, peptone, polyvinyl alcohol, polyacrylamide, sodium polyacrylate, polyvinylpyrrolidone, polyvinyl acetate, polyamino acid, polylactic acid, polymalic acid, polyglycerin, latex, rosin-based sizing agent, petroleum resin-based sizing agent, urea resin, melamine resin, epoxy resin, polyamide resin, polyamide-polyamine resin, polyethyleneimine, polyamine, vegetable gum, polyethylene oxide, hydrophilic crosslinked polymer, polyacrylate, starch polyacrylic acid copolymer, tamarind gum, guar gum, and colloidal silica, and mixtures of one or more thereof. Among these, cellulose derivatives are preferred in terms of their affinity with chemically modified fine cellulose fibers, and carboxymethylcellulose and its salts are particularly preferred. It is believed that water-soluble polymers such as carboxymethylcellulose and its salts penetrate between the fibers of fine cellulose fibers and increase the distance between the fibers, thereby improving redispersibility.
[0050] Examples of surfactants that can be used in the production method of the present invention include, but are not limited to, nonionic surfactants such as fatty acid salts, higher alkyl sulfates, alkylbenzene sulfonates, higher alcohols, alkylphenols, and alkylene oxide adducts of fatty acids, anionic surfactants, cationic surfactants, amphoteric surfactants, organic solvents, proteins, enzymes, natural polymers, synthetic polymers, etc. The surfactants may be composed of a single component of these or a mixture of two or more components.
[0051] When carboxymethylcellulose or a salt thereof is used as the water-soluble polymer, it is preferable to use a carboxymethylcellulose having a degree of substitution of carboxymethyl groups per anhydrous glucose unit of 0.55 to 1.6, more preferably 0.55 to 1.1, and even more preferably 0.65 to 1.1. In addition, a carboxymethylcellulose having a longer molecule (higher viscosity) is preferable because it has a higher effect of widening the distance between nanofibers. In addition, the B-type viscosity of a 1% by mass aqueous solution of carboxymethylcellulose at 25°C and 60 rpm is preferably 3 mPa·s to 14000 mPa·s, more preferably 7 mPa·s to 14000 mPa·s, and even more preferably 1000 mPa·s to 8000 mPa·s. Note that the "carboxymethylcellulose or a salt thereof" as the water-soluble polymer referred to here is completely dissolved in water, and is therefore distinguished from the above-mentioned carboxymethylated cellulose whose fiber shape can be confirmed in water.
[0052] In the mixture before stirring, the blending ratio of the fine cellulose fiber (bone dry solid content) to the dispersant is preferably 5:5 to 8:2, and more preferably 6:4 to 7:3, from the viewpoint of obtaining an effect of improving redispersibility. If the blending ratio of the dispersant is too high above the upper limit, problems such as viscosity characteristics such as thixotropy, which is a characteristic of the fine cellulose fiber, and a decrease in dispersion stability may occur. If the blending ratio of the dispersant is too low below the lower limit, sufficient redispersibility cannot be obtained.
[0053] (Water-based solvent) The aqueous solvent contained in the mixture before stirring used in the present invention may be water, a water-soluble organic solvent, or a mixed solvent of these. Since the cellulose raw material is hydrophilic, it is preferable to use water, which makes it easier to obtain a good dispersion state during dispersion.
[0054] The water-soluble organic solvent is an organic solvent that dissolves in water. Examples of the water-soluble organic solvent include methanol, ethanol, 2-propanol, butanol, glycerin, acetone, methyl ethyl ketone, 1,4-dioxane, N-methyl-2-pyrrolidone, tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, acetonitrile, and combinations thereof. Among them, lower alcohols having 1 to 4 carbon atoms such as methanol, ethanol, and 2-propanol are preferred, and from the viewpoints of safety and availability, methanol and ethanol are more preferred, and ethanol is even more preferred.
[0055] In the case of a mixed solvent, the amount of the water-soluble organic solvent in the mixed solvent is preferably 10% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. The upper limit of the amount is not limited, but is preferably 95% by mass or less, and more preferably 90% by mass or less. In addition, the aqueous solvent may contain a non-water-soluble organic solvent to the extent that the effect of the invention is not impaired.
[0056] The solid content of the mixture before stirring must be 1 to 10% by mass, preferably 1.5 to 8.0% by mass, and more preferably 2.0 to 7.0% by mass. If the solid content of the mixture is lower than the lower limit, the thickness of the film produced is small, and the heat applied to the fine cellulose fibers is large, which advances thermal denaturation, resulting in a poor dispersion state in the redispersion liquid of the obtained dried material. On the other hand, if the solid content is higher than the upper limit, the viscosity is high and there is a risk that the mixture will not be supplied between the drums.
[0057] The method for adjusting the solid content of the mixture before drying is not particularly limited, but may be a method of adding water and stirring with a homodisper.
[0058] (Method of producing dried body) The production method of the present invention includes a stirring step of stirring a mixture containing fine cellulose fibers, a dispersant, and an aqueous solvent and having a solid content concentration of 1 to 10 mass %, and a drying step of drying the mixture that has undergone the stirring step at a temperature of 40 to 100°C under reduced pressure using a vacuum drum dryer.
[0059] (Mixing process) The production method of the present invention includes a stirring step of stirring a mixture containing fine cellulose fibers, a dispersant, and an aqueous solvent. It is important that the stirring step is performed before the drying step, i.e., before the mixture is introduced into a vacuum drum dryer. By carrying out the stirring step before the mixture is introduced into the vacuum drum dryer, it is possible to improve the efficiency of introducing the mixture and the production efficiency of the dried body. The stirring method is not particularly limited as long as it can apply sufficient shear to the mixture, and stirring devices such as a high-function mixer, a ribbon mixer, a Max Blend, a two-stage turbine blade, an in-line mixer, etc., and pumps such as a centrifugal pump, a volute pump, a mono pump, etc. These stirrers may be used alone or in combination. The stirring conditions in the stirrer are not particularly limited since they depend on the type of stirrer, but are preferably 10 to 120 rpm, and more preferably 30 to 60 rpm. The stirred mixture is sent to a vacuum drum dryer described later, and a circulation line may be provided to return a portion of the mixture to the raw material input tank during the transfer. Here, the raw material input tank is a tank for storing the mixture to be input to the mixer, and the mixture stored in the raw material input tank is sent to the mixer by a specified pump or the like. The amount of the mixture returned to the raw material tank through the circulation line is not particularly limited, but is preferably 10 to 80%, more preferably 20 to 50%, of the mixture input to the mixer. By providing a circulation line, the mixture is subjected to shear to reduce its apparent viscosity, thereby providing it with fluidity.
[0060] From the viewpoint of the fluidity of the mixture, the viscosity of the mixture after the stirring step (i.e., the viscosity of the mixture before drying) is preferably 5000 to 100000 mPa s, and more preferably 10000 to 80000 mPa s. The viscosity of the mixture can be measured by a B-type viscometer.
[0061] (Vacuum drum dryer) A vacuum drum dryer is a device in which a heated drum is placed under vacuum or reduced pressure, and a mixture of fine cellulose fibers, a dispersant, and an aqueous solvent is continuously supplied to the drum surface while the drum is rotating, and the aqueous solvent is evaporated and concentrated, while at the same time, a thin film of fine cellulose fibers and a dispersant is adhered to the drum surface and dried, and the dried material formed on the drum surface is scraped off with a knife such as a doctor blade provided in the vacuum drum dryer, thereby producing a dried body.
[0062] When drying is performed in a vacuum or under reduced pressure, drying is preferably performed within the range of 0 to 50 kPa. Since moisture can be evaporated at a lower temperature at a lower pressure, the pressure is preferably 50 kPa or less, more preferably 30 kPa or less, and even more preferably 10 kPa or less.
[0063] In the present invention, the drying temperature means the temperature of the drum surface, and is 40 to 100°C, preferably 60 to 80°C, from the viewpoint of efficiently obtaining a dried product having excellent redispersibility. If the drying temperature is too high above the upper limit, the cellulose is denatured by the influence of heat, and the obtained dried product has poor redispersibility. If the drying temperature is too low above the lower limit, the production efficiency is poor.
[0064] As the drum type dryer, there are a double drum type or twin drum type dryer using two drums, and a single drum type dryer using one drum, and any of them may be used. Among these, it is preferable to use a double drum type dryer from the viewpoint that the thickness of the thin film can be adjusted by adjusting the clearance between the drums.
[0065] The thickness of the thin film formed on the drum surface is preferably 5 to 500 μm, more preferably 50 to 250 μm. If it is 50 μm or more, the effect of further improving redispersibility is observed, and if it is 250 μm or less, it is easy to scrape off after drying.
[0066] The material of the drum surface provided in the vacuum drum dryer used in the present invention is not particularly limited, but may be metal plating such as chrome plating or a ceramic coating. A drum with a ceramic coating formed on its surface has excellent peelability of the dried fine cellulose fiber body, so the force required to press the doctor blade against the drum to scrape off the dried body is smaller than when a drum with a chrome-plated surface in the conventional technology is used. Therefore, when a drum with a ceramic coating is used, frictional heat generated between the doctor blade and the drum can be suppressed, and the obtained dried fine cellulose fiber body is one in which thermal denaturation is suppressed, and this dried body has excellent redispersibility.
[0067] As a method for forming a ceramic coating on the surface of a drum, thermal spraying is preferred from the viewpoint of uniformity of the coating. Thermal spraying is a method in which a thermal spraying material is heated to a molten or softened state and sprayed onto a substrate surface to form a thermal spray coating. The thermal spraying method is not particularly limited, and examples thereof include flame spraying, arc spraying, and plasma spraying, and plasma spraying is preferred from the viewpoint of workability.
[0068] Examples of the thermal spray material include metals, alloys, ceramics, plastics, etc., and it is preferable to use those containing ceramics because of their wear resistance and high strength. Examples of ceramics include tungsten carbide and chromium carbide, and it is preferable to use tungsten carbide from the viewpoint of the peelability of the dried CNF body. When using a thermal spray material containing ceramics, it is preferable to use a metal binder in combination. As the metal binder, at least one selected from chromium, nickel, and cobalt is preferable, at least one selected from chromium and nickel is more preferable, and one containing both chromium and nickel is even more preferable.
[0069] Examples of materials for the doctor blade include SUS, PEEK resin, carbon, phosphor bronze, etc. The peelability of the dried material varies depending on the material of the drum surface, and the force required for scraping varies, so the material may be appropriately selected according to the material of the drum surface. When the material of the drum surface is a ceramic spray coating, it is preferable to use a doctor blade made of PEEK resin or phosphor bronze from the viewpoint of protecting the coating on the drum surface, and it is preferable to use a doctor blade made of phosphor bronze from the viewpoint of the durability of the doctor blade.
[0070] (dry body) The obtained dried product may be appropriately pulverized, classified, or the like to obtain a powder form, but may also be in any other form.
[0071] In the present invention, the term "dried product" refers to a product that has been dried to a moisture content of 15% by mass or less. The moisture content is preferably 0 to 15% by mass, and more preferably 0 to 10% by mass. The product may be one that has been dried in a drying step to a moisture content of 0% (absolute dryness).
[0072] According to the method for producing a dried fine cellulose fiber product of the present invention, a mixture containing fine cellulose fibers, a dispersant, and an aqueous solvent and having a solid content concentration of 1 to 10 mass % is used, so that the thickness of the thin film formed between the drums of a vacuum drum dryer is larger than that when a mixture with a lower concentration is used, and the heat applied to the fine cellulose fibers is smaller, so that denaturation due to heat is suppressed. As a result, the dried product obtained by the production method of the present invention has excellent dispersibility.
[0073] Furthermore, in the method for producing a dried fine cellulose fiber body of the present invention, when a vacuum drum dryer equipped with a drum having a ceramic spray coating formed on its surface is used, the peelability of the obtained dried body is improved, making it unnecessary to press the doctor blade firmly against the drum, and the frictional heat generated between the doctor blade and the drum surface can be suppressed. The obtained dried fine cellulose fiber body is inhibited from being denatured by heat, and this dried body has excellent redispersibility. EXAMPLES
[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. In addition, unless the method of measurement / calculation of each value in each example is specifically stated, it is measured / calculated by the method described in the specification.
[0075] (Production Example 1) (Production of carboxylated (TEMPO oxidized) CNF) 5 g (bone-dry) of bleached, unbeaten kraft pulp (85% brightness) derived from coniferous trees was added to 500 mL of an aqueous solution containing 39 mg of TEMPO (Sigma Aldrich) and 514 mg of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system to a concentration of 5.5 mmol / g to initiate the oxidation reaction. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was acidified using hydrochloric acid, filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain an oxidized pulp (hereinafter sometimes referred to as "carboxylated cellulose", "carboxylated pulp", or "TEMPO oxidized pulp"). The pulp yield was 90%, the time required for the oxidation reaction was 90 minutes, and the amount of carboxyl groups was 1.6 mmol / g. The oxidized pulp obtained in the above process was adjusted to 1.0% (w / v) with water and treated three times with an ultra-high pressure homogenizer (20°C, 150 MPa) to obtain a carboxylated CNF dispersion. The obtained fibers had an average fiber diameter of 3 nm and an aspect ratio of 150. The amount of carboxyl groups, average fiber diameter, average fiber length, and aspect ratio of the carboxylated CNF were measured as follows.
[0076] (Method for measuring the amount of carboxyl groups) 60 mL of a 0.5% by mass slurry (aqueous dispersion) of carboxylated cellulose was prepared, and a 0.1 M aqueous hydrochloric acid solution was added to adjust the pH to 2.5. A 0.05 N aqueous sodium hydroxide solution was then added dropwise to measure the electrical conductivity until the pH reached 11. The electrical conductivity was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity was gradual: Amount of carboxyl groups [mmol / g carboxylated cellulose] = a [mL] × 0.05 / Mass of carboxylated cellulose [g].
[0077] (Measurement of average fiber diameter, average fiber length, and aspect ratio of CNF) The average fiber diameter and average fiber length of CNF were analyzed using an atomic force microscope (AFM) for 200 randomly selected fibers. The aspect ratio was calculated using the following formula: Aspect ratio = average fiber length / average fiber diameter
[0078] Example 1 (Modification of the drum surface of a vacuum drum dryer) A ceramic coating containing tungsten carbide was formed by plasma spraying tungsten carbide and a nickel-chromium binder onto the drum surface of a vacuum drum dryer (Katsuragi Kogyo Co., Ltd., VD-0102 model).
[0079] (Preparation of CNF aqueous dispersion) To the 1.5% by mass aqueous dispersion of carboxylated CNF obtained in Production Example 1, 4 parts by mass of carboxymethylcellulose (trade name: F350HC-4, viscosity (1% by mass, 25°C) about 3000 mPa·s, degree of carboxymethyl substitution about 0.9) was added as a dispersant per 6 parts by mass of solid content of CNF, and the mixture was stirred for 60 minutes with a jet paste (7200 rpm) to prepare an aqueous dispersion of CNF. The pH of this dispersion was about 7. A 0.5% aqueous sodium hydroxide solution was added to this aqueous dispersion to adjust the pH to 8-9. The solid content concentration of the aqueous dispersion (including carboxylated CNF and carboxymethylcellulose) was 2.5% by mass, and the viscosity was 18,400 mPa·s.
[0080] (Mixing process) The resulting aqueous dispersion with a solid content concentration of 2.5% by mass was placed in a raw material supply tank equipped with an agitator (high-function mixer). While applying sufficient shear with the agitator (30 rpm), the liquid was sent to the dryer by the liquid sending pump at the bottom of the tank. At this time, a portion (approximately 30%) was branched off from the liquid sending piping to the dryer, and a circulation line returning to the raw material supply tank was set up to circulate 30% of the raw material sent from the pump. The viscosity of the aqueous dispersion after the agitation process (viscosity before feeding) was 15,000 mPa s. Note that the viscosity before feeding refers to the viscosity of the aqueous dispersion before it is fed to the drum dryer.
[0081] (drying process) After the stirring process, the mixture sent from the tank was fed and spread onto the drum surface on which the ceramic spray coating was formed, forming a thin film with a thickness of about 100 to 200 μm, which was then dried in a drum dryer at a drum surface temperature of 80°C, a steam pressure of 0.05 MPaG, a drum rotation speed of 2 rpm, and an internal pressure of 2 kPa to obtain a dried carboxylated CNF with a solid content of 90.4 mass%. A phosphor bronze doctor blade was used to scrape off the dried CNF from the drum surface. The raw material throughput and production volume were also measured.
[0082] Example 2 A dried carboxylated CNF with a solid content of 89.5 mass% was obtained in the same manner as in Example 1, except that in the stirring step, the solid content of the aqueous dispersion was changed to 5.0%.
[0083] Example 3 A dried carboxylated CNF with a solid content of 90.8 mass% was obtained in the same manner as in Example 1, except that in the stirring step, the solid content of the aqueous dispersion was changed to 7.0%.
[0084] Example 4 A dried carboxylated CNF with a solid content of 89.5% was obtained in the same manner as in Example 1, except that a ribbon mixer and a centrifugal pump were used instead of the high-function mixer in the stirring process, and a circulation line was not used. Stirring was performed with the ribbon mixer at 60 rpm and the centrifugal pump at 3000 rpm.
[0085] Example 5 A dried carboxylated CNF with a solid content of 90.8% was obtained in the same manner as in Example 1, except that a ribbon mixer and an in-line mixer were used instead of the high-function mixer in the stirring process, and a circulation line was not used. Stirring was performed at 60 rpm with the ribbon mixer and 1 m / s with the in-line mixer.
[0086] Comparative Example 1 A dried carboxylated CNF with a solid content of 88.6% was obtained in the same manner as in Example 1, except that the stirring step was not performed.
[0087] Comparative Example 2 A dried carboxylated CNF with a solid content of 89.0% was obtained in the same manner as in Example 2, except that the stirring step was not performed.
[0088] Comparative Example 3 A dried carboxylated CNF with a solid content of 88.2% was obtained in the same manner as in Example 3, except that the stirring step was not performed.
[0089] [Table 1]
[0090] As can be seen from Table 1, in Examples 1 to 5 in which the dried fine cellulose fiber body was produced by a production method including a stirring step of stirring a mixture containing fine cellulose fiber, a dispersant, and an aqueous solvent with a solid content concentration of 1 to 10 mass%, and a drying step of drying the mixture that had undergone the stirring step at a temperature of 40 to 100°C under reduced pressure using a vacuum drum dryer, the introduction efficiency of the aqueous dispersion and the production efficiency of the dried body of carboxylated CNF were superior to those in Comparative Examples 1 to 3 in which the stirring step was not performed. This is particularly noticeable when comparing the Examples and Comparative Examples in which the solid content concentration of the aqueous dispersion used is the same.
Claims
1. a stirring step of stirring a mixture containing fine cellulose fibers, a dispersant, and an aqueous solvent and having a solid content concentration of 1 to 10 mass %; The method includes a drying step of drying the mixture that has been subjected to the stirring step at a temperature of 40 to 100° C. under reduced pressure using a vacuum drum dryer. Method for producing dried fine cellulose fiber material.
2. The method for producing a dried fine cellulose fiber material according to claim 1, wherein the vacuum drum dryer is provided with a drum having a ceramic spray coating formed on a surface thereof by thermal spraying.
3. 3. The method for producing a dried fine cellulose fiber material according to claim 1, wherein the fine cellulose fibers are carboxylated cellulose nanofibers, and the dispersant is carboxymethyl cellulose.
4. The method for producing a dried fine cellulose fiber body according to claim 1 or 2, wherein in the mixture, a blending ratio (parts by mass) of the fine cellulose fiber (bone dry solid content) to the dispersant is in the range of 5:5 to 8:2.
Citation Information
Patent Citations
Production of xerogel of bacterial cellulose and derivative produced thereby
JP1994233691A
Method for producing cellulose nanofiber dry solid
WO2019189318A1