Hard coat film

The hard coat film integrates inorganic metal particles and additional agents to provide enhanced antibacterial, antiviral, and other functional properties, meeting diverse application requirements.

JP2024133881APending Publication Date: 2024-10-03NIPPON PAPER IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023043883
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing hard coat films lack comprehensive functionalities such as antibacterial, antiviral, antistatic, antifogging, high hardness, high haze, and heat shielding properties, failing to meet the increasing functional requirements for applications like face shields and electronic device surfaces.

Method used

A hard coat film configuration with an ionizing radiation curable resin layer containing inorganic metal particles, antistatic agents, antifogging agents, and optionally laminated metal or metal oxide thin films, ensuring the presence of inorganic metal particles within a specific depth range to enhance antibacterial and antiviral properties.

Benefits of technology

The film achieves good antibacterial and antiviral performance, along with antistatic, antifogging, high hardness, high haze, and heat shielding effects, addressing multiple functional needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133881000001
    Figure 2024133881000001
Patent Text Reader

Abstract

To provide a hard coat film having a good antibacterial property and antiviral property.SOLUTION: A hard coat film has a hard coat layer containing an ionizing radiation-curing resin, on at least one surface of a base material. The hard coat layer further contains inorganic metal particles. On a surface on a side opposite to the base material side of the hard coat layer, and in a layer from the surface to a depth of 0.5 μm, 0.03 mass% or more of the inorganic metal particles exist.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a hard coat film having antibacterial and antiviral properties. [Background technology]

[0002] Currently, from the perspective of infectious disease prevention in particular, there is a demand for antibacterial and antiviral properties in products whose surfaces may come into direct contact with people's hands, such as face shield films, partition films, window films, and films for touch panels on electronic devices.

[0003] As prior art, for example, various hard coat films have been proposed in which an antibacterial hard coat layer containing an antibacterial agent or the like is laminated on a film substrate (see, for example, Patent Documents 1 to 3, etc.). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-216750 A [Patent Document 2] JP 2010-234523 A [Patent Document 3] JP 2012-208169 A Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, various hard coat films with antibacterial properties have been proposed in the past, but recently, there has been a demand for films that have not only antibacterial properties but also good antiviral properties. Depending on the application, in addition to antibacterial and antiviral properties, for example, antistatic properties, high hardness, antifogging properties, high haze, heat shielding properties (i.e. heat shielding or heat insulation properties), etc. are required, and thus the functional requirements for hard coat films are increasing.

[0006] Therefore, the object of the present invention is, first, to provide a hard coat film having good antibacterial and antiviral properties, second, to provide a hard coat film having good antibacterial and antiviral properties and further having antistatic performance, third, to provide a hard coat film having good antibacterial and antiviral properties and further having high hardness, fourth, to provide a hard coat film having good antibacterial and antiviral properties and further having antifogging properties, fifth, to provide a hard coat film having good antibacterial and antiviral properties and further having a high haze value, and sixth, to provide a hard coat film having good antibacterial and antiviral properties and further having heat shielding properties. Furthermore, it is also an object of the present invention to provide a hard coat film having multiple properties such as the above-mentioned antistatic performance, high hardness, antifogging properties, high haze, and heat shielding properties in addition to good antibacterial and antiviral properties. [Means for solving the problem]

[0007] The present invention was completed based on various findings obtained through extensive research aimed at solving the above problems. That is, the present invention has the following configuration.

[0008] (First invention) The hard coat film has a hard coat layer containing an ionizing radiation curable resin on at least one side of a substrate, the hard coat layer further containing inorganic metal particles, and the inorganic metal particles are present in an amount of 0.03 mass % or more on the surface of the hard coat layer opposite the substrate side and within a layer up to a depth of 0.5 μm from the surface.

[0009] (Second Invention) In the hard coat film according to the first aspect of the present invention, the inorganic metal particles are an inorganic material containing at least a silver component.

[0010] (Third Invention) In the hard coat film according to the first or second invention, the hard coat layer further contains an antistatic agent.

[0011] (Fourth Invention) In the hard coat film according to the first or second invention, the hard coat layer further contains inorganic fine particles.

[0012] (Fifth Invention) In the hard coat film according to the first or second invention, the hard coat layer further contains an antifogging agent.

[0013] (Sixth Invention) In the hard coat film according to the first or second invention, the hard coat layer further contains organic fine particles.

[0014] (Seventh Invention) The hard coat film according to the first or second invention is characterized in that at least one thin film made of a metal or a metal oxide is laminated on the surface of the substrate opposite to the hard coat layer, or between the substrate and the hard coat layer. Effect of the Invention

[0015] According to the present invention, it is possible to provide a hard coat film having good antibacterial and antiviral properties. Furthermore, according to the present invention, it is possible to provide a hard coat film having good antibacterial and antiviral properties and further having antistatic properties. Furthermore, according to the present invention, it is possible to provide a hard coat film that has excellent antibacterial and antiviral properties and also has high hardness. Furthermore, according to the present invention, it is possible to provide a hard coat film having good antibacterial and antiviral properties as well as antifogging properties. Furthermore, according to the present invention, it is possible to provide a hard coat film having good antibacterial and antiviral properties and further having a high haze value. Furthermore, according to the present invention, it is possible to provide a hard coat film having good antibacterial and antiviral properties and further having heat insulation properties. Furthermore, according to the present invention, it is possible to provide a hard coat film that has not only good antibacterial and antiviral properties, but also multiple properties selected from the above-mentioned antistatic properties, high hardness, antifogging properties, high haze, heat insulation properties, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described in detail. In the present invention, unless otherwise specified, the expression "XX to △△" means "not less than XX and not more than △△."

[0017] The hard coat film of the present invention will be described below. As described above, the hard coat film of the present invention is a hard coat film characterized in that it has a hard coat layer containing an ionizing radiation curable resin on at least one side of a substrate, the hard coat layer further contains inorganic metal particles, and the inorganic metal particles are present in an amount of 0.03 mass % or more on the surface of the hard coat layer opposite the substrate side and within a layer up to a depth of 0.5 μm from the surface.

[0018] The hard coat film of the present invention can be preferably applied to, for example, a face shield film, a partition film, a window film, a table cover film, a bus mirror film, a freezer / refrigerator window film, or a display or touch panel film for electronic devices, etc. Of course, the applications listed here are merely examples, and the applications are not limited to these.

[0019] As the substrate to be coated with this hard coat film, a film substrate is usually used. The film substrate used in the present invention is not particularly limited, and examples thereof include acrylic resins, triacetyl cellulose, polyethylene terephthalate, cycloolefin polymers, polycarbonates, polyethylene naphthalate, polyethylene, polytrimethylene terephthalate, polypropylene, polybutylene terephthalate, polybutylene naphthalate, polystyrene, polymethyl methacrylate, polystyrene glycidyl methacrylate, aromatic polyimides, alicyclic polyimides, polyamideimides, and mixtures thereof. Among these film substrates, polyester films, acrylic films, triacetyl cellulose, polyethylene terephthalate, and polycarbonates are particularly preferred.

[0020] When the hard coat film of the present invention is used as a face shield film, the film substrate is preferably triacetyl cellulose or polyethylene terephthalate from the viewpoints of transparency and cost, and when the hard coat film of the present invention is used as a partition film or window film, the film substrate is preferably an acrylic resin film, or polycarbonate or polyethylene terephthalate from the viewpoints of impact resistance and cost. The substrate may also have ultraviolet ray blocking properties.

[0021] The thickness of the film substrate varies depending on the application and cannot be generally determined, but is usually preferably in the range of 10 to 1000 μm, more preferably in the range of 20 μm to 300 μm.

[0022] Next, the hard coat layer will be described. The resin contained in the hard coat layer can be any resin that forms a coating, without any particular limitation. In particular, it is preferable to use an ionizing radiation curable resin, since it can impart surface hardness (scratch resistance) to the hard coat layer and can adjust the degree of crosslinking by the amount of exposure to ultraviolet light or the like, thereby enabling adjustment of the surface hardness of the hard coat layer.

[0023] The ionizing radiation curable resin used in the present invention is not particularly limited as long as it is a resin that is cured by irradiation with ultraviolet light (hereinafter abbreviated as "UV") or an electron beam (hereinafter abbreviated as "EB"), but in order to provide coating hardness and form a three-dimensional crosslinked structure in the hard coat layer, it is preferable to use a polyfunctional acrylate that is curable by UV or EB and has three or more (meth)acryloyloxy groups in one molecule. Specific examples of UV or EB curable polyfunctional acrylates include urethane acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane ethoxy triacrylate, glycerin propoxy triacrylate, ditrimethylolpropane tetraacrylate, etc. The polyfunctional acrylates may be used alone or in combination of two or more.

[0024] Furthermore, the ionizing radiation curable resin used in the present invention is preferably a polymer having a weight average molecular weight in the range of, for example, 700 to 3600, and preferably has a weight average molecular weight divided by the number of functional groups in the range of 50 to 1500. If the weight average molecular weight divided by the number of functional groups is less than 50, the hard coat film will curl toward the hard coat layer side, causing problems in the subsequent processing steps and poor processing suitability. If the weight average molecular weight divided by the number of functional groups is more than 1500, the hardness will be insufficient and this is not suitable.

[0025] In addition, when the ionizing radiation curable resin used in the present invention has a weight average molecular weight of less than 1500, the number of functional groups in one molecule is preferably 3 or more and less than 10. In addition, when the weight average molecular weight of the ionizing radiation curable resin is 1500 or more, the number of functional groups in one molecule is preferably 3 or more and less than 20. Within the above range, curling can be suppressed while suppressing the occurrence of cracks under high temperature conditions, and appropriate processability can be maintained. For example, it is suitable for use as a window film.

[0026] In addition to the above-mentioned ionizing radiation curable resins, the resin contained in the hard coat layer may include thermoplastic resins such as polyethylene, polypropylene, polystyrene, polycarbonate, polyester, acrylic, styrene-acrylic, and cellulose, and thermosetting resins such as phenol resin, urea resin, unsaturated polyester, epoxy, and silicone resin, within a range that does not impair the hardness and scratch resistance of the hard coat layer.

[0027] In the present invention, by incorporating inorganic metal particles in the hard coat layer, it is possible to obtain a hard coat film having good antibacterial and antiviral properties (also referred to as "antibacterial and antiviral properties").

[0028] The inorganic metal particles used in the present invention are substances formed by incorporating metal ions such as silver, molybdenum, copper, zinc, etc. into an inorganic compound (inorganic material), or substances in which metal ions such as silver, molybdenum, copper, zinc, etc. are supported on an inorganic compound (inorganic material). Specific examples of inorganic metal particles used in the present invention include inorganic antibacterial and antiviral agents such as antibacterial and antiviral zeolite, antibacterial and antiviral apatite, and antibacterial and antiviral zirconia, which are formed by incorporating at least one metal ion of silver, molybdenum, copper, zinc, etc. into inorganic compounds such as zeolite, apatite, and zirconia. In addition, compounds in which at least one metal ion of silver, molybdenum, copper, zinc, etc. is supported on zeolite, apatite, zirconia, glass, etc. are also preferred. By supporting these metal ions on inorganic materials, it is possible to prevent the metal components from falling off over time.

[0029] As the inorganic metal particles used in the present invention, a silver-based material containing silver ions (silver component) is preferred from the viewpoint of being non-toxic to living organisms and excellent in safety. Among them, for example, phosphate glass silver-supported compounds and silver zeolite compounds are more preferred because they exhibit antibacterial and antiviral properties even in small amounts, allowing the amount of addition to be reduced. In addition, silver-molybdenum materials containing both silver and molybdenum components can also be preferably used in the present invention because they exhibit good antibacterial and antiviral properties. The inorganic metal particles in the present invention are preferably inorganic materials containing at least a silver component.

[0030] The average particle diameter of the inorganic metal particles is preferably, for example, in the range of 1 to 30,000 nm, and more preferably in the range of 2.5 to 20,000 nm. If the average particle diameter is less than 1 nm, the materials are limited and difficult to obtain. On the other hand, if the average particle diameter exceeds 30,000 nm, the dispersibility in the hard coat paint is deteriorated, and a grainy feeling remains when applied.

[0031] The amount of the inorganic metal particles added is not particularly limited in the present invention, but is, for example, in the range of 0.20% by mass to 10% by mass based on the solid content in the hard coat layer. If the amount is less than 0.20% by mass, antibacterial and antiviral properties are not fully expressed. On the other hand, if the amount is more than 10% by mass, transparency is reduced, and when visibility is required for face shields, window films, etc., visibility is significantly reduced.

[0032] In the present invention, unless otherwise specified, the term "solid content in the hard coat layer" refers to "solid content in a coating liquid for forming a hard coat layer (paint for hard coat) for forming a hard coat layer." The solid content is, for example, solid content of resin, additives, etc.

[0033] In particular, since the silver-based materials and silver-molybdenum-based materials exhibit good antibacterial and antiviral properties even when added in small amounts, the amount added can be in the range of 0.20 mass % to 5.0 mass % relative to the solid content in the hard coat layer. The inorganic metal particles may be used alone or in combination of two or more kinds.

[0034] As a result of extensive investigations, the present inventors have found that even if the amount of the inorganic metal particles added is within the above-mentioned range, in order for antibacterial and antiviral properties to be fully exhibited, the inorganic metal particles must be present in an amount of 0.03 mass % or more in the surface layer of the hard coat layer, specifically, the surface of the hard coat layer opposite the substrate side and within a layer up to a depth of 0.5 μm from the surface.

[0035] This is because, in order for the hard coat layer to fully exhibit antibacterial and antiviral properties, bacteria and viruses need to come into contact with the inorganic metal particles, and for this to happen, it is important that a certain amount or more of inorganic metal particles are present on the surface of the hard coat layer opposite the substrate and within the layer to a depth of 0.5 μm from said surface.

[0036] The amount of inorganic metal particles present on the surface of the hard coat layer opposite the substrate side and within the layer to a depth of 0.5 μm from the surface can be specified in terms of mass %, and the amount can be measured, for example, using a scanning electron microscope and an energy dispersive X-ray analyzer.

[0037] In the present invention, it is a preferred embodiment that the hard coat layer further contains an antistatic agent. By further containing an antistatic agent in the hard coat layer containing the inorganic metal particles, it is possible to obtain a hard coat film having a hard coat layer having both good antibacterial and antiviral properties and antistatic properties.

[0038] The type of such an antistatic agent is not particularly limited, but for example, an antistatic agent consisting of a conductive filler such as a metal-based conductive filler, a nonmetallic conductive filler, or a carbon-based conductive filler, or an organic antistatic agent dispersed in a binder consisting of an organic compound as required, can be preferably used. In the present invention, for example, a quaternary ammonium salt-based antistatic agent can be preferably used.

[0039] When the antistatic agent, for example, a quaternary ammonium salt-based antistatic agent, is used, the amount of the antistatic agent added is not particularly limited in the present invention, but is, for example, in the range of 1% by mass to 20% by mass based on the solid content in the hard coat layer. If the amount of the antistatic agent added is less than 1% by mass, sufficient antistatic performance cannot be obtained. On the other hand, if the amount of the antistatic agent added exceeds 20% by mass, the strength of the coating film may decrease.

[0040] In addition, in the present invention, it is possible to further improve the surface hardness (scratch resistance, pencil hardness) by incorporating inorganic fine particles in the hard coat layer. That is, by incorporating inorganic fine particles in the hard coat layer containing the inorganic metal particles, it is possible to obtain a hard coat film having good antibacterial and antiviral properties and a hard coat layer with high hardness.

[0041] In this case, the average particle size of the inorganic fine particles is preferably in the range of 5 to 200 nm, more preferably in the range of 10 to 80 nm. If the average particle size is less than 5 nm, it is difficult to obtain sufficient surface hardness. On the other hand, if the average particle size exceeds 200 nm, the gloss and transparency of the hard coat layer are likely to decrease, and the flexibility may also decrease.

[0042] The inorganic fine particles include, for example, inorganic oxide fine particles such as silica, alumina, etc. Alumina, which is mainly composed of aluminum, has high hardness and therefore can be effective with a smaller amount added than silica.

[0043] The amount of inorganic fine particles added is not particularly limited in the present invention, but is, for example, in the range of 10% by mass to 60% by mass based on the solid content in the hard coat layer. If the amount is less than 10% by mass, it is difficult to obtain sufficient surface hardness. On the other hand, if the amount is more than 60% by mass, transparency and appearance are reduced, and when visibility is required for face shields, window films, etc., the visibility is significantly deteriorated.

[0044] In the present invention, the hard coat layer may contain an antifogging agent. By further incorporating an antifogging agent into the hard coat layer containing the inorganic metal particles, a hard coat film having a hard coat layer having both good antibacterial and antiviral properties and antifogging properties can be obtained.

[0045] Such an antifogging agent can be used without any particular restriction as long as it is a substance that forms a hydrophilic region, and examples thereof include surfactants such as anionic surfactants such as fatty acid soaps and alkylbenzene sulfonates, cationic surfactants having a quaternary ammonium group, amphoteric surfactants such as long-chain alkyl amino acids, and nonionic surfactants such as polyoxyethylene nonylphenyl ether, as well as fluorine-based surfactants, hydrophilic monomers such as hydroxyl alkyl (meth)acrylates such as glycosyl ethyl methacrylate, methacrylic acid, acrylic acid, 2-hydroxyl ethyl methacrylate, acrylamide, N,N-dimethylacrylamide, N-vinylpyrrolidone, N-(2-methacryloyloxyethyl)-2-pyrrolidone, glyceryl methacrylate, polyethylene glycol methacrylate, and polyethylene glycol acrylate, polyalkylene glycol mono(meth)acrylates, (meth)acrylamides, and N-vinyl lactams, as well as polymers composed of these monomers. In addition, as the hydrophilic substance, a silane coupling agent having an anionic hydrophilic group (e.g., a sulfonic acid group, etc.), a hydrophilic monomer, and a reactive surfactant having a reactive terminal group such as a vinyl group, an acrylic group, a methacrylic group, a glycidyl group, an allyl group, an epoxy group, a mercapto group, a cyano group, an isocyano group, or an amino group, and a hydrophilic portion such as a sulfonic group, a hydroxyl group, or an ammonium chloride can also be used.

[0046] The amount of the antifogging agent added is not particularly limited in the present invention, but is, for example, in the range of 10% by mass to 70% by mass based on the solid content in the hard coat layer. If the amount is less than 10% by mass, sufficient antifogging properties cannot be obtained. On the other hand, if the amount is more than 70% by mass, the scratch resistance of the film may decrease.

[0047] In the present invention, at least one thin film made of a metal or metal oxide can be laminated on the surface of the substrate opposite to the hard coat layer, or between the substrate and the hard coat layer. By providing a layer made of a metal or metal oxide, the heat shielding effect (heat shielding property) of the hard coat film can be obtained. Specific examples of metals or metal oxides include aluminum, silver, gold, nickel, cobalt, stainless steel, and alloys thereof, titanium dioxide, tin oxide, indium oxide, zinc oxide, and tungsten oxide.

[0048] As a method for forming a layer (thin film) made of the above-mentioned metal or metal oxide, for example, a known thin film forming method such as a vacuum deposition method, a sputtering method, a chemical vapor deposition method (CVD method) or the like can be applied. The thickness of the layer (thin film) made of the above-mentioned metal or metal oxide is preferably in the range of 10 to 1000 nm. If the thickness is less than 10 nm, a sufficient heat shielding effect cannot be obtained, and if it exceeds 1000 nm, the transparency tends to decrease, and it may not be suitable for applications requiring visibility such as window films.

[0049] In order to cure the ionizing radiation curable resin contained in the hard coat layer, the coating liquid for forming the hard coat layer (paint for hard coat) can contain a known photopolymerization initiator. As such a photopolymerization initiator, acetophenones and benzophenones can be used.

[0050] In addition, a leveling agent (surface modifier) ​​can be used in the hard coat layer to improve application properties. For example, known leveling agents such as fluorine-based, acrylic-based, siloxane-based, and adducts or mixtures thereof can be used.

[0051] In order to impart antifouling properties to the hard coat film of the present invention, a fluorine-based or siloxane-based antifouling agent (such as a leveling agent or a surfactant) can be added to the hard coat layer. The amount of the antifouling agent added is not particularly limited, but is preferably 0.05% by mass to 2.0% by mass based on the resin solid content in the hard coat coating material.

[0052] In order to impart opacity to the hard coat film of the present invention, it is preferable to increase the haze value of the hard coat layer. For this purpose, a method of adding organic or inorganic fine particles to the hard coat layer can be mentioned. The presence of organic or inorganic fine particles in the hard coat layer causes light to refract and scatter, resulting in the appearance of haze. Examples of organic fine particles include fine particles of acrylic, melamine-formaldehyde condensate, polyethylene, styrene acrylic, polyester, etc., and examples of inorganic fine particles include fine particles of alumina, zinc oxide, silica, titanium oxide, cerium oxide, etc. In order to increase the haze value, the amount of the fine particles added is preferably within a range of 10% by mass to 80% by mass relative to the solid content in the hard coat layer.

[0053] Other additives that may be added to the hard coat layer include an ultraviolet absorber, an antifoaming agent, a surface tension regulator, an antioxidant, a light stabilizer, and the like, if necessary.

[0054] The hard coat layer can be formed by applying a coating liquid for forming a hard coat layer, which is prepared by dissolving or dispersing the above-mentioned antistatic agent, inorganic fine particles, organic fine particles, antifogging agent, photopolymerization initiator, and other additives in a suitable solvent in addition to the above-mentioned inorganic metal particles and ionizing radiation curable resin, onto the substrate to be coated, drying the coating liquid, and then irradiating the substrate with ionizing radiation such as UV or EB. By using an ionizing radiation curable resin, photopolymerization occurs upon exposure to ionizing radiation, and a hard coat layer having excellent hardness can be obtained.

[0055] The solvent can be appropriately selected depending on the solubility of the resin to be blended, and may be any solvent capable of uniformly dissolving or dispersing at least the solid content (resin, other additives, etc.) As such a solvent, for example, known organic solvents such as aromatic solvents such as toluene, xylene, and n-heptane, aliphatic solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane, ester solvents such as methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, and methyl lactate, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, and alcohol solvents such as methanol, ethanol, isopropyl alcohol, and n-propyl alcohol can be used alone or in combination.

[0056] Furthermore, the concentration (solid content concentration) of the coating liquid is not particularly limited, but can be, for example, in the range of about 10% by mass to 70% by mass.

[0057] The amount of ionizing radiation (UV, EB, etc.) applied after the hard coat layer-forming coating liquid is applied to the substrate and dried may be any amount necessary to provide the hard coat layer with sufficient hardness, and can be appropriately set depending on the type of ionizing radiation curable resin, etc.

[0058] The method for applying the coating solution for forming the hard coat layer is not particularly limited, and examples of the coating method include known coating methods such as gravure coating, microgravure coating, fountain bar coating, slide die coating, slot die coating, screen printing, and spray coating.

[0059] Furthermore, the drying temperature and heating time (drying time) in the drying step after coating can be appropriately set.

[0060] The coating thickness (after drying) of the hard coat layer does not need to be particularly limited because it varies depending on the application of the hard coat film, but it is generally suitable to be in the range of, for example, 1.0 μm to 20.0 μm. If the coating thickness is less than 1.0 μm, it is difficult to obtain the required surface hardness, which is not preferable. Also, if the coating thickness exceeds 20.0 μm, curling is likely to occur, which is not preferable because handling during the manufacturing process is reduced.

[0061] The hard coat film of the present invention comprises a hard coat layer containing at least inorganic metal particles and an ionizing radiation curable resin provided on at least one surface of a substrate. Specific examples (embodiments) of the layer structure are given below. (Embodiment 1) The above-mentioned hard coat layer is provided on both sides of the substrate, one of which is a hard coat layer containing the inorganic metal particles and antistatic agent of the present invention in the layer and having antibacterial / antiviral properties and antistatic performance, and the other is a hard coat layer containing the inorganic metal particles and antifogging agent of the present invention in the layer and having antibacterial / antiviral properties and antifogging properties. Alternatively, the above-mentioned hard coat layer is provided on both sides of the substrate, one of which is a hard coat layer containing the inorganic metal particles and inorganic fine particles of the present invention in the layer, having antibacterial / antiviral properties and high hardness, and the other is a hard coat layer having the above-mentioned antibacterial / antiviral properties and antifogging properties. Such an embodiment of the hard coat film is suitable, for example, as a film for a face shield.

[0062] (Embodiment 2) A hard coat layer having the above-mentioned antibacterial and antiviral properties and antistatic properties is provided on one side of the substrate. Alternatively, a hard coat layer having the above-mentioned antibacterial and antiviral properties and high hardness is provided on one side of the substrate. In either embodiment, an adhesive layer for attaching the hard coat film to a member such as a partition, a window, a table cover, or a touch panel of an electronic device can be provided on the other side of the substrate (the side opposite to the side on which the hard coat layer is provided). Such an embodiment of the hard coat film is suitable, for example, as a partition film, a window film, a table cover film, or a film for displays or touch panels of electronic devices and the like.

[0063] (Embodiment 3) A hard coat layer having the above-mentioned antibacterial, antiviral and antifogging properties is provided on one side of the substrate, and an adhesive layer for attaching the hard coat film to components such as windows, bus mirrors, and refrigerator / freezer windows can be provided on the other side of the substrate (the side opposite to the side on which the hard coat layer is provided). Such hardcoat film embodiments are suitable, for example, as window films, bus mirror films, and refrigerator / freezer window films.

[0064] (Embodiment 4) A hard coat layer having the above-mentioned antibacterial and antiviral properties and antistatic properties is provided on one side of the substrate, or a hard coat layer having the above-mentioned antibacterial and antiviral properties and high hardness is provided on one side of the substrate. In either of these embodiments, at least one thin film made of a metal or metal oxide can be laminated on the other side of the substrate (the side opposite to the side on which the hard coat layer is provided) or between the substrate and the hard coat layer. Such an embodiment of the hard coat film is suitable for applications requiring a heat shielding effect, such as partition films and window films.

[0065] As described above in detail, the present invention can provide a hard coat film having good antibacterial and antiviral properties. The present invention can also provide a hard coat film having good antibacterial and antiviral properties and antistatic properties. The present invention can also provide a hard coat film having good antibacterial and antiviral properties and high hardness. The present invention can also provide a hard coat film having good antibacterial and antiviral properties and antifogging properties. The present invention can also provide a hard coat film having good antibacterial and antiviral properties and a high haze value. Furthermore, a hard coat film having good antibacterial and antiviral properties and a heat shielding effect can be provided. Furthermore, a hard coat film having good antibacterial and antiviral properties as well as a plurality of properties such as the above-mentioned antistatic properties, high hardness, antifogging properties, high haze, and heat shielding properties can be provided. EXAMPLES

[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" means parts by mass unless otherwise specified, and "%" means % by mass unless otherwise specified.

[0067] Example 1 [Preparation of Coating Solution for Forming Hard Coat Layer] The base material was 95 parts of an ionizing radiation curable resin (Shikoh UV-7630B (product name); manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) mainly composed of urethane acrylate, 3.5 parts of Irgacure 184 (photopolymerization initiator, manufactured by BASF), 1.5% (based on solids: 0.5%) of a surface modifier (Megafac R-08MH; manufactured by DIC Corporation), and 0.15% (based on solids: 0.5%) of an antibacterial and antiviral agent containing a silver-molybdenum compound as inorganic metal particles of the present invention. The mixture was diluted with butyl acetate / n-propyl alcohol = 50 / 50 (parts by weight) to prepare a coating liquid for forming a hard coat layer (hereinafter also referred to as "hard coat paint") with a final solids concentration of 30%.

[0068] [Preparation of hard coat film] The hard coat paint having the above composition was applied to one side of a substrate film (film thickness 50 μm) made of polyethylene terephthalate (PET) using a bar coater, and then dried for 60 seconds in a drying oven at 80°C to form a hard coat layer having a film thickness of 4.0 μm after drying. Next, a UV irradiation device set at a height of 60 mm from the coating surface was used to irradiate this hard coat layer with a UV dose of 200 mJ / cm. 2 The coating was cured by irradiation with ultraviolet light of 100 .ANG. to prepare a hard coat film of this Example 1.

[0069] Example 2 The hard coat film of Example 2 was produced using a hard coat paint prepared in the same manner as in Example 1, except that the antibacterial and antiviral agent containing a silver-molybdenum compound in the hard coat paint was blended at a ratio of 0.13% (based on solid content: 0.42%).

[0070] Example 3 The hard coat film of Example 3 was produced using a hard coat paint prepared in the same manner as in Example 1, except that the antibacterial and antiviral agent containing a silver-molybdenum compound in the hard coat paint was blended at a ratio of 0.08% (based on solid content: 0.28%).

[0071] Example 4 [Preparation of hard coat paint] The base material was 95 parts of an ionizing radiation curable resin (Shikoh UV-7630B (trade name); manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) mainly composed of urethane acrylate, mixed with 3.5 parts of Irgacure 184 (photopolymerization initiator, manufactured by BASF) and 1.5% (0.5% solids) of a surface modifier (Megafac R-08MH; manufactured by DIC Corporation), 5 parts of a quaternary ammonium salt-based antistatic agent (1SX-1055F (trade name); manufactured by Taisei Fine Chemical Co., Ltd.), and 0.15% (0.5% solids) of an antibacterial and antiviral agent containing a silver-molybdenum compound as inorganic metal particles of the present invention, and diluted with butyl acetate / n-propyl alcohol = 50 / 50 (parts by weight) to prepare a coating liquid for forming a hard coat layer with a final solids concentration of 30%.

[0072] [Preparation of hard coat film] A hard coat film of Example 4 was produced in the same manner as in Example 1, except that the hard coat coating material having the above composition was used to form a hard coat layer having a film thickness of 4.0 μm after drying.

[0073] Example 5 [Preparation of hard coat paint] The coating solution was made of 95 parts of an ionizing radiation curable resin (Shikoh UV-7630B (product name); manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) mainly composed of urethane acrylate, 3.5 parts of Irgacure 184 (photopolymerization initiator; manufactured by BASF), 30 parts of silica fine particles (average particle size 50 nm), 1.5% (based on solids: 0.5%) of a surface modifier (Megafac R-08MH; manufactured by DIC Corporation), and 0.15% (based on solids: 0.5%) of an antibacterial and antiviral agent containing a silver-molybdenum compound as inorganic metal particles of the present invention. The mixture was diluted with butyl acetate / n-propyl alcohol = 50 / 50 (parts by weight) to prepare a coating solution for forming a hard coat layer with a final solids concentration of 30%.

[0074] [Preparation of hard coat film] A hard coat film of Example 5 was produced in the same manner as in Example 1, except that the hard coat coating material having the above composition was used to form a hard coat layer having a film thickness of 4.0 μm after drying.

[0075] Example 6 [Preparation of hard coat paint] A hard coat paint with a final solids concentration of 40% was prepared by mixing 99.7% of an ionizing radiation curable resin (AICA ITRON Z-942-4 (product name); manufactured by AICA Kogyo Co., Ltd.) containing a fluorine-based surfactant (anti-fogging agent) and consisting mainly of urethane acrylate, and 0.15% (based on solids content: 0.5%) of an antibacterial and antiviral agent containing a silver-molybdenum compound as inorganic metal particles of the present invention. The mixture was then diluted with propylene glycol monomethyl ether (PGME).

[0076] [Preparation of hard coat film] A hard coat film of Example 6 was produced in the same manner as in Example 1, except that the hard coat coating material having the above composition was used to form a hard coat layer having a film thickness of 4.0 μm after drying.

[0077] Example 7 [Preparation of hard coat paint] The coating solution was made of 90 parts of an ionizing radiation curable resin (Shikoh UV-7630B (product name); manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) mainly composed of urethane acrylate, 3.5 parts of Irgacure 184 (photopolymerization initiator, manufactured by BASF), 30 parts of organic fine particles (KMP-605; manufactured by Shin-Etsu Silicones: average particle size 2 μm), 1.5% (based on solids: 0.5%) of a surface modifier (Megafac R-08MH; manufactured by DIC Corporation), and 0.15% (based on solids: 0.5%) of an antibacterial and antiviral agent containing a silver-molybdenum compound as inorganic metal particles of the present invention. The mixture was diluted with butyl acetate / n-propyl alcohol = 50 / 50 (parts by weight) to prepare a coating solution for forming a hard coat layer with a final solids concentration of 30%.

[0078] [Preparation of hard coat film] A hard coat film of Example 7 was produced in the same manner as in Example 1, except that the hard coat coating material having the above composition was used to form a hard coat layer having a film thickness of 4.0 μm after drying.

[0079] Example 8 An indium tin oxide (ITO) layer was formed to a thickness of 600 nm on the surface of the hard coat film of Example 4 opposite the hard coat layer on the substrate using a sputtering apparatus (magnetron sputter MSP-40T (product name); manufactured by Vacuum Device Co., Ltd.), thereby producing a hard coat film of Example 8.

[0080] Example 9 An indium tin oxide (ITO) layer was applied to one side of a substrate film (film thickness 50 μm) made of polyethylene terephthalate (PET) to a thickness of 600 nm using a sputtering device (magnetron sputter MSP-40T (product name); manufactured by Vacuum Device Co., Ltd.). A hard coat layer having a film thickness of 4.0 μm after drying was formed thereon using the same hard coat paint as in Example 4, thereby producing the hard coat film of Example 9.

[0081] Comparative Example 1 A hard coat film of Comparative Example 1 was produced using a hard coat coating material prepared in the same manner as in Example 1, except that the antibacterial and antiviral agent containing a silver-molybdenum compound in the hard coat coating material in Example 1 was not contained (was omitted).

[0082] Comparative Example 2 A hard coat film of Comparative Example 2 was produced using a hard coat coating material prepared in the same manner as in Example 1, except that the antibacterial and antiviral agent containing a silver-molybdenum compound in the hard coat coating material in Example 1 was blended at a ratio of 0.02% (based on solid content: 0.07%).

[0083] <Evaluation> The hard coat films of the Examples and Comparative Examples prepared as described above were evaluated for the following items. The results are summarized in Table 1.

[0084] <Coating thickness> The thickness of the hard coat layer was measured using a Thin-Film Analyzer F20 (product name) (manufactured by FILMETRICS).

[0085] <Inorganic metal particle abundance> The measurement was performed using an energy dispersive X-ray analyzer (Oxford Instruments) mounted on a Hitachi High-Tech FlexSEM. The measurement conditions were an acceleration voltage of 15 KV, a spot intensity of 70, and a measurement area of ​​1.2 mm. 2 The amount of inorganic metal particles present on the surface of the hard coat layer opposite to the substrate side and within the layer from the surface was measured, and the amount present up to a depth of 0.5 μm was calculated.

[0086] <Antibacterial> Measurements were performed according to the method specified in JIS Z 2801: 2010. An antibacterial activity value of 2.0 or higher was determined to be effective.

[0087] <Antiviral> Measurements were performed in accordance with the ISO 21702:2019 standard. An antiviral activity value of 2.0 or higher was determined to be effective.

[0088] <Total light transmittance> Each hard coat film was measured using a haze meter HM-150N manufactured by Murakami Color Research Laboratory Co., Ltd. The measurement was carried out in accordance with the JIS-K7361 standard.

[0089] <Haze> The haze of each of the hard coat films produced in the examples and comparative examples was measured using a haze meter HM-150N manufactured by Murakami Color Research Laboratory Co., Ltd. in accordance with JIS-K7136.

[0090] <Surface resistance (antistatic performance)> The surface resistance of each of the hard coat films prepared in Examples 4, 8, and 9 was measured using a Hiresta-UX MCP-HT800 manufactured by Nitto Seiko Analytech Co., Ltd. A USR probe was used for the measurement, and the applied voltage was 500 V. The evaluation criteria were a surface resistance of 1.0×10 11 Less than 10Ω / □ was considered to be acceptable. 11Ω / □ is the level at which dust does not adhere due to static electricity, etc.

[0091] <Pencil hardness> The pencil hardness of each hard coat film produced in the Examples and Comparative Examples was measured by a test method conforming to JIS-K-5600-5-4. The hardness at which no scratches were generated on the surface was recorded. As for the evaluation criteria, a hardness of 2H or more was considered to be acceptable.

[0092] <Water contact angle> The measurement was performed according to the method of JIS-3257.

[0093] <Anti-fogging properties> The hard coat layer surface was held over hot water heated to 80°C, and visual observation was made to see whether clouding occurred due to steam. ○: No clouding ×: Clouding occurs

[0094] <Heat insulation (shielding coefficient)> The heat shielding property of each of the hard coat films prepared in Examples 8 and 9 was evaluated by the "shielding coefficient". The shielding coefficient was measured in accordance with JIS A 5759. If the shielding coefficient is less than 1.0, the film has heat shielding property (heat shielding effect).

[0095] [Table 1]

[0096] From the results in Table 1, according to the examples of the present invention, it can be seen that a hard coat film having good antibacterial and antiviral properties can be obtained by having the amount of inorganic metal particles present in the surface of the hard coat layer opposite to the substrate side and in the layer up to a depth of 0.5 μm from the surface being 0.03 mass % or more. In addition, in Example 4, in which an antistatic agent is contained in the hard coat layer, a hard coat film having both good antibacterial and antiviral properties and antistatic performance can be obtained. In addition, in Example 5, in which inorganic fine particles are contained in the hard coat layer, a hard coat film having good antibacterial properties and high hardness can be obtained. In addition, in Example 6, in which an antifogging agent is contained in the hard coat layer, a hard coat film having good antibacterial properties, antiviral properties and antifogging properties can be obtained. In addition, in Example 7, a hard coat film having good antibacterial properties, antiviral properties and high haze can be obtained. In addition, in Examples 8 and 9, a hard coat film having good antibacterial properties, antiviral properties and heat shielding effect can be obtained.

[0097] On the other hand, in the hard coat film of Comparative Example 2, in which the amount of inorganic metal particles present on the surface of the hard coat layer and within a depth of 0.5 μm from the surface is less than 0.03 mass%, even though the hard coat layer contains inorganic metal particles, antibacterial and antiviral properties are not exhibited.

Claims

1. A hard coat film having a hard coat layer containing an ionizing radiation curable resin on at least one side of a substrate, the hard coat layer further containing inorganic metal particles, the inorganic metal particles being present in an amount of 0.03 mass % or more on the surface of the hard coat layer opposite to the substrate side and within a layer up to a depth of 0.5 μm from the surface.

2. 2. The hard coat film according to claim 1, wherein the inorganic metal particles are an inorganic material containing at least a silver component.

3. 3. The hard coat film according to claim 1, wherein the hard coat layer further contains an antistatic agent.

4. 3. The hard coat film according to claim 1, wherein the hard coat layer further contains inorganic fine particles.

5. 3. The hard coat film according to claim 1, wherein the hard coat layer further contains an anti-fogging agent.

6. 3. The hard coat film according to claim 1, wherein the hard coat layer further contains organic fine particles.

7. 3. The hard coat film according to claim 1, wherein at least one thin film made of a metal or a metal oxide is laminated on the surface of the substrate opposite to the hard coat layer, or between the substrate and the hard coat layer.

Citation Information

Patent Citations

  • Hard coat film

    JP2009216750A

  • Antibacterial antistatic hard coat laminate

    JP2010234523A

  • Hard coat film, heat ray shielding film and organic element device using the same

    JP2012208169A