Method and apparatus for producing translucent laminate having translucency

The hydrophilization and anodization of a valve metal layer on a translucent base material while moving the laminate addresses surface uniformity and antibacterial efficacy issues, producing a high-productivity, flexible, and uniformly anodized laminate with enhanced translucency.

JP2024133982AInactive Publication Date: 2024-10-03MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044031
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing light-transmitting laminates suffer from issues with surface uniformity and damage during manufacturing, and there is a need for improved antibacterial efficacy and productivity.

Method used

A method involving hydrophilization of a valve metal layer on a translucent base material followed by anodization while moving the laminate in contact with an electrolyte, using a manufacturing apparatus with specific hydrophilizing and anodizing means, to produce a translucent laminate with excellent light-transmitting properties and antibacterial effects.

Benefits of technology

The method suppresses surface damage during manufacturing, enhances translucency, and achieves a wider range of antibacterial effects with high productivity, resulting in a flexible and uniformly anodized laminate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133982000001_ABST
    Figure 2024133982000001_ABST
Patent Text Reader

Abstract

To provide a method and apparatus for producing a translucent laminate capable of producing a translucent laminate capable of suppressing damage to the surface of the translucent laminate during production, and capable of producing a translucent laminate having excellent translucency and exhibiting a wider antibacterial effect with high productivity.SOLUTION: A method for producing translucent laminate having translucency is a method for producing a translucent laminate having a metal oxide layer formed by anodizing a valve metal layer 102 on a translucent substrate 101 comprises a hydrophilizing step of hydrophilizing the surface of the valve metal layer 102 in the laminate 103 having the valve metal layer 102 on the substrate 101, and an anodizing step of anodizing the valve metal layer 102 while continuously moving the laminate 103 in a state where the hydrophilized valve metal layer 102 is in contact with an electrolyte 120.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for producing a light-transmitting laminate having light-transmitting properties. [Background technology]

[0002] Antibiotics have been widely used as medicines, veterinary medicines, pesticides, feed additives, food additives, etc. for the purposes of treating diseases in humans and livestock, improving the productivity of agricultural, livestock and fishery products, preserving food, etc. In recent years, the emergence of resistant bacteria that are resistant to multiple types of antibiotics and against which antibiotics are ineffective or less effective has become a problem.

[0003] In recent years, there has been a trend toward restricting the use of antibiotics in order to prevent the emergence of resistant bacteria, and there is a demand for the development of technology that can inhibit the growth of bacteria without using antibiotics. Patent Document 1 describes a transparent light-transmitting laminate in which an aluminum base material laminated on a light-transmitting resin substrate is completely anodized, as a technology that can exert an antibacterial effect without using antibiotics. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent Publication No. 2022-64648 Summary of the Invention [Problem to be solved by the invention]

[0005] The light-transmitting laminate described in Patent Document 1 may be usable in a wide range of fields, such as packaging materials for food, display front panels, partitions, etc. However, although Patent Document 1 proposes a method for efficiently mass-producing the light-transmitting laminate, there is room for further improvement in terms of surface uniformity.

[0006] An object of the present invention is to provide a method and an apparatus for producing a light-transmitting laminate with high productivity, which suppresses damage to the surface of the light-transmitting laminate during production, has excellent light transmissivity, and can exert an antibacterial effect over a wider range. [Means for solving the problem]

[0007] The present invention relates to the following items [1] to [7]. [1] A method for producing a light-transmitting laminate having a metal oxide layer formed by anodizing a valve metal layer on a light-transmitting substrate, comprising the steps of: A method for manufacturing a light-transmitting laminate, comprising: a hydrophilization step for hydrophilizing a surface of the valve metal layer in a laminate having the valve metal layer on the base material; and an anodization step for anodizing the valve metal layer while continuously moving the laminate with the hydrophilized valve metal layer in contact with an electrolyte. [2] The manufacturing method described in [1], wherein in the anodizing process, a voltage is applied between a cathode plate in contact with the electrolytic solution but not in contact with the valve metal layer, and an anode terminal in contact with the valve metal layer but not in contact with the electrolytic solution. [3] The manufacturing method described in [1] or [2], wherein the difference between the water contact angle of the hydrophilized surface of the valve metal layer and the water contact angle of the surface of the metal oxide layer after anodization is 45° or less. [4] The method according to any one of [1] to [3], wherein the hydrophilization step includes hydrophilizing the surface of the valve metal layer using ultraviolet light. [5] The method according to any one of [1] to [4], wherein the hydrophilization step includes hydrophilizing the surface of the valve metal layer using ozone. [6] The method according to any one of [1] to [5], further comprising continuously carrying out the hydrophilization step while moving the laminate. [7] A manufacturing apparatus for use in the manufacturing method according to any one of [1] to [6], The method includes: a hydrophilizing means for hydrophilizing a surface of the valve metal layer; and anodizing means for anodizing the valve metal layer; An apparatus for manufacturing a light-transmitting laminate having light-transmitting properties, the apparatus anodizing the valve metal layer while continuously moving the laminate in a state in which the hydrophilized valve metal layer is in contact with an electrolyte. Effect of the Invention

[0008] According to the present invention, it is possible to provide a method and an apparatus for producing a light-transmitting laminate, which can suppress damage to the surface of the light-transmitting laminate during production, and can produce a light-transmitting laminate with excellent light transmission and wider antibacterial effect with high productivity. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic side view showing an embodiment of a production apparatus of the present invention. [Diagram 2] FIG. 2 is a schematic side view showing another embodiment of the production apparatus of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In this specification, a numerical range expressed by "to" means a range including the numerical values ​​before and after it as the lower limit and upper limit.

[0011] [Apparatus for manufacturing a light-transmitting laminate having light-transmitting properties] Hereinafter, a manufacturing apparatus that can be preferably used in the manufacturing method of the light-transmitting laminate having light-transmitting properties according to the embodiment will be described. FIG. 1 is a schematic side view showing one aspect of a manufacturing apparatus for carrying out the manufacturing method of the embodiment.

[0012] The manufacturing apparatus 1 shown in Fig. 1 is an apparatus for manufacturing a translucent laminate in which a band-shaped laminate 103 having a valve metal layer 102 on the surface of a translucent base material 101 is subjected to hydrophilic treatment and anodization to change the valve metal layer 102 into a metal oxide layer having antibacterial properties. In addition, by completely anodizing the valve metal layer 102, the valve metal layer 102 is changed into a translucent metal oxide layer.

[0013] The manufacturing apparatus 1 includes a hydrophilizing means 10 for hydrophilizing the surface of the valve metal layer 102 of the laminate 103, and an anodizing means 20 for anodizing the hydrophilized valve metal layer 102. The manufacturing apparatus 1 may include a moving means 30 for transporting the laminate 103 composed of the substrate 101 and the valve metal layer 102.

[0014] (Transportation) From the viewpoint of the manufacturing efficiency of the light-transmitting laminate, the moving means 30 is preferably configured to transport the laminate 103 along the moving direction B in a state where at least a part of the valve metal layer 102 of the laminate 103 is in contact with the electrolytic solution 120 used for anodization. The moving means 30 includes, for example, a guide roll 32 that rotates with the laminate 103 wound around it and transports the laminate 103 in a state where the laminate 103 is in contact with the electrolytic solution 120, and may be provided with rolls 31 and 33 that change the transport direction of the laminate 103. The guide roll 32 rotates in a direction A along the moving direction B of the laminate 103, and rotates at the same speed as the moving speed of the laminate 103.

[0015] (hydrophilic means) The hydrophilizing means 10 may be any means capable of hydrophilizing the surface of the valve metal layer 102 of the laminate 103, and may be, for example, a UV device that hydrophilizes the surface by ultraviolet light, an ozone device that hydrophilizes the surface by using ozone, or a UV ozone device that hydrophilizes the surface by using ultraviolet light and ozone. As the hydrophilizing means 10, one type may be used alone, or two or more types may be used in combination.

[0016] (Anodizing Method) FIG. 2 is a front view of a portion of the anodizing means 20 where the valve metal layer 102 of the laminate 103 is anodized, as viewed from the downstream side in the moving direction B of the laminate 103. As shown in FIG. As shown in Figures 1 and 2, from the viewpoint of the manufacturing efficiency of the translucent laminate, it is preferable that the anodizing means 20 comprises an anode terminal 21 in contact with the valve metal layer 102, a cathode plate 22 arranged opposite the valve metal layer 102 so as not to come into contact with the valve metal layer 102, and an electrolyte tank 23 for holding an electrolyte 120 between the valve metal layer 102 and the cathode plate 22.

[0017] The cathode plate 22 and the anode terminal 21 are connected to a power source (not shown), and a voltage can be applied to the valve metal layer 102 in contact with the electrolytic solution 120. The cathode plate 22 may be arranged so as to be completely immersed in the electrolytic solution 120, or may be arranged so as to be partially exposed from the electrolytic solution 120. In order to obtain a homogeneous light-transmitting laminate, it is preferable that the cathode plate 22 has a shape that covers the periphery of the valve metal layer 102 so that the distance between the cathode plate 22 and the valve metal layer 102 in the electrolytic solution 120 is approximately constant.

[0018] 1 and 2 show an example in which a plate-shaped cathode plate 22 is disposed opposite the laminate 103, but the shape of the cathode plate 22 is not limited to this and any desired shape can be adopted. In addition, the cathode plate is not limited to a single member and may be configured as a plurality of divided cathode plates.

[0019] The anode terminal 21 may be, for example, a contactor that contacts and energizes the valve metal layer 102, or may be an energizing roller. If the anode terminal 21 is in contact with the electrolytic solution 120, a current flows directly to the cathode plate 22 via the electrolytic solution 120, so that the valve metal layer 102 cannot be anodized. Therefore, the anode terminal 21 must be disposed so as not to come into contact with the electrolytic solution 120.

[0020] The anodizing means 20 may be provided with a temperature control device (not shown) that keeps the temperature of the electrolytic solution 120 constant. Usually, in order to cool the valve metal layer 102 to which a voltage is applied, a device that cools the electrolytic solution 120 is used as the temperature control device. The temperature control device may be, for example, a jacket that controls the temperature of the electrolytic solution 120 via the electrolytic solution tank 23, or a device that directly controls the temperature of the electrolytic solution 120 and circulates it. When the valve metal layer 102 is thick, the valve metal layer 102 may generate heat from the contact portion of the anode terminal 21 to the electrolytic solution tank 23. Therefore, it is preferable that the anode terminal 21 is arranged upstream of the electrolytic solution tank 23 and the cathode plate 22 in the moving direction B of the laminate 103. By arranging the anode terminal 21 upstream, the heated valve metal layer 102 can be immersed in the electrolytic solution 120 and cooled.

[0021] (Gas-liquid interface blocking means) In the manufacturing method of the embodiment, since the laminate 103 is moved while performing the anodic oxidation, the gas-liquid interface of the electrolytic solution 120 may be disturbed. In addition, it is difficult to strictly control the temperature at the gas-liquid interface, and the valve metal layer 102 may be rapidly oxidized at the gas-liquid interface. In order to suppress such disturbance of the reaction at the gas-liquid interface, it is preferable to provide the gas-liquid interface blocking means 40 in the manufacturing apparatus 1.

[0022] The gas-liquid interface blocking means 40 is preferably configured to block the gas-liquid interface near the anode terminal 21 and is preferably arranged to block the gas-liquid interface upstream of the moving direction B. The gas-liquid interface blocking means 40 may be, for example, a nip roll arranged to cover the part where the gas-liquid interface and the valve metal layer 102 contact each other. Alternatively, the device may be configured to supply a temperature-controlled inactivating gas that does not affect the anodization to the part where the gas-liquid interface and the valve metal layer 102 contact each other. Alternatively, the device may be configured to wind a protective film or the like attached on the valve metal layer 102 around a nip roll and peel it off in the electrolytic solution 120. By providing such a gas-liquid interface blocking means 40, the entire surface of the valve metal layer 102 can be anodized more uniformly.

[0023] [Method for producing a light-transmitting laminate having light-transmitting properties] The method for producing a light-transmitting laminate according to the embodiment is a method for producing a light-transmitting laminate having a metal oxide layer formed by anodizing a valve metal layer on a light-transmitting base material, and includes the following hydrophilization step and an anodization step. Hydrophilization step: The surface of the valve metal layer in the laminate having the valve metal layer on the substrate is hydrophilized. Anodizing step: the hydrophilized valve metal layer is anodized while the laminate is continuously moved in a state where the hydrophilized valve metal layer is in contact with an electrolyte. Hereinafter, a detailed explanation will be given by taking the case where the above-mentioned manufacturing apparatus 1 is used as an example.

[0024] (hydrophilization process) In the hydrophilization step, the surface of the valve metal layer 102 in the laminate 103 is hydrophilized. By making the surface of the valve metal layer 102 hydrophilic, the anodization of the valve metal layer 102 proceeds sufficiently in the anodization step in which the laminate is moved while the anodization is performed, and a translucent laminate with excellent appearance is obtained.

[0025] It is preferable to make the surface of the valve metal layer 102 hydrophilic by using ultraviolet light, in order to easily prevent bacteria attached to the laminate 103 from adversely affecting the antibacterial properties. It is preferable to make the surface of the valve metal layer 102 hydrophilic by using ozone, in order to easily remove organic matter attached to the laminate 103. In addition, in order to improve productivity, it is preferable to carry out the hydrophilization treatment continuously while moving the laminate 103 in the hydrophilization step.

[0026] The water contact angle of the hydrophilized surface of the valve metal layer 102 is preferably 60° or less, more preferably 45° or less, and even more preferably 25° or less. If the water contact angle is equal to or less than the upper limit, the meniscus formed between the laminate and the electrolyte when the laminate is transported becomes small, and the liquid surface is less likely to shake.

[0027] (Anodizing process) In the anodization process, the valve metal layer 102 is anodized while continuously moving the laminate 103 in a state where the hydrophilized valve metal layer 102 is in contact with the electrolyte 120. As a result, the valve metal layer 102 is changed into a metal oxide layer having antibacterial properties. In addition, by completely anodizing the valve metal layer 102, the valve metal layer 102 is changed into a translucent metal oxide layer.

[0028] In order to efficiently pass electricity through the valve metal layer 102 of the laminate 103, it is preferable to apply a voltage between the cathode plate 22, which is in contact with the electrolytic solution 120 but not in contact with the valve metal layer 102, and the anode terminal 21, which is in contact with the valve metal layer 102 but not in contact with the electrolytic solution 120, during the anodization process.

[0029] The voltage applied during anodization is preferably 5 to 100 V, more preferably 10 to 60 V, and even more preferably 20 to 30 V. When the applied voltage is within the above range, the base material 101 is less likely to be damaged by heat generated during anodization, and the base material 101 is less likely to break.

[0030] The temperature of the electrolytic solution 120 during anodization is preferably 0 to 30° C., and more preferably 0 to 20° C. If the temperature of the electrolytic solution 120 is within the above range, the base material 101 is less likely to be damaged by the heat generated during anodization, and the base material 101 is less likely to break.

[0031] In the conventional technology, the difference in water contact angle before and after anodization was large, whereas in the manufacturing method according to the embodiment, the surface of the valve metal layer 102 is hydrophilized before anodization, thereby reducing the difference in water contact angle after anodization. This reduces the meniscus at the gas-liquid interface of the electrolyte 120, making it possible to suppress rippling of the liquid. As a result, it is possible to manufacture a translucent laminate that is easily prevented from being damaged by current and has low haze and is less likely to break.

[0032] The difference in water contact angle before and after anodization, i.e., the difference between the water contact angle on the surface of the hydrophilized valve metal layer 102 and the water contact angle on the surface of the metal oxide layer after anodization, is preferably 45° or less, more preferably 40° or less, and even more preferably 30° or less. The water contact angle is measured by the sessile drop method using an automatic contact angle meter DM-300 (manufactured by Kyowa Interface Science Co., Ltd.).

[0033] As the electrolytic solution 120, for example, one or more of sulfuric acid, oxalic acid, an aqueous solution of phosphoric acid, and an aqueous solution of ammonium borate can be used, with sulfuric acid being preferred in terms of a fast anodization rate. When sulfuric acid is used as the electrolyte, the concentration of sulfuric acid is preferably 0.3M or more, more preferably 3M or more, and even more preferably 5M or more. If the concentration of sulfuric acid is equal to or more than the lower limit, it is easy to manufacture a light-transmitting laminate exhibiting strong antibacterial properties. The concentration of sulfuric acid is preferably 15M or less, more preferably 12M or less. If the concentration of sulfuric acid is equal to or less than the upper limit, it is easy to stably pass electricity through the valve metal layer 102 during anodization, and it is easy to continuously manufacture a homogeneous light-transmitting laminate.

[0034] (Laminate) A laminate 103 used in the method for producing a light-transmitting laminate according to the embodiment has a valve metal layer 102 laminated on a light-transmitting base material 101 . The substrate 101 may be a single-layer substrate or a multi-layer substrate. The material of the base material 101 is not particularly limited as long as it is light-transmitting, and examples of the material include glass, polypropylene, polyethylene, polyethylene terephthalate, polystyrene, and nylon. The material of the base material 101 may be one type or two or more types.

[0035] The valve metal layer 102 is preferably an aluminum layer because it is easy to process, has few adverse effects, and is inexpensive. The purity of the valve metal in the valve metal layer 102 is preferably 95% by mass or more, more preferably 99% by mass or more, even more preferably 99.9% by mass or more, and particularly preferably 99.99% by mass or more. If the purity of the valve metal is equal to or more than the lower limit, it is easy to prevent the dissimilar metal from falling off during anodization and the occurrence of macroscopic defects on the surface.

[0036] The valve metal layer 102 is preferably a thin film in order to shorten the time required to completely anodize the valve metal layer 102. Specifically, the thickness of the valve metal layer 102 is preferably 20 nm to 1 μm, and more preferably 30 nm to 300 nm.

[0037] The valve metal layer 102 can be formed on the substrate 101 by a conventional method such as vapor deposition, sputtering, or bonding a metal foil. In order to improve the adhesion between the valve metal layer 102 and the substrate 101, various metal thin films (not shown) having a thickness of several nm may be provided between the valve metal layer 102 and the substrate 101.

[0038] (Transparent laminate) The light-transmitting laminate produced by the production method of the present invention is a light-transmitting laminate having a light-transmitting substrate and a metal oxide layer formed from a valve metal layer. The valve metal layer is anodized and doped with anions, so that the metal oxide layer exhibits strong antibacterial properties. The light-transmitting laminate may include an unoxidized valve metal layer as a thin film to the extent that the light-transmitting property is not impaired.

[0039] The total light transmittance of the metal oxide layer in the translucent laminate is preferably 30% or more, more preferably 50% or more, and even more preferably 60% or more. If the total light transmittance of the metal oxide layer is equal to or more than the lower limit, the translucent laminate can be suitably used in applications requiring transparency that requires the contents inside to be visually recognized. The upper limit of the total light transmittance of the metal oxide layer is preferably 95% or less, but is not limited thereto. The total light transmittance of the metal oxide layer is measured by the method described in JIS K 7136:2000 "Determination of haze of plastics-transparent materials".

[0040] The haze of the light-transmitting laminate is preferably 0% or more and 70% or less. If the haze of the light-transmitting laminate is 70% or less, damage to the substrate is suppressed, and the light-transmitting laminate is easily prevented from being broken during processing. The haze of the light-transmitting laminate is measured by the method described in JIS K 7136:2000 "Determination of haze of plastics-transparent materials". EXAMPLES

[0041] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following description.

[0042] [Water contact angle] The water contact angle was measured by the drop method using an automatic contact angle meter DM-300 manufactured by Kyowa Interface Science Co., Ltd.

[0043] [Appearance evaluation] The light-transmitting laminate obtained in each example was visually inspected and evaluated according to the following criteria. <Evaluation criteria> ◯: The anodization of the aluminum layer has progressed sufficiently, and the light transmittance is excellent. ×: Anodization did not proceed sufficiently, and metallic luster was observed.

[0044] [Productivity evaluation] The productivity in the production of the light-transmitting laminate in each example was evaluated according to the following criteria. <Evaluation criteria> ◯: The productivity is excellent because the laminate is moved while the anodic oxidation is carried out continuously. ×: The laminate was in a stationary state during anodization, resulting in poor productivity.

[0045] [Example 1] A laminate in which a 50 nm thick aluminum layer with a purity of 99.99% was formed on a 100 μm thick PET film was cut into a strip of laminate with a width of 5 cm, and the surface of the aluminum layer was subjected to a hydrophilic treatment using a UV ozone device manufactured by Technovision Co., Ltd. The water contact angle of the aluminum layer surface in the laminate before the hydrophilic treatment was 73°, whereas the water contact angle after the hydrophilic treatment was 15°. The obtained laminate after hydrophilization was set in an anodizing treatment device. The laminate was moved through the electrolyte at a conveying speed of 40 mm / min facing a cathode plate, and a direct current voltage of 25 V was applied from the anode terminal in contact with the aluminum layer to anodize the aluminum layer to obtain a translucent laminate. As the electrolyte, sulfuric acid with a concentration of 12 mol / L and adjusted to a temperature of 0°C was used. The water contact angle of the metal oxide layer surface of the obtained translucent laminate was measured and found to be 25°.

[0046] [Comparative Example 1] A light-transmitting laminate was produced in the same manner as in Example 1, except that the hydrophilization treatment was not carried out before the anodization.

[0047] [Comparative Example 2] A light-transmitting laminate was produced in the same manner as in Example 1, except that the hydrophilization treatment was not carried out before the anodization, and the aluminum layer was anodized while the laminate was kept stationary.

[0048] The production conditions and evaluation results for each example are shown in Table 1.

[0049] [Table 1]

[0050] In Example 1, in which the surface of the aluminum layer was hydrophilized before anodization and the laminate was anodized while being moved, the anodization of the aluminum layer proceeded sufficiently to form a metal oxide layer with excellent light transmissivity, and a light-transmitting laminate with good appearance could be produced with high productivity. On the other hand, in Comparative Example 1, in which the surface of the aluminum layer was not hydrophilized before anodization, the aluminum layer of the obtained light-transmitting laminate was not completely anodized, and the appearance had a metallic luster. The difference in water contact angle could not be accurately measured. Also, the productivity of Comparative Example 2, in which the laminate was in a stationary state during anodization, was poor. [Explanation of symbols]

[0051] 1 Manufacturing equipment 10 Hydrophilization means 20 Anodizing Method 21 Anode terminal 22 Cathode plate 23 Electrolyte tank 30 Transportation 31 Rolls 32 Guide Roll 33 Rolls 40 Gas-liquid interface blocking means 101 Base material 102 Valve metal layer 103 Laminate 120 Electrolyte

Claims

1. A method for producing a light-transmitting laminate having a metal oxide layer formed by anodizing a valve metal layer on a light-transmitting substrate, comprising the steps of: A method for manufacturing a light-transmitting laminate, comprising: a hydrophilization step for hydrophilizing a surface of the valve metal layer in a laminate having the valve metal layer on the base material; and an anodization step for anodizing the valve metal layer while continuously moving the laminate with the hydrophilized valve metal layer in contact with an electrolyte.

2. The manufacturing method according to claim 1, wherein in the anodizing process, a voltage is applied between a cathode plate in contact with the electrolytic solution but not in contact with the valve metal layer, and an anode terminal in contact with the valve metal layer but not in contact with the electrolytic solution.

3. 3. The method according to claim 1, wherein the difference between the water contact angle of the hydrophilized surface of the valve metal layer and the water contact angle of the surface of the metal oxide layer after anodization is 45° or less.

4. The manufacturing method according to claim 1 or 2, wherein the hydrophilizing step includes hydrophilizing the surface of the valve metal layer using ultraviolet light.

5. 3. The method according to claim 1, wherein the hydrophilizing step comprises hydrophilizing the surface of the valve metal layer using ozone.

6. The method according to claim 1 or 2, further comprising carrying out the hydrophilization step continuously while moving the laminate.

7. A manufacturing apparatus for use in the manufacturing method according to claim 1 or 2, The method includes: a hydrophilizing means for hydrophilizing a surface of the valve metal layer; and anodizing means for anodizing the valve metal layer; An apparatus for manufacturing a light-transmitting laminate having light-transmitting properties, the apparatus anodizing the valve metal layer while continuously moving the laminate in a state in which the hydrophilized valve metal layer is in contact with an electrolyte.

Citation Information

Patent Citations

  • Production method and production device of antibacterial laminate

    JP2022064648A