Stretched porous film and method for producing the same

A stretched porous film using ethylene/(1-octene) copolymer and calcium carbonate achieves a balance between air permeability and mechanical strength, addressing the limitations of existing films by optimizing filler content and dispersion.

JP2024133997AInactive Publication Date: 2024-10-03MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023044056
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing porous films struggle to achieve a balance between air permeability and mechanical strength, particularly in thin films, with many technologies focusing on either property at the expense of the other.

Method used

A stretched porous film composed of a polyolefin resin, specifically an ethylene/(1-octene) copolymer, and an inorganic filler, such as calcium carbonate, is produced by controlling the content and dispersion of the filler within a predetermined range to enhance both air permeability and mechanical strength.

Benefits of technology

The film achieves an excellent balance between air permeability and mechanical strength, even in thin films, ensuring high flexibility and resistance to puncture while maintaining effective moisture and air transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133997000001
    Figure 2024133997000001
  • Figure 2024133997000002
    Figure 2024133997000002
Patent Text Reader

Abstract

To provide a stretched porous film which is excellent in a balance between air permeability and mechanical strength even if it is a thin film.SOLUTION: A stretched porous film contains a polyolefin-based resin and an inorganic filler, wherein the polyolefin-based resin contains (a) an ethylene-(1-octene) copolymer, the inorganic filler contains (b) calcium carbonate, when the total mass of (a) and (b) is 100 mass%, the content of (b) the calcium carbonate is within a range of 30 mass% or more and 50 mass% or less, and the thickness is less than 35 μm.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretched porous film and a method for producing the same. [Background technology]

[0002] Conventionally, a porous film is known in which a resin composition containing a polyolefin and an inorganic filler is stretched to cause interfacial peeling between the polyolefin and the inorganic filler, forming a large number of voids (micropores). In particular, a stretched porous film made of a resin composition containing a polyolefin and an inorganic filler is used as a moisture-permeable waterproof film that suppresses the penetration of liquids while having high air permeability and moisture permeability, since the internal micropores form interconnected pores. The stretched porous film is widely used in applications requiring breathability, moisture permeability, and waterproofness, such as sanitary materials such as paper diapers and feminine hygiene products, clothing such as work clothes, jumpers, jackets, medical clothing, and chemical protective clothing, masks, covers, drapes, sheets, and wraps. For example, Patent Document 1 discloses a polyethylene-based porous film having improved weather resistance and light resistance, which is a porous film obtained by stretching a film containing 50 to 200 parts by mass of an inorganic filler per 100 parts by mass of a polyethylene-based resin at least in the machine direction of the film to make it porous, and which is characterized in that the polyethylene-based resin contains a linear low-density polyethylene having a Z-average molecular weight (M) of 300,000 or more and being a copolymer of ethylene and an α-olefin having 6 or more carbon atoms.

[0003] By the way, in the case of making a film microporous by an inorganic filler, the porosity can be increased by increasing the content of the filler, thereby improving the air permeability, but the strength of the porous film is reduced.Therefore, for example, Patent Document 2 proposes a porous film having both air permeability and strength, which is a porous film obtained by stretching a film made of a polyethylene resin composition containing a high molecular weight polyethylene (a) having a weight average molecular weight of 250,000 or more and less than 500,000 and a high density polyethylene (b) having a weight average molecular weight of 100,000 or more and less than 250,000 in a composition ratio of (a) / (b)=10 / 90 to 90 / 10, and a resin composition containing a filler (c), and the porous film has an air permeability of 10 to 1000 seconds / 100 ml per 25 μm thickness.

[0004] Patent Document 3 discloses a porous film having excellent mechanical properties such as puncture strength, which is made of a thermoplastic resin composition containing a thermoplastic resin and a filler and has a puncture strength of 1 N or more and less than 2.5 N per 25 μm thickness. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2007-161787 A [Patent Document 2] JP 2007-297583 A [Patent Document 3] JP 2007-112855 A Summary of the Invention [Problem to be solved by the invention]

[0006] The above Patent Document 1 discloses a porous film having excellent weather resistance, but does not focus on the strength of the porous film, nor does it take into consideration the balance between air permeability and mechanical strength in a thin film. On the other hand, Patent Documents 2 and 3 disclose porous films having both air permeability and mechanical strength, but the balance between air permeability and mechanical strength in thin films is not necessarily satisfactory. SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a stretched porous film which, even though thin, has an excellent balance between air permeability and mechanical strength. [Means for solving the problem]

[0007] A first aspect of the present invention is a stretched porous film containing a polyolefin resin and an inorganic filler, and a second aspect of the present invention is a method for producing a stretched porous film, comprising the steps of producing a resin sheet using a resin composition containing a polyolefin and an inorganic filler, and then stretching the resin sheet in at least one axial direction.

[0008] Examples of specific embodiments of the present invention are given below. [1] A stretched porous film comprising a polyolefin resin and an inorganic filler, The polyolefin resin contains (a) an ethylene-(1-octene) copolymer, The inorganic filler includes (b) calcium carbonate, When the total mass of the (a) and (b) is taken as 100 mass%, the content of the (b) calcium carbonate is 30 mass% or more and 50 mass% or less, A stretched porous film having a thickness of less than 35 μm. [2] The stretched porous film according to [1], wherein the polyolefin resin has a melt flow rate (MFR) of 1.0 g / 10 min to 4.0 g / 10 min at 190° C. and 2.16 kg. [3] The density of the polyolefin resin is 0.910 to 0.950 g / cm 3 The stretched porous film according to [1] or [2], [4] The stretched porous film according to any one of [1] to [3], wherein the melt flow rate (MFR) of the (a) ethylene-(1-octene) copolymer at 190°C and 2.16 kg is 1.0 g / 10 min to 4.0 g / 10 min. [5] The density of the (a) ethylene-(1-octene) copolymer is 0.910 to 0.950 g / cm 3 The stretched porous film according to any one of [1] to [4], [6] The stretched porous film according to any one of [1] to [5], wherein the maximum tensile strength of the stretched porous film in the machine direction (MD direction) at 23° C. is 20 MPa or more. [7] The stretched porous film according to any one of [1] to [6], wherein the puncture strength divided by the thickness is 0.040 N / μm or more. [8] The stretched porous film according to any one of [1] to [7], which has an air permeability of 5000 sec / 100 mL or less. [9] A sanitary product comprising the stretched porous film according to any one of [1] to [8].

[10] A method for producing a stretched porous film, comprising the steps of producing a resin sheet using a resin composition containing a polyolefin resin and an inorganic filler, and stretching the resin sheet in at least one axial direction, The polyolefin resin contains (a) an ethylene-(1-octene) copolymer, The inorganic filler includes (b) calcium carbonate, When the total mass of the (a) and (b) is taken as 100 mass%, the content of the (b) calcium carbonate is 30 mass% or more and 50 mass% or less, The method for producing a stretched porous film, wherein the stretched porous film has a thickness of less than 35 μm.

[11] The method for producing a stretched porous film according to

[10] , wherein the polyolefin resin has a melt flow rate (MFR) of 1.0 g / 10 min to 4.0 g / 10 min at 190° C. and 2.16 kg.

[12] The density of the polyolefin resin is 0.910 to 0.950 g / cm 3 The method for producing a stretched porous film according to

[10] or

[11] ,

[13] The method for producing a stretched porous film according to any one of

[10] to

[12] , wherein the melt flow rate (MFR) of the (a) ethylene-(1-octene) copolymer at 190°C and 2.16 kg is 1.0 g / 10 min to 4.0 g / 10 min.

[14] The density of the (a) ethylene-(1-octene) copolymer is 0.910 to 0.950 g / cm 3 The method for producing a stretched porous film according to any one of

[10] to [13p], Effect of the Invention

[0009] According to the present invention, it is possible to provide a stretched porous film that is excellent in balance between air permeability and mechanical strength even though it is a thin film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The stretched porous film of the present invention (hereinafter, sometimes referred to as "the film") will be described below as one example of an embodiment of the present invention. The scope of the present invention is not limited to the embodiments described below.

[0011] <Terminology used in this specification> The term "stretched porous film" refers to a porous film that has been stretched at least in one axial direction, and the porous film refers to a film in which a plurality of fine pores having a pore size of 0.5 μm or less are formed. The pore size can be evaluated as the maximum pore size measured by the bubble point method (JIS K3832 or ASTM F316), and more specifically, the maximum pore size can be measured using a perm porometer.

[0012] Generally, a "film" refers to a thin, flat product that is extremely thin compared to its length and width, has an arbitrarily limited maximum thickness, and is usually supplied in roll form (Japanese Industrial Standard JISK6900). Generally, the term "sheet" is defined in the JIS as a thin, flat product, the thickness of which is generally small relative to its length and width. However, since the boundary between film and sheet is unclear, in this specification, both are used as terms having the same meaning, and both are referred to as "film" unified.

[0013] When it is written "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" and "preferably smaller than Y".

[0014] <Stretched porous film> The stretched porous film of the present invention is formed from a resin composition (hereinafter also referred to as "the present resin composition") containing at least a polyolefin resin and an inorganic filler. The polyolefin resin contains (a) an ethylene-(1-octene) copolymer, and the inorganic filler contains (b) calcium carbonate. The thickness of the stretched porous film is less than 35 μm.

[0015] When the total mass of the (a) ethylene-(1-octene) copolymer and the (b) calcium carbonate is taken as 100 mass%, the content of the (a) ethylene-(1-octene) copolymer is preferably 50 mass% to 70 mass%, more preferably 50 mass% to 65 mass%, and most preferably 50 mass% to 60 mass%.

[0016] When the total mass of (a) ethylene-(1-octene) copolymer and (b) calcium carbonate is taken as 100 mass%, the content of (b) calcium carbonate is preferably 30 mass% to 50 mass%, more preferably 35 mass% to 50 mass%, and most preferably 40 mass% to 50 mass%.

[0017] The stretched porous film of the present invention has the above-mentioned constitution, and therefore has an excellent balance between air permeability and mechanical strength even though it is a thin film. The stretched porous film of the present invention has an excellent balance between air permeability and mechanical strength even though it is a thin film, because the blending amount of calcium carbonate relative to the ethylene-(1-octene) copolymer is adjusted within a predetermined range, and therefore the dispersibility of calcium carbonate can be well maintained.

[0018] (Other resins) The resin composition may contain other resins besides the polyolefin-based resin. Examples of the other resins include polystyrene-based resins, acrylic-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, chlorinated polyethylene-based resins, polyester-based resins, polycarbonate-based resins, polyamide-based resins, ethylene-vinyl alcohol-based copolymers, ethylene-vinyl acetate-based copolymers, polymethylpentene-based resins, polyvinyl alcohol-based resins, polylactic acid-based resins, polybutylene succinate-based resins, polyacrylonitrile-based resins, polyethylene oxide-based resins, and the like. Examples of the other resins include cellulose resins, polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyarylate resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, fluorine resins, polyacetal resins, etc. These other resins may be used alone or in combination.

[0019] The content of other resins in the present resin composition (the content of other resins relative to the total mass (100 mass%) of the present resin composition) is preferably 50 mass% or less, more preferably 45 mass% or less, and most preferably 40 mass% or less.

[0020] (Other additives) The present resin composition may further contain various additives such as a plasticizer, a lubricant, a compatibilizer, a processing aid, an antioxidant, a heat stabilizer, a light stabilizer, an ultraviolet absorber, an antiblocking agent, an antifogging agent, a matting agent, an antibacterial agent, a deodorizer, an antistatic agent, a flame retardant, a colorant, and a pigment.

[0021] <Polyolefin resin> The polyolefin resin is a resin containing an olefin monomer as a main monomer component (the main monomer component refers to the monomer component having the largest content among all monomer components), and in the present invention, the polyolefin resin contains at least (a) ethylene-(1-octene) copolymer. The content of (a) ethylene-(1-octene) copolymer in the polyolefin resin (the content ratio of (a) ethylene-(1-octene) copolymer to the total mass (100 mass%) of the polyolefin resin) is preferably 50 mass% or more, more preferably 55 mass% or more, and even more preferably 60 mass% or more. The content of (a) ethylene-(1-octene) copolymer in the polyolefin resin may be 100 mass%.

[0022] The (a) ethylene-(1-octene) copolymer is a copolymer containing ethylene as a main monomer component and 1-octene as another monomer component, and it is preferable that the content of structural units derived from ethylene in the copolymer is 50 mol % or more. The content ratio is as follows: 1 H-NMR, 13 It can be measured by calculation from the results of NMR measurements such as C-NMR. More specifically, it can be measured using a Bruker Advance400M as a measuring device under the following conditions.

[0023] <Measurement conditions> Measurement temperature: 130℃ Solvent: ODCB+C6D6 Measurement method: 1 H, 13 C, DEPT135

[0024] The polyolefin resin may contain other polyolefin resins than the (a) ethylene-(1-octene) copolymer. Examples of the other polyolefin resins include homopolymers of α-olefins such as ethylene, propylene, 1-butene, 1-hexene, and 4-methyl-1-pentene, and olefin monomers such as dienes, isoprene, butylene, and butadiene, and multicomponent copolymers obtained by copolymerizing two or more of these. Furthermore, the other polyolefin resin may be a copolymer of vinyl acetate, (meth)acrylic acid, (meth)acrylic acid ester, glycidyl (meth)acrylate, vinyl alcohol, ethylene glycol, maleic anhydride, styrene, or a cyclic olefin. Among these, the other polyolefin resins are preferably ethylene / (α-olefin) copolymers such as ethylene / propylene copolymer, ethylene / (1-butene) copolymer, ethylene / (1-hexene) copolymer, and ethylene / (4-methyl-1-pentene) copolymer, or ethylene copolymers such as ethylene / vinyl acetate copolymer, ethylene / (meth)acrylic acid copolymer, ethylene / (meth)acrylic acid ester copolymer, ethylene / glycidyl (meth)acrylate, ethylene / vinyl alcohol copolymer, ethylene / ethylene glycol copolymer, ethylene / maleic anhydride copolymer, ethylene / styrene copolymer, ethylene / diene copolymer, and ethylene / cyclic olefin copolymer.

[0025] The content of other polyolefin resins than (a) ethylene-(1-octene) copolymer in the polyolefin resin (the content ratio of other polyolefin resins relative to the total mass (100 mass%) of the polyolefin resins) is preferably 50 mass% or less, more preferably 45 mass% or less, and most preferably 40 mass% or less.

[0026] <Melt flow rate of polyolefin resin> The melt flow rate (MFR) of the polyolefin resin at 190° C. and 2.16 kg is preferably 1.0 g / 10 min to 4.0 g / 10 min, more preferably 1.0 g / 10 min to 3.0 g / 10 min, and most preferably 1.0 g / 10 min to 2.5 g / 10 min. The melt flow rate is measured in accordance with JIS K 7210-1:2014. More specifically, in the case of a resin whose main monomer component is ethylene monomer, the measurement is performed under conditions of 190°C and a load of 2.16 kg, and in the case of a resin whose main monomer component is propylene monomer, the measurement is performed under conditions of 230°C and a load of 2.16 kg. When two or more kinds of polyolefin resins are used, it is preferable that the melt flow rate of the mixed resins at 190° C. and 2.16 kg is within the above range.

[0027] In addition, the melt flow rate (MFR) of the (a) ethylene-(1-octene) copolymer at 190°C and 2.16 kg is preferably 1.0g / 10min to 4.0g / 10min, more preferably 1.0g / 10min to 2.5g / 10min, and most preferably 1.0g / 10min to 2.3g / 10min. When the melt flow rate of the (a) ethylene-(1-octene) copolymer is in the above range, the moldability and stretchability of the porous film are good, and even a thin film can have both air permeability and mechanical strength. When the melt flow rate is 1.0g / 10min or more, the moldability of the porous film is improved, and when the melt flow rate is 4.0g / 10min or less, the mechanical strength can be increased in addition to improving the moldability and stretchability of the porous film. The melt flow rate is measured in accordance with JIS K 7210-1:2014 at 190°C and a load of 2.16 kg.

[0028] <Density of polyolefin resin> The density of polyolefin resin is 0.880 to 0.950 g / cm 3It is preferable that the density is 0.890 to 0.950 g / cm 3 More preferably, it is 0.910 to 0.950 g / cm 3 More preferably, the density is 0.910 to 0.945 g / cm 3 By setting the density to the above upper limit or less, the stretchability of the porous film becomes good, and it is possible to obtain a thin porous film having high flexibility, good air permeability and no stretching unevenness. The density is measured under the conditions of the pycnometer method in accordance with JIS K 7112:1999 B method, and when two or more polyolefin resins are used, it is preferable that the density of each of the polyolefin resins is within the above range.

[0029] (a) The density of ethylene-(1-octene) copolymer is 0.880-0.950 g / cm 3 It is preferable that the density is 0.890 to 0.950 g / cm 3 More preferably, it is 0.910 to 0.950 g / cm 3 More preferably, the density is 0.910 to 0.945 g / cm 3 By setting the density to the above upper limit or less, the stretchability of the porous film becomes good, and it is possible to obtain a thin porous film having high flexibility, good air permeability and no stretching unevenness. The density is measured under the conditions of the pycnometer method in accordance with JIS K 7112:1999 Method B.

[0030] <Inorganic filler> The present film contains at least (b) calcium carbonate as an inorganic filler. In the total mass of the (a) ethylene-(1-octene) copolymer and the (b) calcium carbonate, 100% by mass, the content of the (b) calcium carbonate is preferably in the range of 30% by mass to 50% by mass, more preferably 35% by mass to 50% by mass, and most preferably 40% by mass to 50% by mass. When the content of the calcium carbonate in the ethylene-(1-octene) copolymer is in the above range, it is considered that the dispersibility of the calcium carbonate in the ethylene-(1-octene) copolymer is good, and a stretched porous film having an excellent balance between air permeability and mechanical strength can be obtained even in a thin film. Inorganic fillers other than calcium carbonate can also be used. Specific examples of the fillers include fine particles and minerals such as calcium sulfate, barium carbonate, barium sulfate, titanium oxide, talc, clay, kaolinite, and montmorillonite.

[0031] <Thickness of this film> The thickness of the present film is less than 35 μm, and in particular, is preferably 5 μm or more, more preferably 5 μm to 30 μm, and most preferably 5 μm to 25 μm. The present film has an excellent balance between air permeability and mechanical strength in the above thickness range, i.e., in the thin film region.

[0032] <Physical properties of this film (1); porosity> The present film is a porous film stretched at least in one direction, and a porous film is a film in which a plurality of micropores having a pore size of 0.5 μm or less are formed. The porosity of the present film is calculated from the specific gravity (W1) of the present film and the specific gravity (W0) of the present resin composition by the following formula. The porosity of the present film is preferably 10% to 50%, more preferably 10% to 45%, and most preferably 10% to 40%. Porosity (%)= 100 ×[ 1-(W1 / W0)]

[0033] The specific gravity of the present film and the present resin composition can be measured as follows. First, the present film is cut into a size of 50 mm in the machine direction (MD) and 50 mm in the transverse direction (TD), and the specific gravity (W1) of the present film is measured. Next, the specific gravity (W0) of the present resin composition (Z) constituting the present film is measured. In measuring the specific gravity (W0) of the present resin composition (Z), an unstretched film of the present film is cut into a size of 50 mm in the machine direction (MD) and 50 mm in the transverse direction (TD), and the specific gravity is measured. Furthermore, if it is difficult to obtain an unstretched sheet, the film can be melted by heating it above its melting point to eliminate any voids, and then a press sample can be prepared. A piece measuring 50 mm in the machine direction (MD) and 50 mm in the transverse direction (TD) can be cut from the press sample to measure its specific gravity. The porosity is calculated from the specific gravity (W1) of the thus obtained film and the specific gravity (W0) of the resin composition (Z) according to the above formula.

[0034] <Physical properties of this film (2); basis weight> The basis weight of this film is 5g / m 2 ~30g / m 2 is preferable, and more preferably 5 g / m 2 ~20g / m 2 The basis weight is 5g / m 2 By satisfying the above, it is easy to ensure sufficient mechanical strength and water resistance. The basis weight is 30 g / m 2 Because the material satisfies the above requirements, it is extremely thin and lightweight, even when used in sanitary materials such as disposable diapers, back sheets for feminine hygiene products, and waterproof films, providing a comfortable fit. The basis weight is determined by measuring the mass (g) of a sample (machine direction (MD): 50 mm, transverse direction (TD): 50 mm) using an electronic balance and multiplying this value by 400.

[0035] <Physical properties of this film (3); Air permeability> The air permeability of the present film is preferably 5000 sec / 100 mL or less, more preferably 3000 sec / 100 mL to 100 sec / 100 mL, and most preferably 1000 sec / 100 mL to 200 sec / 100 mL. An air permeability of 100 sec / 100 mL or more makes it easy to ensure sufficient water resistance and liquid resistance, and an air permeability of 5000 sec / 100 mL or less suggests the presence of sufficient communicating pores. The air permeability is the number of seconds it takes for 100 mL of air to pass through a piece of paper, measured according to the method specified in JIS P8117:2009 (Gurley tester method), and can be measured using, for example, an air permeability measuring device (Oken type air permeability measuring device EGO1-55 model, manufactured by Asahi Seiko Co., Ltd.). In the present invention, the sample is measured at three random points, and the arithmetic average value is taken as the air permeability.

[0036] <Film properties (4): Moisture permeability> The moisture permeability of this film is 7000g / m 2 24h~2000g / m 2 24h is preferred, and 6000g / m 2 24h~3000g / m 2 The moisture permeability of this film is 6000g / m 2 -24 hours or less indicates water resistance. In addition, the moisture permeability is 3000g / m 2 A duration of 24 h or more suggests that the pores have sufficient interconnectivity. The moisture permeability of this film is measured in accordance with JIS Z0208:1976 (Test method for moisture permeability of moisture-proof packaging materials (cup method)) using 15g of calcium chloride as a moisture absorbent under conditions of a constant temperature and humidity environment of a temperature of 40°C and a relative humidity of 90%. Two samples are measured at random, and the arithmetic average value is calculated.

[0037] <Physical properties of this film (5); Maximum tensile strength> The maximum tensile strength in the machine direction (MD) of the present film at 23° C. is preferably 20 MPa or more, more preferably 25 MPa or more, and most preferably 30 MPa or more. When the maximum tensile strength in the machine direction (MD) of the present film is within the above range, sufficient mechanical strength and flexibility for practical use can be ensured. The above-mentioned machine direction (MD direction) refers to the direction in which the film is transported (machine direction) in the production process of the present film described below. The maximum tensile strength is measured in accordance with JIS K7161-1:2014 using three samples cut to a size of 100 mm in the machine direction (MD) x 10 mm in the transverse direction (TD), at a measurement temperature of 23°C, a measurement relative humidity of 50%, a tensile speed of 200 m / min, and a chuck distance of 50 mm. The upper limit of the ultimate tensile strength is usually 200 MPa or less. The maximum tensile strength can be adjusted to within the above range by adjusting the content of calcium carbonate relative to the ethylene-(1-octene) copolymer, adjusting the density or MFR of the polyolefin resin (particularly the ethylene-(1-octene) copolymer) to within the above range, adjusting the stretch ratio of the porous film to within the range described below, or adjusting the thickness to within the above range.

[0038] <Physical properties of this film (6); Puncture strength> The puncture strength of the present film is preferably at least 0.6 N, more preferably at least 0.65 N, and most preferably at least 0.7 N. If the puncture strength is within the above range, it is easy to obtain mechanical strength sufficient for practical use. The puncture strength is a value measured in accordance with JIS Z1707:2019, in which the test piece is fixed in a jig and pierced with a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm at a test speed of 300 mm / min under an environment of a measurement temperature of 23±2°C and a relative humidity of 50±10%, and is the maximum force (N) until the needle penetrates. Furthermore, the value of the puncture strength of the present film divided by the thickness is preferably 0.04 N / μm or more, more preferably 0.05 N / μm or more, and most preferably 0.06 N / μm or more. If the value of the puncture strength divided by the thickness is within the above range, sufficient mechanical strength can be obtained and damage to the film and the associated decrease in water pressure resistance can be prevented. For the same reason, the puncture strength of this film divided by its basis weight is 0.03 N / (g / m 2 ) or more, and preferably 0.035N / (g / m 2 ) or more, and 0.04N / (g / m 2 ) or more is most preferable. The upper limit of each is usually 0.20 N / μm or less or 0.19 N / (g / m 2 ) or less. The above-mentioned puncture strength and the value obtained by dividing the puncture strength by the thickness or basis weight can be adjusted to fall within the above-mentioned ranges by adjusting the content of calcium carbonate relative to the ethylene-(1-octene) copolymer, adjusting the density or MFR of the polyolefin resin (particularly the ethylene-(1-octene) copolymer) to fall within the above-mentioned ranges, adjusting the stretch ratio of the porous film to fall within the ranges described below, or adjusting the thickness to fall within the above-mentioned ranges.

[0039] <Manufacturing method of this film> The present film can be produced by a conventional method, but is preferably produced by a method including a step of producing a resin sheet using the present resin composition and then stretching the resin sheet in at least one axial direction. According to the present film production method, a stretched porous film having an excellent balance between air permeability and mechanical strength can be obtained by a conventional simple and low-cost production method, even if it is a thin film.

[0040] The film may be either planar or tubular, but planar is preferred from the viewpoints of productivity (several products can be produced in the width direction of the raw sheet) and printing on the inner surface. An example of a method for producing a planar film is a method in which the present resin composition is melted using an extruder, extruded into a film shape from a die, and cooled and solidified by a cooling roll, air cooling, or water cooling to obtain a film (unstretched film), which is then stretched in at least one axial direction and wound up by a winder to obtain a film.

[0041] As a method for obtaining the unstretched film, it is preferable to mix the resin composition (Z) constituting the film and then melt-knead it. Specifically, after mixing for an appropriate time with a mixer such as a tumbler mixer, mixing roll, Banbury mixer, ribbon blender, or super mixer, an extruder such as a counter-rotating twin-screw extruder or a co-rotating twin-screw extruder is used to promote uniform dispersion and distribution of the resin composition. The obtained resin composition can be molded into a film by connecting a die such as a T-die or a round die to the tip of the extruder. Alternatively, a strand die may be connected to the tip of a kneader, and the mixture may be pelletized by a method such as strand cutting or die cutting. The pellets (along with an additional composition, if necessary) may then be introduced into a single-screw extruder, etc., and a die such as a T-die or round die may be connected to the tip of the extruder to form a film. For forming into a film, film forming methods such as inflation molding, tubular molding, and T-die molding are preferred. The extrusion temperature is preferably about 180 to 260°C, more preferably 190 to 250°C. Controlling the dispersion state of the material by optimizing the extrusion temperature and shear state is also effective in achieving the desired physical and mechanical properties of the film described above.

[0042] The present film can be produced by stretching the unstretched film. For example, the resin is melted using an extruder, extruded from a T-die or a round die, cooled and solidified with a cooling roll, and stretched at least uniaxially by roll stretching in the machine direction (film flow direction, MD) or tenter stretching in the transverse direction (direction perpendicular to the film flow direction, TD). The film may be stretched in the longitudinal direction and then in the transverse direction, or may be stretched in the transverse direction and then in the longitudinal direction.Furthermore, the film may be stretched in the same direction two or more times, or may be stretched in the longitudinal direction, then in the transverse direction, and then in the longitudinal direction. Alternatively, the film may be stretched simultaneously in the longitudinal and transverse directions using a simultaneous biaxial stretching machine. Alternatively, a tubular unstretched film may be radially stretched by internal pressure by tubular molding.Furthermore, a tubular unstretched film obtained by inflation molding may be stretched in a folded state, and then the edge of the folded tubular stretched porous film may be cut and divided into two pieces, which are then wound up separately, or the edge of the folded unstretched film may be cut and divided into two pieces, which are then stretched and wound up separately.

[0043] In the present invention, it is preferable to perform stretching in the machine direction at least once, and it may be performed two or more times in the machine direction depending on the balance between stretching unevenness and breathability. That is, the present film is preferably a uniaxially stretched porous film. The stretching temperature is preferably 0°C to 120°C, more preferably 20°C to 90°C. The total stretching ratio is preferably 1.2 to 6.0, more preferably 1.5 to 5.5. By making the total stretching ratio 1.2 or more, a stretched porous film having excellent appearance due to uniform stretching can be obtained. On the other hand, by setting the total stretching ratio to 6.0 times or less, breakage of the film can be suppressed.

[0044] If necessary, for the purpose of improving various physical properties, a heat treatment or relaxation treatment can be performed at a temperature of 50° C. to 120° C. after stretching. When stretching is performed by roll stretching, the heat treatment can be performed by contacting the stretched film with a heated roll (anneal roll) between the stretching step and the winding step. Alternatively, while heating is being performed by the anneal roll, the speed of the next roll that comes into contact with the film may be slower than the speed of the anneal roll, thereby enabling the film to be relaxed. These heat treatments and relaxation treatments can also be carried out in separate steps after stretching an unstretched film and winding up the stretched porous film. If the temperature of the heat treatment or relaxation treatment is too low, it is difficult to reduce the shrinkage rate of the film, and if the temperature is too high, the film may wind around the roll or the formed micropores may be blocked. Therefore, it is preferable to carry out the heat treatment or relaxation treatment at a temperature of 50°C or higher and 120°C or lower. These heat treatments and relaxation treatments may be carried out in multiple separate steps.

[0045] If necessary, the present film may be subjected to surface treatments or finishes such as slitting, corona treatment, printing, application of an adhesive, coating, vapor deposition, etc.

[0046] <Application> The film has a large number of fine pores penetrating from the front to the back, and has excellent breathability, and can therefore be suitably used in applications requiring breathability and moisture permeability, such as sanitary products such as disposable diapers and feminine hygiene products, clothing such as work clothes, jumpers, jackets, medical clothing, and chemical protective clothing, and further, masks, covers, drapes, sheets, wraps, etc.

[0047] The above-mentioned sanitary products such as disposable diapers and feminine hygiene products have a structure in which an absorbent body that absorbs and retains bodily fluids and is usually made of cotton-like pulp, absorbent paper, etc. is enclosed between a back sheet material that is placed on the underside and sides of the absorbent body and a top sheet material (facing material) that is placed on the surface of the back sheet material (the side that comes into contact with the skin when in use).

[0048] The absorbent body usually has corners and protrusions, so if this film is used as the back sheet material or top sheet material, it has excellent strength and air permeability despite being a thin film, so there is no risk of the film being torn by the corners or protrusions of the absorbent body, causing bodily fluids to leak. EXAMPLES

[0049] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these. The measured values ​​and evaluations shown in the examples and comparative examples were carried out as follows. In the examples and comparative examples, the machine direction of the film is referred to as the "machine" direction (or MD), and the direction perpendicular thereto is referred to as the "transverse" direction (or TD).

[0050] (1) Porosity of stretched porous film The porosity of the stretched porous films of the Examples and Comparative Examples was measured by the above-mentioned measuring method. The results are shown in Table 2.

[0051] (2) Basis weight of stretched porous film The basis weights of the stretched porous films of the Examples and Comparative Examples were measured by the above-mentioned measuring method. The results are shown in Table 2.

[0052] (3) Air permeability of stretched porous film The air permeability of the stretched porous films of the Examples and Comparative Examples was measured by the above-mentioned measuring method. The results are shown in Table 2.

[0053] (4) Moisture permeability of stretched porous film The moisture permeability of the stretched porous films of the Examples and Comparative Examples was measured by the above-mentioned measuring method. The results are shown in Table 2.

[0054] (5) Maximum tensile strength of stretched porous film (MD direction) The maximum tensile strength (MD direction) of the stretched porous films of the Examples and Comparative Examples was measured by the above-mentioned measuring method. The results are shown in Table 2.

[0055] (6) Puncture strength of stretched porous film, etc. The puncture strength of the stretched porous films of the Examples and Comparative Examples was measured by the above-mentioned measuring method, and the value obtained by dividing the puncture strength by the thickness or basis weight was also calculated. The results are shown in Table 2.

[0056] (7) Evaluation of stretchability of stretched porous film The stretchability of the stretched porous films of the Examples and Comparative Examples was evaluated by visually checking the presence or absence of unstretched parts (uneven stretching) remaining on the porous film with an unwound length of 3 m, and rating the film as A if there were no unstretched parts and B if there were any unstretched parts. The results are shown in Table 2.

[0057] (8) Maximum pore size of stretched porous film The maximum pore diameters of the stretched porous films of the Examples and Comparative Examples were measured by the bubble point method using the above-mentioned measuring method. The results are shown in Table 2.

[0058] The raw materials used in the examples and comparative examples are as shown in Table 1. The physical properties of the raw materials are values ​​measured by the measuring methods described above. The inorganic filler used is heavy calcium carbonate "Lighton BS-0" (average particle size 1.1 μm, surface-treated with stearic acid) manufactured by Bihoku Funka Kogyo Co., Ltd.

[0059] [Table 1]

[0060] <Example 1> The raw materials shown in Table 1 were weighed in the composition ratios shown in Table 2, then charged into a Henschel mixer, mixed and dispersed for 5 minutes, melt-kneaded at a set temperature of 220 ° C. using a co-rotating twin-screw extruder, and then extruded into a T-die connected to the tip of the co-rotating twin-screw extruder, and taken up by a casting roll set at 35 ° C., cooled and solidified to obtain an unstretched film with a thickness of 38 μm. Thereafter, the unstretched film obtained was stretched 4.0 times in the MD between a roll (S) set at 70 ° C. and a roll (T) set at 70 ° C., with a draw ratio of 300% (S)-(T), to obtain a stretched porous film with a thickness of 10 μm. Various evaluations were performed on the obtained stretched porous film. The results are summarized in Table 2.

[0061] <Example 2> The raw materials shown in Table 1 were changed to the composition ratio shown in Table 2, and an unstretched film having a thickness of 42 μm was obtained. The stretching roll temperature was set to 75° C., the (S)-(T) roll draw ratio was set to 250%, and the film was stretched 3.5 times in the MD direction. A stretched porous film having a thickness of 15 μm was obtained in the same manner as in Example 1. Various evaluations were performed on the obtained stretched porous film. The results are summarized in Table 2.

[0062] <Example 3> The raw materials shown in Table 1 were changed to the composition ratio shown in Table 2, and an unstretched film having a thickness of 35 μm was obtained. The (S)-(T) roll draw ratio was set to 400%, and the film was stretched 5.0 times in MD. In the same manner as in Example 1, a stretched porous film having a thickness of 8 μm was obtained. Various evaluations were performed on the obtained stretched porous film. The results are summarized in Table 2.

[0063] <Example 4> The raw materials shown in Table 1 were changed to the composition ratio shown in Table 2, and an unstretched film having a thickness of 35 μm was obtained. The (S)-(T) roll draw ratio was set to 350%, and the film was stretched 4.5 times in the MD. In the same manner as in Example 1, a stretched porous film having a thickness of 9 μm was obtained. Various evaluations were performed on the obtained stretched porous film. The results are summarized in Table 2.

[0064] <Comparative Example 1> The raw materials shown in Table 1 were changed to the composition ratio shown in Table 2, and an unstretched film having a thickness of 41 μm was obtained. The stretching roll temperature was set to 110° C., the (S)-(T) roll draw ratio was set to 150%, and the film was stretched 2.5 times in the MD. A stretched porous film having a thickness of 18 μm was obtained in the same manner as in Example 1. Various evaluations were performed on the obtained stretched porous film. The results are summarized in Table 2.

[0065] <Comparative Example 2> The raw materials shown in Table 1 were changed to the composition ratio shown in Table 2, and an unstretched film having a thickness of 42 μm was obtained. The stretching roll temperature was set to 80° C., the (S)-(T) roll draw ratio was set to 150%, and the film was stretched 2.5 times in the MD. A stretched porous film having a thickness of 18 μm was obtained in the same manner as in Example 1. Various evaluations were performed on the obtained stretched porous film. The results are summarized in Table 2.

[0066] [Table 2]

[0067] The porous films obtained in Examples 1 to 4 were thin films that were uniformly stretched without unevenness, and had excellent air permeability and moisture permeability properties as well as good maximum tensile strength and puncture strength in the film machine direction (MD). These results suggest that the content of calcium carbonate relative to the ethylene-(1-octene) copolymer contained in the resin compositions of Examples 1 to 4 was within a predetermined range, which improved the dispersibility of calcium carbonate in ethylene-(1-octene), thereby allowing the resin compositions to have favorable air permeability and exhibit good mechanical strength even in thin films. On the other hand, in Comparative Example 1, the resin composition did not contain an ethylene-(1-octene) copolymer, and in Comparative Example 2, the content of calcium carbonate relative to the ethylene-(1-octene) copolymer in the resin composition was not within the specified range, so that a porous film with uneven stretching was obtained and the pin puncture strength and maximum tensile strength in the film machine direction (MD) were low values. [Industrial Applicability]

[0068] The stretched porous film of the present invention has an excellent balance between air permeability and mechanical strength even though it is a thin film. Therefore, it can be suitably used as an article (component sheet) for applications requiring air permeability or moisture permeability, such as disposable diapers, feminine hygiene products, etc., clothing such as work clothes, jumpers, jackets, medical clothing, and chemical protective clothing, and further, masks, covers, drapes, sheets, wraps, etc.

Claims

1. A stretched porous film containing a polyolefin resin and an inorganic filler, The polyolefin resin contains (a) an ethylene / (1-octene) copolymer, The inorganic filler includes (b) calcium carbonate, When the total mass of (a) and (b) is taken as 100 mass%, the content of (b) calcium carbonate is 30 mass% or more and 50 mass% or less, A stretched porous film having a thickness of less than 35 μm.

2. 2. The stretched porous film according to claim 1, wherein the melt flow rate (MFR) of the polyolefin resin at 190° C. and 2.16 kg is 1.0 g / 10 min to 4.0 g / 10 min.

3. The density of the polyolefin resin is 0.910 to 0.950 g / cm 3 3. The stretched porous film according to claim 2,

4. 2. The stretched porous film according to claim 1, wherein the melt flow rate (MFR) of the ethylene-(1-octene) copolymer (a) at 190° C. and 2.16 kg is 1.0 g / 10 min to 4.0 g / 10 min.

5. The density of the (a) ethylene (1-octene) copolymer is 0.910 to 0.950 g / cm 3 5. The stretched porous film according to claim 4,

6. 2. The stretched porous film according to claim 1, wherein the maximum tensile strength of the stretched porous film in the machine direction (MD direction) at 23° C. is 20 MPa or more.

7. 2. The stretched porous film according to claim 1, wherein the puncture strength divided by the thickness is 0.040 N / .mu.m or more.

8. 2. The stretched porous film according to claim 1, having an air permeability of 5000 sec / 100 mL or less.

9. A sanitary product comprising the stretched porous film according to any one of claims 1 to 8.

10. A method for producing a stretched porous film, comprising the steps of producing a resin sheet using a resin composition containing a polyolefin resin and an inorganic filler, and stretching the resin sheet in at least one axial direction, The polyolefin resin contains (a) an ethylene-(1-octene) copolymer, The inorganic filler includes (b) calcium carbonate, When the total mass of (a) and (b) is taken as 100 mass%, the content of (b) calcium carbonate is 30 mass% or more and 50 mass% or less, The method for producing a stretched porous film, wherein the stretched porous film has a thickness of less than 35 μm.

11. The method for producing a stretched porous film according to claim 10, wherein the melt flow rate (MFR) of the polyolefin resin at 190° C. and 2.16 kg is 1.0 g / 10 min to 4.0 g / 10 min.

12. The density of the polyolefin resin is 0.910 to 0.950 g / cm 3 The method for producing a stretched porous film according to claim 11,

13. The method for producing a stretched porous film according to claim 10, wherein the melt flow rate (MFR) of the (a) ethylene / (1-octene) copolymer at 190° C. and 2.16 kg is 1.0 g / 10 min to 4.0 g / 10 min.

14. The density of the (a) ethylene-(1-octene) copolymer is 0.910 to 0.950 g / cm 3 The method for producing a stretched porous film according to claim 13,

Citation Information

Patent Citations

  • Porous film

    JP2007112855A

  • Polyethylene porous film

    JP2007161787A

  • Porous film

    JP2007297583A