Method for manufacturing phosphate compound of alkaline earth metal

A two-step pH-controlled reaction process effectively reduces phosphorus in waste liquid during alkaline earth metal phosphate production, enhancing the moldability and yield of the compounds.

JP2024134131APending Publication Date: 2024-10-03JGC CATALYSTS & CHEMICALS LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023044253
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for producing alkaline earth metal phosphate compounds generate waste liquid with high unreacted phosphorus content.

Method used

A two-step process involving the reaction of an alkaline earth metal-containing suspension and a phosphorus-containing solution at different pH levels, followed by pH adjustment to reduce phosphorus content in the waste liquid.

Benefits of technology

The method significantly reduces phosphorus content in the waste liquid, allowing for the production of alkaline earth metal phosphate compounds with improved moldability and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134131000002
    Figure 2024134131000002
  • Figure 2024134131000003
    Figure 2024134131000003
  • Figure 2024134131000001
    Figure 2024134131000001
Patent Text Reader

Abstract

To provide a method for manufacturing a phosphate compound of alkaline earth metal with less unreacted phosphorus contained in a waste fluid.SOLUTION: A method for manufacturing a phosphate compound of alkaline earth metal includes: an alkaline earth metal-containing suspension preparing step of preparing alkaline earth metal-containing suspension in which salt containing alkaline earth metal is dispersed in water; a phosphorus solution preparing step of preparing a phosphorus solution in which a compound containing phosphorus is dissolved; a reaction step of preparing a mixed liquid whose pH is 5.0 or less by mixing the alkaline earth metal-containing suspension and the phosphorus solution; and a PH adjustment step of adjusting pH to a range of 5.5 or more and 7.0 or less by adding the salt containing the alkaline earth metal to the mixed liquid whose pH is 5.0 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an alkaline earth metal phosphate compound. [Background technology]

[0002] Phosphate compounds of alkaline earth metals, such as magnesium phosphate and calcium phosphate, are widely used as fertilizers, refractory binders, flame retardants, additives for food and beverages, and catalyst materials. For example, Patent Document 1 discloses magnesium phosphate used in food and beverages. Patent Document 2 discloses a catalyst containing magnesium phosphate.

[0003] Methods for producing alkaline earth metal phosphate compounds are also widely known. For example, Patent Document 3 discloses a method for producing trimagnesium phosphate compound ceramics, which is characterized by weighing magnesium hydrogen phosphate and magnesium oxide or magnesium carbonate, adding an appropriate amount of water, stirring in a pot mill at room temperature, drying the resulting slurry to obtain polyhydrate trimagnesium phosphate powder, and further calcining to obtain anhydrous trimagnesium phosphate. Patent Document 4 also discloses the preparation of magnesium hydrogen phosphate by a method of adding a slurry of magnesium hydroxide dispersed in water to phosphoric acid. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2000-184864 A [Patent Document 2] Japanese Patent Application Publication No. 7-100384 [Patent Document 3] Japanese Patent Application Publication No. 3-279205 [Patent Document 4] Special Publication No. 47-41824 Summary of the Invention [Problem to be solved by the invention]

[0005] Conventional methods for producing alkaline earth metal phosphate compounds have a problem in that waste liquid is generated during the synthesis of alkaline earth metal phosphate compounds, and this waste liquid contains a large amount of unreacted phosphorus.

[0006] Therefore, an object of the present invention is to provide a method for producing an alkaline earth metal phosphate compound in which the amount of unreacted phosphorus contained in the waste liquid is small. [Means for solving the problem]

[0007] The present inventors have discovered a production method in which an alkaline earth metal-containing salt and a phosphorus-containing compound are reacted in two separate steps at different pH levels to reduce the phosphorus content in the waste liquid after the reaction, and have completed the present invention.

[0008] More specifically, the method includes a step of preparing an alkaline earth metal-containing suspension in which an alkaline earth metal-containing salt is dispersed in water; a phosphorus aqueous solution preparation step of preparing a phosphorus aqueous solution in which a phosphorus-containing compound is dissolved; a reaction step of mixing the alkaline earth metal-containing suspension and the phosphorus aqueous solution to prepare a mixed solution having a pH of 5.0 or less; The method includes a pH adjustment step of adding the salt containing an alkaline earth metal to the mixed solution having a pH of 5.0 or less to adjust the pH to a range of 5.5 to 7.0. By using the method for producing an alkaline earth metal phosphate compound, the phosphorus content in the waste liquid after the reaction can be reduced. Effect of the Invention

[0009] According to the present invention, there is provided a method for producing an alkaline earth metal phosphate compound in which the waste liquid contains little phosphorus. [Brief description of the drawings]

[0010] [Figure 1]1 is a diagram comparing the manufacturing method of Example 1 and the manufacturing method of Comparative Example 1. FIG. [Diagram 2] FIG. 2 is a diagram comparing the manufacturing methods of Examples 1 to 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention includes an invention relating to a method for producing an alkaline earth metal phosphate compound (hereinafter, also referred to as the "production method of the present invention"). The production method of the present invention will be described in detail below.

[0012] [Production method of the present invention] The production method of the present invention includes an alkaline earth metal-containing suspension preparation step of preparing an alkaline earth metal-containing suspension in which a salt containing an alkaline earth metal is dispersed in water; a phosphorus aqueous solution preparation step of preparing an aqueous phosphorus solution in which a phosphorus-containing compound is dissolved; a reaction step of mixing the alkaline earth metal-containing suspension and the aqueous phosphorus solution to prepare a mixed solution having a pH of 5.0 or less; and a pH adjustment step of adding the salt containing an alkaline earth metal to the mixed solution having a pH of 5.0 or less to adjust the pH to a range of 5.5 to 7.0.

[0013] [Alkaline earth metal-containing suspension preparation process] In this step, an alkaline earth metal-containing suspension in which a salt containing an alkaline earth metal is dispersed is prepared. In the present invention, the term "suspension" refers to a liquid in which a solid is dispersed in water. Therefore, in this step, it is preferable to use a salt containing an alkaline earth metal with low solubility in water. Specifically, it is preferable to use any one of an alkaline earth metal carbonate, an alkaline earth metal hydroxide, and a mixture thereof (basic alkaline earth metal carbonate salt), and it is particularly preferable to use an alkaline earth metal hydroxide with low solubility in water. In addition, the alkaline earth metal contained in this salt is at least one selected from Be, Mg, Ca, Sr, Ba, and Ra, preferably at least one selected from Mg, Ca, and Ba, and more preferably Mg.

[0014] In this step, the alkaline earth metal-containing suspension can be prepared by adding the above-mentioned salt containing an alkaline earth metal to water and stirring. The method of preparing the alkaline earth metal-containing suspension is not limited to stirring. For example, after adding the salt containing an alkaline earth metal to water, the salt containing an alkaline earth metal can be dispersed in water by ultrasonic dispersion or shaking. The content of the salt containing an alkaline earth metal contained in the alkaline earth metal-containing suspension obtained in this step is preferably in the range of 1% by mass to 25% by mass, more preferably in the range of 3% by mass to 20% by mass, and particularly preferably in the range of 5% by mass to 15% by mass, in terms of the formula weight of the salt (excluding water of crystallization). By using an alkaline earth metal-containing suspension in which the content of the salt containing an alkaline earth metal is in the above-mentioned range, an alkaline earth metal phosphate compound with better moldability (for example, when molding the alkaline earth metal salt into a tablet shape, it can be molded even at a low pressure) can be obtained.

[0015] In this step, the ratio of the mass of the alkaline earth metal-containing salt used in this step to the mass of the alkaline earth metal-containing salt used in the production method of the present invention is preferably in the range of 85% to 99%, more preferably in the range of 90% to 99%, and particularly preferably in the range of 95% to 99%. The production method of the present invention includes two steps of adding an alkaline earth metal-containing salt (see Figure 1). If the weight of the alkaline earth metal-containing salt used in this step is adjusted to the above-mentioned range, the yield of the finally obtained alkaline earth metal phosphate compound is increased.

[0016] The temperature of the alkaline earth metal-containing suspension may be room temperature, but is preferably in the range of 50° C. to 95° C., more preferably in the range of 75° C. to 95° C., and particularly preferably in the range of 75° C. to 85° C. In order to adjust the temperature of the alkaline earth metal-containing suspension, for example, the alkaline earth metal-containing suspension obtained in the above-mentioned step may be heated with a heater. When the temperature of the alkaline earth metal-containing suspension is in the above-mentioned range, an alkaline earth metal phosphate compound with better moldability can be obtained.

[0017] [Phosphorus aqueous solution preparation process] In this step, a phosphorus aqueous solution containing phosphorus is prepared. In the present invention, the term "aqueous solution" refers to a liquid that does not contain solids and in which all components other than water are dissolved in water. Therefore, in this step, a phosphorus aqueous solution can be prepared by dissolving a compound containing phosphorus that is highly soluble in water in water. For example, a phosphate compound or diphosphorus pentoxide can be dissolved in water to prepare the phosphorus aqueous solution. Phosphorus may be used as it is or may be mixed with water. The phosphorus content of the phosphorus aqueous solution obtained in this step is preferably in the range of 20% by mass or more and less than 85% by mass, more preferably in the range of 25% by mass or more and 80% by mass or less, and particularly preferably in the range of 30% by mass or more and 75% by mass or less, calculated as H3PO4. By using a phosphorus aqueous solution having a phosphorus content in the above-mentioned range, an alkaline earth metal phosphate compound with better moldability can be obtained.

[0018] [Reaction process] In this step, the alkaline earth metal-containing suspension obtained in the alkaline earth metal-containing suspension preparation step and the phosphorus aqueous solution obtained in the phosphorus aqueous solution preparation step are mixed to prepare a mixed solution having a pH of 5.0 or less. If the pH of the mixed solution does not become 5.0 or less, a conventionally known acid such as sulfuric acid, hydrochloric acid, acetic acid, and phosphoric acid is added to adjust the pH. At this time, the phosphate of the alkaline earth metal precipitates as a solid content in the mixed solution obtained by mixing. In this step, the pH of the mixed solution is preferably adjusted to a range of 3.0 to 5.0, more preferably 4.0 to 5.0. If the pH of the mixed solution is in the above-mentioned range, the phosphorus concentration in the waste liquid is more likely to be reduced. The above-mentioned acids and bases such as sodium hydroxide, sodium carbonate, potassium hydroxide, potassium carbonate, and ammonia can be used to adjust the pH.

[0019] In this process, various alkaline earth metal phosphate compounds can be synthesized by adjusting the molar ratio of alkaline earth metal to phosphorus (alkaline earth metal / phosphorus). For example, when synthesizing a magnesium phosphate compound, if the ratio is adjusted to about 1 / 2, monomagnesium phosphate (Mg(H2PO4)2·4H2O) can be synthesized, if the ratio is adjusted to about 1 / 1, dimagnesium phosphate (MgHPO4·3H2O) can be synthesized, and if the ratio is adjusted to about 3 / 2, trimagnesium phosphate (Mg3(PO4)2·8H2O) can be synthesized. At this time, the molar ratio of alkaline earth metal to phosphorus is preferably adjusted to within a range of ±20% of the target molar ratio, and more preferably adjusted to within a range of ±10% of the target molar ratio. For example, when synthesizing dimagnesium phosphate, the molar ratio is preferably adjusted to within a range of 0.8 to 1.2, and more preferably adjusted to within a range of 0.9 to 1.1.

[0020] In this step, a method of adding an aqueous phosphorus solution to an alkaline earth metal-containing suspension, a method of adding an aqueous phosphorus solution to an aqueous phosphorus solution, or a method of simultaneously adding an aqueous phosphorus solution and an aqueous phosphorus solution can be used. In this step, it is preferable to use a method of adding an aqueous phosphorus solution to an aqueous phosphorus solution. By using this method, an alkaline earth metal phosphate compound with better moldability can be obtained. At this time, it is preferable to add the entire amount of the aqueous phosphorus solution to the alkaline earth metal-containing suspension for 5 minutes or more and 120 minutes or less, and it is more preferable to add the entire amount of the aqueous phosphorus solution to the alkaline earth metal-containing suspension for 15 minutes or more and 90 minutes or less. For example, it is preferable to adjust the addition speed using a pump or the like so that the entire amount of the aqueous solution can be added within the above-mentioned time range. When the aqueous solution is added at such an addition speed, an alkaline earth metal phosphate compound with even better moldability can be obtained. If this time is shortened, the particle size of the alkaline earth phosphate compound tends to increase, and the bulk density also tends to increase.

[0021] In this step, the temperature of the mixed liquid rises due to the heat of reaction generated when the alkaline earth metal-containing suspension and the phosphorus aqueous solution are mixed. It is preferable to suppress this temperature rise to 15°C or less, and more preferably to suppress it to 10°C or less. For example, when the temperature rises rapidly, the reaction heat can be suppressed by a method of slowing down the addition rate and waiting for the temperature of the mixed liquid to drop, or by a method of adjusting the heater temperature, etc. By suppressing the temperature rise to the above-mentioned range by such a method, it is possible to obtain an alkaline earth metal phosphate compound with better moldability.

[0022] In this step, the mixed liquid is preferably aged by being held at a temperature in the range of 50° C. to 95° C. for 15 minutes or more. At this time, the temperature of the mixed liquid is preferably adjusted to a range of 75° C. to 95° C., and more preferably adjusted to a range of 75° C. to 85° C. In addition, the holding time is preferably in the range of 30 minutes to 180 minutes, and more preferably in the range of 45 minutes to 90 minutes. The alkaline earth metal phosphate compound obtained by aging under such conditions has particularly good moldability.

[0023] [pH adjustment process] In this step, the salt containing the alkaline earth metal is added to the mixed solution having a pH of 5.0 or less to adjust the pH of the mixed solution to a range of 5.5 to 7.0. By including this step, the production method of the present invention can reduce the concentration of phosphorus contained in the wastewater.

[0024] The salt containing an alkaline earth metal used in this step can be the salt used in the above-mentioned alkaline earth metal-containing suspension preparation step. In this step, the ratio of the mass of the salt containing an alkaline earth metal used in this step to the mass of the salt containing an alkaline earth metal used in the production method of the present invention is preferably in the range of 1% to 15%, more preferably in the range of 1% to 10%, and particularly preferably in the range of 1% to 5%.

[0025] The mixed liquid obtained in this step contains an alkaline earth metal phosphate compound, and if necessary, water can be removed from the mixed liquid to separate the alkaline earth metal phosphate compound. For example, water can be removed by a conventionally known method such as filtration, centrifugation, or decantation to separate the alkaline earth metal phosphate compound. It is also possible to separate the alkaline earth metal phosphate compound by evaporation to dryness using a method such as heating or reducing pressure. In the present invention, even if the separation is performed by a method that does not produce waste liquid, the effect of the present invention can be enjoyed. This is because the yield of the finally obtained alkaline earth metal phosphate increases if the phosphorus contained in the waste liquid, i.e., unreacted phosphorus, is reduced. In addition, the separated alkaline earth metal phosphate may be washed with water or hot water. Furthermore, the separated alkaline earth metal phosphate may be dried, and may be dried at a temperature of 80°C or higher and 150°C or lower. The drying time at this time may be, for example, in the range of 1 hour or higher and 24 hours or lower. Separation may also be performed by a method that does not apply heat, for example, reduced pressure drying.

[0026] The waste liquid containing phosphorus generated from the mixed liquid obtained in this step can be reused in the alkaline earth metal-containing suspension preparation step described above (see FIG. 2). By reusing the waste liquid containing phosphorus in this way, it is possible to substantially eliminate the discharge of waste liquid containing phosphorus. In addition, since the waste liquid obtained by the production method of the present invention has a low phosphorus content, even if it is reused as it is in the alkaline earth metal-containing suspension preparation step described above, it is possible to produce alkaline earth metal phosphate with a stable yield. If waste liquid with a high phosphorus content is reused as it is, the yield is likely to vary. When the waste liquid is reused in the production method of the present invention, it is preferable to use waste liquid with a phosphorus content of 100 ppm or less. EXAMPLES

[0027] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. [Measurement method or evaluation method] The various measurements and evaluations were carried out as follows.

[0028] [1] Phosphorus content measurement 2.0 g of sample was weighed out accurately in a 10 mL measuring flask, and water was added to make the volume 10 mL, which was used as the test solution. The phosphorus concentration in the test solution was determined using an inductively coupled plasma emission spectrometer (Shimadzu Corporation, ICPS-8100, analysis software ICPS-8000).

[0029] [2]pH measurement To measure the pH in each process, we used a pH meter (product name: D-74) and a glass electrode (product name: 9625-10D) manufactured by Horiba Ltd., which had been calibrated with standard solutions of pH 1.68, 6.86, and 9.18. The glass electrode was placed in contact with each measurement target to measure the pH.

[0030] [3] X-ray diffraction measurements For the powders obtained in each Example, powder X-ray diffraction measurements were carried out under the following conditions. X-ray diffraction equipment: MiniFlex600 (Rigaku Corporation) Radiation source: Cu-Kα radiation Acceleration voltage, current: 40 kV, 15 mA Receiving slit: 13mm Scan speed: 5.0° / min Step width: 0.01° Measurement range (2θ): 10~80°

[0031] [Example 1] (Alkaline earth metal-containing suspension preparation step) 300 g of pure water was placed in a 1000 mL glass beaker. 30.41 g (97% of the total weight of magnesium hydroxide) of magnesium hydroxide (product name: UD-650, manufactured by Ube Materials) was added to the beaker and stirred to obtain a magnesium hydroxide suspension. The magnesium hydroxide suspension was heated to 80°C using a heater.

[0032] (Phosphorus aqueous solution preparation process) 122.5 g of a 40% by mass aqueous solution of phosphoric acid was prepared.

[0033] (Reaction process) An aqueous phosphoric acid solution was added to the magnesium hydroxide suspension at 80°C obtained in the above-mentioned process. The addition rate was adjusted so that the entire amount of the aqueous phosphoric acid solution was added in 60 minutes. The mixture obtained after the entire amount of the aqueous phosphoric acid solution was kept at 80°C for 1 hour while stirring to obtain a mixed liquid. The above-mentioned measurement [2] was performed on this mixed liquid, and the pH was 4.3.

[0034] (pH adjustment process) To the above mixture, 0.97 g of magnesium hydroxide (3% based on the total weight of magnesium hydroxide) was added and stirred for 30 minutes. The pH of the resulting mixture was measured as described in [2] above, and found to be 6.0. The solids contained in the resulting mixture were then filtered to separate the solids from the filtrate. The solids were dried at 100°C for 12 hours to obtain a powder. The powder was measured as described in [3] above, and a diffraction peak belonging to dimagnesium phosphate trihydrate was confirmed. The phosphorus content of the filtrate was measured as described in [1] above. The results are shown in Table 1.

[0035] [Example 2: Reuse of the filtrate from Example 1] In the alkaline earth metal-containing suspension preparation step, a powder and a filtrate were obtained in the same manner as in Example 1, except that water obtained by mixing 290 g of the filtrate (phosphorus concentration: 65 ppm) obtained by the method of Example 1 with 10 g of pure water was used instead of 300 g of pure water. Various measurements were performed on these in the same manner as in Example 1. The results are shown in Table 1.

[0036] [Example 3: Reuse of the filtrate from Example 2] In the alkaline earth metal-containing suspension preparation step, a powder and a filtrate were obtained in the same manner as in Example 1, except that water obtained by mixing 279 g of the filtrate (phosphorus concentration: 77 ppm) obtained by the method of Example 2 with 21 g of pure water was used instead of 300 g of pure water. Various measurements were performed on these in the same manner as in Example 1. The results are shown in Table 1.

[0037] [Comparative Example 1] A powder and a filtrate were obtained in the same manner as in Example 1, except that in the alkali metal-containing suspension preparation step, the amount of magnesium hydroxide was changed from 30.41 g (97% relative to the total weight of magnesium hydroxide) to 31.38 g (100% relative to the total weight of magnesium hydroxide), and no magnesium hydroxide was added in the pH adjustment step. Various measurements were performed on these in the same manner as in Example 1. The results are shown in Table 1.

[0038] [Table 1]

Claims

[Claim 1] an alkaline earth metal-containing suspension preparation step of preparing an alkaline earth metal-containing suspension in which a salt containing an alkaline earth metal is dispersed in water; a phosphorus aqueous solution preparation step of preparing a phosphorus aqueous solution in which a phosphorus-containing compound is dissolved; a reaction step of mixing the alkaline earth metal-containing suspension and the phosphorus aqueous solution to prepare a mixed solution having a pH of 5.0 or less; a pH adjustment step of adding the salt containing an alkaline earth metal to the mixed solution having a pH of 5.0 or less to adjust the pH to a range of 5.5 to 7.0, A method for producing alkaline earth metal phosphate compounds.

Citation Information

Patent Citations

  • Production process of calcium hydrogen phosphate dihydrate for fluorine-containing toothpaste

    CN115072684A

  • Manufacture of hydrogen calcium phosphate dihydrate

    JP1984021510A

  • Method for producing anhydride of calcium dihydrogenphosphate in crystalline coarse particle form and said anhydride of calcium dihydrogenphosphate

    JP1994191808A

  • Production of calcium dihydrogenphosphate dihydrate suitable for use in toothpaste