Electrode, secondary battery, battery pack, and vehicle
By integrating a titanium-containing solid electrolyte with a transition metal oxide in the electrode, the battery's discharge capacity is maintained through effective hydrofluoric acid trapping, addressing the deterioration issue and enhancing cycle and output performance.
Patent Information
- Application Number
- JP2023044522
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Non-aqueous electrolyte batteries, such as lithium ion secondary batteries, experience a decrease in discharge capacity due to the deterioration of the active material in the electrodes, primarily caused by hydrofluoric acid generated from side reactions.
Incorporating a titanium-containing solid electrolyte with a transition metal oxide active material in the electrode, where the X-ray absorption fine structure spectrum shows a specific shift in the Ti-K absorption edge, indicating a higher valence state, which traps hydrofluoric acid and suppresses its contact with the active material.
This configuration enhances the cycle performance and output performance of the battery by preventing the deterioration of the active material, leading to improved discharge capacity retention and efficiency.
Smart Images

Figure 2024134294000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]
[0002] 2. Description of the Related Art In non-aqueous electrolyte batteries such as lithium ion secondary batteries, there is a problem that the discharge capacity of the electrodes decreases with the increase in charge / discharge cycles. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2019-239890 [Patent Document 2] JP 2009-140910 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the embodiments is to provide an electrode having excellent cycle performance, a secondary battery including the electrode, a battery pack including the secondary battery, and a vehicle including the battery pack. [Means for solving the problem]
[0005] According to an embodiment, an electrode is provided. The electrode includes an active material and a titanium-containing solid electrolyte. The active material includes a transition metal oxide.
[0006] In an X-ray absorption fine structure spectrum at the Ti-K absorption edge for an electrode in a discharged state, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the first X-ray absorption amount I at a first incident X-ray energy in the range of 4930 eV to 5000 eV satisfies 0.2≦I≦0.6.
[0007] In an X-ray absorption fine structure spectrum at the Ti-K absorption edge for anatase titanium dioxide, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the second X-ray absorption amount at a second incident X-ray energy in the range of incident X-ray energy from 4930 eV to 5000 eV is equal to the first X-ray absorption amount I. The first incident X-ray energy is higher than the second incident X-ray energy.
[0008] According to another embodiment, a secondary battery including the electrode of the embodiment is provided.
[0009] According to another embodiment, a battery pack including the secondary battery of the embodiment is provided.
[0010] According to another embodiment, a vehicle including a battery pack of the embodiment is provided. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Diagram 2] 2 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 1. [Diagram 3] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 4] 4 is an enlarged cross-sectional view of part B of the secondary battery shown in FIG. 3. [Diagram 5] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 6] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 7] 7 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 6. [Figure 8] 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 9] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. [Figure 10] X-ray absorption fine structure spectrum showing an example of a titanium-containing solid electrolyte. [Figure 11] X-ray absorption fine structure spectra showing other examples of titanium-containing solid electrolytes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the embodiments will be described with reference to the drawings as appropriate. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Also, each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.
[0013] (First embodiment) One of the factors that causes the discharge capacity of an electrode to decrease with charge-discharge cycles is deterioration of the active material in the electrode, which can occur, for example, when hydrofluoric acid produced by a side reaction comes into contact with the active material.
[0014] Based on this result, the inventors conducted further research and achieved the electrode according to the first embodiment.
[0015] The electrode according to the first embodiment includes an active material and a titanium-containing solid electrolyte. The active material includes a transition metal oxide.
[0016] In an X-ray absorption fine structure spectrum at the Ti-K absorption edge for an electrode in a discharged state, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the first X-ray absorption amount I at a first incident X-ray energy in the range of 4930 eV to 5000 eV satisfies 0.2≦I≦0.6.
[0017] In an X-ray absorption fine structure spectrum at the Ti-K absorption edge for anatase titanium dioxide, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the second X-ray absorption amount at a second incident X-ray energy in the range of incident X-ray energy from 4930 eV to 5000 eV is equal to the first X-ray absorption amount I. The first incident X-ray energy is higher than the second incident X-ray energy.
[0018] The titanium-containing solid electrolyte can capture (trap) hydrofluoric acid, and therefore, for example, can prevent hydrofluoric acid generated by a side reaction from coming into contact with the active material, thereby preventing the active material from deteriorating.
[0019] The first X-ray absorption amount is a relative value when the X-ray absorption amount when the incident X-ray energy is 5500 eV in an X-ray absorption fine structure (XAFS) spectrum of the electrode in a discharged state is set to 1. The second X-ray absorption amount is a relative value when the X-ray absorption amount when the incident X-ray energy is 5500 eV in an XAFS spectrum of anatase titanium dioxide is set to 1.
[0020] In the XAFS spectrum of the Ti-K absorption edge, the range of incident X-ray energy from 4930 eV to 5000 eV is the X-ray Absorption Near Edge Structure (XANES) region. In the XANES region, the first X-ray absorption amount at the first incident X-ray energy is equal to the second X-ray absorption amount at the second incident X-ray energy, and the first incident X-ray energy is higher than the second incident X-ray energy, which means that the electrode in the discharged state contains a material with a higher valence than anatase titanium dioxide. The valence of anatase titanium dioxide is, for example, tetravalent.
[0021] Note that the first incident X-ray energy may be higher than the second incident X-ray energy at all points in the XANES region where the first X-ray absorption amount at the first incident X-ray energy and the second X-ray absorption amount at the second incident X-ray energy are equal. The first incident X-ray energy may be higher than the second incident X-ray energy at at least one point among points in the XANES region where the first X-ray absorption amount at the first incident X-ray energy and the second X-ray absorption amount at the second incident X-ray energy are equal.
[0022] Examples of materials having a higher valence than anatase titanium dioxide include, for example, titanium-containing solid electrolytes. Titanium-containing solid electrolytes having a higher valence than anatase titanium dioxide have a larger surface area as described below. Therefore, they can efficiently capture hydrofluoric acid. Therefore, cycle performance can be improved.
[0023] Hereinafter, electrodes according to embodiments will be described in detail with reference to the drawings.
[0024] The electrode may be, for example, for a nonaqueous electrolyte battery. The nonaqueous electrolyte battery may be, for example, a nonaqueous electrolyte battery with an alkali metal ion as a carrier ion. For example, it may be a lithium battery (lithium ion battery). The electrode may be, for example, for a secondary battery.
[0025] In the manufacturing process of a non-aqueous electrolyte battery, water is likely to be mixed in as an inevitable impurity. When a non-aqueous electrolyte containing fluorine atoms is used as the non-aqueous electrolyte to be combined with an electrode, a side reaction occurs between water and the non-aqueous electrolyte, and hydrofluoric acid (hydrogen fluoride, HF) may be generated as a decomposition product of the non-aqueous electrolyte. Details of the non-aqueous electrolyte will be described later.
[0026] When hydrofluoric acid comes into contact with a material contained in an electrode, it may dissolve, for example, a transition metal. The dissolved transition metal may be deposited, for example, on the electrode. In addition, when an electrode is combined with an electrolyte, hydrofluoric acid may react with the electrolyte to form lithium fluoride. The lithium fluoride may be deposited, for example, on the electrode. These substances deposited on the electrode may be a cause of an increase in resistance.
[0027] The electrode contains a titanium-containing solid electrolyte, which can suppress the elution of transition metals and the formation of lithium fluoride, thereby improving the output performance of the electrode.
[0028] The titanium-containing solid electrolyte is a solid material that has Li-ion conductivity. Here, "having Li-ion conductivity" means that the Li-ion conductivity is 1×10 -6 It means that the titanium-containing solid electrolyte has a lithium ion conductivity of 1000 S / cm or more. The titanium-containing solid electrolyte may be, for example, in the form of particles. At least a part of the surface of the titanium-containing solid electrolyte particles may be amorphous.
[0029] If the titanium-containing solid electrolyte is completely amorphous, that is, an amorphous solid electrolyte, there is a possibility that side reactions with the non-aqueous electrolyte may increase when combined with the non-aqueous electrolyte. Therefore, it is preferable that the titanium-containing solid electrolyte is at least partially crystalline.
[0030] The titanium-containing solid electrolyte preferably contains a titanium-containing composite oxide. The titanium-containing composite oxide may be, for example, a titanium-containing lithium phosphate composite oxide. Examples of titanium-containing lithium phosphate composite oxides include those having a NASICON (Sodium (Na) Super Ionic Conductor) type structure and represented by the general formula Li 1+x Mα 2 (PO 4 ) 3Examples include lithium phosphate solid electrolytes represented by the following formula. Mα in the general formula contains titanium (Ti). Mα may consist only of titanium (Ti), or may contain Ti and, for example, one or more selected from the group consisting of germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is in the range of 0 ≤ x ≤ 2.
[0031] Specific examples of the lithium phosphate solid electrolyte having a NASICON structure include Li 1+x Al x Ti 2-x (PO 4 ) 3 represented by the formula and having 0.1 ≤ x ≤ 0.5, the LATP compound; Li 1+x Al y Mβ 2-y (PO 4 ) 3 represented by the formula, where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca, and among the compounds having 0 ≤ x ≤ 1 and 0 ≤ y ≤ 1, compounds containing Ti in the composition; and Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 represented by the formula, where Mγ is one or more selected from the group consisting of Ti and Ge, and among the compounds having 0 < x ≤ 2 and 0 ≤ y < 3, compounds containing Ti in the composition can be mentioned.
[0032] The types of titanium-containing solid electrolytes can be one or more than two.
[0033] The content of the lithium phosphate composite oxide in the titanium-containing solid electrolyte is preferably more than 98% by mass. When the titanium-containing solid electrolyte contains more than 98% by mass of the lithium phosphate composite oxide, the fluoric acid capture effect can be easily obtained, so the cycle performance and output performance can be improved. The proportion of the lithium phosphate composite oxide in the titanium-containing solid electrolyte can be 100% by mass.
[0034] 10 is an X-ray absorption fine structure spectrum showing an example of a titanium-containing solid electrolyte that may be included in the electrode of the embodiment. The horizontal axis is incident X-ray energy, and the vertical axis is the relative value of the X-ray absorption. The relative value of the X-ray absorption is a value of the X-ray absorption normalized to 1 when the incident X-ray energy is 5500 eV. Spectrum 10 is an XAFS spectrum of anatase type titanium dioxide. Spectrum 11 is an XAFS spectrum of an example of a titanium-containing solid electrolyte. Spectra 10 and 11 are normalized to 1 when the incident X-ray energy is 5500 eV.
[0035] In spectrum 11, an incident X-ray energy in the range of 4930 eV to 5000 eV is defined as a first incident X-ray energy a, and an X-ray absorption amount for the first incident X-ray energy a is defined as a first X-ray absorption amount. The first X-ray absorption amount I satisfies 0.2≦I≦0.6.
[0036] Furthermore, in spectrum 10, a certain incident X-ray energy in the range of 4930 eV to 5000 eV is defined as a second incident X-ray energy b, and the X-ray absorption amount for the second incident X-ray energy b is defined as a second X-ray absorption amount. The second X-ray absorption amount is set to be equal to the first X-ray absorption amount I.
[0037] By doing so, it is possible to obtain a point a on spectrum 11 of the titanium-containing solid electrolyte where the first incident X-ray energy is higher than the second incident X-ray energy. Therefore, the electrode including the titanium-containing solid electrolyte according to spectrum 11 can have a first incident X-ray energy higher than the second incident X-ray energy. That is, the XAFS spectrum of the electrode can be shifted to the high energy side compared to the XAFS spectrum of anatase titanium dioxide.
[0038] The titanium-containing solid electrolyte according to the example shown in spectrum 11 can be prepared, for example, by subjecting a titanium-containing solid electrolyte to a surface treatment as follows. A crystalline titanium-containing solid electrolyte can be used for the surface treatment. The surface treatment can be performed, for example, by an acid treatment as follows.
[0039] The acid treatment can be carried out, for example, by putting the titanium-containing solid electrolyte into an aqueous hydrofluoric acid solution and stirring it. The concentration of the aqueous hydrofluoric acid solution is preferably 1% by mass or more and 5% by mass or less. The stirring temperature is preferably in the range of 25° C. or more and 45° C. or less. The stirring time is preferably in the range of 1 hour or more and 80 hours or less.
[0040] The surface of the titanium-containing solid electrolyte particles can be made amorphous by the acid treatment. When the concentration of the hydrofluoric acid solution is 1 mass % or more, the amorphization of the surface can be efficiently promoted. When the concentration of the hydrofluoric acid solution is 5 mass % or less, the amorphization can be prevented from proceeding excessively. Therefore, the crystal structure inside the titanium-containing solid electrolyte particles can be easily maintained. Therefore, it is easy to obtain titanium-containing solid electrolyte particles whose particle surfaces are amorphous and at least a part of the particles is crystalline. Such titanium-containing solid electrolyte particles are preferable because the amorphization state is stable.
[0041] The acid treatment can also be performed by immersing the titanium-containing solid electrolyte in a liquid obtained by adding water to a liquid electrolyte containing fluorine atoms. Details of the liquid electrolyte will be described later. An example of the liquid electrolyte containing fluorine atoms is lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF 4 ), lithium arsenic hexafluoride (LiAsF 6 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), or lithium bistrifluoromethylsulfonylimide (LiN(CF 3 SO 2 ) 2) as an electrolyte salt. The liquid electrolyte may contain one or more types of electrolyte salt. The concentration of water in the liquid is preferably 0.1% by mass or more and 1% by mass or less. By setting the concentration of water in the liquid to 0.1% by mass or more, the acid treatment can be carried out efficiently. By setting the concentration of water in the liquid to 1% by mass or less, the excessive progress of amorphization can be suppressed.
[0042] The surface treatment can increase the valence of the titanium-containing solid electrolyte, and therefore the electrode containing the surface-treated titanium-containing solid electrolyte can have a first incident X-ray energy higher than the second incident X-ray energy.
[0043] Furthermore, the surface area of the titanium-containing solid electrolyte particles can be increased by performing the surface treatment. This is because the particle surfaces are made amorphous by the surface treatment. Titanium-containing solid electrolyte particles with amorphous surfaces can efficiently capture hydrofluoric acid.
[0044] This is believed to be due to the following mechanism. The titanium-containing solid electrolyte has functional groups capable of capturing hydrofluoric acid on its surface. When the surface of the titanium-containing solid electrolyte particles is made amorphous by the above-mentioned surface treatment, the surface area of the particles increases. Therefore, the functional groups capable of capturing hydrofluoric acid increase, and the amount of hydrofluoric acid that the titanium-containing solid electrolyte particles can capture increases.
[0045] Therefore, in an electrode in which the first incident X-ray energy is higher than the second incident X-ray energy, the titanium-containing solid electrolyte has a high hydrofluoric acid trapping ability, which can improve cycle performance and output performance.
[0046] The difference (shift amount) between the first incident X-ray energy and the second incident X-ray energy is preferably within a range of 1 eV to 4 eV, and more preferably within a range of 3 eV to 3.5 eV.
[0047] When the difference between the first incident X-ray energy and the second incident X-ray energy is large, the titanium-containing solid electrolyte tends to have a large amount of amorphous portions.
[0048] If the difference between the first incident X-ray energy and the second incident X-ray energy is too large, the titanium-containing solid electrolyte may be amorphous to the inside. If the titanium-containing solid electrolyte is amorphous to the inside, the hydrofluoric acid trapping ability of the titanium-containing solid electrolyte may be reduced. The difference between the first incident X-ray energy and the second incident X-ray energy is preferably 4.0 eV or less, and more preferably 3.5 eV or less.
[0049] In addition, if the difference between the first incident X-ray energy and the second incident X-ray energy is too small, the effect of improving the hydrofluoric acid trapping ability due to at least a part of the surface of the titanium-containing solid electrolyte being amorphous may be reduced. The difference between the first incident X-ray energy and the second incident X-ray energy is preferably 1.0 eV or more, more preferably 3.0 eV or more.
[0050] 11 is an X-ray absorption fine structure spectrum showing another example of a titanium-containing solid electrolyte. The horizontal axis indicates incident X-ray energy, and the vertical axis indicates the relative value of the amount of X-ray absorption. Spectrum 12 is an XAFS spectrum relating to another example of a titanium-containing solid electrolyte. The other example of the titanium-containing solid electrolyte is similar to the titanium-containing solid electrolyte relating to spectrum 11 described above, except that the above-mentioned surface treatment is not performed.
[0051] Spectra 10 and 12 are normalized with the X-ray absorption amount set to 1 when the incident X-ray energy in each spectrum is 5500 eV.
[0052] In spectrum 12, an incident X-ray energy in the range of 4930 eV to 5000 eV is defined as a first incident X-ray energy c, and an X-ray absorption amount for the first incident X-ray energy c is defined as a first X-ray absorption amount I. The first X-ray absorption amount I satisfies 0.2≦I≦0.6.
[0053] Furthermore, in Spectrum 10, for a certain incident X-ray energy within the range where the incident X-ray energy is 4930 eV or more and 5000 eV or less, the second incident X-ray energy is defined as d, and the X-ray absorption amount for the second incident X-ray energy d is defined as the second X-ray absorption amount. The second X-ray absorption amount is made equal to the first X-ray absorption amount I.
[0054] On Spectrum 12, there is no point c where the first incident X-ray energy is higher than the second incident X-ray energy. Therefore, when the electrode includes a titanium-containing solid electrolyte related to Spectrum 12, the first incident X-ray energy cannot be higher than the second incident X-ray energy.
[0055] The X-ray absorption fine structure spectrum can be obtained as follows.
[0056] <X-ray Absorption Fine Structure Analysis> (Preparation of Sample for Measurement) When analyzing substances such as anatase-type titanium dioxide and titanium-containing solid electrolytes, the powder of the substance to be analyzed is subjected to X-ray absorption fine structure (XAFS) analysis. As the anatase-type titanium dioxide, those with a purity of 99.5% or more among commercially available anatase-type titanium dioxide powders can be used.
[0057] When analyzing the electrode, as described below, an electrochemical measurement cell is fabricated using a measurement electrode, and then the electrochemical measurement cell is discharged to bring the electrode into a discharged state.
[0058] When the electrode to be measured is incorporated in a battery, the electrode to be measured is removed from the battery, washed and dried as follows, and then used to prepare an electrochemical measurement cell. First, the battery containing the electrode is disassembled in a glove box filled with argon. The electrode to be measured is removed from the disassembled battery. This electrode is washed with an appropriate solvent. For example, methyl ethyl carbonate can be used as the solvent used for washing. The washed electrode is vacuum dried. In this way, the electrode for measurement is obtained.
[0059] Next, an electrochemical measurement cell is prepared using the measurement electrode. The electrochemical measurement cell can be prepared using the measurement electrode, a metallic lithium foil as a counter electrode, and a non-aqueous electrolyte. The non-aqueous electrolyte is lithium hexafluorophosphate (LiPF 6 ) to a concentration of 1M.
[0060] The prepared electrochemical measurement cell is discharged at 0.05 C, and the potential of the measurement electrode is adjusted to 3.0 V relative to metallic lithium. In this way, the electrode is put into a discharged state.
[0061] The discharged electrodes are subjected to X-ray absorption fine structure (XAFS) analysis.
[0062] (XAFS analysis) XAFS analysis can be performed using a synchrotron radiation facility such as the large synchrotron radiation facility SPring-8.
[0063] The measurement conditions for the Ti K edge XAFS were as follows: ·Spectrometer: Si(111) double crystal spectrometer Higher order light rejection: Rh-coated mirror 6mrad Incident X-ray size: 1mm length x 1mm width ·Measurement method: transmission method Detector: Ion chamber Under the above conditions, the incident light intensity I0 and the transmitted light intensity I1 are measured in the range of incident X-ray energy from 4600 eV to 6000 eV. The X-ray absorption amount for each incident X-ray energy is calculated from I0 and I1 using the following formula. μt in the formula indicates the X-ray absorption amount.
[0064]
number
[0065] An XAFS spectrum can be obtained by plotting the incident X-ray energy on the x-axis and the X-ray absorption amount (μt) on the y-axis. Using the Victoreen equation, which expresses the intensity change due to X-ray scattering, the data before the absorption edge is approximated by the least squares method, and the background is subtracted. Thus, the background is removed from the XAFS spectrum.
[0066] In the XAFS spectrum from which the background has been removed, the amount of X-ray absorption is normalized by setting the amount of X-ray absorption when the incident X-ray energy is 5500 eV as 1. In this way, a normalized spectrum can be obtained.
[0067] By performing XAFS analysis after discharging the electrode, it is possible to determine, for example, that the Ti atoms contained in the active material in the electrode are tetravalent, and therefore it is possible to match the valence of Ti between the anatase-type titanium dioxide used as the comparison standard and the electrode being measured.
[0068] The electrodes according to the embodiment will now be described in further detail.
[0069] Such an electrode may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer may include an active material, a titanium-containing solid electrolyte, and optionally a conductive agent and a binder. The active material includes a transition metal oxide.
[0070] The active material-containing layer may contain, as the active material, one type of transition metal oxide alone, or may contain two or more types of transition metal oxides in combination. The active material may contain a transition metal oxide in combination with another compound.
[0071] The form of the active material is not particularly limited. The active material may be in the form of, for example, primary particles, or in the form of secondary particles formed by aggregation of primary particles. The active material may be a mixture of primary particles and secondary particles. The active material may be in the form of granules or chunks having a larger size than the size of what is called a particle.
[0072] The active material may be in the form of a powder in which primary particles and secondary particles are aggregated. The average particle size of the active material powder may be in the range of 0.1 μm to 30 μm. The average particle size of the active material powder is preferably in the range of 0.5 μm to 30 μm.
[0073] The average particle size can be measured by a laser diffraction scattering method. The particle size at which the cumulative volume distribution in a particle size distribution chart obtained by the laser diffraction scattering method is 50% is defined as the average particle size (D50).
[0074] The specific surface area of the active material is not particularly limited, but is preferably 0.1 m 2 / g or more 200m 2 The specific surface area can be in the range of less than 5 m 2 / g or more 200m 2 It is preferable that the molecular weight is less than 1 / g.
[0075] Specific surface area is 5m 2 If the specific surface area is 200 m / g or more, the contact area with the electrolyte can be secured, so that good discharge rate characteristics can be obtained and the charging time can be shortened. 2 If the surface area is less than 1 / g, the reactivity with the electrolyte is not too high, so that the life characteristics can be improved. In addition, the coating property of the slurry containing the active material can be improved. The slurry will be described later.
[0076] Here, the specific surface area is measured by adsorbing molecules with known adsorption occupancy areas onto the powder particle surfaces at liquid nitrogen temperature, and then calculating the specific surface area of the sample from the amount of adsorption. The most commonly used method is the BET (Brunauer, Emmett, Teller) method, which uses low-temperature, low-humidity physical adsorption of an inert gas. This is the most famous method for calculating specific surface area, and extends the Langmuir theory, which is a theory of monolayer adsorption, to multilayer adsorption. The specific surface area calculated in this way is called the BET specific surface area.
[0077] The following description will be made separately for the case where the electrode is a negative electrode and the case where the electrode is a positive electrode.
[0078] 1) Negative electrode First, a case where the electrode according to the embodiment is a negative electrode will be described.
[0079] When the electrode according to the first embodiment is used as a negative electrode, examples of the transition metal oxide contained in the active material include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti 3 O 7 , 0≦y≦3), lithium titanate having a spinel structure (e.g., Li 4+x Ti 5 O 12 , 0≦x≦3), titanium dioxide (TiO 2 ), anatase type titanium dioxide, rutile type titanium dioxide, niobium pentoxide (Nb 2 O 5 ), hollandite-type titanium composite oxide, orthorhombic titanium-containing composite oxide, and monoclinic niobium titanium oxide.
[0080] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+a M I 2-b Ti 6-c M II d O 14+σ In this case, the compound represented by M Iis at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb and K. II is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na 2 Ti 6 O 14 (0≦a≦6).
[0081] As an example of the monoclinic niobium titanium oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium oxide include Li x Nb 2 TiO 7 (0≦x≦5).
[0082] Another example of monoclinic niobium titanium oxide is Li x Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0083] The conductive agent is blended to improve the current collecting performance and to reduce the contact resistance between the active material and the current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes, and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.
[0084] The binder is blended to fill the gaps between the dispersed active materials and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene-butadiene rubber (SBR), polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0085] The blending ratio of the active material, titanium-containing solid electrolyte, conductive agent, and binder in the active material-containing layer can be appropriately changed depending on the application of the electrode. For example, when the electrode is used as the negative electrode of a secondary battery, the active material (negative electrode active material) is preferably blended at a ratio of 68% by mass or more and 96% by mass or less. The titanium-containing solid electrolyte is preferably blended at a ratio of 0.05% by mass or more and 30% by mass or less. The conductive agent is preferably blended at a ratio of 2% by mass or more and 30% by mass or less. The binder is preferably blended at a ratio of 2% by mass or more and 30% by mass or less.
[0086] The total mixing ratio of the negative electrode active material, the titanium-containing solid electrolyte, the conductive agent, and the binder can be 100% by mass. At this time, the mixing ratio of each material may be any value regardless of the above ratio. For example, when the negative electrode active material is mixed at the above ratio, the mixing ratio of the titanium-containing solid electrolyte, the conductive agent, and the binder can be adjusted to 100% by mass by setting the mixing ratio of the titanium-containing solid electrolyte, the conductive agent, and the binder to any value. The mixing ratio of the conductive agent or the binder may be 0% by mass.
[0087] It is particularly preferable that the mixing ratios of the negative electrode active material, titanium-containing solid electrolyte, conductive agent, and binder are all within the above numerical ranges, and that the total mixing ratio is 100 mass %.
[0088] By making the amount of titanium-containing solid electrolyte 0.05% by mass or more, the output performance can be further improved. By making the amount of conductive agent 2% by mass or more, the current collection performance of the active material-containing layer can be improved. Furthermore, by making the amount of binder 2% by mass or more, the binding between the active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and binder 30% by mass or less each in order to increase capacity. In order to improve energy density, it is preferable to make the titanium-containing solid electrolyte 30% by mass or less.
[0089] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted and removed from the active material. For example, when the active material is used as a negative electrode active material, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The current collector may be, for example, a metal foil containing the above-mentioned material. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0090] The current collector may also include a portion on the surface of which the negative electrode active material-containing layer is not formed, and this portion can function as a negative electrode current collecting tab.
[0091] The negative electrode can be produced, for example, by the following method. First, an active material, a titanium-containing solid electrolyte, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, the negative electrode is produced.
[0092] In producing the negative electrode, for example, water can be used as the solvent for the slurry.
[0093] Alternatively, the negative electrode may be prepared by the following method: first, the active material, the titanium-containing solid electrolyte, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain the negative electrode.
[0094] 2) Positive electrode Next, a case where the electrode according to the embodiment is a positive electrode will be described.
[0095] For example, when the electrode according to the first embodiment is used as a positive electrode, examples of the active material may include, for example, oxides or sulfides. Examples of oxides and sulfides include compounds capable of inserting and desorbing Li or Li ions. The oxide may be a transition metal oxide. The transition metal oxide may be a compound containing a transition metal and oxygen. The type of transition metal may be one or more kinds. The transition metal oxide may be a compound consisting of a transition metal and oxygen, or may be a compound containing an element other than a transition metal and oxygen. Examples of transition metal oxides include, for example, polyanion compounds such as phosphates, sulfates, and silicates. Examples of phosphates include, for example, lithium phosphate having an olivine structure. Examples of sulfates include, for example, iron sulfate.
[0096] Specific examples of the transition metal oxide include, for example, manganese dioxide (MnO 2 ), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (for example, Li x Mn 2 O 4 or Li x MnO 2 ; 0 < x ≦ 1), lithium nickel composite oxide (for example, Li x NiO 2 ; 0 < x ≦ 1), lithium cobalt composite oxide (for example, Li x CoO 2 ; 0 < x ≦ 1), lithium nickel cobalt composite oxide (for example, Li x Ni 1-y Co y O 2 ; 0 < x ≦ 1, 0 < y < 1), lithium manganese cobalt composite oxide (for example, Li x Mn y Co 1-y O 2 ; 0 < x ≦ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (for example, Li x Mn 2-y Ni y O 4 ; 0 < x ≦ 1, 0 < y < 2), lithium phosphate having an olivine structure (for example, Li x FePO 4 ; 0 < x ≦ 1, Li x Fe 1-y Mn y PO 4 ; 0 < x ≦ 1, 0 < y ≦ 1, Li x CoPO 4 ; 0 < x ≦ 1), iron sulfate (Fe 2 (SO 4 ) 3 ), vanadium oxide (for example, V 2 O 5 ), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O 2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) is included.
[0097] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxides having a spinel structure (for example, Li x Mn 2 O 4 ; 0 < x ≤ 1), lithium nickel composite oxides (for example, Li x NiO 2 ; 0 < x ≤ 1), lithium cobalt composite oxides (for example, Li x CoO 2 ; 0 < x ≤ 1), lithium nickel cobalt composite oxides (for example, Li x Ni 1-y Co y O 2 ; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxides having a spinel structure (for example, Li x Mn 2-y Ni y O 4 ; 0 < x ≤ 1, 0 < y < 2), lithium manganese cobalt composite oxides (for example, Li x Mn y Co 1-y O 2 ; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (for example, Li x FePO 4 ; 0 < x ≤ 1), and lithium nickel cobalt manganese composite oxides (Li x Ni 1-y-z Co y Mn z O 2 ; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0098] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0099] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0100] In the positive electrode active material-containing layer, the positive electrode active material is preferably mixed in a ratio of 80% by mass to 98% by mass, the titanium-containing solid electrolyte is preferably mixed in a ratio of 0.05% by mass to 30% by mass, and the binder is preferably mixed in a ratio of 2% by mass to 20% by mass.
[0101] The total mixing ratio of the positive electrode active material, the titanium-containing solid electrolyte, and the binder can be 100% by mass. At this time, the mixing ratio of each material may be any value regardless of the above ratio. For example, when the positive electrode active material is mixed in the above ratio, the mixing ratio of the titanium-containing solid electrolyte and the binder can be adjusted to any value to adjust the total mixing ratio of the positive electrode active material, the titanium-containing solid electrolyte, and the binder to 100% by mass. The mixing ratio of the binder may be 0% by mass.
[0102] It is particularly preferable that the blending proportions of the positive electrode active material, titanium-containing solid electrolyte, and binder are all within the above numerical ranges, and that the total blending proportions is 100 mass %.
[0103] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0104] When a conductive agent is added, the positive electrode active material is preferably mixed in a ratio of 77% by mass to 95% by mass. The titanium-containing solid electrolyte is preferably mixed in a ratio of 0.05% by mass to 30% by mass. The binder is preferably mixed in a ratio of 2% by mass to 20% by mass. The conductive agent is preferably mixed in a ratio of 3% by mass to 15% by mass.
[0105] The total mixing ratio of the positive electrode active material, the titanium-containing solid electrolyte, the conductive agent, and the binder can be 100% by mass. At this time, the mixing ratio of each material may be any value regardless of the above ratio. For example, when the positive electrode active material is mixed at the above ratio, the mixing ratio of the titanium-containing solid electrolyte, the conductive agent, and the binder can be adjusted to 100% by mass by setting the mixing ratio of the titanium-containing solid electrolyte, the conductive agent, and the binder to any value. The mixing ratio of the binder may be 0% by mass.
[0106] It is particularly preferable that the blending proportions of the positive electrode active material, titanium-containing solid electrolyte, conductive agent, and binder are all within the above numerical ranges, and that the total blending proportions is 100 mass %.
[0107] By making the amount of the conductive agent 3% by mass or more, the above-mentioned effects can be achieved. Also, by making the amount of the conductive agent 15% by mass or less, when the electrode is used in combination with an electrolyte, the proportion of the conductive agent in contact with the electrolyte can be reduced. If this proportion is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0108] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si. The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99% by mass or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1% by mass or less.
[0109] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.
[0110] The positive electrode can be produced, for example, by the following method. First, an active material, a titanium-containing solid electrolyte, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. Then, this laminate is pressed. In this way, a positive electrode is produced. In producing the positive electrode, for example, N-methylpyrrolidone (NMP) can be used as the solvent for the slurry.
[0111] Alternatively, the positive electrode may be prepared by the following method: first, the active material, the titanium-containing solid electrolyte, the conductive agent, and the binder are mixed to obtain a mixture, then the mixture is formed into pellets, and then the pellets are placed on a current collector to obtain a positive electrode.
[0112] The electrode according to the first embodiment includes an active material and a titanium-containing solid electrolyte. The active material includes a transition metal oxide.
[0113] In an X-ray absorption fine structure spectrum at the Ti-K absorption edge for an electrode in a discharged state, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the first X-ray absorption amount I at a first incident X-ray energy in the range of 4930 eV to 5000 eV satisfies 0.2≦I≦0.6.
[0114] In the X-ray absorption fine structure spectrum at the Ti-K absorption edge of anatase titanium dioxide, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the second X-ray absorption amount at the second incident X-ray energy in the range of 4930 eV to 5000 eV is equal to the first X-ray absorption amount I. The first incident X-ray energy is higher than the second incident X-ray energy. Therefore, the electrode can improve the cycle performance.
[0115] Second embodiment According to the second embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. At least one of the positive electrode and the negative electrode is the electrode according to the first embodiment. That is, the secondary battery includes the electrode according to the first embodiment.
[0116] The secondary battery may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.
[0117] Moreover, such a secondary battery can further include an exterior member that houses the electrode group and the electrolyte.
[0118] Furthermore, such a secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.
[0119] Such a secondary battery may be, for example, a lithium secondary battery. The secondary battery also includes a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.
[0120] The negative electrode, the positive electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.
[0121] 1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode current collector and the negative electrode active material-containing layer may be the current collector and the active material-containing layer that may be included in the electrode according to the first embodiment, respectively. When the electrode according to the first embodiment is included as the positive electrode, the negative electrode may not be the electrode according to the first embodiment. For example, the negative electrode may not include the titanium-containing solid electrolyte described in the first embodiment.
[0122] Among the details of the negative electrode, those parts that overlap with the details explained in the first embodiment will be omitted.
[0123] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 More than 2.8g / cm 3 A negative electrode having a density of the negative electrode active material-containing layer within this range is excellent in energy density and electrolyte retention. The density of the negative electrode active material-containing layer is preferably 2.1 g / cm or less. 3 More than 2.6g / cm 3 It is more preferable that:
[0124] The negative electrode can be produced, for example, by the same method as that for the electrode according to the first embodiment.
[0125] 2) Positive electrode The positive electrode may include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode current collector and the positive electrode active material-containing layer may be the current collector and the active material-containing layer that may be included in the electrode according to the first embodiment, respectively. When the electrode according to the first embodiment is included as the negative electrode, the positive electrode may not be the electrode according to the first embodiment. For example, the positive electrode may not include the titanium-containing solid electrolyte described in the first embodiment. Details of the positive electrode that overlap with the details described in the first embodiment are omitted.
[0126] When using room temperature molten salt as the electrolyte of the battery, lithium iron phosphate, Li x VPO 4 It is preferable to use a positive electrode active material containing F(0≦x≦1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide, or a mixture thereof. These compounds have low reactivity with room temperature molten salts, so that the cycle life can be improved. Details of the room temperature molten salt will be described later.
[0127] The average primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material having an average primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material having an average primary particle size of 1 μm or less can smoothly diffuse lithium ions in the solid.
[0128] The specific surface area of the positive electrode active material is 0.1 m 2 / g or more 10m 2 / g or less. 2 A positive electrode active material having a specific surface area of 10m / g or more can secure sufficient sites for absorbing and releasing Li ions. 2 A positive electrode active material having a specific surface area of 100 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.
[0129] The positive electrode can be produced, for example, by the same method as that for the electrode according to the first embodiment.
[0130] 3) Electrolytes The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.
[0131] Examples of electrolyte salts include lithium perchlorate (LiClO 4 ), lithium hexafluorophosphate (LiPF 6 ), lithium tetrafluoroborate (LiBF4 ), lithium arsenic hexafluoride (LiAsF 6 ), lithium trifluoromethanesulfonate (LiCF 3 SO 3 ), and lithium bistrifluoromethylsulfonylimide (LiN(CF 3 SO 2 ) 2 The electrolyte salt is preferably one that is not easily oxidized even at high potential, such as LiPF 6 is most preferred.
[0132] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.
[0133] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.
[0134] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.
[0135] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.
[0136] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.
[0137] The inorganic solid electrolyte is a solid substance that has Li-ion conductivity. Here, Li-ion conductivity is defined as a Li-ion conductivity of 1×10 -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 1.0 S / cm or more. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes. Specific examples of the inorganic solid electrolyte are as follows.
[0138] The oxide-based solid electrolyte has a NASICON (Sodium (Na) Super Ionic Conductor) type structure and is represented by the general formula Li 1+x Mα 2 (PO4 ) 3 It is preferable to use a lithium phosphate solid electrolyte represented by the above formula. In the general formula, Mα is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is in the range of 0 ≦ x ≦ 2.
[0139] Specific examples of the lithium phosphate solid electrolyte having a NASICON-type structure include Li 1+x Al x Ti 2-x (PO 4 ) 3 represented by and 0.1 ≦ x ≦ 0.5 LATP compound; Li 1+x Al y Mβ 2-y (PO 4 ) 3 represented by and Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca and 0 ≦ x ≦ 1 and 0 ≦ y ≦ 1 compound; Li 1+x Al x Ge 2-x (PO 4 ) 3 represented by and 0 ≦ x ≦ 2 compound; and, Li 1+x Al x Zr 2-x (PO 4 ) 3 represented by and 0 ≦ x ≦ 2 compound; Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 represented by and Mγ is one or more selected from the group consisting of Ti and Ge and 0 < x ≦ 2, 0 ≦ y < 3 compound; Li 1+2x Zr 1-x Ca x (PO 4 ) 3 represented by and 0 ≦ x < 1 compound can be mentioned.
[0140] In addition, as the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, Li xPO y N z and 2.6≦x≦3.5, 1.9≦y≦3.8, and 0.1≦z≦1.3. 2.9 PO 3.3 N 0.46 ); Garnet-type structure La 5+x A x La 3-x Mδ 2 O 12 A is 1 or more selected from the group consisting of Ca, Sr, and Ba, Mδ is 1 or more selected from the group consisting of Nb and Ta, and 0≦x≦0.5; Li 3 Mδ 2-x L 2 O 12 wherein Mδ is at least one selected from the group consisting of Nb and Ta, and L may contain Zr, and 0≦x≦0.5; Li 7-3x Al x La 3 Zr 3 O 12 and 0≦x≦0.5; Li 5+x La 3 Mδ 2-x Zr x O 12 where Mδ is 1 or more selected from the group consisting of Nb and Ta, and 0≦x≦2. 7 La 3 Zr 2 O 12 ); and La 2 / 3-x Li x TiO 3 and 0.3≦x≦0.7.
[0141] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.
[0142] 4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.
[0143] 5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0144] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0145] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0146] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0147] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.
[0148] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0149] 6) Negative terminal The negative electrode terminal has a potential range of 1V to 3V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.
[0150] 7) Positive terminal The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.
[0151] Next, the secondary battery according to the embodiment will be described more specifically with reference to the drawings.
[0152] Fig. 1 is a cross-sectional view showing an example of a secondary battery, and Fig. 2 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 1.
[0153] The secondary battery 100 shown in Figures 1 and 2 includes a bag-shaped exterior member 2 shown in Figure 1, an electrode group 1 shown in Figures 1 and 2, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.
[0154] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0155] As shown in Fig. 1, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 2, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.
[0156] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 2. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.
[0157] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.
[0158] As shown in FIG. 1, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.
[0159] The secondary battery according to the embodiment is not limited to the secondary battery having the configuration shown in FIGS. 1 and 2, but may be a battery having the configuration shown in FIGS.
[0160] Fig. 3 is a partially cutaway perspective view showing a schematic diagram of another example of a secondary battery, and Fig. 4 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 3.
[0161] The secondary battery 100 shown in Figures 3 and 4 includes an electrode group 1 shown in Figures 3 and 4, an exterior member 2 shown in Figure 3, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.
[0162] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0163] The electrode group 1 is a laminated type electrode group, as shown in Fig. 4. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.
[0164] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0165] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not supported on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 4, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a belt-shaped negative electrode terminal 6. The tip of the belt-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.
[0166] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab 3c. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side of the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.
[0167] The secondary battery according to the second embodiment includes the electrode according to the first embodiment, and therefore the cycle performance of the secondary battery can be improved.
[0168] (Third embodiment) According to a third embodiment, there is provided a battery pack including a plurality of secondary batteries according to the second embodiment.
[0169] In such a battery pack, the individual cells may be electrically connected in series or parallel, or may be arranged in a combination of series and parallel connections.
[0170] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0171] Fig. 5 is a perspective view showing an example of a battery pack. The battery pack 200 shown in Fig. 5 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the second embodiment.
[0172] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 5 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.
[0173] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.
[0174] The battery pack according to the third embodiment includes the secondary battery according to the second embodiment, and therefore can achieve excellent cycle performance.
[0175] (Fourth embodiment) According to a fourth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the third embodiment. The battery pack may include a single secondary battery according to the second embodiment, instead of the battery assembly according to the third embodiment.
[0176] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0177] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0178] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0179] Fig. 6 is an exploded perspective view showing an example of a battery pack, and Fig. 7 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 6.
[0180] The battery pack 300 shown in Figs. 6 and 7 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0181] 6 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0182] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.
[0183] At least one of the plurality of unit cells 100 is a secondary battery according to the second embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 7. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0184] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0185] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.
[0186] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0187] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.
[0188] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0189] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0190] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0191] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0192] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0193] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0194] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0195] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0196] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal 352 and a negative terminal 353, respectively, of the external terminal 350 for current supply.
[0197] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0198] The battery pack according to the fourth embodiment includes the secondary battery according to the second embodiment or the battery pack according to the third embodiment, and therefore the battery pack can achieve excellent cycle performance.
[0199] Fifth embodiment According to a fifth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fourth embodiment.
[0200] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0201] Examples of vehicles include, for example, two to four wheel hybrid electric vehicles, two to four wheel electric vehicles, power assisted bicycles, and rail vehicles.
[0202] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0203] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.
[0204] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0205] FIG. 8 is a partially see-through view that illustrates a schematic example of a vehicle.
[0206] A vehicle 400 shown in Fig. 8 includes a vehicle body 40 and a battery pack 300 according to the fourth embodiment. In the example shown in Fig. 8, the vehicle 400 is a four-wheeled automobile.
[0207] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0208] 8 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0209] Next, an embodiment of a vehicle according to the present embodiment will be described with reference to FIG.
[0210] Fig. 9 is a diagram illustrating an example of a control system for an electrical system in a vehicle. The vehicle 400 illustrated in Fig. 9 is an electric vehicle.
[0211] The vehicle 400 shown in FIG. 9 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.
[0212] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 9, the mounting location of the vehicle power supply 41 is shown diagrammatically.
[0213] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.
[0214] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.
[0215] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the second embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.
[0216] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.
[0217] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.
[0218] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.
[0219] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 9) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a-200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a-200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed in the vicinity of the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.
[0220] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.
[0221] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.
[0222] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.
[0223] One terminal of the connection line L1 is connected to the negative terminal 414 of the vehicle power source 41. The other terminal of the connection line L1 is connected to the negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided in the connection line L1 between the negative terminal 414 and the negative input terminal 417.
[0224] One terminal of the connection line L2 is connected to the positive terminal 413 of the vehicle power source 41. The other terminal of the connection line L2 is connected to the positive input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive terminal 413 and the positive input terminal 418.
[0225] The external terminal 43 is connected to the battery management device 411. The external terminal 43 can be connected to an external power source, for example.
[0226] The vehicle ECU 42 cooperatively controls the vehicle power source 41, the switch device 415, the inverter 44, etc. together with other management devices and control devices including the battery management device 411 in response to operation inputs from the driver or the like. By the cooperative control of the vehicle ECU 42 etc., the output of electric power from the vehicle power source 41 and the charging of the vehicle power source 41 are controlled, and the overall management of the vehicle 400 is performed. Between the battery management device 411 and the vehicle ECU 42, data transfer regarding the preservation of the vehicle power source 41, such as the remaining capacity of the vehicle power source 41, is performed via a communication line.
[0227] The vehicle according to the fifth embodiment mounts the battery pack according to the fourth embodiment. Therefore, since the cycle performance of the battery pack is high, the reliability of the vehicle is high.
Example
[0228] Examples will be described below, but the embodiments are not limited to the examples described below.
[0229] (Example 1) <Surface treatment of LATP> As LATP particles, Li1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 The particles were prepared. The surface treatment of the LATP particles was carried out as follows. A 2% by mass aqueous solution of hydrofluoric acid was placed in a polytetrafluoroethylene (PTFE) beaker, and the LATP particles were added. The mixture was stirred at 45°C for 80 hours. After stirring, the LATP particles were taken out and washed with water. Thus, the surface-treated LATP particles were obtained.
[0230] <Preparation of negative electrode> The negative electrode active material is monoclinic niobium titanium oxide (Nb 2 TiO 7 The average secondary particle diameter of the niobium titanium oxide powder was 7.5 μm. The specific surface area of the niobium titanium oxide powder was 4.0 m 2 / g. In addition, acetylene black was prepared as a conductive agent, and CMC and SBR were prepared as binders. The surface-treated LATP particles described above were prepared as the titanium-containing solid electrolyte. Next, the negative electrode active material, conductive agent, CMC, SBR, and titanium-containing solid electrolyte were added to water as a solvent in a ratio of 88 mass%:5 mass%:2 mass%:2 mass%:3 mass% and mixed to prepare a negative electrode slurry. This negative electrode slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 15 μm. Next, the coating was dried in a thermostatic chamber at 120 ° C. to form a negative electrode active material-containing layer. The negative electrode active material-containing layer was pressed to obtain a negative electrode.
[0231] (Examples 2 to 9) A negative electrode was produced in the same manner as in Example 1, except that the hydrofluoric acid concentration, stirring temperature, and stirring time in the surface treatment of LATP were changed as shown in Table 1.
[0232] Comparative Example 1 In the preparation of the negative electrode, the LATP particles not subjected to the surface treatment were used as the titanium-containing solid electrolyte instead of the surface-treated LATP particles, and the other procedures were the same as those in Example 1. In addition, since the LATP surface treatment was not performed in Comparative Example 1, the columns of the hydrofluoric acid concentration, the stirring temperature, and the stirring time of Comparative Example 1 in Table 1 are indicated with "-".
[0233] Example 10 The surface treatment of LATP was carried out in the same manner as in Example 1. <Preparation of positive electrode> The positive electrode active material is lithium nickel cobalt manganese composite oxide (LiNi 0.5 Co 0.2 Mn 0.3 O 2 ) powder was prepared. Acetylene black was prepared as a conductive agent. Polyvinylidene fluoride (PVdF) was prepared as a binder. The surface-treated LATP particles described above were prepared as a titanium-containing solid electrolyte. Next, the positive electrode active material, the conductive agent, the binder, and the titanium-containing solid electrolyte were added to N-methylpyrrolidone (NMP) as a solvent in a ratio of 87 mass%:5 mass%:5 mass%:3 mass% and mixed to prepare a positive electrode slurry. This positive electrode slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 15 μm. Next, the coating was dried in a thermostatic chamber at 120 ° C. to form a positive electrode active material-containing layer. The positive electrode active material-containing layer was pressed to obtain a positive electrode.
[0234] (Examples 11 to 18) A positive electrode was produced in the same manner as in Example 10, except that the hydrofluoric acid concentration, stirring temperature, and stirring time in the surface treatment of LATP were changed as shown in Table 2.
[0235] Comparative Example 2 In the preparation of the positive electrode slurry, the surface-treated LATP particles were replaced with LATP particles that had not been subjected to surface treatment, and the other procedures were carried out in the same manner as in Example 10 to prepare a positive electrode. In addition, since the surface treatment of LATP was not performed in Comparative Example 2, the columns of hydrofluoric acid concentration, stirring temperature, and stirring time of Comparative Example 2 in Table 2 are indicated with "-".
[0236] <Preparation of electrochemical measurement cell> An electrochemical measurement cell was prepared using a measurement electrode, a metallic lithium foil as a counter electrode, and a non-aqueous electrolyte. The electrodes prepared in each of the Examples and Comparative Examples were used as the measurement electrodes. The non-aqueous electrolyte was a solution of lithium hexafluorophosphate (LiPF 6 ) was dissolved at a concentration of 1M.
[0237] <0.2C discharge capacity measurement> (Examples 1 to 9, Comparative Example 1) The electrochemical measurement cell was then placed in a potential range of 1.0 V to 3.0 V with respect to the metallic lithium electrode. The battery was charged and discharged at room temperature. The current value during charging and discharging was 0.2 C (hourly discharge rate). The capacity during discharging was measured and designated as the 0.2 C discharge capacity (initial discharge capacity).
[0238] (Examples 10 to 18, Comparative Example 2) The capacity during discharge was measured in the same manner as in Examples 1 to 9 and Comparative Example 1, except that the charge / discharge potential range of the electrochemical measurement cell was changed to 3.0 V to 4.2 V based on the metallic lithium electrode, and this was taken as the 0.2 C discharge capacity (initial discharge capacity).
[0239] <10C / 0.2C discharge capacity ratio measurement> The electrochemical measurement cell was charged and discharged in the same manner as in the measurement of the 0.2 C discharge capacity performed for each Example and Comparative Example, except that the current value during discharge was changed to 10 C. The capacity during discharge was measured and defined as the 10 C discharge capacity. The ratio of the 10 C discharge capacity to the initial discharge capacity was calculated.
[0240] <Charge / discharge cycle test> (Examples 1 to 9, Comparative Example 1) The electrochemical measurement cell was charged and discharged at room temperature in a potential range of 1.0 V to 3.0 V with respect to a metallic lithium electrode. The current value during charging and discharging was 1C.
[0241] The above charging and discharging were regarded as one charge-discharge cycle. This charge-discharge cycle was repeated 100 times at room temperature.
[0242] After the charge and discharge were repeated 100 cycles, the 0.2C discharge capacity of the electrochemical measurement cell was measured in the same manner as described above. The discharge capacity at this time was defined as the discharge capacity after 100 cycles. The capacity retention rate (%) was calculated by dividing the discharge capacity after 100 cycles by the initial discharge capacity and multiplying by 100, assuming the initial discharge capacity as 100%.
[0243] (Examples 10 to 18, Comparative Example 2) A charge-discharge cycle test was conducted and the capacity retention rate (%) was calculated in the same manner as in Examples 1 to 9 and Comparative Example 1, except that the potential range of charge and discharge of the electrochemical measurement cell was changed to 3.0V to 4.2V based on the metal lithium electrode.
[0244] <Preparation of Samples for Measurement> As samples for measurement, commercially available anatase-type titanium dioxide powder with a purity of 99.5% was prepared. Also, the electrodes of the examples and comparative examples were put into a discharged state as follows to be used as samples for measurement.
[0245] The electrochemical measurement cell was discharged at 0.05C, and the potential of the electrodes of the examples and comparative examples was adjusted to 3.0V based on the metal lithium. In this way, the electrodes were put into a discharged state.
[0246] In an argon box, the discharged electrodes were taken out from the electrochemical measurement cell and washed with methyl ethyl carbonate (MEC). The washed electrodes were dried under vacuum to be used as samples for measurement.
[0247] <XAFS Analysis> The electrodes of the examples and comparative examples, and the samples for measurement of anatase-type titanium dioxide were subjected to XAFS analysis in the same manner as described above. The XAFS analysis was performed using BL16B2 of SPring-8.
[0248] The normalized spectrum for the electrodes of each of the Examples and Comparative Examples was compared with the normalized spectrum for anatase titanium dioxide in the following manner, and the amount of shift was calculated.
[0249] From the normalized spectrum of the electrodes of each Example and Comparative Example, a point was taken where the first X-ray absorption amount was 0.2 at the first incident X-ray energy in the range of 4930 eV to 5000 eV inclusive.From the normalized spectrum of anatase titanium dioxide, a point was taken where the second X-ray absorption amount was 0.2 at the second incident X-ray energy in the range of 4930 eV to 5000 eV inclusive.
[0250] The difference between the first incident X-ray energy (eV) and the second incident X-ray energy (eV) for each point was calculated and the "TiO 2 The shift from (eV) I = 0.2.
[0251] In the same manner as above, points where the first X-ray absorption amount was 0.5 and points where the second X-ray absorption amount was 0.5 were taken from each spectrum. The difference between the first incident X-ray energy (eV) and the second incident X-ray energy (eV) for each point was calculated, and the "TiO 2 The shift from (eV) I = 0.5.
[0252] The measurement results of each of the examples and comparative examples are shown in Tables 1 and 2.
[0253] [Table 1]
[0254] [Table 2]
[0255] The capacity retention rate is an index of cycle performance, and the 10C / 0.2C discharge capacity ratio is an index of output performance.
[0256] The electrodes in the examples are all made of "TiO 2 Shift from (eV) I=0.2" and "TiO 2 The shift amount (eV) from "I=0.5" was a positive value. That is, when the first X-ray absorption amount and the second X-ray absorption amount were equal at 0.2 and equal at 0.5, the first incident X-ray energy was higher than the second incident X-ray energy. This is considered to be because the electrodes of the examples all contain LATP particles that have been surface-treated as a titanium-containing solid electrolyte. It is considered that the first incident X-ray energy is higher than the second incident X-ray energy because the surface-treated LATP particles have a large valence.
[0257] The electrodes in the comparative examples are electrodes containing a titanium-containing solid electrolyte in the active material-containing layer, but all of them are "TiO 2 Shift from (eV) I=0.2" and "TiO 2 The shift amount (eV) from I=0.5 was 0. That is, when the first X-ray absorption amount and the second X-ray absorption amount were equal at 0.2 and equal at 0.5, the first incident X-ray energy was not higher than the second incident X-ray energy. This is considered to be because the valence of LATP did not change because the LATP particles contained in the electrode of the comparative example were not surface-treated.
[0258] The electrodes of the Examples all had higher 10C / 0.2C discharge capacity ratios and capacity retention rates than the electrodes of the Comparative Examples, demonstrating that the electrodes of the Examples are superior in output performance and cycle performance.
[0259] In addition, "TiO 2 Shift from (eV) I=0.2" and "TiO 2 In Examples 2 to 9 and 11 to 18, in which the shift amount (eV) from "I=0.5" was within the range of 1.0 to 4.0, the 10C / 0.2C discharge capacity ratio and the capacity retention rate were particularly high. 2 Shift from (eV) I=0.2" and "TiO 2Examples 2, 3, 5 to 9, 11, 12, and 14 to 18, in which the shift amount (eV) from "I=0.5" was within the range of 3.0 or more and 3.5 or less, had even higher 10C / 0.2C discharge capacity ratios and capacity maintenance rates. Therefore, it was revealed that an electrode in which the difference between the first incident X-ray energy and the second incident X-ray energy was 1 eV or more and 4 eV or less was particularly excellent in output performance and cycle performance, and an electrode in which the difference was 3 eV or more and 3.5 eV or less was even more excellent in output performance and cycle performance.
[0260] According to at least one embodiment described above, there is provided an electrode. The electrode includes an active material and a titanium-containing solid electrolyte. The active material includes a transition metal oxide.
[0261] In an X-ray absorption fine structure spectrum at the Ti-K absorption edge for an electrode in a discharged state, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the first X-ray absorption amount I at a first incident X-ray energy in the range of 4930 eV to 5000 eV satisfies 0.2≦I≦0.6.
[0262] In the X-ray absorption fine structure spectrum at the Ti-K absorption edge of anatase titanium dioxide, when the X-ray absorption amount is 1 when the incident X-ray energy is 5500 eV, the second X-ray absorption amount at the second incident X-ray energy in the range of 4930 eV to 5000 eV is equal to the first X-ray absorption amount I. The first incident X-ray energy is higher than the second incident X-ray energy. Therefore, the electrode can improve the cycle performance.
[0263] The invention according to the embodiment will be described below.
[0264] [1] An electrode comprising an active material and a titanium-containing solid electrolyte, the active material comprises a transition metal oxide; In the X-ray absorption fine structure spectrum at the Ti-K absorption edge for the electrode in a discharged state, When the incident X-ray energy is 5500 eV, the X-ray absorption amount is set to 1. The first X-ray absorption amount I at the first incident X-ray energy in the range of 4930 eV to 5000 eV satisfies 0.2≦I≦0.6, and In the X-ray absorption fine structure spectrum of anatase titanium dioxide at the Ti-K absorption edge, When the incident X-ray energy is 5500 eV, the X-ray absorption amount is set to 1. a second X-ray absorption amount at a second incident X-ray energy in the range of 4930 eV to 5000 eV is equal to the first X-ray absorption amount I; The first incident x-ray energy is greater than the second incident x-ray energy.
[0265] [2] The electrode according to [1], wherein the titanium-containing solid electrolyte contains a titanium-containing lithium phosphate composite oxide.
[0266] [3] The electrode according to [1] or [2], wherein a difference between the first incident X-ray energy and the second incident X-ray energy is 1 eV or more and 4 eV or less.
[0267] [4] The electrode according to any one of [1] to [3], wherein the transition metal oxide comprises at least one selected from the group consisting of lithium titanate having a ramsdellite structure, lithium titanate having a spinel structure, niobium pentoxide, a hollandite-type titanium composite oxide, an orthorhombic titanium composite oxide, and a monoclinic niobium titanium oxide.
[0268] [5] The electrode according to any one of [1] to [4], wherein the transition metal oxide includes at least one selected from the group consisting of manganese dioxide, iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide, lithium nickel composite oxide, lithium cobalt composite oxide, lithium nickel cobalt composite oxide, lithium manganese cobalt composite oxide, lithium manganese nickel composite oxide having a spinel structure, lithium phosphate oxide having an olivine structure, iron sulfate, vanadium oxide, and lithium nickel cobalt manganese composite oxide.
[0269] [6] A positive electrode; A negative electrode; Electrolytes and A secondary battery comprising: A secondary battery in which at least one selected from the group consisting of the positive electrode and the negative electrode is the electrode according to any one of [1] to [5].
[0270] [7] The secondary battery according to [6], wherein the electrolyte contains fluorine atoms.
[0271] [8] A battery pack including the secondary battery described in [6] or [7].
[0272] [9] An external terminal for supplying current; Protection circuit and The battery pack according to [8], further comprising:
[0273]
[10] A storage battery comprising a plurality of the secondary batteries, The battery pack according to [8] or [9], wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
[0274]
[11] A vehicle including the battery pack described in any one of [8] to
[10] .
[0275]
[12] A vehicle as described in
[11] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
[0276] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0277] 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material-containing layer, 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 22a...other end, 23...negative electrode side lead, 23a...other end, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 200...battery pack, 200a...battery pack, 200b...battery pack, 200c...battery pack, 300...battery pack, 30 0a...battery pack, 300b...battery pack, 300c...battery pack, 301a...assembled battery monitoring device, 301b...assembled battery monitoring device, 301c...assembled battery monitoring device, 342...positive connector, 343...negative connector, 345...thermistor, 346...protection circuit, 342a...wiring, 343a...wiring, 350...external terminal for energization, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.
Claims
1. An electrode comprising an active material and a titanium-containing solid electrolyte, the active material comprises a transition metal oxide; In the X-ray absorption fine structure spectrum at the Ti-K absorption edge for the electrode in a discharged state, When the X-ray absorption amount is set to 1 when the incident X-ray energy is 5500 eV, A first X-ray absorption amount I at a first incident X-ray energy in the range of 4930 eV to 5000 eV satisfies 0.2≦I≦0.6, and In the X-ray absorption fine structure spectrum of anatase titanium dioxide at the Ti-K absorption edge, When the X-ray absorption amount is set to 1 when the incident X-ray energy is 5500 eV, a second X-ray absorption amount at a second incident X-ray energy in the range of 4930 eV to 5000 eV is equal to the first X-ray absorption amount I; The first incident x-ray energy is greater than the second incident x-ray energy.
2. 2. The electrode of claim 1, wherein the titanium-containing solid electrolyte comprises a titanium-containing lithium phosphate composite oxide.
3. 3. The electrode according to claim 1, wherein a difference between the first incident X-ray energy and the second incident X-ray energy is 1 eV or more and 4 eV or less.
4. 3. The electrode according to claim 1, wherein the transition metal oxide comprises at least one selected from the group consisting of lithium titanate having a ramsdellite structure, lithium titanate having a spinel structure, niobium pentoxide, a hollandite-type titanium composite oxide, an orthorhombic titanium composite oxide, and a monoclinic niobium titanium oxide.
5. 3. The electrode according to claim 1 or 2, wherein the transition metal oxide comprises at least one selected from the group consisting of manganese dioxide, iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide, lithium nickel composite oxide, lithium cobalt composite oxide, lithium nickel cobalt composite oxide, lithium manganese cobalt composite oxide, lithium manganese nickel composite oxide having a spinel structure, lithium phosphate oxide having an olivine structure, iron sulfate, vanadium oxide, and lithium nickel cobalt manganese composite oxide.
6. A positive electrode and A negative electrode; Electrolytes and A secondary battery comprising: A secondary battery, wherein at least one selected from the group consisting of the positive electrode and the negative electrode is the electrode according to claim 1 or 2.
7. The secondary battery according to claim 6 , wherein the electrolyte contains fluorine atoms.
8. A battery pack comprising the secondary battery according to claim 6.
9. An external terminal for supplying electricity; Protection circuit and The battery pack of claim 8 further comprising:
10. A plurality of the secondary batteries are included, The battery pack according to claim 8 , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
11. A vehicle including the battery pack of claim 8.
12. The vehicle of claim 11, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP2015170464A
Carbon powder having enhanced electrical characteristics and use of the same
WO2001006583A1
Positive electrode active material for lithium secondary battery and method for producing same
WO2006009177A1
Amorphous solid electrolyte and all solid secondary battery using same
WO2019239890A1
All-solid battery
JP2009140910A
Cited By
Inorganic oxide powder and lithium ion secondary battery including electrode containing the same
JP2026086982A
Lithium-ion secondary battery comprising inorganic oxide powder and electrodes containing the same
JP7932460B2
Secondary battery
WO2026094321A1
Inorganic oxide powder and lithium-ion secondary battery including electrode containing same
WO2026105417A1