Polyamide composition containing graft-modified ethylenic polymer
A polyamide resin composition combining aliphatic long-chain polyamide and graft-modified ethylene/α-olefin copolymer addresses the imbalance in impact resistance, rigidity, and fluidity, resulting in improved mechanical properties of molded articles.
Patent Information
- Application Number
- JP2023044640
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Existing polyamide resin compositions struggle to achieve a balance between impact resistance, rigidity, and fluidity, with improvements in one property often leading to a decrease in the others.
A polyamide resin composition comprising 85.0 to 99.9% by mass of an aliphatic long-chain polyamide and 0.1 to 15.0% by mass of a graft-modified ethylene/α-olefin copolymer, where the graft-modified ethylene/α-olefin copolymer contains 0.1 to 1.5% by mass of skeletal units derived from vinyl compounds with polar groups and a specific ethylene-to-α-olefin ratio, is used to enhance impact resistance, rigidity, and fluidity.
The composition provides a balanced improvement in impact resistance, rigidity, and fluidity, enabling the production of molded articles with enhanced mechanical properties.
Smart Images

Figure 2024134375000001 
Figure 2024134375000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide resin composition containing a graft-modified ethylene / α-olefin copolymer that satisfies specific requirements, and a molded article obtained therefrom. [Background technology]
[0002] Due to their excellent physical properties, engineering plastics such as polyamide resins are used in a variety of electrical and electronic components, machine components, and automotive components. In these applications, molded products are becoming thinner, smaller, and more complex in shape, so there is a demand for an improved balance of impact resistance, rigidity, and fluidity, but this is still not sufficient, and improvements are being considered.
[0003] As a method for improving the impact resistance of polyamide, a method using an ethylene-α-olefin copolymer grafted with an α,β-unsaturated carboxylic acid has been proposed (Patent Document 1). However, it has been recognized that the proposed polyamide composition tends to have a decreased rigidity and fluidity when attempting to improve the impact resistance.
[0004] As a method for improving the fluidity of polyamide, a method of adding a compound having a 9,9-bisarylfluorene skeleton to a polyamide resin has been proposed (Patent Document 2). However, it was found that the proposed polyamide resin composition with improved fluidity tends to have insufficient impact strength.
[0005] Therefore, there is a demand for the development of a polyamide resin composition that has an excellent balance of impact resistance, rigidity, and flowability that are inherent to polyamide resins. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2011-207979 A [Patent Document 2] WO2016 / 139826 publication Summary of the Invention [Problem to be solved by the invention]
[0007] In view of the above circumstances, the present inventors have conducted extensive research and have found that a polyamide resin composition containing a specific polyamide resin and a specific graft-modified ethylene-α-olefin copolymer in a specific range of amounts has an excellent balance of impact resistance, rigidity and fluidity. The present invention aims to obtain a polyamide resin composition having an excellent balance of impact resistance, rigidity and fluidity. [Means for solving the problem]
[0008] Examples of aspects of the present invention are given below. [1] A polyamide resin composition comprising 85.0 to 99.9 mass% of an aliphatic long-chain polyamide (A) satisfying the following requirement (Ai), and 0.1 to 15.0 mass% of a graft-modified ethylene-α-olefin copolymer (B) satisfying the following requirements (Bi) and (B-ii) (the total of the aliphatic long-chain polyamide (A) and the graft-modified ethylene-α-olefin copolymer (B) is 100 mass%). (Ai) The relative viscosity measured in accordance with JIS K 6920-2:2009 (in 96% sulfuric acid, polymer concentration of 10 mg / ml, 25° C.) is 1.80 to 4.50. (Bi) Content of skeletal units derived from vinyl compounds having polar groups M B is 0.1 to 1.5 mass %. (B-ii) Contains 50 to 95 mol % of skeletal units derived from ethylene and 5 to 50 mol % of skeletal units derived from an α-olefin having 3 to 8 carbon atoms (however, the total of the skeletal units derived from ethylene and the skeletal units derived from an α-olefin having 3 to 8 carbon atoms is 100 mol %). [2] The polyamide resin composition according to item [1], wherein the aliphatic long-chain polyamide (A) is one or more selected from the group consisting of nylon 11, nylon 12, and nylon 6,12. [3] The polyamide resin composition according to item [1] or [2], wherein the skeletal unit derived from a vinyl compound having a polar group in the requirement (Bi) is a skeletal unit derived from maleic acid or maleic anhydride. [4] A pellet comprising the polyamide resin composition according to any one of items [1] to [3]. [5] A molded article comprising the polyamide resin composition according to any one of items [1] to [3]. Effect of the Invention
[0009] According to the present invention, a polyamide resin composition having an excellent balance of impact resistance, rigidity and flowability can be provided by adding a fixed amount of a graft-modified ethylene-α-olefin copolymer having a specific degree of modification to a polyamide having a specific viscosity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Specific embodiments of the present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified as appropriate within the scope of the object of the present invention. Herein, in this specification, the term "to" indicating a numerical range is used to mean that the numerical values before and after the range are included as the lower limit and upper limit.
[0011] In the present specification, a combination of two or more preferred embodiments is a more preferred embodiment, and unless otherwise specified, each component in the composition or each structural unit in the polymer may be contained alone or in combination with two or more types.
[0012] In this specification, the content of each component in a composition or each structural unit in a polymer means, when a plurality of substances or structural units corresponding to each structural unit in a component or polymer are present in the composition, the total content of each of the plurality of structural units present in the corresponding substance present in the composition or polymer, unless otherwise specified.
[0013] [Polyamide resin composition] The polyamide resin composition of the present invention contains 85.0 to 99.9 mass % of an aliphatic long-chain polyamide (A) described below, and 0.1 to 15.0 mass % of a graft-modified ethylene-α-olefin copolymer (B) described below (the total of the components (A) and (B) is 100 mass %).
[0014] [Aliphatic long-chain polyamide (A)] The aliphatic long-chain polyamide (A) used in the present invention satisfies the following requirements: (Ai) The relative viscosity measured in accordance with JIS K 6920-2:2009 (in 96% sulfuric acid, polymer concentration 10 mg / ml, 25° C.) is preferably 1.80 to 4.50, more preferably 1.80 to 2.50, and even more preferably 1.85 to 2.25. A viscosity of not more than the above upper limit is preferable in terms of the rigidity of the resin.
[0015] Specific examples of the aliphatic long-chain polyamide (A) include the following resins. (1) Polycondensation products of organic dicarboxylic acids having 4 to 12 carbon atoms and organic diamines having 2 to 13 carbon atoms; Examples of such polyhexamethylene adipamide [6,6 nylon] are a polycondensate of hexamethylene diamine and adipic acid, polyhexamethylene azelamide [6,9 nylon] are a polycondensate of hexamethylene diamine and azelaic acid, polyhexamethylene sebacamide [6,10 nylon] are a polycondensate of hexamethylene diamine and sebacic acid, and polyhexamethylene dodecanoamide [6,12 nylon] are a polycondensate of hexamethylene diamine and dodecanedioic acid.
[0016] Examples of the organic dicarboxylic acid include adipic acid, pimelic acid, suberic acid, sebacic acid, dodecanedioic acid, etc. Examples of the organic diamine include hexamethylenediamine, octamethylenediamine, nonanediamine, octanediamine, decanediamine, undecanediamine, undecanediamine, dodecanediamine, etc.
[0017] (2) polycondensates of ω-amino acids; For example, polyundecaneamide [nylon 11], which is a polycondensation product of ω-aminoundecanoic acid, can be mentioned. (3) Ring-opening polymers of lactams; For example, polypramide [nylon 6], which is a ring-opening polymer of ε-aminocaprolactam, and polylauric lactam [nylon 12], which is a ring-opening polymer of ε-aminolaurolactam, can be mentioned.
[0018] Among the above examples, aliphatic long-chain polyamides containing a repeating unit having 11 or 12 carbon atoms are preferred, and polyundecanoamide [nylon 11], polyhexamethylene dodecanoamide [nylon 6,12], and polylauric lactam [nylon 12] are more preferred. The raw material for the aliphatic long-chain polyamide (A) may be either fossil fuel-derived or biomass-derived. Also, the raw materials derived from fossil fuel and biomass may be used in combination.
[0019] [Graft modified ethylene-α-olefin copolymer (B)] The graft-modified ethylene / α-olefin copolymer (B) used in the present invention satisfies the following requirements (Bi) and (B-ii): (Bi) Content of skeletal units derived from vinyl compounds having polar groups M B (Hereafter, simply "denaturation amount M B ") is 0.1 to 1.5 mass%; (B-ii) 50 to 95 mol % of ethylene-derived skeletal units; 5 to 50 mol % of a backbone unit derived from an α-olefin having 3 to 8 carbon atoms; (However, the total of the skeletal units derived from ethylene and the skeletal units derived from an α-olefin having 3 to 8 carbon atoms is 100 mol %).
[0020] The content M in the requirement (Bi) B The modification amount M is 0.1 to 1.5 mass%, preferably 0.2 to 1.4 mass%, and more preferably 0.3 to 1.2 mass%. BIf the amount of modification, M, is too small, the impact resistance of the molded product may decrease. B If the amount of modification is too large, it becomes necessary to increase the amount of polar monomer or organic peroxide used during modification in a normal modification method. However, such a modification method may result in the inclusion of foreign matter such as gel in the modified polyolefin, graft-modified ethylene-α-olefin copolymer (B). B As described later, the wave number of 1780 cm assigned to the carbonyl group in FT-IR is -1 The intensity is calculated from a calibration curve prepared separately based on the peak intensity. The measurement conditions are as follows: Fourier transform infrared spectrophotometer: JASCO Corporation FT / IR-610 Number of times: 32 Disassembly: 4cm -1
[0021] In the above requirement (Bi), the polar group is preferably a carboxyl group, and the skeletal unit derived from a vinyl compound having a polar group is preferably a skeletal unit derived from maleic acid or anhydride thereof.
[0022] In the requirement (B-ii), the skeletal units derived from ethylene are 50 to 95 mol%, preferably 60 to 92 mol%, more preferably 70 to 90 mol%, even more preferably 75 to 88 mol%, and particularly preferably 80 to 88 mol%, and the skeletal units derived from an α-olefin having 3 to 8 carbon atoms are 5 to 50 mol%, preferably 8 to 40 mol%, more preferably 10 to 30 mol%, even more preferably 12 to 25 mol%, and particularly preferably 12 to 20 mol% (however, the total of the skeletal units derived from ethylene and the skeletal units derived from an α-olefin having 3 to 8 carbon atoms is 100 mol%). When each skeletal unit is within the above range, the copolymer (B) has good flexibility and is easy to handle, and further, a polyamide resin composition capable of providing a molded article having excellent impact resistance can be obtained.
[0023] Examples of the α-olefin having 3 to 8 carbon atoms include propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-heptene, 3-ethyl-1-pentene, 4,4-dimethyl-1-pentene, 4-methyl-1-hexene, 1-octene, 4,4-dimethyl-1-hexene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, and combinations thereof. Among these, propylene, 1-butene, and 1-octene are particularly preferred.
[0024] The graft-modified ethylene / α-olefin copolymer (B) used in the present invention may contain skeletal units derived from other constituent components in addition to skeletal units derived from ethylene and α-olefins having 3 to 8 carbon atoms. The content of the skeletal units derived from the other constituent components may be within a range that does not impair the effects of the present invention, and is, for example, preferably 10 mol % or less, more preferably 5 mol % or less, based on the graft-modified ethylene / α-olefin copolymer (B).
[0025] Specific examples of the other components include α-olefins having 9 or more carbon atoms, such as decene-1, undecene-1, dodecene-1, tridecene-1, tetradecene-1, pentadecene-1, hexadecene-1, heptadecene-1, octadecene-1, nonadecene-1, and eicosene-1; cyclic olefins having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms, such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, and tetracyclododecene; 1,4-hexadecene, 1,4-dimethylphenylolefins having 3 to 30 carbon atoms, preferably 3 to 20 carbon atoms, such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, and tetracyclododecene; linear non-conjugated dienes such as 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene; cyclic non-conjugated dienes such as cyclohexadiene, dicyclopentadiene, methyltetrahydroindene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and 6-chloromethyl-5-isopropenyl-2-norbornene. non-conjugated dienes such as 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,2-norbornadiene, 1,3,7-octatriene, and 1,4,9-decatriene, as well as metal salts thereof such as sodium salts; α,β-unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, methyl methacrylate, and ethyl methacrylate; vinyl esters such as vinyl acetate and vinyl propionate; and polar group-containing monomers such as unsaturated glycidyls such as glycidyl acrylate and glycidyl methacrylate; and aromatic vinyl compounds such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, methoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, p-chlorostyrene, divinylbenzene, α-methylstyrene, and allylbenzene. The monomers constituting the graft-modified ethylene-α-olefin copolymer (B), namely, ethylene, an α-olefin having 3 to 8 carbon atoms, and other constituent components, may be, for example, monomers derived from fossil fuels or monomers derived from biomass, and these monomers may be used alone or in combination of two or more kinds.
[0026] [Production method of graft-modified ethylene-α-olefin copolymer (B)] The graft-modified ethylene / α-olefin copolymer (B) used in the present invention can be obtained by graft-modifying the ethylene / α-olefin copolymer (r) with a vinyl compound having a polar group, such as maleic acid or its anhydride.
[0027] The copolymer (r) contains 50 to 95 mol % of skeletal units derived from ethylene and 5 to 50 mol % of skeletal units derived from an α-olefin having 3 to 8 carbon atoms (the total of the skeletal units derived from ethylene and the skeletal units derived from an α-olefin having 3 to 8 carbon atoms is 100 mol %).
[0028] The copolymer (r) has a melt flow rate (MFR) measured at 230°C under a load of 2.16 kg of 0.01 to 200 g / 10 min, preferably 0.1 to 100 g / 10 min, and more preferably 0.1 to 10 g / 10 min. When the MFR is within the above range, the blendability of the resulting graft-modified ethylene-α-olefin copolymer (B) with the polyamide (A) is improved. In addition, by using the ethylene-α-olefin copolymer (r) satisfying this condition, a polyamide resin composition having excellent moldability can be obtained.
[0029] The ethylene / α-olefin copolymer (r) having the above-mentioned properties can be produced by a conventional method using a vanadium catalyst consisting of a soluble vanadium compound and an alkylaluminum halide compound, or a metallocene catalyst consisting of a zirconium metallocene compound and an organoaluminum oxy compound (e.g., the metallocene catalysts described in WO97 / 10295).
[0030] The copolymer (B) is obtained by adding an additive described later to the copolymer (r) as necessary, and graft polymerizing a vinyl compound having a polar group, such as maleic acid or its anhydride, preferably in the presence of a radical initiator.
[0031] The amount of maleic acid or its anhydride charged is usually 0.010 to 15 parts by mass, preferably 0.010 to 5.0 parts by mass, based on 100 parts by mass of the ethylene-α-olefin copolymer (r). The amount of the radical initiator used is usually 0.0010 to 1.0 part by mass, preferably 0.0010 to 0.30 part by mass, based on 100 parts by mass of the ethylene-α-olefin copolymer (r).
[0032] Examples of the radical initiator that can be used include organic peroxides, azo compounds, and metal hydrides. Examples of the organic peroxides include benzoyl peroxide, dichlorobenzoyl peroxide, and dicumyl peroxide. Examples of the azo compounds include azobisisobutylnitrile and dimethylazoisobutyrate.
[0033] The radical initiator can be used by directly mixing with maleic acid or its anhydride, unmodified polyolefin and other components, or can be used after dissolving in a small amount of organic solvent. The organic solvent is not particularly limited as long as it can dissolve the radical initiator.
[0034] The graft modification with maleic acid or its anhydride can be carried out by a conventionally known method, for example, a method in which a propylene-based polyamide resin composition is dissolved in an organic solvent, and then maleic acid or its anhydride and a radical initiator are added to the solution, and the mixture is reacted at a temperature of 70 to 200°C, preferably 80 to 190°C, for 0.5 to 15 hours, preferably 1 to 10 hours.
[0035] Alternatively, a modified product can be produced by reacting maleic acid or its anhydride with the ethylene-α-olefin copolymer (r) in the presence of a radical initiator without a solvent using an extruder, etc. This reaction is usually carried out at a temperature equal to or higher than the melting point of the ethylene-α-olefin copolymer (r) for 0.5 to 10 minutes.
[0036] Examples of vinyl compounds having a polar group that can be used for modification include vinyl compounds having an oxygen-containing group such as acid, acid anhydride, ester, alcohol, epoxy, or ether; vinyl compounds having a nitrogen-containing group such as isocyanate or amide; and vinyl compounds having a silicon-containing group such as vinylsilane.
[0037] Among these, vinyl compounds having an oxygen-containing group are preferred, and specifically, unsaturated epoxy monomers, unsaturated carboxylic acids and their derivatives are preferred. Examples of unsaturated epoxy monomers include unsaturated glycidyl ethers and unsaturated glycidyl esters (e.g., glycidyl methacrylate). Examples of the unsaturated carboxylic acids include acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acid. TM (endo cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid).
[0038] In addition, examples of the derivatives of the unsaturated carboxylic acids include acid halide compounds, amide compounds, imide compounds, acid anhydrides, and ester compounds of the unsaturated carboxylic acids, etc. Specific examples include malenyl chloride, maleimide, maleic anhydride, citraconic anhydride, monomethyl maleate, dimethyl maleate, and glycidyl maleate.
[0039] Among these, unsaturated dicarboxylic acids and their acid anhydrides are more preferable, and particularly maleic acid and nadic acid. TM and acid anhydrides thereof are particularly preferred. The position at which the vinyl compound having a polar group or a derivative thereof is grafted onto the ethylene-α-olefin copolymer (r) is not particularly limited, so long as the unsaturated carboxylic acid or a derivative thereof is bonded to any carbon atom of the graft-modified ethylene-α-olefin copolymer (B) obtained by modification.
[0040] [Composition of polyamide resin composition] The polyamide resin composition of the present invention contains 85.0 to 99.9 mass% of the aliphatic long-chain polyamide (A) and 0.1 to 15.0 mass% of the graft-modified ethylene-α-olefin copolymer (B) (wherein the sum of the components (A) and (B) is 100 mass%). It preferably contains 86.0 to 98.0 mass% of the component (A) and 2.0 to 14.0 mass% of the component (B), and more preferably contains 87.0 to 96.0 mass% of the component (A) and 4.0 to 13.0 mass% of the component (B). By forming the composition in such a ratio, a molded product having an excellent balance of impact resistance, fluidity and rigidity can be provided.
[0041] [Method for preparing polyamide resin composition] The polyamide resin composition of the present invention is prepared, for example, by melt-mixing the aliphatic long-chain polyamide (A), the graft-modified ethylene-α-olefin copolymer (B), and additives to be added as required by various conventional methods. Specifically, the above components are simultaneously or sequentially charged and mixed in, for example, a Henschel mixer, a V-type blender, a tumbler mixer, a ribbon blender, or the like, and then melt-kneaded in a single-screw extruder, a multi-screw extruder, a kneader, a Banbury mixer, or the like. In particular, when a device with excellent kneading performance such as a multi-screw extruder, a kneader, or a Banbury mixer is used, a high-quality polyamide resin composition in which each component is more uniformly dispersed can be obtained. In addition, other additives, such as an antioxidant, can be added as necessary at any of these stages.
[0042] [Additives] In addition to the aliphatic long-chain polyamide (A) and the graft-modified ethylene-α-olefin copolymer (B), the polyamide resin composition of the present invention may contain, as necessary, additives such as other synthetic resins, other rubbers, antioxidants, heat stabilizers, weather stabilizers, slip agents, antiblocking agents, crystal nucleating agents, pigments, hydrochloric acid absorbers, and copper inhibitors, usually in an amount of 0.01 to 10 parts by mass, and preferably 0.1 to 5 parts by mass, per 100 parts by mass of the polyamide resin composition, within a range that does not impair the object of the present invention. These additives may be added at the stage of preparation of the polyamide resin composition, or before, during, or after preparation of the graft-modified ethylene-α-olefin copolymer (B).
[0043] [Molded body] The polyamide resin composition of the present invention can be molded into various molded articles by known molding methods such as injection molding, extrusion molding, inflation molding, blow molding, extrusion blow molding, injection blow molding, press molding, vacuum molding, calendar molding, and foam molding, and can be used for a variety of known applications.
[0044] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0045] [Aliphatic long-chain polyamide (A)] The aliphatic long-chain polyamides (A) used in the examples and comparative examples are as follows. Polyamide 12 (A-1): 12 nylon (manufactured by Ube Industries, Ltd., UBESTA (registered trademark) 3024U, melting temperature: 178°C, density (measurement method ISO 1183-3): 1020 kg / m 3 , relative viscosity (JIS K 6920-2:2009):1.99), Polyamide 12 (A-2): 12 nylon (manufactured by Ube Industries, Ltd., UBESTA (registered trademark) 3014U, melting temperature: 179°C, density (measurement method ISO 1183-3): 1020 kg / m 3 , relative viscosity (JIS K 6920-2:2009):1.68)
[0046] [Preparation of graft-modified ethylene-α-olefin copolymer (B)] Ethylene-α-olefin copolymer (r), density (ATSM D1505): 861 kg / m 3 The ethylene-1-butene copolymer (EBR) (r-1) used had a MFR (ASTM D1238, 230°C, 2.16 kg load): 0.9 g / 10 min, ethylene-derived skeleton content: 81 mol%, and 1-butene-derived skeleton content: 19 mol%.
[0047] (Method for preparing graft modified ethylene-α-olefin copolymer (B-1)) 10 kg of ethylene-1-butene copolymer (EBR) (r-1) was blended with a solution of 30 g of maleic anhydride (MAH) and 7.5 g of 2,5-dimethyl-2,5-di-(t-butylperoxy)-3-hexyne (trade name Perhexa 25B) dissolved in acetone. The resulting blend was then fed into a hopper of a screw extruder with a screw diameter of 30 mm and L / D of 40, and extruded into strands at a resin temperature of 200°C, a screw speed of 240 rpm, and a discharge rate of 12 kg / hr. The resulting strands were thoroughly cooled and then granulated to obtain ethylene-α-olefin copolymer (B-1).
[0048] (Method for preparing graft modified ethylene-α-olefin copolymer (B-2)) 10 kg of ethylene-1-butene copolymer (EBR) (r-1) was blended with a solution of 60 g of maleic anhydride (MAH) and 15 g of 2,5-dimethyl-2,5-di-(t-butylperoxy)-3-hexyne (trade name Perhexa 25B) dissolved in acetone. The resulting blend was then fed into a hopper of a screw extruder with a screw diameter of 30 mm and L / D of 40, and extruded into strands at a resin temperature of 200°C, a screw speed of 240 rpm, and a discharge rate of 12 kg / hr. The resulting strands were thoroughly cooled and then granulated to obtain ethylene-α-olefin copolymer (B-2).
[0049] (Preparation method of graft modified ethylene-α-olefin copolymer (B-3)) 10 kg of ethylene-1-butene copolymer (EBR) (r-1) was blended with a solution of 90 g of maleic anhydride (MAH) and 22.5 g of 2,5-dimethyl-2,5-di-(t-butylperoxy)-3-hexyne (trade name Perhexa 25B) dissolved in acetone. The resulting blend was then fed into a hopper of a screw extruder with a screw diameter of 30 mm and L / D of 40, and extruded into strands at a resin temperature of 200°C, a screw speed of 240 rpm, and a discharge rate of 12 kg / hr. The resulting strands were thoroughly cooled and then granulated to obtain graft-modified ethylene-α-olefin copolymer (B-3).
[0050] The methods for measuring the physical properties of the graft-modified ethylene / α-olefin copolymer (B) used in the examples and comparative examples are shown below. The results are shown in Table 1.
[0051] <mfr> The melt flow rate (MFR) was measured in accordance with ASTM D1238 at 230° C. under a load of 2.16 kg.
[0052] <density> Density (g / cm 3 ) was determined at 23°C according to ASTM D1505.
[0053] <Content of skeleton units derived from vinyl compounds having polar groups M B > Amount of modification of graft-modified ethylene-α-olefin copolymer (B) M B The wave number assigned to the carbonyl group in FT-IR is 1780 cm -1 The peak intensity was calculated from a separately prepared calibration curve. The measurement conditions were as follows: Fourier transform infrared spectrophotometer: JASCO Corporation FT / IR-610 Number of times: 32 Disassembly: 4cm -1
[0054] [Table 1]
[0055] [Example 1] A dry blend was prepared by mixing 95 parts by mass of polyamide 12 (A-1) and 5 parts by mass of graft-modified ethylene-α-olefin copolymer (B-1) using a Henschel mixer. This dry blend was then fed into a twin-screw extruder set at 245°C to prepare pellets of a polyamide resin composition. The resulting pellets of the polyamide resin composition were dried at 80°C for one day and night, and then injection molded under the following conditions to prepare test pieces for physical property tests. (Injection molding conditions) Cylinder temperature: 245℃ Injection pressure: 40MPa Mold temperature: 80℃ The physical properties of the obtained test pieces for physical property tests and the polyamide compositions were evaluated.
[0056] (1) Bending test Test specimens with a thickness of 1 / 8 inch were used, and the test was performed at a speed of 5 mm / min in accordance with ASTM D790 to measure the flexural modulus (FM; kg / cm 2 The test pieces were prepared in a dry state at 23°C for 2 days.
[0057] (2) Izod impact test Notched Izod impact strength was measured at 23° C. according to ASTM D256 using 1 / 8 inch thick test pieces. The test pieces were conditioned in a dry state at 23° C. for 2 days.
[0058] (3) Fluidity (spiral flow) The material was injection molded into a mold with a 3.8 mmφ semicircular spiral groove using an injection molding machine with a cylinder temperature of 280°C, injection pressure of 100 MPa, mold temperature of 80°C and a clamping force of 50 tonnes, and the flow distance was measured.
[0059] [Examples 2 to 4, Comparative Examples 1 to 5] Except for changing the compositions of the blending components (A) and (B) in Example 1 as shown in Table 2, the polyamide resin composition was pelletized, dried, and a test piece was prepared, and the physical properties were evaluated in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0060] [Table 2] < / mfr>
Claims
1. 85.0 to 99.9% by mass of an aliphatic long-chain polyamide (A) satisfying the following requirement (A-i); 0.1 to 15.0% by mass of a graft-modified ethylene / α-olefin copolymer (B) satisfying the following requirements (Bi) and (B-ii) (the total of the aliphatic long-chain polyamide (A) and the graft-modified ethylene / α-olefin copolymer (B) is 100% by mass); A polyamide resin composition comprising: (A-i) the relative viscosity measured in accordance with JIS K 6920-2:2009 (in 96% sulfuric acid, polymer concentration 10 mg / ml, 25°C) is 1.80 to 4.50; (Bi) Content M of skeletal units derived from vinyl compounds having polar groups B is 0.1 to 1.5% by mass based on the graft-modified ethylene / α-olefin copolymer; (B-ii) 50 to 95 mol % of ethylene-derived skeletal units; 5 to 50 mol % of a backbone unit derived from an α-olefin having 3 to 8 carbon atoms; (However, the total of the skeletal units derived from ethylene and the skeletal units derived from an α-olefin having 3 to 8 carbon atoms is 100 mol %).
2. 2. The polyamide resin composition according to claim 1, wherein the aliphatic long-chain polyamide (A) comprises at least one member selected from the group consisting of nylon 11, nylon 12 and nylon 6,12.
3. 2. The polyamide resin composition according to claim 1, wherein the skeletal unit derived from a vinyl compound having a polar group in the requirement (Bi) is a skeletal unit derived from maleic acid or maleic anhydride.
4. A pellet comprising the polyamide resin composition according to any one of claims 1 to 3.
5. A molded article comprising the polyamide resin composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Polyamide resin composition excellent in low temperature impact property, and molded article thereof
JP2011207979A
Fluidity improver and polyamide resin composition containing same
WO2016139826A1