Manufacturing method of foam-molded article

The method addresses excessive deformation in aliphatic polyester resin foam molding by using a controlled air supply and atmospheric hopper pressure, resulting in reduced deformation and environmentally friendly foam products.

JP2024134382APending Publication Date: 2024-10-03KANEKA CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044651
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Aliphatic polyester resin foam particles exhibit excessive deformation (sink marks) during molding due to the deterioration of their open cell ratio caused by strong impacts during conventional filling methods, which are not suitable for their unique physical properties.

Method used

A method involving a molding device with a hopper at atmospheric pressure, controlled filling air, and adjusted air supply is used to transport and fill aliphatic polyester resin particles, maintaining specific pressure ranges to minimize the deterioration of the open cell ratio and reduce deformation.

Benefits of technology

This approach produces aliphatic polyester resin foam molded articles with reduced deformation, contributing to environmental sustainability by using biodegradable materials and minimizing soil and ocean pollution from disposal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134382000001_ABST
    Figure 2024134382000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a foam-molded article, which can provide a foam-molded article in which deformation is prevented or reduced.SOLUTION: There is provided a manufacturing method of a foam-molded article, the method comprising a step of filling a molding space (21) in a molding die (2) with aliphatic polyester resin foam particles from a hopper (3) through a foam particle transport pipe (4) and a filling machine (1). In the filling step, a pressure inside the hopper (3) is atmospheric pressure, and filling air is supplied from a filling air supply unit (5) and regulated air is supplied from a regulated air supply unit (6).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a foamed molded article. [Background technology]

[0002] Expanded molded articles obtained by molding expanded beads of thermoplastic resins such as polystyrene-based resins and polyolefin-based resins are used in various applications such as containers, packaging materials, sanitary products, etc. As a technique for molding such expanded beads of thermoplastic resins, for example, the technique described in Patent Document 1 is known. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 11-70587 Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, from the viewpoint of reducing the environmental load, technology has been investigated for utilizing aliphatic polyester resins, which are biodegradable thermoplastic resins, in foam molding applications.

[0005] Means for Solving the Problems While conducting intensive research into foamed molded articles made from aliphatic polyester-based resins, the present inventors have newly discovered that when foamed beads made from aliphatic polyester-based resins are molded in the same manner as foamed beads made from conventional thermoplastic resins such as polystyrene-based resins or polyolefin-based resins, there is a problem in that excessive deformation (also known as "sink marks") occurs in the resulting foamed molded article.

[0006] One embodiment of the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a novel method for producing an aliphatic polyester-based resin foam molded article, which can provide an aliphatic polyester-based resin foam molded article in which deformation is prevented or reduced. [Means for solving the problem]

[0007] The present inventors conducted extensive research to solve the above problems and have now completed the present invention.

[0008] That is, one embodiment of the present invention includes the following configuration. [1] A method for producing an aliphatic polyester resin foam molded product, which comprises molding aliphatic polyester resin foam particles using a molding device, the molding device comprising: a hopper for accommodating the aliphatic polyester resin foam particles; a foam particle transport pipe having a regulated air supply unit; and a molding die having a filling machine having a filling air supply unit, the hopper and the filling machine being connected by the foam particle transport pipe, and the molding die having an internal molding space, the method for producing an aliphatic polyester resin foam molded product comprising a filling step of filling the aliphatic polyester resin foam particles from the hopper via the foam particle transport pipe and the filling machine into the molding space, the pressure in the hopper being atmospheric pressure, filling air being supplied from the filling air supply unit, and regulated air being supplied from the regulated air supply unit. [2] The method for producing an aliphatic polyester resin foam molded article according to [1], wherein in the filling step, the pressure of the filling air is 0.30 MPa (gauge pressure) or more and less than 0.68 MPa (gauge pressure). [3] The method for producing an aliphatic polyester resin foam molded body according to [1] or [2], wherein in the filling step, the pressure of the regulated air is 0.01 MPa (gauge pressure) or more and less than 0.34 MPa (gauge pressure). [4] The method for producing an aliphatic polyester resin foam molded article according to any one of [1] to [3], wherein in the filling step, a ratio of the pressure of the regulated air to the pressure of the filled air (100%) is 5% to 50%. [5] The method for producing an aliphatic polyester resin foam molded article according to any one of [1] to [4], wherein in the filling step, the internal pressure of the aliphatic polyester resin foam particles contained in the hopper is equal to or higher than atmospheric pressure and equal to or lower than 0.22 MPa (absolute pressure). [6] The method for producing an aliphatic polyester resin foamed molded article according to [5], wherein in the filling step, the internal pressure of the aliphatic polyester resin foamed particles contained in the hopper is 0.13 MPa (absolute pressure) to 0.18 MPa (absolute pressure). [7] The method for producing an aliphatic polyester resin expansion molded article according to any one of [1] to [6], wherein the expanded aliphatic polyester resin particles are expanded poly(3-hydroxyalkanoate) resin particles. Effect of the Invention

[0009] According to one embodiment of the present invention, there can be provided a novel method for producing an aliphatic polyester resin foam molded article, which can provide an aliphatic polyester resin foam molded article in which deformation is prevented or reduced. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram showing an example of a schematic configuration of a molding device used in a method for producing a foamed molded article according to one embodiment of the present invention. [Diagram 2] 1 is a schematic diagram of a foam molded article according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each configuration described below, and various modifications are possible within the scope of the claims. In addition, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. All academic documents and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more (including A and greater than A) and B or less (including B and smaller than B)".

[0012] In this specification, a repeating unit derived from an X monomer may be referred to as an “X unit.” A repeating unit may also be referred to as a structural unit.

[0013] 1. Technical Concept of One Embodiment of the Present Invention One of the processes when molding thermoplastic resin foam particles (for example, in-mold foam molding) is a filling process in which thermoplastic resin foam particles are transported and filled from a hopper through a transport piping into the molding space in the mold. Conventional methods for filling thermoplastic resin foam particles can be roughly divided into the following cracking filling method (method (1)), pressure filling method (method (2)), and compression filling method (method (3)).

[0014] Methods (1), (2), and (3) all have in common that filling air is ejected from a filling machine attached to a mold to create an air flow, and that the foamed thermoplastic resin particles are transported from a hopper to the molding space in the mold by this air flow. However, methods (1), (2), and (3) differ in the means for smoothly filling (transporting) the foamed thermoplastic resin particles into the molding space.

[0015] Method (1) is used when the air used during filling cannot be sufficiently exhausted only through vents such as core vents and core vent holes arranged in the molds (movable mold and movable mold). In method (1), when filling the mold with thermoplastic resin foamed particles, the movable mold and fixed mold are not completely closed, but a small gap (cracking) (for example, 10% of the thickness of the bottom of the molded body) is left, and the air used during filling is also exhausted through this gap between the movable mold and fixed mold.

[0016] In method (2), the thermoplastic resin foam particles to be filled are stored in a hopper in a pre-air-pressurized state, and the molding space is opened to the atmosphere with the mold closed, and the resulting pressure difference is used to fill the molding space with the thermoplastic resin foam particles.

[0017] In method (3), the thermoplastic resin foam particles to be filled are stored in a hopper that has been air-pressurized in advance, and the molding space in the mold is filled with the thermoplastic resin foam particles in a state in which the molding space in the mold is air-pressurized to a pressure equal to or lower than that of the hopper with the mold closed (a state in which molding space pressure is applied). In method (3), the pressure in the hopper and the molding space is usually controlled at a predetermined pressure (the above-mentioned molding space pressure) during filling with the thermoplastic resin foam particles.

[0018] In the in-mold expansion molding of conventional thermoplastic resin particles such as expanded polystyrene-based resin particles or expanded polyolefin-based resin particles, any of the above-mentioned filling methods (1), (2), and (3) can be adopted and are commonly used.

[0019] On the other hand, the present inventors have newly discovered that in in-mold foam molding using aliphatic polyester resin foamed particles, when conventional filling methods (method (1), method (2), and method (3)) are adopted, a new problem occurs in that the obtained foamed molded article is excessively deformed. In order to solve the above problem, the present inventors have intensively investigated the cause of deformation of the foamed molded article, and have newly discovered that the deterioration (increase) of the open cell ratio of the aliphatic polyester resin foamed particles during the transportation process from the hopper to the molding space is the cause of the excessive deformation of the obtained foamed molded article.

[0020] The reason for the deterioration of the open cell ratio of the expanded aliphatic polyester resin particles is considered to be that the expanded aliphatic polyester resin particles are more fragile than conventional thermoplastic resin particles. More specifically, in the methods (1), (2), and (3), the filling air is too strong, so that the expanded aliphatic polyester resin particles are subjected to a strong impact during transportation, and the bubbles in the outer layer of the expanded aliphatic polyester resin particles are destroyed by the impact. In addition, when the expanded aliphatic polyester resin particles are filled by the methods (2) and (3), the hopper is pressurized in advance, so that the expanded aliphatic polyester resin particles are subjected to a strong impact when the expanded particles are discharged from the hopper to the expanded particle transport pipe, and the bubbles in the outer layer of the expanded aliphatic polyester resin particles are destroyed by the impact.

[0021] The inventors of the present invention, having obtained the above knowledge, thought that if the deterioration of the open cell ratio during the transportation process of the expanded aliphatic polyester resin particles could be suppressed, it would be possible to provide an expanded aliphatic polyester resin product in which deformation is prevented or reduced. As a result of further intensive research based on the above knowledge, it was found that the deterioration of the open cell ratio of the expanded aliphatic polyester resin particles during the transportation process can be suppressed by (1) not pressurizing the hopper in the filling process (the pressure inside the hopper is atmospheric pressure), (2) supplying an appropriate amount of filling air, and further (3) supplying additional air (adjusted air) into the transportation pipe, and as a result, it is possible to provide an expanded aliphatic polyester resin product in which deformation is prevented or reduced, and thus the present invention was completed.

[0022] One embodiment of the present invention was designed in consideration of the unique physical properties of the expanded aliphatic polyester resin particles discovered by the present inventors and the new problems caused by said physical properties. Therefore, it cannot be easily understood from the conventional techniques that are based on molding conventional thermoplastic resin particles that do not have such physical properties, and it can be said to be a novel method that differs in technical concept from the conventional techniques.

[0023] 2. Method for producing foamed molded product A method for producing a foamed molded body according to one embodiment of the present invention is a method for producing a foamed molded body of an aliphatic polyester resin, which comprises molding aliphatic polyester resin foamed particles using a molding apparatus, the molding apparatus comprising a hopper for accommodating the aliphatic polyester resin foamed particles, a foamed particle transport pipe having an adjusted air supply unit, and a molding die having a filling machine having a filling air supply unit, the hopper and the filling machine being connected by the foamed particle transport pipe, and the molding die having a molding space therein, the method for producing aliphatic polyester resin foamed molded bodies comprising a filling step of filling the aliphatic polyester resin foamed particles from the hopper via the foamed particle transport pipe and the filling machine into the molding space, the pressure in the hopper being atmospheric pressure, filling air being supplied from the filling air supply unit, and adjusted air being supplied from the adjusted air supply unit.

[0024] In this specification, the "manufacturing method for a foam molded article according to one embodiment of the present invention" may be referred to as "the present manufacturing method," and the "aliphatic polyester resin expanded particles" may be referred to as "expanded particles." The foam molded article obtained by the present manufacturing method may also be referred to as an "aliphatic polyester resin foam molded article."

[0025] Since the present production method has the above-mentioned configuration, it has an advantage that it can provide an aliphatic polyester resin foam molded article in which deformation is prevented or reduced.

[0026] In addition, because this manufacturing method uses aliphatic polyester resin, which is a biodegradable resin, the resulting foamed molded products can prevent soil and / or marine pollution due to disposal. This is expected to contribute to the achievement of the Sustainable Development Goals (SDGs), such as Goal 12 "Ensure sustainable consumption and production patterns" and / or Goal 14 "Conserve and sustainably use the oceans and marine resources for sustainable development."

[0027] First, the materials (raw materials) used in this production method will be described.

[0028] <Expanded particles> The expanded beads used in this manufacturing method are obtained by expanding aliphatic polyester resin particles obtained by using an aliphatic polyester resin. Further, the expanded molded article is obtained by molding the expanded beads (for example, in-mold expansion molding). It can also be said that the expanded beads are obtained by expanding aliphatic polyester resin particles containing an aliphatic polyester resin.

[0029] Specifically, the aliphatic polyester resin particles that are the raw material for the expanded beads can be obtained, for example, by the following method: (1) Mixing an aliphatic polyester resin, a bubble adjuster such as talc, and other additives such as a fatty acid amide to obtain a mixture; (2) The resulting mixture is melt-kneaded while being heated, for example, using an extruder, to obtain a molten resin composition; (3) The resulting resin composition is cooled with water and then cut to obtain aliphatic polyester resin particles.

[0030] Specifically, the expanded aliphatic polyester resin particles can be obtained by expanding aliphatic polyester resin particles by, for example, the following method: (1) A dispersion medium such as water, aliphatic polyester resin particles, and, if necessary, a crosslinker such as 1,1-di(t-butylperoxy)cyclohexane (TBCH), a dispersant such as calcium phosphate tribasic, and a dispersion aid such as sodium alkanesulfonate are mixed in a container; (2) While stirring the obtained mixture with a stirrer or the like, a blowing agent such as carbon dioxide, ethanol, mixed butane (e.g., a mixture of normal butane and isobutane) is added to the container to prepare a dispersion; (3) heating the dispersion to a foaming temperature, and if necessary, increasing the pressure in the vessel to a foaming pressure; (4) The temperature and pressure in the container are maintained at approximately the foaming temperature and foaming pressure, respectively, for a certain period of time; (5) Next, the dispersion liquid in the vessel is released under atmospheric pressure to obtain expanded particles. Here, the dispersion liquid (mixture) in the container is stirred, for example, with a stirrer, from the step (2) to the step (5) where the dispersion liquid is completely discharged. The steps (1) and (2) may be collectively referred to as the "dispersion step."

[0031] The expanded beads thus obtained may be washed with an aqueous solution of sodium hexametaphosphate or the like, if necessary.

[0032] Alternatively, the aliphatic polyester resin particles described above may be impregnated with a foaming gas (foaming agent) in a pressure-resistant container, and then the aliphatic polyester resin particles containing the foaming agent are placed in a foaming machine and foamed with water vapor or the like to obtain foamed particles.

[0033] The shape of the expanded beads is not particularly limited, but may be, for example, spherical or approximately spherical.

[0034] (Aliphatic polyester resin) As described above, the expanded beads are obtained by expanding aliphatic polyester resin particles containing an aliphatic polyester resin. In other words, the expanded aliphatic polyester resin beads contain an aliphatic polyester resin as a resin component. In this specification, the "resin component" in the expanded beads means the resin component that substantially constitutes the expanded beads, excluding the blowing agent, the cell regulator, and other additives, among the components contained in the expanded beads.

[0035] The resin component of the expanded beads contains, for example, more than 50% by weight of the aliphatic polyester resin in 100% by weight of the resin component, more preferably 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, even more preferably 95% by weight or more, and particularly preferably 100% by weight. In other words, it is particularly preferable that the resin component of the expanded aliphatic polyester resin beads is composed only of an aliphatic polyester resin. The higher the content of the aliphatic polyester resin in the resin component of the expanded beads, the more advantageously soil pollution caused by disposal of the resulting expanded molded article can be suppressed. The advantage is that.

[0036] Examples of the aliphatic polyester resin include one or more selected from the group consisting of poly(3-hydroxyalkanoate) resins, polylactic acid, polyethylene succinate, polybutylene succinate, polyethylene adipate, polybutylene adipate, polyhexamethylene adipate polyethylene succinate adipate, polybutylene succinate adipate, polyethylene adipate terephthalate, polybutylene adipate terephthalate, polyethylene succinate terephthalate, polybutylene succinate terephthalate, polyethylene oxalate, polybutylene oxalate, polyneopentyl oxalate, polyethylene sebacate, polybutylene sebacate, polyhexamethylene sebacate, and polycaprolactone.

[0037] Among the aliphatic polyester resins, poly(3-hydroxyalkanoate) resins having marine decomposition as well as soil decomposition are preferred. In other words, the resin component of the expanded beads preferably contains poly(3-hydroxyalkanoate) resin.

[0038] The resin component of the expanded beads preferably contains more than 50% by weight of poly(3-hydroxyalkanoate) resin in 100% by weight of the resin component. In this specification, expanded beads containing more than 50% by weight of "X" resin in 100% by weight of the resin component may be referred to as X resin expanded beads. For example, expanded beads containing more than 50% by weight of poly(3-hydroxyalkanoate) resin in 100% by weight of the resin component are also referred to as poly(3-hydroxyalkanoate) resin expanded beads. The aliphatic polyester resin expanded beads are preferably poly(3-hydroxyalkanoate) resin expanded beads. This configuration has the advantage of being able to suppress (reduce) soil pollution and marine pollution caused by the disposal of foamed molded bodies.

[0039] The resin component of the expanded beads preferably contains 60% by weight or more of poly(3-hydroxyalkanoate)-based resin, more preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, even more preferably 95% by weight or more, and particularly preferably 100% by weight. In other words, it is particularly preferable that the resin component of the expanded beads is composed only of poly(3-hydroxyalkanoate)-based resin. The higher the content of poly(3-hydroxyalkanoate)-based resin in the resin component of the expanded aliphatic polyester resin beads, the more advantageous it is that soil pollution and / or marine pollution due to disposal of the resulting expanded molded article can be suppressed.

[0040] (Poly(3-hydroxyalkanoate) resin) In this specification, the "poly(3-hydroxyalkanoate)-based resin" may be referred to as "poly(3-hydroxyalkanoate)" or "P3HA." P3HA will be described below.

[0041] P3HA is a polymer having a 3-hydroxyalkanoate unit as an essential constituent unit (monomer unit). In this specification, "3-hydroxyalkanoate" may also be referred to as "3HA". Specifically, P3HA is preferably a polymer containing a repeating unit represented by the following general formula (1): [-CHR-CH2-CO-O-] (1). In the general formula (1), R is C n H 2n+1 where n is an integer of 1 to 15. Examples of R include linear or branched alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, t-butyl, pentyl, and hexyl. n is preferably 1 to 10, and more preferably 1 to 8.

[0042] As P3HA, P3HA produced from a microorganism is particularly preferred. P3HA produced from a microorganism is poly[(R)-3HA] in which all three HA units are (R)-3HA.

[0043] P3HA preferably contains 3HA units (particularly repeating units of general formula (1)) in an amount of 50 mol% or more, more preferably 70 mol% or more, and even more preferably 80 mol% or more, of the total repeating units of P3HA (100 mol%). The repeating units (monomer units) may be 3HA units only, or may contain, in addition to 3HA units, repeating units derived from monomers other than 3HA (e.g., 4-hydroxyalkanoate units, etc.).

[0044] Specific examples of the 3HA unit include a 3-hydroxybutyrate unit, a 3-hydroxyvalerate unit, and a 3-hydroxyhexanoate unit. The melting point and tensile strength of 3-hydroxybutyrate are close to those of propylene. Therefore, it is preferable that the P3HA according to one embodiment of the present invention contains a 3-hydroxybutyrate unit. In this specification, "3-hydroxybutyrate" may also be referred to as "3HB".

[0045] P3HA preferably contains 3HB units (monomer units) in an amount of 80 mol% or more, more preferably 85 mol% or more, of the total repeating units of P3HA (100 mol%). As P3HA, a polymer containing 3HB units, all of which are (R)-3HB (a polymer produced by a microorganism) is particularly preferred.

[0046] When P3HA contains two or more repeating units, the monomer from which the repeating units other than the repeating unit with the largest content are derived is referred to as a comonomer. In this specification, a "repeating unit derived from a comonomer" may also be referred to as a "comonomer unit."

[0047] The comonomer is not particularly limited, but is preferably 3-hydroxyhexanoate (hereinafter sometimes referred to as 3HH) or 4-hydroxybutyrate (hereinafter sometimes referred to as 4HB).

[0048] Specific examples of P3HA include poly(3-hydroxybutyrate), poly(3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate) (hereinafter sometimes referred to as "P3HB3HV"), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-3-hydroxyhexanoate), and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (hereinafter sometimes referred to as "P3HB3HH"). ), poly(3-hydroxybutyrate-co-3-hydroxyheptanoate), poly(3-hydroxybutyrate-co-3-hydroxyoctanoate), poly(3-hydroxybutyrate-co-3-hydroxynonanoate), poly(3-hydroxybutyrate-co-3-hydroxydecanoate), poly(3-hydroxybutyrate-co-3-hydroxyundecanoate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (hereinafter, sometimes referred to as "P3HB4HB"). In particular, from the viewpoints of processability and the physical properties of the foamed molded product, poly(3-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxyvalerate-co-3-hydroxyhexanoate), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) or poly(3-hydroxybutyrate-co-4-hydroxybutyrate) are preferred. In one embodiment of the present invention, the above-mentioned P3HA may be used alone or in combination of two or more.

[0049] It is noted that "-co-X" is intended to include X units as comonomer units.

[0050] It is preferable that P3HA has a 3HB unit as an essential repeating unit (structural unit) and also has a comonomer unit. That is, it is preferable that P3HA is a copolymer having a 3HB unit and a comonomer unit. The case where P3HA has a 3HB unit and a comonomer unit will be described. In this case, the ratio of the 3HB unit and the comonomer unit (3HB unit / comonomer unit) in 100 mol% of all repeating units in P3HA is preferably 99 / 1 (mol% / mol%) to 80 / 20 (mol% / mol%), more preferably 97 / 3 (mol% / mol%) to 80 / 20 (mol% / mol%), and further preferably 95 / 5 (mol% / mol%) to 85 / 15 (mol% / mol%). If the ratio of the comonomer unit in 100 mol% of all repeating units of P3HA is 1 mol% or more, the melt-kneadable temperature range and the thermal decomposition temperature range of P3HA are sufficiently separated, so that the obtained expanded beads have excellent processability. On the other hand, if the ratio of the comonomer units to the total repeating units of P3HA (100 mol%) is 20 mol% or less, the P3HA composition crystallizes quickly during melt kneading, and the productivity is high. P3HA having such a ratio of each monomer unit can be prepared according to a method known to those skilled in the art, for example, the method described in International Publication WO2009 / 145164.

[0051] The ratio of each monomer unit in P3HA can be determined by a method known to those skilled in the art, for example, the method described in WO 2013 / 147139.

[0052] In one embodiment of the present invention, the method for producing P3HA is not particularly limited, and may be a production method by chemical synthesis or a production method using a microorganism. Among them, a production method using a microorganism is preferable. A known method can be applied to the production method of P3HA using a microorganism.

[0053] Specific examples of bacteria that produce copolymers of 3HB and other hydroxyalkanoates include Aeromonas caviae, which produces P3HB3HV and P3HB3HH, and Alcaligenes eutrophus, which produces P3HB4HB. In particular, Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, p4821-4830 (1997)) and the like, which have improved productivity of P3HB3HH by introducing genes of P3HA synthase group, are more preferred. In the method for producing P3HA, microbial cells in which P3HB3HH is accumulated in the cells by culturing microorganisms such as Alcaligenes eutrophus AC32 under appropriate conditions are preferably used. In addition, in addition to the above, genetically modified microorganisms into which various P3HA synthesis-related genes have been introduced may be used as copolymer-producing bacteria according to the P3HA to be produced. In addition, various culture conditions for the microorganisms (bacteria), including the type of substrate, may be optimized according to the P3HA to be produced.

[0054] In one embodiment of the present invention, the method for culturing a microorganism that produces P3HA is not particularly limited, and for example, the method described in International Publication No. WO2019 / 142717 can be used.

[0055] The resin component of the expanded beads may contain a resin other than the aliphatic polyester resin, such as polypropylene, polyethylene, polystyrene, modified starch, or modified cellulose.

[0056] In addition to the resin component containing the aliphatic polyester resin, the expanded particles may contain additives, crystal nucleating agents, cell regulators, crosslinking agents, crosslinking aids, foaming agents, dispersants, dispersion aids, etc. that may be used during the production of the aliphatic polyester resin particles and / or expanded particles. The expanded particles may contain other components that can be used in addition to these to the extent that the effects of one embodiment of the present invention are not impaired. Examples of other components include colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, plasticizers, antioxidants, antioxidants, weather resistance improvers, ultraviolet absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, and sliding improvers. Only one type of other component may be contained, or two or more types may be contained. The content of these other components can be appropriately set by those skilled in the art depending on the purpose of use. As an example, the types and amounts of such additives, foam regulators, crosslinking agents, crosslinking assistants, foaming agents, dispersants, dispersion assistants, and other components may be used. The types and amounts of such additives disclosed in WO 2021 / 002092 can be used.

[0057] As the crosslinking agent, for example, an organic peroxide is preferable. By using a crosslinking agent in the manufacturing process of the aliphatic polyester resin particles and / or the expanded beads, crosslinked expanded beads can be obtained. In other words, it is preferable that the expanded aliphatic polyester resin particles are crosslinked by an organic peroxide.

[0058] The organic peroxide used as the crosslinking agent depends on the type of aliphatic polyester resin used, but is preferably an organic peroxide having a one-hour half-life temperature of 90°C to 160°C, more preferably an organic peroxide having a one-hour half-life temperature of 110°C to 160°C, even more preferably an organic peroxide having a one-hour half-life temperature of 110°C to 125°C, and particularly preferably an organic peroxide having a one-hour half-life temperature of 114°C to 124°C. Specific examples of such organic peroxides include benzoyl peroxide (BPO, one-hour half-life temperature: 92°C), t-butylperoxy-2-ethylhexyl carbonate (TBEC, one-hour half-life temperature: 121°C), and 1,1-di(t-butylperoxy)cyclohexane (TBCH, one-hour half-life temperature: 116°C). When an organic peroxide having a one-hour half-life temperature of 90°C or more is used, there is an advantage that expanded particles having a desired gel fraction tend to be obtained. On the other hand, when an organic peroxide having a one-hour half-life temperature of 160° C. or less is used, it has the advantage that unreacted crosslinking agent is less likely to remain in the final product.

[0059] When a crosslinking agent is used, the amount of the crosslinking agent is not particularly limited. The amount of the crosslinking agent may be appropriately set according to the desired degree of crosslinking and the closed cell ratio in the resulting expanded beads. In addition, the amount of the crosslinking agent is positively correlated with the gel fraction of the expanded beads, and greatly affects the value of the gel fraction of the expanded beads. Therefore, it is also desirable to strictly set the amount of the crosslinking agent in consideration of the gel fraction of the resulting expanded beads.

[0060] The gel fraction of the expanded beads is preferably 30% by weight to 95% by weight, more preferably 50% by weight to 90% by weight, and even more preferably 60% by weight to 85% by weight, based on 100% by weight of the expanded beads. When the gel fraction of the expanded beads is (a) 30% by weight or more based on 100% by weight of the expanded beads, there is an advantage that the molding temperature range of the expanded beads capable of providing a good quality expanded molded article is widened and productivity is improved, and when it is (b) 95% by weight or less, there is an advantage that an expanded molded article having excellent internal fusion property can be easily obtained at a low molding pressure.

[0061] Each step that may be included in this production method will be described in detail below.

[0062] <Method of manufacturing foamed molded product> (filling process) First, a molding apparatus used in the filling step included in the present manufacturing method will be described below with reference to Fig. 1. Fig. 1 is a schematic diagram showing an example of the schematic configuration of a molding apparatus 100 used in one embodiment of the present invention.

[0063] 1, the molding apparatus 100 has at least a hopper 3 for accommodating expanded aliphatic polyester resin beads, an expanded bead transport pipe 4 equipped with a regulated air supply unit 6, and a molding die 2 equipped with a filling machine 1 equipped with a filling air supply unit 5. The arrow indicates the transport direction (movement direction) of the expanded beads.

[0064] In the molding apparatus 100, the hopper 3 and the filling machine 1 are connected by an expanded bead transport pipe 4. The molding apparatus 100 is configured such that the expanded beads contained in the hopper 3 pass through the expanded bead transport pipe 4 and the filling machine 1 in this order and are supplied into the molding die 2.

[0065] Although not shown in the figure, the filling machine 1 is equipped with a filling air supply unit 5 that supplies filling air to the filling machine 1, a piston whose tip is adapted to close the foamed bead inlet of the molding die 2, and an inlet that introduces the foamed beads supplied from the foamed bead transport piping 4 into the filling machine 1.

[0066] The molding die 2 includes a fixed die and a movable die, and is configured such that, as the movable die moves toward the fixed die, the molding die 2 is closed to form a molding space 21 consisting of the fixed die and the movable die. In other words, the molding die 2 has a molding space 21 consisting of the fixed die and the movable die.

[0067] Although not shown, the hopper 3 is provided with an expanded bead outlet for supplying the expanded beads contained in the hopper 3 to the expanded bead transport pipe 4, and is connected to the expanded bead transport pipe 4 via the expanded bead outlet. In addition, the expanded bead outlet may be provided with a shutter that allows the opening and closing of the expanded bead outlet to be controlled.

[0068] The filling air supply unit 5 and the regulated air supply unit 6 have at least an air generator (filling air generator 52 and regulated air generator 62) and an air supply pipe (filling air supply pipe 51 and regulated air supply pipe 61), and the filling air supply pipe 51 and the regulated air supply pipe 61 have air outlets at their openings. The filling air supply unit 5 and the regulated air supply unit 6 supply air (filling air or regulated air) generated by the air generator through the air supply pipe to the filling machine 1 and the expanded particle transport pipe 4, respectively, from the air outlet. The air outlet opens toward the molding die 2, and the supplied air is ejected toward the molding die 2 to form an air flow in the transport direction of the expanded particles. The molding device 100 is configured to supply the expanded particles supplied from the hopper 3 into the expanded particle transport pipe 4 on the air flow into the molding die 2 via the expanded particle transport pipe 4 and the filling machine 1.

[0069] 1 shows an example in which molding apparatus 100 has one each of filling machine 1, filled air supply unit 5, and conditioned air supply unit 6, but molding apparatus 100 may have two or more filling machines 1, filled air supply units 5, and / or conditioned air supply units 6. Also, in FIG. 1, an example in which molding apparatus 100 has individual filled air generator 52 and conditioned air generator 62 is shown, but in molding apparatus 100, one air generator may be used in common (shared) as filled air generator 52 and conditioned air generator 62. Such an example is also included in one embodiment of the present invention.

[0070] The filling step of this production method is a step of filling the expanded beads contained in the hopper 3 into the molding space 21 of the molding die 2 via the expanded bead transport pipe 4 and the filling machine 1.

[0071] In the filling step, the pressure in the hopper 3 is atmospheric pressure. In this specification, "the pressure in the hopper is atmospheric pressure" means that the pressure in the hopper 3 is not manipulated (particularly, not pressurized). "The pressure in the hopper is atmospheric pressure" can also be rephrased as "the inside of the hopper is under atmospheric pressure." In the filling step, by the pressure in the hopper 3 being atmospheric pressure, rapid deformation (particularly, expansion) due to the pressure difference between the inside of the hopper 3 and the inside of the expanded particle transport pipe 4 when the expanded particles are supplied from the hopper 3 to the expanded particle transport pipe 4 can be prevented or reduced, and the formation of open cells in the foamed particles can be prevented or reduced. As a result, an aliphatic polyester resin foam molded article in which deformation is prevented or reduced can be provided.

[0072] In the filling step, the manner in which the filling air and the supply air are supplied (the timing of supply) when the expanded beads are supplied from the hopper 3 into the expanded beads transport pipe 4 is not particularly limited, but may be, for example, the following manner: (1) Open the shutter of the hopper 3, and supply the foamed particles from the hopper 3 into the foamed particle transport pipe 4. At the same time, supply the filling air from the filling air supply unit 5 and supply the conditioned air from the conditioned air supply unit 6; (2) Before supplying the foamed particles into the foamed particle transport pipe 4, the supply of the filling air from the filling air supply unit 5 and the supply of the conditioned air from the conditioned air supply unit 6 are started in advance, and then the shutter of the hopper 3 is opened to supply the foamed particles from the hopper 3 into the foamed particle transport pipe 4; or (3) Before supplying the foamed beads into the foamed bead transport pipe 4, the filling air from the filling air supply unit 5, which has already been started to be supplied, and the conditioned air from the conditioned air supply unit 6 are blown back into the hopper 3 by opening the shutter of the hopper 3, and then the foamed beads are supplied from the hopper 3 into the foamed bead transport pipe 4.

[0073] In the filling step, the pressure of the filling air supplied from the filling air supply unit 5 is preferably 0.10 MPa (gauge pressure) to 1.00 MPa (gauge pressure), preferably 0.15 MPa (gauge pressure) to 0.90 MPa (gauge pressure), particularly preferably 0.3 MPa (gauge pressure) or more and less than 0.68 MPa (gauge pressure), and may be 0.40 MPa (gauge pressure) to 0.60 MPa (gauge pressure). By setting the pressure of the filling air in the above range, the foamed particles can be efficiently filled. In particular, by setting the pressure of the filling air to 0.3 MPa (gauge pressure) or more and less than 0.68 MPa (gauge pressure), the foamed particles can be efficiently filled, and the air flow formed by the filling air can be prevented from becoming excessively strong, and the foamed particles can be subjected to a strong impact due to the strong air flow, which can cause the foamed particles to be damaged (particularly, the bubbles in the outer layer of the foamed particles to become open). As a result, an aliphatic polyester resin foamed molded product having excellent surface properties and in which deformation is prevented or reduced can be provided.

[0074] In the filling step, the pressure of the conditioned air supplied from the conditioned air supply unit 6 is preferably 0.01 MPa (gauge pressure) to 0.50 MPa (gauge pressure), more preferably 0.01 MPa (gauge pressure) to 0.45 MPa (gauge pressure), particularly preferably 0.01 MPa (gauge pressure) or more and less than 0.34 MPa (gauge pressure), and may be 0.02 MPa (gauge pressure) to 0.30 MPa (gauge pressure). By setting the pressure of the conditioned air in the above range, the foamed particles can be efficiently filled. In particular, by setting the pressure of the conditioned air to 0.01 MPa (gauge pressure) or more and less than 0.34 MPa (gauge pressure), it is possible to prevent the air flow formed by the conditioned air from becoming excessively strong and the foamed particles from being subjected to a strong impact due to the strong air flow, which causes the foamed particles to be damaged (particularly, the bubbles in the outer layer of the foamed particles to become open). As a result, it is possible to provide an aliphatic polyester resin foamed molded product having excellent surface properties and further suppressed deformation.

[0075] In the filling step, the ratio of the pressure of the regulated air to the pressure of the filling air (regulated air pressure ratio) is preferably 1.0% to 70.0%, more preferably 3.0% to 55.0%, and particularly preferably 5.0% to 50.0%. By setting the regulated air pressure ratio within the above range, it is possible to provide an aliphatic polyester resin foam molded product that has excellent surface properties and is further prevented or reduced in deformation.

[0076] In the filling step, the expanded beads contained in the hopper 3 may be unpressurized (internal pressure equal to atmospheric pressure), or may be pressurized before being contained and given a predetermined internal pressure higher than atmospheric pressure. The internal pressure of the expanded beads contained in the hopper 3 is preferably atmospheric pressure or more and 0.22 MPa (absolute pressure) or less, more preferably above atmospheric pressure (over 0.10 MPa (absolute pressure)) and 0.22 MPa (absolute pressure), even more preferably 0.13 MPa (absolute pressure) to 0.18 MPa (absolute pressure), and even more preferably 0.14 MPa (absolute pressure) to 0.17 MPa (absolute pressure). By setting the internal pressure of the expanded beads in the above range, particularly 0.13 MPa (absolute pressure) to 0.18 MPa (absolute pressure), it is possible to provide a foamed molded product having excellent surface properties and internal fusion rate. In addition, as a method for applying internal pressure to the expanded beads, a known method can be adopted, for example, the method disclosed in JP-A-7-178747 or JP-A-2022-104389 can be adopted.

[0077] In the filling step, as described above, the movable die and the fixed die of the molding die 2 are closed to form the molding space 21. When closing the mold, a gap (cracking) large enough to prevent the filled foamed particles from leaking may be intentionally left, and the mold may be completely closed after the foamed particles are filled. By filling the molding space 21 with foamed particles in this state of cracking, the filling air and the adjustment air used during filling can be discharged from the cracking while the filling step is performed. This allows an air flow to be formed more efficiently in the transport direction of the foamed particles, and the foamed particles can be efficiently filled into the molding space 21. When the filling step is performed in a state of cracking, the amount of cracking is preferably 1% to 30% of the foamed molded body dimension in the mold opening (mold closing) direction of the foamed molded body to be foam-molded in the mold, and more preferably 2% to 25%. In particular, from the viewpoint of providing a foamed molded body with better surface properties, when non-pressurized (internal pressure is the same as atmospheric pressure) foamed particles are used for filling, it is preferable to perform the filling step with the above amount of cracking.

[0078] (Heating process) The present manufacturing method may include a heating step in which the expanded beads filled in the molding die 2 by the filling step are heated with steam to form the expanded beads. The heating step can also be said to be a step of heat-molding the expanded beads. The heat-molding method of the expanded beads in the heating step is conventionally known, and for example, one or more methods selected from one-sided heating, reverse one-sided heating, and double-sided heating can be applied. In the heating step, the molding die 2 may be preheated as desired before one-sided heating, reverse one-sided heating, and / or double-sided heating. As a more specific heat-molding method of the expanded beads, for example, the methods disclosed in JP-A-2012-233182 or JP-A-2022-050566 can be adopted.

[0079] Heating conditions such as steam pressure and heating time in various heating processes performed in the heating step can be appropriately determined. For example, the steam pressure during preheating may be 0.01 to 0.30 MPa (gauge pressure), and the heating time may be 1 to 30 seconds. The steam pressure during one-sided heating may be 0.01 to 0.30 MPa (gauge pressure), and the heating time may be 1 to 30 seconds. The steam pressure during reverse one-sided heating may be 0.01 to 0.30 MPa (gauge pressure), and the heating time may be 1 to 30 seconds. The steam pressure during double-sided heating may be 0.01 to 0.30 MPa (gauge pressure), and the heating time may be 1 to 30 seconds.

[0080] In this production method, the open cell ratio (also referred to as open cell ratio) of the expanded beads (before filling) to be subjected to the filling step is preferably 7.0% or less, more preferably 6.5% or less, even more preferably 6.0% or less, even more preferably 5.5% or less, and particularly preferably 5.0% or less. By using expanded beads having an open cell ratio before filling within the above range in the filling step, it is possible to provide a foamed molded product in which deformation is further suppressed. The lower the open cell ratio of the expanded beads before filling, the more preferable it is, and it may be 0%. The open cell ratio of the expanded beads can be measured by the method described in the Examples.

[0081] As described above, an excessive increase in the open cell ratio of the expanded beads in the filling step, in other words, the use of expanded beads with an excessively high open cell ratio after filling for molding, can cause excessive deformation in the resulting expanded molded article. Therefore, from the viewpoint of providing an expanded molded article with less deformation, the open cell ratio of the expanded beads (in the mold) after filling is preferably 7.5% or less, more preferably 7.0% or less, even more preferably 6.5% or less, even more preferably 6.0% or less, and particularly preferably 5.5% or less.

[0082] (Other processes) In addition to the above-mentioned filling step and heating step, the present manufacturing method may include other steps such as a heat-retaining step (steaming step), a cooling step, and a removal step. The conditions for carrying out these other steps can be appropriately determined. For example, the temperature of the water sprayed in the cooling step may be 1 to 60°C, and the cooling time may be 1 to 500 seconds.

[0083] 3. Foam Molded Articles According to this manufacturing method, a foam molded product (hereinafter referred to as "the foam molded product") made from an aliphatic polyester resin can be obtained. Since the foam molded product is manufactured by this manufacturing method, it is a foam molded product with suppressed deformation. The deformation amount of the foam molded product can be evaluated by the method described in the examples below.

[0084] From the viewpoint of impact resistance, the internal fusion ratio of the present foamed molded product is preferably 60% or more, more preferably 65% ​​or more, even more preferably 70% or more, even more preferably 75% or more, and most preferably 80%. The internal fusion ratio of the foamed molded product can be measured by the method described in the Examples.

[0085] The foamed molded article can be suitably used, for example, as a packaging cushioning material (e.g., packaging cushioning materials for home appliances such as refrigerators, freezers, air conditioner bodies and their outdoor units, washing machines, air purifiers, humidifiers, rice cookers, microwave ovens, ovens, toasters, electric fans, and storage battery units, and packaging cushioning materials for automobile items such as transmissions, roofs, hoods, doors, batteries, and engines), logistics materials (e.g., agricultural product boxes, fish boxes, etc.), insulation materials, civil engineering and construction components, and automobile components (e.g., tool boxes, bulkheads, core materials for seats, core materials for bumpers, tibia pads, door trims, etc.). EXAMPLES

[0086] The present invention will be specifically described below with reference to examples, but the technical scope of the present invention is not limited to these examples.

[0087] 〔material〕 The substances used in the examples and comparative examples are shown below.

[0088] (Aliphatic polyester resin) The polymer was composed of P3HA:P3HB3HH (monomer ratio: 3HB / 3HH=95 / 5 (mol % / mol %), melting point 145° C.), and was prepared in accordance with the method described in paragraphs

[0064] to

[0125] of International Publication WO2009 / 145164.

[0089] (Crystal nucleating agent) Pentaerythritol (Neuraizer P: Mitsubishi Chemical Corporation) (lubricant) Behenamide (Tokyo Chemical Industry Co., Ltd.) Erucamide (Tokyo Chemical Industry Co., Ltd.) (Foam regulator) Talc (Talc Powder PKS manufactured by Hayashi Kasei Co., Ltd.) (Crosslinking agent (organic peroxide)) 1,1-Di(t-butylperoxy)cyclohexane (TBCH: NOF Corporation) (foaming agent) Carbon dioxide (manufactured by Air Water Inc.) (Dispersant) Tricalcium phosphate (manufactured by Taihei Chemical Industry Co., Ltd., specific gravity 3.1, pH 6) (Dispersion aid) Sodium alkanesulfonate (Latemul PS manufactured by Kao Corporation).

[0090] (Cleaning agent) Sodium hexametaphosphate (manufactured by Taihei Chemical Industry Co., Ltd.).

[0091] [Measurement and evaluation methods] The measurement and evaluation methods carried out in the examples and comparative examples will be described below.

[0092] (Measurement of gel fraction of expanded beads) The gel fraction of the expanded beads was measured by the following methods (1) to (5): (1) 1 g of expanded beads and 100 ml of chloroform were placed in a 150 ml flask; (2) the mixture in the flask was heated under reflux at atmospheric pressure at 62°C for 8 hours; (3) the obtained heat-treated product was filtered using a suction filtration device equipped with a 100-mesh wire screen; (4) the filtered product on the wire screen was dried in an oven at 80°C under vacuum conditions for 8 hours, and the weight of the dried product Wg (g) was measured; (5) the gel fraction was calculated by the following formula: gel fraction (wt%) = Wg / 1 × 100.

[0093] (Measurement of apparent density of expanded beads) The method for measuring the density of the foamed particles was as follows (1) to (3): (1) A measuring cylinder containing ethanol was prepared, and foamed particles with a weight Wd (g) were submerged in the ethanol; (2) The volume of the foamed particles read from the rise in the water level of the ethanol (submersion method) was defined as Vd (cm 3 (3) The apparent density of the expanded beads was calculated by the following formula (1). Apparent density of foam particles (g / cm 3 ) = Wd / Vd (1) (Measurement of internal pressure of foam beads) The measurement method of the internal pressure of the expanded beads was as follows (1) to (5): (1) the weight W1 (g) of the expanded beads after the internal pressure was applied was measured; (2) the expanded beads were heated at 150°C for 30 minutes to dissipate the inorganic gas in the expanded beads; (3) the weight W2 (g) of the expanded beads from which the inorganic gas had dissipated was measured again; (4) the weight of the inorganic gas (ΔW) was calculated from the difference in weight (W1-W2) of the expanded beads before and after the inorganic gas had dissipated; (5) the internal pressure P (MPa (absolute pressure)) of the expanded beads was calculated from the equation of state of an ideal gas (specifically, the following formula): Internal pressure of foam particles P (MPa (absolute pressure)) = (1 + (ΔW / 28.8) x 0.082 x (273 + T) x (ρ x 1000 / W2)) / 9.87 In the above formula, T is the temperature (room temperature) when the weight of the expanded beads after the application of internal pressure is measured, and ρ is the apparent density (g / cc) of the expanded beads after the application of internal pressure (expanded beads having weight W1).

[0094] Here, the method for measuring the apparent density of the expanded beads (expanded beads after applying internal pressure) was as follows (1) to (3): (1) A measuring cylinder containing ethanol was prepared, and expanded beads with a weight Wd (g) were submerged in the ethanol; (2) The volume of the expanded beads read from the rise in the water level of the ethanol (submersion method) was defined as Vd (cc); (3) The apparent density of the expanded beads was calculated by the following formula; Apparent density of foam particles (g / cc) = Wd / Vd.

[0095] (Measurement of open cell ratio of foamed beads) The open cell ratio (interconnected cell ratio) of the expanded beads was measured by the following methods (1) to (3): (1) Using an air comparison type specific gravity meter [Tokyo Science Co., Ltd., Model 1000], the true volume Vc (cm) of the expanded beads was measured in accordance with the method described in PROCEDURE C of ASTM D2856-87. 3 (2) Next, the entire amount of the foamed beads after Vc measurement was submerged in a measuring cylinder containing ethanol, and the apparent volume Va (cm) of the foamed beads was calculated from the rise in the water level in the measuring cylinder (submersion method). 3 (3) The open cell ratio of the expanded beads was calculated using the following formula: Open cell ratio of foam particles (%) = (Va-Vc) x 100 / Va (Evaluation of surface properties of foamed molded products) The surface of the foam molded article was visually observed and the surface properties were evaluated based on the following criteria. Note that the larger the number, the fewer sink marks present on the surface of the foam molded article, in other words, the more excellent the surface properties. 4 (particularly good): Almost no sink marks are observed on the surface of the foam molded article. 3 (Good): Slight sink marks are observed on the surface of the foam molded article. 2 (Pass): Some sink marks are observed on the surface of the foam molded article. 1 (Poor): Sink marks are prominently observed on the surface of the foamed molded article.

[0096] (Internal fusion rate of foam molded body) 2 shows the shape of the foamed molded article 200 obtained in this example. The foamed molded article 200 has a box-like shape having a partition 202 (external dimensions: length 150 mm × width 300 mm × height 130 mm, thickness of the vertical wall 201: 20 mm, thickness of the partition 202: 120 mm, thickness of the bottom 203: 50 mm).

[0097] The evaluation of the fusion property of the foam molded body was carried out according to the following (1) to (4): (1) In one vertical side of the standing wall portion 201 of the in-mold foam molded body 200, at two points each 20 mm from both ends in the vertical direction toward the center, a cutter was used to make a cut (cuts 204a, 204b) of 20 mm in the width direction and 30 mm to 50 mm in the height direction. (2) After that, the above-mentioned one side of the standing wall portion 201 in which the cut was made by the above-mentioned operation was pulled by hand in the width direction toward the outside of the foam molded body to break it. As a result, the foam molded body broke at the position shown as the fracture surface 205 in FIG. 2. (3) The obtained 20 mm × 110 mm fracture surface 205 was visually observed, and the total number of foamed beads present in the fracture surface 205 and the number of foamed beads broken in the fracture surface 205 other than at the foamed bead interface (i.e., foamed beads in which the foamed beads themselves were broken) were counted. (4) The fusion rate of the foamed molded product was calculated based on the following formula: Fusion rate (%) of foamed molded article=(number of foamed particles broken at other than the foamed particle interface in fracture surface 205 / total number of foamed particles present in fracture surface 205)×100.

[0098] (Deformation amount of foam molded body) The foam molded body was placed on a horizontal surface so that the concave portion of the foam molded body faced the horizontal surface (i.e., the bottom 203 of the foam molded body was placed on top), and a taper gauge was inserted into the gap between the foam molded body and the horizontal surface until the taper gauge abutted both the foam molded body and the horizontal surface, and the size of the gap was measured. The size of the measured gap was taken as the amount of deformation of the foam molded body. It can be said that the smaller the amount of deformation, the less deformation the foam molded body has.

[0099] [Production Example 1] <Preparation of foam particles> (Aliphatic polyester resin foam particles) (1) Preparation of aliphatic polyester resin particles (resin particle manufacturing process) 100 parts by weight of P3HA, 1.0 part by weight of pentaerythritol, 0.50 parts by weight of behenamide, 0.50 parts by weight of erucamide, and 0.10 parts by weight of talc were weighed and dry blended to prepare an aliphatic polyester resin composition. The prepared aliphatic polyester resin composition was fed to a twin-screw extruder (TEM-26SX manufactured by Toshiba Machine Co., Ltd.), and the aliphatic polyester resin composition was melt-kneaded at a cylinder set temperature of 130°C to 160°C (melt-kneading step). The melt-kneaded aliphatic polyester resin composition at 179°C was discharged from the nozzle of the die attached to the tip of the extruder. The discharged aliphatic polyester resin composition was cooled with water at 50°C, and then cut to obtain cylindrical aliphatic polyester resin particles with a length / diameter ratio of 2.0 (resin particle molding step).

[0100] (2) Preparation of aliphatic polyester resin foam particles (foaming process) 100 parts by weight (2.5 kg) of aliphatic polyester resin particles obtained in the resin particle manufacturing process, 200 parts by weight of pure water as an aqueous dispersion medium, 2.0 parts by weight of 1,1-di(t-butylperoxy)cyclohexane (TBCH) as a crosslinking agent, 1.0 part by weight of tribasic calcium phosphate as a dispersing agent, and 0.05 parts by weight of sodium alkanesulfonate as a dispersing aid were supplied to a pressure vessel with an agitator having an internal volume of 10 L, and the agitator was rotated at 260 rpm to agitate the raw materials in the pressure vessel. After that, the contents (dispersion) in the pressure vessel were continuously stirred until the release of the dispersion was completed.

[0101] After introducing nitrogen into the pressure vessel, the vessel was evacuated to remove oxygen from the vessel. Carbon dioxide was then supplied as a foaming agent into the vessel to prepare a dispersion (dispersion step). The temperature in the vessel was then raised to a foaming temperature of 129.0°C. Carbon dioxide was then supplied to the vessel to raise the pressure in the vessel to a foaming pressure of 3.3 MPa (gauge pressure) (heating-pressure raising step). The temperature and pressure in the vessel were then maintained at approximately the foaming temperature and foaming pressure, respectively, for 30 minutes (holding step). After the holding step, the valve at the bottom of the vessel was opened, and the dispersion in the vessel was released under atmospheric pressure through an opening orifice with a diameter of 3.6 mm to obtain expanded aliphatic polyester resin particles (releasing step).

[0102] The resulting expanded beads were washed with an aqueous solution of sodium hexametaphosphate and water to remove the dispersant and other substances adhering to the surface of the expanded beads, and then dried at 75° C. The apparent density of the resulting expanded beads was 0.076 g / cm 3 (expanded particle magnification: 16 times) and the gel fraction was 67% by weight.

[0103] Example 1 The expanded beads obtained in Production Example 1 were fed into a pressure vessel at 40° C. While the temperature inside the pressure vessel was maintained at 40° C., the expanded beads in the pressure vessel were pressurized with air to an internal pressure of 0.16 MPa (absolute pressure). The pressure vessel was cooled to 20° C., and the expanded beads (expanded beads to which internal pressure had been applied) in the pressure vessel were taken out.

[0104] <Forming of foamed molded body> A molding die (a molding die capable of molding six foamed molded bodies 200) consisting of a fixed die and a movable die capable of molding the foamed molded body 200 (outer dimensions: length 150 mm × width 300 mm × height 130 mm, thickness of the vertical wall portion 201 20 mm, thickness of the partition portion 202 120 mm, thickness of the bottom portion 203 50 mm) shown in FIG. 2 was mounted on a molding machine (DABO DPM-1300). A total of 12 filling machines (two filling machines for each foamed molded body 200) equipped with a filling air supply unit were connected to the molding die, and a hopper containing the foamed beads to which the above-mentioned internal pressure was applied was connected to the filling machine via a foamed bead transport pipe equipped with an adjusted air supply unit. After starting to supply filling air from the filling air supply unit and adjusted air from the adjusted air supply unit in advance, the shutter of the hopper was opened and the foamed beads in the hopper were filled into the molding space of the molding die with the cracking amount set to 6 mm (filling process). The pressure inside the hopper, molding space pressure, filling air pressure, regulated air pressure, and regulated air pressure ratio during the filling process were as shown in Table 1.

[0105] After the filling was completed, the movable mold was driven toward the fixed mold, and the mold was completely closed. The mold was then preheated with steam, and the mold was further heated in one direction and in the reverse direction with steam, and in addition, the mold was heated on both sides with steam. Through these operations, the filled foam particles were fused to obtain a foamed molded product (foam molding process). Here, the steam pressure during one-way heating and reverse one-way heating (steam pressure A) was 0.03 MPa (gauge pressure), and the steam pressure during both-side heating (steam pressure B) was 0.14 MPa (gauge pressure). The obtained foamed molded product was removed from the mold and dried at 75°C. The internal fusion rate and deformation amount of the dried foamed molded product were measured, and the surface properties were evaluated. The results are shown in Table 1.

[0106] In addition, foamed beads were separately filled into a molding die in the same manner as above, and after filling was completed, the molding die was not closed and the foamed beads filled in the molding die were removed. The open cell ratio of the foamed beads after filling was measured. The results are shown in Table 1.

[0107] [Examples 2 to 15] Except for changing the filling air pressure, the regulating air pressure, and / or the internal pressure of the foamed beads as shown in Table 1, the foamed beads were filled into a molding die and heated in the same manner as in Example 1 to produce a foamed molded article. The measurement results of each physical property and each evaluation result are shown in Table 1.

[0108] [Table 1]

[0109] [Comparative Examples 1 to 5] A foamed molded article was produced by filling and heating the foamed beads in the molding die in the same manner as in Example 1, except that the pressure in the hopper, the molding space pressure, the filling air pressure, the regulated air pressure, and / or the foamed bead internal pressure were changed as shown in Table 2. The measurement results of each physical property and the evaluation results are shown in Table 2. In Comparative Examples 3 and 4, the molding space pressure was adjusted to 0.05 MPa (gauge pressure) in advance by feeding compressed air into the molding space (only compressed air was fed from the steam pipe for heating the molding die), and then the foamed beads were filled, and the molding space pressure was maintained at 0.05 MPa (gauge pressure) during filling. In Comparative Example 5, filling failure occurred, and a foamed molded article could not be obtained.

[0110] [Reference examples 1-3] A foamed molded article was produced by filling and heating the foamed beads in a molding die in the same manner as in Example 1, except that polypropylene (PP) resin foamed beads (Eperan-PP (expansion ratio 30 times) manufactured by Kaneka Corporation) were used instead of the aliphatic polyester resin foamed beads, and the pressure in the hopper, molding space pressure, filling air pressure, regulated air pressure, and / or foamed bead internal pressure were changed as shown in Table 2. The measurement results of each physical property and each evaluation result are shown in Table 2. The molding space pressure in Reference Example 3 was adjusted in the same manner as in Comparative Example 3.

[0111] [Table 2]

[0112] In Tables 1 and 2, (G) indicates gauge pressure. [Industrial Applicability]

[0113] One embodiment of the present invention can be suitably used as a method for producing foamed molded articles for various applications, such as food containers, packaging materials, sanitary products, automobile parts (particularly, tool boxes, etc.), packaging cushioning materials (particularly for home appliances), agricultural boxes, fish boxes, logistics materials, insulation materials, and civil engineering and construction parts. [Explanation of symbols]

[0114] 100 Molding equipment 1 Filling machine 2. Molding tool 3. Hopper 4. Foam particle transport pipe 5. Filling air supply 6 Regulated air supply 21 Molding space 51 Filling air supply pipe 52 Filling air generator 61 Adjusted air supply pipe 62 Regulated air generator

Claims

1. A method for producing an aliphatic polyester resin foamed molded article, comprising molding expanded aliphatic polyester resin particles using a molding device, the method comprising: The molding device includes: a hopper for accommodating the expanded aliphatic polyester resin particles; A foamed particle transport pipe having a regulated air supply; A molding die including a filling machine including a filling air supply unit; The hopper and the filling machine are connected by the foamed particle transport pipe, and The molding die has a molding space therein, The method for producing the aliphatic polyester resin foam molded article comprises the steps of: a filling step of filling the aliphatic polyester resin foamed particles from the hopper through the foamed particle transport pipe and the filling machine into the molding space, In the filling step, The pressure in the hopper is atmospheric pressure; Supplying fill air from the fill air supply unit; and Supplying regulated air from the regulated air supply unit. A method for producing an aliphatic polyester resin foam molded article.

2. 2. The method for producing an aliphatic polyester resin foam molded article according to claim 1, wherein in the filling step, a pressure of the filling air is equal to or higher than 0.30 MPa (gauge pressure) and lower than 0.68 MPa (gauge pressure).

3. 3. The method for producing an aliphatic polyester resin foam molded article according to claim 1, wherein in the filling step, a pressure of the regulated air is equal to or greater than 0.01 MPa (gauge pressure) and less than 0.34 MPa (gauge pressure).

4. 3. The method for producing an aliphatic polyester resin foam molded article according to claim 1, wherein in the filling step, a ratio of a pressure of the regulated air to a pressure of 100% of the filled air is 5% to 50%.

5. 3. The method for producing an aliphatic polyester resin foam molded article according to claim 1, wherein in the filling step, an internal pressure of the aliphatic polyester resin foam particles contained in the hopper is equal to or higher than atmospheric pressure and equal to or lower than 0.22 MPa (absolute pressure).

6. 6. The method for producing an aliphatic polyester resin foamed molded article according to claim 5, wherein the internal pressure of the aliphatic polyester resin foamed particles contained in the hopper in the filling step is 0.13 MPa (absolute pressure) to 0.18 MPa (absolute pressure).

7. 3. The method for producing an aliphatic polyester resin foamed molded article according to claim 1, wherein the expanded aliphatic polyester resin particles are expanded poly(3-hydroxyalkanoate) resin particles.

Citation Information

Patent Citations

  • Device for manufacture of in-mold foam molded body, foamed particle transfer auxiliary member, and manufacture of in-mold foam molded body