Novel vinyl-based polymer

The introduction of a terminal-modified vinyl polymer with specific structural formulas addresses the need for new vinyl polymer functions, offering enhanced properties for surfactants and polymer modification, particularly in copolymers with improved mechanical strength.

JP2024134390APending Publication Date: 2024-10-03KANEKA CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023044660
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

There is a need for the development of novel modified vinyl polymers with new functions and properties to expand their utilization in various applications.

Method used

A terminal-modified vinyl polymer with specific structural formulas is introduced, featuring terminal structures represented by general formula (1), which can be used as surfactants and macromonomers for polymer modification.

Benefits of technology

The terminal-modified vinyl polymer exhibits enhanced properties suitable for applications such as surfactants, epoxy curing agents, and fixed ligands, and when used as macromonomers, it can provide copolymers with improved breaking strain and surface impact strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134390000001
    Figure 2024134390000001
  • Figure 2024134390000002
    Figure 2024134390000002
  • Figure 2024134390000003
    Figure 2024134390000003
Patent Text Reader

Abstract

To provide a novel terminally modified vinyl-based polymer.SOLUTION: The terminally modified vinyl-based polymer has one or more terminal structures represented by the general formula (1) in the figure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel vinyl polymer. [Background technology]

[0002] Vinyl polymers are used in a variety of applications because of their weather resistance, heat resistance, oil resistance, transparency, and the like.

[0003] It is known that modified vinyl polymers obtained by introducing (modifying) functional groups into the molecular terminals and / or side chains of a vinyl polymer can have various physical properties depending on the type of functional group introduced.

[0004] The modified vinyl polymers as described above are used in various applications depending on the physical properties of the modified vinyl polymers. For example, Patent Documents 1 and 2 disclose curable compositions containing modified vinyl polymers, and Patent Document 3 discloses a surfactant containing a modified vinyl polymer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2000-119334 [Patent Document 2] Patent Publication No. 2011-074326 [Patent Document 3] Japanese Patent Publication No. 63-012602 Summary of the Invention [Problem to be solved by the invention]

[0006] There is still much room for development in the technology relating to modified vinyl polymers and their utilization, and there is a demand for the development of novel modified vinyl polymers having hitherto unknown functions or physical properties.

[0007] In view of the above circumstances, an object of one aspect of the present invention is to provide a novel terminal-modified vinyl polymer that can be used as a surfactant, a macromonomer for modifying a polymer, or the like. [Means for solving the problem]

[0008] A terminally modified vinyl polymer according to one embodiment of the present invention has one or more terminal structures represented by the following general formula (1):

[0009] [ka]

[0010] In formula (1), R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )- and; R 2 represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; R exists twice 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different. Effect of the Invention

[0011] According to one aspect of the present invention, it is possible to provide a novel terminal-modified vinyl polymer that can be used as a surfactant, a macromonomer for modifying a polymer, or the like. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An embodiment of the present invention will be described below, but the present invention is not limited thereto. In this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more and B or less." In addition, in this specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0013] [1. Terminally modified vinyl polymer] A terminally modified vinyl polymer according to one embodiment of the present invention (hereinafter, may be referred to as the present terminally modified vinyl polymer) has one or more terminal structures represented by the following general formula (1):

[0014] [ka]

[0015] In formula (1), R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )-and; R 2 represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; R exists twice 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.

[0016] Since the present terminal-modified vinyl polymer has the above-mentioned constitution, it can be suitably used in various applications such as a macromonomer for modifying polymers such as polyamides and polyesters, a surfactant, an epoxy curing agent, an anchoring ligand, etc. For example, when the present terminal-modified vinyl polymer is used as a macromonomer for modifying polymers, it is possible to provide a copolymer excellent in breaking strain and dart impact strength.

[0017] The present terminally modified vinyl polymer can be said to be a polymer having a terminal structure represented by the above general formula (1) and a main chain structure made of a vinyl polymer. The terminal structure and main chain structure constituting the present terminally modified vinyl polymer will be described in detail below.

[0018] (Terminal structure) The present terminally modified vinyl polymer has one or more terminal structures represented by the above general formula (1). Here, "having one or more terminal structures" means that the present terminally modified vinyl polymer has a terminal structure represented by the above general formula (1) at at least one end of the vinyl polymer that is the main chain. The number of terminal structures represented by the above general formula (1) that the present terminally modified vinyl polymer has is not particularly limited as long as it is one or more. For example, when the vinyl polymer that is the main chain is a linear (straight-chain) polymer, only one end of the linear polymer may have the terminal structure represented by the above general formula (1), or both ends may have the terminal structure represented by the above general formula (1). In addition, when the vinyl polymer that is the main chain is a branched polymer having three or more ends, only one end of the branched polymer may have the terminal structure represented by the above general formula (1), some of two or more ends may have the terminal structure represented by the above general formula (1), or all ends may have the terminal structure represented by the above general formula (1).

[0019] The scope of the present invention also includes a composition containing two or more vinyl polymers having the terminal structure represented by the above general formula (1). For example, the composition may contain both a linear polymer having the terminal structure represented by the above general formula (1) at only one end and a linear polymer having the terminal structure represented by the above general formula (1) at both ends.

[0020] More specific embodiments of the terminal structure represented by the above general formula (1) will be described in detail below.

[0021] In the above general formula (1), R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )-. Among them, R 1 is preferably -O(CO)- or -NH-.

[0022] In the above general formula (1), R 2 is a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom.

[0023] R 2 has 1 to 8 carbon atoms, and preferably 1 to 6 carbon atoms.

[0024] R 2 Examples of the heteroatom that may be contained include an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom, and a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).

[0025] R 2 may be a linear structure, a branched structure, or a cyclic structure. 2 When is a cyclic structure, R 2 may have a heterocyclic structure.

[0026] More specifically, R 2is preferably a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl. In this specification, a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl refers to a group obtained by removing two hydrogen atoms from an alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl, which is usually monovalent. In other words, a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl has three bonding sites with other molecules.

[0027] In the above general formula (1), R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom.

[0028] R 3 The number of carbon atoms in R is 0 to 8, preferably 0 to 6, more preferably 0 to 4, and further preferably 0 to 2. 3 The number of carbon atoms in R is 0. 3 is a single bond or consists of only heteroatoms.

[0029] R 3 Examples of the heteroatom that may be contained include an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom, and a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).

[0030] R 3 may be a linear structure, a branched structure, or a cyclic structure. 3 When is a cyclic structure, R 3 may have a heterocyclic structure.

[0031] More specifically, R 3is preferably a divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl. In this specification, the divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl refers to a group obtained by removing one hydrogen atom from an alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl, which is usually monovalent. That is, the divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl has two bonding sites with other molecules. The divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl is also referred to as alkylene, heteroalkylene, cycloalkylene, heterocycloalkylene, arylene or heteroarylene.

[0032] In the above general formula (1), R 4 and R 5 are each independently hydrogen, a methyl group, or an ethyl group. Among these, R 4 and R 5 is preferably hydrogen. Thus, R 4 or R 5 At least one of R is preferably hydrogen. 4 and R 5 More preferably, each of the groups is hydrogen.

[0033] In a preferred embodiment of the present invention, in the above general formula (1), R 2 has 1 to 6 carbon atoms, and R 3 has 0 to 2 carbon atoms, and R 4 and R 5 are both hydrogen.

[0034] In the above general formula (1), n ​​is 2. In other words, the terminal structure represented by the above general formula (1) has two structures represented by the following general formula (1'). -R 3 -N(R 4 )R5 (1') That is, the terminal structure represented by the above general formula (1) is R 3 , R 4 and R 5 Each of the compounds has two structures represented by the following formula:

[0035] R 3 , R 4 and R 5 The structures represented by the above general formula (1') may be the same or different from each other. In other words, the structures represented by the above general formula (1') present in each of the terminal structures represented by the above general formula (1) may be the same or different from each other.

[0036] Specific examples of the terminal structure represented by the above general formula (1) include structures represented by the following formulas (i) to (iii). The present terminal-modified vinyl polymer preferably has, as a terminal structure, any one of structures selected from the following formulas (i) to (iii).

[0037] [ka]

[0038] (Main Chain) The present terminally modified vinyl polymer has a main chain structure composed of structural units derived from a vinyl monomer.

[0039] The vinyl monomer from which the structural unit constituting the main chain of the present terminally modified vinyl polymer is derived is not particularly limited as long as it has a vinyl group. Examples of the vinyl monomer include (meth)acrylic acid monomers, styrene monomers, maleimide monomers, chlorine-containing vinyl monomers, fluorine-containing vinyl monomers, silicon-containing vinyl monomers, nitrile group-containing vinyl monomers, amide group-containing vinyl monomers, vinyl esters, alkenes, and conjugated dienes.

[0040] Examples of the (meth)acrylic acid monomer include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-methyl-3-propanediol ... Hydroxypropyl, stearyl (meth)acrylate, glycidyl (meth)acrylate, 2-aminoethyl (meth)acrylate, γ-((meth)acryloyloxypropyl)trimethoxysilane, ethylene oxide adduct of (meth)acrylic acid, trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, 2-perfluorohexadecylethyl (meth)acrylate, and the like.

[0041] Examples of the styrene monomer include styrene, vinyltoluene, α-methylstyrene, chlorostyrene, styrenesulfonic acid, and salts of styrenesulfonic acid.

[0042] Examples of the maleimide monomer include maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide.

[0043] The chlorine-containing vinyl monomer is not particularly limited, but suitable examples include vinyl chloride, vinylidene chloride, and allyl chloride.

[0044] Examples of the fluorine-containing vinyl monomer include perfluoroethylene, perfluoropropylene, and vinylidene fluoride.

[0045] Examples of the silicon-containing vinyl monomer include vinyltrimethoxysilane and vinyltriethoxysilane.

[0046] Examples of the nitrile group-containing vinyl monomer include acrylonitrile and methacrylonitrile.

[0047] Examples of the amide group-containing vinyl monomer include acrylamide and methacrylamide.

[0048] Examples of vinyl esters include vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, and vinyl cinnamate.

[0049] Examples of alkenes include ethylene, propylene, butylene, and isobutylene.

[0050] Examples of conjugated dienes include butadiene and isoprene.

[0051] Suitable examples of the vinyl monomer from which the structural units constituting the main chain of the present terminally modified vinyl polymer are derived include maleic anhydride, maleic acid, monoalkyl esters of maleic acid, dialkyl esters of maleic acid, fumaric acid, monoalkyl esters of fumaric acid, dialkyl esters of fumaric acid, and allyl alcohol.

[0052] The main chain of the present terminally modified vinyl polymer may be a homopolymer containing only structural units derived from one of the above-mentioned vinyl monomers, or may be a copolymer containing structural units derived from any two or more vinyl monomers.

[0053] In particular, since modification of the polymer terminals is relatively easy, the main chain of the present terminal-modified vinyl polymer is preferably composed mainly of one or more of a constituent unit derived from a (meth)acrylic acid monomer, a constituent unit derived from a styrene monomer, or a constituent unit derived from isobutylene. That is, the main chain of the present terminal-modified vinyl polymer is preferably composed mainly of poly(meth)acrylate, polystyrene, or polyisobutylene. The main chain of the present terminal-modified vinyl polymer may be a copolymer composed mainly of a constituent unit derived from two or more types selected from the group consisting of a (meth)acrylate monomer, a styrene monomer, and isobutylene.

[0054] In this specification, the main chain of a vinyl polymer mainly composed of poly(meth)acrylate means that the main chain contains 50 mol% or more of structural units derived from (meth)acrylic acid monomers out of 100 mol% of all structural units contained in the main chain. When the main chain of the present terminal-modified vinyl polymer is mainly composed of poly(meth)acrylate, the main chain of the present terminal-modified vinyl polymer preferably contains 60 mol% or more of structural units derived from (meth)acrylic acid monomers out of 100 mol% of all structural units contained in the main chain, more preferably contains 70 mol% or more, even more preferably contains 80 mol% or more, even more preferably contains 90 mol% or more, and may even be 100 mol%.

[0055] In this specification, the main chain of a vinyl polymer mainly composed of polystyrene means that the main chain contains 50 mol% or more of structural units derived from styrene monomers out of 100 mol% of all structural units contained in the main chain. When the main chain of the present terminal-modified vinyl polymer is mainly composed of polystyrene, the main chain of the present terminal-modified vinyl polymer preferably contains 60 mol% or more of structural units derived from styrene monomers out of 100 mol% of all structural units contained in the main chain, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, or may even be 100 mol%.

[0056] In this specification, the main chain of a vinyl polymer mainly composed of polyisobutylene means that the main chain contains 50 mol % or more of structural units derived from isobutylene out of 100 mol % of all structural units contained in the main chain. When the main chain of the present terminal-modified vinyl polymer is mainly composed of polyisobutylene, the main chain of the present terminal-modified vinyl polymer preferably contains 60 mol % or more of structural units derived from isobutylene out of 100 mol % of all structural units contained in the main chain, more preferably contains 70 mol % or more, even more preferably contains 80 mol % or more, even more preferably contains 90 mol % or more, and may even be 100 mol %.

[0057] In this specification, the main chain of a vinyl polymer mainly comprises structural units derived from two or more selected from the group consisting of (meth)acrylate, styrene, and isobutylene, meaning that the main chain contains structural units derived from (meth)acrylate monomers, styrene monomers, or isobutylene in a total amount of 50 mol% or more out of 100 mol% of all structural units contained in the main chain. When the main chain of the present terminal-modified vinyl polymer mainly comprises structural units derived from two or more selected from the group consisting of (meth)acrylate monomers, styrene monomers, and isobutylene, the main chain of the present terminal-modified vinyl polymer preferably contains structural units derived from (meth)acrylate monomers, styrene monomers, or isobutylene in a total amount of 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, or may be 100 mol% out of 100 mol% of all structural units contained in the main chain.

[0058] The main chain of the present terminally modified vinyl polymer may contain, in addition to the constituent units derived from the above vinyl monomers, constituent units derived from monomers other than vinyl monomers (other monomers). Examples of the other monomers include vinyl chloride, acrylonitrile, and acrylamide.

[0059] The content of structural units derived from other monomers in the main chain of the present terminally modified vinyl polymer is preferably less than 50 mol%, more preferably 40 mol% or less, more preferably 30 mol% or less, even more preferably 20 mol% or less, even more preferably 10 mol% or less, or may be 0 mol%, based on 100 mol% of all structural units contained in the main chain.

[0060] The structure of the main chain of the present terminal-modified vinyl polymer is not particularly limited, and may be a linear structure or a branched structure, i.e., the main chain of the present terminal-modified vinyl polymer may be a linear polymer or a branched polymer.

[0061] In a preferred embodiment of the present invention, the main chain of the terminally modified vinyl polymer is preferably a linear polymer, and one or both ends of the linear polymer preferably have a terminal structure represented by the above general formula (1).

[0062] The polymerization method for the vinyl polymer that is the main chain of the present terminally modified vinyl polymer is not particularly limited, and examples thereof include the polymerization methods described in JP-A-2005-232419, JP-A-2006-291073, and JP-A-2016-88944.

[0063] The vinyl polymer which is the main chain of the present terminally modified vinyl polymer may have a structure derived from a substance other than the vinyl monomer (e.g., a polymerization catalyst, etc.) in the vinyl polymer (particularly at the terminal). For example, when a vinyl polymer is polymerized by a polymerization method using mercaptans described later, the obtained vinyl polymer may have a structure containing an S group derived from the mercaptans at its terminal. When such a vinyl polymer having an S group at its terminal is used as the main chain, the present terminally modified vinyl polymer may further have a structure containing an S group derived from the mercaptans between the terminal structure represented by the above general formula (1) and the main chain structure consisting of the vinyl monomer.

[0064] The present terminally modified vinyl polymer may have a terminal structure represented by the above general formula (1) at its terminal, and may further have a structure derived from a substance other than the vinyl monomer, such as a polymerization catalyst (e.g., a structure containing an S group), between the terminal structure represented by the above general formula (1) and the main chain structure consisting of the vinyl monomer, as described above. Such an embodiment is also included in one embodiment of the present invention.

[0065] (Weight average molecular weight) The present terminally modified vinyl polymer preferably has a weight average molecular weight of 550 or more, more preferably 1,200 or more, and even more preferably 2,400 or more, as measured by size exclusion chromatography (SEC). The weight average molecular weight is preferably 1,100,000 or less, more preferably 200,000 or less, and even more preferably 50,000 or less. According to this configuration, the number of terminal structures represented by the above general formula (1) introduced into the vinyl polymer can be easily controlled, and a terminally modified vinyl polymer having a desired number of terminal structures represented by general formula (1) can be provided.

[0066] (number average molecular weight) The number average molecular weight of the present terminally modified vinyl polymer, as measured by size exclusion chromatography, is preferably 500 or more, more preferably 1,000 or more, and even more preferably 2,000 or more. The number average molecular weight is preferably 600,000 or less, more preferably 100,000 or less, and even more preferably 30,000 or less. According to this configuration, the number of terminal structures represented by the above general formula (1) introduced into the vinyl polymer can be easily controlled, and a terminally modified vinyl polymer having a desired number of terminal structures represented by general formula (1) can be provided.

[0067] (Molecular weight distribution (Mw / Mn)) The present terminal-modified vinyl polymer preferably has a molecular weight distribution, i.e., the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by size exclusion chromatography, of 1.8 or less, more preferably 1.7 or less, more preferably 1.6 or less, even more preferably 1.5 or less, even more preferably 1.4 or less, and particularly preferably 1.3 or less. According to this configuration, the number of terminal structures represented by the above general formula (1) introduced into the vinyl polymer can be easily controlled, and a terminal-modified vinyl polymer having a desired number of terminal structures represented by general formula (1) can be provided. The lower limit of the molecular weight distribution is theoretically 1.

[0068] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the vinyl polymer in this specification are values ​​measured by SEC and calculated in terms of polystyrene. The specific method for measuring the weight average molecular weight (Mw) and number average molecular weight (Mn) of the vinyl polymer is as described in the Examples.

[0069] 2. Method for producing terminally modified vinyl polymer The method for producing a terminal-modified vinyl polymerization according to one embodiment of the present invention (hereinafter, may be referred to as "the present production method") is not particularly limited as long as it can provide a terminal-modified vinyl polymer having one or more terminal structures represented by the above general formula (1), i.e., the present terminal-modified vinyl polymer. However, the following production method (1) or (2) can be mentioned as a suitable production method: Method (1): A method comprising the step of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the following general formula (2a):

[0070] [ka]

[0071] In formula (2a), X is -OH, -COOH, -NH 2 , -N(CH 3 )H or -N(CH 2 CH 3 )H, or a salt thereof; R 2 represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (2a), there are two R 3 , R4 and R 5 The structures of may be the same or different.

[0072] Method (2): A method comprising the steps of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the following general formula (2b) and reducing the resulting reaction product.

[0073] [ka]

[0074] In formula (2b), X is -OH, -COOH, -NH 2 , -N(CH 3 )H or -N(CH 2 CH 3 )H, or a salt thereof; R 2 represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (2b), there are two R 3 , R 4 and R 5 The structures of may be the same or different.

[0075] In the above formulas (2a) and (2b), examples of the salt for X include salts of alkali metals such as potassium and sodium, and salts of alkaline earth metals such as calcium and magnesium.

[0076] The terminal structure represented by general formula (1) in this production method is as explained above.

[0077] According to the present production method, it is possible to provide a terminal-modified vinyl polymer having one or more terminal structures represented by the above general formula (1). Therefore, the present production method can be suitably used as a method for producing the present terminal-modified vinyl polymer.

[0078] Specific embodiments of the present production method will be described in detail below using methods (1) and (2) as examples, but the method for producing the present terminally modified vinyl polymer is not limited to these methods.

[0079] (Method (1)) In one embodiment of the present invention, as one aspect of the production method, there is provided a method for producing a terminal-modified vinyl polymer, which comprises a step of reacting a halogen group located at the terminal of a vinyl polymer with a compound represented by the above general formula (2a) (method (1)). In this specification, the method for producing a terminal-modified vinyl polymer by method (1) may be referred to as the "first production method".

[0080] (First reaction step) The first production method includes a step of reacting a halogen group located at the terminal of a vinyl polymer with a compound represented by the above general formula (2a) (sometimes referred to as a first reaction step). In this step, the terminal of the vinyl polymer is modified by reacting the compound represented by the above general formula (2a) with the terminal of the vinyl polymer, and a terminal-modified vinyl polymer having one or more terminal structures derived from the compound represented by the above general formula (2a), i.e., the terminal structures represented by the above general formula (1), can be obtained.

[0081] In the first reaction step, the method of reacting the halogen group located at the terminal of the vinyl polymer with the compound represented by the general formula (2a) is not particularly limited, but may include a method of dissolving the vinyl polymer having a halogen group at its terminal and the compound represented by the general formula (2a) in a solvent, and heating (and stirring as necessary) the vinyl polymer and the compound represented by the general formula (2a) in the solvent.

[0082] In the first reaction step, the solvent in which the reaction is carried out is not particularly limited, but since the reaction is a nucleophilic substitution reaction, a polar solvent is preferred. Examples of polar solvents that can be used in the first reaction step include N,N-dimethylacetamide, tetrahydrofuran, dioxane, diethyl ether, acetone, dimethyl sulfoxide, dimethylformamide, hexamethylphosphoric triamide, acetonitrile, etc.

[0083] In the first reaction step, the temperature (heating temperature) at which the vinyl polymer and the compound represented by the general formula (2a) in the solvent are heated is not limited, and is, for example, 30°C to 120°C, preferably 50°C to 100°C, and more preferably 70°C to 90°C.

[0084] The heating time in the first reaction step is not particularly limited, but it is preferable to continue heating until all halogen groups in the vinyl polymer subjected to the reaction are reacted (substituted) with the compound represented by the above general formula (2a). The specific heating time may be, for example, 30 minutes to 6 hours.

[0085] As described above, the terminal structure represented by the general formula (1) of the terminally modified vinyl polymer obtained by the first production method has a structure derived from the compound represented by the general formula (2a). That is, in the terminal structure represented by the general formula (1) of the obtained terminally modified vinyl polymer, R 1 In X, some atoms (e.g., H or metal elements constituting the salt) are replaced with bonds by reaction with the vinyl polymer, and R 1 , R 2 , R 3 , R 4 and R 5 Therefore, R in the compound represented by the general formula (2a) used in the first production method 2 , R 3 , R 4 and R 5 For more detailed aspects of the above, the description in the above section [1. Terminally modified vinyl polymer] is incorporated herein as appropriate.

[0086] Specific examples of the compound represented by the above general formula (2a) include structures represented by the following formulae (iv) to (vi). As the compound represented by the general formula (2a), any compound selected from the following formulae (iv) to (vi) is preferable.

[0087] [ka]

[0088] (Method (2)) In one embodiment of the present invention, as one aspect of the present production method, there is provided a method for producing a terminal-modified vinyl polymer, comprising the steps of reacting a halogen group located at the terminal of a vinyl polymer with a compound represented by the above general formula (2b) and reducing the resulting reaction product (method (2)). In this specification, the method for producing a terminal-modified vinyl polymer by method (2) may be referred to as the "second production method".

[0089] (Second reaction step) The second production method includes a step of reacting a halogen group located at the terminal of a vinyl polymer with a compound represented by the above general formula (2b) (sometimes referred to as a second reaction step). In this step, the terminal of the vinyl polymer is modified by reacting the compound represented by the above general formula (2b) to obtain a terminal-modified vinyl polymer having one or more terminal structures derived from the compound represented by the above general formula (2b).

[0090] In the second reaction step, the method of reacting the halogen group located at the terminal of the vinyl polymer with the compound represented by the general formula (2b) is not particularly limited, but may include a method of dissolving the vinyl polymer having a halogen group at its terminal and the compound represented by the general formula (2b) in a solvent, and heating (and stirring as necessary) the vinyl polymer and the compound represented by the general formula (2b) in the solvent.

[0091] In the second reaction step, the solvent in which the reaction is carried out is not particularly limited, but since the reaction is a nucleophilic substitution reaction, a polar solvent is preferred. Examples of polar solvents that can be used in the second reaction step include N,N-dimethylacetamide, tetrahydrofuran, dioxane, diethyl ether, acetone, dimethyl sulfoxide, dimethylformamide, hexamethylphosphoric triamide, acetonitrile, etc.

[0092] In the second reaction step, the temperature (heating temperature) at which the vinyl polymer and the compound represented by the general formula (2b) in the solvent are heated is not limited, and is, for example, 30°C to 120°C, preferably 50°C to 100°C, and more preferably 70°C to 90°C.

[0093] The heating time in the second reaction step is not particularly limited, but it is preferable to continue heating until all halogen groups in the vinyl polymer subjected to the reaction are reacted (substituted) with the compound represented by the above general formula (2b). The specific heating time may be, for example, 30 minutes to 6 hours.

[0094] (Reduction process) The second production method includes a step of reducing a terminal-modified vinyl polymer having one or more terminal structures derived from the compound represented by the above general formula (2b), i.e., the reaction product obtained in the above second reaction step. In this step, the reaction product obtained in the above second reaction step is reduced, i.e., the nitro group at the end of the reaction product is reduced and converted to an amino group, thereby obtaining a terminal-modified vinyl polymer having one or more terminal structures represented by the above general formula (1) derived from the compound represented by the above general formula (2b). The terminal structure of the terminal-modified vinyl polymer obtained in the second production method is the terminal structure represented by the above general formula (1), which is represented by R 4 and R 5 are terminal structures in which all are H.

[0095] In the reduction step, the method for reducing the reactant obtained in the second reaction step is not particularly limited, but may include a method in which the reactant obtained in the second reaction step is reacted with a reducing agent.

[0096] Examples of reducing agents that can be used in the reduction step include ammonium chloride, hydrogen, hydrazine, lithium aluminum hydride, and sodium borohydride.

[0097] As described above, the terminal structure represented by the general formula (1) of the terminally modified vinyl polymer obtained by the second production method has a structure derived from the compound represented by the general formula (2b). That is, in the terminal structure represented by the general formula (1) of the obtained terminally modified vinyl polymer, R 1 In X, some atoms (e.g., H or metal elements constituting the salt) are replaced with bonds by reaction with the vinyl polymer, resulting in a structure of R 2 and R 3 Therefore, R in the compound represented by the general formula (2b) used in the second production method 1 , R 2 and R 3 For more detailed aspects of the above, the description in the above section [1. Terminally modified vinyl polymer] is incorporated herein as appropriate.

[0098] A specific example of the compound represented by the above general formula (2b) is a structure represented by the following formula (vii): As the compound represented by the general formula (2b), the compound represented by the following formula (vii) is preferred because it causes few side reactions and can quantitatively react with the halogen group located at the end of the vinyl polymer.

[0099] [ka]

[0100] (Method (3)) In one embodiment of the present invention, as an aspect of the present production method other than the above-mentioned method (1) or method (2), there is provided a method for producing a terminal-modified vinyl polymer, comprising a step of reacting a functional group other than a halogen group, such as a hydroxyl group or a carboxyl group, located at the terminal of a vinyl polymer with a compound represented by the following general formula (2c) (method (3)):

[0101] [ka]

[0102] In formula (2c), X' is -OH, -NH 2 , -N(CH 3 )H, -N(CH 2 CH 3 ) H, -COOH, -COZ or -Z (Z is a halogen atom); R 2 represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (2c), there are two R 3 , R 4 and R 5 The structures of may be the same or different. In this specification, the process for producing a terminally modified vinyl polymer by the process (3) is sometimes referred to as the "third process".

[0103] (Third reaction step) The third production method includes a step (sometimes referred to as a third reaction step) of reacting a functional group other than a halogen group, such as a hydroxyl group or a carboxyl group, located at the terminal of a vinyl polymer with a compound of the following general formula (2c). In this step, the terminal of the vinyl polymer is modified by reacting the compound represented by the above general formula (2c) with the terminal of the vinyl polymer, thereby obtaining a terminal-modified vinyl polymer having a terminal structure derived from the compound represented by the above general formula (2c), i.e., one or more terminal structures represented by the above general formula (1).

[0104] As described above, the terminal structure represented by the general formula (1) of the terminal-modified vinyl polymer obtained by the third production method has a structure derived from the compound represented by the general formula (2c). That is, in the terminal structure represented by the general formula (1) of the obtained terminal-modified vinyl polymer, R 1 In X', some atoms (e.g., H, OH, or Z) are replaced with bonds by reaction with the vinyl polymer, and R 1 , R 2 , R 3 , R 4 and R 5 Therefore, R in the compound represented by the general formula (2c) used in the third production method 2 , R 3 , R 4 and R 5 For more detailed aspects of the above, the description in the above section [1. Terminally modified vinyl polymer] is incorporated herein as appropriate.

[0105] (Vinyl polymer preparation process) The first and second manufacturing methods may further include a step of preparing a vinyl polymer having a halogen group at the end (a vinyl polymer preparation step). As a method for preparing (polymerizing) a vinyl polymer having a halogen group at the end, various known polymerization methods such as living cationic polymerization and living radical polymerization can be adopted. In addition, the third manufacturing method may further include a step of preparing a vinyl polymer having a functional group other than a halogen group at the end. As a method for preparing (polymerizing) a vinyl polymer having a functional group other than a halogen group at the end, a polymerization method using a mercaptan having a hydroxyl group such as mercaptoethanol or a mercaptan having a carboxyl group such as mercaptoacetic acid, as described in JP-A-1-203412, can also be used.

[0106] Hereinafter, a specific embodiment of the vinyl polymer preparation process will be described in detail, taking the living radical polymerization method as an example.

[0107] As the vinyl monomer serving as the raw material for the vinyl polymer, any of the vinyl monomers described in the above section [1. Terminally modified vinyl polymer] can be appropriately used.

[0108] Examples of living radical polymerization include (a) a polymerization method using a chain transfer agent such as polysulfide, (b) a polymerization method using a radical scavenger such as an organic tellurium compound, a cobalt porphyrin complex, and / or a nitroxide compound, (c) an atom transfer radical polymerization (ATRP) method using an organic halide or the like as an initiator and a transition metal complex as a catalyst, and (d) a polymerization method (reversible transfer catalytic polymerization (RTCP)) using an organic halide or the like as an initiator and an organic molecule having a central atom such as nitrogen or oxygen as a catalyst. Of these, the atom transfer radical polymerization method is preferred because it is easy to control the molecular weight and molecular weight distribution of the vinyl polymer.

[0109] In living radical polymerization, the number of halogen terminals of the vinyl polymer obtained can be controlled by controlling the polymerization conditions. For example, the number of halogen terminals of the vinyl polymer obtained can be controlled by controlling the type of polymerization initiator. Specifically, when an initiator having one polymerization initiation point is used, a linear vinyl polymer having a halogen group at one end can be prepared, and when an initiator having two polymerization initiation points is used, a linear vinyl polymer having a halogen group at both ends can be prepared.

[0110] Examples of initiators having one polymerization initiation point include ethyl 2-bromoisobutyrate, ethyl bromoacetate, methyl bromoacetate, (1-bromoethyl)benzene, allyl bromide, methyl 2-bromopropionate, methyl chloroacetate, methyl 2-chloropropionate, (1-chloroethyl)benzene, etc. Examples of initiators having two polymerization initiation points include diethyl 2,5-dibromoadipate, dimethyl 2,5-dibromoadipate, diethyl 2,5-dibromoadipate, etc.

[0111] In the vinyl polymer preparation step, the number of halogen terminal groups in the obtained vinyl polymer can be controlled to control the number of compounds represented by general formula (2a) or (2b) which react with the vinyl polymer in the first reaction step or the second reaction step, i.e., the number of terminal structures represented by general formula (1) in the finally obtained terminally modified vinyl polymer.

[0112] In the living radical polymerization, in addition to the initiator, a polymerization catalyst, a polydentate amine (ligand), a base, a reducing agent, a solvent, etc. may be used. The type and amount of each of these components can be appropriately selected by those skilled in the art.

[0113] 3. Uses of the present terminally modified vinyl polymer The uses of the present terminally modified vinyl polymer are not particularly limited, but for example, it can be suitably used in various applications such as a macromonomer for polymer modification; a surfactant; an epoxy curing agent; and an anchoring ligand.

[0114] (Macromonomer for polymer modification) In one embodiment of the present invention, a polymer modifying macromonomer made of the present terminally modified vinyl polymer is provided. When the present terminally modified vinyl polymer is used as a polymer modifying macromonomer, the physical properties of the polymer can be changed. As an example of the polymer modifying effect of the present terminally modified vinyl polymer, it is possible to provide a copolymer (resin) having excellent breaking strain and impact strength compared to a case in which the macromonomer made of the present terminally modified vinyl polymer is not blended.

[0115] The polymer to which the polymer modifying macromonomer made of the present terminally modified vinyl polymer is applied is not particularly limited, but examples thereof include polyamide resins and polyester resins.

[0116] (Surfactant) In one embodiment of the present invention, a surfactant is provided that includes a terminally modified vinyl polymer. The terminally modified vinyl polymer has excellent surface activity and can be suitably used as a surfactant.

[0117] [4. Summary] An embodiment of the present invention may include the following features. [1] A terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1):

[0118] [ka]

[0119] In formula (1), R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH2 CH 3 )- and; R 2 represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; R exists twice 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different. [2] R 2 is a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl; R 3 is a divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl. [3] R 2 has 1 to 6 carbon atoms, R 3 has 0 to 2 carbon atoms, R 4 and R 5 and each of them is hydrogen. [4] The terminal-modified vinyl polymer according to [1], wherein the terminal structure represented by the above general formula (1) has any one of structures selected from the following formulas (i) to (iii):

[0120] [ka]

[0121] [5] The terminal-modified vinyl polymer is a linear polymer, The terminal-modified vinyl polymer according to [1], wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1). [6] The terminally modified vinyl polymer according to [1], wherein the main chain of the terminally modified vinyl polymer is mainly composed of poly(meth)acrylate or polyisobutylene. [7] The terminally modified vinyl polymer according to [1], which has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less, as measured by size exclusion chromatography. [8] A surfactant comprising a terminally modified vinyl polymer according to any one of [1] to [7]. [9] A method for producing a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1), A production method comprising a step of reacting a halogen group located at a terminal of a vinyl polymer with a compound represented by the following general formula (2a):

[0122] [ka]

[0123] [ka]

[0124] In formula (1) and formula (2a), X is -OH, -COOH, -NH 2 , -N(CH 3 )H or -N(CH 2 CH 3 )H, or a salt thereof; R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )-and; R 2represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (1) and formula (2a), there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.

[10] A method for producing a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1), A step of reacting a halogen group located at the terminal of a vinyl polymer with a compound represented by the following general formula (2b): reducing the resulting reaction product; A method of manufacturing the same, comprising:

[0125] [ka]

[0126] [ka]

[0127] In formula (1) and formula (2b), X is -OH, -COOH, -NH 2 , -N(CH 3 )H or -N(CH 2 CH 3 )H, or a salt thereof; R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH3 )-and; R 2 represents a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (1) and formula (2b), there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.

[11] R 2 is a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl; R 3 is a divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl.

[12] R 2 has 1 to 6 carbon atoms, R 3 has 0 to 2 carbon atoms, R 4 and R 5 and are each hydrogen.

[13] The method according to [9], wherein the compound represented by the above general formula (2a) has any one of the structures selected from the following formulae (iv) to (vi):

[0128] [ka]

[0129]

[14] The method according to

[10] , wherein the compound represented by the above general formula (2b) has a structure represented by the following formula (vii):

[0130] [ka]

[0131]

[15] The terminal-modified vinyl polymer is a linear polymer, The method according to any one of [9] to

[14] , wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1).

[16] The method according to any one of [9] to

[15] , wherein the main chain of the terminally modified vinyl polymer is mainly composed of poly(meth)acrylate or polyisobutylene.

[17] The terminal-modified vinyl polymer has a molecular weight of 1.0 or more, when measured by size exclusion chromatography, The method according to any one of [9] to

[16] , wherein the polystyrene-equivalent number average molecular weight is 500 to 600,000 and the molecular weight distribution is 1.8 or less.

[0132] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0133] Hereinafter, one embodiment of the present invention will be described in detail with reference to examples, but the present invention is not limited to the following examples.

[0134] [Analysis method] (Polymerization conversion rate) The conversion rate of monomers to polymers in the production of vinyl polymers was measured using a gas chromatograph (GC (Shimadzu Corporation, GC-2000)). The column used was Agilent J&W GC column HP-1. Toluene was used as the standard.

[0135] (Qualitative and quantitative analysis of functional groups) Qualitative and quantitative analysis of functional groups in polymers 1 The analysis was performed using 1 H NMR (Bruker 400 MHz NMR). 30 mg of the polymer was dissolved in 0.8 g of deuterated chloroform to obtain a solution, which was used as a sample for analysis.

[0136] (Weight average molecular weight (Mw) and number average molecular weight (Mn)) The weight-average molecular weight and number-average molecular weight of the polymer were analyzed using SEC (HLC-8420GPC). The column used was TOSOH TSKgel SuperHM-L, and the standard was a polystyrene standard sample. The eluent was a mixed solvent of chloroform with 1.5% by weight of triethylamine added. 3 mg of the polymer was dissolved in 3 ml of the mixed solvent, and the resulting solution was used as the sample for analysis.

[0137] (Bromine end analysis) After replacing the terminal bromine groups of the polymer with potassium acrylate, 1 The amount of H at the base of the substituent was calculated by H NMR. The method for replacing the terminal bromine group is as follows. A large excess of dimethylacetamide and potassium acrylate was added to the vinyl polymer, and the resulting solution was stirred at 50°C for 30 minutes. An excess of ethyl acetate and water was added to the resulting solution, and only the organic layer was collected from the resulting mixture. The organic layer was then concentrated to obtain a vinyl polymer in which the terminal bromine group had been replaced with potassium acrylate. The resulting vinyl polymer was dissolved in deuterated chloroform, and the resulting solution was used as an analytical sample, 1H NMR measurement was carried out. As a result, a signal of H at the base of the substituent substituted with potassium acrylate was confirmed in the range of 4.8 to 5.2 ppm, and the amount of terminal bromine of the vinyl polymer was calculated from the integral value.

[0138] (Tensile test evaluation) Tensile tests were conducted in accordance with JIS K 6251:2017 to measure the yield stress, breaking strain, and breaking stress of the molded body. For the measurements, test pieces were used that were cut into No. 3 dumbbell shapes from 0.5 mm press-molded sheet-like molded bodies and cured overnight or more in a constant temperature and humidity room at 23°C and 50% RH. The tensile speed was 200 mm / min.

[0139] (Dynamic viscoelasticity (tan δ) evaluation) Using a dynamic viscoelasticity measuring device (IT Measurement & Control, DVA-200), measurements were performed in tensile mode, with a strain of 0.05%, and at temperatures of -70 to 400°C, and the dynamic viscoelasticity (tan δ) of the molded body was measured at a frequency of 10 Hz and 35°C. Test pieces used for the measurements were prepared by cutting out 8 mm x 6 mm from a sheet-like molded body press-molded to 0.5 mm, and curing the cut piece overnight or more in a constant temperature and humidity chamber at 23°C and 50% RH.

[0140] (surface impact strength) A drop weight test was performed with a load of 300 to 500 g using a 15 mm hemispherical impact core in a DuPont impact tester manufactured by Toyo Seiki Co., Ltd., and the fracture energy (J) was measured. For the measurement, a test piece was used, which was made by curing a sheet-like molded body pressed to 0.5 mm in a constant temperature and humidity room at 23°C and 50% RH for at least one night.

[0141] (Measurement of 1% weight loss temperature) Using a simultaneous thermogravimetry and differential thermal analyzer (STA7200, Hitachi High-Tech Science), measurements were performed at a heating rate of 10°C / min in a nitrogen atmosphere at 0 to 500°C. The 1% weight loss temperature was measured as the temperature at which the molded body lost 1% weight. For the measurements, test pieces were used that were prepared by curing a sheet-shaped molded body pressed to 0.5 mm in a constant temperature and humidity chamber at 23°C and 50% RH for at least one night.

[0142] Example 1 [Production Example 1] Production Example 1-1: Production of Polymer 1-1 160 g of methanol, 320 g of butyl acrylate, 55.3 g of ethyl 2-bromoisobutyrate, 4.3 g of triethylamine, 0.16 g of cupric bromide, and 0.16 g of tris[2-(dimethylamino)ethyl]amine were added to the flask. Next, nitrogen was bubbled into the flask. Note that "nitrogen bubbling" refers to the flow of nitrogen into a flask or a target such as a solution to remove oxygen from the target. After the nitrogen bubbling, the mixture in the flask was heated and the temperature was raised to 45°C.

[0143] Separately, 49 g of methanol, 0.25 g of ascorbic acid, and 0.29 g of triethylamine were mixed to obtain a methanol solution, which was then bubbled with nitrogen and added dropwise to the flask at a rate of 5.1 ml / h.

[0144] 0.5 hours after the start of the dropping of the methanol solution, 480 g of butyl acrylate bubbled with nitrogen was dropped into the flask over 1.5 hours. 4 hours after the start of the dropping of the methanol solution, it was confirmed by gas chromatography that the conversion rate of butyl acrylate reached 95% or more, and the dropping of the methanol solution was stopped. Then, the reaction solution in the flask was concentrated at 100°C under vacuum for 1 hour. 800 g of butyl acetate, 8 g of Kyoward 500 (manufactured by Kyowa Chemical Industry), 8 g of Kyoward 700 (manufactured by Kyowa Chemical Industry), and 8 g of Radiolite 900 (manufactured by Showa Chemical Industry) were added to the concentrated reaction solution, and the mixture was stirred at 80°C for 1 hour. Next, the obtained reaction solution was filtered. The obtained filtrate was concentrated at 100°C under vacuum for 2 hours to obtain polybutyl acrylate (polymer 1-1) having bromine at one end. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-1 was 2574 and the molecular weight distribution was 1.30. Furthermore, it was found that polymer 1-1 has an average of 0.86 bromine terminals per molecule. 1 Confirmed by 1 H NMR.

[0145] Production Example 1-2: Production of Polymer 1-2 160g of methanol, 309g of butyl acrylate, 83g of ethyl acrylate, 9g of 2-methoxyethyl acrylate, 12g of diethyl 2,5-dibromoadipate, 4.3g of triethylamine, 0.16g of cupric bromide, and 0.16g of tris[2-(dimethylamino)ethyl]amine were added to the flask. Nitrogen was then bubbled through the flask. The mixture in the flask was heated to 45°C.

[0146] Separately, 49 g of methanol, 0.25 g of ascorbic acid, and 0.29 g of triethylamine were mixed to obtain a methanol solution, which was then bubbled with nitrogen and added dropwise to the flask at a rate of 5.1 ml / h.

[0147] 0.5 hours after the start of the dripping of the methanol solution, a mixture of 463 g of butyl acrylate, 124 g of ethyl acrylate, and 13 g of 2-methoxyethyl acrylate, which had been bubbled with nitrogen, was dripped into the flask over 1.5 hours. 4 hours after the start of the dripping of the methanol solution, it was confirmed by gas chromatography that the conversion rates of butyl acrylate, ethyl acrylate, and 2-methoxyethyl acrylate reached 95% or more, respectively, and the dripping of the methanol solution was stopped. Thereafter, the reaction solution in the flask was concentrated at 100°C under vacuum for 1 hour. To the concentrated reaction solution, 1000 g of butyl acetate, 10 g of Kyoward 500 (manufactured by Kyowa Chemical), 10 g of Kyoward 700 (manufactured by Kyowa Chemical), and 10 g of Radiolite 900 (manufactured by Showa Chemical) were added, and the mixture was stirred at 80°C for 1 hour. Next, the resulting reaction solution was filtered. The filtrate was concentrated at 100°C under vacuum for 2 hours to obtain a copolymer of butyl acrylate, ethyl acrylate, and 2-methoxyethyl acrylate having bromine at both ends (polymer 1-2). The number average molecular weight of the obtained polymer 1-2 was 35,316, and the molecular weight distribution was 1.1, as confirmed by SEC. Furthermore, polymer 1-2 was found to have an average of 1.9 bromine ends per molecule. 1 Confirmed by 1 H NMR.

[0148] (Example 1-1) 10 g of polymer 1-1 and 10 g of N,N-dimethylacetamide were added to a flask and stirred to make it uniform. 0.95 g of tris(2-aminoethyl)amine was added while stirring. The flask was then heated and stirred at 80°C for 1 hour. After that, 30 g of 1-butanol and 30 g of water were added, stirred at room temperature, and allowed to stand for separation. An extraction operation was performed three times to extract only the organic layer. The organic layer obtained was concentrated at 50°C under vacuum for 1 hour to obtain a terminal-modified vinyl polymer (polymer 1-3) in which the bromine terminal of polymer 1-1 was replaced with a structure derived from tris(2-aminoethyl)amine. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-3 was 3355 and the molecular weight distribution was 1.80. It was further confirmed that the bromine terminal of polymer 1-3 was completely eliminated. 1 Confirmed by 1 H NMR.

[0149] 1 g of water, 1 g of butyl acetate, and 0.1 g of polymer 1-3 were placed in a vial, stirred at 1000 rpm for 1 minute with a vortex mixer, and allowed to stand for 1 minute. When the inside of the vial was visually inspected after standing, both the organic layer and the aqueous layer were in a suspended state, suggesting that the oil-water interface had been activated.

[0150] (Example 1-2) A terminal-modified vinyl polymer (polymer 1-4) was obtained by the same procedure as in Example 1-1, except that the amount of tris(2-aminoethyl)amine was changed to 1.90 g. The number average molecular weight of the obtained polymer 1-4 was 3445, and the molecular weight distribution was 1.31, as confirmed by SEC. Furthermore, it was confirmed that the bromine terminals of polymer 1-4 were completely eliminated. 1 Confirmed by 1 H NMR.

[0151] 1 g of water, 1 g of butyl acetate, and 0.1 g of polymer 1-4 were placed in a vial, stirred at 1000 rpm for 1 minute with a vortex mixer, and allowed to stand for 1 minute. When the inside of the vial was visually inspected after standing, both the organic layer and the aqueous layer were in a suspended state, suggesting that the oil-water interface had been activated.

[0152] (Examples 1-3) 50 g of polymer 1-2 and 50 g of N,N-dimethylacetamide were added to a flask and stirred to make the mixture homogenous. 1.83 g of tris(2-aminoethyl)amine was added while stirring. The flask was then heated and stirred at 80°C for 1 hour. Then, 150 g of 1-butanol and 150 g of water were added, stirred at room temperature, and allowed to stand for separation. An extraction operation was performed three times to extract only the organic layer. The organic layer obtained was concentrated at 50°C under vacuum for 1 hour to obtain a terminal-modified vinyl polymer (polymer 1-5) in which the bromine terminals of polymer 1-2 were replaced with a structure derived from tris(2-aminoethyl)amine. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-5 was 22416 and the molecular weight distribution was 1.52. It was further confirmed that the bromine terminals of polymer 1-5 were completely eliminated. 1 Confirmed by 1 H NMR.

[0153] 1 g of water, 1 g of butyl acetate, and 0.1 g of polymer 1-5 were placed in a vial, stirred at 1000 rpm for 1 minute with a vortex mixer, and allowed to stand for 1 minute. When the inside of the vial was visually inspected after standing, both the organic layer and the aqueous layer were in a suspended state, suggesting that the oil-water interface had been activated.

[0154] (Examples 1 to 4) 150 g of polymer 1-1 and 150 g of N,N-dimethylacetamide were added to a flask and stirred to make the mixture homogenous. 13.5 g of potassium carbonate and 16.4 g of diaminobenzoic acid were added while stirring. The flask was then heated and stirred at 80°C for 4 hours. Then, 450 g of 1-butanol and 450 g of water were added, stirred at room temperature, and allowed to stand for separation. An extraction operation was performed three times to extract only the organic layer. The organic layer obtained was concentrated at 50°C under vacuum for 1 hour to obtain a terminal-modified vinyl polymer (polymer 1-6) in which the bromine terminal of polymer 1-1 was replaced with a structure derived from diaminobenzoic acid. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-6 was 2628 and the molecular weight distribution was 1.19. Furthermore, it was confirmed that the bromine terminal of polymer 1-6 was completely replaced with the ester group of diaminobenzoic acid. 1 Confirmed by 1 H NMR.

[0155] 1 g of water, 1 g of butyl acetate, and 0.1 g of polymer 1-6 were placed in a vial, stirred at 1000 rpm for 1 minute with a vortex mixer, and allowed to stand for 1 minute. When the inside of the vial was visually inspected after standing, the aqueous layer was in a suspended state, suggesting that the oil-water interface had been activated.

[0156] (Examples 1 to 5) 50 g of polymer 1-1 and 50 g of N,N-dimethylacetamide were added to a flask and stirred to make the mixture homogenous. 4.5 g of potassium carbonate and 5.2 g of dinitrobenzoic acid were added while stirring. The flask was then heated and stirred at 80°C for 4 hours. Then, 150 g of 1-butanol and 150 g of water were added, stirred at room temperature, and allowed to stand for separation. This extraction procedure was repeated three times to extract only the organic layer. The organic layer was concentrated at 50°C under vacuum for 1 hour to obtain a polymer (polymer 1-7') in which the bromine terminals of polymer 1-1 were replaced with a structure derived from dinitrobenzoic acid. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-7' was 3126 and the molecular weight distribution was 1.10. It was further confirmed that the bromine terminals of the obtained polymer 1-7' were completely replaced with ester groups of dinitrobenzoic acid. 1 Confirmed by 1 H NMR.

[0157] Next, 10 g of the obtained polymer 1-7', 4 g of ethanol, 10 g of water, 0.91 g of iron powder, and 0.69 g of ammonium chloride were added to a flask, and the mixture was heated and stirred at 80°C for 9 hours. Then, 10 g of 1-butanol was added and filtered. 20 g of water was added to the obtained filtrate, and the mixture was stirred and allowed to stand for separation, and an extraction operation was performed three times to extract only the organic layer. The obtained organic layer was concentrated at 50°C under vacuum for 1 hour, to obtain a polymer (polymer 1-7) in which the nitro groups in the terminal groups of polymer 1-7' were converted to amino groups. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-7 was 2981 and the molecular weight distribution was 1.29. Furthermore, it was confirmed that the bromine terminals of polymer 1-7 were completely replaced with ester groups of diaminobenzoic acid. 1 Confirmed by 1 H NMR.

[0158] (Examples 1 to 6) 10 g of polymer 1-1 and 10 g of N,N-dimethylacetamide were added to a flask and stirred to make the mixture homogenous. 1.64 g of melamine was further added while stirring. Next, the flask was heated and stirred at 120°C for 13 hours. After that, 30 g of 1-butanol and 30 g of water were added, and the mixture was stirred at room temperature, allowed to stand for separation, and an extraction operation was performed three times to collect only the organic layer. The obtained organic layer was concentrated at 50°C under vacuum for 1 hour to obtain a polymer (polymer 1-8) in which the bromine terminals of polymer 1-1 were replaced with a structure derived from melamine. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-8 was 3009 and the molecular weight distribution was 1.12. It was further confirmed that 94% of the bromine terminals of polymer 1-8 had disappeared. 1 Confirmed by 1 H NMR.

[0159] 1 g of water, 1 g of butyl acetate, and 0.1 g of polymer 1-8 were placed in a vial, stirred at 1000 rpm for 1 minute with a vortex mixer, and allowed to stand for 1 minute. When the inside of the vial was visually inspected after standing, the aqueous layer was in a suspended state, suggesting that the oil-water interface had been activated.

[0160] (Comparative Example 1-1) 1 g of water, 1 g of butyl acetate, and 0.1 g of polymer 1-3 were placed in a vial, stirred at 1000 rpm for 1 minute with a vortex mixer, and allowed to stand for 1 minute. When the inside of the vial was visually inspected after standing, both the organic layer and the aqueous layer were clear, suggesting that the oil-water interface had not been activated.

[0161] (Comparative Example 1-2) 1 g of water, 1 g of butyl acetate, and 0.1 g of polymer 1-3 were placed in a vial, stirred at 1000 rpm for 1 minute with a vortex mixer, and allowed to stand for 1 minute. When the inside of the vial was visually inspected after standing, both the organic layer and the aqueous layer were clear, suggesting that the oil-water interface had not been activated.

[0162] [Table 1]

[0163] From Table 1, it was shown that the polymers of Comparative Examples 1-1 and 1-2, which are terminally unmodified, do not exhibit surface activity, while the polymers of Examples 1-1 to 1-6, which are terminally modified vinyl polymers having diamine terminals (i.e., the present terminally modified vinyl polymers), have surface activity. This suggests that the present terminally modified vinyl polymers can be suitably used as surfactants.

[0164] Example 2 [Production Example 2] Manufacturing Example 2-1 The same procedure as in Production Example 1-1 was carried out to obtain polybutyl acrylate (polymer 2-1) having bromine at one end. The number average molecular weight of the obtained polymer 2-1 was 2574, and the molecular weight distribution was 1.30, as confirmed by SEC. Furthermore, it was confirmed that polymer 2-1 had an average of 0.86 bromine terminals per molecule. 1 Confirmed by 1 H NMR.

[0165] Manufacturing Example 2-2 The same procedure as in Production Example 1-2 was carried out to obtain a copolymer of butyl acrylate, ethyl acrylate, and 2-methoxyethyl acrylate having bromine at both ends (Polymer 2-2). The number average molecular weight of the obtained polymer 2-2 was 35,316, and the molecular weight distribution was 1.1, as confirmed by SEC. Furthermore, it was confirmed that polymer 2-2 had an average of 1.9 bromine terminals per molecule. 1 Confirmed by 1 H NMR.

[0166] (Example 2-1) The same procedure as in Example 1-4 was carried out except that polymer 2-1 was used instead of polymer 1-1, to obtain a terminal-modified vinyl polymer (polymer 2-3) in which the bromine terminals of polymer 2-1 were replaced with structures derived from diaminobenzoic acid. The number average molecular weight of the obtained polymer 2-3 was 2628, and the molecular weight distribution was 1.19, as confirmed by SEC. Furthermore, it was confirmed that the bromine terminals of polymer 2-3 were completely replaced with ester groups of diaminobenzoic acid. 1 Confirmed by 1 H NMR.

[0167] (Example 2-2) The same procedure as in Example 1-2 was carried out except that polymer 2-1 was used instead of polymer 1-1, to obtain a terminal-modified vinyl polymer (polymer 2-4). The number average molecular weight of the obtained polymer 2-4 was 3445, and the molecular weight distribution was 1.31, as confirmed by SEC. Furthermore, it was confirmed that polymer 2-4 had no bromine terminals at all. 1 Confirmed by 1 H NMR.

[0168] (Examples 2-3 and 2-4) 12-aminododecanoic acid, adipic acid, and sodium hypophosphite monohydrate were added to the flask, and nitrogen was flowed for 10 minutes to replace the atmosphere in the flask with nitrogen. Polymer 2-3 was added while heating to 200°C. Isophoronediamine was further added, and the mixture was heated and stirred at 200°C for 2 hours. Then, the mixture was further heated and stirred at 230°C for 2 hours. Sumilizer GA-80 was further added, and the mixture was heated and stirred at 210°C for 5 minutes to obtain a polyamide polymer. The obtained polyamide polymer was vacuum dried at 170°C for 4 hours, and then compressed to a thickness of 0.5 mm at 250°C and 5 MPa to obtain a polyamide molded product. The number average molecular weight and molecular weight distribution of the obtained polymer were confirmed by SEC. The physical properties of the molded product were also evaluated by tensile tests, dynamic viscoelasticity measurements, and TG / DTA measurements. The results are shown in Table 2.

[0169] (Examples 2-5) The same procedure as in Example 2-3 was repeated except that Polymer 2-4 was used instead of Polymer 2-3 to obtain a polymer and a molded product, and the physical properties were measured and evaluated. The results are shown in Table 2.

[0170] (Comparative Example 2-1) The same procedure as in Example 2-3 was repeated except that Polymer 2-3 was not used to obtain a polymer and a molded product, and the physical properties were measured and evaluated. The results are shown in Table 2.

[0171] [Table 2]

[0172] From Table 2, it can be seen that the molded bodies made of the polyamide polymers of Examples 2-3 to 2-5, which are copolymerized with a terminal-modified vinyl polymer having a diamine terminal, are superior in break strain and surface impact strength as well as dynamic viscoelasticity compared to the molded body of Comparative Example 2-1 made of a polyamide polymer not copolymerized with a terminal-modified vinyl polymer having a diamine terminal. On the other hand, there was almost no change in the yield stress, break stress, and 1% weight loss temperature. From the above, it was suggested that the polyamide resin copolymerized with a terminal-modified vinyl polymer having a diamine terminal (i.e., this terminal-modified vinyl polymer) is superior in break strain and surface impact strength, and has improved flexibility and low-temperature properties. From this, it was suggested that this terminal-modified vinyl polymer can be suitably used as a macromonomer for polymer modification. [Industrial Applicability]

[0173] According to one embodiment of the present invention, a novel terminal-modified vinyl polymer can be provided. The novel terminal-modified vinyl polymer according to one embodiment of the present invention can be suitably used for applications such as surfactants and macromonomers for polymer modification.

Claims

1. A terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1): 【Chemistry 1】 In formula (1), R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )—wherein R 2 is a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 is a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; There are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.

2. R 2 is a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl; R 3 The terminal-modified vinyl polymer according to claim 1 , wherein is a divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl.

3. R 2 has 1 to 6 carbon atoms, R 3 has 0 to 2 carbon atoms, R 4 and R 5 and each of the above is hydrogen.

4. 2. The terminal-modified vinyl polymer according to claim 1, wherein the terminal structure represented by the above general formula (1) has any structure selected from the following formulas (i) to (iii): 【Chemistry 2】

5. The terminal-modified vinyl polymer is a linear polymer, 2. The terminal-modified vinyl polymer according to claim 1, wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1).

6. 2. The terminally modified vinyl polymer according to claim 1, wherein the main chain of the terminally modified vinyl polymer is mainly composed of poly(meth)acrylate or polyisobutylene.

7. The terminally modified vinyl polymer has a molecular weight of 1.01 or more, when measured by size exclusion chromatography.

2. The terminally modified vinyl polymer according to claim 1, which has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less.

8. A surfactant comprising the terminally modified vinyl polymer according to any one of claims 1 to 7.

9. A method for producing a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1), A production method comprising a step of reacting a halogen group located at a terminal of a vinyl polymer with a compound represented by the following general formula (2a): 【Chemistry 3】 【Chemistry 4】 In formula (1) and formula (2a), X is -OH, -COOH, -NH 2 , -N(CH 3 )H or -N(CH 2 CH 3 ) H, or a salt thereof; R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )—wherein R 2 is a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 is a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (1) and formula (2a), there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.

10. A method for producing a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1), A process for reacting a halogen group located at a terminal of a vinyl polymer with a compound represented by the following general formula (2b): reducing the resulting reaction product; A method of manufacturing the same, comprising: 【Chemistry 5】 【Chemistry 6】 In formula (1) and formula (2b), X is -OH, -COOH, -NH 2 , -N(CH 3 )H or -N(CH 2 CH 3 ) H, or a salt thereof; R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )—wherein R 2 is a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 is a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (1) and formula (2b), there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.

11. R 2 is a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl; R 3 The method according to claim 9 or 10, wherein is a divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl.

12. R 2 has 1 to 6 carbon atoms, R 3 has 0 to 2 carbon atoms, R 4 and R 5 The method according to claim 9 or 10, wherein each of

13. The method according to claim 9, wherein the compound represented by the general formula (2a) has any one of the structures selected from the following formulas (iv) to (vi). 【Chemistry 7】

14. The method according to claim 10, wherein the compound represented by the general formula (2b) has a structure represented by the following formula (vii): 【Chemistry 8】

15. The terminal-modified vinyl polymer is a linear polymer, The method according to claim 9 or 10, wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1).

16. 11. The method according to claim 9, wherein the main chain of the terminally modified vinyl polymer is mainly composed of poly(meth)acrylate or polyisobutylene.

17. The terminally modified vinyl polymer has a molecular weight of 1.01 or more, when measured by size exclusion chromatography. The process according to claim 9 or 10, wherein the polystyrene-equivalent number average molecular weight is 500 to 600,000 and the molecular weight distribution is 1.8 or less.

Citation Information

Patent Citations

  • Production of modified diene-based polymer rubber

    JP1989217011A

  • Elastomer composition

    JP1999209524A

  • Functionalized and halogenated polymers for microencapsulation

    JP2005514473A

  • Polyfunctional hyperbranched and hyperbranched polymers and methods for their production

    JP2009519369A

  • Method for producing polar group-containing polyolefin

    JP2019081897A