Liquid resin composition
A balanced blend of epoxy resins and conductive powders with varying specific surface areas addresses the challenges of high viscosity and thixotropy in conductive adhesives, providing improved applicability and connectivity in electronic components.
Patent Information
- Application Number
- JP2023044763
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Conductive adhesives used in electronic components face challenges with high viscosity and thixotropy, which affect applicability and ability to form fine electrical connections and penetrate gaps, while achieving low resistance and flexibility is difficult with existing resin compositions.
A liquid resin composition combining high viscosity epoxy resins with conductive powders of varying specific surface areas to balance viscosity, thixotropy, and resistance, using a blend of conductive powders with large and small specific surface areas along with a latent curing agent.
The composition achieves low viscosity, low thixotropy, and low resistance, enhancing applicability and connectivity in electronic component assembly, particularly in compact devices like mobile phones.
Smart Images

Figure 2024134448000001 
Figure 2024134448000002 
Figure 2024134448000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid resin composition having low viscosity, low thixotropy and low resistance. [Background technology]
[0002] In the manufacture of electronic components and printed wiring boards, etc., a conductive adhesive (also called a conductive paste) may be used to establish electrical connections between components, etc., and to form wiring and electrodes. For example, Patent Document 1 discloses a liquid resin composition containing an epoxy resin, silver particles, etc., which is useful as a conductive adhesive. Furthermore, when a conductive adhesive is used in a portable electronic device, the cured product may be required to have functionality such as drop impact resistance. To achieve drop impact resistance, it is possible to impart flexibility to the cured product. In order to impart flexibility to the cured product, it is possible to use an epoxy resin with a flexible skeleton, but resins with a flexible skeleton generally have a high molecular weight and tend to increase the viscosity and thixotropy of the conductive adhesive. Similarly, when high reliability and high heat resistance are required for the conductive adhesive, it is possible to use an epoxy resin with a rigid skeleton, but such epoxy resins also tend to increase the viscosity and thixotropy of the conductive adhesive. However, if the viscosity or thixotropy of the conductive adhesive is high, the applicability may be reduced. If the applicability is reduced, for example, when the conductive adhesive is discharged through a nozzle during application, it may be disadvantageous in forming fine electrical connections. Also, when the conductive adhesive is used by permeating into gaps in an adherend, if the viscosity or thixotropy of the conductive adhesive is high, the permeability into the gaps may be reduced. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-42696 A Summary of the Invention [Problem to be solved by the invention]
[0004] One method to reduce the viscosity and thixotropy of conductive adhesives is to use silver particles with a small specific surface area, but this increases the resistivity and reduces the conductivity.On the other hand, if silver particles with a large specific surface area are used, the resistivity decreases, but there is a problem that the viscosity and thixotropy increase.
[0005] The present invention has been made in light of the above circumstances, and an object of the present invention is to provide a liquid resin composition that is useful as a conductive adhesive and has low viscosity, low thixotropy, and low resistance (a well-balanced relationship between viscosity, thixotropic index value, and resistivity). [Means for solving the problem]
[0006] As a result of intensive research into solving the above problems, the present inventors discovered that in a liquid resin composition containing a high-viscosity or solid epoxy resin, by using a conductive powder having a large specific surface area in combination with a conductive powder having a small specific surface area, a liquid resin composition having low viscosity, low thixotropy and low resistance can be obtained, and thus completed the present invention.
[0007] That is, the present invention has the following features. [1] The following components (A) to (D): (A) one or more epoxy resins selected from liquid epoxy resins and solid epoxy resins having a viscosity of 15 Pa s or more at 25°C; (B) Specific surface area is 0.30 m 2 / g or more conductive powder, (C) Specific surface area is 0.25 m 2 / g or less conductive powder, (D) Latent hardener and having a viscosity of less than 20 Pa·s at 25°C. [2] The liquid resin composition according to [1], having a thixotropic index (TI) value at 25°C of 1.0 or more and less than 3.5. [3] The liquid resin composition according to [1] or [2], having a viscosity at 25°C of 1 Pa·s or more and less than 20 Pa·s. [4] The liquid resin composition according to any one of [1] to [3], wherein the content of component (A) is 1% by mass or more and 10% by mass or less, based on 100% by mass of the non-volatile components in the liquid resin composition. [5] The liquid resin composition according to any one of [1] to [4], wherein the component (A) is a flexible epoxy resin having (a) a bisphenol structural unit and (b) a linear hydrocarbon structural unit having 4 or more carbon atoms and / or a polyalkylene ether structural unit having 3 or more ether oxygen atoms. [6] (B) component has a specific surface area of 0.30 m 2 / g or more 0.60m 2 The liquid resin composition according to any one of [1] to [5], wherein the conductive powder is less than or equal to 1 g. [7] The liquid resin composition according to any one of [1] to [6], wherein the tap density of component (B) is 5.2 g / cc or less. [8] The liquid resin composition according to any one of [1] to [7], wherein the tap density of component (B) is 3.0 g / cc or more and 5.2 g / cc or less. [9] (C) component has a specific surface area of 0.05 m 2 / g or more 0.25m 2 The liquid resin composition according to any one of [1] to [8], wherein the conductive powder is less than or equal to 1 g / g.
[10] The liquid resin composition according to any one of [1] to [9], wherein the tap density of component (C) is 5.7 g / cc or more.
[11] The liquid resin composition according to any one of [1] to
[10] , wherein the tap density of component (C) is 5.7 g / cc or more and 9.0 g / cc or less.
[12] The liquid resin composition according to any one of [1] to
[11] , wherein the total content of the (B) component and the (C) component is 60 mass% or more based on 100 mass% of the non-volatile components in the liquid resin composition.
[13] The liquid resin composition according to any one of [1] to
[12] , wherein the total content of the (B) component and the (C) component is 60% by mass or more and 80% by mass or less, based on 100% by mass of the non-volatile components in the liquid resin composition.
[14] The liquid resin composition according to any one of [1] to
[13] , wherein the mass ratio of the component (B) to the component (C) in the liquid resin composition is 1:9 to 9:1.
[15] The liquid resin composition according to any one of [1] to
[14] , wherein the component (B) and the component (C) are silver powder.
[16] The liquid resin composition according to any one of [1] to
[15] , wherein the component (D) is one or more selected from the group consisting of a tertiary amino group-containing modified polyamine, a urea bond-containing modified polyamine, and an imidazole-containing modified polyamine.
[17] (A') The liquid resin composition according to any one of [1] to
[16] , further comprising an epoxy resin having a viscosity at 25°C of 50 mPa·s or more and less than 15 Pa·s.
[18] The liquid resin composition according to
[17] , wherein the content of the (A') component is 50% by mass or more and 95% by mass or less, relative to 100% by mass of the combined total of the (A) and (A') components contained in the liquid resin composition.
[19] The liquid resin composition according to any one of [1] to
[18] , which may or may not contain a resin having a viscosity of less than 50 mPa s and / or an organic solvent, and the total content of these components is from 0% by mass to 3% by mass, relative to 100% by mass of the liquid resin composition (including volatile components). Effect of the Invention
[0008] According to the present invention, it is possible to provide a liquid resin composition having low viscosity, low thixotropy and low resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described below based on preferred embodiments thereof. The liquid resin composition of the present invention contains the following components (A) to (D) as essential components and has a viscosity at 25° C. of less than 20 Pa s: (A) one or more epoxy resins selected from liquid epoxy resins and solid epoxy resins having a viscosity of 15 Pa s or more at 25°C; (B) Specific surface area is 0.30 m 2 / g or more conductive powder, (C) Specific surface area is 0.25 m 2 / g or less conductive powder, (D) Latent hardener.
[0010] <Component (A)> Component (A) is one or more epoxy resins selected from liquid epoxy resins and solid epoxy resins having a viscosity of 15 Pa s or more at 25° C. By adding component (A), it is possible to impart physical properties such as flexibility (drop impact resistance) to the cured product of the liquid resin composition.
[0011] (Liquid epoxy resin with a viscosity of 15 Pa·s or more at 25°C) The liquid epoxy resin having a viscosity of 15 Pa·s or more at 25°C is not particularly limited as long as it has a viscosity of 15 Pa·s or more at 25°C, and includes liquid epoxy resins having the following fluidity at 25°C. In the present invention, "liquid" refers to a resin having a viscosity of less than 1500 Pa·s measured by the following measurement method. 0.2 to 0.3 ml of the resin (or resin composition) to be measured is measured with a syringe using a RE-80 type viscometer (manufactured by Toki Sangyo Co., Ltd.). During measurement, the temperature of the measurement chamber of the viscometer is controlled at 25.0°C in an external circulation type thermostatic bath. The rotor rotation speed is set to 20 rpm, and the viscosity after 120 seconds is measured. In the present invention, a solid epoxy resin is a concept including semi-solid epoxy resins, and refers to an epoxy resin having a viscosity of 1500 Pa·s or more measured by the above measurement method. Note that a solid epoxy resin in the present invention also includes one having a viscosity above the measurement limit of the above measurement method and a solid epoxy resin that has no fluidity at all.
[0012] Liquid epoxy resins having a viscosity of 15 Pa·s or more at 25°C preferably have an average of two or more epoxy groups per molecule. Examples of the epoxy resin include bisphenol A type epoxy resins, biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, phenol aralkyl type epoxy resins, naphthol type epoxy resins, naphthalene type epoxy resins, bisphenol F type epoxy resins, phosphorus-containing epoxy resins, bisphenol S type epoxy resins, aromatic glycidylamine type epoxy resins (e.g., tetraglycidyldiaminodiphenylmethane, triglycidyl-p-aminophenol, diglycidyl toluidine, diglycidyl aniline, etc.), alicyclic epoxy resins, aliphatic chain epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, epoxy resins having a butadiene structure, epoxy resins having a dicyclopentadiene structure, diglycidyl ethers of bisphenols, diglycidyl ethers of naphthalene diols, glycidyl ethers of phenols, and diglycidyl ethers of alcohols, as well as alkyl substituted, halogenated and hydrogenated versions of these epoxy resins. These may be used alone or in combination of two or more.
[0013] The viscosity of the liquid epoxy resin having a viscosity of 15 Pa·s or more at 25°C is preferably 20 Pa·s or more, and the upper limit is not particularly limited as long as the liquid epoxy resin has fluidity at 25°C. From the viewpoint of low viscosity and low thixotropy, the viscosity is preferably 2000 Pa·s or less, and more preferably 1500 Pa·s or less. In one embodiment of the present invention, an epoxy resin having a viscosity of 15 Pa·s or more and 2000 Pa·s or less at 25°C is preferred, and an epoxy resin having a viscosity of 30 Pa·s or more and 1500 Pa·s or less at 25°C is more preferred. In the present invention, "a viscosity of 15 Pa·s or more at 25°C" means that the viscosity measured at 25°C and 20 rpm using an E-type viscometer is 15 Pa·s or more. A liquid epoxy resin having a viscosity of 15 Pa·s or more at 25°C is also included in the liquid epoxy resin having a viscosity of 15 Pa·s or more at 25°C, so long as the epoxy resin falls within the definition of "liquid".
[0014] In a preferred embodiment of the present invention, the liquid epoxy resin having a viscosity of 15 Pa s or more at 25° C. is a flexible epoxy resin having (a) a bisphenol structural unit and (b) a linear hydrocarbon structural unit having 4 or more carbon atoms and / or a polyalkylene ether structural unit having 3 or more ether oxygen atoms. When an epoxy resin having such a flexible skeleton is used, the elastic modulus of the cured product can be easily set low, and the drop impact resistance of the cured product can be improved.
[0015] The flexible epoxy resin may be used alone or in combination of two or more kinds. The structural units (a) and (b) may each be of one type or of two or more types.
[0016] The bisphenol structural unit may be a structural unit derived from bisphenol A, bisphenol F, or bisphenol S. Specific examples include units derived from these without the OH groups at their terminals and units represented by the following general formula (1), and the ring may be hydrogenated. Furthermore, these rings may have a substituent such as a hydrocarbon group, an alkoxyl group, an aryl group, an aryloxy group, or a hydroxyl group.
[0017] [ka]
[0018] The linear hydrocarbon structural unit having 4 or more carbon atoms or the polyalkylene ether structural unit must be present in addition to the bisphenol structural unit. Among these, the linear hydrocarbon structural unit having 4 or more carbon atoms is -(CH 2 ) x - is a structural unit in which x is 4 or more. x is preferably 4 to 20, and more preferably 4 to 10. In place of the hydrogen atom, a substituent such as a hydroxyl group may be present, and further, at least one of the hydrogen atoms may be substituted with a hydrocarbon group, an alkoxyl group, an aryl group, an aryloxy group, or the like. The hydrocarbon or alkoxyl group as the substituent preferably has 4 or less carbon atoms, and the aryl group of the aryl group or aryloxy group is preferably a phenyl group. These substituents can be present within a range that does not impair the flexibility of the structural unit (b).
[0019] The polyalkylene ether structural unit has 3 or more ether oxygen atoms, preferably 3 to 20, more preferably 3 to 10. Specific examples include structural units derived from a polymer of one or more alkylene oxides selected from ethylene oxide, propylene oxide, butylene oxide, isobutylene oxide, neopentylene oxide, tetramethylene oxide, etc. In addition, examples include those in which one or more hydrogen atoms of this alkylene oxide are substituted with, for example, a hydroxyl group, an alkoxyl group, an aryl group, an aryloxy group, a hydrocarbon group, etc. The hydrocarbon or alkoxyl group as the substituent preferably has 4 or less carbon atoms, and the aryl group of the aryl group or aryloxy group is preferably a phenyl group. These substituents can be present within a range that does not impair the flexibility of the structural unit (b).
[0020] The linear hydrocarbon structural unit having 4 or more carbon atoms gives a cured product with high heat resistance, and the polyalkylene ether structural unit improves adhesion and adhesion to, for example, metal substrates, etc. By appropriately selecting these structural units, it is possible to accommodate a variety of substrates, manufacturing processes, and required performance.
[0021] In the present invention, the molar ratio of the structural unit (a) to the structural unit (b) is preferably 10:1 to 1:5, more preferably 5:1 to 1:3. If the structural unit (a) is more than this range, the epoxy cured product will not have sufficient flexibility, and the thermal stress of the cured product will not be sufficiently relieved, which will cause cracking or peeling of the cured product. If the structural unit (a) is less than the above range, the Tg of the epoxy cured product will be too low, and the heat resistance will decrease.
[0022] Specifically, the flexible epoxy resin is preferably an epoxy resin having one or more structures shown in the following structural formulas (2-i) to (2-iv). In addition, multiple hydroxyl groups in the structural formulas shown below may undergo a crosslinking reaction, and oxygen atoms of the hydroxyl groups may bond unspecified structures.
[0023] [ka]
[0024] In structural formulas (2-i) to (2-iv), Ar 1 , Ar 2 are bisphenol type structural units (a) which may be the same or different, may be hydrogenated, and may have a substituent, and X is a linear hydrocarbon group having 4 or more carbon atoms and / or a polyalkylene ether structure having 1 or more ether oxygen atoms. When X is a linear hydrocarbon group having 4 or more carbon atoms, X is a structural unit (b), and when X is a polyalkylene ether structure having 1 or more ether oxygen atoms, -OXO- has ether oxygens at both ends which constitute the structural unit (b). Also, n is the average value of the repeating units and is 1 to 30.
[0025] As a method for obtaining such a flexible epoxy resin, a method of curing a predetermined epoxy resin with a curing agent can be mentioned. As for this predetermined epoxy resin, in addition to the method of using an epoxy resin having the structural units (a) and (b) as described above, it is also possible to use a method of using a combination of an epoxy resin having at least one of the following structural units (a) or (b) with an epoxy resin having at least the other structural unit, or a method of combining an epoxy resin having the following structural unit (a) with a chain extender capable of imparting the structural unit (b) to the epoxy resin by reaction.
[0026] Examples of flexible epoxy resins having the structure shown in the above structural formula include those having the following structure:
[0027] [ka]
[0028] (wherein n=1 to 5) is an example of an epoxy resin.
[0029] Commercially available flexible epoxy resins include "EPICLON EXA-4850-150", "EPICLON EXA-4816", "EPICLON EXA-4822", and "HP-A-4860" (all trade names of DIC Corporation), "YL7175-500", and "YL7175-1000" (all trade names of Mitsubishi Chemical Corporation), etc.
[0030] The number average molecular weight of the flexible epoxy resin is preferably 400 or more, more preferably 600 or more, from the viewpoint of flexibility. The upper limit of the number average molecular weight of the flexible epoxy resin is not particularly limited, but is preferably 3000 or less, more preferably 2000 or less, from the viewpoint of workability and viscosity. In one embodiment of the present invention, the number average molecular weight of the flexible epoxy resin is preferably 400 to 3000, more preferably 600 to 2000. The number average molecular weight of each component is measured by gel permeation chromatography (GPC) method (polystyrene equivalent). Specifically, the number average molecular weight by the GPC method is measured using "LC-9A / RID-6A" manufactured by Shimadzu Corporation as a measuring device, "Shodex K-800P / K-804L / K-804L" manufactured by Resonaq Corporation as a column, toluene or the like as a mobile phase, at a column temperature of 40°C, and can be calculated using a calibration curve of standard polystyrene.
[0031] The epoxy equivalent of the flexible epoxy resin is preferably 200 to 800 g / eq, more preferably 200 to 600 g / eq, from the viewpoints of workability and viscosity. The epoxy equivalent can be obtained based on JIS K 7236-1995.
[0032] (Solid epoxy resin) In the present invention, the term "solid" in the term "solid epoxy resin" is as described above. The solid epoxy resin is not particularly limited as long as it is solid, but it is preferable that the solid epoxy resin has an average of two or more epoxy groups per molecule. Examples of the epoxy resin include bisphenol A type epoxy resins, biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, phenol aralkyl type epoxy resins, naphthol type epoxy resins, naphthalene type epoxy resins, bisphenol F type epoxy resins, phosphorus-containing epoxy resins, bisphenol S type epoxy resins, aromatic glycidylamine type epoxy resins (e.g., tetraglycidyldiaminodiphenylmethane, triglycidyl-p-aminophenol, diglycidyl toluidine, diglycidyl aniline, etc.), alicyclic epoxy resins, aliphatic chain epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, epoxy resins having a butadiene structure, epoxy resins having a dicyclopentadiene structure, diglycidyl ethers of bisphenols, diglycidyl ethers of naphthalene diols, glycidyl ethers of phenols, and diglycidyl ethers of alcohols, as well as alkyl substituted, halogenated and hydrogenated versions of these epoxy resins. These may be used alone or in combination of two or more.
[0033] From the viewpoint of flexibility and the like, the number average molecular weight of the solid epoxy resin is preferably 200 or more, more preferably 300 or more. The upper limit of the number average molecular weight of the solid epoxy resin is not particularly limited, but from the viewpoint of workability and viscosity, it is preferably 6000 or less, more preferably 5000 or less. In one embodiment of the present invention, the number average molecular weight of the solid epoxy resin is preferably 200 to 6000, more preferably 300 to 5000.
[0034] The epoxy equivalent of the solid epoxy resin is preferably 300 to 10,000 g / eq, more preferably 400 to 8,000 g / eq, from the viewpoints of workability, viscosity, and softening point. The epoxy equivalent can be obtained based on JIS K 7236-1995.
[0035] The content of the (A) component is preferably 5% by mass or more, more preferably 20% by mass or more, based on 100% by mass of the nonvolatile components in the liquid resin composition. The upper limit of the content of the (A) component is preferably 50% by mass or less, more preferably 35% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition. In one embodiment of the present invention, the content of the (A) component is preferably 5% by mass or more and 50% by mass or less, more preferably 20% by mass or more and 35% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition. In another embodiment of the present invention, the content of the (A) component is preferably 1% by mass or more and 10% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition.
[0036] <(B) component> Component (B) has a specific surface area (hereinafter sometimes abbreviated as "SSA") of 0.30 m 2 The conductive powder of component (B) has a large specific surface area, which results in many contacts between the conductive powder particles, thereby enabling the specific resistance of the liquid resin composition to be reduced.
[0037] The specific surface area of component (B) is 0.30 m 2 / g or more, preferably 0.33m 2 / g or more, and the upper limit is not particularly limited, but from the viewpoint of not excessively increasing the viscosity of the final liquid resin composition, it is preferably 0.60 m 2 / g or less, and more preferably 0.55m 2 In one embodiment of the present invention, from the viewpoint of resistivity, dispenseability (in this specification, dispenseability means application performance such as ease of application when filling a syringe with a liquid resin composition and applying it with a dispenser), and the like, the specific surface area of the (B) component is preferably 0.30 m2 / g or more 0.60m 2 / g or less, and more preferably 0.33m 2 / g or more 0.55m 2 / g or less. In the present invention, the "specific surface area" can be measured by the BET method.
[0038] From the viewpoint of preventing the viscosity of the final liquid resin composition from being too significantly increased, the tap density of the (B) component is preferably 5.2 g / cc or less, more preferably 4.8 g / cc or less, preferably 3.0 g / cc or more, and more preferably 3.3 g / cc or more. In one embodiment of the present invention, the tap density of the (B) component is preferably 3.0 g / cc or more and 5.2 g / cc or less, more preferably 3.3 g / cc or more and 4.8 g / cc or less. In the present invention, the "tap density" can be measured according to JIS Z2512.
[0039] The particle size of component (B) is preferably 1 to 30 μm, more preferably 1 to 20 μm, taking into consideration the handleability of the resulting liquid resin composition, the occurrence of nozzle clogging when applying with a dispenser, etc. In the present invention, the "particle size" is measured using a laser diffraction particle size distribution meter, taking the particle size (median size) at a relative particle amount of 50% (50% of the total particle amount, the particle size at the midpoint of the particle amount when the total particle amount and particle size are graphed).
[0040] <(C) component> Component (C) has a specific surface area of 0.25 m 2 The conductive powder of component (C) has a small specific surface area, so that the conductivity can be increased without a significant increase in viscosity.
[0041] The specific surface area of component (C) is 0.25 m 2 / g or less, preferably 0.23m 2 The lower limit is not particularly limited, but from the viewpoint of the occurrence of nozzle clogging when applying with a dispenser, it is preferably 0.05 m 2 / g or more, more preferably 0.08m 2 In one embodiment of the present invention, from the viewpoints of resistivity, dispenseability, and the like, the specific surface area of component (C) is preferably 0.05 m 2 / g or more 0.25m 2 / g or less, more preferably 0.08m 2 / g or more 0.23m 2 / g or less.
[0042] From the viewpoint of viscosity, the tap density of the (C) component is preferably 5.7 g / cc or more, more preferably 5.9 g / cc or more, and preferably 9.0 g / cc or less, and more preferably 8.9 g / cc or less. In one embodiment of the present invention, the tap density of the (C) component is preferably 5.7 g / cc or more and 9.0 g / cc or less, and more preferably 5.9 g / cc or more and 8.9 g / cc or less.
[0043] The particle size of component (C) is preferably 1 to 30 μm, and more preferably 1 to 20 μm, taking into consideration the handleability of the resulting liquid resin composition and the occurrence of nozzle clogging when applied with a dispenser.
[0044] From the viewpoint of resistance value and viscosity, the total content of the (B) component and the (C) component is preferably 60% by mass or more, more preferably 63% by mass or more, and preferably 80% by mass or less, and more preferably 70% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition. In one embodiment of the present invention, the total content of the (B) component and the (C) component is preferably 60% by mass or more and 80% by mass or less, more preferably 63% by mass or more and 70% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition.
[0045] The mass ratio of the (B) component to the (C) component in the liquid resin composition is preferably 1:9 to 9:1, and more preferably 3:7 to 7:3, from the viewpoint of viscosity.
[0046] Examples of the conductive powder of components (B) and (C) include silver powder, copper powder, nickel powder, copper powder having a silver layer on its surface, and silica powder having a silver layer on its surface. From the viewpoints of conductivity and workability, silver powder is preferred.
[0047] The conductive powder of components (B) and (C) is not particularly limited in shape, and known shapes such as spheres, flakes, needles, dendrites, rods, etc. can be used, but flakes are preferred from the viewpoint of obtaining good resistivity. Flakes are plate-like in shape (see JIS Z2500:2000), and are also called scale-like because they are thin and plate-like like scales.
[0048] The conductive powders of both components (B) and (C) may be of one type or a mixture of two or more different types of conductive powders. Conductive powders of the same shape may be used, or conductive powders of different shapes may be used in combination.
[0049] <(D) component> The component (D) is a latent curing agent. The latent curing agent is not particularly limited as long as it can cure the epoxy resin of the component (A) and the epoxy resin of the optional component (A') described below, and examples of the latent curing agent include modified polyamines such as tertiary amino group-containing modified polyamines, urea bond-containing modified polyamines, and imidazole-containing modified polyamines.
[0050] In the present invention, the term "latent curing agent" refers to a curing agent that does not react with functional groups such as epoxy groups under normal storage conditions (such as room temperature and visible light) of the liquid resin composition of the present invention, but exhibits reactive activity toward functional groups by heat or light, and can cure the liquid resin composition. These may be used alone or in combination of two or more. From the viewpoint of adhesion, it is preferable to use one or more selected from the group consisting of tertiary amino group-containing modified polyamines, urea bond-containing modified polyamines, and imidazole-containing modified polyamines, and it is more preferable to use a urea bond-containing modified polyamine and an imidazole-containing modified polyamine in combination.
[0051] In this specification, the tertiary amino group-containing modified polyamine is a compound that has a polymer structure containing an aliphatic tertiary amine other than imidazole, in which the active amine forms a stabilized structure with an epoxy resin and / or a phenolic resin and can be used as a latent curing agent. Examples of the tertiary amino group-containing modified polyamine include EH4380S, EH3616S, EH5001P, and EH4357S manufactured by ADEKA CORPORATION.
[0052] The imidazole group-containing modified polyamine is a compound that has a polymer structure containing imidazole, in which an active amine forms a stabilized structure with an epoxy resin and / or a phenolic resin and can be used as a latent curing agent. Examples of the imidazole group-containing modified polyamine include PN-23, PN-H, and PN-40 manufactured by Ajinomoto Fine-Techno Co., Ltd., EH4346S manufactured by ADEKA Co., Ltd., FXR-1121 manufactured by T&K TOKA Co., Ltd., and Sanmide LH210 manufactured by Air Products Japan Co., Ltd.
[0053] The urea bond-containing modified polyamine is a compound in which an active amine has a stabilized structure due to the urea bond formed with an isocyanate resin, and can be used as a latent curing agent. Examples of the urea bond-containing modified polyamine include FXR-1020 and FXR-1081 manufactured by T&K TOKA Corporation.
[0054] From the viewpoint of degree of cure and storage stability, the content of the (D) component is preferably 10% by mass or more, more preferably 15% by mass or more, and preferably 30% by mass or less, and more preferably 25% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition. In one embodiment of the present invention, the content of the (D) component is preferably 10% by mass or more and 30% by mass or less, more preferably 15% by mass or more and 25% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition.
[0055] The liquid resin composition of the present invention may contain components other than the components (A) to (D) as long as the effects of the present invention are not impaired.
[0056] (Epoxy resin with a viscosity of 50 mPa·s or more and less than 15 Pa·s at 25°C (hereinafter referred to as "Component (A')")) The liquid resin composition of the present invention preferably contains an epoxy resin having a viscosity of 50 mPa·s or more and less than 15 Pa·s at 25°C. By blending component (A'), it is possible to reduce the viscosity and thixotropy of the final liquid resin composition. In the present invention, "a viscosity of 50 mPa·s or more at 25°C" means that the viscosity is 50 mPa·s or more when measured at 25°C and a rotation speed of 20 rpm using an E-type viscometer.
[0057] There are no particular limitations on the epoxy resin of component (A') so long as it has a viscosity at 25°C of 50 mPa·s or more and less than 15 Pa·s, but it is preferable for it to have an average of two or more epoxy groups per molecule. Examples of the epoxy resin include bisphenol A type epoxy resins, biphenyl type epoxy resins, biphenyl aralkyl type epoxy resins, phenol aralkyl type epoxy resins, naphthol type epoxy resins, naphthalene type epoxy resins, bisphenol F type epoxy resins, phosphorus-containing epoxy resins, bisphenol S type epoxy resins, aromatic glycidylamine type epoxy resins (e.g., tetraglycidyldiaminodiphenylmethane, triglycidyl-p-aminophenol, diglycidyl toluidine, diglycidyl aniline, etc.), alicyclic epoxy resins, aliphatic chain epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, epoxy resins having a butadiene structure, epoxy resins having a dicyclopentadiene structure, diglycidyl ethers of bisphenols, diglycidyl ethers of naphthalene diols, glycidyl ethers of phenols, and diglycidyl ethers of alcohols, as well as alkyl substituted, halogenated and hydrogenated versions of these epoxy resins. These may be used alone or in combination of two or more.
[0058] The epoxy resin of component (A') has a viscosity of 50 mPa·s or more and less than 15 Pa·s, preferably less than 12 Pa·s, and preferably 100 mPa·s or more. In one embodiment of the present invention, an epoxy resin having a viscosity at 25°C of 100 mPa·s or more and less than 12 Pa·s is more preferred.
[0059] From the viewpoint of volatility, the number average molecular weight of the epoxy resin of component (A') is preferably 150 or more, more preferably 200 or more, and from the viewpoint of viscosity, it is preferably 1000 or less, more preferably 800 or less. In one embodiment of the present invention, the number average molecular weight of the epoxy resin of component (A') is preferably 150-1000, more preferably 200-800.
[0060] The component (A') may be a commercially available product, such as "ZX-1059" and "ZX-1542" manufactured by Nippon Steel Chemical & Material Co., Ltd., or "EP-4088S" manufactured by ADEKA Corporation.
[0061] From the viewpoints of workability and viscosity, the content of the (A') component is preferably 50% by mass or more and 95% by mass or less, and more preferably 60% by mass or more and 90% by mass or less, relative to 100% by mass of the total of the (A) and (A') components contained in the liquid resin composition. That is, the mass ratio of the (A) component to the (A') component in the liquid resin composition is preferably 5:95 to 50:50, and more preferably 10:90 to 40:60.
[0062] The liquid resin composition of the present invention may or may not contain a resin and / or an organic solvent having a viscosity of less than 50 mPa·s at 25°C within a range in which the effects of the present invention can be achieved. In the present invention, "a viscosity of less than 50 mPa·s at 25°C" means that the viscosity measured at 25°C and 50 rpm using an E-type viscometer is less than 50 mPa·s. While such a component can reduce the viscosity and thixotropy of the liquid resin composition, like component (A'), there are cases in which the impact of volatilization on the working environment and the impact on the quality of parts using the adhesive are problems. In the present invention, it is possible to reduce the viscosity and thixotropy of the conductive adhesive by using or not using a resin and / or an organic solvent having a viscosity of less than 50 mPa·s at 25°C within a range in which such effects do not occur. When the liquid resin composition contains a resin and / or an organic solvent having a viscosity of less than 50 mPa·s at 25°C, the total content of the resin and the organic solvent having a viscosity of less than 50 mPa·s at 25°C is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less, based on 100% by mass of the liquid resin composition (including volatile components). That is, the total content of the resin and the organic solvent having a viscosity of less than 50 mPa·s at 25°C in the liquid resin composition of the present invention is preferably 0 to 5% by mass, more preferably 0 to 3% by mass, and even more preferably 0 to 1% by mass, based on 100% by mass of the liquid resin composition (including volatile components). In particular, the organic solvent is preferably 3% by mass or less, more preferably 1% by mass or less, and even more preferably 0% by mass, based on 100% by mass of the liquid resin composition (including volatile components).
[0063] When using a resin with a viscosity of less than 50 mPa s at 25°C, it is preferable to use one that functions as a reactive diluent, preferably one that has 1 to 3 epoxy groups in the molecule, and more preferably one that has 1 to 2 epoxy groups in the molecule.
[0064] When an organic solvent is used, the organic solvent is not particularly limited, and examples thereof include ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, and γ-butyrolactone; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, and anisole; alcohol-based solvents such as methanol, ethanol, propanol, butanol, and ethylene glycol; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, meth Examples of the organic solvent include ether ester solvents such as methyl oxypropionate; ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate; ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butyl carbitol); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone; sulfoxide solvents such as dimethyl sulfoxide; nitrile solvents such as acetonitrile and propionitrile; aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane; and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. The organic solvent may be used alone or in combination of two or more.
[0065] <Metal powder other than components (B) and (C)> The liquid resin composition of the present invention may contain a metal powder other than the components (B) and (C), i.e., a metal powder other than a conductive powder (also referred to as "component (E)"). Preferred examples of the metal powder other than a conductive powder include tin powder, zinc powder, and aluminum powder. The shape of component (E) is not particularly limited, and known shapes such as spherical, flake, and needle shapes can be used, but spherical shapes are preferred from the viewpoint of viscosity.
[0066] The particle size of the component (E) is preferably 1 to 15 μm, and more preferably 1 to 10 μm, taking into consideration the handleability of the resulting liquid resin composition and the occurrence of nozzle clogging when applied with a dispenser.
[0067] The specific surface area of component (E) is preferably 0.1 to 1.5 m from the viewpoints of resistivity, dispensability, etc. 2 / g, more preferably 0.1 to 1.0 m 2 / g.
[0068] From the viewpoint of suppressing contact resistance under high temperature and high humidity, the content of the (E) component is preferably 3% by mass or more, more preferably 5% by mass or more, and preferably 20% by mass or less, and more preferably 15% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition. In one embodiment of the present invention, the content of the (E) component is preferably 3% by mass or more and 20% by mass or less, more preferably 5% by mass or more and 15% by mass or less, based on 100% by mass of the nonvolatile components in the liquid resin composition.
[0069] Other additives that can be added to the liquid resin composition of the present invention include core-shell polymers, storage stabilizers, silane coupling agents, thixotropic agents such as aerosil, and corrosion inhibitors such as benzimidazole.
[0070] By blending the core-shell polymer, the adhesiveness of the obtained liquid resin composition can be improved, and stress relaxation properties can be imparted to the obtained liquid resin composition. The core-shell polymer is a polymer having a core portion and a shell portion, and is obtained by polymerizing a relatively hard shell layer prepared from a (meth)acrylic acid ester, an aromatic vinyl, a vinyl cyanide, an epoxy alkyl vinyl ether, an unsaturated acid derivative, a (meth)acrylamide derivative, and / or a maleimide derivative, etc., on a relatively soft core portion prepared from a rubber elastomer prepared from a diene monomer, a (meth)acrylic acid ester monomer, and / or a vinyl monomer, etc., a polysiloxane rubber elastomer, or a mixture thereof. Available core-shell polymers include MX120, MX125, MX130, MX135, MX960, and MX965 manufactured by Kaneka Corporation, RKB3040 and RKB1133 manufactured by Resinous Chemicals Co., Ltd., JF-001 and JF-003 manufactured by Mitsubishi Rayon Co., Ltd., and F351G manufactured by Ganz Chemicals Co., Ltd. The core-shell polymer may be a known one in a powder state or one dispersed in an epoxy resin. These may be used alone in a powder state or in a dispersed state, or may be used in combination with a powder state and a dispersed state. The core-shell polymer may be used in an amount of preferably 15 to 30 parts by weight, more preferably 17 to 30 parts by weight, per 100 parts by weight of component (A).
[0071] By blending a storage stabilizer, the pot life of the obtained liquid resin composition can be secured. As the storage stabilizer, for example, borate esters such as trimethyl borate and triethyl borate, titanate ester compounds, aluminate compounds, zirconate compounds, isocyanate compounds, carboxylic acids, acid anhydrides, and mercapto organic acids can be used. These may be used alone or in combination of two or more. The storage stabilizer can be used in an amount of preferably 0.5 to 1.2 parts by weight, more preferably 0.7 to 1 part by weight, per 100 parts by weight of component (A).
[0072] In consideration of the use of the liquid resin composition of the present invention in which the composition is allowed to soak into gaps in an adherend for bonding, the liquid resin composition of the present invention has a viscosity at 25°C of less than 20 Pa·s, preferably 15 Pa·s or less, preferably 1 Pa·s or more, more preferably 5 Pa·s or more, and even more preferably 7 Pa·s or more. In one embodiment of the present invention, the viscosity of the liquid resin composition at 25°C is preferably 1 Pa·s or more and less than 20 Pa·s, more preferably 5 Pa·s or more and less than 20 Pa·s, and even more preferably 7 Pa·s or more and 15 Pa·s or less. In the present invention, the "viscosity of the liquid resin composition at 25°C" is a value measured using an E-type viscometer at 25°C and a rotation speed of 10 rpm.
[0073] In consideration of application properties, the liquid resin composition of the present invention preferably has a thixotropic index (TI) value at 25° C. of 1.0 or more and less than 3.5, more preferably 1.0 or more and less than 3.0. In the present invention, the "thixotropic index (TI) value at 25° C." is measured by the method described in the following examples.
[0074] The liquid resin composition of the present invention can be produced by mixing the above-mentioned components in a conventional manner and dispersing them uniformly using a planetary mixer, a roll mill or the like to form a paste.
[0075] The liquid resin composition of the present invention can be suitably used as a conductive adhesive in the assembly of electronic components and the like and in the method of connecting them to substrates, particularly in the assembly of compact camera modules for mobile phones and the like. EXAMPLES
[0076] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples, and can be implemented with appropriate modifications within the scope of the above and below spirit, all of which are included in the technical scope of the present invention.
[0077] [Preparation of one-liquid resin composition] The components were mixed according to the blending ratio shown in Table 1 to prepare liquid resin compositions according to Examples 1 to 9 and Comparative Examples 1 to 4. In Table 1, the blending amount of each component means parts by mass. Specifically, the high-viscosity liquid epoxy resin (A) component and the liquid epoxy resin (A') component shown in Table 1 were weighed into a dedicated plastic container. If the high-viscosity liquid epoxy resin (A) component was a highly viscous liquid and difficult to handle, it was heated in a constant temperature bath at 60°C for more than 1 hour before use. Then, using a planetary centrifugal mixer, Awatori Rentaro (Thinky Corporation: ARE-310), the mixture was thoroughly mixed at room temperature of 25°C at 2000 rpm for about 30 seconds to 1 minute. The latent curing agent (D) component was added thereto, and the mixture was thoroughly mixed at room temperature of 25°C at 2000 rpm for about 30 seconds to 1 minute using a planetary centrifugal mixer. Finally, the mixture was degassed for 2 minutes at 900 rpm under vacuum (pressure set to 0) using an automatic planetary centrifugal mixer, Kyoritsu Seiki Co., Ltd. HM-200W, to obtain a master batch of the desired liquid resin composition. Thereafter, an appropriate amount of the master batch was weighed out, and the corresponding amounts of silver powder (B), (C) and other metal powder (E) were added, and the mixture was thoroughly mixed for about 30 seconds to 1 minute at 2000 rpm using a planetary centrifugal mixer at room temperature of 25° C. Finally, the mixture was degassed for 2 minutes at 900 rpm under vacuum (pressure set to 0) using a Kyoritsu Seiki Co., Ltd. automatic planetary centrifugal mixer and degassing machine HM-200W to obtain the desired liquid resin composition.
[0078] The details of the materials used are as follows: [High viscosity liquid epoxy resin; component (A)] HP-A-4860: DIC Corporation, epoxy equivalent 400g / eq, viscosity at 25℃ 1400Pa·s, number average molecular weight 800 EXA-4850-150: DIC Corporation, epoxy equivalent 450g / eq, viscosity at 25℃ 15Pa·s, number average molecular weight 900 [Liquid epoxy resin; component (A')] ZX-1059: Manufactured by Nippon Steel Chemical & Material Co., Ltd., bisphenol A type (BPA type) / bisphenol F type (BPF type) epoxy resin, epoxy equivalent 165g / eq, viscosity at 25℃ 2Pa·s, number average molecular weight 330 EP-4088S: ADEKA Corporation, dicyclopentadiene type epoxy resin, epoxy equivalent 170g / eq, viscosity at 25℃ 225mPa·s, number average molecular weight 460 ZX-1542: Nippon Steel Chemical & Material Co., Ltd., trimethylolpropane triglycidyl ether, epoxy equivalent 130g / eq, viscosity at 25℃ 60mPa·s, number average molecular weight 390 [SSA0.30m 2 / g or more silver powder; (B) component] SSA0.60m 2 / g Silver powder: Tap density 4.4g / cc, particle size 7.0μm SSA0.31m 2 / g Silver powder: Tap density 5.1g / cc, particle size 8.2μm [SSA0.25m 2 / g or less silver powder; (C) component] SSA0.24m 2 / g Silver powder: Tap density 5.8g / cc, particle size 8.9μm SSA0.08m 2 / g Silver powder: Tap density 6.0g / cc, particle size 20.1μm [Latent hardener; component (D)] PN-H: Ajinomoto Fine-Techno Co., Ltd., product name "Amicure", imidazole group-containing modified polyamine [Other metal powders; component (E)] Zinc powder: manufactured by Hakusui Tech Co., Ltd., product name "Zinc Powder R Powder", particle size 5.2 μm, SSA 0.25 m 2 / g
[0079] [Measurement of viscosity of liquid epoxy resin] The temperature of the liquid epoxy resin was kept at 25°C (±2°C) and the viscosity (Pa s) was measured using an E-type viscometer (Toki Sangyo Co., Ltd. "RE-85L", 1°34' x R24 rotor) with a measurement sample of 1.2 ml, a rotation speed of 20 rpm, and measurement time of 2 minutes. [Evaluation of Viscosity and Thixotropic Index (TI) Value of Each Liquid Resin Composition] The temperature of each liquid resin composition obtained in the Examples and Comparative Examples was kept at 25°C (±2°C), and the viscosity (Pa s) was measured using an E-type viscometer (Toki Sangyo Co., Ltd. "RE-85U", 3° x R9.7 rotor) with 0.4 ml of the measurement sample at rotation speeds of 1 rpm and 10 rpm for 2 minutes. The TI value was then calculated as follows. [TI value] = [Viscosity measured at 1 rpm] / [Viscosity measured at 10 rpm] [Evaluation of resistivity value] A 120 mm line with a width of 2 mm and a thickness of approximately 80 μm was bar-coated on an FR-4 substrate with the liquid resin compositions of the Examples and Comparative Examples, and cured at 80°C for 60 minutes in a heat circulation oven (DF-610, manufactured by Yamato Scientific Co., Ltd.) to prepare a test sample for resistivity measurement. The resistance of the test sample was measured in four-terminal mode at a distance of 100 mm using a digital multimeter (R6552 manufactured by Advantest Corporation), and the resistivity (Ω·cm) was calculated.
[0080] The liquid resin compositions of the Examples and Comparative Examples were evaluated for 10 rpm viscosity, TI value, and specific resistance value according to the following criteria.
[0081] 10rpm viscosity ◎: Less than 10 Pa s ○: 10 Pa s or more and less than 15 Pa s △: 15 Pa·s or more and less than 20 Pa·s ×:20Pa·s or more
[0082] TI value ◎: Less than 2.5 ○: 2.5 or more and less than 3.0 △: 3.0 or more and less than 3.5 ×: 3.5 or higher
[0083] Resistivity value ◎:2.0×10 -3 Less than Ω cm ○:2.0×10 -3 Ω cm or more 5.0×10 -3 Less than Ω cm △:5.0×10 -3 Ω cm or more 1.0×10-2 Less than Ω cm ×:1.0×10 -2 Ω cm or more
[0084] When component (B) is filled alone, both the viscosity and the TI value, or either the viscosity or the TI value, tend to increase, whereas when component (C) is filled alone, the resistivity tends to increase significantly. On the other hand, when components (B) and (C) are used in combination at an addition ratio of 1:1 with the same mass, it is found that a liquid resin composition with a good balance of viscosity, TI value, and resistivity is obtained (comparison of Examples 1, 2, 3, and 4 with Comparative Examples 1, 2, 3, and 4).
[0085] It can be seen that by increasing the mass percentage of component (B) + component (C) in the liquid resin composition, the resistivity can be further reduced without a significant increase in viscosity (compare Example 2 with Examples 5 and 6).
[0086] It can be seen that the resistivity can be further reduced without a significant increase in viscosity by changing the addition ratio of component (B) + component (C) in the liquid resin composition (comparison between Example 2 and Example 7).
[0087] [Table 1]
[0088] Comparative example 1: SSA0.25m 2 / g or less No silver powder, Comparative Example 2: SSA 0.25m 2 / g or less No silver powder (SSA0.30m 2 / g or more) (Difference in type of silver powder) Comparative example 3: SSA0.30m 2 / g or more No silver powder, Comparative Example 4: SSA0.30m 2 / g or more without silver powder (SSA0.25m 2 / g or less) (Differences in types of silver powder) [Industrial Applicability]
[0089] The liquid resin composition of the present invention has low viscosity, low thixotropy, and low resistance (i.e., the viscosity, thixotropic index value, and resistivity value are well balanced), and is therefore useful, for example, in applications such as the assembly of electronic components and the like and a method for connecting them to substrates.
Claims
1. The following components (A) to (D): (A) one or more epoxy resins selected from liquid epoxy resins and solid epoxy resins having a viscosity of 15 Pa·s or more at 25° C.; (B) Specific surface area is 0.30 m 2 / g or more of conductive powder, (C) Specific surface area is 0.25 m 2 / g or less conductive powder, and (D) Latent hardener and having a viscosity of less than 20 Pa·s at 25°C.
2. 2. The liquid resin composition according to claim 1, having a thixotropic index (TI) value at 25° C. of 1.0 or more and less than 3.
5.
3. 2. The liquid resin composition according to claim 1, having a viscosity at 25°C of 1 Pa·s or more and less than 20 Pa·s.
4. 2. The liquid resin composition according to claim 1, wherein the content of the component (A) is from 1% by mass to 10% by mass, based on 100% by mass of non-volatile components in the liquid resin composition.
5. 2. The liquid resin composition according to claim 1, wherein component (A) is a flexible epoxy resin having (a) a bisphenol structural unit and (b) a linear hydrocarbon structural unit having 4 or more carbon atoms and / or a polyalkylene ether structural unit having 3 or more ether oxygen atoms.
6. Component (B) has a specific surface area of 0.30 m 2 / g or more 0.60m 2 The liquid resin composition according to claim 1, wherein the conductive powder has a surface area of 100 μm or less.
7. 2. The liquid resin composition according to claim 1, wherein the tap density of component (B) is 5.2 g / cc or less.
8. 2. The liquid resin composition according to claim 1, wherein the tap density of component (B) is 3.0 g / cc or more and 5.2 g / cc or less.
9. Component (C) has a specific surface area of 0.05 m 2 / g or more 0.25m 2 The liquid resin composition according to claim 1, wherein the conductive powder has a surface area of 100 μm or less.
10. 2. The liquid resin composition according to claim 1, wherein component (C) has a tap density of 5.7 g / cc or more.
11. 2. The liquid resin composition according to claim 1, wherein the tap density of component (C) is 5.7 g / cc or more and 9.0 g / cc or less.
12. 2. The liquid resin composition according to claim 1, wherein the total content of the components (B) and (C) is 60% by mass or more based on 100% by mass of the non-volatile components in the liquid resin composition.
13. 2. The liquid resin composition according to claim 1, wherein the total content of the components (B) and (C) is 60% by mass or more and 80% by mass or less based on 100% by mass of the non-volatile components in the liquid resin composition.
14. 2. The liquid resin composition according to claim 1, wherein the mass ratio of the component (B) to the component (C) in the liquid resin composition is 1:9 to 9:
1.
15. 2. The liquid resin composition according to claim 1, wherein the components (B) and (C) are silver powders.
16. 2. The liquid resin composition according to claim 1, wherein the component (D) is at least one member selected from the group consisting of a tertiary amino group-containing modified polyamine, a urea bond-containing modified polyamine, and an imidazole-containing modified polyamine.
17. 2. The liquid resin composition according to claim 1, further comprising (A') an epoxy resin having a viscosity at 25°C of 50 mPa·s or more and less than 15 Pa·s.
18. 18. The liquid resin composition according to claim 17, wherein the content of the component (A') is 50% by mass or more and 95% by mass or less, based on 100% by mass of the total of the components (A) and (A') contained in the liquid resin composition.
19. 2. The liquid resin composition according to claim 1, which contains or does not contain a resin having a viscosity of less than 50 mPa·s and / or an organic solvent, and the total content thereof is 0% by mass or more and 3% by mass or less relative to 100% by mass of the liquid resin composition (including volatile components).
Citation Information
Patent Citations
Photosensitive conductive ink and cured product of the same
JP2014142587A
Conductive adhesive
JP2015042696A
Curable resin composition, adhesive, and bonding method
JP2023129848A
Electrically conductive resin composition, material having high thermal conductivity, and semiconductor device
WO2022202505A1