Laminate, method for manufacturing laminate, optical member, and image display device

A laminate with a resin layer containing particles of varying sizes balances flexibility and hardness, addressing the trade-off in existing laminates by enhancing both properties simultaneously.

JP2024134472AInactive Publication Date: 2024-10-03NITTO DENKO CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023044789
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing laminates used in image display devices face a trade-off between flexibility and hardness, where improving flexibility to prevent cracking can lead to reduced scratch resistance, and enhancing scratch resistance can compromise flexibility.

Method used

A laminate structure is developed with a resin layer containing at least two types of particles having different number average particle diameters, with a specific diameter ratio and weight ratio, to balance flexibility and hardness.

Benefits of technology

The laminate achieves both flexibility and hardness, preventing cracking when bent while maintaining effective scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134472000001_ABST
    Figure 2024134472000001_ABST
Patent Text Reader

Abstract

To provide a laminate which achieves both flexibility and hardness.SOLUTION: A laminate 10 or 10a has a resin layer 12 formed on at least one surface of a resin base material 11, wherein the resin layer 12 contains at least two kinds of particles having different number average particle sizes in the same layer, the resin layer 12 has a number average particle size ratio (r1 / r2) of a number average particle size (r1) of particles (A) 13a having the largest number average particle size to a number average particle size (r2) of particles (B) 13b having the smallest number average particle size of 1.4 or more. The laminate contains the particles, and has a weight ratio (A:B) of particles (A) 13a to particles (B) 13b of 80:20 to 95:5.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminate, a method for manufacturing a laminate, an optical member, and an image display device. [Background technology]

[0002] 2. Description of the Related Art Among laminates used in image display devices and the like, there are those in which a resin layer is formed on the surface of a resin substrate in order to prevent scratches on the screen and the like (Patent Document 1).

[0003] Furthermore, in recent years, image display devices have become thinner than ever before, and flexible sheet-like devices have also come into practical use (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-221746 A [Patent Document 2] JP 2003-280548 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the resin layer for preventing scratches on the screen as described above may crack when bent. On the other hand, if the flexibility is improved to prevent cracks, the hardness is reduced, and it may become impossible to prevent scratches on the screen.

[0006] Therefore, an object of the present invention is to provide a laminate, a method for manufacturing a laminate, an optical member, and an image display device that achieve both flexibility and hardness. [Means for solving the problem]

[0007] In order to achieve the above object, the laminate of the present invention comprises: A resin layer is formed on at least one surface of the resin substrate, the resin layer contains at least two types of particles having different number average particle diameters within the same layer, a number average particle diameter ratio (r1 / r2) of a number average particle diameter (r1) of a particle (A) having the largest number average particle diameter among the particles to a number average particle diameter (r2) of a particle (B) having the smallest number average particle diameter among the particles is 1.4 or more; The weight ratio (A:B) of the particles (A) to the particles (B) is 80:20 to 95:5.

[0008] The method for producing the laminate of the present invention comprises the steps of: A resin layer forming step of forming the resin layer on the resin substrate, The resin layer forming step includes a coating step of applying a coating liquid for forming a resin layer onto the resin substrate, The resin layer forming coating liquid is characterized in that it contains a resin and at least two types of particles having different number average particle sizes.

[0009] The optical member of the present invention is characterized by including the laminate of the present invention.

[0010] The image display device of the present invention is characterized by including the laminate of the present invention or the optical member of the present invention. Effect of the Invention

[0011] According to the present invention, it is possible to provide a laminate, a method for manufacturing a laminate, an optical member, and an image display device that achieve both flexibility and hardness. [Brief description of the drawings]

[0012] [Figure 1] 1(a) and (b) are cross-sectional views illustrating examples of the configuration of the laminate of the present invention. [Diagram 2] 2(a) and (b) are cross-sectional views showing other examples of the structure of the laminate of the present invention. [Diagram 3] 3(a) and (b) are cross-sectional views showing still another example of the structure of the laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following description in any way.

[0014] In the present invention, unless otherwise specified, "mass %" and "weight %" may be read interchangeably, and "parts by mass" and "parts by weight" may be read interchangeably.

[0015] In the present invention, "on" or "on the surface" may refer to a state of being in direct contact with the surface or a state of being via another layer or the like.

[0016] In the present invention, the "adhesive layer" refers to a layer formed by at least one of a pressure-sensitive adhesive and an adhesive. In the present invention, unless otherwise specified, the "adhesive layer" may be an "adhesive layer" formed by a pressure-sensitive adhesive, an "adhesive layer" formed by an adhesive, or a layer containing both a pressure-sensitive adhesive and an adhesive. In addition, in the present invention, a pressure-sensitive adhesive and an adhesive may be collectively referred to as a "adhesive". In general, an agent having a relatively weak adhesive or bonding strength (e.g., an agent that allows the adherend to be peeled off again) may be called an "adhesive", and an agent having a relatively strong adhesive or bonding strength (e.g., an agent that does not allow the adherend to be peeled off again or is very difficult to peel off again) may be called an "adhesive". In the present invention, there is no clear distinction between a pressure-sensitive adhesive and an adhesive. In the present invention, there is no clear distinction between "adhesive strength" and "adhesive strength".

[0017] [1. Laminate] The cross-sectional view of FIG. 1(a) shows an example of the configuration of the laminate of the present invention. As shown in the figure, in this laminate 10, a resin layer 12 is directly laminated on one side of a resin substrate 11. In addition, the cross-sectional view of FIG. 1(b) shows another example of the configuration of the laminate of the present invention. As shown in the figure, in this laminate 10a, a resin layer 12 is directly laminated on both sides of a resin substrate 11. The resin layer 12 contains two types of particles (particles 13a, particles 13b) having different number average particle diameters. Of these, the particles 13a are particles (A) having the largest number average particle diameter, and the particles 13b are particles (B) having the smallest number average particle diameter. In addition, the number average particle diameter ratio (r1 / r2) between the number average particle diameter (r1) of the particles 13a and the number average particle diameter (r2) of the particles 13b is 1.4 or more. Furthermore, the weight ratio of the particles 13a to the particles 13b is 80:20 to 95:5. The particles having different number average particle sizes include only two types in Fig. 1, but are not limited thereto and may include, for example, three or more types. The same applies to Figs. 2 and 3 described below.

[0018] In addition, in the laminate 10b of FIG. 2(a), as shown in the figure, a resin layer 12 containing particles 13a and particles 13b is laminated on one side of a resin substrate 11 via a surface treatment layer 14. This laminate 10b is the same as the laminate 10 of FIG. 1(a) except that a surface treatment layer 14 exists between the resin substrate 11 and the resin layer 12. The surface treatment layer 14 is a layer formed by corona treatment, easy adhesion treatment, or the like. In the laminate 10c of FIG. 2(b), as shown in the figure, a resin layer 12 containing particles 13a and particles 13b is laminated on both sides of a resin substrate 11 via a surface treatment layer 14. This laminate 10c is the same as the laminate 10a of FIG. 1(b) except that a surface treatment layer 14 exists between the resin substrate 11 and each resin layer 12. The surface treatment layer 14 is a layer formed by corona treatment, easy adhesion treatment, or the like, as in FIG. 2(a).

[0019] In addition, the laminate of the present invention may or may not include other components other than the resin substrate and the resin layer. The other components are not particularly limited, and may be, for example, a surface treatment layer as shown in FIG. 2 or a tacky adhesive layer. FIG. 3 shows an example of such a laminate of the present invention. The laminate 10d of FIG. 3(a) is the same as the laminate 10 of FIG. 1(a) except that, as shown in the figure, a tacky adhesive layer 15 is provided on the surface of the resin substrate 11 opposite to the resin layer 12 in the resin substrate 11 in direct contact with the resin layer 12. The laminate 10e of FIG. 3(b) is the same as the laminate 10b of FIG. 2(a) except that, as shown in the figure, a tacky adhesive layer 15 is provided on the surface of the resin substrate 11 opposite to the resin layer 12 containing the particles 13a and particles 13b via a surface treatment layer 14. However, the present invention is not limited thereto, and for example, other components may be present between the tacky adhesive layer 15 and the resin substrate 11 or the surface treatment layer 14. The other components are not particularly limited, and may be, for example, an optical functional layer. The optical functional layer is not particularly limited, and may be, for example, an optical functional layer used in a general optical film, such as a microlens film, a prism film, a diffusion film, a polarizing reflective film, a polarizing film, a retardation film, or a high refractive index layer.

[0020] As described above, the laminate of the present invention has a resin layer formed on at least one surface of the resin substrate. Examples of the resin substrate include polyester-based polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose, polycarbonate-based polymers, and acrylic polymers such as polymethyl methacrylate. Examples of the material for forming the resin substrate include styrene-based polymers such as polystyrene and acrylonitrile-styrene copolymers, olefin-based polymers such as polyethylene, polypropylene, polyolefins having a cyclic or norbornene structure, ethylene-propylene copolymers, vinyl chloride-based polymers, and amide-based polymers such as nylon and aromatic polyamide. Examples of the material for forming the resin substrate include imide-based polymers, sulfone-based polymers, polyethersulfone-based polymers, polyetheretherketone-based polymers, polyphenylene sulfide-based polymers, vinyl alcohol-based polymers, vinylidene chloride-based polymers, vinyl butyral-based polymers, arylate-based polymers, polyoxymethylene-based polymers, epoxy-based polymers, and blends of the above polymers. The resin substrate may or may not have light transmittance.

[0021] The laminate of the present invention can be used as a protective film for a polarizing plate, for example. In this case, the resin substrate is preferably a film formed from triacetyl cellulose, polycarbonate, an acrylic polymer, a polyolefin having a cyclic or norbornene structure, or the like. In the present invention, the resin substrate may be a polarizer itself. With such a configuration, a protective layer made of TAC or the like is not required, and the structure of the polarizing plate can be simplified, so that the number of manufacturing steps for the polarizing plate or the image display device can be reduced, and production efficiency can be improved. With such a configuration, the polarizing plate can be made thinner. In addition, when the resin substrate is a polarizer, the resin layer plays the role of a conventional protective layer. With such a configuration, the laminate also functions as a cover plate attached to the surface of a liquid crystal cell.

[0022] The resin substrate may be, for example, a substrate having at least one surface subjected to a surface treatment such as a corona treatment, an easy-adhesion treatment, etc. The surface treatment may be, for example, performed before forming a resin layer, or may be performed in the same process as the step of forming a resin layer (resin layer forming step).

[0023] The thickness of the resin substrate is not particularly limited, but is preferably in the range of 10 to 500 μm, more preferably in the range of 20 to 300 μm, and most preferably in the range of 30 to 200 μm, in consideration of, for example, strength, workability such as handleability, thin layer property, etc. When the resin substrate has optical transparency, the refractive index is not particularly limited, but is, for example, in the range of 1.30 to 1.80 or 1.40 to 1.70.

[0024] The thickness of the resin layer (hereinafter sometimes simply referred to as "film thickness") may be, for example, 1 μm or more, 1.5 μm or more, 2 μm or more, 2.5 μm or more, or 3 μm or more, or may be 6 μm or less, 5 μm or less, or 4 μm or less.

[0025] As described above, the laminate of the present invention contains at least two types of particles having different number average particle diameters in the same layer. The types of particles may be, for example, only two types, or may be, for example, three, four, five or more types.

[0026] As described above, the laminate of the present invention contains particles in the resin layer, the number average particle diameter ratio (r1 / r2) of the number average particle diameter (r1) of the particle (A) having the largest number average particle diameter to the number average particle diameter (r2) of the particle (B) having the smallest number average particle diameter being 1.4 or more. The number average particle diameter ratio (r1 / r2) may be, for example, 2.0 or more, 2.3 or more, or 2.6 or more, or may be, for example, 25 or less, 20 or less, 15 or less, 10 or less, 6.0 or less, 5.0 or less, 4.0 or less, or 3.0 or less.

[0027] As described above, in the laminate of the present invention, the weight ratio (A:B) of the particles (A) to the particles (B) is 80:20 to 95:5. The weight ratio (A:B) may be, for example, 81:19 to 94:6.

[0028] The filling rate (wt%) of the particles with respect to the entire resin layer may be, for example, 60 wt% or more and 65 wt% or less as described above. The filling rate (wt%) may be, for example, 62 wt% or more and 64 wt% or less.

[0029] The number average particle diameter of the particles (A) may be, for example, 35 nm or more and 150 nm or less, as described above. The upper limit of the number average particle diameter of the particles (A) may be, for example, 140 nm or less, 130 nm or less, 120 nm or less, 110 nm or less, or 100 nm or less, and the lower limit may be, for example, 40 nm or more, 45 nm or more, 50 nm or more, 55 nm or more, 60 nm or more, or 70 nm or more. In addition, the particle size distribution showing the variation in particle size of the particles (A) is not particularly limited, and for example, particles having a particle diameter of 45 μm to 150 μm are 50 to 99.9 wt%, 80 to 99.8 wt%, or 90 to 99.7 wt%, or particles having a particle diameter of 45 μm to 150 μm are 0.1 to 50 wt%, 0.2 to 20 wt%, or 0.3 to 10 wt%. The particle size distribution can be measured, for example, by a particle size distribution evaluation device or an electron microscope.

[0030] The number average particle diameter of the particles (B) may be, for example, 6 nm or more and 25 nm or less, as described above. The upper limit of the number average particle diameter of the particles (B) may be, for example, 20 nm or less, 15 nm or less, or 10 nm or less, and the lower limit may be, for example, 8 nm or more, 9 nm or more, or 10 nm or more. The particle size distribution showing the variation in particle size of the particles (B) is not particularly limited, and for example, particles with a particle size of 6 μm to 14 μm are 50 to 99.9 wt%, 80 to 99.8 wt%, or 90 to 99.7 wt%, or particles with a particle size of 14 μm to 25 μm are 0.1 to 50 wt%, 0.2 to 20 wt%, or 0.3 to 10 wt%.

[0031] In the present invention, the number-average particle diameter of the particles (A) and (B) can be measured, for example, by the Coulter counting method. For example, a particle size distribution measuring device using a pore electrical resistance method (product name: Coulter Multisizer, manufactured by Beckman Coulter, Inc.) is used to measure the number and volume of the particles by measuring the electrical resistance of the electrolyte equivalent to the volume of the particles when the particles pass through the pores, and the number-average particle diameter is calculated.

[0032] In addition, in the present invention, the number-average particle diameter can also be measured by observing the cross-section of the particle using a transmission electron microscope (TEM). For example, the diameter of the particle can be measured from the cross-section of the particle included in the observation image obtained by TEM observation, and the measured average value can be regarded as the number-average particle diameter. In this case, if the number-average particle diameter of the particles included in a rectangular range of 0.58 μm×0.33 μm at any point in the TEM observation image satisfies the number-average particle diameter, it is deemed to satisfy the condition of the number-average particle diameter in the present invention. More specifically, for example, it can be measured by the measurement method described in the examples below.

[0033] The number average particle diameter in the present invention may be any number average particle diameter obtained by either the Coulter count method or the TEM observation method, as long as the number average particle diameter falls within the numerical range of the number average particle diameter in the present invention.

[0034] The resin layer may be formed, for example, as described above, by a copolymer of an oligomer having a functional group and a monomer. The oligomer having a functional group is not particularly limited, but for example, a curable urethane acrylate resin is exemplified. The curable urethane acrylate resin is, for example, an aromatic polyester-based urethane acrylate. The monomer is not particularly limited, but for example, a multifunctional acrylate is exemplified. The multifunctional acrylate is, for example, a multifunctional acrylate containing pentaerythritol or trimethylolpropane.

[0035] The resin layer may be, for example, a copolymer of a curable urethane acrylate resin and a polyfunctional acrylate.

[0036] The resin layer may have, for example, a scratch hardness (pencil method) of not less than H under a load of 500 g. The scratch hardness (pencil method) can be tested, for example, by the method described in the examples below.

[0037] The resin layer may have a flexibility of, for example, 2 mmφ or less. The flexibility can be tested, for example, by the method described in the Examples below.

[0038] In the laminate of the present invention, at least one of the particles (A) and the particles (B) may be an inorganic particle, as described above. For example, both the particles (A) and the particles (B) may be inorganic particles.

[0039] The inorganic particles may be, for example, silicon oxide particles as described above. The silicon oxide particles may be, for example, silica particles (silicon dioxide particles). The inorganic particles may be, for example, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles, calcium sulfate particles, etc. These inorganic particles may be used alone or in combination of two or more kinds.

[0040] In the case where particles other than the inorganic particles are included, for example, organic particles may be included. Examples of the organic particles include polymethyl methacrylate resin powder (PMMA particles), silicone resin powder, polystyrene resin powder, polycarbonate resin powder, acrylic styrene resin powder, benzoguanamine resin powder, melamine resin powder, polyolefin resin powder, polyester resin powder, polyamide resin powder, polyimide resin powder, and polyethylene fluoride resin powder. These organic particles may be used alone or in combination of two or more kinds.

[0041] The laminate of the present invention may have a tacky adhesive layer formed on at least one surface of the resin substrate, as described above. The tacky adhesive or adhesive forming the tacky adhesive layer is not particularly limited, and for example, a general tacky adhesive or adhesive can be used. Examples of the tacky adhesive or adhesive include polymer adhesives such as acrylic, vinyl alcohol, silicone, polyester, polyurethane, and polyether adhesives, and rubber adhesives. Examples of the tacky adhesive include adhesives composed of water-soluble crosslinking agents of vinyl alcohol polymers such as glutaraldehyde, melamine, and oxalic acid. Examples of the tacky adhesive include the tacky adhesives described above. These tacky adhesives and adhesives may be used alone or in combination (for example, mixed, laminated, etc.). The thickness of the tacky adhesive layer is not particularly limited, and is, for example, 0.1 to 100 μm, 5 to 50 μm, 10 to 30 μm, or 12 to 25 μm.

[0042] [2. Manufacturing method of laminate] As described above, the method for producing a laminate of the present invention includes a resin layer forming step of forming the resin layer on the resin substrate, and the resin layer forming step includes a coating step of applying a coating liquid for forming a resin layer onto the resin substrate.

[0043] In the coating step, for example, a coating method such as a fountain coating method, a die coating method, a spray coating method, a comma coating method, a gravure coating method, a roll coating method, or a bar coating method can be used.

[0044] In the method for producing the laminate of the present invention, for example, as described above, the resin layer forming step may further include a coating film forming step of drying the applied resin layer forming coating liquid to form a coating film. The drying may be, for example, natural drying, air drying by blowing air, heat drying by hot air, oven, infrared rays, or the like, or a combination of these methods.

[0045] The drying temperature in the coating film forming step may be, for example, 30° C. or more, 40° C. or more, 50° C. or more, 60° C. or more, 70° C. or more, 80° C. or more, 90° C. or more, or 100° C. or more, and may be 200° C. or less, 190° C. or less, 180° C. or less, 170° C. or less, 160° C. or less, 150° C. or less, 140° C. or less, 135° C. or less, 130° C. or less, 120° C. or less, or 110° C. or less. The drying time is not particularly limited, and may be, for example, 30 seconds or more, 40 seconds or more, 50 seconds or more, or 60 seconds or more, and may be 150 seconds or less, 130 seconds or less, 110 seconds or less, or 90 seconds or less.

[0046] As described above, in the method for producing a laminate of the present invention, the resin layer forming coating liquid contains a resin and at least two kinds of particles having different number average particle diameters. The resin may have, for example, an oligomer and a monomer having a functional group. The oligomer and the monomer having a functional group are, for example, the same as those forming the resin layer in the above embodiment.

[0047] The resin layer forming coating liquid may further contain a dilution solvent. Examples of the dilution solvent (hereinafter, sometimes simply referred to as "solvent") include alcohols such as methanol, ethanol, isopropyl alcohol (IPA), butanol, t-butyl alcohol (TBA), and 2-methoxyethanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclopentanone; esters such as methyl acetate, ethyl acetate, and butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; glycols such as ethylene glycol and propylene glycol; cellosolves such as ethyl cellosolve and butyl cellosolve; aliphatic hydrocarbons such as hexane, heptane, and octane; and aromatic hydrocarbons such as benzene, toluene, and xylene. In addition, for example, the solvent may contain a hydrocarbon solvent and a ketone solvent. The hydrocarbon solvent may be, for example, an aromatic hydrocarbon. The aromatic hydrocarbon may be, for example, at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene, ethylbenzene, and benzene. The ketone solvent may be, for example, at least one selected from the group consisting of cyclopentanone, acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, cyclohexanone, isophorone, and acetophenone.

[0048] In the method for producing the laminate of the present invention, for example, the resin layer forming step may further include a curing step of curing the coating film as described above. The curing step may be, for example, a curing step using heat, light (ultraviolet rays, etc.), or an electron beam. When the curing step is ultraviolet curing, the irradiation amount of the energy ray source is, for example, 50 to 500 mJ / cm as an integrated exposure amount at an ultraviolet wavelength of 365 nm. 2 The irradiation dose is preferably 50 mJ / cm. 2 If the curing rate is 500 mJ / cm or more, the curing process will proceed sufficiently and the hardness of the resin layer formed will tend to be high. 2If the radiation intensity is less than 100 kV, the resin layer formed can be prevented from being colored. When the curing step is performed by electron beam curing, the radiation dose is preferably, for example, 5 to 50 kGy, or 5 to 40 kGy, so as not to deteriorate or color the resin substrate. The acceleration voltage of the electron beam is preferably 100 to 3000 kV, or 150 to 300 kV.

[0049] In the method for producing a laminate of the present invention, for example, at least one type of particles among the particles may be inorganic particles. Also, for example, all of the particles among the particles may be inorganic particles. The inorganic particles are, for example, the same as those in the case where the particles contained in the resin layer of the above embodiment are inorganic particles.

[0050] In the case where the resin layer contains particles other than the inorganic particles, the resin layer may contain, for example, organic particles. The organic particles are, for example, the same as the organic particles in the case where the resin layer contains particles other than the inorganic particles in the resin layer of the above embodiment.

[0051] The method for producing a laminate of the present invention may further include a step of forming a tacky adhesive layer on the resin substrate. Specifically, for example, the tacky adhesive layer may be formed by applying (coating) a pressure sensitive adhesive or adhesive on the resin substrate. The tacky adhesive layer may be formed on the resin substrate by bonding the tacky adhesive layer side of a substrate such as an adhesive tape having the tacky adhesive layer laminated thereon to the resin substrate. In this case, the substrate such as the adhesive tape may be left as it is or may be peeled off from the tacky adhesive layer.

[0052] [3. Optical components and image display devices] The optical member of the present invention may be, for example, a hard coat film.

[0053] The image display device of the present invention may be any type of image display device, and examples thereof include a liquid crystal display device and an organic EL display device.

[0054] The use of the laminate of the present invention is not particularly limited, and it can be used for any purpose. Examples of the uses include office automation equipment such as personal computer monitors, notebook computers, and copy machines, portable devices such as mobile phones, watches, digital cameras, personal digital assistants (PDAs), and portable game consoles, home electric appliances such as video cameras, televisions, and microwave ovens, in-vehicle equipment such as back monitors, monitors for car navigation systems, and car audio, exhibition equipment such as information monitors for commercial stores, security equipment such as surveillance monitors, and nursing and medical equipment such as nursing monitors and medical monitors. In addition, since the laminate of the present invention has both flexibility and hardness, it can also be used, for example, in foldable devices, rollable devices, and the like. EXAMPLES

[0055] Next, examples of the present invention will be described, but the present invention is not limited to the following examples.

[0056] In the following Reference Examples, Examples, and Comparative Examples, the number of parts (relative amount used) of each substance is by mass (parts by weight) unless otherwise specified.

[0057] In the following Examples and Comparative Examples, the number average particle size, film thickness, flexibility (mandrel test), and scratch hardness (pencil method) were measured by the following methods.

[0058] <Number average particle size> Measurement was performed from a TEM observation image using a TEM device. First, a sample for TEM observation was prepared from the laminate of the present invention by ultra-thin sectioning. Next, the prepared sample was dyed with a heavy metal. The cross-section of the dyed sample was observed using a TEM device (manufactured by Hitachi, Ltd., product name: HT7820) at an acceleration voltage of 100 kV, and an image was obtained in an observation field of 0.58 μm × 0.33 μm. The diameter of the particles present in the obtained image was measured and the average value was calculated, which was taken as the number-average particle diameter.

[0059] <Film thickness> The laminate of the present invention was cut with a diamond knife using a microtome (manufactured by LEICA MICROSYSTEMS Co., Ltd., product name: LEICAEM UC7) to expose the cross section to be observed. Then, the sample with the exposed cross section was coated with a metal thin film using a magnetron sputtering device (manufactured by Vacuum Device Co., Ltd., product name: MSP-20TK) under discharge conditions (atmospheric pressure: 3 Pa, plasma gas: argon, current: 10 mA, discharge time: 30 seconds), and a conductive treatment was performed to observe the cross section layer with an electron microscope. Then, a secondary electron image of the conductive treated sample was obtained at a magnification of 10,000 times using a SEM device (manufactured by Hitachi High-Tech Corporation, product name: Regulus8230). The corresponding film thickness was measured using the obtained image, and the calculation was performed.

[0060] <Flexibility (mandrel test)> Measurements were performed using a mandrel tester (manufactured by Coating Star Co., Ltd., product name: bending tester (cylindrical mandrel method) type I) based on a method conforming to JIS K 5600-5-1. The laminate of the present invention was placed in the mandrel tester with the coated surface facing outward, and an outward bending test was performed with a mandrel diameter of 2 mm. After placing the sample in the bending tester, the body was evenly bent 180° over approximately 1 to 2 seconds, then opened 180° and returned to its original state, and the bending property was evaluated by visually observing cracks and splits in the coating film.

[0061] Bendability evaluation criteria OK: No cracks or splits in the coating NG: The coating was cracked or broken.

[0062] <Scratch hardness (pencil method)> The test was conducted in accordance with JIS K 5600-5-4. Pencils of various hardness were placed on the surface of the sample at a 45° angle, and a scratch test was performed under load. The hardest pencil that did not cause a scratch was recorded as the pencil hardness.

[0063] [Example 1] <1. Preparation of Coating Liquid for Forming Resin Layer> A coating liquid for forming a resin layer of this reference example (Reference Example 1) was prepared by the following procedure.

[0064] As the resin contained in the hard coat layer forming material, 100 parts by weight of ultraviolet-curable multifunctional acrylate resin was prepared. Per 100 parts by weight of the total solid content of the resin, 180 parts by weight of particles (A) (silica particles, number average particle diameter 35 to 150 nm), 180 parts by weight of particles (B) (silica particles, number average particle diameter 6 to 25 nm), 4 parts by weight of a photopolymerization initiator (manufactured by BASF Ltd., product name: OMNIRAD2959), and 0.05 parts by weight of a leveling agent (manufactured by Kyoseisha Chemical Co., Ltd., product name: LE303) were mixed. This mixture was diluted with MIBK so that the solid content concentration was 40% by weight, and a hard coat layer forming material (coating liquid) was prepared. The number average particle diameter of the particles (A) was 35 to 150 nm, and the number average particle diameter of the particles (B) was 6 to 25 nm.

[0065] <2. Manufacturing of Laminate> The resin layer-forming coating liquid prepared in Reference Example 1 was applied onto a PET film having a thickness of 50 μm (manufactured by Toyobo Co., Ltd., product name: Lumirror (registered trademark) U-48). A bar coater was used for the coating. The hard coat layer-forming material (coating liquid) was applied onto one side of the PET film using the bar coater to form a coating film. Thereafter, the PET film on which the coating film was formed was dried in a drying oven (manufactured by Ushio Inc., product name: UVC-025616S1AGM01, No. 1209001) at 85° C. for 1 minute. Next, the resin layer surface was irradiated with UV light (accumulated light amount 230 mJ / cm 2 ). 2 ) was carried out to produce the laminate of this example. The thickness of the resin layer was 3 to 4 μm.

[0066] [Examples 2 to 6 and Comparative Examples 1 to 16] The coating liquid for forming a resin layer was prepared and the laminate was produced under the same conditions as in Example 1, except that the particle blending ratio (parts) in the above-mentioned "1. Preparation of coating liquid for forming a resin layer" was changed as shown in Table 1 below, to produce the laminates of Examples 2 to 6 and Comparative Examples 1 to 16.

[0067] [Table 1]

[0068] As shown in Table 1, in Examples 1 to 6, in which at least two kinds of particles having different number average particle diameters are contained in the same layer, the number average particle diameter ratio (r1 / r2) between the number average particle diameter (r1) of the particles (A) having the largest number average particle diameter and the number average particle diameter (r2) of the particles (B) having the smallest number average particle diameter is 1.4 or more, and the weight ratio (A:B) of the particles (A) to the particles (B) is 80:20 to 95:5, the mandrel test evaluation was good, and the scratch hardness (pencil method) test results were also good. That is, the laminates of Examples 1 to 6 were able to achieve both flexibility and hardness.

[0069] In contrast, the laminates of Comparative Examples 1 to 16, which did not satisfy the above conditions, were poor in at least one of the evaluations of the mandrel test and the scratch hardness (pencil method) test. That is, the laminates of Comparative Examples 1 to 16 could not achieve both flexibility and hardness.

[0070] <Additional Notes> A part or all of the above-described embodiments and examples may be described as follows, but is not limited to the following. (Appendix 1) A resin layer is formed on at least one surface of the resin substrate, the resin layer contains at least two types of particles having different number average particle diameters within the same layer, a number average particle diameter ratio (r1 / r2) of a number average particle diameter (r1) of a particle (A) having the largest number average particle diameter among the particles to a number average particle diameter (r2) of a particle (B) having the smallest number average particle diameter among the particles is 1.4 or more; A laminate, wherein a weight ratio (A:B) of the particles (A) to the particles (B) is 80:20 to 95:5. (Appendix 2) 2. The laminate according to claim 1, wherein a filling rate (weight %) of the particles with respect to the entire resin layer is 60 weight % or more and 65 weight % or less. (Appendix 3) 3. The laminate according to claim 1 or 2, wherein the resin layer is formed on one surface of the resin substrate. (Appendix 4) The number average particle diameter of the particles (A) is 35 nm or more and 150 nm or less, 4. The laminate according to any one of claims 1 to 3, wherein the number-average particle diameter of the particles (B) is 6 nm or more and 25 nm or less. (Appendix 5) 5. The laminate according to claim 1, wherein the resin layer is formed from a copolymer of an oligomer and a monomer having a functional group. (Appendix 6) 6. The laminate according to any one of claims 1 to 5, wherein at least one of the particles (A) and the particles (B) is an inorganic particle. (Appendix 7) 7. The laminate according to claim 6, wherein the inorganic particles are silicon oxide particles. (Appendix 8) 8. The laminate according to claim 1, wherein the resin layer is formed on one surface of the resin substrate, and an adhesive layer is formed on the other surface of the resin substrate. (Appendix 9) A resin layer forming step of forming the resin layer on the resin substrate, The resin layer forming step includes a coating step of applying a coating liquid for forming a resin layer onto the resin substrate, 9. The method for producing a laminate according to any one of claims 1 to 8, wherein the resin layer-forming coating liquid contains a resin and at least two types of particles having different number average particle diameters. (Appendix 10) The manufacturing method according to claim 9, wherein the resin layer forming step further comprises a coating film forming step of drying the applied resin layer forming coating liquid to form a coating film. (Appendix 11) 11. The method according to claim 9, wherein the resin layer forming step further comprises a curing step of curing the coating film. (Appendix 12) An optical member comprising the laminate according to any one of claims 1 to 8. (Appendix 13) 13. The optical member according to claim 12, which is a hard coat film. (Appendix 14) An image display device comprising the laminate according to any one of claims 1 to 8, or the optical member according to claim 12 or 13. (Appendix 15) 15. The image display device according to claim 14, which is a foldable display. [Industrial Applicability]

[0071] As described above, according to the present invention, it is possible to provide a laminate, a manufacturing method for a laminate, an optical member, and an image display device that have both flexibility and hardness. The use of the present invention is not particularly limited. According to the laminate of the present invention, for example, even when folded at a low angle, no cracks occur, and the surface hardness is good, so that it is particularly suitable for a hard coat film on the surface of a foldable display. Furthermore, the use of the laminate of the present invention is not limited to the optical member and image display device of the present invention, and is arbitrary, and can be used for a wide range of uses. [Explanation of symbols]

[0072] 10, 10a, 10b, 10c, 10d, 10e Laminate 11 Resin substrate 12 Resin layer 13a Particle (A) 13b Particle (B) 14 Surface treatment layer 15 Adhesive layer

Claims

1. A resin layer is formed on at least one surface of the resin substrate, the resin layer contains at least two types of particles having different number average particle diameters in the same layer, a number average particle diameter ratio (r1 / r2) of a number average particle diameter (r1) of the particles (A) having the largest number average particle diameter to a number average particle diameter (r2) of the particles (B) having the smallest number average particle diameter among the particles is 1.4 or more; A laminate, characterized in that a weight ratio (A:B) of the particles (A) to the particles (B) is 80:20 to 95:

5.

2. 2. The laminate according to claim 1, wherein a filling rate (wt %) of the particles relative to the entire resin layer is 60 wt % or more and 65 wt % or less.

3. 2. The laminate according to claim 1, wherein the resin layer is formed on one surface of the resin substrate.

4. The number average particle diameter of the particles (A) is 35 nm or more and 150 nm or less, 2. The laminate according to claim 1, wherein the number average particle diameter of the particles (B) is 6 nm or more and 25 nm or less.

5. 2. The laminate according to claim 1, wherein the resin layer is formed from a copolymer of an oligomer and a monomer having a functional group.

6. 2. The laminate according to claim 1, wherein at least one of the particles (A) and the particles (B) is an inorganic particle.

7. 7. The laminate according to claim 6, wherein the inorganic particles are silicon oxide particles.

8. 2. The laminate according to claim 1, wherein the resin layer is formed on one surface of the resin substrate, and an adhesive layer is formed on the other surface of the resin substrate.

9. A resin layer forming step of forming the resin layer on the resin substrate, The resin layer forming step includes a coating step of applying a coating liquid for forming a resin layer onto the resin substrate, 2. The method for producing a laminate according to claim 1, wherein the resin layer-forming coating liquid contains a resin and at least two types of particles having different number average particle sizes.

10. The method according to claim 9 , wherein the resin layer forming step further comprises a coating film forming step of drying the applied resin layer forming coating liquid to form a coating film.

11. The method according to claim 9 or 10, wherein the resin layer forming step further comprises a curing step of curing the coating film.

12. An optical member comprising the laminate according to claim 1.

13. The optical member according to claim 12, which is a hard coat film.

14. An image display device comprising the laminate according to claim 1 , or the optical member according to claim 12 or 13 .

15. The image display device according to claim 14, which is a foldable display.

Citation Information

Patent Citations

  • Flexible display panel

    JP2003280548A

  • Hard coat film, hard coat film laminate and image display device

    JP2008221746A