Fiber-reinforced resin composition and molding

The fiber-reinforced resin composition with a sea-island structure and specific components addresses interfacial peeling issues, enhancing mechanical properties and reducing creep strain.

JP2024134510APending Publication Date: 2024-10-03MITSUI CHEMICALS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023214009
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-20
Filing Date
2023-12-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Fiber-reinforced resin compositions with phase-separated polyolefin and polyamide are prone to interfacial peeling, leading to brittle fracture and reduced bending and tensile properties, along with increased tensile creep strain.

Method used

A fiber-reinforced resin composition comprising unmodified polyolefin, polyamide with a structural unit derived from a monomer with 10 or more carbon atoms, reinforcing fibers, and modified polyolefin, with specific mass ratios and a sea-island structure to enhance dispersibility and interfacial adhesion.

Benefits of technology

Suppresses interfacial peeling between polyolefin and polyamide, maintaining bending and tensile properties while reducing tensile creep strain, resulting in improved mechanical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134510000001
    Figure 2024134510000001
  • Figure 2024134510000002
    Figure 2024134510000002
Patent Text Reader

Abstract

To provide a fiber-reinforced resin composition which can suppress lowering of flexural properties and tensile properties and increase of tensile creep strain, while suppressing interfacial peeling between polyolefin and polyamide in a molding.SOLUTION: A fiber-reinforced resin composition contains non-modified polyolefin (A), polyamide (B) having a structural unit derived from a monomer having 10 or more carbon atoms, a reinforcement fiber (C), and modified polyolefin (D), wherein when the total of contents of the polyolefin (A), the polyamide (B) and the reinforcement fiber (C) is 100 pts.mass, the content of the polyolefin (A) is 20 pts.mass or more and 80 pts.mass or less, the content of the polyamide (B) is 1 pts.mass or more and 20 pts.mass or less, the content of the reinforcement fiber (C) is 10 pts.mass or more and 70 pts.mass or less, and the content of the modified polyolefin (D) is 1 pts.mass or more and 5 pts.mass or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber-reinforced resin composition and a molded article. [Background technology]

[0002] 2. Description of the Related Art Fiber-reinforced resin compositions, which are resin compositions containing reinforcing fibers, are used in a variety of applications since they can be used to mold lightweight, high-strength molded articles.

[0003] As such a fiber-reinforced resin composition, Patent Document 1 describes a fiber-reinforced resin composition having a resin component in which polyolefin and polyamide are phase-separated. In the fiber-reinforced resin composition described in Patent Document 1, the total cross-sectional area of ​​the dispersed phase (one of the polyolefin and polyamide phases) having a cross-sectional area equal to or less than the average cross-sectional area of ​​the reinforcing fibers is 10% or less by area relative to the total cross-sectional area of ​​all dispersed phases. It is described that this results in a molded product that is less susceptible to brittle fracture by suppressing the generation and progression of cracks due to the dispersed phase. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-210379 A Summary of the Invention [Problem to be solved by the invention]

[0005] Patent Document 1 describes that by using a fiber-reinforced resin composition in which polyolefin and polyamide are phase-separated, a molded body that is less susceptible to brittle fracture can be obtained. However, the present inventors have found that the molded body molded from the fiber-reinforced resin composition described in Patent Document 1 is actually prone to microcracks. When the cause of this was investigated in detail, it was found that the molded body molded from the fiber-reinforced resin composition described in Patent Document 1 has interfacial peeling between the polyolefin phase and the polyamide phase, and that this interfacial peeling is the starting point of the partial crack.

[0006] The inventors therefore investigated various methods for suppressing interfacial delamination between polyolefin and polyamide, but attempts to make interfacial delamination less likely to occur often resulted in a decrease in the bending and tensile properties of the molded body, or in the body being more susceptible to deformation due to load over time (specifically, an increase in tensile creep strain).

[0007] In view of the above problems, the present invention aims to provide a fiber-reinforced resin composition that can suppress interfacial peeling between polyolefin and polyamide in a molded body while suppressing a decrease in bending properties and tensile properties and an increase in tensile creep strain, and a molded body obtained by molding the fiber-reinforced resin composition. [Means for solving the problem]

[0008] One aspect of the present invention for solving the above problems relates to the following fiber-reinforced resin compositions [1] to [7]. [1] An unmodified polyolefin (A), A polyamide (B) having a structural unit derived from a monomer having 10 or more carbon atoms; Reinforcing fiber (C); A modified polyolefin (D), When the total content of the polyolefin (A), the polyamide (B) and the reinforcing fiber (C) is 100 parts by mass, The content of the polyolefin (A) is 40 parts by mass or more and 80 parts by mass or less, The content of the polyamide (B) is 1 part by mass or more and 20 parts by mass or less, The content of the reinforcing fiber (C) is 10 parts by mass or more and 70 parts by mass or less, The content of the modified polyolefin (D) is 1 part by mass or more and 5 parts by mass or less. Fiber reinforced resin composition. [2] When the total content of the polyolefin (A), the polyamide (B) and the reinforcing fiber (C) is 100 parts by mass, The content of the polyolefin (A) is 35 parts by mass or more and 55 parts by mass or less, The content of the reinforcing fiber (C) is 40 parts by mass or more and 60 parts by mass or less, The fiber-reinforced resin composition according to [1]. [3] The reinforcing fibers (C) are bundled with an acrylic sizing agent or a polyamide sizing agent. The fiber-reinforced resin composition according to [1] or [2]. [4] The polyolefin (A) and the polyamide (B) form a sea-island structure in which a dispersed phase of the polyamide (B) is dispersed in a continuous phase of the polyolefin (A), The average equivalent circle diameter of the dispersed phase is 1.0 μm or less. The fiber-reinforced resin composition according to any one of [1] to [3]. [5] The polyamide (B) is polyamide 12. The fiber-reinforced resin composition according to any one of [1] to [4]. [6] The polyolefin (A) is polypropylene. The fiber-reinforced resin composition according to any one of [1] to [5]. [7] The reinforcing fiber (C) is a glass fiber or a carbon fiber; The fiber-reinforced resin composition according to any one of [1] to [6].

[0009] Another aspect of the present invention for solving the above problems relates to the following molded article [8][9]. [8] A molded article obtained by molding the fiber-reinforced resin composition according to any one of [1] to [7]. [9] The molded body according to [8], which is an automotive part. Effect of the Invention

[0010] According to the present invention, there is provided a fiber-reinforced resin composition that can suppress interfacial peeling between polyolefin and polyamide in a molded body while suppressing a decrease in bending properties and tensile properties and an increase in tensile creep strain, and a molded body obtained by molding the fiber-reinforced resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] 1. Fiber-reinforced resin composition One embodiment of the present invention relates to a fiber-reinforced resin composition containing a polyolefin and a polyamide as resin components. The fiber-reinforced resin composition contains an unmodified polyolefin (A), a polyamide (B) having a structural unit derived from a monomer having 10 or more carbon atoms, a reinforcing fiber (C), and a modified polyolefin (D).

[0012] 1-1.Polyolefin (A) The polyolefin (A) is an unmodified polyolefin.

[0013] The type of polyolefin (A) is not limited, and polymers of α-olefins, cyclic olefins, non-conjugated dienes, aromatic olefins, and the like can be widely used. Among these, polymers mainly composed of α-olefins are preferred. The polymer mainly composed of α-olefins means a polymer in which the ratio of the structural units derived from α-olefins to all structural units constituting the polymer is 50 mol% or more and 100 mol% or less. The ratio of the structural units derived from α-olefins to all structural units constituting the polyolefin (A) is preferably 60 mol% or more and 100 mol% or less, and more preferably 70 mol% or more and 100 mol% or less. The ratio of each structural unit constituting the polyolefin (A) is as follows: 13It can be measured by C-NMR method. The monomer constituting the polyolefin (A) may be derived from a fossil fuel, may be derived from a biomass raw material, or may be a mixture of these.

[0014] The α-olefin preferably has a carbon number of 2 or more and 20 or less, more preferably 2 or more and 10 or less, and even more preferably 2 or more and 8 or less. Examples of such α-olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 3-methyl-1-butene, and 4-methyl-1-pentene. These α-olefins may be used alone or in combination of two or more to form a copolymer.

[0015] Examples of polyolefin (A) include polyethylene, which is an ethylene homopolymer or a copolymer of ethylene and other α-olefins, and polypropylene, which is a propylene homopolymer or a copolymer of propylene and other α-olefins. In these polyethylenes and polypropylenes, the ratio of the structural units derived from ethylene to all structural units and the ratio of the structural units derived from propylene to all structural units are preferably 50 mol% or more and 100 mol% or less, more preferably 70 mol% or more and 100 mol% or less, and even more preferably 90 mol% or more and 100 mol% or less. As polyolefin (A), only one of these polyolefins may be used, or two or more may be used in combination.

[0016] From the viewpoint of improving mechanical properties, heat resistance, and water resistance, the polyolefin (A) is preferably polypropylene, and more preferably a propylene homopolymer.

[0017] The polypropylene preferably has a melting point of 130° C. or more and 180° C. or less, more preferably 140° C. or more and 170° C. or less, as measured by a differential scanning calorimeter (DSC) at a heating rate of 10° C. / min.

[0018] From the viewpoint of improving the impregnation property of the reinforcing fiber (C), the polyolefin (A) preferably has a melt flow rate (MFR) measured under a load of 2.16 kg in accordance with JISK 7210 of 0.01 g / 10 min to 300 g / 10 min, more preferably 0.1 g / 10 min to 300 g / 10 min, even more preferably 1 g / 10 min to 300 g / 10 min, even more preferably 10 g / 10 min to 300 g / 10 min, and particularly preferably 50 g / 10 min to 300 g / 10 min. The MFR is a value measured at 190°C for polyethylene and 230°C for polypropylene.

[0019] From the viewpoint of enhancing the impregnation property into the reinforcing fiber (C), the polyolefin (A) has a melt viscosity η at 250°C and a shear rate of 120 / sec. A The viscosity is preferably 30 Pa·s or more and 160 Pa·s or less, and more preferably 30 Pa·s or more and 100 Pa·s or less.

[0020] 1-2.Polyamide (B) The polyamide (B) can make it difficult for a molded article made from the fiber-reinforced resin composition to deform due to load over time. For example, the polyamide (B) can reduce the tensile creep strain of the molded article made from the fiber-reinforced resin composition.

[0021] The type of polyamide (B) is not limited, and a wide variety of compounds having amino and carboxy groups in the molecule (amino acid monomers) or polymers of their dehydration condensation products, copolymers of diamines and dicarboxylic acids, and copolymers thereof can be used. The monomers constituting polyamide (B) may be derived from fossil fuels, may be derived from biomass raw materials, or may be a mixture of these.

[0022] The polyamide (B) has a structural unit derived from a monomer having 10 or more carbon atoms. This enhances the affinity between the polyolefin (A) and the polyamide (B), making it difficult for interfacial peeling to occur between them. From the above viewpoint, the polyamide (B) preferably has a structural unit derived from a monomer having a linear or branched alkyl group having 10 or more carbon atoms, and more preferably has a structural unit derived from a monomer having a linear or branched alkyl group having 10 or more carbon atoms.

[0023] Furthermore, in the polyamide (B), the ratio of the structural units derived from the above-mentioned monomers having 10 or more carbon atoms to all structural units constituting the polyamide (B) is preferably 60 mol% or more and 100 mol% or less, more preferably 70 mol% or more and 100 mol% or less, and even more preferably 90 mol% or more and 100 mol% or less.

[0024] Examples of the amino acid monomer having 10 or more carbon atoms include amino acids such as aminoundecanoic acid and aminododecanoic acid, and lactams such as undecane lactam and ω-lauryllactam. These amino acid monomers may be used alone or in combination of two or more to form a copolymer.

[0025] Examples of the diamines, which are monomers having 10 or more carbon atoms, include aliphatic diamines such as 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,13-diaminotridecane, 1,14-diaminotetradecane, 1,15-diaminopentadecane, 1,16-diaminohexadecane, 1,17-diaminoheptadecane, 1,18-diaminooctadecane, 1,19-diaminononadecane, and 1,20-diaminoeicosane, as well as alicyclic diamines such as bis(4-aminocyclohexyl)methane. Only one of these diamines may be used, or two or more of them may be used in combination to form a copolymer.

[0026] Examples of the dicarboxylic acid which is a monomer having 10 or more carbon atoms include aliphatic dicarboxylic acids such as sebacic acid, undecanedioic acid, dodecanedioic acid, brassicic acid, tetradecanedioic acid, pentadecanedioic acid, and octadecanedioic acid, and aromatic dicarboxylic acids such as naphthalenedicarboxylic acid, etc. These dicarboxylic acids may be used alone or in combination of two or more to form a copolymer.

[0027] The polyamide (B) may be a copolymer of these monomers having 10 or more carbon atoms and monomers having 9 or less carbon atoms. Examples of amino acid monomers having 9 or less carbon atoms include amino acids such as aminocaproic acid and paraaminomethylbenzoic acid, and lactams such as ε-caprolactam. Examples of diamines having 9 or less carbon atoms include aliphatic diamines such as ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 2-methyl-1,5-diaminopentane (2M-5), and 2-methyl-1,8-diaminooctane (2M-8), alicyclic diamines such as cyclohexanediamine, and aromatic diamines such as p-phenylenediamine, m-phenylenediamine, p-xylylenediamine, and m-xylylenediamine. Examples of dicarboxylic acids which are monomers having 9 or less carbon atoms include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, and azelaic acid, alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid, and aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, and isophthalic acid. These monomers having 9 or less carbon atoms may be used alone or in combination of two or more.

[0028] Specific examples of polyamide (B) include polyamide 6 / 10, polyamide 6 / 12, polyamide 6 / 14, polyamide 11, polyamide 12, polyamide 10 / 10, polyamide 10 / 12, polyamide 10 / T, etc. Among these, polyamide 12 is preferred from the viewpoint of improving water resistance. These polyamides may be used alone or in combination of two or more kinds.

[0029] From the viewpoint of improving the impregnation of the reinforcing fiber (C), the polyamide (B) preferably has a melt flow rate (MFR) measured under a load of 2.16 kg in accordance with JISK 7210 of 1 g / 10 min to 500 g / 10 min, more preferably 5 g / 10 min to 500 g / 10 min, even more preferably 10 g / 10 min to 300 g / 10 min, even more preferably 20 g / 10 min to 300 g / 10 min, and particularly preferably 60 g / 10 min to 100 g / 10 min. The MFR is a value measured at 230°C for PA12.

[0030] From the viewpoint of improving the impregnation property into the reinforcing fiber (C), the polyamide (B) preferably has a melting point of 160°C or more and 260°C or less, more preferably 170°C or more and 220°C or less, as measured by a differential scanning calorimeter (DSC) at a heating rate of 10°C / min.

[0031] 1-3. Reinforced fiber (C) The type of reinforcing fiber (C) is not limited, and may be inorganic or organic. Examples of inorganic fibers include metal fibers such as glass fibers, carbon fibers, aluminum fibers, aluminum alloy fibers, copper fibers, brass fibers, steel fibers, stainless steel fibers, and titanium fibers, as well as ceramic fibers such as silicon carbide fibers, silicon nitride fibers, alumina fibers, and zirconia fibers. Examples of organic fibers include synthetic fibers made of synthetic resins such as fully aromatic polyamides (such as aramids), fully aromatic polyesters, fully aromatic polyesteramides, fully aromatic polyethers, fully aromatic polycarbonates, fully aromatic polyazomethines, polyphenylene sulfides, polyparaphenylene benzobisoxazoles, poly(para-phenylene benzobisthiazoles), polybenzimidazoles, polyether ether ketones, polyamide imides, polyimides, polytetrafluoroethylene, polyvinyl alcohols, polyolefins, polyarylates, and fluorine-based polymers, as well as natural fibers such as cotton fibers, silk fibers, wood fibers, and cellulose fibers. Among these, glass fiber and carbon fiber are preferred, and glass fiber is more preferred from the viewpoint of reducing production costs. As the reinforcing fiber (C), only one of these may be used, or two or more of them may be used in combination.

[0032] Examples of glass fibers include glass fibers having compositions such as A-glass, C-glass, D-glass, E-glass, and S-glass. Among these, glass fibers having a composition of E-glass (alkali-free glass) are preferred. These glass fibers may be used alone or in combination of two or more kinds.

[0033] The glass fibers may be fibers having a length of 10 mm or more, chopped strands cut to a length of 1 mm or more and 10 mm or less, or milled fibers pulverized to a length of 10 μm or more and 500 μm or less.

[0034] The carbon fiber may be any of polyacrylonitrile-based, rayon-based, pitch-based, polyvinyl alcohol-based, regenerated cellulose-based, and pitch-based carbon fibers produced from mesophase pitch. The carbon fiber may be a general-purpose fiber or a high-strength fiber. The carbon fiber may be a recycled fiber. A plurality of carbon fibers may be bundled together using a bundling agent.

[0035] The natural fibers are preferably cellulose fibers, and the cellulose fibers are preferably cellulose nanofibers, lignocellulose nanofibers, cellulose microfibers, and the like.

[0036] The reinforcing fiber (C) may be a short fiber having an average fiber length of less than 1.0 mm, or a long fiber having an average fiber length of 1.0 mm or more. When the reinforcing fiber (C) is a short fiber, it may be a chopped fiber (cut fiber) having no fibril (microfiber split in the axial direction and divided into smaller pieces), or a pulp-like fiber having fibril. The reinforcing fiber (C) may be a single fiber, or a twisted yarn formed by twisting together a plurality of single fibers.

[0037] The average fiber length of the reinforcing fibers (C) is preferably 0.01 mm or more and 100 mm or less, more preferably 0.1 mm or more and 50 mm or less, and even more preferably 1 mm or more and 30 mm or less. When the average fiber length is within the above range, the mechanical strength of the molded product is easily increased, and from the viewpoint of suppressing the generation of dry fibers due to the detachment of relatively short reinforcing fibers from the fiber reinforced resin composition, the ratio of the number of reinforcing fibers having a fiber length of less than 0.1 mm to the number of all reinforcing fibers in the reinforcing fibers (C) is preferably 18% or less.

[0038] The average fiber diameter of the reinforcing fiber (C) is preferably 1 μm or more and 30 μm or less, more preferably 5 μm or more and 20 μm or less. When the average fiber diameter is in the above range, the mechanical strength (particularly impact resistance and rigidity) and heat resistance of the molded body are easily increased, and the appearance of the molded body is good. In addition, when the average fiber diameter is in the above range, the reinforcing fiber (C) is easily impregnated with the resin component.

[0039] The average fiber length and the average fiber diameter can be determined, for example, by measuring the lengths or diameters of 100 reinforcing fibers (C) randomly selected from a photograph of the reinforcing fibers (C) taken with an optical microscope, and taking the arithmetic average of these.

[0040] The reinforcing fiber (C) may be bundled by a bundling agent. The bundling agent may be any bundling agent such as a polyolefin-based bundling agent, an acrylic-based bundling agent, a urethane-based bundling agent, an acid copolymer-based bundling agent, a polyamide-based bundling agent, or an epoxy-based bundling agent. Among these, from the viewpoint of increasing the bending modulus, bending strength, and impact resistance of the molded body, acrylic-based bundling agents and polyamide-based bundling agents are preferred, and acrylic-based bundling agents are more preferred. These bundling agents are highly reactive with polyamide (B) and modified polyolefin (D), and therefore are considered to facilitate adhesion of the reinforcing fiber (C) bundled by these bundling agents to other resin components. In addition, when the reinforcing fiber (C) is a long fiber (especially a long fiber, glass fiber), the impregnation of the resin component is good, so acrylic-based bundling agents and acid copolymer-based bundling agents are preferred, and acid copolymer-based bundling agents are more preferred.

[0041] The mass ratio (ignition loss) of the sizing agent to the reinforcing fiber (C) is preferably 0.1% by mass or more and 1.5% by mass or less. When the ignition loss is 0.1% by mass or more, the interface between the polyamide (B) and the reinforcing fiber (C) is stabilized, and the heat resistance of the molded body is easily improved. When the ignition loss is 1.5% by mass or less, the heat resistance of the molded body is less likely to be reduced by the sizing agent. The mass ratio (ignition loss) of the sizing agent is a value measured on the fibers obtained by applying the sizing agent to the reinforcing fiber with an applicator or the like and drying the fiber to completely volatilize the volatile substances, in accordance with JIS R 3420:2006 7.3.2.

[0042] 1-4. Modified polyolefin (D) The modified polyolefin (D) improves the interaction between the polyolefin (A) and the polyamide (B) to enhance the dispersibility of the polyamide (B) in the polyolefin (A). As a result, in this embodiment, unlike the structure shown in the drawing of Patent Document 1, the polyamide (B) can be more uniformly dispersed so that the shape of the cross-sectional photograph is closer to a perfect circle. By dispersing the polyamide (B) more uniformly, the tensile creep strain of the molded body molded from the fiber reinforced resin composition can be reduced, and the heat distortion resistance of the molded body can be improved. The modified polyolefin (D) may be used alone or in combination of two or more kinds. The monomer constituting the modified polyolefin (D) may be derived from a fossil fuel, may be derived from a biomass raw material, or may be a mixture of these.

[0043] The modified polyolefin (D) is preferably a resin obtained by modifying an unmodified polyolefin with an unsaturated carboxylic acid or a derivative thereof.

[0044] The unmodified polyolefin may be any of the various polyolefins exemplified as polyolefin (A). In this case, it is preferable that the polyolefin (A) and the unmodified polyolefin used as the raw material for the modified polyolefin (D) are the same type of resin. For example, when the polyolefin (A) is polyethylene, the unmodified polyolefin used as the raw material for the modified polyolefin (D) is also preferably polyethylene, and when the polyolefin (A) is polypropylene, the unmodified polyolefin used as the raw material for the modified polyolefin (D) is also preferably polypropylene. These unmodified polyolefins may be used alone or in combination of two or more.

[0045] Examples of the unsaturated carboxylic acid used for the modification include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, sorbic acid, and angelic acid, and unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, mesaconic acid, tetrahydrophthalic acid, norbornene dicarboxylic acid, and bicyclo[2.2.1]hept-2-ene-5,6-dicarboxylic acid.

[0046] Examples of the unsaturated carboxylic acid derivatives used for the modification include acid anhydrides, acid halides, esters, amides, imides, and metal salts of the above-mentioned unsaturated carboxylic acids. Specific examples of the unsaturated carboxylic acid derivative include unsaturated dicarboxylic acid anhydrides such as maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, and bicyclo[2.2.1]hept-2-ene-5,6-dicarboxylic anhydride; unsaturated dicarboxylic acid halides such as malenyl chloride; acrylic acid esters such as methyl acrylate, ethyl acrylate, propyl acrylate, and butyl acrylate; methacrylic acid esters such as methyl methacrylate and glycidyl methacrylate; maleic acid esters such as monomethyl maleate, monoethyl maleate, dimethyl maleate, and diethyl maleate; other esters such as diethyl fumarate, dimethyl itaconate, diethyl citraconic acid, dimethyl tetrahydrophthalate, and dimethyl bicyclo[2.2.1]hept-2-ene-5,6-dicarboxylate; acrylamide, maleic acid amide, maleimide, sodium acrylate, and sodium methacrylate.

[0047] Among these, unsaturated dicarboxylic acids or derivatives thereof are preferred, unsaturated dicarboxylic acids or anhydrides thereof are more preferred, and maleic acid or maleic anhydride is even more preferred. Alternatively, it may be modified by combining an acrylic acid ester with glycidyl methacrylate. These unsaturated carboxylic acids or derivatives thereof may be used alone or in combination of two or more.

[0048] The modified polyolefin (D) may have an unsaturated dicarboxylic acid or a derivative thereof grafted to a side chain, or may have an unsaturated dicarboxylic acid or a derivative thereof copolymerized in the main chain.

[0049] In the modified polyolefin resin (D), the proportion of the constitutional unit derived from the unsaturated carboxylic acid or its derivative is preferably 0.1% by mass or more and 5% by mass or less, more preferably 0.2% by mass or more and 1% by mass or less, based on the total mass of the modified polyolefin resin (D). The proportion of the constitutional unit derived from the unsaturated carboxylic acid or its derivative can be measured by infrared absorption spectroscopy or the like.

[0050] 1-5.Other ingredients The fiber reinforced resin composition may contain components other than the above-mentioned components (A) to (D). Examples of the other components include polyamides other than component (B), thermoplastic resins other than components (A), (B) and (C), flame retardants, flame retardant auxiliaries, fillers, colorants, antibacterial agents, and antistatic agents. These components may be used alone or in combination of two or more.

[0051] Examples of polyamides other than component (B) include polyamide 6, polyamide 66, polyamide 6T, polyamide 6I, polyamide 9T, polyamide M5T, polyamide MXD6, polyamide 6T / 66, polyamide 6T / 6I, polyamide 6T / 6I / 66, polyamide 6T / 2M-5T, and polyamide 9T / 2M-8T.

[0052] Examples of the thermoplastic resin other than the components (A), (B) and (C) include styrene-based thermoplastic elastomers such as styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-styrene copolymer (SIS), styrene-ethylene / butylene-styrene copolymer (SEBS) and styrene-ethylene / propylene-styrene copolymer (SEPS). These thermoplastic resins may be derived from fossil fuels, may be derived from biomass raw materials, or may be a mixture thereof.

[0053] Examples of the flame retardant include halogen-based flame retardants such as halogenated aromatic compounds, phosphorus-based flame retardants such as nitrogen-containing phosphate compounds and phosphoric acid esters, nitrogen-based flame retardants such as guanidine, triazine, melamine and derivatives thereof, inorganic flame retardants such as metal hydroxides, boron-based flame retardants, silicone-based flame retardants, sulfur-based flame retardants, and red phosphorus-based flame retardants.

[0054] Examples of the flame retardant synergist include antimony compounds, metal compounds containing zinc, metal compounds containing bismuth, magnesium hydroxide, and clay silicates.

[0055] Examples of fillers include glass components such as glass beads and glass flakes, silica, graphite, calcium silicate, aluminum silicate, kaolin, talc, clay, and other silicate compounds, metal oxides such as iron oxide, titanium oxide, zinc oxide, antimony oxide, and alumina, calcium, magnesium, and metal carbonates or sulfates.

[0056] Examples of colorants include pigments and dyes.

[0057] 1-6. Mixture ratio When the total content of polyolefin (A), polyamide (B) and reinforcing fiber (C) is 100 parts by mass, the content of polyolefin (A) is 20 parts by mass or more and 80 parts by mass or less, more preferably 30 parts by mass or more and 70 parts by mass or less, more preferably 35 parts by mass or more and 65 parts by mass or less, even more preferably 35 parts by mass or more and 55 parts by mass or less, and particularly preferably 40 parts by mass or more and 55 parts by mass or less. When the ratio of (A) component is 20 parts by mass or more, it is easy to make the molded body lightweight. When the ratio of (A) component is 80 parts by mass or more, other components can be sufficiently blended.

[0058] When the total content of polyolefin (A), polyamide (B) and reinforcing fiber (C) is 100 parts by mass, the content of polyamide (B) is 1 part by mass or more and 20 parts by mass or less, preferably 3 parts by mass or more and 15 parts by mass or less, and more preferably 3 parts by mass or more and 10 parts by mass or less. When the ratio of (B) component is 1 part by mass or more, the mechanical properties of the molded body are easily improved and the tensile creep strain of the molded body is easily reduced. When the ratio of (B) component is 20 parts by mass or less, the impregnation of the resin component into the reinforcing fiber (C) is good, and cracks of the molded body due to the reinforcing fiber (C) not impregnated with the resin component (dry fiber), exposure of the reinforcing fiber (C) on the surface of the molded body, and retention (bridging) of the fiber-reinforced resin composition during injection molding are unlikely to occur. In addition, when the impregnation is good, the tensile creep strain of the molded body is easily reduced.

[0059] When the total content of polyolefin (A), polyamide (B) and reinforcing fiber (C) is 100 parts by mass, the content of reinforcing fiber (C) is 10 parts by mass or more and 70 parts by mass or less, preferably 20 parts by mass or more and 65 parts by mass or less, more preferably 25 parts by mass or more and 60 parts by mass or less, even more preferably 40 parts by mass or more and 60 parts by mass or less, and particularly preferably 45 parts by mass or more and 55 parts by mass or less. When the proportion of (C) component is 10 parts by mass or more, the bending strength and tensile strength of the molded body are easily increased. In addition, when the proportion of (C) component is increased, the bending modulus, bending strength, tensile modulus and tensile strength of the molded body are further increased.

[0060] When the total content of polyolefin (A), polyamide (B) and reinforcing fiber (C) is taken as 100 parts by mass, the content of modified polyolefin (D) is 1 part by mass or more and 5 parts by mass or less, preferably 1 part by mass or more and 4 parts by mass or less, more preferably 1 part by mass or more and 3 parts by mass or less, and even more preferably 1 part by mass or more and 2 parts by mass or less. When the ratio of (D) component is 1 part by mass or more, the impregnation of the resin component into the reinforcing fiber (C) is good, and cracks of the molded body due to the reinforcing fiber (C) not impregnated with the resin component (dry fiber), exposure of the reinforcing fiber (C) on the surface of the molded body, and retention (bridging) of the fiber-reinforced resin composition during injection molding are unlikely to occur. In addition, when the impregnation is good, the tensile creep strain of the molded body is easily reduced.

[0061] When the total content of polyolefin (A), polyamide (B) and modified polyolefin (D) is 100 parts by mass, the content of polyamide (B) is preferably 1 part by mass or more and 20 parts by mass or less, more preferably 2 parts by mass or more and 18 parts by mass or less, and even more preferably 5 parts by mass or more and 15 parts by mass or less. When the content of polyamide (B) is 5 parts by mass or more, the bending strength of the molded body is likely to be increased. When the content of polyamide (B) is 20 parts by mass or less, the impregnation of the resin component into the reinforcing fiber (C) is good, and cracks of the molded body due to the reinforcing fiber (C) not impregnated with the resin component (dry fiber), exposure of the reinforcing fiber (C) on the surface of the molded body, and retention (bridging) of the fiber reinforced resin composition during injection molding are unlikely to occur. In addition, when the impregnation is good, the tensile creep strain of the molded body is easily reduced.

[0062] The total content of the polyolefin (A), polyamide (B), reinforcing fiber (C) and modified polyolefin (D) relative to the total mass of the fiber reinforced resin composition is preferably 70 mass% or more and 100 mass% or less, more preferably 80 mass% or more and 100 mass% or less, and even more preferably 90 mass% or more and 100 mass% or less.

[0063] 1-7. Dispersion state It is preferable that the polyolefin (A) and the polyamide (B) form a sea-island structure in which a dispersed phase of the polyamide (B) is dispersed in a continuous phase of the polyolefin (A). In this embodiment, the modified polyolefin (D) improves the interaction between the polyolefin (A) and the polyamide (B) to enhance the dispersibility of the polyamide (B) in the polyolefin (A). This allows the polyamide (B) to be dispersed more uniformly so that the shape of the fiber-reinforced resin composition is closer to a perfect circle in a cross-sectional photograph. By dispersing the polyamide (B) more uniformly, the impregnation of the resin component into the reinforcing fiber (C) is improved, and cracks of the molded body due to the reinforcing fiber (C) not impregnated with the resin component (dry fiber), exposure of the reinforcing fiber (C) to the surface of the molded body, and retention (bridging) of the fiber-reinforced resin composition during injection molding are less likely to occur. In addition, by improving the impregnation, the tensile creep strain of the molded body molded from the fiber-reinforced resin composition can be reduced.

[0064] More specifically, in a cross-sectional photograph of the fiber-reinforced resin composition, the average equivalent circle diameter of the dispersed phase of polyamide (B) is preferably 1.0 μm or less, more preferably 0.1 μm or more and 1.0 μm or less, and even more preferably 0.3 μm or more and 0.6 μm or less. When the average equivalent circle diameter is 1.0 μm or less, polyamide (B) is more uniformly dispersed, and the impregnation of the resin component into the reinforcing fiber (C) is good.

[0065] The above-mentioned circle equivalent diameter and aspect ratio can be determined by analyzing an image of the fiber-reinforced resin composition taken by a transmission electron microscope using known image analysis software, and calculating the particle diameter and major axis / minor axis corresponding to the dispersed phase of polyamide (B) by blob analysis.

[0066] 1-8.Form The form of the fiber-reinforced resin composition is not particularly limited, and may be a composition in a molten state (fluid state) containing each heated and melted resin material, reinforcing fiber (C) and other components, or the resin material may be cooled to be in a solid state such as pellets or sheets.

[0067] The reinforcing fibers (C) may be oriented in a random direction and dispersed in the fiber-reinforced resin composition, or may be oriented in one direction and arranged. For example, the fiber-reinforced resin composition may be a thin-film fiber-reinforced resin (UD sheet) in which a resin component is impregnated into a plurality of reinforcing fibers (C) arranged in one direction, a thin-film fiber-reinforced resin (cross sheet) in which a resin component is impregnated into a woven fabric of a plurality of reinforcing fibers arranged in one direction, or a pellet-shaped resin composition (long fiber thermoplastics: LFT) in which a resin component is impregnated into a plurality of reinforcing fibers (C) arranged in one direction. Of these, LFT is preferred because it is applicable to mechanical injection molding and has high moldability.

[0068] For example, the LFT may be a cylindrical pellet having a length in the stretching direction of the reinforcing fibers (C) of 3 mm to 100 mm, preferably 5 mm to 50 mm. The average fiber length of the reinforcing fibers (C) contained in the LFT is approximately the same as the length of the pellet, and more preferably 80% to 100%, more preferably 90% to 100% of the length of the pellet.

[0069] 2. Manufacturing method The fiber-reinforced resin composition may be prepared by melt-kneading the above-mentioned components, or by impregnating reinforcing fibers (C) oriented in one direction with a resin component and other components.

[0070] For example, when the reinforcing fibers (C) are short fibers, the above-mentioned components can be melt-kneaded to obtain a fiber-reinforced resin composition in which the reinforcing fibers (C) are randomly oriented and dispersed. The melt-kneading temperature is preferably 5°C to 100°C higher than the melting point of the resin with the highest melting point among the resin components, and more preferably 10°C to 60°C higher. The melt-kneading time is preferably 30 seconds to 15 minutes, and more preferably 1 minute to 10 minutes.

[0071] For example, the above-mentioned components may be melt-kneaded with a melt kneader such as a roll mill, a Banbury mixer, or a kneader. Alternatively, the components may be dry-blended with a kneader such as a tumbler blender, a Henschel mixer, or a ribbon mixer, and then melt-kneaded and extruded with an extruder such as a single-screw extruder or a twin-screw extruder. The melt-kneaded fiber-reinforced resin composition in a molten state may be directly injected into a molding machine and molded, or the extruded fiber-reinforced resin composition may be processed into a predetermined shape (for example, pellets) to form a solid fiber-reinforced resin composition.

[0072] When the reinforcing fibers (C) are long fibers, the reinforcing fibers (C) aligned in one direction can be impregnated with molten resin components and other components to produce a fiber-reinforced resin composition that is a UD sheet, a cross-seat, or an LFT. The temperature of the molten resin at this time is preferably 5°C to 100°C higher than the melting point of the resin with the highest melting point among the resin components, and more preferably 10°C to 60°C higher.

[0073] For example, the reinforcing fibers (C) aligned in one direction can be made to travel through an impregnation roll or an impregnation die, and then brought into contact with the molten resin component and other components in the impregnation roll or the impregnation die, thereby impregnating them. After the impregnation, the resin component can be cooled and solidified, and then processed into a predetermined shape (for example, a sheet or pellet) to form a solid fiber-reinforced resin composition.

[0074] 3.Applications The fiber-reinforced resin composition can be processed into a molded article by a known molding method such as injection molding, extrusion molding, press molding, etc. The above-mentioned sea-island structure is also retained in the molded article.

[0075] The molded article can be used in a wide range of applications, from household goods such as daily necessities and recreational uses to general industrial applications and industrial goods. Examples of applications of the molded article include home appliance material parts, communication device parts, electric parts, electronic parts, automobile parts, parts of vehicles other than automobiles, ships, aircraft materials, machine mechanism parts, building materials, civil engineering materials, agricultural materials, power tool parts, food containers, films, sheets, and fibers.

[0076] As for automobile parts, the material can be used in various parts such as power train parts due to improved heat resistance, mechanism parts due to improved tensile creep resistance, and exterior panel parts due to improved bending properties, but can also be applied to other parts. Examples of automobile parts include intake manifolds, oil pans, cylinder heads, cylinder head covers, engine covers, shrouds, mirror brackets, interior consoles, sunroofs, sunroof frames, front doors, back doors, sliding doors, front end modules, door modules, fenders, wheel caps, gasoline tanks, belts, ceiling coverings, convertible tops, armrests, door trims, rear package trays, sun visors, wheel covers, mattress covers, airbags, insulation materials, electric wire covering materials, electrical insulation materials, covering materials, floor materials, corner walls, deck panels, covers, plywood, ceiling panels, partition panels, side walls, wallpaper, wall covering materials, exterior materials, interior materials, roofing materials, soundproofing panels, and heat insulating panels.

[0077] Examples of home appliance material parts, communication device parts, electric parts, and electronic parts include battery pack parts (covers, trays, module cases), office and OA equipment such as printers, personal computers, word processors, keyboards, personal digital assistants (PDAs), headphone stereos, mobile phones, telephones, facsimiles, copiers, electronic cash registers (ECRs), calculators, electronic organizers, electronic dictionaries, cards, holders, and stationery; home appliances such as washing machines, refrigerators, vacuum cleaners, microwave ovens, lighting fixtures, game consoles, irons, and kotatsu; AV equipment such as televisions, video players, video cameras, radio cassette players, tape recorders, minidiscs, CD players, speakers, and liquid crystal displays; connectors, relays, capacitors, switches, printed circuit boards, coil bobbins, semiconductor encapsulating materials, electric wires, cables, transformers, deflection yokes, distribution boards, and clocks.

[0078] Examples of everyday items include living and sporting goods such as plywood, synthetic boards, buckets, containers, bags, cases, goggles, skis, rackets, tents, bicycles, and musical instruments. EXAMPLES

[0079] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to the descriptions in the examples.

[0080] 1. Preparation of materials The following materials were prepared:

[0081] 1-1. Unmodified polyolefin (A) Polypropylene (PP-1) Prime Polymer J13B, MFR (JIS K7210 compliant, 230℃, 2.16kg load): 220g / 10min Polypropylene (PP-2) Mitsui Chemicals TAFMER PN2060, MFR (JIS K7210 compliant, 230℃, 2.16kg load): 6.6g / 10min

[0082] 1-2.Polyamide (B) Polyamide 12 (PA12) UBE 3012U, MFR (JIS K7210 compliant, 230℃, 2.16kg load): 130g / 10min Polyamide 6 (PA6-1) Toray Industries, Inc. CM1026, MFR (JIS K7210 compliant, 230°C, 2.16kg load): 2g / 10min Polyamide 6 (PA6-2) Toray Industries, Inc. CM1007, MFR (JIS K7210 compliant, 230°C, 2.16 kg load): 67g / 10min

[0083] 1-3. Reinforced fiber (C) Glass fiber (GF-1) Long-fiber glass roving surface-treated with polyolefin-based sizing agent Nitto Boseki RS2400QR-489 (TEX number 2400, filament diameter 17μm) Glass fiber (GF-2) Long fiber glass roving surface treated with acid copolymer-based sizing agent Nippon Electric Glass T-425N (TEX number 2400, filament diameter 17μm) Glass fiber (GF-3) Long fiber glass roving surface treated with acrylic sizing agent Nitto Boseki Co., Ltd. RSX230QR-483AS (TEX number 2300, filament diameter 17μm)

[0084] 1-4. Modified polyolefin (D) Maleic acid modified polyolefin (modified PP) Admer AT2606, manufactured by Mitsui Chemicals, Inc.

[0085] 2. Preparation of fiber-reinforced resin composition and test specimens 2-1. Preparation of fiber reinforced resin composition 1 and test piece 1 (Example 1) PP as polyolefin resin (A), PA12 as polyamide resin (B), and modified PP as modified polyolefin resin (D) were blended in the ratios (units: mass%) shown in Table 1, and fed into the hopper of a twin-screw melt kneading extruder (TEX30α manufactured by JSW, L / D=53, D=30mm) whose temperature was adjusted to 295 ° C. Also, glass fiber roving (GF-1) was expanded and opened as reinforcing fiber (C) and introduced into the impregnation die. The above melted resin components (i.e., a mixture of polyolefin resin (A), polyamide resin (B), and modified polyolefin resin (D)) were supplied to the impregnation die, and the reinforcing fiber (C) was impregnated with the above resin components inside the impregnation die. The moving speed of the reinforcing fiber (C) at this time was adjusted so that the ratio of the reinforcing fiber (C) in the obtained fiber reinforced resin composition was the amount shown in Table 1. Thereafter, the resin component impregnated into the reinforcing fibers (C) was cooled and solidified, and the reinforcing fibers (C) and the resin component were cut into pellets with a strand cutter to a length of 9 mm to obtain a pellet-shaped fiber-reinforced resin composition (fiber-reinforced resin composition 1).

[0086] This fiber-reinforced resin composition was injection molded using an injection molding machine (manufactured by The Japan Steel Works, Ltd., J100ADS-180U) under injection conditions of a set temperature of 250°C and a mold temperature of 60°C, and molded into dumbbell-shaped test pieces for evaluation tests (compliant with JIS K7139 (ISO 3176:93)) (these test pieces are referred to as test pieces 1).

[0087] 2-2. Preparation of fiber reinforced resin composition 2 and test piece 2 (Example 2) Fiber reinforced resin composition 2 was obtained in the same manner as fiber reinforced resin composition 1, except that the amounts of the resin components were changed so that the compounding ratio of each component was the ratio shown in Table 1. This fiber reinforced resin composition 2 was molded in the same manner as test piece 1 to obtain test piece 2.

[0088] 2-3. Preparation of fiber reinforced resin composition 3 and test piece 3 (Example 3) Fiber reinforced resin composition 3 was obtained in the same manner as fiber reinforced resin composition 1, except that the amounts of the resin components were changed so that the compounding ratio of each component was the ratio shown in Table 1. This fiber reinforced resin composition 3 was molded in the same manner as test piece 1, to obtain test piece 3.

[0089] 2-4. Preparation of fiber reinforced resin composition 4 and test piece 4 (Example 4) Fiber reinforced resin composition 4 was obtained in the same manner as fiber reinforced resin composition 1, except that the amounts of the resin components were changed so that the compounding ratio of each component was the ratio shown in Table 1. This fiber reinforced resin composition 4 was molded in the same manner as test piece 1 to obtain test piece 4.

[0090] 2-5. Preparation of fiber reinforced resin composition 5 and test piece 5 (Example 5) Fiber reinforced resin composition 5 was obtained in the same manner as fiber reinforced resin composition 1, except that the amounts of the resin components were changed so that the compounding ratio of each component was the ratio shown in Table 1. This fiber reinforced resin composition 5 was molded in the same manner as test piece 1 to obtain test piece 5.

[0091] 2-6. Preparation of fiber reinforced resin composition 6 and test piece 6 (Comparative Example 1) A polypropylene long fiber composite material (L-50719, manufactured by Prime Polymer Co., Ltd., polypropylene content: 50 wt%, glass fiber content: 50 wt%) was heated and melted, and diluted with the above PP until the reinforcing fiber content became 30 mass%, to obtain a fiber reinforced resin composition 6. This fiber reinforced resin composition 6 was molded into the same shape as the test piece 1, to obtain a test piece 6.

[0092] 2-7. Preparation of Fiber Reinforced Resin Compositions 7 to 10 and Test Pieces 7 to 10 (Comparative Examples 2 to 5) Fiber reinforced resin compositions 7 to 10 were obtained in the same manner as in the preparation of fiber reinforced resin composition 1, except that the amounts of the resin components were changed so that the compounding ratio of each component was the ratio shown in Table 1. These fiber reinforced resin compositions were molded in the same manner as in test piece 1, to obtain test pieces 7 to 10.

[0093] 3. Evaluation The above test pieces were used to carry out the following evaluations.

[0094] 3-1. Bending test A bending test was performed at 23°C in accordance with JIS K7171 using a dumbbell-shaped test piece for evaluation. A linear regression was performed between 0.05% and 0.25% strain on the stress-strain curve obtained by the bending test at a test speed of 2 mm / min to determine the bending modulus FM (GPa). The first maximum stress measured in a tensile test at a test speed of 5 mm / min was taken as the bending strength FS (MPa).

[0095] 3-2.Tensile test Using a dumbbell-shaped test piece for evaluation, a tensile test was performed in a 23°C environment in accordance with JIS K7161. A linear regression was performed between 0.05% and 0.25% strain on the stress-strain curve obtained by the tensile test at a test speed of 2 mm / min to determine the tensile modulus TM (GPa). The first maximum stress measured in the tensile test at a test speed of 5 mm / min was taken as the tensile strength TS (MPa).

[0096] 3-3.Charpy impact resistance test The dumbbell-shaped test specimen for evaluation testing was processed into a shape (Type 1) with a V-shaped notch conforming to JIS K7111, and the impact resistance value (KJ / m 2 ) was sought.

[0097] 3-4. Tensile creep strain Using dumbbell-shaped test pieces for evaluation testing, a tensile creep test was performed in a 120°C environment with an initial stress of 20 MPa and a test time of 500 hours in accordance with JIS K7115. The difference in strain between the strain value after the 500-hour tensile creep test and the creep value at 0 hours (initial time) was taken as the tensile creep strain.

[0098] 3-5. Dry fiber ratio and degree of impregnation Each pellet-shaped fiber-reinforced resin composition was put into a foreign matter separator (Pelletron-20, manufactured by Pelletron Corporation) and classified using internal compressor air. The air pressure was set to 0.2 MPa to separate dry fibers (glass fibers not impregnated with resin), and the separated dry fibers were weighed. The dry fiber ratio was calculated using the following formula. Dry Fiber Ratio = (mass of separated dry fiber (g) / mass of pelletized fiber reinforced resin composition (g) ×100 (%)

[0099] Then, based on the calculated dry fiber ratio, the degree of impregnation of the resin component for each fiber reinforced resin composition was evaluated according to the following criteria. Dry fiber ratio is less than 0.2% by mass × Dry fiber ratio is 0.2% by mass or more

[0100] 3-6. Average equivalent circle diameter of dispersed phase The center of the dumbbell-shaped test piece for evaluation was cut, and the resulting small piece was embedded in resin. The embedded small piece was trimmed to prepare an ultrathin section, and carbon deposition was performed. Then, an image of PA dispersed in the section was taken with a transmission electron microscope (Hitachi High-Tech Corporation, H-7650). The obtained transmission electron microscope image was analyzed using image analysis software (WinROOF2018), and the particle size equivalent to the dispersed phase of PA was calculated by blob analysis. Specifically, binarization was performed at the boundary between the PA dispersed phase and the other resin parts, and the circular equivalent diameter of the PA dispersed phase was calculated. This circular equivalent diameter was calculated at 300 points, and the average value was taken as the average circular equivalent diameter of the dispersed phase.

[0101] 3-7.PP / PA interface peeling Transmission electron microscope images were taken at 20 different locations using the method described above in "3-6. Average equivalent circle diameter of dispersed phase," and the images were visually observed to determine whether interfacial peeling occurred between PP and PA. The transmission electron microscope images were evaluated according to the following criteria based on the number of images in which interfacial peeling was observed among the 20 images. Interfacial peeling was observed in less than 4 out of 20 images. × Interfacial peeling was observed in 4 or more of the 20 images.

[0102] 4.Results Tables 1 and 2 show the composition of the fiber-reinforced resin composition and the evaluation results of the test pieces prepared in each experiment.

[0103] [Table 1]

[0104] [Table 2]

[0105] As is clear from Tables 1 and 2, the fiber-reinforced resin composition contains an unmodified polyolefin (A), a polyamide (B) having a structural unit derived from a monomer having 10 or more carbon atoms, a reinforcing fiber (C), and a modified polyolefin (D), and when the total content of the polyolefin (A), the polyamide (B), and the reinforcing fiber (C) is 100 parts by mass, the content of the polyolefin (A) is 40 parts by mass or more and 80 parts by mass or less, the content of the polyamide (B) is 1 part by mass or more and 20 parts by mass or less, the content of the reinforcing fiber (C) is 10 parts by mass or more and 50 parts by mass or less, and the content of the modified polyolefin (D) is 1 part by mass or more and 5 parts by mass or less. While suppressing interfacial peeling between the polyolefin and the polyamide in the molded body, it was also possible to suppress a decrease in bending properties and tensile properties and an increase in tensile creep strain. [Industrial Applicability]

[0106] According to the present invention, a molded article having various excellent physical properties can be produced.

Claims

1. An unmodified polyolefin (A); A polyamide (B) having a structural unit derived from a monomer having 10 or more carbon atoms; Reinforcing fibers (C); A modified polyolefin (D), When the total content of the polyolefin (A), the polyamide (B) and the reinforcing fiber (C) is 100 parts by mass, The content of the polyolefin (A) is 20 parts by mass or more and 80 parts by mass or less, The content of the polyamide (B) is 1 part by mass or more and 20 parts by mass or less, The content of the reinforcing fiber (C) is 10 parts by mass or more and 70 parts by mass or less, The content of the modified polyolefin (D) is 1 part by mass or more and 5 parts by mass or less. Fiber reinforced resin composition.

2. When the total content of the polyolefin (A), the polyamide (B) and the reinforcing fiber (C) is 100 parts by mass, The content of the polyolefin (A) is 35 parts by mass or more and 55 parts by mass or less, The content of the reinforcing fiber (C) is 40 parts by mass or more and 60 parts by mass or less, The fiber reinforced resin composition according to claim 1.

3. The reinforcing fibers (C) are bundled with an acrylic sizing agent or a polyamide sizing agent. The fiber reinforced resin composition according to claim 1.

4. the polyolefin (A) and the polyamide (B) form a sea-island structure in which a dispersed phase of the polyamide (B) is dispersed in a continuous phase of the polyolefin (A), The average equivalent circular diameter of the dispersed phase is 1.0 μm or less. The fiber reinforced resin composition according to claim 1.

5. The polyamide (B) is polyamide 12. The fiber reinforced resin composition according to claim 1.

6. The polyolefin (A) is polypropylene. The fiber reinforced resin composition according to claim 1.

7. The reinforcing fiber (C) is a glass fiber or a carbon fiber. The fiber reinforced resin composition according to claim 1.

8. A molded article obtained by molding the fiber reinforced resin composition according to any one of claims 1 to 7.

9. The molded article according to claim 8, which is an automobile part.

Citation Information

Patent Citations

  • Fiber-reinforced resin composition and its production method

    JP2019210379A