Adhesive sheet, method for manufacturing electronic component, and method for manufacturing adhesive sheet
The adhesive sheet with a rubber-based elastomer and silicone resin composition addresses transmission loss and adhesion issues in high-frequency electronic devices, maintaining performance and resistance to high temperatures.
Patent Information
- Application Number
- JP2023215910
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2023-12-21
- Publication Date
- 2024-10-03
AI Technical Summary
The increasing frequency of transmission signals in electronic devices, particularly in 5G systems, leads to higher transmission loss, and existing adhesive sheets fail to adequately suppress this loss while maintaining adhesion and heat resistance, especially when exposed to high temperatures, which can cause foaming and deterioration of adhesive properties.
An adhesive sheet with a specific composition including a rubber-based elastomer, a silicone resin, and a radical inhibitor, with a dielectric loss tangent of 0.003 or less at 10 GHz, a gel fraction of 30% or more, and a 90° peel force of 5.0 N/25 mm or more, which is crosslinked using energy ray irradiation without introducing polar groups, ensuring low dielectric properties and heat resistance.
The adhesive sheet effectively suppresses transmission loss, maintains adhesion even at high frequencies, and prevents foaming and deterioration of appearance and function after peeling, ensuring reliable performance in high-temperature environments.
Smart Images

Figure 2024134512000006 
Figure 2024134512000007 
Figure 2024134512000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive sheet. The present invention also relates to a method for producing an electronic component using the pressure-sensitive adhesive sheet, and a method for producing the pressure-sensitive adhesive sheet. [Background technology]
[0002] Adhesive sheets are widely used in a variety of fields, for example, for assembling portable electronic devices such as mobile phones and personal digital assistants (PDAs), or for fixing in-vehicle electronic device components such as in-vehicle panels to the vehicle body (e.g., Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2009-242541 A [Patent Document 2] JP 2009-258274 A Summary of the Invention [Problem to be solved by the invention]
[0004] In recent years, in the field of electronic devices, there has been a demand for faster transmission and reception of larger volumes of data, and the practical application of the so-called fifth generation mobile communication system (5G) is also progressing, which is accompanied by an increase in the frequency of transmitted signals. However, this increase in frequency has given rise to a problem in that the amount of attenuation of the transmitted signals (called "transmission loss") increases. There is a demand for pressure-sensitive adhesive sheets capable of suppressing such transmission loss as pressure-sensitive adhesive sheets used in electronic devices. For example, in small antenna base stations, vehicle-mounted antennas, etc., film-based structures have been increasingly adopted in recent years, and there is a demand for pressure-sensitive adhesive sheets capable of suppressing transmission loss and being suitably used even when the transmission signal is at a high frequency as pressure-sensitive adhesive sheets used for bonding between internal members of such antenna films or bonding between antenna films and other members.
[0005] Since the transmission loss increases in proportion to the frequency, it is inevitable that the transmission loss increases as the frequency of the transmission signal increases. Since the transmission loss is affected not only by the frequency but also by the dielectric constant and dielectric loss tangent of the insulating part present around the conductive part, in order to suppress the transmission loss in the high frequency band (for example, around 1 to 80 GHz), it is expected that the transmission loss can be suppressed, for example, by using an adhesive sheet with a small dielectric loss tangent and excellent low dielectric properties in the high frequency band.
[0006] On the other hand, for example, antennas such as small antenna base stations and vehicle-mounted antennas are often used outdoors, so the adhesive sheets used for bonding between internal members of the antenna film or bonding between the antenna film and other members are exposed to high temperatures (about 120°C). When an adhesive sheet attached to an adherend (other member) is exposed to high temperatures, outgassing may occur from the adherend, or microbubbles that have entered between the adherend and the adhesive sheet due to insufficient adhesion to the adherend may grow larger at high temperatures, causing foaming at the interface between the adherend and the adhesive sheet, resulting in a decrease in adhesive strength. In addition, foaming at the interface between the adherend and the adhesive sheet may change the dielectric properties in the high frequency band, adversely affecting signal transmission.
[0007] A method for crosslinking the base resin constituting the adhesive layer of an adhesive sheet is irradiation with energy rays such as electron beams (EB). Energy ray irradiation allows crosslinking to proceed without introducing polar groups into the base resin, and therefore can improve the low dielectric properties and heat resistance of the adhesive sheet. However, when an adhesive sheet in which the base resin has been crosslinked by energy ray irradiation is used, the separator becomes difficult to peel off, and when the separator is peeled off, the appearance, adhesiveness, and other functions may be impaired. On the other hand, when the base resin is crosslinked by energy ray irradiation after the separator is peeled off, the low dielectric properties may deteriorate due to the radicals derived from the base resin generated by energy ray irradiation combining with oxygen in the air.
[0008] The present invention aims to provide a pressure-sensitive adhesive sheet that can be suitably used even when the transmission signal is at a high frequency, has excellent heat resistance, and is capable of suppressing impairment of appearance and function after peeling off a separator. The present invention also aims to provide a method for producing an electronic component using the pressure-sensitive adhesive sheet, and a method for producing the pressure-sensitive adhesive sheet. [Means for solving the problem]
[0009] Disclosure 1 is a pressure-sensitive adhesive sheet having an adhesive layer formed using an adhesive containing a base resin and a separator on at least one surface of the adhesive layer, wherein the base resin contains a rubber-based elastomer, the adhesive layer has a dielectric tangent of 0.003 or less at a frequency of 10 GHz and a gel fraction of 30 mass% or more, the separator has a separator substrate and a release agent layer, the release agent layer contains a silicone resin and a radical inhibitor, and the content of the radical inhibitor in the release agent layer per 100 mass parts of the silicone resin is 0.1 part by mass or more and 10 parts by mass or less. Disclosure 2 is an adhesive sheet having an adhesive layer formed using an adhesive containing a base resin and a separator on at least one surface of the adhesive layer, the base resin containing a rubber-based elastomer, the adhesive layer having a dielectric tangent of 0.003 or less at a frequency of 10 GHz and a gel fraction of 30 mass% or more, the separator having a separator substrate and a release agent layer, the release agent layer containing a silicone resin and a radical inhibitor, the content of the radical inhibitor in the release agent layer being 0.1 part by mass or more and 10 parts by mass or less per 100 parts by mass of the silicone resin, and the separator having a 180° peel force from the adhesive layer of 1.0 N / 25 mm or less. The present disclosure 3 is the pressure-sensitive adhesive sheet according to the present disclosure 1 or 2, wherein the pressure-sensitive adhesive layer has a 90° peel strength from glass of 5.0 N / 25 mm or more. The present disclosure 4 is the pressure-sensitive adhesive sheet according to the present disclosure 1, 2, or 3, wherein the rubber-based elastomer comprises at least one selected from the group consisting of a styrene-based elastomer and a hydrogenated styrene-based elastomer. A fifth aspect of the present disclosure is the pressure-sensitive adhesive sheet of the fourth aspect of the present disclosure, wherein the rubber-based elastomer comprises a hydrogenated styrene-based elastomer. A sixth aspect of the present disclosure is the pressure-sensitive adhesive sheet according to the fifth aspect of the present disclosure, wherein the hydrogenated styrene-based elastomer is a hydrogenated product of a block copolymer having an aromatic alkenyl polymer block and a conjugated diene polymer block. The present disclosure 7 is the pressure-sensitive adhesive sheet of the present disclosure 6, wherein the hydrogenated product of the block copolymer having the aromatic alkenyl polymer block and the conjugated diene polymer block is a hydrogenated product of a radial type block copolymer represented by the following formula (1): The present disclosure 8 is the pressure-sensitive adhesive sheet of the present disclosure 1, 2, 3, 4, 5, 6, or 7, wherein the pressure-sensitive adhesive further contains a crosslinking auxiliary, and the content of the crosslinking auxiliary per 100 parts by mass of the base resin is 15 parts by mass or less. A ninth aspect of the present disclosure is the pressure-sensitive adhesive sheet according to the eighth aspect of the present disclosure, wherein the crosslinking aid comprises a (meth)acrylic monomer. The present disclosure 10 is the PSA sheet of the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, or 9, wherein the PSA further contains a tackifier resin, and the tackifier resin includes a tackifier resin having no carbon-carbon double bond. The present disclosure 11 is the pressure-sensitive adhesive sheet of the present disclosure 10, wherein the tackifier resin is composed solely of a tackifier resin having no carbon-carbon double bond. Present Disclosure 12 is the PSA sheet of Present Disclosure 10 or 11, wherein the content of the tackifier resin per 100 parts by mass of the base resin is 20 parts by mass or more and 80 parts by mass or less. The present disclosure 13 is a pressure-sensitive adhesive sheet according to the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12, which is a non-support type having no substrate other than the separator substrate. Disclosure 14 is the adhesive sheet of Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or 13 used in manufacturing a device that transmits or receives electromagnetic waves with a frequency of 1 GHz or more. Disclosure 15 is a method for producing an electronic component, comprising a step of bonding internal components of a laminate including a film having a conductive pattern formed thereon via an adhesive sheet of Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, or 14 from which the separator has been peeled off, or a step of bonding a laminate including a film having a conductive pattern formed thereon to another component via an adhesive sheet of Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, or 14 from which the separator has been peeled off. The present disclosure 16 is a method for producing a pressure-sensitive adhesive sheet according to the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, or 14, comprising a step of irradiating an energy ray from the separator side of a laminate having a layer containing the pressure-sensitive adhesive and the separator on at least one side of the layer containing the pressure-sensitive adhesive, in the direction of the layer containing the pressure-sensitive adhesive.
[0010] [ka]
[0011] In formula (1), A is an aromatic alkenyl polymer block, B is a conjugated diene polymer block, C is a segment derived from a coupling agent, and n is an integer of 3 or more. The present invention will be described in detail below.
[0012] The present inventors have investigated an adhesive sheet having an adhesive layer made of an adhesive containing a rubber-based elastomer as a base resin and a separator on at least one side of the adhesive layer, by adjusting the dielectric tangent and gel fraction of the adhesive layer and by making the separator have a release agent layer containing a silicone resin and a radical inhibitor at a specific content ratio. As a result, they have found that an adhesive sheet can be obtained that can be suitably used even when the transmission signal is at a high frequency, has excellent heat resistance, and can suppress the deterioration of appearance and function after the separator is peeled off, and have completed the present invention.
[0013] The pressure-sensitive adhesive sheet of the present invention has a pressure-sensitive adhesive layer formed using a pressure-sensitive adhesive containing a base resin. The adhesive layer has an upper limit of the dielectric loss tangent at a frequency of 10 GHz of 0.003. Since the dielectric loss tangent at a frequency of 10 GHz of the adhesive layer is 0.003 or less, the adhesive sheet of the present invention can be suitably used even when the transmission signal has a high frequency. The preferred upper limit of the dielectric loss tangent at a frequency of 10 GHz of the adhesive layer is 0.002, and the more preferred upper limit is 0.001. The lower limit of the dielectric loss tangent at a frequency of 10 GHz of the adhesive layer is not particularly limited, and the lower the better. The dielectric tangent of the adhesive layer at a frequency of 10 GHz can be measured in accordance with JIS C2565, for example, in an environment of 23°C and 50% RH using a dielectric constant measuring device (such as "ADMS01Nc" manufactured by AET Corporation) in the measurement mode of a TM mode resonator.
[0014] Examples of the method for adjusting the dielectric tangent of the adhesive layer at a frequency of 10 GHz within the above range include a method for adjusting the composition or content of the base resin described below, a method for reducing the molecular polarizability (for example, a method for introducing fluorine atoms, hydrocarbon groups, etc.), a method for increasing the molecular volume (for example, a method for introducing an alicyclic structure), etc. Also included are a method for mixing a substance exhibiting a low dielectric tangent into the adhesive layer (for example, a method for blending a filler such as a hollow cell, a fluorine filler, a silica filler, or a glass fiber). Furthermore, examples of the method for reducing the mobility of the molecules contained in the adhesive layer (for example, a method for blending a crystalline polymer), a method for increasing the average molecular weight of the polymer contained in the adhesive layer, and a method for reducing the water absorption rate or water content of the polymer contained in the adhesive layer (for example, a method for introducing fluorine atoms or a substituent, a method for introducing a hydrocarbon group), etc.
[0015] The adhesive layer has a gel fraction of 30% by mass or more. When the gel fraction of the adhesive layer is 30% by mass or more, the adhesive sheet of the present invention is less likely to foam at the interface with the adherend even in a high-temperature environment, and the heat resistance is improved. The preferred lower limit of the gel fraction of the adhesive layer is 35% by mass, and the more preferred lower limit is 40% by mass. From the viewpoint of suppressing the generation of foaming at the interface with the adherend in a high-temperature environment while at the same time achieving superior adhesive strength, the upper limit of the gel fraction of the adhesive layer is preferably 70% by mass. The gel fraction of the pressure-sensitive adhesive layer can be measured, for example, as follows. That is, the separator of the adhesive sheet is peeled off to collect the adhesive layer (mass: W0 (g)), and the collected adhesive layer is immersed in 50 mL of toluene and shaken in a shaker at 23°C and 200 rpm for 24 hours. After shaking, the adhesive layer that has absorbed and swollen with toluene is filtered using a metal mesh (opening #200 mesh, mass: W1 (g)). The separated adhesive layer is dried at 110°C for 1 hour, and the mass W2 (g) of the adhesive layer including the metal mesh is measured. Then, the gel fraction can be calculated from the obtained W0, W1, and W2 using the following formula (I). Gel fraction (mass%) = 100 × (W2-W1) / W0(I)
[0016] Examples of the method for adjusting the gel fraction of the adhesive layer within the above range include a method in which the adhesive layer is formed by crosslinking a base resin, a tackifier resin, etc. described below, and then adjusting the type and amount of the base resin, the tackifier resin, etc., or a method for adjusting the crosslinking conditions, etc. Examples of the method for adjusting the crosslinking conditions include a method for adjusting the type and amount of a crosslinking reaction initiator that causes a crosslinking reaction, a crosslinking assistant that promotes crosslinking, etc., a method for adjusting the irradiation intensity and irradiation time of UV light, which is an energy ray that promotes crosslinking, a method for adjusting the irradiation intensity, irradiation time, and acceleration voltage of electron beam irradiation, and a method for adjusting the type and amount of a crosslinking inhibitor, etc. Examples of the crosslinking method include a method of crosslinking a base resin or a tackifier resin by irradiating them with energy rays such as UV light or electron beams, which will be described later, and a method of introducing a crosslinkable functional group into the base resin or the tackifier resin, grafting the functional group by irradiating them with electron beams, and then crosslinking the functional group by heat. In particular, when the crosslinking method by irradiating them with energy rays such as UV light or electron beams is used, crosslinking can proceed without introducing a polar group into the base resin or the tackifier resin, so that the gel fraction of the adhesive layer can be easily adjusted within the above range while the dielectric loss tangent at a frequency of 10 GHz of the adhesive layer satisfies an appropriate range, and the adhesive sheet obtained can be more suitably used even when the transmission signal is at a high frequency, and has better heat resistance. Among these, the method of crosslinking by irradiating electron beams is more preferable from the viewpoint of increasing the production speed of the adhesive sheet.
[0017] The adhesive layer has a preferred lower limit of 5.0 N / 25 mm in 90° peel strength against glass. When the adhesive layer has a 90° peel strength against glass of 5.0 N / 25 mm or more, bubbles are less likely to form at the interface with the adherend even in a high-temperature environment. A more preferred lower limit of the adhesive layer's 90° peel strength against glass is 7.0 N / 25 mm, and an even more preferred lower limit is 10 N / 25 mm. There is no particular preferred upper limit of the adhesive layer's 90° peel strength against glass, but the substantial upper limit is 30 N / 25 mm. The 90° peel strength of the pressure-sensitive adhesive layer from glass can be measured by the following method. That is, first, the adhesive sheet is cut into a flat rectangular shape with a length of 100 mm and a width of 25 mm, and then the separator is peeled off, and a cycloolefin film (e.g., "ZF16-100 μm" manufactured by Nippon Zeon Co., Ltd.) is laminated on the exposed adhesive layer. The other separator of the adhesive sheet is peeled off to expose the adhesive surface, and the exposed adhesive surface is placed on a glass plate (e.g., float plate glass "FL3" manufactured by AGC Co., Ltd.). The surface of the glass plate is washed with ethanol, wiped dry, and visually confirmed to be free of scratches before use. A 2.0 kg rubber roller is rolled back and forth once on the cycloolefin film at a speed of 300 mm / min, and the film is left to stand at 23°C for 24 hours to prepare a test piece. The obtained test piece is peeled off in the 90° direction at 23°C and a tensile speed of 50 mm / min using a tensile tester (e.g., "AG-IS" manufactured by Shimadzu Corporation, etc.) to measure the adhesive strength (90° peel strength). When the pressure-sensitive adhesive sheet is a single-sided tape, the measurement is performed without using a cycloolefin film.
[0018] Examples of methods for adjusting the 90° peel strength of the adhesive layer against glass within the above range include a method for adjusting the type and amount of a base resin or a tackifier resin, etc., which will be described later, a method for modifying the surface of the adhesive layer by a plasma treatment method or a corona treatment method, etc. Also included are a method for decreasing the styrene content of a rubber-based elastomer, a method for increasing the proportion of a diblock structure in the rubber-based elastomer, a method for increasing the thickness of the adhesive layer, a method for incorporating a filler into the adhesive layer, etc.
[0019] The pressure-sensitive adhesive contains a base resin. The base resin includes a rubber-based elastomer. The rubber-based elastomer preferably contains at least one selected from the group consisting of styrene-based elastomers and hydrogenated styrene-based elastomers. In particular, the rubber-based elastomer preferably contains the hydrogenated styrene-based elastomer, since the double bond (unsaturated bond) content is low, and therefore the resulting pressure-sensitive adhesive sheet has better heat resistance and is less susceptible to changes in optical properties in a high-temperature environment. In addition, the hydrogenated styrene-based elastomer has a smaller dielectric constant and dielectric loss tangent in a high-frequency band than acrylic polymers and the like. Therefore, by containing the hydrogenated styrene-based elastomer as a base resin in the pressure-sensitive adhesive, the dielectric loss tangent of the pressure-sensitive adhesive layer at a frequency of 10 GHz is more likely to satisfy an appropriate range, and the resulting pressure-sensitive adhesive sheet can be more suitably used even when the transmission signal is at a high frequency. The hydrogenated styrene-based elastomer may be a partially hydrogenated product or a completely hydrogenated product. Among them, hydrogenated styrene-based elastomers in which 80% or more of the double bonds (unsaturated bonds) of the repeating units derived from the conjugated diene compound described later are converted to saturated bonds by hydrogenation, that is, hydrogenated styrene-based elastomers having a hydrogenation rate of 80% or more are preferred. The lower limit of the hydrogenation rate of the hydrogenated styrene-based elastomer is more preferably 90%, even more preferably 95%, and even more preferably 96%. The hydrogenation rate of the hydrogenated styrene-based elastomer is measured by using deuterated chloroform as a solvent and heating at 20 Hz. 1 It can be calculated by measuring the H-NMR spectrum.
[0020] The hydrogenated styrene-based elastomer is preferably a hydrogenated product of a block copolymer having an aromatic alkenyl polymer block and a conjugated diene polymer block.
[0021] The hydrogenated product of the block copolymer having the aromatic alkenyl polymer block and the conjugated diene polymer block is not particularly limited as long as it has rubber elasticity at room temperature and has a hard segment and a soft segment, where the aromatic alkenyl polymer block is the hard segment and the conjugated diene polymer block is the soft segment.
[0022] The aromatic alkenyl polymer block represented by A means a block having a repeating unit derived from an aromatic alkenyl compound. The aromatic alkenyl polymer block represented by A may contain, in addition to the repeating units derived from the aromatic alkenyl compound, repeating units derived from other compounds such as ethylene and 1,3-butadiene (which are converted to an ethylene-butylene structure by hydrogenation).
[0023] Examples of the aromatic alkenyl compound include alkylstyrenes, halogenated styrenes, halogen-substituted alkylstyrenes, alkoxystyrenes, carboxyalkylstyrenes, alkyl ether styrenes, alkylsilylstyrenes, vinylbenzyl dimethoxyphosphide, vinylnaphthalene, vinylanthracene, N,N-diethyl-p-aminoethylstyrene, and vinylpyridine. Examples of the alkylstyrene include styrene, methylstyrene, dimethylstyrene, and t-butylstyrene. Examples of the halogenated styrene include chlorostyrene, bromostyrene, and fluorostyrene. The halogen-substituted alkylstyrene includes, for example, chloromethylstyrene. Examples of the alkoxystyrene include methoxystyrene and ethoxystyrene. The carboxyalkylstyrene may, for example, be carboxymethylstyrene. The alkyl ether styrene includes, for example, vinylbenzyl propyl ether. The alkylsilylstyrene may, for example, be trimethylsilylstyrene. These aromatic alkenyl compounds may be used alone or in combination of two or more. Among them, styrene, methylstyrene, and dimethylstyrene are preferred, and styrene is more preferred because it is easily available industrially.
[0024] The conjugated diene polymer block represented by B means a block having a repeating unit derived from a conjugated diene compound. The conjugated diene polymer block represented by B may contain, in addition to the repeating units derived from the conjugated diene compound, repeating units derived from other compounds such as ethylene and 2,5-dihydrofuran-2,5-dione.
[0025] Examples of the conjugated diene compound include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-octadiene, 1,3-hexadiene, 1,3-cyclohexadiene, 4,5-diethyl-1,3-octadiene, 3-butyl-1,3-octadiene, myrcene, and chloroprene. These conjugated diene compounds may be used alone or in combination of two or more. Among them, 1,3-butadiene and isoprene are preferred because they have high polymerization reactivity and are easily available industrially.
[0026] Specific examples of the hydrogenated product of the block copolymer having the aromatic alkenyl polymer block and the conjugated diene polymer block include a hydrogenated product of a block copolymer having a structure represented by the formula ABA, a hydrogenated product of a radial block copolymer having a structure represented by the formula (1), and the like. Among them, a hydrogenated product of a radial block copolymer having a structure represented by the formula (1) is preferred. By using a hydrogenated product of a radial block copolymer having a structure represented by the formula (1), crosslinking proceeds well, so that the gel fraction of the adhesive layer is more likely to satisfy an appropriate range, and the resulting adhesive sheet has better heat resistance. In addition, by the adhesive containing a hydrogenated product of a radial block copolymer having a structure represented by the formula (1), the adhesive strength of the adhesive layer is further improved, and foaming at the interface between the adhesive sheet and the adherend in a high-temperature environment is more unlikely to occur. Furthermore, the improved adhesive strength of the adhesive layer allows the content of a tackifier resin (particularly, a tackifier resin (T2) that is prone to self-polymerization as described below) to be reduced.
[0027] Examples of the hydrogenated block copolymer having the structure represented by the above formula ABA include styrene-ethylene-butylene-styrene (SEBS) block copolymer, styrene-ethylene-propylene-styrene (SEPS) block copolymer, styrene-ethylene-ethylene-propylene-styrene (SEEPS) block copolymer, and styrene-isobutylene-styrene (SIBS) block copolymer. Among them, SEBS block copolymers are preferred because crosslinking proceeds well and the gel fraction of the adhesive layer is more likely to satisfy the appropriate range, and branched SEBS block copolymers are more preferred. The number of branches in the branched SEBS block copolymer is preferably 2 or more from the viewpoint of crosslinking proceeding well.
[0028] The hydrogenated product of the radial block copolymer having the structure represented by the above formula (1) is a hydrogenated product of a branched styrene-based block copolymer having a structure in which multiple diblock structures (AB), each of which is formed by bonding one of the above hard segments and one of the above soft segments, protrude radially from the segment (C) derived from the coupling agent at the center. In the above formula (1), n may be an integer of 3 or more, but is preferably 4 or more in order to further improve the adhesive strength of the adhesive layer. In addition, the upper limit of n in the above formula (1) is not particularly limited, but is usually 8 or less in order to prevent the hydrogenated product of the radial block copolymer having the structure represented by the above formula (1) from becoming too hard.
[0029] The coupling agent from which the coupling agent-derived segment represented by C is derived is a polyfunctional compound that radially bonds the diblock structure (AB). Examples of the coupling agent include silane compounds such as halogenated silanes and alkoxysilanes, tin compounds such as tin halides, epoxy compounds such as epoxysilanes and epoxidized soybean oil, (meth)acrylic esters such as pentaerythritol tetra(meth)acrylate, divinyl compounds such as divinylbenzene, polycarboxylic acid esters, etc. Specific examples include trichlorosilane, tribromosilane, tetrachlorosilane, tetrabromosilane, methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, tetramethoxysilane, tetraethoxysilane, tetrachlorotin, diethyl adipate, etc. In this specification, the term "(meth)acrylate" means acrylate or methacrylate, and the term "(meth)acrylic" means acrylic or methacrylic.
[0030] The preferred lower limit of the content of the aromatic alkenyl polymer block represented by A in the hydrogenated product of the radial block copolymer having the structure represented by formula (1) is 5% by mass, and the preferred upper limit is 30% by mass. When the content of the aromatic alkenyl polymer block represented by A is within this range, the adhesive strength of the adhesive layer is further improved. The more preferred lower limit of the content of the aromatic alkenyl polymer block represented by A in the hydrogenated product of the radial block copolymer having the structure represented by formula (1) is 8% by mass, and the more preferred upper limit is 25% by mass, and the even more preferred lower limit is 9% by mass, and the even more preferred upper limit is 20% by mass.
[0031] The preferred upper limit of the styrene content of the hydrogenated styrene-based elastomer is 30% by mass. By making the styrene content 30% by mass or less, the adhesive layer has a suitable adhesive strength, and the dielectric loss tangent of the adhesive layer at a frequency of 10 GHz is more likely to satisfy the appropriate range, so that the adhesive sheet obtained can be more suitably used even when the transmission signal is at a high frequency. The more preferred upper limit of the styrene content is 20% by mass. From the viewpoint of maintaining the cohesive strength of the adhesive layer, a preferable lower limit of the styrene content is 8 mass %. In this specification, the "styrene content" is derived from the mass ratio (r1) of the aromatic alkenyl compound before polymerization. That is, the styrene content (R1) (mass%) can be calculated as 100×r1 (mass%) using the mass ratio (r1) of the aromatic alkenyl compound before polymerization: (mass of aromatic alkenyl compound before polymerization) / (mass of aromatic alkenyl compound before polymerization+mass of conjugated diene compound before polymerization). In addition, when the mass ratio of the aromatic alkenyl compounds before polymerization is unknown, 1The styrene content can be predicted from the molar ratio (r2) of the aromatic alkenyl polymer block obtained from the peak area ratio of each block measured by H-NMR. That is, the styrene content (R2) (mol%) can be predicted as 100×r2 (mol%) using the molar ratio (r2) of the aromatic alkenyl polymer block: (molar ratio of aromatic alkenyl polymer block) / (molar ratio of aromatic alkenyl polymer block+molar ratio of conjugated diene polymer block). The styrene content (R2) is different from the styrene content (R1), but in the case of the SEBS block copolymer, for example, there is the following tendency. Styrene content (R1): 10% by mass, Styrene content (R2): 4 mol% to 7.9 mol% Styrene content (R1): 15% by mass, Styrene content (R2): 8% by mol or more and 9.9% by mol or less Styrene content (R1): 20% by mass, Styrene content (R2): 10% by mol or more and 15% by mol or less Styrene content (R1): 30% by mass, Styrene content (R2): 15% by mol or more and 20% by mol or less When using a commercially available product whose catalog states its styrene content, that value shall be used as the styrene content.
[0032] The weight average molecular weight of the rubber elastomer is preferably 100,000 at its lower limit. The weight average molecular weight of the rubber elastomer is 100,000 or more, so that the adhesive strength of the adhesive layer is improved, and the dielectric tangent of the adhesive layer at a frequency of 10 GHz is more likely to fall within an appropriate range, and the adhesive sheet obtained can be more suitably used even when the transmission signal is at a high frequency. The weight average molecular weight of the rubber elastomer is more preferably 200,000 at its lower limit, and even more preferably 250,000 at its lower limit. In addition, there is no particular preferred upper limit to the weight average molecular weight of the rubber-based elastomer. However, the larger the weight average molecular weight of the rubber-based elastomer, the greater the adhesive strength of the adhesive layer can be, but the greater the viscosity of the adhesive increases and the lower the processability. Therefore, from the standpoint of production of the adhesive sheet, the substantial upper limit is 700,000. In this specification, the term "weight average molecular weight" refers to a weight average molecular weight measured as a polystyrene equivalent molecular weight by gel permeation chromatography (GPC). The weight average molecular weight can be measured by the GPC method, for example, as follows. That is, first, a solution in which a rubber-based elastomer is dissolved in tetrahydrofuran (THF) is filtered through a filter (material: polytetrafluoroethylene, pore size: 0.2 μm) to obtain a GPC test solution. The obtained GPC test solution was analyzed using a GPC system, "ACQUITY TM Advanced Polymer Chromatography TM The GPC column was Waters' HSPgel TM GPC measurements are performed using a HR MB-M (6.0 mm x 150 mm) and a differential refractive index detector (Waters, "2414") as a detector. The sample injection amount is 20 mg / mL, the solution is 10 μL, the flow rate is 0.5 mL / min, and the column temperature is 40°C. Empower3, which comes with the device, is used as the analysis software. Polystyrene (peak top molecular weight: 2110000, 1090000, 427000, 190000, 37900, 18100, 5970, 2420, 500) (Tosoh Corporation) is used as a standard. The polystyrene standard is measured, and a calibration curve is created using analysis software to convert the elution volume into the polystyrene molecular weight, and the weight average molecular weight is converted from the GPC elution volume using this calibration curve.
[0033] The preferred lower limit of the content of the rubber-based elastomer in 100 parts by mass of the base resin is 80 parts by mass. By having the content of the rubber-based elastomer be 80 parts by mass or more, the resulting pressure-sensitive adhesive sheet is less likely to foam at the interface with the adherend in a high-temperature environment, and the dielectric loss tangent of the pressure-sensitive adhesive layer at a frequency of 10 GHz is more likely to satisfy the range, making it more suitable for use even when the transmission signal is at a high frequency. The more preferred lower limit of the content of the rubber-based elastomer is 90 parts by mass. There is no particular upper limit to the amount of the rubber elastomer, and it may be 100 parts by mass. That is, the base resin may consist of only the rubber elastomer.
[0034] The pressure-sensitive adhesive preferably further contains a crosslinking auxiliary. When the pressure-sensitive adhesive contains a crosslinking aid, crosslinking of the base resin proceeds well, the gel fraction of the pressure-sensitive adhesive layer is more likely to fall within an appropriate range, and the heat resistance of the resulting pressure-sensitive adhesive sheet is further improved.
[0035] Examples of the crosslinking aid include (meth)acrylic monomers and triallyl isocyanurate. These crosslinking aids are easily radicalized, so that the adhesive layer contains these crosslinking aids, and crosslinking of the base resin by energy ray irradiation proceeds well. As a result, the gel fraction of the adhesive layer is more likely to fall within an appropriate range, and the heat resistance of the adhesive sheet of the present invention is further improved. Among them, the crosslinking aid preferably contains the (meth)acrylic monomer.
[0036] Examples of the (meth)acrylic monomer include (meth)acrylic acid esters that are generally used as monomers constituting (meth)acrylic copolymers. The number of functional groups of the (meth)acrylic monomer may be any of bifunctional, trifunctional, tetrafunctional, pentafunctional, hexafunctional, etc. Specific examples of the (meth)acrylic monomer include ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc. These (meth)acrylic monomers may be used alone or in combination of two or more. Among them, methacrylic acid esters are preferred from the viewpoint of efficient crosslinking. In addition, it is preferred that they have good compatibility with the rubber elastomer, can more efficiently crosslink the rubber elastomer, and have little effect on the dielectric properties of the pressure-sensitive adhesive sheet of the present invention. Therefore, among the above methacrylic acid esters, neopentyl glycol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, and trimethylolpropane trimethacrylate are more preferable.
[0037] The content of the crosslinking aid is preferably 15 parts by mass or less relative to 100 parts by mass of the base resin. By making the content of the crosslinking aid 15 parts by mass or less, the crosslinking aid does not bleed out, and the adhesive strength of the adhesive layer is further improved. The content of the crosslinking aid is more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less. In addition, the preferred lower limit of the content of the crosslinking aid is 2 parts by mass. By having the content of the crosslinking aid be 2 parts by mass or more, the crosslinking of the rubber-based elastomer proceeds well, the gel fraction of the adhesive layer is more likely to fall within an appropriate range, and the heat resistance of the resulting adhesive sheet is further improved. The more preferred lower limit of the content of the crosslinking aid is 3 parts by mass, and the even more preferred lower limit is 4 parts by mass.
[0038] The pressure-sensitive adhesive preferably further contains a tackifier resin. By including a tackifier resin in the pressure-sensitive adhesive, the adhesive strength of the pressure-sensitive adhesive layer is further improved and foaming at the interface with the adherend in a high-temperature environment is less likely to occur, thereby further improving the heat resistance of the resulting pressure-sensitive adhesive sheet.
[0039] The tackifier resin may be a tackifier resin (T1) having no carbon-carbon double bond (unsaturated bond), or a tackifier resin (T2) having at least one selected from the group consisting of a carbon-carbon double bond and an aromatic ring. Among them, it is preferable to contain the tackifier resin (T1), and the content of the tackifier resin (T1) in the tackifier resin is more preferably 80% by mass or more, and even more preferably 90% by mass or more, and it is particularly preferable that the tackifier resin consists only of the tackifier resin (T1) having no carbon-carbon double bond. The tackifier resin (T1) has a smaller dielectric constant and dielectric loss tangent in the high frequency band, and therefore, by containing the tackifier resin (T1) in the adhesive layer, the dielectric loss tangent of the adhesive layer at a frequency of 10 GHz is more likely to satisfy the appropriate range, and the adhesive sheet obtained can be used more suitably even when the transmission signal is at a high frequency. In addition, the tackifier resin (T1) is less likely to self-polymerize than the tackifier resin (T2). Therefore, by containing the tackifier resin (T1) in the adhesive layer, the crosslinking of the base resin proceeds well, and the gel fraction of the adhesive layer is more likely to satisfy the appropriate range. As a result, the heat resistance of the adhesive sheet obtained is further improved. The tackifier resins may be used alone or in combination of two or more kinds.
[0040] The preferred upper limit of the SP value of the tackifier resin (T1) is 9.0. By making the SP value of the tackifier resin (T1) 9.0 or less, the dielectric constant and the dielectric loss tangent become smaller in the high frequency band. The more preferred upper limit of the SP value of the tackifier resin (T1) is 8.5. Further, there is no particular preferred lower limit for the SP value of the tackifier resin (T1), but in consideration of the SP values of general tackifier resins, the substantial lower limit is 7.5. In this specification, the above-mentioned "SP value" is a parameter that determines the activity of each component in a multi-component system, which is determined based on Hildebrand's theory of regular solutions, and means the SP value calculated by Small's method using Hoy's constant according to the following formula (II). SP value (δ) = d * (ΣG) / M (II) (d: density (g / mL), G: Hoy's molecular gravitation constant for each functional group, M: molecular weight (g / mol)) The method for calculating the SP value is described in the following reference document. KLHoy,New values of the solubility parameters from vapor pressure data,J.Paint Techn.,Vol.42,No.541,p.76(1970);KLHoy,The Hoy tables of solubility parameters,Union Carbide Corp.,1985;KLHoy,Solubility Parameters as a design parameter for water borne polymers and coatings.Preprints 14th Int.Conf.Athene,1988.;KLHoy, J.Coated Fabrics,19,p.53(1989).
[0041] Examples of the tackifier resin (T1) include hydrogenated C5 petroleum resins, alicyclic saturated hydrocarbon resins, hydrogenated C9 petroleum resins, hydrogenated C9 aromatic resins, hydrogenated α-methylstyrene resins, ultra-light-colored rosin esters, etc. Among these, the tackifier resin (T1) is preferably an alicyclic saturated hydrocarbon resin having excellent low dielectric properties.
[0042] Examples of the tackifier resin (T2) include terpene, aromatic modified terpene, aromatic modified hydrogenated terpene, terpene phenol, hydrogenated terpene phenol, rosin ester, rosin phenol, styrene copolymer tackifier resin, C5 petroleum resin, C9 petroleum resin, C5 aliphatic resin, alicyclic petroleum resin, C9 aromatic resin, pure C9 monomer resin, etc. Among them, terpene, aromatic modified terpene, and rosin ester are preferred, and terpene is more preferred, from the viewpoint of being easily compatible with the rubber elastomer and further improving the adhesive strength of the adhesive layer. Also, alicyclic petroleum resin is preferred from the viewpoint of excellent low dielectric properties.
[0043] The softening point of the tackifier resin is preferably 80° C. or more. When the softening point of the tackifier resin is 80° C. or more, the adhesive strength of the adhesive layer at high temperatures is improved, and foaming at the interface with the adherend in a high-temperature environment is less likely to occur. The softening point of the tackifier resin is more preferably 90° C. or less, and even more preferably 100° C. or less. The softening point of the tackifier resin is preferably 140° C. or lower, taking into consideration the temperature at which it is used. The softening point of the tackifier resin can be measured by a method in accordance with JIS K2207.
[0044] The content of the tackifier resin is preferably 20 parts by mass at the lower limit and 80 parts by mass at the upper limit relative to 100 parts by mass of the base resin. When the content of the tackifier resin is 20 parts by mass or more, the adhesive strength of the adhesive layer is further improved. When the content of the tackifier resin is 80 parts by mass or less, even if the adhesive layer contains the tackifier resin, crosslinking of the base resin proceeds well, the gel fraction of the adhesive layer is more likely to satisfy an appropriate range, and the heat resistance of the adhesive sheet of the present invention is further improved. The more preferred lower limit of the content of the tackifier resin is 30 parts by mass, and the more preferred upper limit is 70 parts by mass.
[0045] The pressure-sensitive adhesive may further contain a radical inhibitor (hereinafter also referred to as "radical inhibitor for pressure-sensitive adhesive layer"). The above-mentioned radical inhibitor for adhesive layer has a role of suppressing the association of radicals derived from the base resin with oxygen in the air when the base resin is crosslinked by energy ray irradiation, and by containing the above-mentioned radical inhibitor for adhesive layer in the above-mentioned adhesive, the obtained adhesive sheet can be used more suitably even when the transmission signal has a high frequency. In addition, the reaction caused by radicals between the adhesive layer and the release agent layer of the separator is suppressed, the separator becomes difficult to peel off, and the deterioration of the appearance, adhesiveness, and other functions when the separator is peeled off can be suppressed.
[0046] From the viewpoints of heat resistance and excellent optical properties with little discoloration, the above-mentioned radical inhibitor for adhesive layer preferably contains at least one selected from the group consisting of hindered phenols and hindered amines. Examples of the hindered phenols include 2-(1-(2-hydroxy-3,5-di-t-pentylphenyl)ethyl)-4,6-di-t-pentylphenyl (meth)acrylate, 2,6-di-t-butyl-4-methylphenol, 2-t-butyl-6-(3'-t-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl (meth)acrylate, and 2,2'-methylene-bis-(4-methyl-6-t-butylphenol). Examples of the hindered amine include bis-(1-(octyloxy)-2,2,6,6-tetramethyl-4-piperidinyl)sebacate and bis-(N-methyl-2,2,6,6-tetramethyl-4-piperidinyl)sebacate.
[0047] The content of the radical inhibitor for the adhesive layer is preferably 0.1 parts by mass and 10 parts by mass relative to 100 parts by mass of the base resin. When the content of the radical inhibitor for the adhesive layer is 0.1 parts by mass or more, the radicals derived from the base resin can be more effectively prevented from associating with oxygen in the air, so that the adhesive sheet obtained can be more suitably used even when the transmission signal has a high frequency. When the content of the radical inhibitor for the adhesive layer is 10 parts by mass or less, the crosslinking of the base resin proceeds well, the gel fraction of the adhesive layer is more likely to satisfy an appropriate range, and the heat resistance of the adhesive sheet obtained is further improved. The more preferable lower limit of the content of the radical inhibitor for the adhesive layer is 0.5 parts by mass, the more preferable upper limit is 8 parts by mass, the even more preferable lower limit is 1.0 parts by mass, and the even more preferable upper limit is 5 parts by mass.
[0048] The pressure-sensitive adhesive may further contain a softener. By including the softener in the pressure-sensitive adhesive, the adhesive strength of the resulting pressure-sensitive adhesive sheet is further improved. Examples of the softener include polybutene, n-butene-isobutylene copolymer, polyisoprene, paraffin oil, etc. Among them, polybutene is preferred because it is highly compatible with the rubber elastomer. On the other hand, when the softener is used, the adhesive strength of the resulting pressure-sensitive adhesive sheet at high temperatures decreases. Therefore, it is necessary to adjust the content of the softener according to the performance, crosslinking degree, etc. of the base resin used. When using the base resin that can exert high adhesive strength at room temperature even by itself, the content of the softener is preferably small, and the pressure-sensitive adhesive may not contain the softener.
[0049] The pressure-sensitive adhesive may contain other additives as necessary within the scope of not impairing the object of the present invention.
[0050] The preferred lower limit of the thickness of the adhesive layer is 1 μm, and the preferred upper limit is 300 μm. By having the thickness of the adhesive layer within this range, the resulting adhesive sheet can have both sufficient adhesive strength and ease of handling. The more preferred lower limit of the thickness of the adhesive layer is 2.5 μm, and the more preferred upper limit is 200 μm.
[0051] The pressure-sensitive adhesive sheet of the present invention has a separator on at least one surface of the pressure-sensitive adhesive layer. That is, the pressure-sensitive adhesive sheet of the present invention may be a pressure-sensitive adhesive sheet having a separator on one side of the pressure-sensitive adhesive layer, or may be a pressure-sensitive adhesive sheet having separators on both sides of the pressure-sensitive adhesive layer.
[0052] The separator includes a separator substrate and a release agent layer. When the pressure-sensitive adhesive sheet of the present invention has the separator on both sides, only the separator on one side may have the release agent layer, or both separators may have the release agent layer.
[0053] The separator substrate is not particularly limited, and any substrate that has been conventionally used as a separator substrate can be appropriately selected and used. For example, plastic films such as polyester, polyethylene, polypropylene, polymethylpentene, and polycarbonate, metal foils such as aluminum and stainless steel, and paper substrates such as glassine paper, wood-free paper, coated paper, impregnated paper, synthetic paper, and kraft paper can be used. Among these, polyester is preferred from the viewpoint of suppressing the inclusion of foreign matter originating from the separator. Examples of the polyester include polyethylene terephthalate (PET) and polybutylene terephthalate (PBT).
[0054] The release agent layer contains a silicone resin. The silicone resin is preferably an addition reaction type silicone resin. The addition reaction type silicone resin may, for example, be polydimethylsiloxane having an alkenyl group in the molecule.
[0055] The release agent layer contains a radical inhibitor (hereinafter also referred to as "radical inhibitor for release agent layer"). The radical inhibitor for the release agent layer has the role of capturing radicals generated in the separator when the base resin is crosslinked by irradiation with energy rays. When the release agent layer contains the radical inhibitor for the release agent layer, it is possible to prevent the separator from becoming difficult to peel off.
[0056] The radical inhibitor for the release agent layer is not particularly limited as long as it does not interfere with the crosslinking of the silicone resin, inhibits the generation of radicals, or captures the generated radicals. Examples of the radical inhibitor include N,N'-disalicylidene-1,2-propanediamine, 2,6-di-t-butylphenol, 2,4-di-t-butylphenol, 2-t-butyl-4-methoxyphenol, 2-t-butyl-4,6-dimethylphenol, 2,6-di-t-butyl-4-methylphenol, 2,6-di-t-butyl-4-ethylphenol, and 2,4,6-tri-t-butylphenol. , 2,6-di-t-butyl-4-hydroxymethylphenol, 2,6-di-t-butyl-2-dimethylamino-p-cresol, 2,5-di-t-butylhydroquinone, 2,5-di-t-amylhydroquinone, n-octadecyl-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)-propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine, styrenated phenol, styrenated cresol, 2-t-butyl-6-(3'-t-butyl 2,2'-methylene-bis-(4-methyl-6-t-butylphenol), 2,2'-methylene-bis-(4-ethyl-6-t-butylphenol), 2,2'-methylene-bis-(6-cyclohexyl-4-methylphenol), 2,2'-methylene-bis-6-(1-methylcyclohexyl)-p-cresol, 2,2'-ethylidene-bis-(2,4-di-t-butylphenol), 2,2'-butylidene-bis-(2-t-butyl-4-methyl phenol), 4,4'-methylene-bis-(2,6-di-t-butylphenol), 4,4'-butylidene-bis-(3-methyl-6-t-butylphenol), 1,6-hexanediol-bis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)-propionate], triethylene glycol-bis-[3-(3-t-butyl-5-methyl-4-hydroxyphenyl)propionate], N,N'-bis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyl]hydrazine, N,N'-bis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyl]hexamethylenediamine, 2,2'-thio-bis-(4-methyl-6-t-butylphenol), 2-(1-(2-hydroxy-3,5-di-t-pentylphenyl)ethyl)-4,6-di-t-pentylphenyl (meth)acrylate, 4,4'-thio-bis-(3-methyl-6-t-butylphenol), 2,2'-thio-diethylene-bis-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate], bis[2-t-butyl-4-methyl- 6-(3-t-butyl-5-methyl-2-hydroxybenzyl)phenyl]terephate, 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris-(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tris(3,5-di-t-butyl-4-hydroxybenzyl)isocyanurate, tris[2-(3',5'-di-t-butyl-4'-hydroxyhydro-cinnamoyloxyl)ethyl]isocyanurate, tris-(4-t-butyl -2,6-dimethyl-3-hydroxybenzyl) isocyanurate, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, metal salts (e.g. calcium salts) of ethyl-(3,5-di-t-butyl-4-hydroxybenzyl)phosphate, propyl-3,4,5-trihydroxybenzenecarbonate, octyl-3,4,5-trihydroxybenzenecarbonate, dodecyl-3,4,5-trihydroxybenzenecarbonate, 2,2'-methylene-bis-(4- Methyl-6-t-butylphenol), 4,4'-methylene-bis-(2,6-di-t-butylphenol), 1,1-bis-(4-hydroxyphenyl)-cyclohexane, 1,1,3-tris(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris-(3,5-di-t-butyl-4-hydroxybenzyl)benzene, 3,9-bis[1,1-dimethyl-2-{β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy}ethyl]-2,4,8,Phenol compounds such as 10-tetraoxaspiro[5.5]undecane and their derivatives (e.g., alkyl and aryl substituted compounds), salicylate compounds such as phenyl salicylate, 4-t-butylphenyl salicylate, 2,4-di-t-butylphenyl-3,5'-di-t-butyl-4'-hydroxybenzoate, 4-t-octylphenyl salicylate and their derivatives (e.g., alkyl and aryl substituted compounds), 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, Zofenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid, 2-hydroxy-4-n-octoxybenzophenone, 2-hydroxy-4-n-dodecyloxybenzophenone, 2-hydroxy-4-benzyloxybenzophenone, bis(5-benzoyl-4-hydroxy-2-methoxyphenyl)methane, 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone Benzophenone compounds such as benzotriazole, 4-dodecyloxy-2-hydroxybenzophenone, 2-hydroxy-4-methoxy-2'-carboxybenzophenone, and their derivatives (e.g., alkyl and aryl substituted derivatives), benzotriazole, tolyltriazole, tolyltriazole metal salts (e.g., potassium salts), 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-[2'-hydroxy-3',5'-bis(α,α-dimethylbenzyl)phenyl]benzotriazole, 2 -(2'-hydroxy-3',5'-di-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-t-amyl)benzotriazole, 2-(2'-hydroxy-5'-t-octylphenyl)benzotriazole, 2,2'-methylene-bis[4-(1,1,3,3-tetramethylbutyl)-6-(2N-benzotriazol-2-yl)phenol] and their derivatives (e.g., alkyl and aryl substituted), and other benzotriazole compounds, phenyl-4-piperidinyl carbonate, bis-(2,2,6,6-tetramethyl-4-piperidinyl)sebacate, bis-(N-methyl-2,2,6,6-tetramethyl-4-piperidinyl)sebacate, bis-(1,2,2,6,6-pentamethyl-4-piperidinyl)-2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butylmalonate, Poly[[6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)iminol]], tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarboxylate, 1,1'-(1,2-ethanediyl)bis(3,3,5,5-tetramethylpiperazinone), succinic acid and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidinone Copolymers of 1,2,3,4-butanetetracarboxylic acid and 1,2,2,6,6-pentamethyl-4-piperidyl-1,2,3,4-butanetetracarboxylate, 2,2,6,6-tetramethyl-4-tridecyl-1,2,3,4-butanetetracarboxylate, 1,2,2,6,6-pentamethyl-4-piperidyl-1,2,3,4-butanetetracarboxylate, 1,2,2,6,6-pentamethyl-4-tridecyl-1,2,3,4-butanetetracarboxylate, 1,2,3,4-butanetetracarboxylic acid and 1,2,2,6,6-pentamethyl-4-piperidyl-1,2,3,4-butanetetracarboxylate Hindered amine compounds such as condensation products of diols with β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5.5]undecane)diethanol and their derivatives (e.g., alkyl and aryl substituted derivatives); [2,2'-thio-bis(4-t-octylphenolate)]-2-ethylhexylaminenickel(II), nickel dibutyl-dithiocarbamate, [2,2'-thio-bis(4-t-octylphenolate)]-n-butylaminenickel(II), nickel bis(octylphenyl)sulfide, 3,Ni-based compounds such as 5-di-t-butyl-4-hydroxybenzilic acid monoethyl ester-Ni complex, 2,2'-thio-bis(4-t-octylphenolate)triethanolaminenickel(II) and their derivatives (e.g., alkyl, aryl substituted compounds), cyano(meth)acrylate-based compounds such as ethyl-2-cyano-3,3-diphenyl(meth)acrylate, 2-ethylhexyl-2-cyano-3,3'-diphenyl(meth)acrylate, butyl-2-cyano-3-methyl-3-(p-methoxyphenyl)(meth)acrylate and their derivatives (e.g., alkyl, aryl substituted compounds), 2-ethoxy-2'-ethyloxalic acid bisanilide, 2-ethoxy-5-t-butyl-2'-ethyloxalic acid bisanilide, Examples of the oxalic acid anilide compounds include derivatives thereof (e.g., alkyl- or aryl-substituted derivatives), salicylic acid derivatives such as 3-(N-salicyloyl)amino-1,2,4-triazole, 1,12-dodecanoic acid-bis[2-(2-hydroxybenzoyl)hydrazide], N-salicyloyl-N'-salicylidenehydrazine, and derivatives thereof (e.g., alkyl- or aryl-substituted derivatives), hydrazide derivatives such as N,N'-bis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionyl]hydrazine, isophthalic acid-bis[2-phenoxypropionylhydrazide], and derivatives thereof (e.g., alkyl- or aryl-substituted derivatives), acid amine compounds, guanidines, and mercaptobenzothiazole metal salts (e.g., sodium salts). Of these, 2-(1-(2-hydroxy-3,5-di-t-pentylphenyl)ethyl)-4,6-di-t-pentylphenyl acrylate, 2,6-di-t-butyl-4-methylphenol, 2-t-butyl-6-(3'-t-butyl-5'-methyl-2'-hydroxybenzyl)-4-methylphenyl acrylate, and 2,2'-methylene-bis-(4-methyl-6-t-butylphenol) are preferred because of their industrial ease of availability.
[0057] The content of the radical inhibitor for the release agent layer is 0.1 parts by mass at the lower limit and 10 parts by mass at the upper limit with respect to 100 parts by mass of the silicone resin. When the content of the radical inhibitor for the release agent layer is 0.1 parts by mass or more, the radicals generated in the separator can be appropriately captured, so that the separator can be prevented from becoming difficult to peel off. When the content of the radical inhibitor for the release agent layer is 10 parts by mass or less, the radical inhibitor can be prevented from migrating to the interface between the separator substrate and the release agent layer, and the adhesion between the release agent layer and the substrate can be prevented from decreasing. In addition, the radical inhibitor can be prevented from being present on the surface of the release agent layer, migrating to the surface of the adhesive layer, and reducing the adhesive strength. The lower limit of the content of the radical inhibitor for the release agent layer is preferably 0.5 parts by mass, the upper limit is preferably 5 parts by mass, the more preferable lower limit is 1 part by mass, and the more preferable upper limit is 3 parts by mass.
[0058] The separator preferably has an upper limit of 180° peel strength from the adhesive layer of 1.0 N / 25 mm. By setting the 180° peel strength of the separator to the adhesive layer to be 1.0 N / 25 mm or less, it is possible to further prevent the appearance and function of the resulting adhesive sheet from being impaired after the separator is peeled off.The upper limit of the 180° peel strength of the separator to the adhesive layer is more preferably 0.8 N / 25 mm, and even more preferably 0.5 N / 25 mm. Further, there is no particular preferred lower limit for the 180° peel strength of the separator with respect to the adhesive layer, but the substantial lower limit is 0.01 N / 25 mm. The 180° peel strength of the separator with respect to the pressure-sensitive adhesive layer can be measured by the following method. That is, first, the adhesive sheet is cut into a flat rectangular shape of 100 mm in length and 25 mm in width to obtain a test piece. The separator of the obtained test piece is peeled off in a 180° direction at 23° C. and a tensile speed of 300 mm / min using a tensile tester (e.g., Shimadzu Corporation's "AG-IS"), and the adhesive strength (180° peel strength) is measured. In addition, if the pressure-sensitive adhesive sheet is a double-sided pressure-sensitive adhesive sheet having an adhesive layer and a separator on both sides of the substrate, after cutting the pressure-sensitive adhesive sheet, the separator on the side not being measured is peeled off, and a SUS plate is placed on the exposed adhesive layer and bonded by rolling a 2.0 kg rubber roller back and forth at a speed of 300 mm / min., and then left to stand at 23°C for 24 hours to use as the test specimen.
[0059] The upper limit of the thickness of the separator is preferably 188 μm. By making the thickness of the separator 188 μm or less, the 180° peeling force of the separator against the adhesive layer is further reduced, and the appearance and function of the obtained adhesive sheet can be further prevented from being impaired after the separator is peeled off. The upper limit of the thickness of the separator is more preferably 100 μm, and even more preferably 75 μm. Although there is no particular preferred lower limit for the thickness of the separator, the substantial lower limit is 3 μm.
[0060] The pressure-sensitive adhesive sheet of the present invention may be a supported type having a substrate other than the separator substrate, or a non-supported type having no substrate other than the separator substrate, as long as the pressure-sensitive adhesive sheet has the pressure-sensitive adhesive layer and the separator on at least one side thereof. Among these, the non-supported type is preferable from the viewpoints of cost, thinness, and optical properties, and from the viewpoint of suppressing the dielectric loss tangent to a lower value.
[0061] The pressure-sensitive adhesive sheet of the present invention has a preferred lower limit of transmission loss at a frequency of 40 GHz for a polyimide substrate of -10 dB. Since the transmission loss at a frequency of 40 GHz for the polyimide substrate is -10 dB or more, the pressure-sensitive adhesive sheet of the present invention can be used more suitably even when the transmission signal is at a high frequency. The more preferred lower limit of the transmission loss at a frequency of 40 GHz for the polyimide substrate is -9 dB, and the even more preferred lower limit is -8 dB. Furthermore, the transmission loss of the pressure-sensitive adhesive sheet of the present invention with respect to a polyimide substrate at a frequency of 40 GHz is preferably as close to 0 dB as possible. The transmission loss at a frequency of 40 GHz for the polyimide substrate can be obtained by, for example, measuring the transmission loss of an evaluation sample at a frequency of 40 GHz and an impedance value of 50Ω using a vector network analyzer (Agilent Technologies, "N523OA") and a measurement probe (SUSS MicroTec, "B90-122391"). The evaluation sample can be prepared by laminating polyimide and copper, etching the polyimide substrate to form a microstrip line, and attaching an adhesive sheet onto the copper wiring.
[0062] The haze of the pressure-sensitive adhesive sheet of the present invention is not particularly limited, but is preferably 5.0% or less, and more preferably less than 1.0%. The color tone of the pressure-sensitive adhesive sheet of the present invention is also not particularly limited, but is preferably 0.01 to 0.1%. * The pressure-sensitive adhesive sheet of the present invention is resistant to changes in optical properties such as yellowing even in a high-temperature environment, and the haze and yellowing index b * It is preferable that the (b value) falls within the above range. In addition, the above haze and yellowing degree b * The (b value) can be measured, for example, using a spectrophotometer (such as "CM3700A" manufactured by Konica Minolta).
[0063] The present invention also includes a method for producing a pressure-sensitive adhesive sheet of the present invention, which includes a step of irradiating an energy ray from the separator side of a laminate having a layer containing the pressure-sensitive adhesive and the separator on at least one side of the layer containing the pressure-sensitive adhesive in the direction of the layer containing the pressure-sensitive adhesive. By including a step of irradiating energy rays from the separator side toward the layer containing the pressure-sensitive adhesive, it is possible to further suppress the radicals derived from the base resin generated by the energy ray irradiation from associating with oxygen in the air, and the dielectric loss tangent of the pressure-sensitive adhesive layer at a frequency of 10 GHz is more likely to satisfy an appropriate range. As a result, the pressure-sensitive adhesive sheet of the present invention can be used more suitably even when the transmission signal is at a high frequency. In addition, the reaction caused by radicals between the pressure-sensitive adhesive and the release agent layer of the separator is suppressed, making it difficult for the separator to peel off, and preventing the appearance, adhesion, and other functions from being impaired when the separator is peeled off.
[0064] When the pressure-sensitive adhesive sheet of the present invention has the separator on both sides of the pressure-sensitive adhesive layer, a laminate having a layer containing the pressure-sensitive adhesive and the separator on both sides of the layer containing the pressure-sensitive adhesive may be irradiated with energy rays from the separator side on both sides in the direction of the layer containing the pressure-sensitive adhesive. In particular, when the adhesive layer is thick, it is necessary to increase the irradiation intensity of the energy ray in order to advance the crosslinking of the base resin and adjust the gel fraction of the adhesive layer within the above range. Therefore, when the energy ray is irradiated only from the separator side on one side, a high irradiation intensity is required, but when the energy ray is irradiated from the separator side on both sides, the crosslinking of the base resin can be advanced and the gel fraction of the adhesive layer can be adjusted within the above range at a lower irradiation intensity than when the energy ray is irradiated only from the separator side on one side. As a result, it is possible to further suppress the radicals derived from the base resin generated by the energy ray irradiation from associating with oxygen in the air, and it is easy to adjust the dielectric loss tangent of the adhesive layer at a frequency of 10 GHz within the above range. As a result, the adhesive sheet of the present invention can be used more suitably even when the transmission signal is high-frequency. In addition, in the process of irradiating energy rays from the separator side of both sides, the 180° peel force of the separator against the adhesive layer on each side can be adjusted by adjusting the irradiation intensity, irradiation time, and acceleration voltage of the energy rays irradiated from the separator side on each side.
[0065] In the method for producing the pressure-sensitive adhesive sheet of the present invention, the preferred lower limit of the irradiation intensity of the energy ray is 5 kGy, and the preferred upper limit is 300 kGy. When the irradiation intensity of the energy ray is 5 kGy or more, the crosslinking of the base resin proceeds more, and the gel fraction of the pressure-sensitive adhesive layer can be more easily adjusted within the above range, and the heat resistance of the pressure-sensitive adhesive sheet of the present invention is further improved. When the irradiation intensity of the energy ray is 300 kGy or less, the generation of radicals in the separator can be more suppressed, and the 180° peeling force of the separator against the pressure-sensitive adhesive layer becomes smaller, so that the appearance and function of the obtained pressure-sensitive adhesive sheet can be more suppressed after the separator is peeled off. The more preferred lower limit of the irradiation intensity of the energy ray is 10 kGy, and the more preferred upper limit is 250 kGy, and the even more preferred lower limit is 20 kGy, and the even more preferred upper limit is 200 kGy.
[0066] A laminate having a layer containing the above-mentioned pressure-sensitive adhesive and the above-mentioned separator on at least one side of the layer containing the pressure-sensitive adhesive can be produced, for example, by applying a pressure-sensitive adhesive solution containing the above-mentioned base resin and, if necessary, other additives such as the above-mentioned tackifier resin onto the separator, drying it to form a layer containing the pressure-sensitive adhesive, and superimposing a substrate or another of the above-mentioned separator on the layer containing the pressure-sensitive adhesive.
[0067] The method for applying the adhesive solution to the separator is not particularly limited, but application with a comma coater is preferred because this makes it easier to adjust the 180° peel strength of the separator relative to the adhesive layer within the above range.
[0068] The use of the pressure-sensitive adhesive sheet of the present invention is not particularly limited, but it is preferably used for manufacturing a device that transmits or receives electromagnetic waves. The device that transmits or receives electromagnetic waves preferably includes a laminate including the pressure-sensitive adhesive sheet of the present invention and a film on which a conductive pattern is formed. The pressure-sensitive adhesive sheet of the present invention can be suitably used even when the transmission signal is at a high frequency, and is therefore more preferably used in the manufacture of devices that transmit or receive electromagnetic waves with a frequency of 1 GHz or more. The device that transmits or receives the electromagnetic waves with a frequency of 1 GHz or more is not particularly limited, and examples thereof include small antenna base stations, antennas such as vehicle-mounted antennas, smartphones, tablet terminals, other portable electronic devices, vehicle-mounted electronic devices, smart glasses, etc. In particular, the pressure-sensitive adhesive sheet of the present invention is preferably used for bonding internal members of a laminate (e.g., an antenna film, a substrate, etc.) containing a film having a conductive pattern formed thereon, or bonding a laminate containing a film having a conductive pattern formed thereon to another member, in a device that transmits or receives electromagnetic waves having a frequency of 1 GHz or more. A method for producing an electronic component, comprising a step of bonding internal members of a laminate containing a film having a conductive pattern formed thereon via the pressure-sensitive adhesive sheet of the present invention from which the separator has been peeled off, or a step of bonding a laminate containing a film having a conductive pattern formed thereon to another member via the pressure-sensitive adhesive sheet of the present invention from which the separator has been peeled off, is also one aspect of the present invention.
[0069] FIG. 1 is a cross-sectional view that illustrates a schematic state in which the pressure-sensitive adhesive sheet of the present invention is used to bond internal members of a laminate that includes a film having a conductive pattern formed thereon. 1, in a laminate 2 including a film having a conductive pattern formed thereon, internal members 21 and 22 are bonded together by a pressure-sensitive adhesive sheet 1 of the present invention from which the separator has been peeled off. The laminate 2 including a film having a conductive pattern formed thereon may further include members (for example, members 23 and 24 as shown in FIG. 1) in addition to the pressure-sensitive adhesive sheet 1 of the present invention from which the separator has been peeled off and members 21 and 22. FIG. 2 is a cross-sectional view that illustrates a schematic state in which a laminate including a film having a conductive pattern formed thereon is bonded to another member using the pressure-sensitive adhesive sheet of the present invention. In FIG. 2, a laminate 2 including a film on which a conductive pattern has been formed and another member 3 are bonded together by a pressure-sensitive adhesive sheet 1 of the present invention from which the separator has been peeled off. Effect of the Invention
[0070] According to the present invention, it is possible to provide a pressure-sensitive adhesive sheet that can be suitably used even when the transmission signal is at a high frequency, has excellent heat resistance, and is capable of suppressing impairment of appearance and function after peeling off the separator. Also, according to the present invention, it is possible to provide a method for manufacturing an electronic component using the pressure-sensitive adhesive sheet, and a method for manufacturing the pressure-sensitive adhesive sheet. [Brief description of the drawings]
[0071] [Figure 1] FIG. 2 is a cross-sectional view showing a schematic view of the state in which the pressure-sensitive adhesive sheet of the present invention is used to bond members inside a laminate including a film having a conductive pattern formed thereon. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a state in which a laminate including a film having a conductive pattern formed thereon is bonded to another member using the pressure-sensitive adhesive sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0072] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0073] (Synthesis of radial hydrogenated styrene elastomer A) In an autoclave, 4000 g of degassed and dehydrated cyclohexane, 200 g of 1,3-butadiene monomer, 3.0 g of n-butyl lithium (n-BuLi), and tetrahydrofuran (THF) were added in a molar ratio of n-BuLi / THF=40. The resulting mixture was heated at 40° C. for 40 minutes, after which 100 g of styrene monomer was added and heated at 40° C. for 60 minutes to allow the polymerization reaction to proceed (aromatic alkenyl polymer block (A)). Next, 700 g of 1,3-butadiene monomer was added and heated at 40° C. for 150 minutes to allow the polymerization reaction to proceed (diblock structured styrene-based block copolymer (AB)). 0.25 mol of tetrachlorosilane (SiCl4) was added as a coupling agent to carry out a coupling reaction of the diblock styrene-based block copolymer (AB) to obtain a styrene-based block copolymer with a styrene content of 10 mass %. The obtained styrene-based block copolymer was diluted with purified and dried cyclohexane to prepare a styrene-based block copolymer solution having a polymer concentration of 5 mass %. The obtained styrene-based block copolymer solution was subjected to a hydrogenation reaction.
[0074] In the hydrogenation reaction, first, 1000 g of the styrene block copolymer solution was charged into a thoroughly dried 2 L autoclave equipped with a stirrer, degassed under reduced pressure, replaced with hydrogen, and maintained at 90° C. with stirring. Next, 50 mL of a cyclohexane solution containing 0.2 mmol of di-p-tolylbis(η-cyclopentadienyl)titanium and 10 mL of a cyclohexane solution containing 0.108 mmol of n-butyllithium (n-BuLi) were mixed at 0°C and 2.0 kg / cm 2 The mixture was mixed under a hydrogen pressure of 0.7 MPa and added to the styrene block copolymer solution in the autoclave. Thereafter, the hydrogenation reaction was started under conditions of a hydrogen gas supply pressure of 0.7 MPa-Gauge and a reaction temperature of 80°C while stirring. When the absorption of hydrogen was completed, the reaction solution was returned to room temperature and pressure and extracted from the reaction vessel to obtain a radial hydrogenated styrene elastomer A (a hydrogenated product of the radial block copolymer in which n is 4 in the above formula (1)). The obtained radial type hydrogenated styrene-based elastomer A has the following properties: 1 H-NMR analysis confirmed that 95% or more of the butadiene units and less than 5% of the styrene units were hydrogenated. In addition, the weight average molecular weight of the radial type hydrogenated styrene elastomer A measured as a polystyrene equivalent molecular weight by the GPC method was 300,000.
[0075] (Preparation of adhesive solution) Each material was added to 350 parts by mass of toluene according to the adhesive composition shown in Tables 1 to 3 and stirred to obtain an adhesive solution.
[0076] (Preparation of separator) After mixing the materials according to the release agent composition shown in Tables 1 to 3, the materials were diluted with a mixed solvent of toluene and hexane (volume ratio 1:1) so that the concentration of the silicone resin became 0.7% by mass to obtain a release agent solution. The obtained release agent solution was applied to a 25 μm-thick PET film (manufactured by Toyobo Co., Ltd., "E5100") as a separator substrate with a wire bar #9, and then dried at 130° C. for 1 minute to obtain a separator. It should be noted that, although KS-847T and KS-3703 listed in Tables 1 to 3 contain a solvent, the content of the silicone resin in the release agent composition listed in Tables 1 to 3 is the content of only the silicone resin.
[0077] (Examples 1 to 20, Comparative Examples 1 to 4 and 6) (1) Preparation of adhesive sheet The adhesive solution was applied onto the release agent layer of a 75 μm thick separator (manufactured by Toyo Cross Co., Ltd., "SP8001") so that the thickness after drying would be 50 μm, and then dried at 110° C. for 5 minutes. Thereafter, the separator obtained in the above "(Preparation of Separator)" was laminated onto the surface of the adhesive-containing layer on which the separator was not laminated, so that the release agent layer was on the side of the adhesive-containing layer, to obtain a laminate. Furthermore, according to the electron beam irradiation conditions shown in Tables 1 to 3, electron beam irradiation was performed from the separator side obtained in the above "(Preparation of Separator)" of the laminate toward the adhesive-containing layer using an electron beam irradiation device (manufactured by NHV Corporation, "EBC-200"), to crosslink the base resin in the adhesive to form an adhesive layer, and to obtain an adhesive sheet.
[0078] (2) Measurement of the dielectric tangent of the adhesive layer at a frequency of 10 GHz The separators on both sides of the obtained adhesive sheet were peeled off, and the adhesive layer was laminated to a thickness of 100 μm. PET films with a thickness of 50 μm were attached to the top and bottom surfaces of the laminated adhesive layer. The obtained laminate of the PET film and adhesive layer was cut to a width of 3 mm and a length of 80 mm, and the dielectric loss tangent was measured in the measurement mode of the TM mode resonator using a dielectric constant measuring device (manufactured by AET Corporation, "ADMS01Nc") in accordance with JIS C2565. The dielectric loss tangent of the PET film alone was also measured by the above method, and the dielectric loss tangent of the adhesive layer alone was calculated using the measured values of the laminate of the PET film and the adhesive layer and the measured values of the PET film alone. The results are shown in Tables 1 to 3.
[0079] (3) Measurement of gel fraction of adhesive layer The separators on both sides were peeled off from the obtained adhesive sheet to collect an adhesive layer (mass: W0 (g)). The collected adhesive layer was then immersed in 50 mL of toluene and shaken in a shaker at 23°C and 200 rpm for 24 hours. After shaking, the adhesive layer that had absorbed toluene and swollen was filtered using a metal mesh (opening #200 mesh, mass: W1 (g)). The separated adhesive layer was dried at 110°C for 1 hour, and the mass W2 (g) of the adhesive layer including the metal mesh was measured. The gel fraction was calculated from the obtained W0, W1, and W2 using the above formula (I). The results are shown in Tables 1 to 3.
[0080] (4) Measurement of 180° peel strength of the separator obtained in the above "(Preparation of separator)" against the adhesive layer The obtained adhesive sheet was cut into a flat rectangular shape with a length of 100 mm and a width of 25 mm. The separator (the side not to be measured) other than the separator obtained in the above "(Preparation of separator)" was peeled off from the cut adhesive sheet. A SUS plate was placed on the exposed adhesive layer, and the two were bonded by rolling a 2.0 kg rubber roller back and forth at a speed of 300 mm / min, and left to stand at 23°C for 24 hours to obtain a test piece. The separator obtained in the above "(Preparation of separator)" was peeled off in the 180° direction from the obtained test piece using a tensile tester (Shimadzu Corporation, "AG-IS") at 23°C and a tensile speed of 300 mm / min, and the adhesive strength (180° peel strength) was measured. In addition, in the above test piece preparation operation, if the separator obtained in the above "(Preparation of separator)" peeled off first, the adhesive sheet cut into a flat rectangular shape of 100 mm in length and 25 mm in width was attached to a SUS plate with double-sided tape, and then the separator obtained in the above "(Preparation of separator)" was peeled off under the conditions described above, and measurements were performed. The results are shown in Tables 1 to 3.
[0081] (5) Measurement of 90° peel strength against glass The obtained adhesive sheet was cut to have a planar rectangular shape of 100 mm in length and 25 mm in width. The separator other than the separator obtained in the above "(Preparation of separator)" was peeled off from the cut adhesive sheet and laminated on a cycloolefin film (manufactured by Zeon Corporation, "ZF16-100 μm"). Next, the separator obtained in the above "(Preparation of separator)" of the adhesive sheet was peeled off, and a glass plate (manufactured by AGC Corporation, float plate glass "FL3") was placed on the exposed adhesive layer, and a 2.0 kg rubber roller was moved back and forth once at a speed of 300 mm / min on the cycloolefin film to laminate it. Then, the test piece was prepared by leaving it at 23 ° C for 24 hours. The surface of the glass plate was washed with ethanol and then wiped dry, and it was confirmed that there were no scratches by visual inspection before use. The adhesive strength (90° peel strength) of the obtained test samples was measured using a tensile tester (Shimadzu Corporation, "AG-IS") at 23° C. and a tensile speed of 50 mm / min, by peeling in a 90° direction. The results are shown in Tables 1 to 3.
[0082] Comparative Example 5 Adhesive sheets were obtained in the same manner as in "(1) Preparation of Adhesive Sheet" in Examples 1 to 20 and Comparative Examples 1 to 4 and 6 above, except that when irradiating with electron beams, the separator obtained in "(Preparation of Separator)" above was peeled off and then the adhesive was directly irradiated with electron beams according to the electron beam irradiation conditions shown in Table 3. Furthermore, measurements were performed in the same manner as in the above "(2) Measurement of the dielectric tangent of the adhesive layer at a frequency of 10 GHz", "(3) Measurement of the gel fraction of the adhesive layer", "(4) Measurement of the 180° peel strength of the separator against the adhesive layer", and "(5) Measurement of the 90° peel strength against glass" in Examples 1 to 20 and Comparative Examples 1 to 4 and 6. The results are shown in Table 3.
[0083] <Evaluation> The pressure-sensitive adhesive sheets obtained in the examples and comparative examples were evaluated as follows, and the results are shown in Tables 1 to 3.
[0084] (Low dielectric properties) A polyimide substrate with a microstrip line was fabricated by laminating polyimide and copper and etching the laminate. The obtained adhesive sheet was cut to match the shape of the polyimide substrate. The separator on one side of the cut adhesive sheet was peeled off, and a 2.0 kg rubber roller was placed on the sheet and run back and forth at a speed of 300 mm / min to bond the sheet to the copper wiring of the polyimide substrate. The sheet was then left to stand at 23°C for 24 hours to prepare an evaluation sample. At 23°C and 50% RH, a vector network analyzer and a measurement probe were used to measure the transmission loss of the evaluation sample at a frequency of 40 GHz and an impedance value of 50 Ω, and the transmission loss at a frequency of 40 GHz for the polyimide substrate was obtained. The vector network analyzer used was N523OA (manufactured by Agilent Technologies), and the measurement probe used was B90-122391 (manufactured by SUSS MicroTec). The low dielectric properties of the adhesive sheet were evaluated by rating it as follows: if the transmission loss at a frequency of 40 GHz for the obtained polyimide substrate was -8 dB or more, it was marked "◎"; if it was -10 dB or more but less than -8 dB, it was marked "○"; if it was less than -10 dB, it was marked "×".
[0085] (Heat resistance) The obtained adhesive sheet was cut to have a planar shape of 60 mm x 60 mm. The separator on one side of the cut adhesive sheet was peeled off, and the sheet was laminated on a polyimide film (manufactured by Toray DuPont, "200H-50 μm"). The separator on the other side of the adhesive sheet was peeled off to expose the adhesive layer, and the exposed side of the adhesive sheet was placed on the same polyimide film. A 2.0 kg rubber roller was placed on the obtained laminate, and the rubber roller was moved back and forth at a speed of 300 mm / min to laminate the polyimide film and the adhesive sheet together, and the laminate was left to stand at 23 ° C for 24 hours to obtain a test specimen. The obtained test piece was subjected to a heat treatment in an environment of 85° C. and 85% RH for 1 day, and then naturally cooled to 25° C. After that, the test piece was observed at a magnification of 20 times using an optical microscope from a direction perpendicular to the interface between the pressure-sensitive adhesive sheet and the polyimide film, and the air bubble area at the interface between the pressure-sensitive adhesive sheet and the polyimide film was calculated. Heat resistance was evaluated as follows: when the bubble area was less than 1%, it was marked "◎", when the bubble area was 1% or more but less than 5%, it was marked "○", when the bubble area was 5% or more but less than 10%, it was marked "△", and when the bubble area was 10% or more, it was marked "X".
[0086] (Appearance of adhesive layer after peeling off separator) Both surfaces of the adhesive layer of the adhesive sheet from which the separator had been peeled off in the above "(4) Measurement of 180° peel strength from the adhesive layer of the separator" were visually observed. The appearance of the adhesive layer after peeling off the separator was evaluated as follows: if no roughness was found on the surface of the adhesive layer, it was marked "◎"; if minor roughness was found on the surface of the adhesive layer that did not affect functional expression, it was marked "○"; if roughness was found on part of the surface of the adhesive layer such that it made it difficult to express its function, it was marked "△"; and if roughness was found on the entire surface of the adhesive layer such that it made it difficult to express its function, it was marked "X".
[0087] [Table 1]
[0088] [Table 2]
[0089] [Table 3] [Industrial Applicability]
[0090] According to the present invention, it is possible to provide a pressure-sensitive adhesive sheet that can be suitably used even when the transmission signal is at a high frequency, has excellent heat resistance, and is capable of suppressing impairment of appearance and function after peeling off the separator. Also, according to the present invention, it is possible to provide a method for manufacturing an electronic component using the pressure-sensitive adhesive sheet, and a method for manufacturing the pressure-sensitive adhesive sheet. [Explanation of symbols]
[0091] 1 Adhesive sheet 2. Laminate including a film on which a conductive pattern is formed 21, 22, 23, 24 Parts (internal parts) 3 Other materials
Claims
1. The adhesive layer is made of an adhesive containing a base resin, and a separator is provided on at least one surface of the adhesive layer. The base resin includes a rubber-based elastomer, The adhesive layer has a dielectric tangent of 0.003 or less at a frequency of 10 GHz and a gel fraction of 30 mass% or more, The separator has a separator substrate and a release agent layer, the release agent layer contains a silicone resin and a radical inhibitor, In the release agent layer, the content of the radical inhibitor relative to 100 parts by mass of the silicone resin is 0.1 parts by mass or more and 10 parts by mass or less. A pressure-sensitive adhesive sheet characterized by:
2. The adhesive layer is made of an adhesive containing a base resin, and a separator is provided on at least one surface of the adhesive layer. The base resin includes a rubber-based elastomer, The adhesive layer has a dielectric tangent of 0.003 or less at a frequency of 10 GHz and a gel fraction of 30 mass% or more, The separator has a separator substrate and a release agent layer, the release agent layer contains a silicone resin and a radical inhibitor, In the release agent layer, the content of the radical inhibitor relative to 100 parts by mass of the silicone resin is 0.1 parts by mass or more and 10 parts by mass or less, The separator has a 180° peel strength with respect to the adhesive layer of 1.0 N / 25 mm or less. A pressure-sensitive adhesive sheet characterized by:
3. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive layer has a 90° peel strength from glass of 5.0 N / 25 mm or more.
4. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the rubber-based elastomer comprises at least one selected from the group consisting of a styrene-based elastomer and a hydrogenated styrene-based elastomer.
5. The pressure-sensitive adhesive sheet according to claim 4 , wherein the rubber-based elastomer includes a hydrogenated styrene-based elastomer.
6. 6. The pressure-sensitive adhesive sheet according to claim 5, wherein the hydrogenated styrene-based elastomer is a hydrogenated product of a block copolymer having an aromatic alkenyl polymer block and a conjugated diene polymer block.
7. The pressure-sensitive adhesive sheet according to claim 6, wherein the hydrogenated product of the block copolymer having an aromatic alkenyl polymer block and a conjugated diene polymer block is a hydrogenated product of a radial type block copolymer represented by the following formula (1): [Formula 1] In formula (1), A is an aromatic alkenyl polymer block, B is a conjugated diene polymer block, C is a segment derived from a coupling agent, and n is an integer of 3 or more.
8. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive further comprises a cross-linking auxiliary, and the content of the cross-linking auxiliary per 100 parts by mass of the base resin is 15 parts by mass or less.
9. The pressure-sensitive adhesive sheet according to claim 8 , wherein the crosslinking aid comprises a (meth)acrylic monomer.
10. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive further comprises a tackifier resin, the tackifier resin including a tackifier resin having no carbon-carbon double bond.
11. 11. The pressure-sensitive adhesive sheet according to claim 10, wherein the tackifier resin consists solely of a tackifier resin having no carbon-carbon double bonds.
12. The pressure-sensitive adhesive sheet according to claim 10, wherein the content of the tackifier resin relative to 100 parts by mass of the base resin is 20 parts by mass or more and 80 parts by mass or less.
13. 3. The pressure-sensitive adhesive sheet according to claim 1, which is a non-support type having no substrate other than the separator substrate.
14. 3. The pressure-sensitive adhesive sheet according to claim 1, which is used in the manufacture of a device for transmitting or receiving electromagnetic waves having a frequency of 1 GHz or more.
15. 3. A method for manufacturing an electronic component, comprising: a step of bonding internal components of a laminate including a film having a conductive pattern thereon via the adhesive sheet of claim 1 or 2 from which the separator has been peeled off; or a step of bonding a laminate including a film having a conductive pattern thereon and another component via the adhesive sheet of claim 1 or 2 from which the separator has been peeled off.
16. 3. The method for producing a pressure-sensitive adhesive sheet according to claim 1, further comprising a step of irradiating an energy ray from the separator side of a laminate having a layer containing the pressure-sensitive adhesive and the separator on at least one side of the layer containing the pressure-sensitive adhesive, in the direction of the layer containing the pressure-sensitive adhesive.
Citation Information
Patent Citations
Impact-absorbing tape
JP2009242541A
Pressure-sensitive adhesive sheet for front plate of display device
JP2009258274A