Decorative sheet, and decorative plate

A decorative sheet with a transparent resin layer blend of biomass-derived homopolypropylene and petroleum-derived random polypropylene addresses transparency and cold resistance issues, enhancing processability and production speed in low-temperature environments.

JP2024134524APending Publication Date: 2024-10-03DAI NIPPON PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024025431
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-20
Filing Date
2024-02-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Biomass-derived polypropylene, while offering excellent scratch resistance, has low transparency and cold resistance issues, leading to processing challenges and reduced production speed during extrusion film formation, making it unsuitable for decorative sheets.

Method used

A decorative sheet design incorporating a transparent resin layer composed of 80% biomass-derived homopolypropylene and 20-80% petroleum-derived random polypropylene, with a thickness of 40-150 μm, and optionally containing a lubricant like calcium stearate, enhances processability in low-temperature environments.

Benefits of technology

The solution improves processability in low-temperature conditions and maintains production speed during extrusion film formation, while reducing environmental impact by utilizing biomass-derived materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134524000001_ABST
    Figure 2024134524000001_ABST
Patent Text Reader

Abstract

To provide a decorative sheet which can suppress lowering of workability under low temperature environment and production speed in extrusion film formation, even when biomass-derived homopolypropylene is used.SOLUTION: A decorative sheet has at least a pattern layer, a transparent resin layer, and a surface protective layer in this order on one surface side of a base material sheet, wherein the transparent resin layer contains biomass-derived homopolypropylene, and petroleum-derived random polypropylene, the transparent resin layer is 80 mass% or more and 20 mass% or less with respect to the mass of the resin component constituting the transparent resin layer, and the content of the petroleum-derived random polypropylene is 20 mass% or more and 80 mass% or less with respect to the mass of the resin component constituting the transparent resin layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a decorative sheet and a decorative board. [Background technology]

[0002] 2. Description of the Related Art When it is desired to decorate components used in building materials, furniture, home appliances, and the like, decorative panels having a decorative sheet with a design attached thereto are generally used.

[0003] Plastics are often used as the main component of materials constituting decorative sheets. Petroleum-derived plastics are widely used as the above-mentioned plastics, but are not preferable from the viewpoint of reducing the environmental load.

[0004] Therefore, the use of biomass-derived plastics, which are made from renewable biological resources, as a material with less environmental impact than petroleum-derived plastics, for decorative sheets is being considered.

[0005] For example, Patent Document 1 discloses a decorative sheet in which a colored thermoplastic resin layer has a pattern layer printed on its surface, a transparent thermoplastic resin layer having a surface with irregularities formed thereon, and a surface protective layer are laminated in this order via a transparent adhesive resin layer, and the transparent thermoplastic resin layer is made of a resin composition blended with 20% by mass or more and 60% by mass or less of biomass low-density polyethylene resin and 40% by mass or more and 80% by mass or less of biomass high-density polyethylene resin. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2020-179553 A Summary of the Invention [Problem to be solved by the invention]

[0007] The use of biomass-derived polypropylene as a biomass-derived plastic is also being considered. Biomass-derived polypropylene has properties such as being less susceptible to scratches (excellent scratch resistance) compared to biomass-derived polyethylene.

[0008] Currently, only block polypropylene and homopolypropylene are mass-produced as biomass-derived polypropylene. However, biomass-derived block polypropylene has low transparency and is therefore not suitable for use in the field of decorative sheets, where design is required.In addition, biomass-derived homopolypropylene has problems such as cracking during processing in low-temperature environments due to its low cold resistance, and the need to reduce the production speed during extrusion film production to stabilize the film thickness.

[0009] Therefore, when attempting to use biomass-derived homopolypropylene in the transparent resin layer of a decorative sheet (the transparent thermoplastic resin layer in Patent Document 1), there were issues such as a decrease in production speed when extrusion laminating the biomass-derived homopolypropylene onto the pattern layer, and the occurrence of cracks when the decorative sheet is processed in a low-temperature environment. [Means for solving the problem]

[0010] The inventors have conducted extensive research into the introduction of biomass-derived polypropylene into decorative sheets for building materials, etc., and have found that by blending a specific amount of petroleum-derived random polypropylene with biomass-derived homopolypropylene, processability in low-temperature environments can be improved and a decrease in production rate during extrusion film production can be suppressed.

[0011] In other words, the present disclosure provides a decorative sheet having at least a pattern layer, a transparent resin layer, and a surface protective layer, in that order, on one side of a base sheet, the transparent resin layer containing a biomass-derived homopolypropylene and a petroleum-derived random polypropylene, the transparent resin layer having a content of the biomass-derived homopolypropylene of 20% by mass or more and 80% by mass or less relative to the mass of the resin components constituting the transparent resin layer, and a content of the petroleum-derived random polypropylene of 20% by mass or more and 80% by mass or less relative to the mass of the resin components constituting the transparent resin layer.

[0012] In the decorative sheet of the present disclosure, the biomass-derived homopolypropylene preferably has a biomass degree of 30% or more. The transparent resin layer preferably has a thickness of 40 μm or more and 150 μm or less. In addition, it is preferable that the transparent resin layer has an uneven shape on the side having the surface protective layer. The transparent resin layer preferably contains a lubricant. The lubricant is preferably calcium stearate. It is also preferable that the substrate sheet has an adhesive auxiliary layer on the side opposite to the side having the design layer. In addition, the base sheet preferably contains a biomass-derived polyolefin. Moreover, the surface protective layer preferably contains at least one agent selected from the group consisting of an antibacterial agent, an antiviral agent, and an antiallergen agent. The present disclosure also relates to a decorative board comprising an adherend on the side of the base sheet of the decorative sheet opposite the side having the pattern layer. Effect of the Invention

[0013] The present disclosure provides a decorative sheet that is easy to process in a low-temperature environment and prevents a decrease in production rate during extrusion film formation, even when using homopolypropylene derived from biomass. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of a preferred example of the decorative sheet of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] <Decorative sheet> The decorative sheet of the present disclosure has at least a pattern layer, a transparent resin layer, and a surface protection layer, in this order, on one side of a base sheet, and is characterized in that the transparent resin layer contains a biomass-derived homopolypropylene and a petroleum-derived random polypropylene, and the transparent resin layer has a content of the biomass-derived homopolypropylene of 20% by mass or more and 80% by mass or less relative to the mass of the resin components constituting the transparent resin layer, and a content of the petroleum-derived random polypropylene of 20% by mass or more and 80% by mass or less relative to the mass of the resin components constituting the transparent resin layer.

[0016] FIG. 1 is a cross-sectional view that illustrates a schematic diagram of a preferred example of the decorative sheet of the present disclosure. As shown in FIG. 1, the decorative sheet 10 has a design layer 3, a transparent resin layer 6, and a surface protective layer 8 laminated in this order on one surface of a base sheet 1. Also, as shown in FIG. 1, an adhesive auxiliary layer 2 (also called a pattern auxiliary layer) may be provided between the base sheet 1 and the pattern layer 3, an adhesive auxiliary layer 4 (also called a back surface adhesive auxiliary layer) may be provided on the side of the base sheet 1 opposite to the side having the pattern layer 3, an adhesive layer 5 may be provided between the pattern layer 3 and the transparent resin layer 6, and an adhesive auxiliary layer 7 (surface adhesive auxiliary layer) may be provided between the transparent resin layer 6 and the surface protective layer 8. Each component of the decorative sheet of the present disclosure will be described in detail below.

[0017] (Base sheet) The decorative sheet of the present disclosure has a base sheet.

[0018] The resin constituting the base sheet is preferably an olefin resin. As the olefin resin, a polyolefin-based thermoplastic resin can be used, and examples thereof include polyethylene, ethylene-α-olefin copolymer, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, propylene-butene copolymer, ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, etc. Among these, polyethylene and polypropylene are preferred.

[0019] The base sheet may be a polyester-based resin, for example, a polyester-based thermoplastic resin can be used, and examples of such resins include polyethylene terephthalate, highly heat-resistant polyalkylene terephthalate (for example, polyethylene terephthalate in which part of ethylene glycol is replaced with 1,4-cyclohexanedimethanol or diethylene glycol, so-called product name PET-G (manufactured by Eastman Chemical Company)), polybutylene terephthalate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, etc. Among these, highly heat-resistant polyalkylene terephthalate is preferred.

[0020] The base sheet may comprise a biomass-derived polyolefin. By including a biomass-derived polyolefin in the base sheet, it is possible to preferably reduce the amount of raw materials derived from fossil fuels and thus to preferably reduce the environmental load. Here, the term "biomass-derived polyolefin" refers to a material that uses a biomass-derived polyolefin as at least a part of the raw material, but does not mean that the entire raw material is a biomass-derived polyolefin.

[0021] Examples of biomass-derived polyolefins include biomass-derived polyethylene, polypropylene, polybutylene, and the like.

[0022] As the biomass-derived polyethylene, for example, at least one selected from the group consisting of high-density polyethylene, medium-density polyethylene, low-density polyethylene, and linear low-density polyethylene can be used. In addition, it may be a mixture of two or more selected from the group consisting of high-density polyethylene, medium-density polyethylene, low-density polyethylene, and linear low-density polyethylene.

[0023] As the biomass-derived polypropylene, a biomass-derived homopolypropylene can be suitably used. The homopolypropylene derived from biomass may be appropriately selected from those described in the transparent resin layer described below.

[0024] From the viewpoint of suitably reducing the environmental load, the biomass-derived polyolefin preferably has a biomass ratio of 30% or more, and more preferably 40% or more. The upper limit of the biomass content of biomass-derived polyolefin is, for example, 70%.

[0025] In this specification, the "biomass degree" is a value measured by measuring the content of carbon derived from biomass by radiocarbon (C14) measurement. Carbon dioxide in the atmosphere contains a certain proportion of C14 (105.5 pMC), and it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. On the other hand, it is also known that fossil fuels contain almost no C14. Therefore, the proportion of carbon derived from biomass can be calculated by measuring the proportion of C14 contained in the total carbon atoms in the layer of the base sheet of the present disclosure (or in the layer of the transparent resin layer described later). That is, the content of C14 in the layer of the base sheet of the present disclosure (or in the layer of the transparent resin layer) is P C14 The content of carbon derived from biomass, P bio It can be calculated as follows: P bio (%)=(P C14 / 105.5)×100

[0026] The base sheet may contain various additives, such as colorants, fillers, matting agents, foaming agents, flame retardants, lubricants, antistatic agents, UV absorbers, antioxidants, and light stabilizers, as necessary. The content of the additive is preferably 20% by mass or more and 40% by mass or less based on the mass of the base sheet.

[0027] The substrate sheet may be colored as necessary. The surface of the substrate sheet may be subjected to a surface treatment such as corona discharge treatment, plasma treatment, or ozone treatment, or may be coated with a primer, which is a base coating material, for improving adhesion to adjacent layers.

[0028] The thickness of the base sheet is, for example, preferably 50 μm or more and less than 100 μm, and more preferably 60 μm or more and 80 μm or less.

[0029] The specific method for forming a film (sheeting) of the base sheet is not particularly limited, and examples thereof include the T-die method in which molten resin is extruded and laminated using a T-die, the calendar method, the circular die method (inflation method, tubular method), etc. Among these, the T-die method is preferred when improving production efficiency (production speed) and alleviating internal stress during sheeting. The calendar method is preferred when making the thickness of the base sheet uniform and reducing foreign matter defects.

[0030] (Picture layer) The decorative sheet of the present disclosure has a design layer on one side of the base sheet.

[0031] The design layer imparts a desired design to the decorative sheet, and the type of design is not limited. Examples of the design include wood grain, stone grain, sand grain, tiled, brickwork, fabric, leather, geometric shapes, letters, symbols, and abstract patterns.

[0032] The ink used to form the design layer contains a colorant component, a resin component, and a liquid component. The ink may contain an extender pigment, a solvent, a stabilizer, a plasticizer, a catalyst, a hardener, etc.

[0033] Examples of the colorant component include inorganic pigments such as carbon black (ink), iron black, titanium white, antimony white, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue; organic pigments or dyes such as quinacridone red, isoindolinone yellow, and phthalocyanine blue; scaly foil metal pigments such as aluminum and brass; and scaly foil pearlescent (pearl) pigments such as titanium dioxide-coated mica and basic lead carbonate. There are no particular limitations on the resin component, and any of the following may be used alone or in combination: urethane-based resins, acrylic-based resins, ester-based resins, amide-based resins, butyral-based resins, styrene-based resins, nitrocellulose (nitrocellulose)-based resins, cellulose acetate-based resins, acrylic-urethane-based resins, vinyl chloride-vinyl acetate-based copolymer resins, vinyl chloride-vinyl acetate-acrylic copolymer resins, and chlorinated polypropylene-based resins. As the liquid component, for example, an organic solvent such as methyl ethyl ketone, toluene, cyclohexanone, ethyl acetate alcohol, ethanol, or methanol, or water can be used.

[0034] The design layer can be formed by partially printing an ink containing a colorant component, a resin component, and a liquid component by a gravure printing method using an intaglio roll. The design layer may be formed by partially printing ink of the same or different composition in different regions and / or by overlapping the same region multiple times.

[0035] The thickness of the design layer is preferably, for example, 0.1 μm or more and 5 μm or less, which can improve the film quality and adhesion. The thickness of the design layer is more preferably 0.5 μm or more and 3 μm or less.

[0036] (Transparent resin layer) The decorative sheet of the present disclosure has a transparent resin layer on one side of a base sheet. In addition, the term "transparency" refers to a range in which the design layer can be seen, and may be semi-transparent or colored.

[0037] The transparent resin layer contains homopolypropylene derived from biomass and random polypropylene derived from petroleum.

[0038] Biomass-derived homopolypropylene is produced by polymerizing only propylene, and the propylene used in the polymerization includes biomass-derived propylene. Examples of homopolypropylene derived from biomass include isotactic homopolypropylene, atactic homopolypropylene, and syndiotactic homopolypropylene.

[0039] From the viewpoint of reducing the environmental burden, the biomass-derived homopolypropylene preferably has a biomass ratio of 30% or more.

[0040] The petroleum-derived random polypropylene may be any polypropylene obtained by randomly copolymerizing propylene with a monomer other than propylene, and examples thereof include copolymers using ethylene, 1-butene, and the like.

[0041] The transparent resin layer has a biomass-derived homopolypropylene content of 20% by mass or more and 80% by mass or less based on the mass of the resin component constituting the transparent resin layer.

[0042] The transparent resin layer has a petroleum-derived random polypropylene content of 20% by mass or more and 80% by mass or less based on the mass of the resin component constituting the transparent resin layer. From the viewpoint of imparting favorable processability in a low-temperature environment, the transparent resin layer preferably contains petroleum-derived random polypropylene in an amount of 50% by mass or more relative to the mass of the resin components constituting the transparent resin layer.

[0043] The transparent resin layer may contain petroleum-derived homopolypropylene. Petroleum-derived homopolypropylene is made by polymerizing only petroleum-derived propylene. Examples of petroleum-derived homopolypropylene include isotactic homopolypropylene, atactic homopolypropylene, and syndiotactic homopolypropylene.

[0044] From the viewpoint of imparting favorable processability in low-temperature environments and favorably suppressing a decrease in production speed during extrusion film formation, the content of petroleum-derived homopolypropylene is preferably 60 mass% or less, more preferably 40 mass% or less, even more preferably 20 mass% or less, and particularly preferably 0 mass% (i.e., the resin component constituting the transparent resin layer consists of biomass-derived homopolypropylene and petroleum-derived random polypropylene), relative to the mass of the resin components constituting the transparent resin layer.

[0045] The transparent resin layer preferably contains a lubricant from the viewpoints of reducing friction with machines during film formation and improving the fluidity and releasability of the resin. Examples of the lubricant include paraffin wax, polyethylene wax, stearic acid, stearic acid amide, oleic acid amide, butyl stearate, stearyl alcohol, magnesium stearate, and calcium stearate.

[0046] The content of the lubricant is preferably 0.01% by mass or more and 0.2% by mass or less based on the mass of the transparent resin layer.

[0047] The transparent resin layer may further contain various additives as necessary. For example, antioxidants, ultraviolet absorbers, light stabilizers, colorants such as dyes and pigments, etc. These additives can be appropriately selected and used from known additives.

[0048] The content of the additive is preferably 0.01% by mass or more and 0.2% by mass or less based on the mass of the transparent resin layer.

[0049] The thickness of the transparent resin layer is preferably 40 μm or more and 150 μm or less. By making the thickness of the transparent resin layer 40 μm or more, the scratch resistance of the decorative sheet can be suitably improved and durability can be imparted.By making the thickness of the transparent resin layer 150 μm or less, the amount of materials derived from fossil fuels can be suitably reduced in the entire decorative sheet, and the environmental load can be suitably reduced. In addition, when the transparent resin layer has an uneven shape, the thickness of the transparent resin layer means the thickness in a flat portion avoiding the uneven shape. The thicknesses of the surface protective layer described later and the adhesive auxiliary layer described later also mean the thicknesses in the flat portion avoiding the uneven shape.

[0050] The method for laminating the transparent resin layer is not limited as long as it is a common method, and examples thereof include a dry lamination method and an extrusion lamination method in which a molten resin is extruded using a T-die to perform lamination. A T-die or the like capable of extruding molten resin can be used as the extrusion mechanism described above.

[0051] The transparent resin layer may be subjected to a surface treatment such as a saponification treatment, a glow discharge treatment, a corona discharge treatment, a plasma discharge treatment, an ultraviolet (UV) treatment, or a flame treatment.

[0052] (Surface protective layer) The decorative sheet of the present disclosure has a surface protective layer on one side of the base sheet.

[0053] The surface protective layer may contain, for example, a cured product of a thermosetting component or a cured product of an ionizing radiation curable component as a main component. The cured product is preferably transparent.

[0054] Examples of the cured product of the thermosetting component include ester-based urethane and acrylic-based urethane.

[0055] The cured product of the ionizing radiation curable component may be, for example, a cured product of an oligomer and / or monomer having a radically polymerizable unsaturated group or a cationic polymerizable functional group in the molecule. The ionizing radiation means electromagnetic waves or charged particles having energy capable of polymerizing or crosslinking molecules, and generally includes electron beams (EB) or ultraviolet rays (UV). The method for forming the surface protective layer is not particularly limited, and known methods can be used.

[0056] As the oligomer having a radical polymerizable unsaturated group in the molecule, for example, oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, epoxy (meth)acrylate, melamine (meth)acrylate, triazine (meth)acrylate, etc. can be preferably used, and urethane (meth)acrylate oligomer is more preferable. As the molecular weight, those of about 250 or more and 100,000 or less are usually used.

[0057] As the monomer having a radically polymerizable unsaturated group in the molecule, for example, a polyfunctional monomer is preferable, and a polyfunctional (meth)acrylate is more preferable. Examples of polyfunctional (meth)acrylates include diethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, bisphenol A ethylene oxide modified di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane ethylene oxide tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate {pentafunctional (meth)acrylate}, dipentaerythritol hexa(meth)acrylate {hexafunctional (meth)acrylate}, etc. Monofunctional monomers may also be used as appropriate.

[0058] The ionizing radiation curable component preferably contains a urethane acrylate oligomer and a polyfunctional monomer in a mass ratio of urethane acrylate oligomer / polyfunctional monomer in the range of 6 / 4 or more and 9 / 1 or less.

[0059] When the ionizing radiation curable resin is crosslinked by ultraviolet light, it is preferable to use a photopolymerization initiator. The amount of the photopolymerization initiator added is, for example, 0.1 to 10 parts by mass per 100 parts by mass of the ionizing radiation curable component.

[0060] The surface protective layer may contain additives other than the inorganic filler as necessary. Examples of additives include fillers such as calcium carbonate and clay, flame retardants such as magnesium hydroxide, antioxidants, lubricants, foaming agents, ultraviolet absorbers, light stabilizers, deodorizers, antibacterial agents, antiviral agents, antiallergens, and antifungal agents. The above additives may be used alone or in combination of two or more.

[0061] The surface protective layer preferably contains at least one agent selected from the group consisting of an antibacterial agent, an antiviral agent, and an antiallergen agent.

[0062] Antibacterial agents include inorganic antibacterial agents and organic antibacterial agents. In particular, inorganic antibacterial agents are preferable because they are generally safer than organic antibacterial agents and have excellent durability and heat resistance. Inorganic antibacterial agents include antibacterial metals such as silver, copper, and zinc supported on various inorganic carriers.

[0063] When the surface protective layer contains an antibacterial agent, the amount is preferably 0.1 to 10 parts by mass per 100 parts by mass of the heat-curable component or ionizing radiation-curable component, but can be appropriately adjusted depending on the type of antibacterial agent.

[0064] Antiviral agents can generally be broadly divided into organic and inorganic types. Examples of organic antiviral agents include quaternary ammonium salts, quaternary phosphonium salts, pyridines, pyrithiones, benzimidazoles, organic iodines, isothiazolinones, and anions. Inorganic antiviral agents include those in which metal ions such as silver, copper, and zinc are supported on zeolite, apatite, zirconia, glass, molybdenum oxide, and the like. When the surface protective layer contains an antiviral agent, the amount is preferably 0.1 to 10 parts by mass per 100 parts by mass of the heat-curable component or ionizing radiation-curable component, but can be appropriately adjusted depending on the type of antiviral agent.

[0065] As the anionic antiviral agent, for example, those containing a styrene polymer derivative compound and an unsaturated carboxylic acid derivative compound are preferable.

[0066] As the inorganic antiviral agent, a silver-based antiviral agent is preferable from the viewpoint of lack of biotoxicity and excellent safety, and among them, a phosphate glass-supported silver compound or a silver zeolite compound, and a molybdenum oxide-silver double salt compound are more preferable because they exhibit antiviral performance even in small amounts and therefore the amount added can be reduced.

[0067] The antiallergen agent contains either an inorganic compound or an organic compound, and each may be used alone or two or more different types may be mixed. The inorganic compound is preferably a material supporting a metal. The amount of the antiallergen agent added is preferably 1.0 to 40 parts by mass, more preferably 1 to 10 parts by mass, per 100 parts by mass of the heat-curable component or ionizing radiation-curable component, but can be appropriately adjusted depending on the type of antiallergen agent.

[0068] As the inorganic material of the inorganic compound, for example, at least one selected from the group consisting of titanium oxide, calcium phosphate, calcium silicate, zirconium phosphate, zeolite, silica alumina, magnesium silicate, and magnesium phosphate is preferable, and among these, titanium oxide, zirconium phosphate, etc. are more preferable. As a commercially available product, for example, "Allerimub (trade name)" manufactured by Toagosei Co., Ltd. can be used.

[0069] The metal supported on the inorganic material is preferably at least one selected from the group consisting of gold, platinum, zinc and copper other than silver, and among these, zinc is preferred.

[0070] As a commercially available product, for example, "Atomy Ball TZ-R: Titanium oxide carrying zinc" manufactured by JGC Catalysts Co., Ltd. can be suitably used. These anti-allergen agents are effective against various allergens such as mites and pollen.

[0071] The organic compound is preferably a water-insoluble polymer containing a phenolic hydroxyl group, a polyphenol compound supported on an inorganic solid acid, or a polymer containing at least one monomer component selected from the group consisting of styrenesulfonic acid and its salts.

[0072] As the water-insoluble polymer containing a phenolic hydroxyl group, commercially available products such as "Allerbuster (trade name)" manufactured by Sekisui Chemical Co., Ltd. and "Marukalinker M (trade name)" manufactured by Maruzen Oil Co., Ltd. can be used. These anti-allergen agents are effective against various allergens such as mites and pollen.

[0073] The surface protective layer may have a gloss / matt effect. The gloss matte effect refers to a design effect that makes glossy areas stand out and non-glossy areas appear recessed. The method of imparting the matte gloss effect is not particularly limited, and may include a gloss regulator in the surface protective layer, or may be realized by the uneven shape described later. The uneven shape may have a maximum height Rz of 10 μm or more and 60 μm or less. The pattern formed by the matte gloss effect of the surface protective layer may or may not be in harmony with the whole or part of the pattern formed by the pattern layer.

[0074] The thickness of the surface protective layer is not particularly limited, but is, for example, 1 μm to 50 μm. If the thickness of the surface protective layer is less than 1 μm, sufficient durability (scratch resistance, stain resistance, weather resistance, etc.) may not be imparted, and if it exceeds 50 μm, the transmittance may decrease, resulting in reduced visibility of the pattern of the pattern layer. The thickness of the surface protective layer may be 3 μm or more and 40 μm or may be 5 μm or more and 35 μm or more.

[0075] (uneven shape) From the standpoint of providing a suitable design, the decorative sheet of the present disclosure preferably has an uneven shape on the surface opposite to the side provided with the base sheet of the present disclosure (the surface of the surface protective layer). The uneven shape may reach the transparent resin layer or the adhesive auxiliary layer (adhesive auxiliary layer 7 in FIG. 1) described later.

[0076] The maximum height Rz of the uneven shape is preferably 10 μm or more and 60 μm or less. By having the above-mentioned uneven shape, it is possible to suitably impart an excellent design that gives a three-dimensional feel not only visually but also tactilely (touch-wise). Incidentally, "maximum height Rz" refers to the maximum height Rz specified in JIS B 0601 (2001).

[0077] The method for forming the uneven shape is not particularly limited, and examples thereof include a method of embossing with heat, a method of transferring the uneven shape using a shaping sheet, and the like. The thermal embossing process may be carried out, for example, by using a well-known sheet-type or rotary embossing machine. Examples of embossed patterns include sand grain, hairline, matte finish, wood grain vascular grooves, stone slab surface irregularities, cloth surface texture, and striped grooves.

[0078] (adhesion auxiliary layer) The decorative sheet of the present disclosure may have an adhesive auxiliary layer between each layer (between the base sheet and the pattern layer, and between the transparent resin layer and the surface protective layer), and may have an adhesive auxiliary layer (back adhesive auxiliary layer) on the back surface of the base sheet (the side opposite to the side having the pattern layer). The adhesion auxiliary layer functions as a primer layer or an easy-adhesion layer.

[0079] For the adhesive auxiliary layer, for example, a urethane adhesive such as an ester-based urethane or an acrylic-based urethane, an acrylic adhesive, an epoxy adhesive, or a rubber adhesive can be used.

[0080] The adhesive auxiliary layer may contain an ultraviolet absorbing agent and a light stabilizer. The ultraviolet absorbing agent and the light stabilizer can be appropriately selected from those described in the transparent resin layer.

[0081] From the viewpoint of suitably suppressing poor adhesion between layers, the adhesion auxiliary layer preferably has a thickness of 0.1 μm or more and 30 μm or less. The method for forming the adhesive auxiliary layer is not particularly limited, and any known method may be appropriately selected.

[0082] (adhesive layer) The decorative sheet of the present disclosure may have an adhesive layer between the design layer and the transparent resin layer. The adhesive layer is preferably transparent.

[0083] As the adhesive for the adhesive layer, for example, a urethane-based adhesive such as an ester-based urethane or an acrylic-based urethane, an acrylic-based adhesive, an epoxy-based adhesive, or a rubber-based adhesive can be used.

[0084] The thickness of the adhesive layer is, for example, not less than 0.1 μm and not more than 30 μm. The method for forming the adhesive layer is not particularly limited, and any known method may be appropriately selected.

[0085] (Method of manufacturing decorative sheets) In the method for producing a decorative sheet according to the present disclosure, the order in which the above-mentioned layers are formed is not particularly important. For example, an adhesive auxiliary layer (also called a pattern auxiliary layer), a pattern layer, an adhesive layer, a transparent resin layer, an adhesive auxiliary layer, and a surface protective layer may be formed in this order on one side of the base sheet of the present disclosure. Furthermore, the steps of forming each layer do not have to proceed consecutively, and other steps or treatments may be carried out between these steps.

[0086] <Decorative board> The decorative board of the present disclosure has an adherend laminated on the side of the base sheet of the decorative sheet of the present disclosure opposite the side having the pattern layer.

[0087] Examples of the adherend include a wood board, a gypsum board, a cement board, a ceramic board, a metal board, a resin board, and a fiber-reinforced plastic board. For example, the adherend may be laminated on the side of the substrate sheet of the present disclosure opposite the side having the pattern layer using an adhesive that forms the adhesive layer described above.

[0088] The present specification discloses the following:

[0089] The present disclosure (1) is a decorative sheet having at least a pattern layer, a transparent resin layer, and a surface protective layer, in this order, on one side of a base sheet, the transparent resin layer containing a biomass-derived homopolypropylene and a petroleum-derived random polypropylene, the content of the biomass-derived homopolypropylene being 20% ​​by mass or more and 80% by mass or less relative to the mass of the resin components constituting the transparent resin layer, and the content of the petroleum-derived random polypropylene being 20% ​​by mass or more and 80% by mass or less relative to the mass of the resin components constituting the transparent resin layer. The present disclosure (2) is the decorative sheet according to the present disclosure (1), wherein the biomass-derived homopolypropylene has a biomass degree of 30% or more. The present disclosure (3) is the decorative sheet according to the present disclosure (1) or (2), in which the transparent resin layer has a thickness of 40 μm or more and 150 μm or less. The present disclosure (4) is the decorative sheet according to any one of the present disclosures (1) to (3), wherein the transparent resin layer has an uneven shape on the side having the surface protective layer. The present disclosure (5) is the decorative sheet according to any one of the present disclosures (1) to (4), wherein the transparent resin layer contains a lubricant. The present disclosure (6) is the decorative sheet according to the present disclosure (5), wherein the lubricant is calcium stearate. The present disclosure (7) is a decorative sheet according to any one of the present disclosures (1) to (6), which has an adhesive auxiliary layer on the side of the base sheet opposite to the side having the design layer. The present disclosure (8) is the decorative sheet according to any one of the present disclosures (1) to (7), wherein the base sheet contains a biomass-derived polyolefin. The present disclosure (9) is a decorative sheet according to any one of the present disclosures (1) to (8), wherein the surface protective layer contains at least one agent selected from the group consisting of an antibacterial agent, an antiviral agent, and an antiallergen agent. The present disclosure (10) is a decorative board comprising an adherend on the side of the base sheet of the decorative sheet according to any one of the present disclosures (1) to (9) opposite to the side having the pattern layer. EXAMPLES

[0090] The present invention will now be described in more detail with reference to examples, but the present disclosure is not limited to these examples.

[0091] Example 1 A colored polypropylene sheet having a thickness of 60 μm was prepared as a base sheet. An ink containing an organic solvent was solid-printed on one side of the base sheet using a gravure printing method with an intaglio roll to form a back adhesion auxiliary layer made primarily of an ester-based polyurethane resin that covered one side of the base sheet. On the other side of the base sheet, an ink containing an organic solvent was solid-printed by gravure printing using an intaglio roll to form a design layer mainly composed of an acrylic-urethane resin. An ester-based polyurethane was applied to the surface of the design layer opposite the substrate sheet to form an adhesive layer having a thickness of 10 μm. Thereafter, a transparent resin layer having a thickness of 60 μm was formed on the adhesive layer by extrusion molding, using dry lamination. The transparent resin layer was made of a resin blended with 80% by mass of homopolypropylene derived from biomass (biomass content 50%) and 20% by mass of random polypropylene derived from petroleum. Furthermore, an adhesive auxiliary layer made of an acrylic-urethane copolymer resin having a thickness of 2 μm was formed on the side opposite the adhesive layer of the transparent resin layer, and a coating agent (urethane acrylate-based ionizing radiation curable resin composition) was applied onto the adhesive auxiliary layer by gravure coating. After that, the coating agent was cured by irradiating with ionizing radiation to form a surface protection layer having a thickness of 5 μm. Finally, the surface having the surface protective layer was embossed with heat and pressure to form a concave-convex shape, thereby producing a decorative sheet. The biomass degree of the biomass-derived homopolypropylene was calculated by the method described in this specification.

[0092] (Examples 2 to 4, Comparative Examples 1 to 3) A resin was prepared by blending biomass-derived homopolypropylene, petroleum-derived random polypropylene, and petroleum-derived homopolypropylene in the ratios shown in Table 1, and a decorative sheet was produced in the same manner as in Example 1, except that this was used as the transparent resin layer. In Table 1, biomass-derived homopolypropylene is abbreviated as "biomass homo PP," petroleum-derived homopolypropylene is abbreviated as "petroleum homo PP," and petroleum-derived random polypropylene is abbreviated as "petroleum random PP." In addition, in Table 1, the numerical values ​​listed in the right column of the resin components such as "biomass homo-PP" in each example indicate the content (mass %) of each resin component relative to the mass of the resin component constituting the transparent resin layer.

[0093] Example 5 A decorative sheet was produced in the same manner as in Example 1, except that 3 parts by mass of a phosphate-based glass-silver-supported compound (PG-711, manufactured by Koa Glass Co., Ltd.) was added as an antiviral agent per 100 parts by mass of the coating agent (urethane acrylate-based ionizing radiation-curable resin composition) used to form the surface protective layer.

[0094] Example 6 A decorative sheet was produced in the same manner as in Example 1, except that 16 parts by mass each of an anionic phenol-based material (anti-allergen agent, EXP20530A manufactured by DIC Corporation) and a zinc-based material (anti-allergen agent, EXP20530B manufactured by DIC Corporation) were blended with 100 parts by mass of the coating agent (urethane acrylate-based ionizing radiation curable resin composition) used to form the surface protective layer.

[0095] <Evaluation method>

[0096] (1) Processability in low temperature environments The side of the prepared decorative sheet with the back adhesive auxiliary layer and the MDF were attached with an emulsion adhesive (application amount 75 g / m 2 ) were used to create a test piece (width 30 cm, length 30 cm, thickness 2.5 mm). After curing the test pieces, a V-shaped groove (2.4 mm deep, 4 mm wide) was dug in the side of the MDF that did not have the decorative sheet attached, and the piece was wrapped around a rectangular piece of wood (20 cm long, 10 cm wide, 5 cm high) in an environment of 5°C, with the side of the MDF that did not have the decorative sheet attached touching the surface, to create a V-cut product. The V-cut products were visually inspected under a light source of 500 lux or more and rated according to the following criteria. ++: No cracks in the sheet at the corners (folded parts) were found from a distance of 50 cm. +: No cracks in the sheet were found at the corners (bends) from a distance of 1m. -: No cracks in the sheet can be seen from 50 cm away, but cracks in the sheet can be seen at the corners (folded parts) from 1 meter away. In the above test, a "++" or "+" rating was considered a pass, and a "-" rating was considered a fail.

[0097] (2) Production speed during extrusion film production The production speed (m / min) during extrusion film formation of biomass-derived homopolypropylene (biomass content 100%, thickness 60 μm) and the production speed (m / min) during extrusion film formation of the prepared transparent resin layer were measured. The degree of improvement in production speed was calculated using the following formula and evaluated according to the following criteria. (formula) [(Production rate of the prepared transparent resin layer during extrusion film production - Production rate of the biomass-derived homopolypropylene during extrusion film production) / Production rate of the biomass-derived homopolypropylene during extrusion film production] x 100 +: Production speed increased by 10% or more -:Production speed improvement is less than 10% In the above test, a "+" rating was considered a pass and a "-" rating was considered a fail.

[0098] (3) Antiviral activity The decorative sheets produced in Examples 1 and 5 were subjected to an antiviral performance test in accordance with the antiviral test method (ISO21702), and the antiviral activity value against influenza virus was calculated and evaluated based on the following evaluation criteria. The results are shown in Table 2. In addition, the antiviral agent (parts by mass) in Table 2 means the amount (parts by mass) of the antiviral agent used per 100 parts by mass of the coating agent (urethane acrylate-based ionizing radiation curable resin composition). +: Antiviral activity value was 2.0 or higher -: Antiviral activity value was less than 2.0 A "+" was considered a pass and a "-" was considered a fail.

[0099] (4) Anti-allergen properties The decorative sheets produced in Examples 1 and 6 were evaluated for anti-allergen performance. Specifically, the decorative sheets (10 cm x 10 cm) produced in Examples 1 and 6 were cut into small pieces and immersed in 60 mL of an aqueous solution of 20 to 30 ng / mL of allergen derived from Dermatophagoides farinae for one day. The amount of allergen was then visually confirmed by horizontal development chromatography (Mighty Checker) and evaluated according to the following evaluation criteria. The results are shown in Table 3. In addition, the anionic phenol-based material (parts by mass) and zinc-based material (parts by mass) listed in Table 3 refer to the amount (parts by mass) of the anionic phenol-based material and zinc-based material used per 100 parts by mass of the coating agent (urethane acrylate-based ionizing radiation curable resin composition). +: A reduction in the amount of allergens was confirmed (the mite allergen level was below + (i.e., about 100 mites / m 2 below) -: No reduction in allergens was confirmed (mite allergen level judged as + or higher) A "+" was considered a pass and a "-" was considered a fail.

[0100] [Table 1]

[0101] [Table 2]

[0102] [Table 3]

[0103] As shown in Table 1, the decorative sheet of the embodiment in which the transparent resin layer contains biomass-derived homopolypropylene and petroleum-derived random polypropylene, and the content of biomass-derived homopolypropylene is 20% by mass or more and 80% by mass or less, and the content of petroleum-derived random polypropylene is 20% by mass or more and 80% by mass or less, has excellent processability in low-temperature environments and can suppress a decrease in production speed during extrusion film formation. Furthermore, as can be seen from Table 2, the surface protective layer can have antiviral properties by including an antiviral agent, and as can be seen from Table 3, the surface protective layer can have antiallergen properties by including an antiallergen agent. [Explanation of symbols]

[0104] 1 Base sheet 2 Adhesive auxiliary layer (pattern auxiliary layer) 3. Picture layer 4 Adhesion auxiliary layer (back side adhesion auxiliary layer) 5 Adhesive layer 6 Transparent resin layer 7 Adhesion auxiliary layer (surface adhesion auxiliary layer) 8 Surface protective layer 10 Decorative Sheet

Claims

1. A substrate sheet has, on one surface thereof, at least a design layer, a transparent resin layer, and a surface protective layer, in this order; the transparent resin layer contains a homopolypropylene derived from biomass and a random polypropylene derived from petroleum, The transparent resin layer has a content of the biomass-derived homopolypropylene of 20% by mass or more and 80% by mass or less relative to the mass of the resin component constituting the transparent resin layer, and a content of the petroleum-derived random polypropylene of 20% by mass or more and 80% by mass or less relative to the mass of the resin component constituting the transparent resin layer. A decorative sheet characterized by:

2. The decorative sheet according to claim 1 , wherein the biomass-derived homopolypropylene has a biomass content of 30% or more.

3. 3. The decorative sheet according to claim 1, wherein the transparent resin layer has a thickness of 40 μm or more and 150 μm or less.

4. 3. The decorative sheet according to claim 1, wherein the transparent resin layer has an uneven shape on the side having the surface protective layer.

5. 3. The decorative sheet according to claim 1, wherein the transparent resin layer contains a lubricant.

6. 6. The decorative sheet according to claim 5, wherein said lubricant is calcium stearate.

7. 3. The decorative sheet according to claim 1, further comprising an adhesive auxiliary layer on the surface of said base sheet opposite to said design layer.

8. The decorative sheet according to claim 1 or 2, wherein the base sheet comprises a biomass-derived polyolefin.

9. 3. The decorative sheet according to claim 1, wherein the surface protective layer comprises at least one agent selected from the group consisting of an antibacterial agent, an antiviral agent, and an antiallergen agent.

10. A decorative board comprising an adherend on a surface of the base sheet of the decorative sheet according to claim 1 or 2 opposite to the surface having the pattern layer.