Novel modified polyamide-based polymer
The modified polyamide polymer, featuring terminal-modified vinyl structures, addresses the limitations of conventional polyamide polymers by enhancing breaking strain and surface impact strength, offering improved flexibility and low-temperature performance.
Patent Information
- Application Number
- JP2024036161
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional polyamide polymers lack improvements in physical properties such as breaking strain and surface impact strength.
A modified polyamide-based polymer is developed, comprising a macromonomer with terminal structures represented by a specific general formula, formed by polymerizing diamine and dicarboxylic acid with macromonomers containing terminal structures derived from vinyl monomers, enhancing the polymer's physical properties.
The modified polyamide polymer exhibits improved breaking strain and surface impact strength, along with enhanced flexibility and low-temperature properties, making it suitable for various applications.
Smart Images

Figure 2024134531000020 
Figure 2024134531000001 
Figure 2024134531000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel modified polyamide polymer. [Background technology]
[0002] Polyamide polymers are used in a variety of applications due to their excellent strength, heat resistance, chemical resistance, and the like.
[0003] For example, Patent Document 1 discloses a tube using a polyamide polymer, and Patent Document 2 discloses a film using a polyamide polymer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2020 / 175290 [Patent Document 2] Patent Publication No. 2019-104939 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the above-mentioned conventional polyamide polymers have room for improvement in physical properties such as breaking strain and / or dart impact strength.
[0006] In view of the above circumstances, an object of one aspect of the present invention is to provide a novel modified polyamide-based polymer. [Means for solving the problem]
[0007] The modified polyamide-based polymer according to one embodiment of the present invention (hereinafter, may be referred to as the "modified polyamide-based polymer") has the following properties: A macromonomer which is a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1): Diamine, A dicarboxylic acid, A polymer obtained by polymerizing a group of monomers including:
[0008] [ka]
[0009] In formula (1), R 1 is -O-, -O(CO)-, -NH-, -N(CH3)- or -N(CH2CH3)-; R 2 and R 3 each independently represents a single bond or a divalent or trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 1 or 2; When n is 2, there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different. Effect of the Invention
[0010] According to one aspect of the present invention, a novel modified polyamide polymer can be provided. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic diagram showing the structure of a modified polyamide polymer according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] An embodiment of the present invention will be described below, but the present invention is not limited thereto. In this specification, unless otherwise specified, "A to B" representing a numerical range means "A or more and B or less." In addition, in this specification, "(meth)acrylic" means acrylic and / or methacrylic.
[0013] [1. Modified polyamide polymer] The modified polyamide-based polymer according to one embodiment of the present invention (hereinafter, may be referred to as "the modified polyamide-based polymer") is A macromonomer which is a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1): Diamine, A dicarboxylic acid, A polymer obtained by polymerizing a group of monomers including:
[0014] [ka]
[0015] In formula (1), R 1 is -O-, -O(CO)-, -NH-, -N(CH3)- or -N(CH2CH3)-; R 2 and R 3 each independently represents a single bond or a divalent or trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 1 or 2; When n is 2, there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.
[0016] Since the present modified polyamide polymer has the above-mentioned structure, it is possible to improve physical properties such as breaking strain and / or dart impact strength.
[0017] The modified polyamide polymer is a polymer made from a monomer group containing the macromonomer, diamine, and dicarboxylic acid, and is a polymer containing, as constituent units, a constituent unit derived from the macromonomer, a constituent unit derived from the diamine, and a constituent unit derived from the dicarboxylic acid. The monomer group as the raw material of the modified polyamide polymer and each monomer component contained in the monomer group will be described in detail below.
[0018] <Macromonomer> The macromonomer, which is one component of the monomer group that is the raw material of the present modified polyamide polymer, is a terminal-modified vinyl polymer having one or more terminal structures represented by the above general formula (1).
[0019] (Terminal structure) The macromonomer has one or more terminal structures represented by the general formula (1). Here, "having one or more terminal structures" means that the macromonomer has a terminal structure represented by the general formula (1) at at least one end of the vinyl polymer that is the main chain. The number of terminal structures represented by the general formula (1) that the macromonomer has is not particularly limited as long as it is one or more. For example, when the vinyl polymer that is the main chain is a linear (straight-chain) polymer, only one end of the linear polymer may have the terminal structure represented by the general formula (1), or both ends may have the terminal structure represented by the general formula (1). In addition, when the vinyl polymer that is the main chain is a branched polymer having three or more ends, only one end of the branched polymer may have the terminal structure represented by the general formula (1), some of two or more ends may have the terminal structure represented by the general formula (1), or all ends may have the terminal structure represented by the general formula (1).
[0020] As the macromonomer, one type of vinyl polymer having the terminal structure represented by the above general formula (1) may be used alone, or two or more types may be used in combination. For example, the modified polyamide polymer may contain, as a macromonomer component, both a linear polymer having the terminal structure represented by the above general formula (1) at only one end, and a linear polymer having the terminal structure represented by the above general formula (1) at both ends.
[0021] A more specific embodiment of the terminal structure represented by the above general formula (1) in the above macromonomer will be described in detail below.
[0022] In the above general formula (1), R 1 is -O-, -O(CO)-, -NH-, -N(CH3)- or -N(CH2CH3)-. 1 is preferably -O(CO)- or -NH-.
[0023] In the above general formula (1), R 2 is a divalent or trivalent group having 1 to 8 carbon atoms, which may have a heteroatom.
[0024] R 2 has 1 to 8 carbon atoms, and preferably 1 to 6 carbon atoms.
[0025] R 2 Examples of the heteroatom that may be contained include an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom, and a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).
[0026] R 2 may be a linear structure, a branched structure, or a cyclic structure. 2 When is a cyclic structure, R 2 may have a heterocyclic structure.
[0027] More specifically, R 2is preferably a divalent or trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl.
[0028] In this specification, divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl refers to a group in which one hydrogen atom is removed from a normally monovalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl. That is, divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl has two bonding sites with other molecules. Divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl is also referred to as alkylene, heteroalkylene, cycloalkylene, heterocycloalkylene, arylene, or heteroarylene.
[0029] In addition, in this specification, trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl refers to a group in which two hydrogen atoms have been removed from a normally monovalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl. In other words, a trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl has three bonding sites with other molecules.
[0030] In the above general formula (1), R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom.
[0031] R 3 The number of carbon atoms in R is 0 to 8, preferably 0 to 6, more preferably 0 to 4, and further preferably 0 to 2. 3 The number of carbon atoms in R is 0. 3 is a single bond or consists of only heteroatoms.
[0032] R 3 Examples of the heteroatom that may be contained include an oxygen atom, a nitrogen atom, a sulfur atom, a phosphorus atom, and a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom).
[0033] R 3 may be a linear structure, a branched structure, or a cyclic structure. 3 When is a cyclic structure, R 3 may have a heterocyclic structure.
[0034] More specifically, R 3 is preferably a divalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl.
[0035] In the above general formula (1), R 4 and R 5 are each independently hydrogen, a methyl group, or an ethyl group. Among these, R 4 and R 5 is preferably hydrogen. Thus, R 4 or R 5 At least one of R is preferably hydrogen. 4 and R 5 More preferably, each of the groups is hydrogen.
[0036] In a preferred embodiment of the present invention, in the above general formula (1), R 2 has 1 to 6 carbon atoms, and R 3 has 0 to 2 carbon atoms, and R 4 and R 5 are both hydrogen.
[0037] In the above general formula (1), n is 1 or 2. In other words, the terminal structure represented by the above general formula (1) has one structure represented by the following general formula (1') when (i) n is 1, and has two structures represented by the following general formula (1') when (ii) n is 2. -R3 -N(R 4 )R 5 (1') That is, when n is 2, the terminal structure represented by the above general formula (1) is R 3 , R 4 and R 5 Each of the compounds has two structures represented by the following formula:
[0038] When n is 2, R 3 , R 4 and R 5 may be the same or different. In other words, when n is 2, the structures represented by the above general formula (1') present in each of the terminal structures represented by the above general formula (1) may be the same or different.
[0039] Specific examples of the terminal structure represented by the above general formula (1) include structures represented by the following formulas (i) to (iii). The above macromonomer preferably has any one of structures selected from the following formulas (i) to (iii) as a terminal structure.
[0040] [ka]
[0041] (Main Chain) The macromonomer has a main chain structure composed of structural units derived from a vinyl monomer.
[0042] The vinyl monomer from which the structural unit constituting the main chain of the macromonomer is derived is not particularly limited as long as it has a vinyl group.Examples of the vinyl monomer include (meth)acrylic acid monomers, styrene monomers, maleimide monomers, chlorine-containing vinyl monomers, fluorine-containing vinyl monomers, silicon-containing vinyl monomers, nitrile group-containing vinyl monomers, amide group-containing vinyl monomers, vinyl esters, alkenes, and conjugated dienes.
[0043] Examples of the (meth)acrylic acid monomer include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-methyl-3-propanediol ... Hydroxypropyl, stearyl (meth)acrylate, glycidyl (meth)acrylate, 2-aminoethyl (meth)acrylate, γ-((meth)acryloyloxypropyl)trimethoxysilane, ethylene oxide adduct of (meth)acrylic acid, trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, 2-perfluoroethyl (meth)acrylate, perfluoromethyl (meth)acrylate, diperfluoromethylmethyl (meth)acrylate, 2-perfluoromethyl-2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, 2-perfluorohexadecylethyl (meth)acrylate, and the like.
[0044] Examples of the styrene monomer include styrene, vinyltoluene, α-methylstyrene, chlorostyrene, styrenesulfonic acid, and salts of styrenesulfonic acid.
[0045] Examples of the maleimide monomer include maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide.
[0046] The chlorine-containing vinyl monomer is not particularly limited, but suitable examples include vinyl chloride, vinylidene chloride, and allyl chloride.
[0047] Examples of the fluorine-containing vinyl monomer include perfluoroethylene, perfluoropropylene, and vinylidene fluoride.
[0048] Examples of the silicon-containing vinyl monomer include vinyltrimethoxysilane and vinyltriethoxysilane.
[0049] Examples of the nitrile group-containing vinyl monomer include acrylonitrile and methacrylonitrile.
[0050] Examples of the amide group-containing vinyl monomer include acrylamide and methacrylamide.
[0051] Examples of vinyl esters include vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, and vinyl cinnamate.
[0052] Examples of alkenes include ethylene, propylene, butylene, and isobutylene.
[0053] Examples of conjugated dienes include butadiene and isoprene.
[0054] Suitable examples of the vinyl monomer from which the structural units constituting the main chain of the macromonomer are derived include maleic anhydride, maleic acid, monoalkyl esters of maleic acid, dialkyl esters of maleic acid, fumaric acid, monoalkyl esters of fumaric acid, dialkyl esters of fumaric acid, and allyl alcohol.
[0055] The main chain of the macromonomer may be a homopolymer containing only structural units derived from one of the vinyl monomers described above, or may be a copolymer containing structural units derived from any two or more vinyl monomers.
[0056] In particular, since modification of the polymer terminals is relatively easy, the main chain of the macromonomer is preferably composed mainly of one or more of a constituent unit derived from a (meth)acrylic acid monomer, a constituent unit derived from a styrene monomer, or a constituent unit derived from isobutylene. That is, the main chain of the macromonomer is preferably composed mainly of poly(meth)acrylate, polystyrene, or polyisobutylene. The main chain of the macromonomer may be a copolymer composed mainly of a constituent unit derived from two or more types selected from the group consisting of a (meth)acrylate monomer, a styrene monomer, and isobutylene.
[0057] In this specification, the vinyl polymer In this specification, the main chain of a vinyl polymer mainly comprises poly(meth)acrylate means that the main chain contains 50 mol% or more of structural units derived from (meth)acrylic acid out of 100 mol% of all structural units contained in the main chain. When the main chain of the macromonomer is mainly comprised of poly(meth)acrylate, the main chain of the macromonomer preferably contains 60 mol% or more of structural units derived from (meth)acrylic acid out of 100 mol% of all structural units contained in the main chain, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, and may even be 100 mol%.
[0058] In this specification, the main chain of a vinyl polymer mainly composed of polystyrene means that the main chain contains 50 mol% or more of structural units derived from styrene monomers out of 100 mol% of all structural units contained in the main chain. When the main chain of the present terminal-modified vinyl polymer is mainly composed of polystyrene, the main chain of the present terminal-modified vinyl polymer preferably contains 60 mol% or more of structural units derived from styrene monomers out of 100 mol% of all structural units contained in the main chain, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, or may even be 100 mol%.
[0059] In this specification, the main chain of a vinyl polymer mainly composed of polyisobutylene means that, out of 100 mol% of all structural units contained in the main chain, structural units derived from isobutylene account for 50 mol% or more. When the main chain of the macromonomer is mainly composed of polyisobutylene, the main chain of the macromonomer preferably contains structural units derived from isobutylene at 60 mol% or more, more preferably at 70 mol% or more, even more preferably at 80 mol% or more, even more preferably at 90 mol% or more, or may even be 100 mol%.
[0060] In this specification, the main chain of a vinyl polymer mainly comprises structural units derived from two or more selected from the group consisting of (meth)acrylate, styrene, and isobutylene, meaning that the main chain contains structural units derived from (meth)acrylate monomers, styrene monomers, or isobutylene in a total amount of 50 mol% or more out of 100 mol% of all structural units contained in the main chain. When the main chain of the present terminally modified vinyl polymer mainly comprises structural units derived from two or more selected from the group consisting of (meth)acrylate monomers, styrene monomers, and isobutylene, the main chain of the macromonomer preferably contains structural units derived from (meth)acrylate monomers, styrene monomers, or isobutylene in a total amount of 60 mol% or more out of 100 mol% of all structural units contained in the main chain, more preferably contains 70 mol% or more, even more preferably contains 80 mol% or more, even more preferably contains 90 mol% or more, and may be 100 mol%.
[0061] The main chain of the macromonomer may contain, in addition to the constituent units derived from the vinyl monomers, constituent units derived from monomers other than the vinyl monomers (other monomers). Examples of the other monomers include vinyl chloride, acrylonitrile, and acrylamide.
[0062] The content of structural units derived from other monomers in the main chain of the macromonomer is preferably less than 50 mol%, more preferably 40 mol% or less, more preferably 30 mol% or less, even more preferably 20 mol% or less, even more preferably 10 mol% or less, and may be 0 mol%, based on 100 mol% of all structural units contained in the main chain.
[0063] The structure of the main chain of the macromonomer is not particularly limited, and may be a linear structure or a branched structure, i.e., the main chain of the macromonomer may be a linear polymer or a branched polymer.
[0064] In a preferred embodiment of the present invention, the main chain of the macromonomer is preferably a linear polymer, and one or both ends of the linear polymer preferably have a terminal structure represented by the general formula (1) above.
[0065] The polymerization method for the vinyl polymer that is the main chain of the macromonomer is not particularly limited, and examples thereof include the polymerization methods described in JP-A-2005-232419, JP-A-2006-291073, and JP-A-2016-88944.
[0066] The vinyl polymer, which is the main chain of the macromonomer, may have a structure derived from a substance other than the vinyl monomer (e.g., a polymerization catalyst, etc.) in the vinyl polymer (particularly at the terminal). For example, when a vinyl polymer is polymerized by a polymerization method using mercaptans described later, the obtained vinyl polymer may have a structure containing an S group derived from the mercaptans at its terminal. When such a vinyl polymer having an S group at its terminal is used as the main chain, the macromonomer may further have a structure containing an S group derived from the mercaptans between the terminal structure represented by the general formula (1) and the main chain structure consisting of the vinyl monomer.
[0067] The macromonomer may have a terminal structure represented by the general formula (1) at its terminal, and may further have a structure derived from a substance other than the vinyl monomer, such as a polymerization catalyst (e.g., a structure containing an S group), between the terminal structure represented by the general formula (1) and the main chain structure consisting of the vinyl monomer, as described above. Such an embodiment is also included in one embodiment of the present invention.
[0068] (Weight average molecular weight) The macromonomer preferably has a weight average molecular weight of 550 or more, more preferably 1,200 or more, and even more preferably 2,400 or more, as measured by size exclusion chromatography (SEC). The weight average molecular weight is preferably 1,100,000 or less, more preferably 200,000 or less, and even more preferably 50,000 or less. According to this configuration, the number of terminal structures represented by the general formula (1) introduced into the vinyl polymer can be easily controlled, and a macromonomer having a desired number of terminal structures represented by the general formula (1) can be provided.
[0069] (number average molecular weight) The macromonomer preferably has a number average molecular weight of 500 or more, more preferably 1,000 or more, and even more preferably 2,000 or more, as measured by size exclusion chromatography. The number average molecular weight is preferably 600,000 or less, more preferably 100,000 or less, and even more preferably 30,000 or less. According to this configuration, the number of terminal structures represented by the general formula (1) introduced into the vinyl polymer can be easily controlled, and a macromonomer having a desired number of terminal structures represented by the general formula (1) can be provided.
[0070] (Molecular weight distribution (Mw / Mn)) The macromonomer preferably has a molecular weight distribution, i.e., a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) measured by size exclusion chromatography of 1.8 or less, more preferably 1.7 or less, more preferably 1.6 or less, even more preferably 1.5 or less, even more preferably 1.4 or less, and particularly preferably 1.3 or less. According to this configuration, the number of terminal structures represented by the above general formula (1) introduced into the vinyl polymer can be easily controlled, and a macromonomer having a desired number of terminal structures represented by general formula (1) can be provided. The lower limit of the molecular weight distribution is theoretically 1.
[0071] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the vinyl polymer in this specification are values measured by SEC and calculated in terms of polystyrene. The specific method for measuring the weight average molecular weight (Mw) and number average molecular weight (Mn) of the vinyl polymer is as described in the Examples.
[0072] (Method of producing macromonomer) The method for producing the macromonomer is not particularly limited as long as it can provide a macromonomer, i.e., a terminal-modified vinyl polymer having one or more terminal structures represented by the above general formula (1). However, the following method (1) or method (2) can be mentioned as a preferred method for producing the macromonomer: Method (1): A method comprising the step of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the following general formula (2a):
[0073] [ka]
[0074] In formula (2a), X is -OH, -COOH, -NH2, -N(CH3)H or -N(CH2CH3)H, or a salt thereof; R 2 is a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; R, which exists twice in formula (1) and formula (2a), 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.
[0075] Method (2): A method comprising the steps of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the following general formula (2b) and reducing the resulting reaction product.
[0076] [ka]
[0077] In formula (2b), X is -OH, -COOH, -NH2, -N(CH3)H or -N(CH2CH3)H, or a salt thereof; R 2 is a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (1) and formula (2b), there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.
[0078] In the above formulas (2a) and (2b), examples of the salt for X include salts of alkali metals such as potassium and sodium, and salts of alkaline earth metals such as calcium and magnesium.
[0079] According to these methods for producing a macromonomer, it is possible to provide a macromonomer having one or more terminal structures represented by the above general formula (1). Therefore, these methods for producing a macromonomer can be suitably used as the method for producing the macromonomer.
[0080] Specific methods for producing the macromonomer will be described in detail below using methods (1) and (2) as examples, but the method for producing the macromonomer is not limited to these methods.
[0081] (Method (1)) The method for producing a macromonomer by method (1) (sometimes referred to as the "first method for producing a macromonomer") includes a step of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the above general formula (2a).
[0082] (First reaction step) The method for producing the first macromonomer includes a step of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the above general formula (2a) (sometimes referred to as the "first reaction step"). In this step, the end of the vinyl polymer is modified by reacting the compound represented by the above general formula (2a) with the end of the vinyl polymer, and a macromonomer having an end structure derived from the compound represented by the above general formula (2a), i.e., one or more end structures represented by the above general formula (1), can be obtained.
[0083] In the first reaction step, the method of reacting the halogen group located at the terminal of the vinyl polymer with the compound represented by the general formula (2a) is not particularly limited, but may include a method of dissolving the vinyl polymer having a halogen group at its terminal and the compound represented by the general formula (2a) in a solvent, and heating (and stirring as necessary) the vinyl polymer and the compound represented by the general formula (2a) in the solvent.
[0084] In the first reaction step, the solvent in which the reaction is carried out is not particularly limited, but since the reaction is a nucleophilic substitution reaction, a polar solvent is preferred. Examples of polar solvents that can be used in the first reaction step include N,N-dimethylacetamide, tetrahydrofuran, dioxane, diethyl ether, acetone, dimethyl sulfoxide, dimethylformamide, hexamethylphosphoric triamide, acetonitrile, etc.
[0085] In the first reaction step, the temperature (heating temperature) at which the vinyl polymer and the compound represented by the general formula (2a) in the solvent are heated is not limited, and is, for example, 30°C to 120°C, preferably 50°C to 100°C, and more preferably 70°C to 90°C.
[0086] The heating time in the first reaction step is not particularly limited, but it is preferable to continue heating until all halogen groups in the vinyl polymer subjected to the reaction are reacted (substituted) with the compound represented by the above general formula (2a). The specific heating time may be, for example, 30 minutes to 6 hours.
[0087] As described above, the terminal structure represented by the general formula (1) of the macromonomer obtained by the first method for producing a macromonomer has a structure derived from the compound represented by the general formula (2a). That is, in the terminal structure represented by the general formula (1) of the obtained macromonomer, R 1 In X, some atoms (e.g., H or metal elements constituting the salt) are replaced with bonds by reaction with the vinyl polymer, and R 1 , R 2 , R 3 , R 4 and R 5 Therefore, R in the compound represented by the general formula (2a) used in the method for producing the first macromonomer 2 , R 3 , R 4 and R 5 For more detailed aspects of the above, the description in the (Terminal Structure) section is incorporated as appropriate.
[0088] Specific examples of the compound represented by the above general formula (2a) include structures represented by the following formulae (iv) to (vi). As the compound represented by the general formula (2a), any compound selected from the following formulae (iv) to (vi) is preferable.
[0089] [ka]
[0090] (Method (2)) The method for producing a macromonomer by method (2) (sometimes referred to as the "second method for producing a macromonomer") comprises the steps of reacting a halogen group located at the end of a vinyl polymer with a compound represented by the following general formula (2b) and reducing the resulting reaction product.
[0091] (Second reaction step) The second method for producing a macromonomer includes a step of reacting a halogen group located at the terminal of a vinyl polymer with a compound represented by the above general formula (2b) (sometimes referred to as a "second reaction step"). In this step, the terminal of the vinyl polymer is modified by reacting the compound represented by the above general formula (2b) with the terminal of the vinyl polymer, thereby obtaining a terminal-modified vinyl polymer having one or more terminal structures derived from the compound represented by the above general formula (2b).
[0092] In the second reaction step, the method of reacting the halogen group located at the terminal of the vinyl polymer with the compound represented by the general formula (2b) is not particularly limited, but may include a method of dissolving the vinyl polymer having a halogen group at its terminal and the compound represented by the general formula (2b) in a solvent, and heating (and stirring as necessary) the vinyl polymer and the compound represented by the general formula (2b) in the solvent.
[0093] In the second reaction step, the solvent in which the reaction is carried out is not particularly limited, but since the reaction is a nucleophilic substitution reaction, a polar solvent is preferred. Examples of polar solvents that can be used in the second reaction step include N,N-dimethylacetamide, tetrahydrofuran, dioxane, diethyl ether, acetone, dimethyl sulfoxide, dimethylformamide, hexamethylphosphoric triamide, acetonitrile, etc.
[0094] In the second reaction step, the temperature (heating temperature) at which the vinyl polymer and the compound represented by the general formula (2b) in the solvent are heated is not limited, and is, for example, 30°C to 120°C, preferably 50°C to 100°C, and more preferably 70°C to 90°C.
[0095] The heating time in the second reaction step is not particularly limited, but it is preferable to continue heating until all halogen groups in the vinyl polymer subjected to the reaction are reacted (substituted) with the compound represented by the above general formula (2b). The specific heating time may be, for example, 30 minutes to 6 hours.
[0096] (Reduction process) The second method for producing a macromonomer includes a step of reducing a terminally modified vinyl polymer having one or more terminal structures derived from the compound represented by the above general formula (2b), i.e., the reaction product obtained in the above second reaction step. In this step, the reaction product obtained in the above second reaction step is reduced, i.e., the nitro groups at the terminals of the reaction product are reduced and converted to amino groups, thereby obtaining a macromonomer having one or more terminal structures represented by the above general formula (1) which are derived from the compound represented by the above general formula (2b). Therefore, the terminal structure of the macromonomer obtained in the second method for producing a macromonomer is a macromonomer having one or more terminal structures represented by the above general formula (1) which are derived from the compound represented by the above general formula (1). 4 and R 5 are terminal structures in which all are H.
[0097] In the reduction step, the method for reducing the reactant obtained in the second reaction step is not particularly limited, but may include a method in which the reactant obtained in the second reaction step is reacted with a reducing agent.
[0098] Examples of reducing agents that can be used in the reduction step include ammonium chloride, hydrogen, hydrazine, lithium aluminum hydride, and sodium borohydride.
[0099] As described above, the terminal structure represented by the general formula (1) of the terminally modified vinyl polymer obtained by the second method for producing a macromonomer has a structure derived from the compound represented by the general formula (2b). 1 In X, some atoms (e.g., H or metal elements constituting the salt) are replaced with bonds by reaction with the vinyl polymer, resulting in a structure of R 2 and R 3 Therefore, R in the compound represented by the general formula (2b) used in the method for producing the second macromonomer 1 , R 2 and R 3 For more detailed aspects of the above, the description in the (Terminal Structure) section is incorporated as appropriate.
[0100] A specific example of the compound represented by the above general formula (2b) is a structure represented by the following formula (vii): As the compound represented by the general formula (2b), the compound represented by the following formula (vii) is preferred because it causes few side reactions and can quantitatively react with the halogen group located at the end of the vinyl polymer.
[0101] [ka]
[0102] (Method (3)) In one embodiment of the present invention, as an aspect of the present production method other than the above-mentioned method (1) or method (2), there is provided a method for producing a terminal-modified vinyl polymer, comprising a step of reacting a functional group other than a halogen group, such as a hydroxyl group or a carboxyl group, located at the terminal of a vinyl polymer with a compound represented by the following general formula (2c) (method (3)):
[0103] [ka]
[0104] In formula (2c), X' is -OH, -NH2, -N(CH3)H, -N(CH2CH3)H, -COOH, -COZ or -Z (Z is a halogen atom); R 2 is a trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 3 represents a single bond or a divalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 2; In formula (2c), there are two R 3 , R 4 and R 5 The structures of may be the same or different. In this specification, the process for producing a terminally modified vinyl polymer by the process (3) is sometimes referred to as the "third process".
[0105] (Third reaction step) The third production method includes a step (sometimes referred to as a third reaction step) of reacting a functional group other than a halogen group, such as a hydroxyl group or a carboxyl group, located at the terminal of a vinyl polymer with a compound of the following general formula (2c). In this step, the terminal of the vinyl polymer is modified by reacting the compound represented by the above general formula (2c) with the terminal of the vinyl polymer, thereby obtaining a terminal-modified vinyl polymer having a terminal structure derived from the compound represented by the above general formula (2c), i.e., one or more terminal structures represented by the above general formula (1).
[0106] As described above, the terminal structure represented by the general formula (1) of the terminally modified vinyl polymer obtained by the third production method has a structure derived from the compound represented by the general formula (2c). That is, in the terminal structure represented by the general formula (1) of the obtained terminally modified vinyl polymer, R 1 In X', some atoms (e.g., H, OH, or Z) are replaced with bonds by reaction with the vinyl polymer, and R 1 , R 2 , R 3 , R 4 and R 5 Therefore, R in the compound represented by the general formula (2c) used in the third production method 2 , R 3 , R 4 and R 5 For more detailed aspects of the above, the above description is incorporated as appropriate.
[0107] (Vinyl polymer preparation process) The first macromonomer production method and the second macromonomer production method may further include a step of preparing a vinyl polymer having a halogen group at the end (vinyl polymer preparation step). As a method for preparing (polymerizing) a vinyl polymer having a halogen group at the end, various known polymerization methods such as living cationic polymerization and living radical polymerization can be adopted. In addition, the third production method may further include a step of preparing a vinyl polymer having a functional group other than a halogen group at the end. As a method for preparing (polymerizing) a vinyl polymer having a functional group other than a halogen group at the end, a polymerization method using a mercaptan having a hydroxyl group such as mercaptoethanol or a mercaptan having a carboxyl group such as mercaptoacetic acid, as described in JP-A-1-203412, can also be used.
[0108] Hereinafter, a specific embodiment of the vinyl polymer preparation process will be described in detail, taking the living radical polymerization method as an example.
[0109] As the vinyl monomer serving as the raw material for the vinyl polymer, each of the vinyl monomers described above in the section (Main Chain) can be appropriately used.
[0110] Examples of living radical polymerization include (a) a polymerization method using a chain transfer agent such as polysulfide, (b) a polymerization method using a radical scavenger such as an organic tellurium compound, a cobalt porphyrin complex, and / or a nitroxide compound, (c) an atom transfer radical polymerization (ATRP) method using an organic halide or the like as an initiator and a transition metal complex as a catalyst, and (d) a polymerization (reversible transfer catalytic polymerization (RTCP)) method using an organic halide or the like as an initiator and an organic molecule having a central atom such as nitrogen or oxygen as a catalyst. Of these, the atom transfer radical polymerization method is preferred because it is easy to control the molecular weight and molecular weight distribution of the vinyl polymer.
[0111] In living radical polymerization, the number of halogen terminals of the vinyl polymer obtained can be controlled by controlling the polymerization conditions. For example, the number of halogen terminals of the vinyl polymer obtained can be controlled by controlling the type of polymerization initiator. Specifically, when an initiator having one polymerization initiation point is used, a linear vinyl polymer having a halogen group at one end can be prepared, and when an initiator having two polymerization initiation points is used, a linear vinyl polymer having a halogen group at both ends can be prepared.
[0112] Examples of initiators having one polymerization initiation point include ethyl 2-bromoisobutyrate, ethyl bromoacetate, methyl bromoacetate, (1-bromoethyl)benzene, allyl bromide, methyl 2-bromopropionate, methyl chloroacetate, methyl 2-chloropropionate, (1-chloroethyl)benzene, etc. Examples of initiators having two polymerization initiation points include diethyl 2,5-dibromoadipate, dimethyl 2,5-dibromoadipate, diethyl 2,5-dibromoadipate, etc.
[0113] In the vinyl polymer preparation step, the number of halogen group terminals in the obtained vinyl polymer can be controlled, thereby controlling the number of compounds represented by general formula (2a) or (2b) which react with the vinyl polymer in the first reaction step or the second reaction step, i.e., the number of terminal structures represented by general formula (1) in the finally obtained macromonomer.
[0114] In the living radical polymerization, in addition to the initiator, a polymerization catalyst, a polydentate amine (ligand), a base, a reducing agent, a solvent, etc. may be used. The type and amount of each of these components can be appropriately selected by those skilled in the art.
[0115] (Macromonomer content) The content of the macromonomer in the monomer group, which is the raw material of the modified polyamide polymer, based on mass is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 1 mass% or more, based on the total amount of the monomer group (100 mass%). If the content of the macromonomer is 0.1 mass% or more, it is effective to improve physical properties such as breaking strain and / or dart impact strength. In addition, the content of the macromonomer is preferably 50 mass% or less, more preferably 30 mass% or less, and even more preferably 10 mass% or less, based on the total amount of the monomer group (100 mass%). If the content of the macromonomer is 50 mass% or less, it is effective to improve physical properties such as breaking strain and / or dart impact strength.
[0116] The content of the macromonomer on a molar basis in the monomer group as the raw material of the modified polyamide polymer is preferably 0.01 mol% or more, more preferably 0.02 mol% or more, and even more preferably 0.05 mol% or more, based on 100 mol% of the total amount of the monomer group. If the content of the macromonomer is 0.01 mol% or more, it is effective to improve physical properties such as breaking strain and / or dart impact strength. In addition, the content of the macromonomer on a molar basis is preferably 10 mol% or less, more preferably 3 mol% or less, and even more preferably 1 mol% or less, based on 100 mol% of the total amount of the monomer group. If the content of the macromonomer is 10 mol% or less, it is effective to improve physical properties such as breaking strain and / or dart impact strength.
[0117] <Diamine> The diamine, which is one of the monomers used as the raw material for the modified polyamide polymer, is a compound having two amines (amino groups) in one molecule. The diamine is not particularly limited as long as it has two amines (amino groups) in one molecule, and preferred examples of the diamine include aromatic diamines, aliphatic diamines, and polyether diamines.
[0118] Aliphatic diamines are diamines that have a linear, branched or cyclic hydrocarbon structure in the molecule.Specific examples of aliphatic diamines include 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, 1,13-diaminotridecane, 1,14-diaminotetradecane, 1,15-diaminopentadecane, 1,16-diaminohexadecane, 1,17-diaminoheptadecane, 1,18-diaminooctadecane, 1,19-diaminononadecane, 1,20-diaminoeicosane, cyclohexanediamine, and bis-(4-aminocyclohexyl)methane.
[0119] Aromatic diamines are diamines having an aromatic ring structure in the molecule. More specifically, aromatic diamines include 4,4'-diaminodiphenyl ether (ODA), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), p-phenylenediamine (PDA), 4,4'-diaminodiphenylmethane, benzidine, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone ... Examples of suitable amines include amine diphenyl ether, 3,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-phenylamine, 1,3-diaminobenzene, 1,2-diaminobenzene and the like.
[0120] Polyether diamines are diamines having a polyether structure in the molecule. More specifically, aromatic diamines include amino-modified polyoxyalkylenes (e.g., polyoxyethylene, 1,2-polyoxypropylene, 1,3-polyoxypropylene, or copolymers thereof).
[0121] As the diamine component, one of the above diamines may be used alone, or two or more of them may be used in any combination.
[0122] The diamine content in the monomer group, which is the raw material of the present modified polyamide-based polymer, is preferably 0 mol% or more, more preferably 20 mol% or more, and even more preferably 40 mol% or more, based on 100 mol% of the total amount of the monomer group. The diamine content is preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 55 mol% or less, based on 100 mol% of the total amount of the monomer group. If the diamine content is 70 mol% or less, a high molecular weight polyamide-based polymer can be obtained.
[0123] In this specification, even if a compound has two amines (amino groups) in one molecule, a compound having the structure of the above general formula (1) is not considered to be a diamine according to one embodiment of the present invention.
[0124] <Dicarboxylic acid> Dicarboxylic acid, which is one of the monomers used as the raw material for the modified polyamide polymer, is a compound having two carboxylic acids (carbonyl groups) in one molecule. The dicarboxylic acid is not particularly limited as long as it has two carboxylic acids (carbonyl groups) in one molecule, and aromatic dicarboxylic acids or aliphatic dicarboxylic acids are preferred. Aliphatic dicarboxylic acids are dicarboxylic acids having a linear, branched or cyclic hydrocarbon structure in the molecule. More specifically, aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, brassicic acid, tetradecanedioic acid, pentadecanedioic acid, and octadecanedioic acid.
[0125] The aromatic dicarboxylic acid is a dicarboxylic acid having an aromatic ring structure in the molecule. More specifically, examples of the aromatic dicarboxylic acid include terephthalic acid, phthalic acid, isophthalic acid, naphthalenedicarboxylic acid, and 2,6-naphthalenedicarboxylic acid.
[0126] As the dicarboxylic acid component, one of the above dicarboxylic acids may be used alone, or a plurality of dicarboxylic acids may be used in any combination.
[0127] In addition, the dicarboxylic acid used as the raw material of the present modified polyamide polymer may have a halogenated carboxylic acid (carbonyl group) contained in the molecule of the dicarboxylic acid. That is, a dicarboxylic acid halide (e.g., dicarboxylic acid chloride, etc.) may also be used as the dicarboxylic acid component used as the raw material of the present modified polyamide polymer.
[0128] The dicarboxylic acid content in the monomer group, which is the raw material of the present modified polyamide-based polymer, is preferably 0 mol% or more, more preferably 20 mol% or more, and even more preferably 40 mol% or more, based on 100 mol% of the total amount of the monomer group. The diamine content is preferably 70 mol% or less, more preferably 60 mol% or less, and even more preferably 55 mol% or less, based on 100 mol% of the total amount of the monomer group. If the dicarboxylic acid content is 70 mol% or less, a high molecular weight polyamide-based polymer can be obtained.
[0129] <Other monomers> The monomer group as the raw material of the present modified polyamide-based polymer may contain monomers (other monomers) other than the above-mentioned macromonomers, diamines, and dicarboxylic acids. In other words, the present modified polyamide-based polymer may contain structural units derived from other monomers. Such other monomers include aminocarboxylic acids, lactams, and the like. Among them, it is preferable that the monomer group as the raw material of the present modified polyamide-based polymer contains aminocarboxylic acids, since the molecular weight can be increased without changing the composition ratio of diamines and dicarboxylic acids, and the molecular weight can be easily adjusted.
[0130] Examples of aminocarboxylic acids include 12-aminododecanoic acid, 6-aminocaproic acid, 11-aminoundecanoic acid, para-aminomethylbenzoic acid, 4-aminocyclohexanecarboxylic acid, glycine, and alanine.
[0131] Examples of lactams include ε-caprolactam, ε-aminolaurolactam, ω-enantholactam, ω-undecanelactam, ω-dodecanelactam, α-pyrrolidone, and α-piperidone.
[0132] As the other monomer, one of the above-mentioned various monomers may be used alone, or a plurality of types may be used in any combination.
[0133] The content of other monomers in the monomer group that is the raw material of the present modified polyamide polymer is preferably 0 mol% or more, more preferably 10 mol% or more, and even more preferably 30 mol% or more, based on 100 mol% of the total amount of the monomer group. If the content of other monomers is 0 mol% or more, the effect of the function derived from the other monomers is exhibited. Moreover, the content of other monomers is preferably 99 mol% or less, more preferably 90 mol% or less, and even more preferably 70 mol% or less, based on 100 mol% of the total amount of the monomer group.
[0134] <Additives> The modified polyamide polymer can be made into a composition containing various additives according to the desired purpose, such as phosphorus compounds (e.g., phosphoric acid, pyrophosphoric acid, polyphosphoric acid, phosphorous acid, hypophosphorous acid, or alkali metal or alkaline earth metal salts thereof), heat resistance agents, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, lubricants, slipping agents, crystal nucleating agents, tackifiers, release agents, plasticizers, pigments, dyes, flame retardants, reinforcing materials, inorganic fillers, microfibers, X-ray opaque agents, etc.
[0135] As the additive, one of the various additives described above may be used alone, or multiple types may be used in any combination. Moreover, the type and amount of these additives can be appropriately selected by those skilled in the art according to the desired purpose.
[0136] <Structure of modified polyamide polymer> The modified polyamide polymer of the present invention can have different structures depending on the type (structure) of the macromonomer contained in the raw monomer group.
[0137] Consider the case where a macromonomer (macromonomer A) having one terminal structure in which n is 2 or more in general formula (1) is used as the macromonomer (case A). Macromonomer A is a macromonomer having two amino groups at one end. In case A, macromonomer A reacts with dicarboxylic acid via the terminal amino group to form modified polyamide polymer A, which is a copolymer of macromonomer A, dicarboxylic acid, and diamine. The obtained modified polyamide polymer A has a structure in which the main chain structure of macromonomer A is grafted to a polyamide main chain structure formed by bonding a structural unit derived from macromonomer A and diamine and a structural unit derived from dicarboxylic acid via an amide bond. Such a structure of modified polyamide polymer A is represented by the schematic diagram (a) in FIG. 1. In the schematic diagram (a), the thick band is the polyamide main chain structure, the thin line is the main chain structure of macromonomer A, and the circle is the bonding site between the polyamide main chain structure and macromonomer A.
[0138] Consider the case where a macromonomer (macromonomer B) having two or more terminal structures in which n is 2 or more in general formula (1) is used as the macromonomer (case B). Macromonomer B is a macromonomer having two amino groups at each of two or more terminals. In case B, macromonomer B reacts with dicarboxylic acid at each terminal through the amino group at the terminal to form a copolymer of macromonomer B, dicarboxylic acid, and diamine. As a result, the obtained modified polyamide polymer B has a structure in which one or two or more polyamide main chain structures formed by bonding a structural unit derived from macromonomer B and diamine to a structural unit derived from dicarboxylic acid through an amide bond are crosslinked through the main chain structure of macromonomer B. When two or more polyamide main chain structures are crosslinked, the structure of such modified polyamide polymer B is represented by the schematic diagram (b-1) shown in FIG. 1. In the schematic diagram (b-1), the thick band is the polyamide main chain structure, the thin line is the main chain structure of macromonomer B, and the circle is the bonding site between the polyamide main chain structure and macromonomer B. When one polyamide main chain structure is crosslinked (intramolecular crosslinking), the structure of such a modified polyamide polymer B is represented by the schematic diagram (b-2) shown in FIG. 1. In the schematic diagram (b-2), the thick band is the polyamide main chain structure, the thin line is the main chain structure of macromonomer B, and the circle is the bonding site between the polyamide main chain structure and macromonomer B.
[0139] Consider the case where a macromonomer (macromonomer C) having two or more terminal structures in which n is 1 in general formula (1) is used as the macromonomer (Case C). The macromonomer C is a macromonomer having one amino group at each of two or more terminals. In Case C, the macromonomer C reacts with the carboxylic acid terminal of the copolymer of dicarboxylic acid and diamine through the amino group at each terminal to form a copolymer of macromonomer C, dicarboxylic acid and diamine. As a result, the modified polyamide polymer C obtained has a structure in which the terminals of one or more polyamide main chain structures formed by bonding a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid through an amide bond are crosslinked through the main chain structure of the macromonomer C. The modified polyamide polymer C can also be said to be a block copolymer consisting of a polyamide block consisting of a structural unit derived from a diamine and a structural unit derived from a dicarboxylic acid, and a block consisting of the main chain structure of the macromonomer C. When the terminals of two or more polyamide main chain structures are crosslinked, the structure of such a modified polyamide polymer C is represented by the schematic diagram (c-1) shown in FIG. 1. In the schematic diagram (c-1), the thick band is the polyamide main chain structure, the thin line is the main chain structure of macromonomer C, and the circle is the bonding site between the polyamide main chain structure and the macromonomer C. When the terminal of one polyamide main chain structure is crosslinked (intramolecular crosslinking), the structure of such a modified polyamide polymer C is represented by the schematic diagram (c-2) shown in FIG. 1. In the schematic diagram (c-2), the thick band is the polyamide main chain structure, the thin line is the main chain structure of macromonomer C, and the circle is the bonding site between the polyamide main chain structure and the macromonomer C.
[0140] 2. Method for producing modified polyamide polymer In one embodiment of the present invention, there is provided a method for producing a modified polyamide polymer, comprising a step (polymerization step) of polymerizing a monomer group including a macromonomer, a diamine, and a dicarboxylic acid, the macromonomer being a terminal-modified vinyl polymer having one or more terminal structures represented by the above general formula (1).
[0141] According to a method for producing a terminally modified vinyl polymer according to one embodiment of the present invention (hereinafter, sometimes referred to as "the present production method"), it is possible to provide a modified polyamide polymer that is a terminally modified vinyl polymer having one or more terminal structures represented by the above general formula (1), and that contains a macromonomer, a diamine, and a dicarboxylic acid as constituent units. Therefore, the present production method can be suitably used as a method for producing the present terminally modified vinyl polymer.
[0142] For specific embodiments of the macromonomer, diamine, and dicarboxylic acid (as well as other monomers and additives that may be used optionally) used in this production method, the descriptions in the above section [1. Modified polyamide polymer] are incorporated as appropriate.
[0143] <Polymerization process> The mode of the polymerization step in the present production method is not particularly limited as long as it is possible to polymerize a monomer group containing the macromonomer, diamine, dicarboxylic acid, and optionally other monomers to obtain a modified polyamide-based polymer that is a copolymer of each monomer contained in the monomer group. For example, the following polymerization method (1) or (2) can be mentioned as a preferred mode: Method (1): A method of simultaneously mixing and reacting (polymerizing) each monomer contained in the above monomer group to obtain a copolymer; Method (2): The macromonomer, dicarboxylic acid, and, if the monomer group contains other monomers, the other monomers are mixed and reacted (polymerized) to obtain a prepolymer, and the prepolymer and diamine are further mixed and reacted (polymerized) to obtain a copolymer.
[0144] The polymerization reaction of the monomer group in the polymerization step can be carried out in a solvent or in a solvent-free state without using a solvent. Since no purification or the like is required and a modified polyamide-based polymer can be obtained by a simple operation, it is preferable to react (polymerize) the monomer group in a solvent-free state in the polymerization step. Such a reaction in a solvent-free state can be carried out, for example, by a melt-kneading method. In the polymerization step, it is preferable to use water as a solvent to form a salt of a diamine and a dicarboxylic acid and then react (polymerize) the salt, since it is easy to adjust the mixing ratio of the diamine and the dicarboxylic acid.
[0145] The polymerization reaction of the monomer group in the polymerization step may be carried out under pressure, normal pressure, or reduced pressure, but from the viewpoint of improving reactivity, it is preferable to carry out the polymerization reaction under reduced pressure. For example, the method of carrying out the polymerization reaction under reduced pressure includes a method of replacing the air in the reaction system with nitrogen and carrying out the polymerization reaction under a nitrogen atmosphere. From the viewpoint of maintaining the composition ratio of the volatile monomer, it is preferable to carry out the polymerization reaction of the monomer group under pressure. For example, the method of carrying out the polymerization reaction under pressure includes a method of replacing the air in the reaction system with nitrogen in a pressure-resistant container and carrying out the polymerization reaction under a nitrogen atmosphere.
[0146] In the polymerization step, additives may be further mixed with the monomer group. For specific examples of additives that can be used in the polymerization step, the description in the above section [1. Modified polyamide polymer] is appropriately incorporated. Among additives, phosphorus compounds are preferred because they function as catalysts for the reaction (polymerization) of the monomer group.
[0147] In the polymerization step, the temperature at which the monomers are reacted (polymerized) is not particularly limited, but is preferably 160 to 300° C., more preferably 180 to 250° C., in order to achieve both an improvement in the reaction rate and suppression of thermal decomposition of the monomers.
[0148] The reaction time of the polymerization reaction in the polymerization step is not particularly limited, but is preferably 2 to 10 hours, and more preferably 3 to 8 hours, from the viewpoint of suppressing coloration, etc. When a multi-stage polymerization reaction is carried out as in method (2), the reaction time refers to the total reaction time of each polymerization reaction.
[0149] <Forming process> The present production method may further include a molding step of molding the modified polyamide polymer obtained in the polymerization step to obtain a polyamide molded article. The molding method in the molding step is not particularly limited, and known molding methods such as compression molding, extrusion molding, blow molding, and injection molding can be used.
[0150] The shape of the polyamide-based molded product obtained in the molding step is not particularly limited, and examples of such shapes include films, sheets, fibers, etc. In one embodiment, the polyamide-based molded product made of the present modified polyamide-based polymer has excellent physical properties such as breaking strain and / or surface impact strength, and therefore can be suitably used as a molded product having a film shape or a sheet shape.
[0151] [3.Applications] The present modified polyamide-based polymer can be suitably used as a raw material for a molded article whose main raw material is the present modified polyamide-based polymer, or as a resin modifier to be added to other resins.
[0152] Molded articles using the present modified polyamide-based polymer as a main raw material are not particularly limited, but include food packaging films, automobile parts, computers and related devices, optical device parts, electric and electronic devices, information and communication devices, precision instruments, civil engineering and construction supplies, medical devices, household goods, etc. That is, the present modified polyamide-based polymer can be used for these wide range of applications. In addition, the present modified polyamide-based polymer can be a polymer excellent in impact resistance and low temperature properties, etc. Molded articles using such polymers as a raw material are particularly useful for applications such as food packaging films, automobile parts, electric and electronic devices, and medical devices.
[0153] The content of the present modified polyamide polymer in a molded product made from the present modified polyamide polymer is not particularly limited, but from the viewpoint of providing a molded product having excellent impact strength and low-temperature properties, etc., the content is preferably 10% by mass or more, preferably 50% by mass or more, may be 70% by mass or more, 80% by mass or more, or may be 90% by mass or more, based on a total amount (100% by mass) of the molded product. The upper limit of the content of the present modified polyamide polymer in the molded product is not particularly limited, and may be 100% by mass.
[0154] The present modified polyamide-based polymer can function as a resin modifier that modifies the physical properties of other resins by adding it to resins other than the present modified polyamide-based polymer (other resins). More specifically, the resin modifier containing the present modified polyamide-based polymer can be used in a wide range of applications, such as impact strength improver, low-temperature impact improver, flexibility improver, moldability improver, scratch resistance improver, friction and wear improver, squeak sound prevention material, weather resistance improver, and recyclability improver.
[0155] Other resins that can be modified by adding the present modified polyamide-based polymer are not particularly limited, but include polyamide-based resins, polyester-based resins, polycarbonate-based resins, polyolefin-based resins, polystyrene-based resins, polyvinyl chloride-based resins, acrylic-based resins, ABS-based resins, polyurethane-based resins, etc. In other words, the present modified polyamide-based polymer can be used as a resin modifier for these various resins.
[0156] When the present modified polyamide polymer is used as a resin modifier, the amount of the present modified polyamide polymer used (added amount) is not particularly limited, but for example, it is preferably 0.01 parts by mass or more, preferably 0.1 parts by mass or more, and may be 1 part by mass or more, or may be 5 parts by mass or more, relative to 100 parts by mass of the resin to be modified. In addition, the upper limit of the amount of the present modified polyamide polymer used (added amount) as a resin modifier is not particularly limited, and for example, it may be 50 parts by mass or less, 10 parts by mass or less, or may be 1 part by mass or less, relative to 100 parts by mass of the resin to be modified.
[0157] [4. Summary] An embodiment of the present invention may include the following features. [1] A macromonomer which is a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1): Diamine, A dicarboxylic acid, A modified polyamide-based polymer obtained by polymerizing a monomer group including:
[0158] [ka]
[0159] In formula (1), R 1 is -O-, -O(CO)-, -NH-, -N(CH3)- or -N(CH2CH3)-; R 2 and R 3 each independently represents a single bond or a divalent or trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 1 or 2; When n is 2, there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different. [2] R 2 and R 3 are each independently a divalent or trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl. [3] R 2 has 1 to 6 carbon atoms, R3 has 0 to 2 carbon atoms, R 4 and R 5 and each of are hydrogen. [4] The modified polyamide polymer according to any one of [1] to [3], wherein the terminal structure represented by the above general formula (1) has any structure selected from the following formulas (i) to (iii):
[0160] [ka]
[0161] [5] The macromonomer is a linear polymer, The modified polyamide polymer according to any one of [1] to [4], wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1). [6] The modified polyamide polymer according to any one of [1] to [5], wherein the main chain of the macromonomer is mainly composed of poly(meth)acrylate or polyisobutylene. [7] The modified polyamide polymer according to any one of [1] to [6], wherein the macromonomer has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less, as measured by size exclusion chromatography. [8] The modified polyamide polymer according to any one of [1] to [7], wherein the monomer group further contains an aminocarboxylic acid. [9] A macromonomer which is a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1): Diamine, A dicarboxylic acid, A method for producing a modified polyamide polymer, comprising the step of polymerizing a monomer group comprising:
[0162] [ka]
[0163] In formula (1), R 1 is -O-, -O(CO)-, -NH-, -N(CH3)- or -N(CH2CH3)-; R 2 and R 3 each independently represents a single bond or a divalent or trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 1 or 2; When n is 2, there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.
[10] R 2 and R 3 The method according to [9], wherein each of the is independently a divalent or trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl.
[11] R 2 has 1 to 6 carbon atoms, R 3 has 0 to 2 carbon atoms, R 4 and R 5 and are both hydrogen.
[12] The method according to any one of [9] to
[11] , wherein the terminal structure represented by the above general formula (1) has any structure selected from the following formulas (i) to (iii):
[0164] [ka]
[0165]
[13] The macromonomer is a linear polymer, The method according to any one of [9] to
[12] , wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1).
[14] The method according to any one of [9] to
[13] , wherein the main chain of the macromonomer is mainly composed of poly(meth)acrylate or polyisobutylene.
[15] The method according to any one of [9] to
[14] , wherein the macromonomer has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less, as measured by size exclusion chromatography.
[16] The method according to any one of [9] to
[15] , wherein the monomer group further contains an amino carboxylic acid.
[17] A molded article comprising the modified polyamide polymer according to any one of [1] to [8].
[18] A resin modifier comprising the modified polyamide polymer according to any one of [1] to [8].
[0166] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention. EXAMPLES
[0167] Hereinafter, one embodiment of the present invention will be described in detail with reference to examples, but the present invention is not limited to the following examples.
[0168] [Analysis method] (Polymerization conversion rate) The conversion rate of monomers to polymers in the production of vinyl polymers, which are raw materials for macromonomers, was measured using a gas chromatograph (GC (Shimadzu Corporation, GC-2000)). The column used was Agilent J&W GC column HP-1. Toluene was used as the standard.
[0169] (Qualitative and quantitative analysis of functional groups) The qualitative and quantitative analysis of functional groups in vinyl polymers and macromonomers, which are the raw materials for macromonomers, is carried out as follows: 1 The analysis was performed using 1 H NMR (Bruker 400 MHz NMR). 30 mg of the macromonomer was dissolved in 0.8 g of deuterated chloroform, and the resulting solution was used as the analytical sample.
[0170] (Weight average molecular weight (Mw) and number average molecular weight (Mn)) The weight-average molecular weight and number-average molecular weight of the vinyl polymer and macromonomer, which are the raw materials for the macromonomer, were analyzed using SEC (HLC-8420GPC). A TOSOH TSKgel SuperHM-L was used as the column, and a polystyrene standard sample was used as the standard. A mixed solvent of chloroform with 1.5% by weight of triethylamine added was used as the eluent. 3 mg of the vinyl polymer or macromonomer to be measured was dissolved in 3 ml of the mixed solvent, and the solution obtained was used as the sample for analysis.
[0171] (Bromine end analysis) After replacing the terminal bromine groups of the vinyl polymer used as the raw material for the macromonomer with potassium acrylate, 1 The amount of H at the base of the substituent was calculated by H NMR. The method for replacing the terminal bromine group is as follows. A large excess of dimethylacetamide and potassium acrylate was added to the vinyl polymer, and the resulting solution was stirred at 50°C for 30 minutes. An excess of ethyl acetate and water was added to the resulting solution, and only the organic layer was collected from the resulting mixture. The organic layer was then concentrated to obtain a vinyl polymer in which the terminal bromine group had been replaced with potassium acrylate. The resulting vinyl polymer was dissolved in deuterated chloroform, and the resulting solution was used as an analytical sample, 1 H NMR measurement was carried out, and as a result, a signal of H at the base of the substituent substituted with potassium acrylate was confirmed in the range of 4.8 to 5.2 ppm, and the amount of terminal bromine of the vinyl polymer was calculated from the integral value of the signal.
[0172] (Tensile test evaluation) A tensile test was conducted in accordance with JIS K 6251:2017 to measure the yield stress, breaking strain, and breaking stress of the polyamide molded body. For the measurement, a test piece was used, which was made by cutting a 0.5 mm press-molded sheet-like molded body into a dumbbell No. 3 shape and curing it overnight or more in a constant temperature and humidity room at 23°C and 50% RH. The tensile speed was 200 mm / min.
[0173] (Dynamic viscoelasticity (tan δ) evaluation) Using a dynamic viscoelasticity measuring device (IT Measurement & Control, DVA-200), measurements were performed in tensile mode, with a strain of 0.05%, and at temperatures from -70 to 400°C, and the dynamic viscoelasticity (tan δ) of the polyamide-based molded body was measured at a vibration frequency of 10 Hz, 35°C, and -35°C. Test pieces used for the measurements were prepared by cutting out 8 mm x 6 mm pieces of a sheet-like molded body press-molded to 0.5 mm, and curing the cut pieces overnight or more in a constant temperature and humidity room at 23°C and 50% RH.
[0174] (surface impact strength) A drop weight test was performed with a load of 300 to 500 g using a 15 mm hemispherical impact core in a DuPont impact tester manufactured by Toyo Seiki Co., Ltd., and the fracture energy (J) was measured. For the measurement, a test piece was used, which was made by curing a sheet-like molded body pressed to 0.5 mm in a constant temperature and humidity room at 23°C and 50% RH for at least one night.
[0175] (Measurement of 1% weight loss temperature) Using a simultaneous thermogravimetry and differential thermal analyzer (STA7200, Hitachi High-Tech Science), measurements were performed at a heating rate of 10°C / min in a nitrogen atmosphere at 0 to 500°C. The 1% weight loss temperature was measured as the temperature at which the weight of the polyamide-based molded article decreased by 1%. For the measurements, test pieces were used, which were prepared by curing a sheet-shaped molded article pressed to 0.5 mm in a constant temperature and humidity chamber at 23°C and 50% RH for at least one night.
[0176] Example 1 [Production Example 1] (Production Example 1-1) 160 g of methanol, 320 g of butyl acrylate, 55.3 g of ethyl 2-bromoisobutyrate, 4.3 g of triethylamine, 0.16 g of cupric bromide, and 0.16 g of tris[2-(dimethylamino)ethyl]amine were added to the flask. Next, nitrogen was bubbled into the flask. Note that "nitrogen bubbling" refers to the flow of nitrogen into a flask or a target such as a solution to remove oxygen from the target. After the nitrogen bubbling, the mixture in the flask was heated and the temperature was raised to 45°C.
[0177] Separately, 49 g of methanol, 0.25 g of ascorbic acid, and 0.29 g of triethylamine were mixed to obtain a methanol solution, which was then bubbled with nitrogen and added dropwise to the flask at a rate of 5.1 ml / h.
[0178] 0.5 hours after the start of the dropping of the methanol solution, 480 g of butyl acrylate bubbled with nitrogen was dropped into the flask over 1.5 hours. 4 hours after the start of the dropping of the methanol solution, it was confirmed by gas chromatography that the conversion rate of butyl acrylate reached 95% or more, and the dropping of the methanol solution was stopped. Then, the reaction solution in the flask was concentrated at 100°C under vacuum for 1 hour. 800 g of butyl acetate, 8 g of Kyoward 500 (manufactured by Kyowa Chemical Industry), 8 g of Kyoward 700 (manufactured by Kyowa Chemical Industry), and 8 g of Radiolite 900 (manufactured by Showa Chemical Industry) were added to the concentrated reaction solution, and the mixture was stirred at 80°C for 1 hour. Next, the obtained reaction solution was filtered. The obtained filtrate was concentrated at 100°C under vacuum for 2 hours to obtain polybutyl acrylate (polymer 1-1) having bromine at one end. It was confirmed by SEC that the number average molecular weight of the obtained polymer 1-1 was 2574 and the molecular weight distribution was 1.30. Furthermore, it was found that polymer 1-1 has an average of 0.86 bromine terminals per molecule. 1 Confirmed by 1 H NMR.
[0179] (Production Example 1-2) 160g of methanol, 309g of butyl acrylate, 83g of ethyl acrylate, 9g of 2-methoxyethyl acrylate, 12g of diethyl 2,5-dibromoadipate, 4.3g of triethylamine, 0.16g of cupric bromide, and 0.16g of tris[2-(dimethylamino)ethyl]amine were added to the flask. Nitrogen was then bubbled through the flask. The mixture in the flask was heated to 45°C.
[0180] Separately, 49 g of methanol, 0.25 g of ascorbic acid, and 0.29 g of triethylamine were mixed to obtain a methanol solution, which was then bubbled with nitrogen and added dropwise to the flask at a rate of 5.1 ml / h.
[0181] 0.5 hours after the start of the dripping of the methanol solution, a mixture of 463 g of butyl acrylate, 124 g of ethyl acrylate, and 13 g of 2-methoxyethyl acrylate, which had been bubbled with nitrogen, was dripped into the flask over 1.5 hours. 4 hours after the start of the dripping of the methanol solution, it was confirmed by gas chromatography that the conversion rates of butyl acrylate, ethyl acrylate, and 2-methoxyethyl acrylate reached 95% or more, respectively, and the dripping of the methanol solution was stopped. Thereafter, the reaction solution in the flask was concentrated at 100°C under vacuum for 1 hour. To the concentrated reaction solution, 1000 g of butyl acetate, 10 g of Kyoward 500 (manufactured by Kyowa Chemical), 10 g of Kyoward 700 (manufactured by Kyowa Chemical), and 10 g of Radiolite 900 (manufactured by Showa Chemical) were added, and the mixture was stirred at 80°C for 1 hour. Next, the resulting reaction solution was filtered. The filtrate was concentrated at 100°C under vacuum for 2 hours to obtain a copolymer of butyl acrylate, ethyl acrylate, and 2-methoxyethyl acrylate having bromine at both ends (polymer 1-2). The number average molecular weight of the obtained polymer 1-2 was 35,316, and the molecular weight distribution was 1.1, as confirmed by SEC. Furthermore, polymer 1-2 was found to have an average of 1.9 bromine ends per molecule. 1 Confirmed by 1 H NMR.
[0182] (Production Example 1-3) 150 g of polymer 1-1 and 150 g of N,N-dimethylacetamide were added to a flask and stirred to make a homogenate. 13.5 g of potassium carbonate and 16.4 g of diaminobenzoic acid were added while stirring. The flask was then heated and stirred at 80°C for 4 hours. After that, 450 g of 1-butanol and 450 g of water were added, stirred at room temperature, and allowed to stand for separation. An extraction operation was performed three times to extract only the organic layer. The organic layer obtained was concentrated at 50°C under vacuum for 1 hour to obtain a macromonomer (macromonomer 1-1) in which the bromine terminal of polymer 1-1 was replaced with a structure derived from diaminobenzoic acid. It was confirmed by SEC that the number average molecular weight of the obtained macromonomer 1-1 was 2628 and the molecular weight distribution was 1.19. Furthermore, it was confirmed that the bromine terminal of macromonomer 1-1 was completely replaced with the ester group of diaminobenzoic acid. 1 Confirmed by 1 H NMR.
[0183] (Production Example 1-4) 10 g of polymer 1-1 and 10 g of N,N-dimethylacetamide were added to a flask and stirred to make it uniform. 1.90 g of tris(2-aminoethyl)amine was added while stirring. The flask was then heated and stirred at 80°C for 1 hour. After that, 30 g of 1-butanol and 30 g of water were added, stirred at room temperature, and allowed to stand for separation. This extraction operation was repeated three times to extract only the organic layer. The organic layer obtained was concentrated at 50°C under vacuum for 1 hour to obtain a macromonomer (macromonomer 1-2) in which the bromine terminals of polymer 1-1 were replaced with a structure derived from tris(2-aminoethyl)amine. It was confirmed by SEC that the number average molecular weight of the obtained macromonomer 1-2 was 3445 and the molecular weight distribution was 1.31. It was further confirmed that the bromine terminals of macromonomer 1-2 were completely removed. 1 Confirmed by 1 H NMR.
[0184] (Examples 1-1 and 1-2) The flask was charged with 12-aminododecanoic acid and adipic acid in the molar amounts shown in Table 1, and 0.09 mol% sodium hypophosphite monohydrate. Nitrogen was passed through the flask for 10 minutes to replace the atmosphere with nitrogen. Next, the flask was heated to 200°C, and macromonomer 1-1 in the molar amount shown in Table 1 was added. The amount of macromonomer 1-1 added in terms of weight was 4% by mass in Example 1-1 and 7% by mass in Example 1-2, based on 100% by mass of the total amount of the monomer group. Furthermore, isophoronediamine in the molar amount shown in Table 1 was added to the flask, and the mixture was heated and stirred at 200°C for 2 hours. Then, the mixture was further heated and stirred at 230°C for 2 hours. An antioxidant (Sumilizer GA-80) was added to the flask in an amount of 0.5% by mass relative to the total amount of the mixture in the flask, and the mixture was heated and stirred at 210°C for 5 minutes to obtain a modified polyamide polymer. The resulting polyamide polymer was vacuum dried at 170°C for 4 hours, and then compressed at 250°C and 5 MPa to a thickness of 0.5 mm to obtain a polyamide molded product. The number average molecular weight and molecular weight distribution of the resulting polymer were confirmed by SEC. The physical properties of the molded product were evaluated by tensile tests, dynamic viscoelasticity measurements, and TG / DTA measurements. The results are shown in Table 1.
[0185] (Examples 1-3) The same procedure as in Example 1-2 was repeated except that Macromonomer 1-2 was used instead of Macromonomer 1-1 to obtain a modified polyamide polymer and a polyamide molded article, and the physical properties were measured and evaluated. The results are shown in Table 1.
[0186] (Comparative Example 1-1) The same procedure as in Example 1-1 was repeated except that macromonomer 1-1 was not used to obtain a polymer and a molded product, and the physical properties were measured and evaluated. The results are shown in Table 1.
[0187] [Table 1]
[0188] From Table 1, it can be seen that the molded bodies made of the modified polyamide-based polymers of Examples 1-1 to 1-3, which are obtained by copolymerizing a macromonomer (macromonomers 1-1 to 1-2), a diamine, and a dicarboxylic acid, have higher breaking strain and dart impact strength, and also higher dynamic viscoelasticity (tan δ) at 35°C and -35°C, compared to the molded body of Comparative Example 1-1, which is made of a polyamide-based polymer not copolymerized with a macromonomer (unmodified). The fact that the modified polyamide polymer has a higher breaking strain and dart impact strength as well as a higher tan δ at 35°C (room temperature) than the unmodified polyamide-based polymer indicates that the flexibility of the modified polyamide polymer is improved. Furthermore, the higher tan δ at -35°C indicates that the low-temperature properties of the modified polyamide polymer are improved. From the above, it was suggested that the modified polyamide-based polymer copolymerized with a macromonomer (i.e., the present terminal-modified vinyl-based polymer) may have improved physical properties such as breaking strain and dart impact strength, and may have improved flexibility and low-temperature properties.
[0189] (Examples 2-1 to 2-3) The flask was charged with 1,12-diaminododecane and adipic acid in the molar amounts shown in Table 2, and 0.09 mol% sodium hypophosphite monohydrate. An antioxidant (Sumilizer GA-80) was then added to the flask so that the amount was 0.5% by mass relative to the total amount of the mixture in the flask. Nitrogen was then passed through the flask for 10 minutes to replace the atmosphere in the flask with nitrogen. Next, the flask was heated to 170°C, and macromonomer 1-1 in the molar amount shown in Table 2 was added. The amount of macromonomer 1-1 added in terms of weight was 1% by mass in Example 2-1, 3% by mass in Example 2-2, and 8% by mass in Example 2-3, relative to the total amount of the monomer group (100% by mass). The mixture in the flask was heated and stirred under reflux of volatile matter for 1 hour at 200°C, 1 hour at 230°C, 30 minutes at 250°C, 10 minutes at 270°C, 50 minutes at 290°C, and 30 minutes at 300°C, in this order, while increasing the temperature. The mixture in the flask after heating and stirring was then heated and stirred for another 30 minutes at 300°C under vacuum conditions to obtain a modified polyamide polymer. The obtained polyamide polymer was compressed to a thickness of 0.5 mm at 270°C and 5 MPa to obtain a polyamide molded product. The number average molecular weight and molecular weight distribution of the obtained polymer were confirmed by SEC. The physical properties of the obtained molded product were also evaluated by tensile testing, dynamic viscoelasticity measurement, and TG / DTA measurement. The results are shown in Table 2.
[0190] (Comparative Example 2-1) The same procedure as in Example 2-1 was repeated except that macromonomer 1-1 was not used to obtain a polymer and a molded product, and the physical properties were measured and evaluated. The results are shown in Table 2.
[0191] [Table 2]
[0192] From Table 2, it can be seen that the molded bodies made of the modified polyamide-based polymers of Examples 2-1 to 1-3, which are copolymerized with a macromonomer (macromonomer 1-1), a diamine, and a dicarboxylic acid, have a higher breaking strain and also a higher dynamic viscoelasticity (tan δ) at 35°C and -35°C, compared to the molded body of Comparative Example 2-1 made of a polyamide-based polymer not copolymerized with a macromonomer (unmodified). The fact that the modified polyamide polymer has a higher breaking strain and a higher tan δ at 35°C (room temperature) than the unmodified polyamide-based polymer indicates that the flexibility of the modified polyamide polymer is improved. Furthermore, the fact that the tan δ at -35°C is higher indicates that the low-temperature properties of the modified polyamide polymer are improved. The above results also suggest that the modified polyamide-based polymer copolymerized with a macromonomer (i.e., the present terminal-modified vinyl-based polymer) can have improved physical properties such as breaking strain, and can have improved flexibility and low-temperature properties. [Industrial Applicability]
[0193] According to one embodiment of the present invention, the physical properties of polyamide can be improved.
Claims
1. A macromonomer which is a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1): Diamine, A dicarboxylic acid, A modified polyamide-based polymer obtained by polymerizing a monomer group including: [Formula 1] In formula (1), R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )—and R 2 and R 3 each independently represents a single bond or a divalent or trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 1 or 2; When n is 2, there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.
2. R 2 and R 3 The modified polyamide polymer according to claim 1 , wherein each of the is independently a divalent or trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl or heteroaryl.
3. R 2 has 1 to 6 carbon atoms, R 3 has 0 to 2 carbon atoms, R 4 and R 5and each of them is hydrogen.
4. The modified polyamide polymer according to claim 1, wherein the terminal structure represented by the general formula (1) has any structure selected from the following formulas (i) to (iii): [Case 2]
5. The macromonomer is a linear polymer, 2. The modified polyamide polymer according to claim 1, wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1).
6. 2. The modified polyamide polymer according to claim 1, wherein the main chain of the macromonomer is mainly composed of poly(meth)acrylate or polyisobutylene.
7. 2. The modified polyamide polymer according to claim 1, wherein the macromonomer has a polystyrene-equivalent number average molecular weight of 500 to 600,000 and a molecular weight distribution of 1.8 or less, as measured by size exclusion chromatography.
8. The modified polyamide polymer according to claim 1 , wherein the monomer group further includes an amino carboxylic acid.
9. A macromonomer which is a terminal-modified vinyl polymer having one or more terminal structures represented by the following general formula (1): Diamine, A dicarboxylic acid, A method for producing a modified polyamide polymer, comprising a step of polymerizing a monomer group comprising: [C3] In formula (1), R 1 -O-, -O(CO)-, -NH-, -N(CH 3 )- or -N(CH 2 CH 3 )—and R 2 and R 3each independently represents a single bond or a divalent or trivalent group having 1 to 8 carbon atoms, which may have a heteroatom; R 4 and R 5 are each independently a hydrogen atom, a methyl group, or an ethyl group; n is 1 or 2; When n is 2, there are two R 3 , R 4 and R 5 may be the same or different; When there are two or more terminal structures represented by general formula (1), the terminal structures may be the same or different.
10. R 2 and R 3 The method according to claim 9, wherein each of the groups is independently a divalent or trivalent alkyl, heteroalkyl, cycloalkyl, heterocycloalkyl, aryl, or heteroaryl.
11. R 2 has 1 to 6 carbon atoms, R 3 has 0 to 2 carbon atoms, R 4 and R 5 and each of are hydrogen.
12. The method according to claim 9, wherein the terminal structure represented by the general formula (1) has any structure selected from the following formulas (i) to (iii): [C4]
13. The macromonomer is a linear polymer, The method according to claim 9 , wherein one or both ends of the linear polymer have a terminal structure represented by the general formula (1).
14. The method according to claim 9 , wherein the main chain of the macromonomer is mainly composed of poly(meth)acrylate or polyisobutylene.
15. 10. The method according to claim 9, wherein the macromonomer has a number average molecular weight in terms of polystyrene of 500 to 600,000 and a molecular weight distribution of 1.8 or less, as measured by size exclusion chromatography.
16. The method of claim 9 , wherein the monomer group further comprises an amino carboxylic acid.
17. A molded article comprising the modified polyamide polymer according to any one of claims 1 to 8.
18. A resin modifier comprising the modified polyamide polymer according to any one of claims 1 to 8.
Citation Information
Patent Citations
Film, resin composition, and production method for polyamide-imide resin
JP2019104939A
Tube, and polyamide resin composition
WO2020175290A1