Thermosetting composition, cured product, thermal conductive sheet, and composite molding
A thermosetting composition combining boron nitride and alumina particles addresses heat and reliability issues in power semiconductor devices by enhancing thermal conductivity and solder reflow resistance, ensuring strong adhesion and minimal void formation.
Patent Information
- Application Number
- JP2024042017
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-20
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-03
AI Technical Summary
Power semiconductor devices face issues with heat generation and reliability due to void formation during solder reflow, which compromises insulation and adhesion between the thermally conductive sheet and the substrate, especially when using thermosetting compounds and inorganic fillers.
A thermosetting composition is developed containing a combination of boron nitride and alumina particles, with specific particle characteristics to enhance thermal conductivity and solder reflow resistance, ensuring strong adhesion and minimal void formation.
The composition achieves high thermal conductivity and solder reflow resistance, enabling the formation of composite molded articles suitable for heat dissipating circuit boards and semiconductor devices with improved reliability and stability.
Smart Images

Figure 2024134539000006 
Figure 2024134539000001 
Figure 2024134539000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting composition having thermosetting properties, a cured product obtained using the thermosetting composition, a thermally conductive sheet, and a composite molded product. [Background technology]
[0002] Among devices that use semiconductors, those that control and convert power from power sources and the like are called "power semiconductor devices." Power semiconductor devices are generally configured as a power module (semiconductor module) in which a power semiconductor device (semiconductor device) that converts and controls electric power and electronic components are mounted on a substrate that functions as a heat sink. In recent years, power semiconductor devices used in various fields such as railways, automobiles, industry, and general home appliances are being shifted from conventional Si power semiconductors to power semiconductors using SiC, AlN, GaN, etc. in order to achieve further miniaturization, cost reduction, and efficiency improvement.
[0003] Various issues have been pointed out for the practical application of such power semiconductor devices, one of which is the issue of heat generation from the devices. While power semiconductor devices can achieve high output and high density by operating at high temperatures, there are concerns that heat generated by device switching and other operations will reduce the reliability of the power semiconductor devices.
[0004] In recent years, heat generation due to the high density of integrated circuits has become a major problem in the electrical and electronic fields, and how to dissipate heat has become an urgent issue. For example, when semiconductor devices used to control the central processing unit of a personal computer or the motor of an electric vehicle operate stably, heat sinks, heat dissipation fins, etc. are indispensable for dissipating heat, and there is a demand for materials that can achieve both thermal conductivity and insulation as materials for connecting semiconductor devices to heat sinks, etc.
[0005] Ceramic substrates with high thermal conductivity, such as alumina substrates and aluminum nitride substrates, have traditionally been used as materials that can provide both thermal conductivity and electrical insulation, but ceramic substrates have issues such as being easily cracked when subjected to impact, and being difficult to make thin and compact. In view of this, a sheet having thermal conductivity has been proposed which uses a thermosetting compound such as an epoxy compound and an inorganic filler.
[0006] Regarding a sheet using a thermosetting compound and an inorganic filler, for example, Patent Document 1 discloses a sealing resin sheet that contains alumina particles and boron nitride in addition to a thermosetting compound and a thermoplastic resin, and has a thermal conductivity of 3 W / m K or more in the thickness direction of the sheet after thermal curing. Patent Document 2 proposes a heat dissipating resin sheet containing an epoxy compound having a Tg of 60° C. or less and boron nitride, in which the boron nitride content is 30 volume % or more and 60 volume % or less.
[0007] Boron nitride (hereinafter referred to as "BN") is an insulating ceramic that has attracted particular attention in recent years in the field of electrical and electronic materials due to its excellent thermal conductivity, solid lubricity, chemical stability, and heat resistance. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2016-204545 A [Patent Document 2] JP 2017-036415 A Summary of the Invention [Problem to be solved by the invention]
[0009] For example, when a power semiconductor device is manufactured using a thermally conductive sheet containing a thermosetting resin such as an epoxy compound and an inorganic filler, electronic components are placed on a substrate (Cu) equipped with the thermally conductive sheet and solder reflow is performed. During solder reflow, the substrate is exposed to high temperatures of 260°C or higher, which may cause peeling between the resin and the inorganic filler, resulting in the formation of voids. These voids may cause a decrease in insulation and peeling between the thermally conductive sheet and the substrate (Cu).
[0010] An object of the present invention is to provide a thermosetting composition that can achieve both high thermal conductivity and high solder reflow resistance, as well as a cured product, a thermally conductive sheet, and a composite molded body made using the thermosetting composition. [Means for solving the problem]
[0011] The present inventors have found that the above-mentioned problems can be solved by configuring a thermosetting composition containing an inorganic filler and a thermosetting compound by combining the inorganic filler with a specified boron nitride particle and a specified alumina particle. That is, the present invention proposes a thermosetting composition, a cured product, a thermally conductive sheet, and a composite molded product having the following configurations.
[0012] [1] A first aspect of the present invention is a thermosetting composition comprising an inorganic filler and a thermosetting compound, The content of the inorganic filler is 60% by mass or more relative to 100% by mass of the solid content in the thermosetting composition, the inorganic filler is composed of two or more kinds of fillers, at least one of the inorganic fillers is boron nitride particles, and the boron nitride particles are agglomerated particles; At least one other type is alumina particles; The alumina particles have an areal circularity of 0.95 or less as measured by an image particle size distribution measuring device, and the proportion of the alumina particles is 50% by number or more and 70% by number or less with respect to 100% by number of all the alumina particles; The thermosetting composition has a ratio of all alumina particles to all inorganic fillers of 35 mass % or more.
[0013] [2] A second aspect of the present invention is the thermosetting composition according to the first aspect, wherein the alumina particles have an average particle size of 0.5 μm or more and 30 μm or less. [3] A third aspect of the present invention is the thermosetting composition according to the first or second aspect, wherein the alumina particles have an area circularity of 0.90 or less, as measured by an image particle size distribution analyzer, and the proportion of the alumina particles is 20% by number or more and 40% by number or less, relative to 100% by number of the total alumina particles. [4] A fourth aspect of the present invention is a thermosetting composition according to any one of the first to third aspects, wherein the alumina particles have an aspect ratio of less than 0.85, as measured by an image particle size distribution analyzer, of 50% by number or more and 80% by number or less, relative to 100% by number of the total alumina particles.
[0014] [5] A fifth aspect of the present invention is a thermosetting composition according to any one of the first to fourth aspects, wherein the alumina particles have an aspect ratio of less than 0.7, as measured by an image particle size distribution analyzer, of 15% by number or more and 40% by number or less, relative to 100% by number of the total alumina particles. [6] A sixth aspect of the present invention is a thermosetting composition according to any one of the first to fifth aspects, wherein the alumina particles have a circumferential length envelope ratio of more than 0.970 and less than 0.985, as measured by an image particle size distribution analyzer, and the ratio of the alumina particles is from 5 to 40% by number, relative to 100% by number of the total alumina particles. [7] A seventh aspect of the present invention is a thermosetting composition according to any one of the first to sixth aspects, wherein the alumina particles have an area envelope index of less than 0.950 as measured by an image particle size distribution analyzer, and the proportion of the alumina particles having an area envelope index of less than 0.950 as measured by an image particle size distribution analyzer is 5% by number or more and 40% by number or less, relative to 100% by number of the total alumina particles.
[0015] [8] An eighth aspect of the present invention is a thermosetting composition according to any one of the first to seventh aspects, comprising a polymer having a mass average molecular weight of 10,000 or more. [9] A ninth aspect of the present invention is the thermosetting composition of the eighth aspect, comprising 10% by mass or more and less than 30% by mass of a polymer with a mass average molecular weight of 10,000 or more, relative to 100% by mass of solids in the thermosetting composition excluding inorganic fillers.
[0016]
[10] A tenth aspect of the present invention is a thermosetting composition according to any one of the first to ninth aspects, comprising, as the thermosetting compound, a multifunctional epoxy compound having three or more epoxy groups per molecule and a molecular weight of 650 or less.
[11] An eleventh aspect of the present invention is the thermosetting composition according to the tenth aspect, wherein the polyfunctional epoxy compound is an epoxy compound having four or more glycidyl groups in one molecule.
[0017]
[12] A twelfth aspect of the present invention is a cured product using the thermosetting composition according to any one of the first to eleventh aspects.
[13] A thirteenth aspect of the present invention is a thermally conductive sheet comprising the cured product according to the twelfth aspect.
[14] A fourteenth aspect of the present invention is a composite molded article having a cured product of the thermosetting composition according to any one of the first to eleventh aspects and a metal part. Effect of the Invention
[0018] The thermosetting composition proposed by the present invention contains a combination of specified boron nitride particles and specified alumina particles as an inorganic filler, and when made into a sheet-like cured product, the contact area between the inorganic fillers is increased, thereby increasing the bonding strength, and as a result, it is possible to achieve both high thermal conductivity and high solder reflow resistance. Therefore, by forming a composite molded body using a thermally conductive sheet and a cured product obtained by curing the thermosetting composition proposed by the present invention, it is possible to suitably form, for example, a heat dissipating circuit board, a semiconductor device, a power module, etc. [Brief description of the drawings]
[0019] [Figure 1]FIG. 2 is a schematic diagram of a particle cross-section according to an example of an agglomerated boron nitride particle having a house-of-card structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] An embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and various modifications can be made within the scope of the present invention.
[0021] <<The composition>> A composition according to an embodiment of the present invention (hereinafter referred to as "the composition") is a thermosetting composition containing a thermosetting compound and an inorganic filler.
[0022] In the present invention, the term "thermosetting composition" refers to a composition containing a compound or resin having the property of being cured by heat. That is, it is sufficient if the composition has a curing property that allows room for curing by heat, and may be one that has already been cured to a state where room for curing remains (also referred to as "temporarily cured"), or one that has not yet been cured at all (referred to as "uncured"). The present composition may be in any form, such as a powder, a slurry, a liquid, a solid, or a molded product such as a sheet.
[0023] The present composition can be cured by heating (also referred to as "cured product"). In addition, the present composition can be formed into a sheet-like thermosetting composition (also referred to as a "thermosetting sheet") by forming it into a sheet, and a sheet having thermal conductivity (referred to as the present thermally conductive sheet) can be formed by curing the thermosetting sheet. In other words, the present thermally conductive sheet is a cured product of the thermosetting sheet.
[0024] <Thermosetting compounds> Examples of the thermosetting compound contained in the present composition include epoxy compounds, phenolic resins, polycarbonate resins, unsaturated polyester resins, urethane resins, melamine resins, urea resins, and benzoxazine compounds.
[0025] The content of resin components including thermosetting compounds, for example components including thermosetting compounds (including high molecular weight epoxy resins), curing agents and curing accelerators, is preferably 5% by mass or more and 40% by mass or less relative to 100% by mass of the volatile components in the composition, i.e., components excluding solvents and solvents (referred to as the "solids content"). If the content of the resin component is 5% by mass or more, it is preferable because the moldability is good, while if it is 40% by mass or less, it is preferable because the content of other components can be secured and thermal conductivity can be increased. From this viewpoint, the content of the resin component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, relative to 100% by mass of the solid content in the composition, while it is more preferably 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less.
[0026] (Epoxy compounds) The composition preferably contains an epoxy compound as the thermosetting compound.
[0027] Of the thermosetting compounds contained in the present composition, it is preferable that the epoxy compounds account for 30 mass% or more and 100 mass% or less, and even more preferably 40 mass% or more of these, more preferably 50 mass% or more of these, more preferably 60 mass% or more of these, and even more preferably 70 mass% or more of these. The epoxy compound in this case also includes high molecular weight epoxy resins, which will be described later.
[0028] The epoxy compound as the thermosetting compound contained in the present composition may be any compound having one or more oxirane rings (epoxy groups) in one molecule.
[0029] The oxirane ring (epoxy group) contained in the epoxy compound may be either an alicyclic epoxy group or a glycidyl group, and is more preferably a glycidyl group from the viewpoint of reaction rate or heat resistance.
[0030] Examples of the epoxy compound include an epoxy group-containing silicon compound, an aliphatic epoxy compound, a bisphenol A or F type epoxy compound, a novolac type epoxy compound, an aromatic epoxy compound, an alicyclic epoxy compound, a glycidyl ester type epoxy compound, a polyfunctional epoxy compound, and a polymer type epoxy compound.
[0031] The epoxy compound may be an aromatic oxirane ring (epoxy group)-containing compound.Specific examples thereof include bisphenol-type epoxy compounds obtained by glycidylating bisphenols such as bisphenol A, bisphenol F, bisphenol AD, bisphenol S, tetramethyl bisphenol A, tetramethyl bisphenol F, tetramethyl bisphenol AD, tetramethyl bisphenol S, and tetrafluorobisphenol A, biphenyl-type epoxy compounds, epoxy compounds obtained by glycidylating divalent phenols such as dihydroxynaphthalene and 9,9-bis(4-hydroxyphenyl)fluorene, epoxy compounds obtained by glycidylating trisphenols such as 1,1,1-tris(4-hydroxyphenyl)methane, epoxy compounds obtained by glycidylating tetrakisphenols such as 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane, and novolac-type epoxy compounds obtained by glycidylating novolacs such as phenol novolac, cresol novolac, bisphenol A novolac, and brominated bisphenol A novolac.
[0032] [Multifunctional epoxy compounds] The present composition preferably contains a polyfunctional epoxy compound, which will be described next.
[0033] A polyfunctional epoxy compound refers to an epoxy compound that has two or more oxirane rings (epoxy groups) in one molecule and has a mass average molecular weight of less than 10,000. By including such a polyfunctional epoxy compound, it is possible to introduce highly polar oxirane rings (epoxy groups) at a high density, which increases the effects of physical interactions such as van der Waals forces and hydrogen bonds, and for example, improves the adhesion between the thermally conductive sheet formed from the composition and a conductor. In addition, by including a polyfunctional epoxy compound, it is possible to increase the storage modulus of the thermally conductive sheet, which then exerts a strong anchor effect after the cured product of the composition penetrates into the unevenness of the conductor surface, which is the adherend, and improves the adhesion between the thermally conductive sheet and the conductor. On the other hand, the inclusion of a polyfunctional epoxy compound tends to increase the hygroscopicity of the composition, but by improving the reactivity of the oxirane ring (epoxy group), the amount of hydroxyl groups during the reaction can be reduced, thereby suppressing the increase in hygroscopicity. Furthermore, by producing the present composition by combining the above-mentioned high molecular weight epoxy resin and polyfunctional epoxy compound, it is possible to achieve both high elasticity and low moisture absorption in the present thermally conductive sheet.
[0034] The polyfunctional epoxy compound may be an epoxy compound having two or more oxirane rings (epoxy groups) in one molecule, from the viewpoint of increasing the storage modulus of the cured product after thermal curing, particularly at high temperatures, which is important when the heat generation is large, such as in power semiconductors. Among them, an epoxy compound having three or more oxirane rings (epoxy groups) in one molecule is preferable, and an epoxy compound having four or more glycidyl groups in one molecule is even more preferable. By having a plurality of oxirane rings (epoxy groups), particularly glycidyl groups, in one molecule, the crosslink density of the cured product is improved, and the obtained cured product, the present thermal conductive sheet, has a higher strength. As a result, when internal stress occurs in the present thermal conductive sheet during a moisture absorption reflow test, the present thermal conductive sheet does not deform or break, but maintains its shape, thereby suppressing the occurrence of voids and other voids in the present thermal conductive sheet.
[0035] From the viewpoint of increasing the storage modulus of the heat dissipation sheet after thermal curing, the molecular weight of the polyfunctional epoxy compound is preferably 650 or less, particularly 100 or more or 630 or less, and more preferably 200 or more or 600 or less. To improve the handling properties of the sheet, it is preferable to include one that is liquid at 25° C. From the viewpoint of achieving lower moisture absorption and higher crosslinking, it is preferable not to include an amine-based or amide-based structure that contains a nitrogen atom.
[0036] Specific examples of polyfunctional epoxy compounds include polyfunctional epoxy compounds having three or more epoxy groups per molecule and a molecular weight of 650 or less. That is, it is preferable to include a polyfunctional epoxy compound having three or more epoxy groups per molecule and a molecular weight of 650 or less as the thermosetting compound. For example, EX321L, DLC301, DLC402, etc. manufactured by Nagase ChemteX Corporation can be used. These polyfunctional epoxy compounds may be used alone or in combination of two or more kinds.
[0037] The content of the polyfunctional epoxy compound is preferably 5% by mass or more and 80% by mass or less, based on 100% by mass of the solid content of the composition excluding the inorganic filler. If the content of the polyfunctional epoxy compound is 5% by mass or more, it is preferable because the elastic modulus of the cured product of the thermosetting composition can be maintained, and if it is 80% by mass or less, it is preferable because the water absorption rate does not become too high. In particular, for a multifunctional epoxy having three or more epoxy groups per molecule and a molecular weight of 650 or less, the content is preferably 5% by mass or more and 75% by mass or less, relative to 100% by mass of the solid content in the composition excluding the inorganic filler, and more preferably 10% by mass or more or 70% by mass or less, and even more preferably 15% by mass or more or 50% by mass or less.
[0038] As described later, when a high molecular weight epoxy resin and a polyfunctional epoxy compound are used in combination, from the viewpoints of the film-forming properties of the sheet and the elastic modulus of the cured sheet, the content of the polyfunctional epoxy compound is preferably 20% by mass or more and 500% by mass or less, more preferably 30% by mass or more or 400% by mass or less, and even more preferably 40% by mass or more or 350% by mass or less, relative to 100% by mass of the high molecular weight epoxy resin.
[0039] <Inorganic filler> The inorganic filler contained in the present composition is composed of two or more types of fillers, at least one of which is boron nitride particles and at least another of which is alumina particles.
[0040] (Boron nitride particles) Since the present composition contains boron nitride particles as an inorganic filler, when cured, it is possible to provide a present cured product and a present thermally conductive sheet having excellent thermal conductivity.
[0041] The boron nitride particles are preferably agglomerated particles (also referred to as "agglomerated boron nitride particles"). In the present invention, the "aggregated particles" refer to aggregates of boron nitride primary particles, preferably aggregates of scaly boron nitride primary particles. By including the aggregated boron nitride particles in the composition, the thermal conductivity of the cured product and the thermal conductive sheet can be further increased. In particular, for example, the thermal conductivity of the thermal conductive sheet in the sheet thickness direction can be further increased. Furthermore, by combining the aggregated boron nitride particles with a specific alumina particle described later, the contact area between the inorganic fillers can be further increased, the bonding strength can be increased, and the thermal conductivity can be further increased. In addition, the generation of voids during reflow treatment can be suppressed, and the peeling between the thermal conductive sheet and the substrate (copper) can be prevented.
[0042] The aggregated structure of the aggregated boron nitride particles is preferably a house of card structure from the viewpoint of improving thermal conductivity. Therefore, the boron nitride particles preferably include aggregated boron nitride particles having a house of card structure. However, the aggregated structure of the boron nitride particles may be a structure other than the house of card structure. The aggregate structure of the aggregated boron nitride particles can be confirmed by a scanning electron microscope (SEM).
[0043] The house of cards structure is a structure in which plate-shaped particles are stacked in a complex manner without being oriented, as described in "Ceramics 43 No. 2" (published by the Ceramic Society of Japan in 2008). More specifically, it is a structure in which the flat surface of the primary particles that form the aggregate particle is in contact with the end surface of other primary particles that exist within the aggregate particle. A schematic diagram of the house of cards structure is shown in Figure 1. The card-house structured aggregated particles have a very high breaking strength due to their structure, and do not break even during the pressurizing process performed during sheet molding of the thermal conductive sheet. Therefore, the primary particles that are usually oriented in the longitudinal direction of the thermal conductive sheet can be made to exist in a random direction. Therefore, by using the card-house structured aggregated particles, the proportion of the primary particles that have the ab plane oriented in the thickness direction of the thermal conductive sheet can be increased, so that heat can be effectively conducted in the thickness direction of the sheet, and the thermal conductivity in the thickness direction can be further increased.
[0044] In addition, agglomerated boron nitride particles having a house-of-cards structure can be produced, for example, by the method described in WO 2015 / 119198.
[0045] The agglomerated boron nitride particles having a house-of-card structure may be surface-treated with a surface treatment agent. As the surface treatment agent, for example, a known surface treatment agent such as a silane coupling treatment can be used. In general, direct affinity or adhesion is not observed between inorganic filler and thermosetting compound in many cases, and this is also the case when boron nitride particles having a card house structure are used as inorganic filler. It is considered that the thermal conductivity attenuation at the interface can be further reduced by increasing the adhesion at the interface between inorganic filler and matrix resin such as thermosetting compound by chemical treatment.
[0046] The shape of the agglomerated boron nitride particles is preferably spherical, as shown in FIG. 1, from the viewpoint of increasing the filling rate of the agglomerated boron nitride particles in the thermosetting composition.
[0047] Regarding the particle size of the agglomerated boron nitride particles, by increasing the particle size of the inorganic filler, the heat transfer paths between the inorganic fillers via the thermosetting compound with low thermal conductivity can be reduced, and therefore the increase in thermal resistance in the heat transfer paths in the thickness direction can be reduced. From the above viewpoint, the lower limit of the maximum particle size of the aggregated boron nitride particles is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 40 μm or more, while the upper limit of the maximum particle size is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and even more preferably 90 μm or less.
[0048] The average particle size of the aggregated boron nitride particles is not particularly limited. Among them, 5 μm or more is preferable, 10 μm or more is more preferable, and particularly 15 μm or more is even more preferable. Also, 100 μm or less is preferable, and 90 μm or less is more preferable. When the average particle size of the aggregated boron nitride particles is 5 μm or more, the number of particles in the thermosetting composition and the cured product using the thermosetting composition is relatively small, and the number of interparticle interfaces is reduced, so that the thermal resistance is reduced, and the thermal conductive sheet may have a high thermal conductivity. Also, when the average particle size is 100 μm or less, the surface smoothness of the thermal conductive sheet tends to be obtained.
[0049] By having the average particle size or maximum particle size of the agglomerated boron nitride particles be equal to or less than the above upper limit, when the agglomerated boron nitride particles are contained in a thermosetting compound, i.e., a matrix resin, a high-quality film without surface roughness can be formed. By having the average particle size or maximum particle size be equal to or more than the above lower limit, the interface between the matrix resin and the agglomerated boron nitride particles is reduced, resulting in a smaller thermal resistance and a higher thermal conductivity, while providing a sufficient thermal conductivity improvement effect as an inorganic filler required for power semiconductor devices.
[0050] It is also considered that the effect of the thermal resistance at the interface between the matrix resin and the agglomerated boron nitride particles on the thickness of the thermal conductive sheet becomes significant when the size of the agglomerated boron nitride particles is 1 / 10 or less of the thickness of the thermal conductive sheet. In particular, in the case of power semiconductor devices, the thermal conductive sheet has a thickness of 100 μm to 300 μm, and therefore, from the viewpoint of thermal conductivity, it is preferable that the maximum particle size of the agglomerated boron nitride particles is larger than the above lower limit. Furthermore, by having the maximum particle size of the agglomerated boron nitride particles be equal to or greater than the above lower limit, not only is the increase in thermal resistance caused by the interface between the agglomerated boron nitride particles and the matrix resin suppressed, but the number of required thermal conduction paths between particles is reduced, increasing the probability that they will connect from one side to the other in the thickness direction of the thermally conductive sheet. On the other hand, by having the maximum particle size of the agglomerated boron nitride particles be equal to or less than the above upper limit, the agglomerated boron nitride particles are prevented from protruding onto the surface of the thermal conductive sheet, and a good surface shape without surface roughness is obtained. Therefore, when the sheet is produced by bonding it to a copper substrate, sufficient adhesion is obtained and excellent voltage resistance characteristics can be obtained.
[0051] The ratio of the size (maximum particle diameter) of the agglomerated boron nitride particles to the thickness of the thermally conductive sheet (maximum particle diameter / thickness) is preferably 0.2 or more and 1.0 or less, more preferably 0.3 or more and 0.95 or less, and even more preferably 0.3 or more and 0.9 or less.
[0052] The maximum particle size and average particle size of the agglomerated boron nitride particles can be measured, for example, by the following method. The maximum particle size and average particle size of the agglomerated boron nitride particles used as a raw material can be determined as the maximum particle size Dmax and average particle size D50 of the agglomerated boron nitride particles from the particle size distribution obtained by measuring the particle size distribution of a sample in which agglomerated boron nitride particles are dispersed in a solvent, specifically, a sample in which agglomerated boron nitride particles are dispersed in a pure water medium containing a dispersion stabilizer, using a laser diffraction / scattering particle size distribution measuring device. Here, Dmax and D50 are the maximum particle size and the cumulative volume 50% particle size in a volume-based particle size distribution obtained by measurement using a laser diffraction / scattering particle size distribution measurement method. The maximum particle size and the average particle size can also be determined using a dry particle size distribution measuring device such as Morphologi 4 (manufactured by Malvern Instruments).
[0053] On the other hand, the maximum particle size and average particle size of the agglomerated boron nitride particles in this composition or this thermally conductive sheet can also be measured in the same manner as above by dissolving and removing organic components such as thermosetting compounds in a solvent (including a heated solvent), or by swelling the organic components to reduce the adhesive strength with the agglomerated boron nitride particles and then physically removing them, and further by heating the organic components in air to incinerate them and remove them. Regarding the maximum particle size and average particle size of the agglomerated boron nitride particles in the composition or the thermally conductive sheet, it is also possible to directly observe any 10 or more agglomerated boron nitride particles on a cross section of the composition or the thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a Raman microspectrometer, an atomic force microscope or the like, and measure the particle size of the particles to determine the maximum particle size and average particle size. In this case, if the particles are non-spherical, the longest and shortest diameters are measured, and the average value thereof is regarded as the particle diameter of the particle.
[0054] (Alumina particles) The alumina particles contained in the present composition preferably have an areal circularity of 0.95 or less as measured by an image particle size distribution analyzer, and the proportion of these alumina particles is preferably 50% by number to 70% by number of all the alumina particles. If the ratio of alumina particles having an areal circularity of 0.95 or less as measured by an image particle size distribution analyzer is 50% or more by number of all alumina particles, the contact area between the fillers is increased, which is preferable since the contact thermal resistance is reduced. On the other hand, if the ratio is 70% or less by number, the packing rate of the alumina particles is improved, which is preferable since voids are less likely to occur. From this viewpoint, the proportion of alumina particles having an areal circularity of 0.95 or less as measured by an image particle size distribution analyzer is preferably 50% by number or more of the total alumina particles, more preferably 55% by number or more, and even more preferably 60% by number or more, and on the other hand, is preferably 70% by number or less, more preferably 68% by number or less, and even more preferably 65% by number or less.
[0055] The alumina particles contained in the present composition preferably have an areal circularity of 0.90 or less as measured by an image particle size distribution analyzer, and the proportion of these particles is preferably 20% to 40% by number of all the alumina particles. If the ratio of alumina particles having an areal circularity of 0.90 or less as measured by an image particle size distribution analyzer is 20% or more by number of the total alumina particles, the contact area between the fillers becomes large, which is preferable since the contact thermal resistance decreases. On the other hand, if the ratio is 40% or less by number, the packing rate of the alumina particles becomes good, which is preferable since voids are less likely to occur. From this viewpoint, the proportion of alumina particles having an areal circularity of 0.90 or less as measured by an image particle size distribution analyzer is preferably 20% by number or more of the total alumina particles, more preferably 25% by number or more, and even more preferably 27% by number or more, while it is preferably 40% by number or less, more preferably 39% by number or less, and even more preferably 38% by number or less.
[0056] The areal circularity of the alumina particles can be measured by the following method. The areal circularity of the alumina particles used as the raw material can be calculated by measuring the circular area and actual particle perimeter using an image-based particle size distribution analyzer (e.g., Morphologi 4 manufactured by Malvern Panalytical), and using the formula: circular area / square of actual particle perimeter. The areal circularity of the alumina particles in this composition or this thermally conductive sheet can be calculated by removing the organic components of this composition or this thermally conductive sheet at high temperature, separating the alumina from the remaining inorganic components by centrifugation utilizing the difference in specific gravity, measuring the circular area and actual particle perimeter of the separated alumina particles using an image particle size distribution measuring device, and then using the formula: circular area / actual particle perimeter squared. It is also possible to directly observe a cross section of the composition or the thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a Raman microspectrometer, an atomic force microscope, or the like, and measure the circular area and actual particle perimeter of any 10 or more alumina particles, and then calculate the circular area / actual particle perimeter squared.
[0057] The ratio (number %) of alumina particles having a predetermined circularity of area to all alumina particles can be calculated by excluding particle images with a perimeter envelope of less than 0.97 from the obtained data, taking the number of particles with a perimeter envelope of 0.97 or more as the total number of alumina particles, and calculating the number of alumina particles having a predetermined circularity of area / total number of alumina particles. Here, images of particles with a perimeter envelope of less than 0.97 are excluded because they can be determined as agglomerated particles. The number of alumina particles measured at this time is preferably 1000 or more, more preferably 3000 or more, even more preferably 5000 or more, and even more preferably 10000 or more.
[0058] The alumina particles contained in the present composition preferably have an average aspect ratio of 0.60 or more and 0.82 or less. If the average aspect ratio of the alumina particles is 0.82 or less, the contact area between the fillers is increased, suppressing the contact thermal resistance, while if it is 0.60 or more, the filling rate can be increased, suppressing the generation of voids. From this viewpoint, the average aspect ratio of the alumina particles contained in the present composition is preferably 0.82 or less, more preferably 0.81 or less, and even more preferably 0.80 or less, while it is preferably 0.60 or more, more preferably 0.65 or more, and even more preferably 0.70 or more.
[0059] The aspect ratio of the alumina particles can be measured by the following method. The aspect ratio of the alumina particles used as the raw material can be calculated by measuring the short diameter (maximum perpendicular length to the maximum length) and maximum length using an image particle size distribution analyzer (e.g., Morphologi 4 manufactured by Malvern Panalytical) and using the formula aspect ratio = short diameter / maximum length. The aspect ratio of the alumina particles in this composition or this thermally conductive sheet can be determined by removing the organic components of this composition or this thermally conductive sheet at high temperature, separating the alumina from the remaining inorganic components by centrifugation utilizing the difference in specific gravity, and measuring the short diameter (maximum perpendicular length relative to the maximum length) and maximum length of the separated alumina particles using an image particle size distribution measuring device, using the formula aspect ratio = short diameter / maximum length. It is also possible to directly observe the cross section of this composition or this thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a Raman microscope, an atomic force microscope, or the like, for any 10 or more alumina particles, measure the short diameter (maximum perpendicular length relative to the maximum length) and maximum length, and calculate the aspect ratio using the formula: short diameter / maximum length.
[0060] The alumina particles contained in the present composition preferably have an aspect ratio of less than 0.85 in a proportion of 50% by number to 80% by number of all the alumina particles. It is preferable that the proportion of alumina particles having an aspect ratio of less than 0.85 is 50% or more of the total alumina particles, since the contact area between the fillers is increased and the contact thermal resistance can be suppressed.On the other hand, it is preferable that the proportion is 80% or less, since the filling rate can be increased and the generation of voids can be suppressed. From this viewpoint, the proportion of alumina particles having an aspect ratio smaller than 0.85 is preferably 50% by number or more of the total alumina particles, more preferably 60% by number or more, and even more preferably 65% by number or more. On the other hand, in order to increase the filling rate and suppress the generation of voids, it is preferably 80% by number or less, more preferably 75% by number or less, and even more preferably 70% by number or less.
[0061] The alumina particles contained in the present composition preferably have an aspect ratio of less than 0.7 in a proportion of 15% by number to 40% by number of all the alumina particles. It is preferable that the ratio of alumina particles having an aspect ratio of less than 0.7 is 15% by number or more of the total alumina particles, since the contact area between the fillers is increased and the contact thermal resistance can be suppressed.On the other hand, it is preferable that the ratio is 40% by number or less, since the filling rate can be increased and the generation of voids can be suppressed. From this viewpoint, the proportion of alumina particles having an aspect ratio smaller than 0.7 is preferably 15% by number or more of the total alumina particles, more preferably 20% by number or more, and even more preferably 25% by number or more, while it is preferably 40% by number or less, more preferably 35% by number or less, and even more preferably 31% by number or less.
[0062] The ratio (number %) of alumina particles having a given aspect ratio to all alumina particles can be calculated by excluding particle images with a perimeter envelope of less than 0.97 from the obtained data, taking the total number of alumina particles as the number of alumina particles with a perimeter envelope of 0.97 or more, and calculating the number of alumina particles with a given aspect ratio / total number of alumina particles. Here, images of particles with a perimeter envelope of less than 0.97 are excluded because they can be determined as agglomerated particles. The number of alumina particles measured at this time is preferably 1000 or more, more preferably 3000 or more, even more preferably 5000 or more, and even more preferably 10000 or more.
[0063] The alumina particles contained in the present composition preferably have a perimeter-envelope ratio of greater than 0.970 and smaller than 0.985, the proportion of which is 5% by number or more and 40% by number or less of all the alumina particles. If the ratio of alumina particles having a circumferential envelope ratio of more than 0.970 and less than 0.985 is 5% or more by number of the total alumina particles, the contact area between the fillers becomes large and the contact thermal resistance can be suppressed, which is preferable. On the other hand, if the ratio is 40% or less by number, the filling rate can be increased and the occurrence of voids can be suppressed, which is preferable. From this viewpoint, the proportion of alumina particles having a perimeter envelope ratio of more than 0.970 and less than 0.985 is preferably 5% by number or more of the total alumina particles, more preferably 7% by number or more, more preferably 10% by number or more, and even more preferably 13% by number or more. On the other hand, it is preferably 40% by number or less, more preferably 30% by number or less, and even more preferably 25% by number or less.
[0064] The "perimeter envelope" of an alumina particle is the ratio of the particle perimeter measured by end face contact to the actual perimeter (particle perimeter (end face contact) / actual particle perimeter). The perimeter envelope of the alumina particles used as the raw material can be calculated by measuring the particle perimeter by end contact and the actual perimeter using an image-based particle size distribution analyzer (e.g., Morphologi 4 manufactured by Malvern Panalytical) and using the formula perimeter envelope = particle perimeter (end contact) / actual particle perimeter. On the other hand, the perimeter envelope of the alumina particles in this composition or this thermally conductive sheet can be obtained by removing the organic components of this composition or this thermally conductive sheet at high temperature, separating the alumina from the remaining inorganic components by centrifugation utilizing the difference in specific gravity, and measuring the particle perimeter and actual perimeter of the separated alumina particles by end face contact using an image particle size distribution measuring device, and then calculating the perimeter envelope using the formula: perimeter envelope = particle perimeter (end face contact) / actual particle perimeter. It is also possible to directly observe the cross section of this composition or this thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a Raman microscope, an atomic force microscope, or the like for any 10 or more alumina particles, measure the particle perimeter by end face contact and the actual perimeter, and calculate the perimeter envelope using the formula perimeter envelope = particle perimeter (end face contact) / actual particle perimeter.
[0065] The ratio (number %) of alumina particles having a predetermined perimeter envelope to all alumina particles can be calculated by excluding particle images with a perimeter envelope of less than 0.97 from the obtained data, taking the number of particles with a perimeter envelope of 0.97 or more as the total number of alumina particles, and calculating the number of alumina particles having a predetermined perimeter envelope / total number of alumina particles. Here, images of particles with a perimeter envelope of less than 0.97 are excluded because they can be determined as agglomerated particles. The number of alumina particles measured at this time is preferably 1000 or more, more preferably 3000 or more, even more preferably 5000 or more, and even more preferably 10000 or more.
[0066] The alumina particles contained in the present composition preferably have an area envelopment ratio of less than 0.950 in a proportion of 5% by number to 40% by number of all the alumina particles. If the alumina particles having an area envelopment ratio of less than 0.950 account for 5% or more of the total alumina particles, the contact area between the fillers becomes large and the contact thermal resistance can be suppressed, which is preferable, whereas if the alumina particles have an area envelopment ratio of less than 40% by number, the filling rate can be increased and the generation of voids can be suppressed, which is preferable. From this viewpoint, the proportion of alumina particles having an area envelopment ratio smaller than 0.950 is preferably 5% by number or more of the total alumina particles, more preferably 7% by number or more, more preferably 9% by number or more, and even more preferably 11% by number or more. On the other hand, it is preferably 40% by number or less, more preferably 35% by number or less, and even more preferably 30% by number or less.
[0067] The "area envelope" of an alumina particle is the ratio of the actual particle area to the envelope area at end contact measured using an image particle size distribution analyzer (e.g., Morphologi 4 manufactured by Malvern Panalytical). The areal envelope of the alumina particles used as the raw material can be calculated by measuring the actual particle area and the particle area (end contact) using an image-based particle size distribution analyzer (e.g., Morphologi 4 manufactured by Malvern Panalytical), and using the formula: areal envelope = actual particle area / particle area (end contact). The areal envelope of the alumina particles in this composition or this thermally conductive sheet can be determined by removing the organic components of this composition or this thermally conductive sheet at high temperature, separating the alumina from the remaining inorganic components by centrifugation utilizing the difference in specific gravity, and measuring the actual particle area and particle area (end surface contact) of the separated alumina particles using an image particle size distribution measuring device, and then calculating the areal envelope using the formula: actual particle area / particle area (end surface contact). It is also possible to directly observe a cross section of this composition or this thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a micro-Raman spectrometer, an atomic force microscope, or the like, and measure the area envelope of any 10 or more alumina particles.
[0068] The ratio (number %) of alumina particles having a predetermined areal envelope to all alumina particles can be calculated by excluding particle images with a perimeter envelope of less than 0.97 from the obtained data, taking the number of particles with a perimeter envelope of 0.97 or more as the total number of alumina particles, and calculating the number of alumina particles having a predetermined areal envelope / total number of alumina particles. Here, images of particles with a perimeter envelope of less than 0.97 are excluded because they can be determined as agglomerated particles. The number of alumina particles measured at this time is preferably 1000 or more, more preferably 3000 or more, even more preferably 5000 or more, and even more preferably 10000 or more.
[0069] The alumina particles contained in the present composition preferably have an average particle size of 0.5 μm or more and 30 μm or less. If the average particle size of the alumina particles is 0.5 μm or more, the number of contacts between the inorganic fillers can be increased, the contact thermal resistance can be reduced, and the thermal conductivity can be increased. On the other hand, if the average particle size of the alumina particles is 30 μm or less, the filling rate can be increased and the generation of voids can be suppressed. From this viewpoint, the average particle size of the alumina particles is preferably 0.5 μm or more, more preferably 0.8 μm or more, and even more preferably 1.0 μm or more, and is preferably 30 μm or less, more preferably 28 μm or less, and even more preferably 25 μm or less.
[0070] The average particle size of the alumina particles can be measured, for example, by the following method. The average particle diameter of the alumina particles used as the raw material can be determined as the average particle diameter D50 of the alumina particles from the particle size distribution obtained by measuring the particle size distribution of a sample in which alumina particles are dispersed in a solvent, specifically, a sample in which alumina particles are dispersed in a pure water medium containing a dispersion stabilizer, using a laser diffraction / scattering type particle size distribution analyzer. Here, D50 is the cumulative volume 50% particle diameter in the volume-based particle size distribution obtained by measurement using a laser diffraction scattering particle size distribution measurement method. The average particle size can also be determined using a dry particle size distribution measuring device such as Morphologi 4 (manufactured by Malvern Instruments). The average particle diameter D50 of the alumina particles in this composition or this thermally conductive sheet can also be measured in a similar manner to that described above by dissolving and removing organic components such as thermosetting compounds in a solvent (including a heated solvent), or by swelling the organic components to reduce the adhesive strength with the alumina particles and then physically removing them, and then heating the organic components in air to incinerate them and remove them. The average particle size of the alumina particles in the composition or the thermally conductive sheet can also be determined by directly observing 10 or more arbitrary alumina particles on a cross section of the composition or the thermally conductive sheet using a scanning electron microscope, a transmission electron microscope, a Raman microspectrometer, an atomic force microscope, etc., and calculating the arithmetic average of the particle sizes. In this case, if the particles are non-spherical, the longest and shortest diameters are measured, and the average value is taken as the particle size of the particles.
[0071] (Other inorganic fillers) The present composition may contain inorganic fillers other than the agglomerated boron nitride particles and alumina particles (also referred to as "other inorganic fillers").
[0072] The other inorganic fillers contained in the present composition preferably have a thermal conductivity of 2.0 W / m·K or more, particularly preferably 3.0 W / m·K or more, particularly preferably 5.0 W / m·K or more, and particularly preferably 10.0 W / m·K or more.
[0073] Examples of such inorganic fillers include electrically insulating fillers consisting only of carbon, fillers consisting of metal carbides or semi-metal carbides, metal oxides or semi-metal oxides, and metal nitrides or semi-metal nitrides.
[0074] An example of the electrically insulating filler consisting only of carbon is diamond (thermal conductivity: approximately 2000 W / m·K). Examples of the metal carbide or semi-metal carbide include silicon carbide (thermal conductivity: about 60 to 270 W / m·K), titanium carbide (thermal conductivity: about 21 W / m·K), and tungsten carbide (thermal conductivity: about 120 W / m·K).
[0075] Examples of the metal oxides or semi-metal oxides include magnesium oxide (thermal conductivity: about 40 W / m·K), zinc oxide (thermal conductivity: about 54 W / m·K), yttrium oxide (thermal conductivity: about 27 W / m·K), zirconium oxide (thermal conductivity: about 3 W / m·K), ytterbium oxide (thermal conductivity: about 38.5 W / m·K), beryllium oxide (thermal conductivity: about 250 W / m·K), and "sialon" (ceramics composed of silicon, aluminum, oxygen, and nitrogen, thermal conductivity: about 21 W / m·K). Examples of the metal nitride or semi-metal nitride include boron nitride (thermal conductivity in the plane direction of a plate-like particle of hexagonal boron nitride (h-BN): approximately 200 to 500 W / m K), aluminum nitride (thermal conductivity: approximately 160 to 285 W / m K), and silicon nitride (thermal conductivity: approximately 30 to 80 W / m K).
[0076] These other inorganic fillers may be used alone or in combination of two or more kinds.
[0077] The shape of these other inorganic fillers may be irregular particles, spheres, whiskers, fibers, plates, or aggregates or mixtures thereof. Furthermore, if these other inorganic fillers have the same area circularity, aspect ratio, perimeter envelope ratio, area envelope ratio and average particle diameter (D50) as the alumina particles described above, the same effects as the alumina particles described above can be expected.
[0078] (Inorganic filler content) The content of the inorganic filler is preferably 60% by mass or more relative to 100% by mass of the solid content in the composition. If the content of the inorganic filler is 60% by mass or more relative to 100% by mass of the solid content in the composition, the insulating property and thermal conductivity can be improved. From this viewpoint, the content of the inorganic filler is preferably 60% by mass or more relative to 100% by mass of the solid content in the composition, more preferably 65% by mass or more, and even more preferably 70% by mass or more. On the other hand, if the content of the inorganic filler is 85% by mass or less, it is preferable from the viewpoint of maintaining the handling property and the film-forming property. Therefore, from such a viewpoint, the content of the inorganic filler is more preferably 83% by mass or less, and among these, even more preferably 81% by mass or less.
[0079] The content of the agglomerated boron nitride particles is preferably 15% by mass or more and 65% by mass or less with respect to 100% by mass of the total inorganic filler. If the content of the aggregated boron nitride particles is 15% by mass or more relative to 100% by mass of the total inorganic filler, the insulating property and thermal conductivity can be improved, while if the content is 65% by mass or less, the handling property and film-forming property can be maintained. From this viewpoint, the content of the aggregated boron nitride particles is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more, based on 100% by mass of the total inorganic filler, and is preferably 65% by mass or less, more preferably 50% by mass or less, and even more preferably 45% by mass or less.
[0080] The content of the alumina particles is preferably 35% by mass or more relative to 100% by mass of the total inorganic filler. If the content of the alumina particles is less than 35% by mass, the dispersion stability becomes poor when the present composition is made into a slurry, the inorganic filler becomes prone to settling, and the uniformity of the coating film is impaired, which is undesirable. Therefore, the content of the alumina particles is preferably 35% by mass or more, more preferably 40% by mass or more, even more preferably 45% by mass or more, and even more preferably 55% by mass or more, based on 100% by mass of the total inorganic filler. On the other hand, from the viewpoint of improving insulation and thermal conductivity, it is preferably 85 mass % or less, more preferably 81 mass % or less, even more preferably 77 mass % or less, and even more preferably 74 mass % or less.
[0081] The content of the alumina particles is preferably 120 parts by mass or more and 280 parts by mass or less per 100 parts by mass of the agglomerated boron nitride particles. It is preferable that the content of the alumina particles is 120 parts by mass or more relative to 100 parts by mass of the aggregated boron nitride particles, since the insulating property and the thermal conductivity can be improved, while it is preferable that the content is 280 parts by mass or less, since the dispersion stability is improved when the slurry is made, the inorganic filler is less likely to settle, and the uniformity of the coating film is maintained. From this viewpoint, the content of the alumina particles is preferably 120 parts by mass or more, more preferably 130 parts by mass or more, even more preferably 150 parts by mass or more, relative to 100 parts by mass of the aggregated boron nitride particles, and is preferably 280 parts by mass or less, more preferably 270 parts by mass or less, even more preferably 260 parts by mass or less, even more preferably 250 parts by mass or less.
[0082] <Polymers with molecular weight of 10,000 or more> The present composition preferably contains a polymer having a weight average molecular weight of 10,000 or more. By including a polymer having a mass average molecular weight of 10,000 or more in the present composition, the handling properties are improved and film-forming properties can be improved even if the content of inorganic filler, particularly agglomerated boron nitride particles, is increased.
[0083] The polymer may be any of a thermoplastic resin and a thermosetting compound. Examples of the thermoplastic resin and the thermosetting compound include thermoplastic resins such as polyphenylene ether, polyphenylene sulfide, polyarylate, polysulfone, polyether sulfone, polyether ether ketone, and polyether ketone. In addition, as the thermoplastic resin and the thermosetting compound, a group of heat-resistant resins called super engineering plastics, such as thermoplastic polyimide, thermosetting polyimide, benzoxazine, and a reaction product of polybenzoxazole and benzoxazine, can also be used. In addition, styrene-based polymers such as styrene and alkylstyrene, (meth)acrylic polymers such as alkyl (meth)acrylate and glycidyl (meth)acrylate, styrene-based-(meth)acrylic copolymers such as styrene-glycidyl methacrylate, polyvinyl alcohol derivatives such as polyvinyl butyral, polyvinyl benzal, and polyvinyl acetal, norbornene-based polymers containing a norbornene compound, and phenoxy resins can also be used. Among them, phenoxy resins are preferable in terms of heat resistance and compatibility with the thermosetting compound. The thermoplastic resin and the thermosetting compound may each be used alone or in combination of two or more kinds. Either one of the thermoplastic resin and the thermosetting compound may be used, or the thermoplastic resin and the thermosetting compound may be used in combination.
[0084] Among the above, the polymer is preferably one having a functional group reactive with the epoxy compound from the viewpoint of improving heat resistance. Here, examples of the functional group that reacts with the epoxy compound include a phenolic hydroxyl group, an epoxy group, a carboxylic acid group, a carboxylic anhydride group, and an active ester, as a functional group that reacts with an epoxy group. As a preferred example of such a polymer, from the viewpoint of solubility in other resin components, there can be mentioned a high molecular weight epoxy resin which will be described below.
[0085] (High molecular weight epoxy resin) From the viewpoint of the coatability of the thermosetting composition, the present composition preferably contains, as the polymer having a mass average molecular weight of 10,000 or more, an epoxy resin having a mass average molecular weight of 10,000 or more (referred to as a "high molecular weight epoxy resin"). Examples of high molecular weight epoxy resins include phenoxy resins having at least one skeleton selected from the group consisting of a bisphenol A type skeleton, a bisphenol F type skeleton, a bisphenol A / F mixed type skeleton, a naphthalene skeleton, a fluorene skeleton, a biphenyl skeleton, anthracene skeleton, a pyrene skeleton, a xanthene skeleton, an adamantane skeleton, and a dicyclopentadiene skeleton.
[0086] Examples of the high molecular weight epoxy resin include epoxy resins having at least one structure selected from a structure represented by the following formula (1) (hereinafter also referred to as "structure (1)") and a structure represented by the following formula (2) (hereinafter also referred to as "structure (2)").
[0087] TIFF2024134539000001.tif69170
[0088] In formula (1), R 1 and R 2 Each of R represents an organic group, at least one of which is an organic group having a molecular weight of 16 or more. 3 represents a divalent cyclic organic group.
[0089] The term "organic group" includes any group containing carbon atoms, and specific examples thereof include alkyl groups, alkenyl groups, and aryl groups, which may be substituted with halogen atoms, groups containing heteroatoms, or other hydrocarbon groups. The same applies hereinafter.
[0090] Furthermore, examples of high molecular weight epoxy resins include epoxy resins having a structure represented by the following formula (3) (hereinafter also referred to as "structure (3)").
[0091] TIFF2024134539000002.tif40170
[0092] In formula (3), R 4 , R 5 , R 6 , R 7 represents an organic group having a molecular weight of 15 or more.
[0093] In the above formula (1), R 1 and R 2 At least one of R represents an organic group having a molecular weight of 16 or more, preferably a molecular weight of 16 to 1000, and examples thereof include alkyl groups such as ethyl, propyl, butyl, pentyl, hexyl, and heptyl groups, and aryl groups such as phenyl, tolyl, xylyl, naphthyl, and fluorenyl groups. 1 and R 2may both be organic groups having a molecular weight of 16 or more, or one may be an organic group having a molecular weight of 16 or more and the other an organic group having a molecular weight of 15 or less or a hydrogen atom. Preferably, one is an organic group having a molecular weight of 16 or more and the other an organic group having a molecular weight of 15 or less, and in particular, one of them is a methyl group and the other a phenyl group, which is preferable from the viewpoints of easy control of handleability such as resin viscosity and strength of the cured product.
[0094] In the above formula (2), R 3 is a divalent cyclic organic group, which may be an aromatic ring structure such as a benzene ring structure, a naphthalene ring structure, or a fluorene ring structure, or an aliphatic ring structure such as cyclobutane, cyclopentane, or cyclohexane. They may also independently have a substituent such as a hydrocarbon group or a halogen atom. The divalent bond may be a divalent group on a single carbon atom or a divalent group on different carbon atoms. Preferred examples include divalent aromatic groups having 6 to 100 carbon atoms and groups derived from cycloalkanes having 2 to 100 carbon atoms such as cyclopropane and cyclohexane. In particular, a 3,3,5-trimethyl-1,1-cyclohexylene group represented by the following formula (4) (hereinafter also referred to as "structure (4)") is preferred from the viewpoints of controlling the handleability such as the resin viscosity and the strength of the cured product.
[0095] TIFF2024134539000003.tif44170
[0096] In the above formula (3), R 4 , R 5 , R 6 , R 7 Each of R is an organic group having a molecular weight of 15 or more. Preferably, R is an alkyl group having a molecular weight of 15 to 1000. 4 , R 5 , R 6 , R 7 It is preferable that all of the above be methyl groups from the viewpoints of controlling the handleability of the resin, such as viscosity, and strength of the cured product.
[0097] From the viewpoint of achieving both reduced moisture absorption and strength retention of the present cured product and the present thermal conductive sheet, it is particularly preferable for the high molecular weight epoxy resin to be an epoxy resin containing either one of Structure (1) and Structure (2) and Structure (3).
[0098] Such high molecular weight epoxy resins contain more hydrophobic hydrocarbon and aromatic structures than typical epoxy resins having bisphenol A or bisphenol F skeletons, so by blending high molecular weight epoxy resins, the moisture absorption amount of the resulting cured product, the thermal conductive sheet, can be reduced. From the viewpoint of reducing the amount of moisture absorption, the high molecular weight epoxy resin is preferably one that contains a large amount of structures (1), (2), and (3), which are hydrophobic structures. Specifically, it is more preferable that the high molecular weight epoxy resin has a mass average molecular weight of 20,000 or more, and even more preferably that the high molecular weight epoxy resin has a mass average molecular weight of 30,000 or more, for example, 30,000 to 80,000.
[0099] In addition, it is preferable that the high molecular weight epoxy resin is more hydrophobic, and from this viewpoint, the epoxy equivalent of the epoxy component is preferably large, specifically, 5,000 g / equivalent or more is preferable, and 7,000 g / equivalent or more, for example, 8,000 to 15,000 g / equivalent is more preferable.
[0100] The mass average molecular weight of the epoxy resin is a value calculated as polystyrene equivalent and measured by gel permeation chromatography. The epoxy equivalent is defined as "the mass of an epoxy resin containing one equivalent of an epoxy group" and can be measured in accordance with JIS K7236.
[0101] Such high molecular weight epoxy resins may be used alone or in combination of two or more kinds.
[0102] (Content) The content of the polymer having a mass average molecular weight of 10,000 or more is preferably 10% by mass or more and less than 30% by mass based on 100% by mass of the solid content in the present composition excluding the inorganic filler. The polymer is preferably contained in an amount of 10% by mass or more based on 100% by mass of the solid content of the composition excluding the inorganic filler, since it can maintain the inorganic filler retention and film-forming properties, whereas the polymer is preferably contained in an amount of less than 30% by mass, since it can maintain the strength when cured. From this viewpoint, the content of the polymer is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, based on 100% by mass of the solid content of the composition excluding the inorganic filler, and is preferably less than 30% by mass, and even more preferably 29% by mass or less. The content of the high molecular weight epoxy resin is the same as the content of the polymer having a mass average molecular weight of 10,000 or more.
[0103] <Hardening agent> The present composition preferably contains a curing agent, if necessary. Examples of the curing agent include phenol resins, compounds having a heterocyclic structure containing a nitrogen atom (hereinafter also referred to as "nitrogen-containing heterocyclic compounds"), acid anhydrides having an aromatic skeleton or an alicyclic skeleton, water additives of the acid anhydrides, or modified products of the acid anhydrides, etc. Only one type of curing agent may be used, or two or more types may be used in combination. By using these preferable curing agents, it is possible to obtain a cured product having an excellent balance of heat resistance, moisture resistance, and electrical properties.
[0104] Examples of the phenolic resin include phenolic novolac, o-cresol novolac, p-cresol novolac, t-butylphenol novolac, dicyclopentadiene cresol, polyparavinylphenol, bisphenol A type novolac, xylylene modified novolac, decalin modified novolac, poly(di-o-hydroxyphenyl)methane, poly(di-m-hydroxyphenyl)methane, or poly(di-p-hydroxyphenyl)methane. Among them, in order to further improve the flexibility and flame retardancy of the present composition, the present cured product, and the present thermal conductive sheet, and to improve the mechanical properties and heat resistance of the cured product, novolac type phenolic resins having a rigid main chain skeleton and phenolic resins having a triazine skeleton are preferred. In addition, in order to improve the flexibility of the uncured thermosetting composition and the toughness of the resin cured product, phenolic resins having an allyl group are preferred.
[0105] Examples of the heterocyclic structure of the nitrogen-containing heterocyclic compound include structures derived from imidazole, triazine, triazole, pyrimidine, pyrazine, pyridine, and azole. From the viewpoint of improving the insulating properties and adhesion to metals of the cured product, imidazole-based compounds and triazine-based compounds are preferred. Preferable imidazole compounds and triazine compounds include, for example, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4-diamino-6-vinyl-s-triazine, 2,4-diamino-6-vinyl-s-triazine isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-s-triazine, 2,4-diamino-6-methacryloyloxyethyl-s-triazine isocyanuric acid adduct, and the like can be mentioned.
[0106] Among these, those having a structure derived from imidazole and those having a structure derived from triazine are particularly preferred, since they have high resin compatibility and a high reaction activation temperature, and thus the curing rate and physical properties after curing can be easily adjusted, thereby enabling improvement in the storage stability of the composition and further improvement in the adhesive strength after heat molding to be realized. Therefore, those having a structure derived from imidazole and those having a structure derived from triazine are particularly preferred. As the heterocyclic structure of the nitrogen-containing heterocyclic compound, a structure derived from 1,3,5-triazine is particularly preferable, and the compound may have a plurality of the structural moieties exemplified above.
[0107] Depending on the structure, the nitrogen-containing heterocyclic compound may contain a thermosetting catalyst, which will be described later, and therefore the present composition may contain a nitrogen-containing heterocyclic compound as a thermosetting catalyst. The nitrogen-containing heterocyclic compound may be used alone or in combination of two or more kinds. Also, one molecule may simultaneously have a plurality of heterocyclic structures. The molecular weight of the nitrogen-containing heterocyclic compound is preferably 1,000 or less, and more preferably 500 or less.
[0108] The acid anhydride having an aromatic skeleton, the water-added product of the acid anhydride, or the modified product of the acid anhydride is not particularly limited.
[0109] The acid anhydride having an alicyclic skeleton, a water adduct of the acid anhydride, or a modified product of the acid anhydride is preferably an acid anhydride having a polyalicyclic skeleton, a water adduct of the acid anhydride, or a modified product of the acid anhydride, or an acid anhydride having an alicyclic skeleton obtained by an addition reaction of a terpene compound with maleic anhydride, a water adduct of the acid anhydride, or a modified product of the acid anhydride.
[0110] The curing agent is preferably contained in an amount of 0% by mass to 70% by mass, particularly 0% by mass to 55% by mass, based on 100% by mass of the solid content of the composition excluding the inorganic filler. If the content of the curing agent is equal to or more than the lower limit, sufficient curing performance can be obtained, and if it is equal to or less than the upper limit, the reaction proceeds effectively, the crosslinking density can be improved, the strength can be increased, and the film formability can be improved.
[0111] <Curing accelerator> The present composition may contain a thermosetting catalyst as a curing accelerator, if necessary, in order to adjust the curing rate and the physical properties of the cured product.
[0112] It is preferable to appropriately select the thermosetting catalyst depending on the type of thermosetting compound and curing agent. Specific examples of the thermosetting catalyst include linear or cyclic tertiary amines, organic phosphorus compounds, diazabicycloalkenes such as quaternary phosphonium salts or organic acid salts, and imidazoles. In addition, organic metal compounds, quaternary ammonium salts, metal halides, and the like can also be used. Examples of the organic metal compounds include zinc octylate, tin octylate, and aluminum acetylacetone complexes. Furthermore, the nitrogen-containing heterocyclic compound described above as a curing agent also functions as a thermosetting catalyst, and therefore may be blended as a thermosetting catalyst.
[0113] Among these, compounds having imidazole (referred to as "imidazole-based compounds") are preferred, particularly from the viewpoints of storage stability, heat resistance, and curing speed. Preferred imidazole compounds include, for example, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, Examples of the compound include 4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole. In particular, by using an imidazole-based compound having a melting point of 100° C. or higher, more preferably 200° C. or higher, a cured product having excellent storage stability and adhesion can be obtained. Furthermore, from the viewpoint of adhesion, those containing a nitrogen-containing heterocyclic compound other than the above-mentioned imidazole ring are more preferable. The thermosetting catalyst may be used alone or in combination of two or more kinds.
[0114] The thermosetting catalyst is preferably contained in an amount of 0.1% by mass to 10% by mass, particularly 0.1% by mass to 5% by mass, based on 100% by mass of the solid content of the composition excluding the inorganic filler. When the content of the thermosetting catalyst is equal to or more than the lower limit, the progress of the curing reaction can be sufficiently promoted to achieve good curing, and when it is equal to or less than the upper limit, the curing speed is not too fast, and therefore the storage stability of the composition can be improved.
[0115] <Organic solvent> The present composition may contain an organic solvent as necessary, for example, to improve the coatability when forming a sheet-like cured product through a coating step. Examples of organic solvents that may be contained in the present composition include methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether acetate, butyl acetate, isobutyl acetate, propylene glycol monomethyl ether, etc. These organic solvents may be used alone or in combination of two or more.
[0116] When the composition contains an organic solvent, the content is appropriately determined depending on the handleability during the preparation of the thermally conductive sheet, etc. Usually, the organic solvent is preferably used so that the solid content (total of components other than the solvent) in the composition is 10% by mass or more and 90% by mass or less, particularly 40% by mass or more or 80% by mass or less. In addition, when formed into a sheet, the organic solvent is preferably used so that the solids concentration (total of components other than the solvent) in the composition is 95 mass % or more, more preferably 97 mass % or more, even more preferably 98 mass % or more, and even more preferably 99 mass % or more.
[0117] <Other ingredients> The present composition may contain other ingredients in addition to the above ingredients. Examples of the other components include additives such as dispersants, thermoplastic resins, organic fillers, inorganic fillers, and silane coupling agents that improve the interfacial adhesive strength between inorganic fillers and resin components, additives that can be expected to have the effect of increasing the adhesive strength between a resin sheet and a metal plate-shaped material, insulating carbon components such as reducing agents, viscosity adjusters, thixotropic agents, flame retardants, colorants, various antioxidants such as phosphorus-based and phenol-based, process stabilizers such as phenol acrylate-based, heat stabilizers, hindered amine radical scavengers (HAAS), impact modifiers, processing aids, metal deactivators, copper inhibitors, antistatic agents, extenders, etc. The amount of these additives added when used may usually be within the range of the amount used for these purposes.
[0118] <<Uses of this composition>> The present composition can be turned into a cured product by heating, and the present conductive sheet can be obtained by forming the cured product into a sheet shape. The present composition can be used, for example, in composite molded articles having the present cured product and a metal part, such as heat dissipating laminates, heat dissipating circuit boards, semiconductor devices, and power modules, which will be described later.
[0119] <Thermal conductive sheet> The present thermally conductive sheet according to one embodiment of the present invention may be a thermally conductive sheet formed from a cured product of the present composition.
[0120] The thermal conductivity of the thermal conductive sheet in the thickness direction at 25° C. is preferably 8 W / m K or more, and more preferably 8.2 W / m K or more. When the thermal conductivity in the thickness direction is equal to or more than the above lower limit, the sheet can be suitably used in power semiconductor devices that operate at high temperatures. The thermal conductivity can be adjusted by the type and physical properties such as melt viscosity of the thermosetting compound, the type and content of the inorganic filler, the mixing method of the thermosetting compound and the inorganic filler, and the conditions in the heating and kneading process described below.
[0121] The thermal conductivity of the thermally conductive sheet in the thickness direction can be measured by the following method. For example, the thermal conductivity can be determined from the slope of a graph obtained by plotting thermal resistance against thickness using a thermal resistance measuring device (manufactured by Mentor Graphics Corporation, product name "T3ster").
[0122] The lower limit of the thickness of the thermally conductive sheet is preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more, while the upper limit of the thickness is preferably 400 μm or less, more preferably 300 μm or less, and even more preferably 250 μm or less. By making the thickness of this thermally conductive sheet 50 μm or more, sufficient voltage resistance characteristics can be ensured. On the other hand, by making the thickness 400 μm or less, it is possible to achieve a smaller and thinner device, particularly when the thermally conductive sheet is used in a power semiconductor device, and the thin film can reduce the thermal resistance in the thickness direction compared to insulating thermally conductive layers made of ceramic materials.
[0123] <Method of manufacturing thermally conductive sheet> An example of the method for producing the thermally conductive sheet will now be described.
[0124] The present thermally conductive sheet is prepared by forming the present composition into a sheet (this process is referred to as the "film-forming process"), drying the composition as necessary (this process is referred to as the "drying process"), and further applying pressure as necessary (this process is referred to as the "pressing process"). The sheet-shaped resin composition thus obtained is then cured to produce the present thermally conductive sheet as a sheet-shaped cured product (this process is referred to as the "curing process").
[0125] (Film forming process) For example, the present composition in a slurry form can be formed into a sheet by a coating method such as a blade method, a solvent casting method, or an extrusion film forming method.
[0126] When forming a film in a sheet form by the above coating method, the present composition in a slurry form is first coated on the surface of a substrate to form a coating film, that is, the present composition in a slurry form is used to form a coating film on the substrate by a dip method, a spin coating method, a spray coating method, a blade method, or any other method. The present composition in a slurry form can be applied using a coating device such as a spin coater, a slit coater, a die coater, a blade coater, etc. Such a coating device can uniformly form a coating film of a predetermined thickness on a substrate. As the substrate, a copper plate or copper foil or a PET film, which will be described later, is generally used, but there is no limitation thereto.
[0127] (drying process) The composition formed into a sheet as described above is usually dried at a temperature of 10°C or higher and 150°C or lower, preferably 25°C or higher or 120°C or lower, and more preferably 30°C or higher or 110°C or lower, in order to remove the solvent and low molecular weight components. By keeping the drying temperature at or below the upper limit, curing of the resin in the composition is suppressed, and the resin in the sheet-shaped thermosetting composition tends to flow in the subsequent pressurizing step, making it easier to remove voids. By keeping the drying temperature at or above the lower limit, the solvent can be effectively removed, and productivity tends to improve. The drying time is not particularly limited, and can be appropriately adjusted depending on the state of the composition, the drying environment, etc. The drying time is preferably 1 minute or more, more preferably 2 minutes or more, and even more preferably 5 minutes or more. The drying time is preferably 24 hours or less, more preferably 10 hours or less, even more preferably 4 hours or less, and particularly preferably 2 hours or less. By setting the drying time to the above lower limit or more, the solvent can be sufficiently removed, and the residual solvent tends to be prevented from forming voids in the cured resin. By setting the drying time to the above upper limit or less, the productivity tends to be improved, and the production cost tends to be reduced.
[0128] (Pressure process) After the drying step, it is desirable to apply pressure to the obtained sheet-like composition for the purposes of bonding inorganic fillers together to form a heat conduction path, eliminating voids and gaps in the sheet, improving adhesion to the substrate, etc. However, depending on the purpose, pressure may not be applied.
[0129] In the pressing step, it is desirable to apply a load of 2 MPa or more to the sheet-like composition on the substrate. The load is preferably 5 MPa or more, more preferably 7 MPa or more, and even more preferably 9 MPa or more. The load is preferably 1500 MPa or less, more preferably 1000 MPa or less, and even more preferably 800 MPa or less. By setting the load during pressing to the above upper limit or less, the secondary particles of the aggregated boron nitride particles are not destroyed, and a sheet having high thermal conductivity and no voids in the sheet-like composition can be obtained. By setting the load to the above lower limit or more, contact between the inorganic fillers becomes good, making it easier to form a thermal conduction path, and a cured product having high thermal conductivity can be obtained.
[0130] The heating temperature of the sheet-like composition on the substrate in the pressurizing step is not particularly limited. The heating temperature is preferably 10° C. or higher, more preferably 20° C. or higher, and even more preferably 30° C. or higher. The heating temperature is preferably 300° C. or lower, more preferably 250° C. or lower, even more preferably 200° C. or lower, even more preferably 100° C. or lower, and particularly preferably 90° C. or lower. By carrying out the pressurization step within this temperature range, the melt viscosity of the resin in the sheet-shaped present composition can be reduced, and voids and gaps in the present cured product can be further reduced. In addition, by heating at or below the upper limit value, decomposition of organic components in the sheet-shaped present composition and the present cured product, and voids caused by residual solvent tend to be suppressed.
[0131] The time of the pressurizing step is not particularly limited. The time of the pressurizing step is preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 3 minutes or more, and particularly preferably 5 minutes or more. The time of the pressurizing step is preferably 1 hour or less, more preferably 30 minutes or less, and even more preferably 20 minutes or less. By keeping the pressurizing time at or below the upper limit, the production time of the cured product can be reduced, and production costs tend to be reduced.By keeping the pressurizing time at or above the lower limit, voids and gaps in the cured product can be sufficiently removed, and heat transfer performance and voltage resistance tend to be improved.
[0132] (hardening process) The composition can be cured by heating. In this case, the heating temperature is preferably 30° C. or higher and 400° C. or lower, more preferably 50° C. or higher, and even more preferably 90° C. or higher. On the other hand, it is preferably 300° C. or lower, and even more preferably 250° C. or lower.
[0133] The curing step for completely curing the composition may be carried out under pressure or without pressure. When pressure is applied, it is preferable to carry out the step under the same conditions as the above-mentioned pressurizing step for the same reasons as above. The pressurizing step and the curing step may be carried out simultaneously. In particular, in the sheet forming process which involves a pressing step and a hardening step, it is preferable to apply a load within the above range and carry out the pressing and hardening.
[0134] The load applied when the pressing step and the curing step are carried out simultaneously is not particularly limited. In this case, it is preferable to apply a load of 5 MPa or more to the sheet-like composition on the substrate, more preferably 7 MPa or more, even more preferably 9 MPa or more, and particularly preferably 20 MPa or more. In addition, the load is preferably 2000 MPa or less, more preferably 1500 MPa or less. By setting the load when the pressurizing step and the curing step are carried out simultaneously to the above upper limit value or less, the secondary particles of the aggregated boron nitride particles are not destroyed, and a sheet-like cured product having high thermal conductivity and no voids in the sheet-like present composition can be obtained. In addition, by setting the load to the above lower limit value or more, contact between the inorganic fillers becomes good, making it easier to form a thermal conduction path, and therefore a cured product having high thermal conductivity can be obtained.
[0135] When the pressing step and the curing step are performed simultaneously, the pressing time is not particularly limited. The pressing time is preferably 30 seconds or more, more preferably 1 minute or more, even more preferably 3 minutes or more, and particularly preferably 5 minutes or more. The pressing time is preferably 3 hours or less, more preferably 2 hours 45 minutes or less, and even more preferably 2 hours 30 minutes or less. By keeping the pressurizing time at or below the upper limit, the production time for the sheet-shaped cured resin material can be reduced, and production costs tend to be reduced.By keeping the pressurizing time at or above the lower limit, voids and gaps in the sheet-shaped cured material, i.e., the thermally conductive sheet, can be sufficiently removed, and heat transfer performance and voltage resistance tend to be improved.
[0136] <<Composite molded body>> A composite molded article according to one embodiment of the present invention (referred to as "the present composite molded article") is a composite molded article having a cured product of the present composition and a metal part. Next, as examples of the present composite molded article, a heat dissipating laminate, a heat dissipating circuit board, and a semiconductor device will be described, although the present composite molded article is not limited to these.
[0137] <<Heat dissipation laminate>> A heat dissipation laminate according to one embodiment of the present invention (referred to as "the present heat dissipation laminate") may be a laminate including the present thermally conductive sheet.
[0138] An example of the present heat dissipating laminate is one in which a heat dissipating metal layer containing a heat dissipating material is laminated on one surface of the present heat conductive sheet.
[0139] The heat dissipating material is not particularly limited as long as it is made of a material having good thermal conductivity. In particular, in order to increase the thermal conductivity in the laminated structure, it is preferable to use a heat dissipating metal material, and more preferably to use a flat metal material. The type of metal material is not particularly limited, but among them, a copper plate, an aluminum plate, an aluminum alloy plate, etc. are preferable because they have good thermal conductivity and are relatively inexpensive.
[0140] The thermal conductive sheet and the heat dissipation metal layer can be laminated and integrated by press molding, which is a batch process. In this case, the press equipment and press conditions are the same as those for obtaining the thermal conductive sheet.
[0141] <<Heat dissipation circuit board>> A heat dissipation circuit board according to one embodiment of the present invention (hereinafter referred to as "the present heat dissipation circuit board") may be any circuit board provided with the present thermally conductive sheet. An example of the present heat dissipating circuit board is one in which the above-mentioned heat dissipating metal layer is laminated on one surface of the present heat conductive sheet, and a circuit board is formed on the surface of the present heat conductive sheet opposite the heat dissipating metal layer, for example, by etching or the like. Specifically, an integrated structure of "heat dissipating metal layer / the present heat conductive sheet / conductive circuit" is more preferable. The state before the circuit etching can be, for example, an integrated structure of "heat dissipating metal layer / the present heat conductive sheet / metal layer for forming conductive circuit", in which the metal layer for forming conductive circuit is flat and formed on the entire surface of one side of the present heat conductive sheet, or formed on a partial area.
[0142] The material of the conductive circuit-forming metal layer is not particularly limited. In particular, it is generally preferable to form the conductive circuit-forming metal layer from a copper thin plate having a thickness of 0.05 mm to 1.2 mm in terms of electrical conductivity, etching properties, cost, and the like.
[0143] <<Semiconductor Devices>> A semiconductor device according to an example of an embodiment of the present invention (hereinafter referred to as "the present semiconductor device") may be any device that includes the present heat dissipation circuit board. An example of the present semiconductor device is one having a configuration in which a silicon wafer or a rewiring layer on which a pre-divided semiconductor chip is mounted is formed on the present heat dissipation circuit board.
[0144] <<Power module>> A power module according to an example of an embodiment of the present invention (hereinafter referred to as "the present power module") may be any module that includes the present thermally conductive sheet. An example of the present power module is one in which the present thermally conductive sheet is mounted as the present heat dissipating circuit board on a power semiconductor device. In this power semiconductor device, conventionally known materials can be appropriately used for the aluminum wiring, sealing material, packaging material, heat sink, thermal paste, solder, and other materials other than the thermally conductive sheet or the heat dissipation laminate.
[0145] <<Explanation of terms>> In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "it is preferably greater than X" or "it is preferably less than Y". In the present invention, the term "sheet" conceptually encompasses a sheet, a film, and a tape. In addition, in this specification, the expression "preferably" encompasses the meaning of "not necessarily essential, but it is better to make it essential". In addition, in this specification, the expression "and / or" means "and / or." EXAMPLES
[0146] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as the gist of the present invention is not exceeded.
[0147] <Materials used> The materials used in the examples and comparative examples are as follows.
[0148] (Inorganic filler) Inorganic filler A: spherical agglomerated boron nitride particles having a house-of-cards structure manufactured based on International Publication No. 2015 / 119198 (average particle size (D50): 45 μm, maximum particle size (Dmax): 90 μm)
[0149] Inorganic filler B-1: Nippon Light Metal Co., Ltd., alumina particles, average particle diameter (D50): 4.0 μm, maximum particle diameter (Dmax): 18.3 μm, area circularity, aspect ratio, average aspect ratio, perimeter envelopment and area envelopment are listed in Table 1. Inorganic filler B-2: Manufactured by Resonac, alumina particles, average particle diameter (D50): 22.4 μm, maximum particle diameter (Dmax): 61.4 μm, area circularity, aspect ratio, average aspect ratio, perimeter envelope and area envelope are listed in Table 1. Inorganic filler B-3: Admatechs Co., Ltd., spherical alumina particles, average particle diameter (D50): 11.7 μm, maximum particle diameter (Dmax): 30.8 μm, area circularity, aspect ratio, average aspect ratio, perimeter envelope and area envelope are shown in Table 1.
[0150] In the present invention, the term "spherical particles" refers to particles containing 50% or more by number of particles having an area circularity of 0.95 or more.
[0151] [Average particle size (D50) and maximum particle size (Dmax)] The average particle size (D50) and maximum particle size (Dmax) of inorganic filler A were determined by dispersing inorganic filler A in a pure water medium containing sodium hexametaphosphate as a dispersion stabilizer, measuring the volumetric particle size distribution using a laser diffraction / scattering particle size distribution analyzer LA-300 (manufactured by HORIBA, Ltd.), and determining the cumulative volume 50% particle size (average particle size D50) and maximum particle size Dmax from the obtained particle size distribution. The average particle size (D50) and maximum particle size (Dmax) of inorganic fillers B-1, B-2, and B-3 were measured using an image particle size distribution analyzer (Malvern Panalytical Morphologi 4) with a sample size of 5 mm 3 The volumetric particle size distribution was measured at an airflow dispersion pressure of 4.0 barr (injection pressure) and an objective lens magnification of 20x, and particles with a circumferential envelope ratio of less than 0.97, which were considered to be aggregated, were excluded, and the cumulative volume 50% particle diameter (average particle diameter D50) and maximum particle diameter Dmax were calculated from the particle size distribution obtained. The particle diameter of non-spherical particles was calculated from the circle equivalent area. At this time, the number of particles excluding particles with a circumferential envelope ratio of less than 0.97 was 10,000 or more.
[0152] [Circularity of area] The circularity of the inorganic fillers B-1, B-2 and B-3 was measured using an image particle size distribution analyzer (Malvern Panalytical Morphologi 4) with a sample of 5 mm 3 The airflow dispersion pressure was 4.0 bar (injection pressure) and the objective lens magnification was 20x. The circular area and actual particle perimeter were measured and calculated using the formula: circular area / actual particle perimeter squared. The ratio (number %) of alumina particles having a predetermined circularity in all alumina particles was calculated by excluding particle images with a perimeter envelope ratio of less than 0.97 from the obtained data, and taking the number of particles with a perimeter envelope ratio of 0.97 or more as the total number of alumina particles, using the formula "number of alumina particles having a predetermined circularity in area / total number of alumina particles." In this case, the number of particles excluding particles with a perimeter envelope ratio of less than 0.97 was 10,000 or more. The percentage by number (number %) of alumina particles having an area circularity of 0.95 or less to all alumina particles is shown in Table 1 as "area circularity of 0.95 or less / total alumina", and the percentage by number (number %) of alumina particles having an area circularity of 0.90 or less to all alumina particles is shown in Table 1 as "area circularity of 0.90 or less / total alumina".
[0153] [Aspect ratio and average aspect ratio] The aspect ratios of inorganic fillers B-1, B-2, and B-3 were measured using an image particle size distribution analyzer (Malvern Panalytical Morphologi 4) with a sample size of 5 mm 3 The airflow dispersion pressure was 4.0 bar (injection pressure), and the objective lens magnification was 20x. The minor axis (maximum perpendicular length to the maximum length) and maximum length were measured, and the aspect ratio was calculated using the formula: minor axis (maximum perpendicular length to the maximum length) / maximum length. The proportion (number %) of alumina particles having a given aspect ratio to all alumina particles was calculated by excluding particle images with a perimeter envelope of less than 0.97 from the obtained data, counting particles with a perimeter envelope of 0.97 or more as the total number of alumina particles, and using the formula "number of alumina particles having a given aspect ratio / total number of alumina particles." In this case, the number of particles excluding particles with a perimeter envelope of less than 0.97 was 10,000 or more. The percentage by number (%) of alumina particles having an aspect ratio of less than 0.85 to all alumina particles is shown in Table 1 as "aspect ratio less than 0.85 / total alumina", and the percentage by number (%) of alumina particles having an aspect ratio of less than 0.7 to all alumina particles is shown in Table 1 as "aspect ratio less than 0.7 / total alumina". In addition, from the obtained data, particle images with a perimeter-to-envelope ratio of less than 0.97, which could be determined to be agglomerated particles, were excluded, and particles with a perimeter-to-envelope ratio of 0.97 or more were counted as the total number of alumina particles, and the average of these aspect values was defined as the "average aspect ratio."
[0154] [Perimeter Envelope and Area Envelope] The perimeter envelope and area envelope of inorganic fillers B-1, B-2, and B-3 were measured using an image-based particle size distribution analyzer (Malvern Panalytical's Morphologi 4) with a sample size of 5 mm 3 The envelope area and envelope perimeter obtained from the end surface contact of the particles were measured under conditions of an airflow dispersion pressure of 4.0 bar (injection pressure) and an objective lens magnification of 20x, while the actual perimeter and actual area were measured and calculated using the formulas "area envelopment ratio = actual area / envelope area" and "perimeter envelopment ratio = envelope perimeter (end surface contact) / actual perimeter". The proportion (number %) of alumina particles having a given perimeter envelope degree to all alumina particles was calculated by excluding particle images with a perimeter envelope degree of less than 0.97 from the obtained data, taking the total number of alumina particles as the number of particles with a perimeter envelope degree of 0.97 or more, and using the formula "number of alumina particles having a given perimeter envelope degree or area envelope degree / total number of alumina particles." In this case, the number of particles excluding particles with a perimeter envelope degree of less than 0.97 was 10,000 or more. The proportion (number %) of alumina particles with a perimeter envelope ratio greater than 0.970 and smaller than 0.985 to all alumina particles is shown in Table 1 as "0.970 < perimeter envelope ratio < 0.985," and the proportion (number %) of alumina particles with an area envelope ratio smaller than 0.950 to all alumina particles is shown in Table 1 as "area envelope ratio < 0.950."
[0155] [Table 1]
[0156] (thermosetting compound) High molecular weight epoxy resin C: a bifunctional epoxy resin disclosed as resin component 1 in the examples of JP 2020-63438 A, having a polystyrene-equivalent weight average molecular weight of 30,000 and an epoxy equivalent of 9,000 g / equivalent. It has structures represented by the above formulas (2), (3), and (4). Aromatic epoxy compound D: Difunctional aromatic backbone epoxy compound, molecular weight approximately 400. · Polyfunctional epoxy compound E: Polyfunctional epoxy compound (molecular weight 500 or less) with a structure containing 4 or more glycidyl groups per molecule, not including an amine or amide structure containing a nitrogen atom.
[0157] (Other Ingredients) Hardener F: Phenol resin hardener "MEH-8000H" (manufactured by Meiwa Kasei Co., Ltd.) -Thermosetting catalyst G: 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine. Contains both a structure derived from imidazole and a structure derived from triazine in one molecule ("Curesol 2E4MZ-A" manufactured by Shikoku Kasei Co., Ltd.) -Thermosetting catalyst H: 2-phenyl-4,5-dihydroxymethylimidazole ("Curezol 2PHZ-PW" manufactured by Shikoku Kasei Co., Ltd.) Organic solvent: Mixture of methyl ethyl ketone and cyclohexanone
[0158] <Examples 1, 2, and 3 and Comparative Examples 1 and 2> Using a planetary stirring device, inorganic filler A, inorganic filler B, high molecular weight epoxy resin C, aromatic epoxy compound D, polyfunctional epoxy compound E, curing agent F, thermosetting catalyst G, and thermosetting catalyst H were weighed out in the mass ratios shown in Table 2, and these were added to and mixed with an organic solvent consisting of methyl ethyl ketone and cyclohexanone to prepare a thermosetting composition as a coating slurry. At this time, methyl ethyl ketone and cyclohexanone were used so that the solid content concentration was 80 mass%.
[0159] The obtained slurry-like thermosetting composition was applied to a PET substrate by a doctor blade method and dried by heating at 60° C. for 120 minutes to obtain a sheet-like molded product (uncured) having a thickness of 150 μm, which was made of the thermosetting composition. The total content of methyl ethyl ketone and cyclohexanone in the sheet-like molded product was 1 mass % or less.
[0160] <Evaluation of Sheet-Shaped Molded Product> The sheet-like molded products obtained in the above Examples and Comparative Examples were evaluated as follows.
[0161] (Measurement of thermal conductivity in the thickness direction of the cured sheet-like molded body) The sheet-like molded products obtained in the Examples and Comparative Examples were cured by heating to 120° C. while being pressed at the pressures shown in Table 2, to obtain evaluation sample sheets made of the cured products with a thickness of 150 μm. In addition, two, three, four, and five of the sheet-like molded articles obtained in the Examples and Comparative Examples were stacked and pressed and heated in the same manner as above to obtain five types of evaluation sample sheets with different thicknesses.
[0162] The thickness, area, and thermal resistance of these five evaluation sample sheets with different thicknesses were measured as shown in (1) to (3) below, and the thermal conductivity (25°C) in the sheet thickness direction using the steady-state method was calculated from the slope represented by the thermal resistance value versus sheet thickness as shown in (4) below (in accordance with ASTM D5470). (1) Thickness: Thickness (μm) when pressed at a pressure of 3400 kPa using a Mentor Graphics T3Ster-DynTIM (2) Measurement area: The area (cm) of the part that transfers heat when measuring using a Mentor Graphics T3Ster-DynTIM 2 ) (3) Thermal resistance: Thermal resistance (K / W) when pressed at a pressure of 3400 kPa using Mentor Graphics T3Ster-DynTIM. (4) Thermal conductivity: The thermal resistance of five sheets of different thicknesses was measured, and the thermal conductivity (W / m K) was calculated using the following formula. Formula: Thermal conductivity (W / m K) = 1 / ((slope (thermal resistance value / thickness): K / (W μm)) × (area: cm 2 ))×10 -2
[0163] When the measured thermal conductivity was 8 W / m K or higher, it was judged as "◯ (good)", and when it was less than 8 W / m K, it was judged as "× (poor)".
[0164] <Solder reflow resistance test> The surfaces of two copper plates, one with a thickness of 500 μm and the other with a thickness of 2,000 μm, were roughened with #120 sandpaper 100 times each. The sheet-like molded body obtained in the Examples and Comparative Examples was sandwiched between these copper plates and pressed using a hot press at 120°C for 30 minutes with the pressure shown in Table 2. The temperature was then raised and the molded body was pressed at 175°C for 30 minutes with the pressure shown in Table 2. The temperature was then further raised and the molded body was pressed at 200°C for 30 minutes with the pressure shown in Table 2 to obtain a composite molded body. The obtained composite molded body was protected by 2,000 μm of copper, and 500 μm of copper was etched to pattern a 500 μm copper plate to prepare a sample for solder reflow resistance test. At this time, the pattern was left with two circular patterns of φ25 mm.
[0165] The solder reflow resistance test sample thus prepared was stored in an environment of 85°C and 85% RH for 3 days using a thermohygrostat SH-221 (manufactured by Espec Corporation). Next, in a nitrogen atmosphere, the temperature was raised from room temperature to 290°C in 12 minutes, and after holding at 290°C for 10 minutes, it was cooled to room temperature (solder reflow resistance test). After that, the bonding interface between the copper plate and the sheet-shaped molded body was observed using an ultrasonic imaging device FineSAT (FS300III) (manufactured by Hitachi Power Solutions). The measurement was performed using a probe with a frequency of 50 MHz, a gain of 30 dB, and a pitch of 0.2 mm, and the sample was placed in water.
[0166] A case where no interfacial peeling occurred in the solder reflow resistance test was judged as "◯ (good)", and a case where interfacial peeling occurred in the solder reflow resistance test was judged as "× (poor)". Note that no interfacial peeling occurs when the bonding area is 99.5% or more of the patterning area.
[0167] [Table 2]
[0168] In Table 2, the "total amount of thermosetting composition" refers to the amount of components (solid content) excluding the organic solvent in the "thermosetting composition" prepared in the Examples and Comparative Examples, i.e., the total parts by mass of the inorganic filler, the thermosetting compound, the curing agent, and the thermosetting catalyst. The "mass ratio of the total resin components" refers to the ratio (mass %) of the total parts by mass of the thermosetting compound, the curing agent, and the thermosetting catalyst to the total amount of the thermosetting composition (100 mass %). The "amount of inorganic filler relative to the thermosetting composition" refers to the total mass ratio (mass %) of inorganic filler A and inorganic filler B relative to the total amount of the thermosetting composition (100 mass %). The "alumina content relative to the inorganic filler" refers to the mass ratio (mass %) of the alumina component, that is, inorganic filler B, relative to the combined mass of inorganic filler A and inorganic filler B being 100 mass %.
[0169] (Consideration) From the above examples and the results of tests conducted by the inventors thus far, it has been found that by forming a cured product, specifically a thermally conductive sheet, using a thermosetting composition containing agglomerated boron nitride particles and alumina particles (referred to as "non-spherical alumina particles") in which the proportion of alumina particles with an area circularity of 0.95 or less is 50% or more and 70% or less by number, relative to 100% by number of the total alumina particles, and in which the alumina particles account for 35% or more by mass of the inorganic filler, it is possible to achieve both thermal conductivity and solder reflow resistance. The reason for this is presumably because the flat surfaces of the agglomerated boron nitride particles and non-spherical alumina particles are more likely to meet, increasing the contact area between the two and reducing the contact thermal resistance, thereby improving the thermal conductivity. It is also presumed that the contact area between the agglomerated boron nitride particles and non-spherical alumina particles is larger, improving the bonding strength between the two, making it less likely for voids to occur during the solder reflow resistance test, which prevents peeling between the thermally conductive sheet and the substrate (Cu). Considering this mechanism of action, it is presumed that similar effects can be obtained even when other inorganic fillers having particles with similar areal circularity in a similar ratio are used instead of the alumina particles in the above examples.
[0170] In addition, from the above examples and the results of tests conducted by the inventors, when scaly boron nitride particles are used instead of agglomerated boron nitride particles, the scales of the scaly boron nitride particles are oriented horizontally in the thickness direction during molding. In contrast, when agglomerated boron nitride particles, particularly spherical agglomerated boron nitride particles, are used, they are not oriented in a specific direction, so it has been found that the thermal conductivity in the thickness direction during molding, for example, the thickness direction of the sheet, can be further increased. In addition, when spherical alumina particles are used instead of the non-spherical alumina particles, even when combined with aggregated boron nitride particles, the state of association between the two particles becomes point contact instead of surface contact, which increases the contact thermal resistance and makes it impossible to increase the thermal conductivity. Also, it was found that peeling occurs between the resin and the filler during solder reflow, creating voids, which causes the thermal conductive sheet to peel off from the substrate (copper).
Claims
1. A thermosetting composition containing an inorganic filler and a thermosetting compound, The content of the inorganic filler is 60% by mass or more relative to 100% by mass of the solid content in the thermosetting composition, the inorganic filler is composed of two or more kinds of fillers, at least one of the inorganic fillers is boron nitride particles, and the boron nitride particles are agglomerated particles; At least one other type is alumina particles; the alumina particles have an areal circularity of 0.95 or less as measured by an image particle size distribution measuring device, and the proportion of the alumina particles is 50% by number or more and 70% by number or less with respect to 100% by number of all the alumina particles; A thermosetting composition, wherein the ratio of all alumina particles to the total inorganic filler is 35 mass% or more.
2. 2. The thermosetting composition according to claim 1, wherein the alumina particles have an average particle size of 0.5 μm or more and 30 μm or less.
3. 2. The thermosetting composition according to claim 1, wherein the alumina particles have an area circularity of 0.90 or less as measured by an image particle size distribution measuring device, and the proportion of the alumina particles having an area circularity of 0.90 or less as measured by an image particle size distribution measuring device is 20% by number or more and 40% by number or less with respect to 100% by number of all the alumina particles.
4. 2. The thermosetting composition according to claim 1, wherein the alumina particles have an aspect ratio of less than 0.85 as measured by an image particle size distribution analyzer, and the proportion of the alumina particles is 50% by number or more and 80% by number or less relative to 100% by number of all the alumina particles.
5. 2. The thermosetting composition according to claim 1, wherein the alumina particles have an aspect ratio of less than 0.7 as measured by an image particle size distribution analyzer, and the proportion of the alumina particles is 15% by number or more and 40% by number or less relative to 100% by number of all the alumina particles.
6. 2. The thermosetting composition according to claim 1, wherein the alumina particles have a circumferential length envelope ratio of more than 0.970 and less than 0.985 as measured by an image particle size distribution analyzer, and the ratio of the alumina particles is 5% by number or more and 40% by number or less relative to 100% by number of the total alumina particles.
7. 2. The thermosetting composition according to claim 1, wherein the alumina particles have an area envelope ratio of less than 0.950 as measured by an image particle size distribution analyzer, and the ratio of the alumina particles is 5% by number or more and 40% by number or less relative to 100% by number of all the alumina particles.
8. 10. The thermosetting composition of claim 1 comprising a polymer having a weight average molecular weight of 10,000 or greater.
9. 9. The thermosetting composition according to claim 8, comprising a polymer having a mass average molecular weight of 10,000 or more in a proportion of 10 mass% or more and less than 30 mass% relative to 100 mass% of a solid content in the thermosetting composition excluding an inorganic filler.
10. The thermosetting composition according to claim 1 , comprising, as the thermosetting compound, a polyfunctional epoxy compound having three or more epoxy groups per molecule and a molecular weight of 650 or less.
11. The thermosetting composition according to claim 10, wherein the polyfunctional epoxy compound is an epoxy compound having four or more glycidyl groups in one molecule.
12. A cured product obtained by using the thermosetting composition according to any one of claims 1 to 11.
13. A thermally conductive sheet comprising the cured product according to claim 12.
14. A composite molded article comprising a cured product of the thermosetting composition according to any one of claims 1 to 11 and a metal part.
Citation Information
Patent Citations
Encapsulation resin sheet and electronic device
JP2016204545A
Heat release resin sheet and device containing heat release resin sheet
JP2017036415A