Catalyst for propylene polymerization and method for producing propylene-based polymer

The propylene polymerization catalyst stabilizes molecular weight changes and reduces high-temperature activity, addressing lump formation and reactor efficiency issues by using a specific catalyst composition, thereby enhancing polymer production stability.

JP2024134609APending Publication Date: 2024-10-04JAPAN POLYPROPYLENE CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023044882
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing propylene polymerization catalysts face issues with excessive heat generation during polymerization, leading to lump formation and reduced productivity due to high polymerization activity and significant changes in molecular weight (MFR) with temperature fluctuations, which affect reactor load and piping clogging.

Method used

A propylene polymerization catalyst comprising a solid catalyst component formed by contacting titanium, magnesium, halogen, and electron donor with a silane compound having an alkenyl group, an alkoxysilane compound, and an organoaluminum compound, along with a compound represented by the formula R1C(O)OR2, which reduces polymerization activity at high temperatures and stabilizes molecular weight changes.

Benefits of technology

The catalyst significantly reduces polymerization activity at high temperatures and minimizes the range of molecular weight variation (MFR) of the obtained polymer, preventing lump formation and maintaining reactor efficiency while ensuring stable polymer properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134609000003
    Figure 2024134609000003
  • Figure 2024134609000004
    Figure 2024134609000004
  • Figure 2024134609000001
    Figure 2024134609000001
Patent Text Reader

Abstract

To provide a catalyst for propylene polymerization which significantly decreases polymerization activity at high temperatures and can reduce the change rate in MFR of the resulting polymer with respect to temperature.SOLUTION: There is provided a catalyst for propylene polymerization which comprises a solid catalyst component (A) obtained by subjecting the following components (a2), (3) and (a4) to contact treatment with the following component (a1), an organoaluminum compound (B) and a compound (C) represented by the following general formula (1). Component (a1): a solid component containing titanium, magnesium, halogen and an electron donor. Component (a2): a silane compound having an alkenyl group. Component (a3): an alkoxysilane compound [which is different from a silane compound having an alkenyl group]. Component (a4): an organoaluminum compound. R1C(O)OR2 Formula(1) (wherein, R1 and R2 each independently represents a hydrocarbon group which may contain a heteroatom.)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a propylene polymerization catalyst and a method for producing a propylene polymer using the propylene polymerization catalyst. [Background technology]

[0002] α-olefin polymers, typified by polypropylene, are excellent in various physical properties such as rigidity and heat resistance, have excellent moldability, can be produced relatively inexpensively, and pose few environmental problems. For these reasons, they are used in a wide range of applications as basic industrial resin materials, and the demand for them is increasing. As described above, α-olefin polymers such as polypropylene, which have excellent performance and advantages from each viewpoint, have traditionally been produced industrially primarily using Ziegler-Natta catalysts.

[0003] In the field of Ziegler-Natta catalysts, first, a catalyst was developed that uses a magnesium compound as a catalyst support and a solid catalyst component that contains titanium and a halogen as essential components. Numerous studies have been conducted on the use of various supports, the use of electron donor compounds (internal and external donor components), and the combined use of silicon compounds with special structures having alkenyl groups such as vinyl groups and allyl groups, and highly active catalysts have been developed (e.g., Patent Documents 1 to 6).

[0004] As the activity of the catalyst increases, excessive heat is generated during the polymerization period in an actual polyolefin polymerization apparatus, and when the temperature rises close to the melting point of the polymer, lumpy or sheet-like polymers are generated, which can cause problems such as increased load on the heat removal and stirring capacity of the polymerization reactor, clogging of piping, etc., and can reduce productivity. As a method for solving such problems, it is known to use additives during polymerization (Patent Document 7, Non-Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 61-285203 [Patent Document 2] Japanese Patent Application Publication No. 11706 / 1983 [Patent Document 3] Japanese Patent Application Publication No. 3-234707 [Patent Document 4] JP 2006-169283 A [Patent Document 5] JP 2007-106939 A [Patent Document 6] JP 2003-292523 A [Patent Document 7] Special Publication No. 2012-500319 [Non-patent literature]

[0006] [Non-Patent Document 1] Particuology 2010, 8, p.578-581 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the techniques disclosed in Patent Document 7 and Non-Patent Document 1, even if the polymerization activity at high temperatures decreases, the MFR of the polymer polymerized at high temperatures changes significantly, and thus it is not possible to produce polyolefins with stable physical properties. A technology for stably producing polyolefins, such as reducing polymerization activity at high temperatures and minimizing the range of change in molecular weight (MFR) of the resulting polymer versus temperature, has not yet been realized, and there is a strong demand for the development of a polymerization catalyst with such capabilities.

[0008] Under such circumstances, an object of the present invention is to provide a propylene polymerization catalyst which exhibits a significant decrease in polymerization activity at high temperatures and can reduce the variation in molecular weight (MFR) of the resulting polymer with respect to temperature, and a method for producing a propylene polymer using the same. [Means for solving the problem]

[0009] As a result of intensive research conducted by the present researchers to achieve the above-mentioned objective, they discovered a propylene polymerization catalyst in which the polymerization activity at high temperatures is significantly reduced and the range of change in the molecular weight (MFR) of the resulting polymer with respect to temperature is reduced. That is, the present invention includes the following aspects.

[0010] <1> A propylene polymerization catalyst comprising: a solid catalyst component (A) obtained by contact-treating the following component (a1) with components (a2), (a3) ​​and (a4); an organoaluminum compound (B); and a compound (C) represented by the following general formula (1). Component (a1): A solid component containing titanium, magnesium, a halogen, and an electron donor. Component (a2): Silane compound having an alkenyl group Component (a3): an alkoxysilane compound (however, different from a silane compound having an alkenyl group). Component (a4): Organoaluminum compound Formula (1) R 1 C(O)OR 2 (In formula (1), R 1 and R 2 each independently represents a hydrocarbon group which may contain a heteroatom. <2> the amount of the compound (C) used is in a molar ratio to the organoaluminum compound (B) (the number of moles of the compound (C) / the number of moles of the organoaluminum compound (B)) of 0.05 to 2.0; <1> The propylene polymerization catalyst according to claim 1, <3> The component (a2) is a compound represented by the following general formula (3): <1> or <2> The propylene polymerization catalyst according to claim 1, Formula (3) SiR 6 n R 7 4-n (In formula (3), R 6represents an alkenyl group. R 7 represents a hydrogen atom, a halogen atom or an alkyl group. n is 1, 2, 3, or 4; when n is 1 or 2, R 7 They may be linked to each other to form a ring structure.) <4> The component (a3) ​​is a compound represented by the following general formula (2): <1> ~ <3> 13. The propylene polymerization catalyst according to claim 12. Formula (2) R 3 R 4 m Si(OR 5 ) n (In formula (2), R 3 represents a hydrocarbon group which may contain a hetero atom. R 4 represents a hydrogen atom, a halogen atom, or a hydrocarbon group which may contain a hetero atom. R 5 represents a hydrocarbon group. m is 0, 1 or 2, n is 1, 2 or 3, and m+n=3 is satisfied. <5> The above <1> ~ <4> 1. A method for producing a propylene-based polymer, comprising homopolymerizing or copolymerizing propylene in the presence of the propylene polymerization catalyst according to any one of claims 1 to 9. Effect of the Invention

[0011] According to the present invention, it is possible to provide a propylene polymerization catalyst which exhibits a significant decrease in polymerization activity at high temperatures and can reduce the variation in molecular weight (MFR) of the resulting polymer with respect to temperature, and a method for producing a propylene polymer using the same. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 shows a graph in which activity is plotted against polymerization temperature for Examples 1 to 3 and Comparative Example 1. [Diagram 2]FIG. 2 shows a graph in which the MFR is plotted against the polymerization temperature for each of the Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The propylene polymerization catalyst and the method for producing a propylene-based polymer of the present invention will be described in detail below. In this specification, the symbol "to" indicating a range of values ​​is used to mean that the values ​​before and after the symbol are included as the lower and upper limits.

[0014] I. Propylene Polymerization Catalysts The propylene polymerization catalyst of the present invention is a propylene polymerization catalyst comprising a solid catalyst component (A) obtained by contact-treating the following component (a1) with components (a2), (a3) ​​and (a4), an organoaluminum compound (B), and a compound (C) represented by the following general formula (1). Component (a1): A solid component containing titanium, magnesium, a halogen, and an electron donor. Component (a2): Silane compound having an alkenyl group Component (a3): an alkoxysilane compound (however, different from a silane compound having an alkenyl group). Component (a4): Organoaluminum compound Formula (1) R 1 C(O)OR 2 (In formula (1), R 1 and R 2 each independently represents a hydrocarbon group which may contain a heteroatom.

[0015] The method for producing the propylene polymerization catalyst of the present invention may include the following steps 1 and 2. Step 1: A step of contacting the following components (a1), (a2), (a3) ​​and (a4) to obtain a solid catalyst component (A): Component (a1): A solid component containing titanium, magnesium, a halogen, and an electron donor. Component (a2): Silane compound having an alkenyl group Component (a3): an alkoxysilane compound (however, different from a silane compound having an alkenyl group). Component (a4): Organoaluminum compound Step 2: A step of mixing the solid catalyst component (A), an organoaluminum compound (B), and a compound (C) represented by the following general formula (1) to prepare a propylene polymerization catalyst. Formula (1) R 1 C(O)OR 2 (In formula (1), R 1 and R 2 each independently represents a hydrocarbon group which may contain a heteroatom.

[0016] In the present invention, the components (a1), (a2), (a3) ​​and (a4) are contact-treated to obtain a solid catalyst component (A), and the propylene polymerization catalyst contains the solid catalyst component (A), an organoaluminum compound (B) and a compound (C) represented by the general formula (1). When a propylene-based polymer is produced using the propylene polymerization catalyst, the polymerization activity at high temperatures is significantly reduced, and the change in molecular weight (MFR) of the resulting polymer with respect to temperature can be reduced. It is believed that the compound (C) represented by the general formula (1) used in the present invention undergoes a decomposition reaction with the organoaluminum (B) at a specific temperature or higher, generating aldehydes or ketones with a small structure. It is believed that at high temperatures, the decomposition reaction products of the compound (C) represented by the general formula (1) can poison the active species, thereby significantly reducing the polymerization activity at high temperatures. In addition, since the solid catalyst component (A) used in the present invention is obtained by contacting the components (a1), (a2), (a3) ​​and (a4), it has been found that even if propylene is polymerized at high temperatures in the presence of the organoaluminum compound (B) and the compound (C) represented by the general formula (1), the change in MFR is smaller than that of a propylene-based polymer obtained from a catalyst not using the solid catalyst component (A). It was not previously known that the change in MFR is smaller under high-temperature polymerization when the solid catalyst component (A) obtained by contacting the components (a1), (a2), (a3) ​​and (a4) is used, and this is the effect found in the present invention. Although the mechanism of this action has not yet been clarified, it is believed to be as follows. The alkenyl group of the silane compound (a2) having the alkenyl group protects the active species (Ti) and stabilizes the active species. This suppresses the deterioration of the active species due to heat, so that it is presumed that the change in MFR is suppressed even when polymerized at high temperatures, and the change in the molecular weight (MFR) of the obtained polymer with respect to temperature can be reduced.

[0017] 1.Solid catalyst component (A) The solid catalyst component (A) used in the present invention is obtained by contacting the following component (a1) with components (a2), (a3) ​​and (a4). Component (a1): A solid component containing titanium, magnesium, a halogen, and an electron donor. Component (a2): Silane compound having an alkenyl group Component (a3): an alkoxysilane compound (however, different from a silane compound having an alkenyl group). Component (a4): Organoaluminum compound

[0018] 1-1. Component (a1) Component (a1) according to the present invention is a solid component containing titanium, magnesium, halogen, and an electron donor.

[0019] 1-1-1. Magnesium As the magnesium compound serving as the magnesium source used for the solid component (a1) according to the present invention, any magnesium compound can be used. Representative examples thereof include the compounds disclosed in JP-A-3-234707. Generally, magnesium halide compounds typified by magnesium chloride, alkoxymagnesium compounds typified by diethoxymagnesium, metallic magnesium, oxymagnesium compounds typified by magnesium oxide, hydroxymagnesium compounds typified by magnesium hydroxide, Grignard compounds typified by butylmagnesium chloride, organomagnesium compounds typified by butyloctylmagnesium, magnesium salt compounds of inorganic acids and organic acids typified by magnesium carbonate and magnesium stearate, and mixtures thereof and compounds having an average composition formula that is a mixed formula thereof (for example, Mg(OEt) m Cl 2-m ; compounds such as 0 <m <2, etc.) can be used. Among these, magnesium chloride, diethoxymagnesium, metallic magnesium, and butylmagnesium chloride are particularly preferred.

[0020] In particular, when producing large particles, it is preferable to use dialkoxymagnesium, which is easy to control the catalyst particle size. As the dialkoxymagnesium, not only the pre-produced one can be used, but also the one obtained by reacting alcohol in the presence of metallic magnesium and halogen or a halogen-containing metal compound during the catalyst production process can be used. Furthermore, in the present invention, the dialkoxymagnesium is preferably in the form of granules or powder, and its shape may be amorphous or spherical. For example, when a spherical dialkoxymagnesium is used, a polymer powder having a better particle shape and a narrow particle size distribution is obtained, the handling of the produced polymer powder during the polymerization operation is improved, and problems such as clogging caused by fine powder contained in the produced polymer powder are eliminated.

[0021] The above-mentioned spherical dialkoxymagnesium does not necessarily have to be a perfect sphere, and elliptical or potato-shaped ones can also be used. Specifically, the particle shape has a ratio (l / w) of the major axis diameter l to the minor axis diameter w of 3 or less, preferably 1 to 2, and more preferably 1 to 1.5. The dialkoxymagnesium may have an average particle size of 1 μm to 200 μm, preferably 5 μm to 150 μm. In the case of spherical dialkoxymagnesium, the average particle size is 1 μm to 100 μm, preferably 5 μm to 50 μm, and more preferably 10 μm to 40 μm. As for the particle size, it is desirable to use one with a narrow particle size distribution with few fine and coarse powders. Specifically, the particles of 5 μm or less are 20% or less, preferably 10% or less. On the other hand, the particles of 100 μm or more are 10% or less, preferably 5% or less. Furthermore, when the particle size distribution is expressed as ln(D90 / D10) (where D90 is the particle size at 90% of the cumulative particle size, and D10 is the particle size at 10% of the cumulative particle size), it is 3 or less, and preferably 2 or less.

[0022] Methods for producing the above-mentioned spherical dialkoxymagnesium are exemplified in, for example, JP-A-58-41832, JP-A-62-51633, JP-A-3-74341, JP-A-4-368391, JP-A-8-73388 and the like.

[0023] 1-1-2.Titanium As the titanium compound serving as the titanium source used in the solid component (a1) according to the present invention, any compound can be used. Representative examples include the compounds disclosed in JP-A-3-234707. Regarding the valence of titanium, a titanium compound having any valence of tetravalent, trivalent, divalent, or zero-valent can be used, but preferably a tetravalent and trivalent titanium compound, and more preferably a tetravalent titanium compound.

[0024] Specific examples of the tetravalent titanium compound include titanium halide compounds typified by titanium tetrachloride, alkoxytitanium compounds typified by tetrabutoxytitanium, condensed compounds of alkoxytitanium having a Ti—O—Ti bond typified by tetrabutoxytitanium dimer (BuO)3Ti—O—Ti(OBu)3, and organometallic titanium compounds typified by dicyclopentadienyltitanium dichloride. Among these, titanium tetrachloride and tetrabutoxytitanium are particularly preferred.

[0025] Specific examples of the trivalent titanium compound include titanium halide compounds typified by titanium trichloride. Titanium trichloride can be a compound produced by any known method such as a hydrogen reduction type, a metal aluminum reduction type, a metal titanium reduction type, or an organoaluminum reduction type. The above titanium compounds can be used not only alone but also in combination of a plurality of compounds. Further, mixtures of the above titanium compounds and compounds having an average composition formula that is a mixed formula thereof (for example, compounds such as Ti(OBu) m Cl 4-m ; 0 <m <4, etc.), and complexes with other compounds such as phthalic acid esters (for example, compounds such as Ph(CO2Bu)2·TiCl4) can be used.

[0026] 1-1-3. Halogen As the halogen used in the solid component (a1) according to the present invention, fluorine, chlorine, bromine, iodine, and mixtures thereof can be used. Among these, chlorine is particularly preferred. Halogen is generally supplied from the titanium compound and / or magnesium compound, but can also be supplied from other compounds.Typical examples include silicon halide compounds such as silicon tetrachloride, aluminum halide compounds such as aluminum chloride, organic halide compounds such as 1,2-dichloroethane and benzyl chloride, borane halide compounds such as trichloroborane, phosphorus halide compounds such as phosphorus pentachloride, tungsten halide compounds such as tungsten hexachloride, and molybdenum halide compounds such as molybdenum pentachloride.These compounds can be used alone or in combination.Among these, silicon tetrachloride is particularly preferred.

[0027] 1-1-4. Electron donor Representative examples of the electron donor used in the solid component (a1) according to the present invention include the compounds disclosed in JP 2004-124090 A. In general, organic acids, inorganic acids and their derivatives (esters, acid anhydrides, acid halides, amides), ether compounds, ketone compounds, aldehyde compounds, alcohol compounds, amine compounds, etc. can be used, and the donor may be one or a mixture of two or more selected from the group consisting of organic acids, inorganic acids and their derivatives, ether compounds, and ketone compounds.

[0028] Examples of organic acid compounds that can be used as electron donors include aromatic polycarboxylic acid compounds such as phthalic acid, aromatic carboxylic acid compounds such as benzoic acid, aliphatic polycarboxylic acid compounds such as malonic acid having one or two substituents at the 2-position, such as 2-n-butyl-malonic acid, and succinic acid having one or two substituents at the 2-position or one or more substituents at each of the 2-position and the 3-position, such as 2-n-butyl-succinic acid, aliphatic carboxylic acid compounds such as propionic acid, and aromatic and aliphatic sulfonic acid compounds such as benzenesulfonic acid and methanesulfonic acid. These carboxylic acid compounds and sulfonic acid compounds may have any number of unsaturated bonds at any position in the molecule, like maleic acid, regardless of whether they are aromatic or aliphatic.

[0029] Examples of derivative compounds of organic acids that can be used as electron donors include esters (carboxylate compounds), acid anhydrides, acid halides, and amides of the above organic acids. The alcohol that is a component of the ester may be an aliphatic or aromatic alcohol. Among these alcohols, alcohols having an aliphatic free radical with 1 to 20 carbon atoms, such as an ethyl group, a butyl group, an isobutyl group, a heptyl group, an octyl group, or a dodecyl group, are preferred. More preferably, alcohols having an aliphatic free radical with 2 to 12 carbon atoms are preferred. In addition, alcohols having an alicyclic free radical, such as a cyclopentyl group, a cyclohexyl group, or a cycloheptyl group, may also be used.

[0030] The halogen that is a component of the acid halide may be fluorine, chlorine, bromine, iodine, etc. Among them, chlorine is most preferable. In the case of a polyhalide of a polyvalent organic acid, the multiple halogens may be the same or different. In addition, as the amine that is a component of the amide, aliphatic and aromatic amines can be used. Among these amines, preferred examples include ammonia, aliphatic amines such as ethylamine and dibutylamine, and amines having an aromatic free radical in the molecule such as aniline and benzylamine.

[0031] Examples of inorganic acid compounds that can be used as electron donors include carbonic acid, phosphoric acid, silicic acid, sulfuric acid, and nitric acid. As the derivative compounds of these inorganic acids, it is preferable to use esters, specific examples of which include tetraethoxysilane (ethyl silicate), tetrabutoxysilane (butyl silicate), and tributyl phosphate.

[0032] Examples of ether compounds that can be used as electron donors include aliphatic ether compounds such as dibutyl ether, aromatic ether compounds such as diphenyl ether, aliphatic polyvalent ether compounds such as 1,3-dimethoxypropane having one or two substituents at the 2-position, e.g., 2-isopropyl-2-isobutyl-1,3-dimethoxypropane and 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and polyvalent ether compounds having an aromatic free radical in the molecule, e.g., 9,9-bis(methoxymethyl)fluorene.

[0033] Examples of ketone compounds that can be used as electron donors include aliphatic ketone compounds such as methyl ethyl ketone, aromatic ketone compounds such as acetophenone, and polyhydric ketone compounds such as 2,2,4,6,6-pentamethyl-3,5-heptanedione. Examples of aldehyde compounds that can be used as electron donors include aliphatic aldehyde compounds such as propionaldehyde, and aromatic aldehyde compounds such as benzaldehyde. Further, examples of alcohol compounds that can be used as electron donors include aliphatic alcohol compounds such as butanol and 2-ethylhexanol, phenol derivative compounds such as phenol and cresol, and aliphatic or aromatic polyhydric alcohol compounds such as glycerin and 1,1'-bi-2-naphthol.

[0034] Examples of amine compounds that can be used as electron donors include aliphatic amine compounds such as diethylamine, nitrogen-containing alicyclic compounds such as 2,2,6,6-tetramethyl-piperidine, aromatic amine compounds such as aniline, polyvalent amine compounds such as 1,3-bis(dimethylamino)-2,2-dimethylpropane, and nitrogen-containing aromatic compounds.

[0035] Furthermore, as a compound that can be used as an electron donor, a compound containing the above-mentioned multiple functional groups in the same molecule can also be used. Examples of such compounds include carboxylate compounds having an alkoxy group in the molecule, such as ethyl acetate (2-ethoxyethyl) and ethyl 3-ethoxy-2-t-butylpropionate, ketoester compounds, such as ethyl 2-benzoylbenzoate, ketoether compounds, such as 1-t-butyl-2-methoxyethyl)methyl ketone, aminoether compounds, such as N,N-dimethyl-2,2-dimethyl-3-methoxypropylamine, and halogenoether compounds, such as epoxychloropropane.

[0036] These electron donors can be used not only alone but also in combination of two or more compounds. Among these, preferred are phthalic acid diester compounds such as diethyl phthalate, dibutyl phthalate, diisobutyl phthalate, and diheptyl phthalate; phthalic acid dihalide compounds such as phthaloyl dichloride; malonic acid ester compounds having one or two substituents at the 2-position such as 2-n-butyl-diethyl malonate; succinic acid ester compounds having one or two substituents at the 2-position or one or more substituents at each of the 2-position and the 3-position such as 2-n-butyl-diethyl succinate; aliphatic polyvalent ether compounds such as 1,3-dimethoxypropane having one or two substituents at the 2-position such as 2-isopropyl-2-isobutyl-1,3-dimethoxypropane and 2-isopropyl-2-isopentyl-1,3-dimethoxypropane; polyvalent ether compounds having an aromatic free radical in the molecule such as 9,9-bis(methoxymethyl)fluorene; and cyclic ether compounds such as 2,5-dimethylfuran and 2,5-diphenylfuran. Among these, particularly preferred are organic acid ester compounds, acid halide compounds and ether compounds, and particularly preferred are those selected from the group consisting of phthalic acid diester compounds and phthalic acid dihalide compounds. The ratio of the amounts of the components constituting the solid component (a1) used in the present invention may be any amount within a range that does not impair the effects of the present invention, but is generally preferably within the following ranges.

[0037] The amount of the titanium compound used relative to the amount of the magnesium compound used is preferably within a range of 0.0001 to 1,000, more preferably 0.001 to 100, and particularly preferably 0.01 to 50, in terms of molar ratio (number of moles of titanium compound / number of moles of magnesium compound).

[0038] When a compound serving as a halogen source other than a magnesium compound and a titanium compound is used, the amount of the compound used is, regardless of whether each of the magnesium compound and the titanium compound contains a halogen or not, preferably within a range of 0.01 to 1,000, particularly preferably 0.1 to 100, in terms of molar ratio (number of moles of compound serving as a halogen source / number of moles of magnesium compound) relative to the amount of the magnesium compound used, preferably within a range of 0.01 to 1,000, particularly preferably 0.1 to 100.

[0039] The amount of the electron donor used is preferably within a range of 0.001 to 10, particularly preferably 0.01 to 5, in terms of molar ratio (number of moles of electron donor / number of moles of magnesium compound) relative to the amount of the magnesium compound used.

[0040] The solid component (a1) according to the present invention can be obtained by contacting the above-mentioned constituent components in the above-mentioned ratios. The contact conditions for the components must be such that oxygen is not present, but any conditions can be used as long as the effects of the present invention are not impaired. In general, the following conditions are preferred: The contact temperature is about -50°C to 200°C, preferably 0°C to 150°C. Examples of the contact method include a mechanical method using a rotating ball mill or a vibrating mill, and a method in which the mixture is contacted by stirring in the presence of an inert diluent.

[0041] In the preparation of the solid component (a1), intermediate and / or final washing with an inert solvent may be carried out. Preferred examples of the solvent include aliphatic hydrocarbon compounds such as heptane, aromatic hydrocarbon compounds such as toluene and xylene, and halogen-containing hydrocarbon compounds such as 1,2-dichloroethylene and chlorobenzene.

[0042] As a method for preparing the solid component (a1) according to the present invention, any method can be used, and specifically, the following methods (i) to (vii) can be exemplified. However, the present invention is not limited to the following examples.

[0043] (i) Co-grinding method This is a method in which a halogen-containing magnesium compound, typically magnesium chloride, is co-ground with a titanium compound to support the titanium compound on the magnesium compound. An electron donor may be co-ground simultaneously or in a separate step. As the mechanical pulverization method, any pulverizer such as a rotary ball mill or a vibration mill can be used. Not only a dry pulverization method that does not use a solvent, but also a wet pulverization method in which co-pulverization is performed in the presence of an inert solvent can be used.

[0044] (ii) Heat treatment method This method involves stirring a halogen-containing magnesium compound, typically magnesium chloride, with a titanium compound in an inert solvent to carry out a contact treatment, thereby supporting the titanium compound on the magnesium compound. An electron donor may be contacted simultaneously or in a separate step. When a liquid compound such as titanium tetrachloride is used as the titanium compound, the contact treatment can be carried out without using an inert solvent. If necessary, an optional component such as a silicon halide compound may be contacted simultaneously or in a separate step. There is no particular limitation on the contact temperature, but it is often preferable to carry out the contact treatment at a relatively high temperature of about 90°C to 130°C.

[0045] (iii) Elution method The dissolution-precipitation method is a method in which a halogen-containing magnesium compound, such as magnesium chloride, is dissolved by contacting it with an electron donor, and the resulting solution is brought into contact with a precipitating agent to cause a precipitation reaction, thereby forming particles. Examples of the electron donor used for dissolution include alcohol compounds, epoxy compounds, phosphoric acid ester compounds, silicon compounds having an alkoxy group, titanium compounds having an alkoxy group, and ether compounds. Examples of the precipitating agent include titanium halide compounds, silicon halide compounds, hydrogen chloride, halogen-containing hydrocarbon compounds, siloxane compounds having a Si-H bond (including polysiloxane compounds), aluminum compounds, and the like. The method for bringing the dissolving solution into contact with the precipitating agent may be to add the precipitating agent to the dissolving solution, or to add the dissolving solution to the precipitating agent. In either the dissolution or precipitation step, when a titanium compound is not used, the particles formed by the precipitation reaction are further contacted with a titanium compound, thereby supporting the titanium compound on the magnesium compound. If necessary, the particles formed by the above method may be contacted with optional components such as titanium halide compounds or silicon halide compounds, or with an electron donor, which may be different from or the same as that used for dissolution. The order of contacting these optional components is not particularly limited, and they may be contacted as independent steps or may be contacted together during dissolution, precipitation and contact with titanium compounds. An inert solvent may be present in any of the steps of dissolution, precipitation, and contact with an optional component.

[0046] (iv) Granulation method The granulation method is a method in which, like the dissolution-precipitation method, a halogen-containing magnesium compound, such as magnesium chloride, is dissolved by contacting it with an electron donor, and the resulting solution is granulated mainly by a physical method. Examples of the electron donor used for dissolution are the same as those in the dissolution-precipitation method. Examples of granulation techniques include a method of dropping a high-temperature solution into a low-temperature inert solvent, a method of spraying a solution from a nozzle toward a high-temperature gas phase and drying it, and a method of spraying a solution from a nozzle toward a low-temperature gas phase and cooling it. The particles formed by granulation are brought into contact with a titanium compound, thereby supporting the titanium compound on the magnesium compound. If necessary, the mixture may be contacted with optional components such as halogenated silicon compounds and electron donors. In this case, the electron donor may be different from or the same as that used in the dissolution. The order of contacting these optional components is not particularly limited, and they may be contacted as independent steps or may be contacted together when dissolving or contacting with the titanium compound. An inert solvent may be present in any of the steps of dissolution, contact with titanium compounds, and contact with optional components.

[0047] (v) Halogenation of magnesium (Mg) compounds The halogenation method of a magnesium (Mg) compound is a method in which a halogen-free magnesium compound is contacted with a halogenating agent to halogenate it, and an electron donor may be contacted simultaneously or in a separate step. Examples of halogen-free magnesium compounds include dialkoxymagnesium compounds, magnesium oxide, magnesium carbonate, magnesium salts of fatty acids, and the like. When a dialkoxymagnesium compound is used, it is also possible to use one prepared in situ by reacting metallic magnesium with an alcohol. When using this preparation method, it is common to form particles by granulation or the like at the stage of the starting material, the magnesium compound not containing a halogen. Examples of the halogenating agent include titanium halide compounds, silicon halide compounds, and phosphorus halide compounds. When a titanium halide compound is not used as the halogenating agent, the halogen-containing magnesium compound formed by halogenation is further contacted with a titanium compound, thereby supporting the titanium compound on the magnesium compound. If necessary, the grains formed by the above method may be contacted with an optional component such as a titanium halide compound or a silicon halide compound, or may be contacted with an electron donor. The order of contacting these optional components is not particularly limited, and they may be contacted as independent steps, or they may be contacted together with the halogenation of a halogen-free magnesium compound or the contact with a titanium compound. An inert solvent may be present in either step of contacting with the titanium halide compound or the step of contacting with the optional component.

[0048] (vi) Precipitation from organomagnesium compounds This method involves contacting a precipitating agent with a solution of an organomagnesium compound such as a Grignard reagent typified by butylmagnesium chloride or a dialkylmagnesium compound, and the electron donor may be contacted simultaneously or in a separate step. Examples of the precipitating agent include titanium compounds, silicon compounds, hydrogen chloride, and the like. When a titanium compound is not used as the precipitating agent, the particles formed by the precipitation reaction are further contacted with a titanium compound, thereby supporting the titanium compound on the magnesium compound. If necessary, the grains formed by the above method may be contacted with an optional component such as a titanium halide compound or a silicon halide compound, or may be contacted with an electron donor. There is no particular restriction on the order of contacting these optional components, and they may be contacted as independent steps or together with the precipitation or contact with the titanium compound. An inert solvent may be present in any of the steps of precipitation, contact with titanium compounds, and contact with optional components.

[0049] (vii) Impregnation method This method involves impregnating an inorganic compound support or an organic compound support with a solution of an organomagnesium compound or a solution in which a magnesium compound is dissolved with an electron donor. Examples of organomagnesium compounds are the same as those in the example of the precipitation method from an organomagnesium compound. The magnesium compound used for dissolving the magnesium compound may or may not contain a halogen, and examples of electron donors are the same as those in the example of the dissolution-precipitation method. Examples of inorganic carriers include silica, alumina, and magnesia. Examples of organic carriers include polyethylene, polypropylene, polystyrene, and the like. After the impregnation treatment, the carrier particles are subjected to a chemical reaction with a precipitating agent or a physical treatment such as drying to precipitate and immobilize the magnesium compound. Examples of the precipitating agent are the same as those in the dissolution-precipitation method. When a titanium compound is not used as a precipitating agent, the thus-formed particles are further contacted with a titanium compound to support the titanium compound on the magnesium compound. If necessary, the thus-formed particles may be further contacted with an optional component such as a titanium halide compound or a silicon halide compound, or may be contacted with an electron donor. The order of contacting these optional components is not particularly limited, and they may be contacted as independent steps, or they may be contacted together during impregnation, precipitation, drying, and contact with titanium compounds. In addition, an inert solvent may be present in any of the steps of impregnation, precipitation, contact with titanium compounds, and contact with optional components.

[0050] (viii) Combined method The above methods (i) to (vii) can also be used in combination. Examples of the combination include "a method of co-grinding magnesium chloride with an electron donor, followed by heat treatment with a titanium halide compound", "a method of co-grinding a magnesium chloride compound with an electron donor, dissolving it with another electron donor, and then precipitating it with a precipitating agent", "a method of dissolving a dialkoxy magnesium compound with an electron donor, contacting it with a titanium halide compound to precipitate and simultaneously halogenate the magnesium compound", and "a method of contacting a dialkoxy magnesium compound with carbon dioxide to generate and simultaneously dissolve magnesium carbonate ester compounds, impregnating silica with the resulting solution, then contacting it with hydrogen chloride to halogenate the magnesium compound, simultaneously precipitating and fixing it, and further contacting it with a titanium halide compound to support the titanium compound".

[0051] 1-1-5. Prepolymerization of solid component (a1) In the present invention, the solid component (a1) may be prepolymerized using a polymerization monomer in the presence of an organoaluminum compound as a co-catalyst. As the polymerization monomer in the preliminary polymerization, the compounds disclosed in JP-A-2004-124090 and the like can be used, and specific examples thereof include ethylene, propylene, and α-olefins having 4 to 22 carbon atoms and represented by the general formula (5) described later. The reaction conditions of the solid component (a1) with the above-mentioned polymerizable monomers can be any conditions within the range that does not impair the effects of the present invention. In general, the following ranges are preferred. The amount of the prepolymerized monomer per gram of the solid component (a1) is within a range of 0.001 g to 100 g, preferably 0.1 g to 50 g, and more preferably 0.5 g to 10 g. The reaction temperature during the preliminary polymerization is −150° C. to 150° C., and preferably 0° C. to 100° C. The reaction temperature during the preliminary polymerization is desirably lower than the polymerization temperature during the main polymerization. The reaction is generally preferably carried out under stirring, and an inert solvent such as hexane or heptane may be present. The prepolymerization may be carried out several times, and the monomers used for polymerization may be the same or different. After the prepolymerization, washing may be carried out with an inert solvent such as hexane or heptane. The material and amount of the organoaluminum compound used may be the same as those described below for component (a4).

[0052] 1-2. Silane compounds having alkenyl groups (a2) As the silane compound (a2) having an alkenyl group used in the present invention, compounds disclosed in JP-A-2-34707, JP-A-2003-292522, JP-A-2006-169283, and JP-A-2011-74360 can be used.

[0053] In general, it is desirable to use a compound represented by the following general formula (3), but the present invention is not limited to this compound. Formula (3) SiR 6 n R 7 4-n (In formula (3), R 6 represents an alkenyl group. R 7 represents a hydrogen atom, a halogen atom or an alkyl group. n is 1, 2, 3, or 4; when n is 1 or 2, R 7 They may be linked to each other to form a ring structure.)

[0054] R 6 represents an alkenyl group, preferably a vinyl group, an allyl group, or a 3-butenyl group, more preferably a vinyl group or an allyl group, and further preferably a vinyl group. 6 may be the same or different. n may be 1, 2, or 3, and may be 1 or 2.

[0055] R 7 represents a hydrogen atom, a halogen atom, or an alkyl group. R 7 Examples of halogen atoms that can be used as the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Also, R 7 The alkyl group as R may be a linear alkyl group, a branched alkyl group, or a cycloalkyl group. 7 When is an alkyl group, it is preferably an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 1 to 12 carbon atoms. Specific preferred examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an i-butyl group, an s-butyl group, a t-butyl group, a thexyl group, a cyclopentyl group, and a cyclohexyl group. If n is 2 or less, there are multiple R 7 may be the same or different. When n is 1 or 2, R 7 They may be linked together to form a ring structure. R 7 is preferably a halogen atom or an alkyl group, more preferably an alkyl group having 1 to 20 carbon atoms, even more preferably an alkyl group having 1 to 10 carbon atoms, and particularly preferably an alkyl group having 1 to 4 carbon atoms.

[0056] Specific examples of the silane compound (a2) having an alkenyl group include vinyl silane, methyl vinyl silane, dimethyl vinyl silane, trimethyl vinyl silane, trichloro vinyl silane, dichloro methyl vinyl silane, chloro dimethyl vinyl silane, chloro methyl vinyl silane, triethyl vinyl silane, chloro diethyl vinyl silane, dichloro ethyl vinyl silane, dimethyl ethyl vinyl silane, diethyl methyl vinyl silane, tripentyl vinyl silane, triphenyl vinyl silane, diphenyl methyl vinyl silane, Nylsilane, dimethylphenylvinylsilane, CH2=CH-Si(CH3)2(C6H4CH3), (CH2=CH)(CH3)2Si-O-Si(CH3)2(CH=CH2), divinylsilane, dichlorodivinylsilane, dimethyldivinylsilane, diphenyldivinylsilane, allyltrimethylsilane, allyltriethylsilane, allyltrivinylsilane, allylmethyldivinylsilane, allyldimethylvinylsilane, allylmethyldichlorosilane, allyltrichlorosilane, allyltribromo Silane, diallyl dimethyl silane, diallyl diethyl silane, diallyl divinyl silane, diallyl methyl vinyl silane, diallyl methyl chloro silane, diallyl dichloro silane, diallyl dibromo silane, triallyl methyl silane, triallyl ethyl silane, triallyl vinyl silane, triallyl chloro silane, triallyl bromo silane, tetraallyl silane, di-3-butenyl dimethyl silane, di-3-butenyl silane diethyl silane, di-3-butenyl silane divinyl silane, di-3-butenyl Silane methylvinylsilane, di-3-butenylsilane methylchlorosilane, di-3-butenylsilane dichlorosilane, tri-3-butenylsilane ethylsilane, tri-3-butenylsilane vinylsilane, tri-3-butenylsilane chlorosilane, tri-3-butenylsilane bromosilane, tetra-3-butenylsilane, 1-methyl-1-vinylsilacyclobutane, 1-methyl-1-vinylsilacyclopentane, 1-methyl-1-vinylsilacyclohexane, 1,1-divinylsilacyclopentane, 1,Examples of the silacyclohexane include 1-divinylsilacyclohexane, 1-chloro-1-vinylsilacyclopentane, 1-chloro-1-vinylsilacyclohexane, 1-allyl-1-methylsilacyclopentane, and 1-allyl-1-methylsilacyclohexane. Among these, vinylsilane compounds containing a vinyl group are preferred, with trimethylvinylsilane, trichlorovinylsilane, dimethyldivinylsilane, and 1-methyl-1-vinylsilacyclopentane being particularly preferred.

[0057] The amount of the silane compound (a2) having an alkenyl group may be any amount within a range that does not impair the effects of the present invention, but is generally preferably within the following range. The amount of the silane compound (a2) having an alkenyl group used is, in terms of a molar ratio to the titanium component constituting the solid component (a1) (number of moles of the silane compound (a2) having an alkenyl group / number of moles of titanium atoms in the solid component (a1)), preferably within the range of 0.001 to 1,000, more preferably within the range of 0.01 to 100.

[0058] The role of the silane compound (a2) having an alkenyl group is speculated as follows. The silane compound (a2) having an alkenyl group used in the present invention is generally more sterically hindered than the α-olefin monomer used in polymerization, and is not polymerized with a Ziegler-Natta catalyst. However, due to the presence of an organic silyl group with very strong electron donating properties, the charge density of the carbon-carbon double bond is very high, and it is thought that it coordinates or inserts into the titanium atom, which is the active site. Therefore, it is expected to have an effect of preventing over-reduction of the titanium atom by the organic aluminum compound used in the preparation of the solid catalyst component (A) and deactivation of the active site due to impurities. In addition, in the present invention, the alkenyl group of the silane compound (a2) having an alkenyl group protects the active species (Ti) and stabilizes the active species. As a result, the deterioration of the active species due to heat is suppressed, and it is presumed that the change in MFR is suppressed even when polymerized at high temperatures, and the change range of the molecular weight (MFR) of the polymer obtained with respect to temperature can be reduced. In the silane compound having an alkenyl group, the alkenyl moiety is coordinated to or inserted into a titanium atom, forming a reaction product.

[0059] 1-3. Alkoxysilane compound (a3) The alkoxysilane compound (A3) used in the present invention is different from the above-mentioned silane compound (a2) having an alkenyl group. In the present invention, the component (a3) ​​may be a silicon compound represented by the following general formula (2). Formula (2) R 3 R 4 m Si(OR 5 ) n (In formula (2), R 3 represents a hydrocarbon group which may contain a hetero atom. R 4 represents a hydrogen atom, a halogen atom, or a hydrocarbon group which may contain a hetero atom. R 5 represents a hydrocarbon group. m is 0, 1 or 2, n is 1, 2 or 3, and m+n=3 is satisfied.

[0060] In general formula (2), R 3 represents a hydrocarbon group which may contain a heteroatom. R 3 When is a hydrocarbon group, it is a hydrocarbon group excluding an alkenyl group. R 3 The hydrocarbon group that can be used as R generally has 1 to 20 carbon atoms, preferably 3 to 10 carbon atoms. 3 Specific examples of the hydrocarbon group that can be used as R include linear aliphatic hydrocarbon groups such as n-propyl groups, branched aliphatic hydrocarbon groups such as i-propyl groups and t-butyl groups, alicyclic hydrocarbon groups such as cyclopentyl groups and cyclohexyl groups, and aromatic hydrocarbon groups such as phenyl groups. 3It is preferable to use a branched aliphatic hydrocarbon group or an alicyclic hydrocarbon group as the alkyl group, and it is particularly preferable to use an i-propyl group, an i-butyl group, a t-butyl group, a thexyl group, a cyclopentyl group, a cyclohexyl group, or the like. Also, R 3 When is a heteroatom-containing hydrocarbon group, the heteroatom is preferably selected from nitrogen, oxygen, sulfur, phosphorus or silicon, and is particularly preferably nitrogen or oxygen. R 3 The backbone structure of the heteroatom-containing hydrocarbon group is R 3 is a hydrocarbon group. In particular, an N,N-diethylamino group, a quinolino group, an isoquinolino group, etc. are preferred.

[0061] In addition, in the formula, R 4 represents a hydrogen atom, a halogen atom, or a hydrocarbon group which may contain a hetero atom. R 4 Examples of the halogen atom that can be used as the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Also, R 4 When is a hydrocarbon group, it is a hydrocarbon group excluding an alkenyl group. R 4 The hydrocarbon group that can be used as R generally has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms. 4 Specific examples of the hydrocarbon group that can be used as include linear aliphatic hydrocarbon groups such as methyl and ethyl groups, branched aliphatic hydrocarbon groups such as i-propyl and t-butyl groups, alicyclic hydrocarbon groups such as cyclopentyl and cyclohexyl groups, and aromatic hydrocarbon groups such as phenyl groups. Of these, it is preferable to use methyl, ethyl, propyl, i-propyl, i-butyl, s-butyl, t-butyl, thexyl, cyclopentyl, and cyclohexyl groups. Also, R 4 When R is a heteroatom-containing hydrocarbon group, R 3is a heteroatom-containing hydrocarbon group. In particular, an N,N-diethylamino group, a quinolino group, an isoquinolino group, etc. are preferred. In addition, regardless of the value of m, R 4 is R 3 may be the same as or different from.

[0062] In addition, in the formula, R 5 R represents a hydrocarbon group. 5 The hydrocarbon group that can be used as the radical generally has 1 to 20 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 5 carbon atoms. R 5 Specific examples of the hydrocarbon group that can be used as R include linear aliphatic hydrocarbon groups such as methyl and ethyl groups, and branched aliphatic hydrocarbon groups such as i-propyl and t-butyl groups. Among these, methyl and ethyl groups are most preferred. When the value of n is 2 or more, multiple R 5 may be the same or different.

[0063] Preferred examples of the alkoxysilane compound (a3) ​​that can be used in the present invention include t-butylmethyldimethoxysilane, t-butylmethyldiethoxysilane, t-butylethyldimethoxysilane, t-butyl-n-propyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylethyldimethoxysilane, dicyclopentyldimethoxysilane, diisopropyldimethoxysilane, diisobutyldimethoxysilane, isobutylisopropyldimethoxysilane, n-propylmethyldimethoxysilane, t-butyltriethoxysilane, bis(diethylamino)dimethoxysilane, diethylaminotriethoxysilanemethoxysilane, and bisperhydroisoquinolinodimethoxysilane. These alkoxysilane compounds can be used not only alone but also in combination of two or more compounds.

[0064] The amount ratio of the alkoxysilane compound (a3) ​​used may be any amount within a range that does not impair the effects of the present invention, but is generally preferably within the following range. The amount of the alkoxysilane compound (a3) ​​used is, in terms of a molar ratio to the titanium component constituting the solid component (a1) (number of moles of alkoxysilane compound (a3) / number of moles of titanium atoms in the solid component (a1)), preferably within a range of 0.01 to 1,000, particularly preferably within a range of 0.1 to 100.

[0065] The alkoxysilane compound (a3) ​​used in the present invention is thought to be coordinated in the vicinity of a titanium atom that can serve as an active site, and to control the catalytic performance such as the catalytic activity of the active site and the regularity of the polymer.

[0066] 1-4.Organoaluminum (a4) As the organoaluminum compound (a4) used in the present invention, the compounds disclosed in JP-A-2004-124090 and the like can be used. In general, it is desirable to use a compound represented by the following general formula (4). Formula (4) R 8 a AIX b (OR 9 ) c (In general formula (4), R 8 represents a hydrocarbon group having 1 to 10 carbon atoms. X represents a halogen atom or a hydrogen atom. R 9 represents a hydrocarbon group or an Al-based crosslinking group. a is a real number of 1 or more, b is a real number of 0 to 2, c is a real number of 0 to 2, and a+b+c=3.

[0067] R 8 R is a hydrocarbon group having 1 to 10 carbon atoms, preferably a hydrocarbon group having 1 to 8 carbon atoms, and more preferably a hydrocarbon group having 1 to 6 carbon atoms. 8 Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an isobutyl group, an n-hexyl group, an n-octyl group, etc. Among these, a methyl group, an ethyl group, and an isobutyl group are most preferred. X is a halogen atom or a hydrogen atom. Examples of the halogen atom that can be used as X include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Among these, chlorine is particularly preferred. R 9 R is a hydrocarbon group or a bridging group due to an aluminum atom (Al). 9 When R is a hydrocarbon group, 8 Examples of hydrocarbon groups from the same group R 9 It is also possible to use an alumoxane compound, such as methylalumoxane, as the organoaluminum compound (a4). In this case, R 9 represents a crosslinking group due to Al.

[0068] Examples of compounds that can be used as the organoaluminum compound (a4) include trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-octylaluminum, diethylaluminum chloride, ethylaluminum chloride, diethylaluminum ethoxide, and methylalumoxane. Of the organoaluminum compounds (a4), triethylaluminum and triisobutylaluminum are preferred. The organoaluminum compound (a4) may be used not only as a single compound, but also as a combination of two or more compounds.

[0069] The amount of the organoaluminum compound (a4) used may be adjusted within a range that does not impair the effects of the present invention. It can be anything, but generally it is preferred that it is within the ranges given below. The amount of the organoaluminum compound (a4) used is preferably in the range of 0.1 to 100, particularly preferably 1 to 50, in terms of the molar ratio to the titanium component constituting the solid component (a1) (the number of moles of aluminum atoms / the number of moles of titanium atoms in the solid component (a1)).

[0070] The organoaluminum compound (a4) used in the present invention is used mainly for the purpose of efficiently supporting the alkoxysilane compound (a2) in the solid catalyst component (A). Therefore, it is distinguished from the organoaluminum compound used as a cocatalyst for the polymerization reaction during the prepolymerization or main polymerization, because the main purpose is different. Note that the organoaluminum (a4) reacts with halogen and electron donor to become a reaction product.

[0071] 1-5. Preparation method of solid catalyst component (A) (Step 1) In the present invention, the solid catalyst component (A) can be prepared by contacting a solid component (a1) with a silane compound (a2) having an alkenyl group, an alkoxysilane compound (a3), and an organoaluminum compound (a4) at a predetermined temperature. In the production method of the present invention, the contact treatment may be carried out multiple times during the preparation of the solid catalyst component (A). When the contact treatment is carried out multiple times, the alkenyl group-containing silane compound (a2), the alkoxysilane compound (a3), and the organoaluminum compound (a4) used in each of the multiple contact treatments may be the same or different. The solid catalyst component (A) used in the present invention can be obtained by contacting the above-mentioned constituent components in the above-mentioned ratios. Additionally, the range of the amount of each component used was indicated above, but this is the amount used per contact. From the second time onwards, the components may be contacted any number of times as long as the amount used per contact is within the range of the amount used above.

[0072] The contact conditions of the components of the solid catalyst component (A) must be such that oxygen is not present, but any conditions can be used as long as the effects of the present invention are not impaired. In general, the following conditions are preferred. Examples of the contact method include a mechanical method using a rotary ball mill or a vibration mill, and a method of contacting by stirring in the presence of an inert diluent, etc. It is preferable to use the method of contacting by stirring in the presence of an inert diluent.

[0073] In the method for producing the solid catalyst component (A) of the present invention, the temperature for the contact treatment may be from 10°C to 60°C, and preferably from 10°C to 50°C. In preparing the solid catalyst component (A), the contents of the electron donor, the silane compound having an alkenyl group (a2) and the alkoxysilane compound (a3) ​​can be controlled by changing the temperature of the contact treatment.

[0074] In the contact treatment, any procedure can be used for contacting the solid component (a1), the silane compound (a2) having an alkenyl group, the alkoxysilane compound (a3), and the organoaluminum compound (a4). Specific examples include the following procedures (i) to (iv), among which procedures (i) and (ii) are preferred. Step (i): A method in which a solid component (a1) is contacted with a silane compound (a2) having an alkenyl group, then with an alkoxysilane compound (A3), and thereafter with an organoaluminum compound (A4). Step (ii): A method in which a solid component (a1) is contacted with a silane compound (a2) having an alkenyl group and an alkoxysilane compound (a3), and then with an organoaluminum compound (a4). Step (iii): A method in which the solid component (a1) is contacted with an alkoxysilane compound (a3), then with a silane compound (a2) having an alkenyl group, and finally with an organoaluminum compound (aA4). Procedure (iv): A method in which all compounds are contacted simultaneously.

[0075] In the preparation of the solid catalyst component (A), washing with an inert solvent may be carried out intermediately and / or finally. Preferred examples of the solvent used for washing include aliphatic hydrocarbon compounds such as heptane, aromatic hydrocarbon compounds such as toluene and xylene, and halogen-containing hydrocarbon compounds such as 1,2-dichloroethylene and chlorobenzene.

[0076] 1-6. Prepolymerization of solid catalyst component (A) The solid catalyst component (A) may be prepolymerized using a polymerization monomer in the presence of an organoaluminum compound as a reaction co-catalyst before being mixed with the organoaluminum compound (B) and the compound (C) represented by the general formula (1). By forming a small amount of polymer around the catalyst in advance prior to the polymerization process, the catalyst becomes more uniform and the amount of fine powder generated can be reduced.

[0077] As the polymerization monomer in the preliminary polymerization, compounds disclosed in JP-A-2004-124090 and the like can be used, and examples thereof include ethylene, propylene, and α-olefins having 4 to 22 carbon atoms and represented by the general formula (5) described below. When a prepolymerized solid catalyst component (A) is used, the prepolymerization can be carried out in any procedure in the preparation procedure. For example, the solid component (a1) can be prepolymerized, and then the components (a2) to (a4) can be contacted. Furthermore, when the solid component (a1) is contacted with the components (a2) to (a4), the prepolymerization can be carried out at the same time.

[0078] The reaction conditions of the solid catalyst component (A) with the above-mentioned polymerization monomers can be any conditions within the range that does not impair the effects of the present invention. Generally, the reaction conditions may be within the following ranges. The amount of the prepolymerized monomer per gram of the solid catalyst component (A) may be within a range of 0.001 g to 100 g, preferably 0.1 g to 50 g, and more preferably 0.5 g to 10 g. The reaction temperature during the preliminary polymerization is −150° C. to 150° C., and preferably 0° C. to 100° C. The reaction temperature during the preliminary polymerization may be lower than the polymerization temperature during the main polymerization. The reaction is generally preferably carried out under stirring, and an inert solvent such as hexane or heptane may be present. The prepolymerization may be carried out several times, and the monomers used for polymerization may be the same or different. After the prepolymerization, washing may be carried out with an inert solvent such as hexane or heptane.

[0079] 2. Organoaluminum Compounds (B) The organoaluminum compound (B) used in the present invention acts mainly as a promoter and also as a scavenger for removing water and other impurities from the system. As the organoaluminum compound (B) that can be used in the present invention, the compounds disclosed in JP-A-2004-124090 and the like can be used. Preferably, it can be selected from the same group as the examples of the organoaluminum compound (a4) which is a component in preparing the solid catalyst component (A).

[0080] The organoaluminum compound (B) may be the same as or different from the organoaluminum compound (a4) that can be used in preparing the solid catalyst component (A). The organoaluminum compound (B) may be used not only as a single compound, but also as a combination of two or more compounds. The amount ratio of the organoaluminum compound (B) used may be any amount within a range that does not impair the effects of the present invention, but is generally preferably within the following range. The amount of the organoaluminum compound (B) used is preferably in the range of 1 to 5,000, particularly preferably 10 to 500, in terms of the molar ratio to the titanium component constituting the solid catalyst component (A) (the number of moles of the organoaluminum compound (B) / the number of moles of titanium atoms in the solid catalyst component (A)).

[0081] 3. Compound (C) represented by general formula (1) In the present invention, a compound (C) represented by the following general formula (1) is used. Formula (1) R 1 C(O)OR 2 (In formula (1), R 1 and R 2 each independently represents a hydrocarbon group which may contain a heteroatom.

[0082] In general formula (1), R 1 and R 2each independently represents a hydrocarbon group which may contain a heteroatom. R 1 and R 2 The hydrocarbon group used as R may have 1 to 30 carbon atoms, may have 1 to 20 carbon atoms, or may have 2 to 15 carbon atoms. 1 and R 2 Specific examples of the hydrocarbon group that can be used as the alkyl group include linear aliphatic hydrocarbon groups such as an n-propyl group, branched aliphatic hydrocarbon groups such as an i-propyl group and a t-butyl group, alicyclic hydrocarbon groups such as a cyclopentyl group and a cyclohexyl group, and aromatic hydrocarbon groups such as a phenyl group. Also, R 1 and R 2 When is a hydrocarbon group containing a heteroatom, the heteroatom is desirably selected from halogen, nitrogen, oxygen, sulfur, phosphorus, or silicon atoms. The hydrocarbon group containing a heteroatom may be partially substituted with a nitrogen, oxygen, sulfur, or phosphorus atom, or the hydrocarbon group may contain a heteroatom as a substituent. Examples of the substituent containing a heteroatom include -OR a (where R a is a hydrocarbon group having 1 to 30 carbon atoms), -SR b (where R b is a hydrocarbon group having 1 to 30 carbon atoms), -N(R c )2(where R c is a hydrocarbon group having 1 to 30 carbon atoms), -Si(R d )4 (where R d R is a hydrocarbon group having 1 to 30 carbon atoms, a halogen atom, etc. a , R b , R c , and R d The hydrocarbon group having 1 to 30 carbon atoms in the formula (I) may be the same as the hydrocarbon group explained above.

[0083] R 1 As the alkyl group, it is preferable to use a linear aliphatic hydrocarbon group or an aromatic hydrocarbon group. R 1The linear aliphatic hydrocarbon group in may have 4 to 30 carbon atoms, may have 8 to 20 carbon atoms, or may have 10 to 20 carbon atoms. R 1 As the alkyl group, it is particularly preferable to use a linear aliphatic hydrocarbon group having 10 to 20 carbon atoms, a phenyl group, or a phenyl group having a substituent at the 4-position. a’ (where R a’ may be a hydrocarbon group having 1 to 6 carbon atoms), and in particular, may be an alkoxy group having 1 to 6 carbon atoms, may be an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, or an n-pentoxy group.

[0084] R 2 As the alkyl group, a linear aliphatic hydrocarbon group or a branched aliphatic hydrocarbon group is preferable, and a linear aliphatic hydrocarbon group or a branched aliphatic hydrocarbon group having 1 to 6 carbon atoms is preferable, which may be partially substituted with a halogen atom. R 2 As the alkyl group, it is particularly preferable to use a methyl group, an ethyl group, a propyl group, an i-propyl group, a butyl group, an i-butyl group, a t-butyl group, a 2,2,2-trifluoroethyl group, or the like.

[0085] Preferred examples of the compound (C) represented by general formula (1) that can be used in the present invention include isopropyl laurate, isopropyl myristate, isopropyl palmitate, 2,2,2-trifluoroethyl myristate, ethyl benzoate, ethyl 4-methylbenzoate, and ethyl 4-ethoxybenzoate. These compounds (C) represented by the general formula (1) can be used not only alone but also in combination of two or more compounds.

[0086] The amount of the compound (C) represented by the general formula (1) used in the present invention, in terms of the molar ratio to the titanium atoms in the solid catalyst component (A) (the number of moles of the compound (C) represented by the general formula (1) / the number of moles of the titanium atoms in the solid catalyst component (A)), is within a range of 100 to 100,000, preferably within a range of 500 to 50,000, and particularly preferably within a range of 1,000 to 30,000.

[0087] It is believed that the compound (C) represented by the general formula (1) used in the present invention undergoes a decomposition reaction with the organoaluminum (B) at a specific temperature or higher, generating aldehydes or ketones having small structures. At high temperatures, the decomposition reaction products of the compound (C) represented by the general formula (1) are believed to poison the active species, thereby significantly reducing the polymerization activity at high temperatures.

[0088] 4. Method for preparing propylene polymerization catalyst The propylene polymerization catalyst of the present invention is not particularly limited as long as it contains the solid catalyst component (A), the organoaluminum compound (B), and the compound (C) represented by general formula (1). The propylene polymerization catalyst of the present invention can be prepared by mixing the solid catalyst component (A), the organoaluminum compound (B), and the compound (C) represented by general formula (1). Hereinafter, the organoaluminum compound (B) may be referred to as component (B), and the compound (C) represented by general formula (1) may be referred to as component (C).

[0089] The contact conditions of the solid catalyst component (A), component (B) and component (C) must be such that oxygen is not present in the presence of α-olefin, but any conditions can be used as long as they do not impair the effects of the present invention. In general, the following conditions are preferred. Specific examples include the following steps (i) to (ii). Step (i): A method in which component (B) and component (C) are simultaneously contacted in the presence of an α-olefin in an apparatus having a stirring function and a temperature control function, and then a solid catalyst component (A) is contacted therewith. Step (ii): A method in which all compounds are simultaneously contacted in an apparatus having a stirring function and a temperature control function. The contact temperature can be exemplified by the polymerization temperature of α-olefins described later. The apparatus having a stirring function and a temperature control function can be a conventionally known apparatus.

[0090] II. Method for producing α-olefin polymers The process for producing an α-olefin polymer of the present invention is characterized in that an α-olefin is homopolymerized or copolymerized in the presence of the propylene polymerization catalyst of the present invention. The process for producing an α-olefin polymer of the present invention may be carried out by contacting the above solid catalyst component (A), the above component (B) and the above component (C) in the presence of an α-olefin. The solid catalyst component (A), the component (B) and the component (C) are contacted in the presence of an α-olefin to obtain a propylene polymerization catalyst, and an α-olefin polymer is produced by homopolymerizing or copolymerizing an α-olefin in the presence of the propylene polymerization catalyst.

[0091] 1. α-Olefins The α-olefins used in the present invention include ethylene, propylene, α-olefins having 4 to 22 carbon atoms represented by the following general formula (5), dienes, and styrenes, and may contain at least propylene. Formula (5) R 10 -CH=CH2 (In general formula (c), R 10 is a hydrocarbon group having 2 to 20 carbon atoms, which may have a branched group.)

[0092] Examples of α-olefins having 4 to 22 carbon atoms include butene-1, pentene-1, and hexene. -1, 4-methylpentene-1, etc. The α-olefin used in the polymerization in the present invention is preferably propylene, and may be only propylene, or a combination of two types of propylene and ethylene, or a combination of two or more types of propylene and an α-olefin having 4 to 22 carbon atoms and represented by the above general formula (5).

[0093] 2. α-Olefin Polymerization The polymerization of α-olefins may be carried out by slurry polymerization using a hydrocarbon solvent, liquid phase solventless polymerization substantially without a solvent, or gas phase polymerization, etc. In the case of slurry polymerization, a hydrocarbon solvent such as pentane, hexane, heptane, or cyclohexane is used as the polymerization solvent. The polymerization method employed may be any method such as continuous polymerization, batch polymerization or multi-stage polymerization. The polymerization temperature is usually about 30° C. to 200° C., preferably 50° C. to 150° C., and hydrogen may be used as a molecular weight regulator.

[0094] It is also possible to carry out block copolymerization in which an α-olefin, preferably propylene, is homopolymerized in the first stage and then randomly copolymerized in the second stage. The copolymerizable monomer can be used in an amount of up to 15% by mass in random copolymerization and up to 50% by mass in block copolymerization. Among them, homopolymerization and block copolymerization of propylene are preferred, and homopolymerization of propylene and block copolymerization in which the first stage is homopolymerization of propylene are most preferred.

[0095] 3. Propylene-based polymers The index of the propylene-based polymer polymerized according to the present invention is not particularly limited, and can be appropriately adjusted according to various applications. The MFR of the propylene polymer is preferably within the range of 0.01 g / 10 min to 10,000 g / 10 min, and particularly preferably within the range of 0.1 g / 10 min to 1,000 g / 10 min. EXAMPLES

[0096] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples. The methods for measuring the various physical properties in the present invention are shown below.

[0097] (1) Titanium content: The sample was accurately weighed, hydrolyzed, and measured by colorimetry. For samples after prepolymerization, the titanium content was calculated using the weight excluding the prepolymerized polymer. (2) Alkoxysilane compound content: The sample was accurately weighed and decomposed with methanol. The concentration of silicon compounds in the resulting methanol solution was determined by comparing with a standard sample using gas chromatography. The content of silicon compounds contained in the sample was calculated from the concentration of silicon compounds in methanol and the weight of the sample. For samples after prepolymerization, the content was calculated using the weight excluding the prepolymerized polymer. (3) MFR: Using a melt indexer manufactured by Takara Corporation, evaluation was performed under conditions of 230°C and 21.18N based on JIS-K6921.

[0098] All of the following operations were carried out under a nitrogen atmosphere. The abbreviations shown below are as follows: Me: methyl, Et: ethyl, i-Pr: isopropyl

[0099] Example 1 [Preparation of solid catalyst component (A)] A 10L autoclave equipped with a stirrer was thoroughly purged with nitrogen, and 2L of purified toluene was introduced. 200g of Mg(OEt)2 and 1L of TiCl4 were added to the autoclave at room temperature. The temperature was raised to 90°C, and 50ml of di-n-butyl phthalate was introduced. The temperature was then raised to 110°C, and contact treatment was carried out for 3 hours. The reaction product was thoroughly washed with purified toluene. Next, refined toluene was introduced to adjust the total liquid volume to 2 L. 1 L of TiCl4 was added at room temperature, and the temperature was raised to 110°C for 2 hours for contact treatment. The reaction product was thoroughly washed with refined toluene. Furthermore, the toluene was replaced with n-heptane using purified n-heptane to obtain a slurry of solid component (a1). A part of this slurry was sampled and dried. Analysis revealed that the Ti content of solid component (a1) was 2.7% by weight.

[0100] Next, a 20 L autoclave equipped with a stirrer was thoroughly purged with nitrogen, and 100 g of the slurry of the solid component (a1) was introduced as the solid component (a1). Purified n-heptane was introduced to adjust the concentration of the solid component (a1) to 25 g / L. 50 ml of SiCl4 was added thereto, and contact treatment was carried out at 90°C for 1 hour. The reaction product was thoroughly washed with purified n-heptane. After that, refined n-heptane was introduced to adjust the liquid level to 4 L. 30 ml of dimethyldivinylsilane as component (a2), 30 ml of (i-Pr)2Si(OMe)2 as component (a3), and 80 g of n-heptane diluted triethylaluminum (Et3Al) as component (a4) were added, and contact treatment was carried out at 40°C for 2 hours. The reaction product was thoroughly washed with refined n-heptane, and a part of the obtained slurry was sampled and dried. Analysis showed that the solid components contained 1.2 wt% Ti and 8.8 wt% (i-Pr)2Si(OMe)2.

[0101] [Prepolymerization] The solid catalyst component obtained above was used to carry out preliminary polymerization according to the following procedure. Purified n-heptane was introduced into the above slurry to adjust the concentration of the solid component to 20 g / L. After cooling the slurry to 10°C, 10 g of Et3Al diluted in n-heptane was added as Et3Al, and 210 g of propylene was fed over 4 hours. After the propylene feed was completed, the reaction was continued for another 30 minutes. Next, the gas phase was thoroughly replaced with nitrogen, and the reaction product was thoroughly washed with purified n-heptane. The resulting slurry was removed from the autoclave and vacuum dried to obtain solid catalyst component (A). This solid catalyst component (A) contained 2.0 g of polypropylene per 1 g of solid component. Analysis revealed that the portion of this solid catalyst component (A) excluding polypropylene contained 1.0 wt% Ti and 8.2 wt% (i-Pr)2Si(OMe)2.

[0102] [Polymerization of propylene] A 2.4L stainless steel autoclave equipped with stirring and temperature control was heated and dried under a nitrogen atmosphere and cooled to room temperature. 1.0L of heptane was introduced therein, then 400mg of Et3Al as an organoaluminum compound (B) and 1150ml of hydrogen were introduced, and the internal temperature was adjusted to 70°C. Then, propylene was introduced up to 0.70MPa, and 522mg of isopropyl myristate as compound (C) and 1.0mg of the above solid catalyst component (A) were pressed in. Polymerization was carried out by continuously introducing propylene so that the pressure during polymerization was 0.70MPa. After 1 hour, the introduction of propylene was stopped, and 10ml of ethanol was pressed in to stop the polymerization. In addition, polymerization was carried out by the same operation method, with the internal temperature set to 100°C and 120°C. At this time, polymerization was carried out under the conditions of Table 1 so that the same concentrations of hydrogen and propylene in heptane were obtained. The results are shown in Table 2.

[0103] [Table 1]

[0104] Example 2 Except for using 697 mg of isopropyl myristate as compound (C), propylene polymerization was carried out in the same manner as in Example 1. The results are shown in Table 2.

[0105] Example 3 Propylene polymerization was carried out in the same manner as in Example 1, except that 125 mg of ethyl 4-ethoxybenzoate was used as compound (C) instead of isopropyl myristate. The results are shown in Table 2.

[0106] Comparative Example 1 Propylene polymerization was carried out in the same manner as in Example 1, except that compound (C) was not used. The results are shown in Table 2.

[0107] Comparative Example 2 [Prepolymerization] The slurry of the solid component (a1) obtained in Example 1 was used as the solid component in an amount of 100 g, and preliminary polymerization was carried out according to the following procedure. Purified n-heptane was introduced into the above slurry to adjust the concentration of the solid component to 20 g / L. After cooling the slurry to 10°C, 10 g of Et3Al diluted in n-heptane was added as Et3Al, and 210 g of propylene was fed over 4 hours. After the propylene feed was completed, the reaction was continued for another 30 minutes. Next, the gas phase was thoroughly replaced with nitrogen, and the reaction product was thoroughly washed with purified n-heptane. The resulting slurry was removed from the autoclave and vacuum dried to obtain a solid catalyst component (Ac1). This solid catalyst component (Ac1) contained 2.0 g of polypropylene per 1 g of solid component. Analysis revealed that the portion of this solid catalyst component (Ac1) excluding polypropylene contained 2.2 wt % Ti. [Polymerization of propylene] Propylene polymerization was carried out in the same manner as in Example 1, except that the solid catalyst component (Ac1) obtained above was used instead of the solid catalyst component (A) in Example 1. The results are shown in Table 2.

[0108] Comparative Example 3 Propylene polymerization was carried out in the same manner as in Comparative Example 2, except that compound (C) was not used. The results are shown in Table 2.

[0109] [Table 2]

[0110] FIG. 1 shows a graph in which activity is plotted against polymerization temperature for Examples 1 to 3 and Comparative Example 1. FIG. 2 shows a graph in which the MFR is plotted against the polymerization temperature for each of the Examples and Comparative Examples.

[0111] (Explanation of Examples and Comparative Examples) As is clear from Table 2, when the Examples and Comparative Examples are compared, the catalyst of the present invention exhibits a marked decrease in polymerization activity at high temperatures, and can reduce the range of change in MFR of the resulting polymer with respect to temperature. Specifically, when Examples 1 to 3 are compared with Comparative Example 1 (FIG. 1), it is found that the catalyst containing compound (C) has a significantly reduced polymerization activity at 100° C. and 120° C. In this way, the catalyst containing compound (C) is deactivated when the polymerization temperature rises locally, and as a result, it is considered that the catalyst is less likely to affect the plant operation performance due to the generation of lumps or fouling. In addition, when Examples 1 to 3 are compared with Comparative Examples 2 and 3 (FIG. 2), it is found that the use of solid catalyst component (A1) obtained by contact treatment of components (a2), (a3) ​​and (a4) results in a small change in MFR under high-temperature polymerization. This suggests that the effect on the physical properties of the resulting polymer is small. Therefore, the catalysts in the examples of the present invention are catalysts that exhibit a significant decrease in polymerization activity at high temperatures and can reduce the range of change in MFR of propylene-based polymers during high-temperature polymerization, and thus can be said to have achieved superior results to the comparative examples. Incidentally, it was not previously known that the use of the solid catalyst component (A1) obtained by contact treatment of the components (a2), (a3) ​​and (a4) reduces the change in MFR during high-temperature polymerization, and this effect has become evident in the present invention. [Industrial Applicability]

[0112] According to the present invention, a propylene polymerization catalyst is used which exhibits a significant decrease in polymerization activity at high temperatures and can reduce the variation in molecular weight (MFR) of the resulting polymer with respect to temperature. This makes it possible to produce a propylene polymer while suppressing the influence on the plant operation performance due to the generation of lumps and fouling, and also has little effect on the physical properties of the resulting polymer, and thus has high industrial applicability.

Claims

1. A propylene polymerization catalyst comprising: a solid catalyst component (A) obtained by contact-treating the following component (a1) with components (a2), (a3) ​​and (a4); an organoaluminum compound (B); and a compound (C) represented by the following general formula (1): Component (a1): A solid component containing titanium, magnesium, a halogen, and an electron donor. Component (a2): Silane compound having an alkenyl group Component (a3): Alkoxysilane compound [however, different from a silane compound having an alkenyl group] Component (a4): Organoaluminum compound Formula (1) R 1 C(O)OR 2 (In formula (1), R 1 and R 2 each independently represents a hydrocarbon group which may contain a heteroatom.

2. The propylene polymerization catalyst according to claim 1, wherein the amount of the compound (C) used is, in terms of a molar ratio to the organoaluminum compound (B) (the number of moles of the compound (C) / the number of moles of the organoaluminum compound (B)), 0.05 to 2.

0.

3. The propylene polymerization catalyst according to claim 1, wherein the component (a2) is a compound represented by the following general formula (3): Formula (3) SiR 6 n R 7 4-n (In formula (3), R 6 represents an alkenyl group. R 7 represents a hydrogen atom, a halogen atom or an alkyl group. n is 1, 2, 3, or 4; when n is 1 or 2, R 7 They may be linked to each other to form a ring structure.)

4. The propylene polymerization catalyst according to claim 1, wherein the component (a3) ​​is a compound represented by the following general formula (2): Formula (2) R 3 R 4 m Si(OR 5 ) n (In formula (2), R 3 represents a hydrocarbon group which may contain a hetero atom. R 4 represents a hydrogen atom, a halogen atom, or a hydrocarbon group which may contain a hetero atom. R 5 represents a hydrocarbon group. m is 0, 1 or 2, n is 1, 2 or 3, and m+n=3 is satisfied.

5. A method for producing a propylene-based polymer, comprising homopolymerizing or copolymerizing propylene in the presence of the propylene polymerization catalyst according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Catalytic component for olefin polymerization

    JP1986285203A

  • Production of olefinic polymer

    JP1987011706A

  • Production of alpha-olefin polymer

    JP1991234707A

  • CATALYST FOR alpha-OLEFIN POLYMERIZATION AND METHOD FOR PRODUCING alpha-OLEFIN POLYMER BY USING THE SAME

    JP2003292523A

  • Solid catalyst component, catalyst for olefin polymerization, and method for producing olefin polymer or copolymer

    JP2006169283A