Manufacturing method of laminate, and manufacturing method of one side and both sides flexible metal-clad laminate
By using adhesive sheets with a three-layer structure and silane coupling agent treatment, the method addresses the challenge of producing thick insulating layers in metal-clad laminates, improving adhesion and enabling advanced electronic components.
Patent Information
- Application Number
- JP2023044898
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods struggle to produce a metal-clad laminate with a thick insulating layer, as conventional adhesive sheets are limited to 50 μm or less, and bonding multiple sheets results in poor adhesion, making it difficult to manufacture thicker laminates suitable for advanced electronic components.
A method involving adhesive sheets with a three-layer structure, comprising a heat-resistant film and thermoplastic resin layers on both sides, treated with a silane coupling agent to enhance adhesion, allowing for laminates with a thickness of 51 μm or more, which are then bonded using thermocompression techniques.
The method improves adhesion strength and enables the production of single-sided or double-sided flexible metal-clad laminates with thick insulating layers, enhancing the quality and functionality of electronic components.
Smart Images

Figure 2024134620000002 
Figure 2024134620000003 
Figure 2024134620000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a laminate and a method for producing a single-sided and double-sided flexible metal-clad laminate. [Background technology]
[0002] In recent years, electronic devices have rapidly become more powerful, more functional, and more compact, and this has led to a growing demand for smaller and thinner electronic components used in electronic devices. In addition, costs have been reduced, and the materials that make up FPCs have become more diverse in response to these demands. Meanwhile, technical fields that require thicker FPCs to ensure a wide range of functions are also becoming evident.
[0003] Conventionally, as a metal-clad laminate suitable for a printed circuit board for electronic and electrical devices, a double-sided flexible metal-clad laminate having a structure in which metal foil is laminated on both sides of a polyimide film has been known. As a method for producing a double-sided flexible metal-clad laminate having such a structure, a method has been proposed in which a polyimide film and a metal foil are thermocompression-bonded (hereinafter also referred to as thermal lamination) at high temperature between a pair of metal rolls with a protective film interposed therebetween (for example, Patent Document 1).
[0004] Incidentally, the polyimide film used as described above is often an adhesive sheet having a structure in which a non-thermoplastic polyimide layer serves as a core layer (heat-resistant film) and thermoplastic polyimide layers are disposed on both the front and back sides of the core layer.
[0005] However, for example, the adhesive sheet is generally no greater than 50 μm, and when producing a metal-clad laminate with a thick insulating layer, it is necessary to stack multiple adhesive sheets to form a multi-layer structure.
[0006] When manufacturing such thick double-sided flexible metal-clad laminates by methods such as thermocompression bonding, unlike thin double-sided flexible metal-clad laminates, it is necessary to stack multiple adhesive sheets, and for example, a technique for bonding single-sided flexible metal-clad laminates has been introduced (for example, Patent Document 2). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2001-129918 A [Patent Document 2] JP 2014-195947 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, Patent Document 2 only discloses an insulating layer containing polyimide having a thickness of 50 μm or less. Furthermore, since the method for forming the adhesive sheet employs a method of coating (also called casting) a polyimide precursor solution onto a metal foil, there is a problem that the method cannot be implemented by manufacturers of metal-clad laminates that do not have a coating device (casting device). Furthermore, since it is a coating method, it is difficult to manufacture an insulating layer that is thicker than 50 μm.
[0009] Furthermore, when a metal-clad laminate is manufactured using a plurality of commonly available adhesive sheets, the adhesive sheets do not adhere to each other well, which creates quality issues.
[0010] The present invention has been made in view of the above-mentioned problems, and its object is to provide a method for manufacturing a generally available The present invention provides a method for producing a laminate having a thick insulating layer by laminating a plurality of adhesive sheets, and a method for producing a single-sided or double-sided flexible metal-clad laminate using the laminate. [Means for solving the problem]
[0011] As a result of extensive research to solve the above-mentioned problems, the inventors discovered that the following method can be used to obtain a laminate having the desired thick insulating layer, and a single-sided or double-sided flexible metal-clad laminate using said laminate, thereby completing the present invention.
[0012] 1) At least two adhesive sheets having a three-layer structure including a heat-resistant film containing at least a polyimide film and a thermoplastic resin layer laminated on each side of the heat-resistant film are laminated together, and the thickness of the laminated sheet is 51 μm or more; A method for producing a laminate, comprising the steps of: applying a surface treatment agent to at least one of the surfaces of the adhesive sheet to be laminated when the adhesive sheets are laminated; and drying the surface treatment agent.
[0013] 2) The method for producing a laminate according to 1), wherein the surface treatment agent is a silane coupling agent having a trifunctional alkoxyl group or a difunctional alkoxyl group.
[0014] 3) A method for producing a single-sided flexible metal-clad laminate, comprising laminating a metal foil and a laminate having a thickness of 51 μm or more, in which two or more adhesive sheets are laminated together, or laminating a metal foil and two or more adhesive sheets together, the adhesive sheet has a three-layer structure including a heat-resistant film including at least a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film, The thickness after lamination of the adhesive sheet is 51 μm or more, A method for producing a single-sided flexible metal-clad laminate, characterized in that at least one of the surfaces where the adhesive sheets are to be laminated together during lamination is subjected to a surface treatment by applying a surface treatment agent and drying it.
[0015] 4) The method for producing a single-sided flexible metal-clad laminate according to 3), wherein the surface treatment agent is a silane coupling agent having a trifunctional alkoxyl group or a difunctional alkoxyl group.
[0016] 5) A method for producing a double-sided flexible metal-clad laminate, comprising laminating a metal foil, a laminate having a thickness of 51 μm or more obtained by laminating two or more adhesive sheets, and a metal foil, or laminating a metal foil, two or more adhesive sheets, and a metal foil, the adhesive sheet has a three-layer structure including a heat-resistant film including at least a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film, The thickness after lamination of the adhesive sheet is 51 μm or more, A method for producing a double-sided flexible metal-clad laminate, characterized in that at least one of the surfaces to be laminated with the adhesive sheets during lamination is subjected to a surface treatment by coating and drying a surface treatment agent.
[0017] 6) The method for producing a double-sided flexible metal-clad laminate according to 5), wherein the surface treatment agent is a silane coupling agent having a trifunctional alkoxyl group or a difunctional alkoxyl group.
[0018] 7) A method for producing a double-sided flexible metal-clad laminate having a microstrip line structure, comprising forming the double-sided flexible metal-clad laminate described in 5) or 6) into a microstrip line structure, the total thickness of the two or more overlapping adhesive layers being 75 to 200 μm. Effect of the Invention
[0019] According to the present invention, by applying a surface treatment agent in advance to one or both sides of a commonly available heat-resistant adhesive sheet and drying it, it is possible to improve the adhesion through chemical bonding, and by bonding at least two or more adhesive sheets together, it is possible to provide a method for producing a laminate with a thick insulating layer, and a method for producing a single-sided or double-sided flexible metal-clad laminate using the laminate. [Brief description of the drawings]
[0020] [Figure 1]1 is a schematic diagram of a cross section of a double-sided flexible metal-clad laminate having a microstrip line structure. [Diagram 2] 1 is a schematic diagram of a cross section of a multilayer flexible metal-clad laminate having a stripline structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to these embodiments, and various modifications can be made within the scope of the description.
[0022] Unless otherwise specified in this specification, "A to B" expressing a numerical range means "A or more (including and greater than A) to B or less (including and smaller than B)."
[0023] The method for producing a laminate of the present invention is characterized in that at least two or more adhesive sheets having a three-layer structure including at least a heat-resistant film containing a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film are laminated together, the laminate has a thickness of 51 μm or more after lamination, and at least one of the surfaces to be laminated with the adhesive sheet during lamination is surface-treated by applying and drying a surface treatment agent.
[0024] <Heat-resistant film (A)> In the present invention, "heat resistance" means that it can withstand use at the heating temperature during thermal lamination. Therefore, the heat-resistant film (A) is not particularly limited as long as it satisfies the above-mentioned properties, and various known films such as polyimide films and polyethylene naphthalate films can be used. Among them, heat-resistant polyimide films are preferable because they are excellent not only in heat resistance but also in physical properties such as electrical properties.
[0025] The "heat-resistant polyimide film" may be formed containing 90% by weight or more of non-thermoplastic polyimide, and the molecular structure and thickness of the non-thermoplastic polyimide are not particularly limited. The non-thermoplastic polyimide used in forming the heat-resistant polyimide film is generally produced using polyamic acid (also called polyamic acid) as a precursor. Here, non-thermoplastic polyimide generally refers to polyimide that does not soften or exhibit adhesiveness even when heated. In the present invention, it refers to polyimide that maintains a film shape (flat film shape) when fixed in a film state to a metal fixing frame and heated at a heating temperature of 380°C for 1 minute, or polyimide that does not substantially have a glass transition temperature. The glass transition temperature can be determined from the inflection point value of the storage modulus measured by a dynamic viscoelasticity measuring device (DMA). In addition, "substantially does not have a glass transition temperature" refers to one that starts thermal decomposition before reaching a glass transition state.
[0026] Generally, polyimide films can be produced using polyamic acid as a precursor. Any known method can be used to produce polyamic acid. Usually, polyamic acid can be produced by dissolving substantially equimolar amounts of aromatic tetracarboxylic dianhydride and aromatic diamine in an organic solvent and stirring the mixture under controlled temperature conditions until the polymerization of the aromatic tetracarboxylic dianhydride and aromatic diamine is completed. These polyamic acid solutions are usually obtained at a concentration of 5 to 35% by weight, preferably 10 to 30% by weight. When the concentration is within this range, suitable molecular weight and solution viscosity can be obtained.
[0027] As the polymerization method, any known method or a combination of these methods can be used. The characteristic of the polymerization method in the polymerization of polyamic acid is the order of addition of the monomers, and by controlling the order of addition of the monomers, the physical properties of the resulting polyimide can be controlled. Therefore, in the present invention, any method of adding monomers can be used for the polymerization of polyamic acid.
[0028] Representative polymerization methods include the following. 1) A method in which an aromatic diamine is dissolved in an organic polar solvent and reacted with an aromatic tetracarboxylic dianhydride in a substantially equimolar amount to polymerize the resulting solution. 2) A method in which an aromatic tetracarboxylic dianhydride is reacted with an aromatic diamine compound in a molar amount smaller than that of the aromatic tetracarboxylic dianhydride in an organic polar solvent to obtain a prepolymer having acid anhydride groups at both ends, and then polymerized using an aromatic diamine compound so that the aromatic tetracarboxylic dianhydride and the aromatic diamine compound are substantially equimolar in all steps. 3) A method in which an aromatic tetracarboxylic dianhydride is reacted with an excess molar amount of an aromatic diamine compound in an organic polar solvent to obtain a prepolymer having amino groups at both ends, and then the prepolymer is polymerized using an aromatic tetracarboxylic dianhydride such that the aromatic tetracarboxylic dianhydride and the aromatic diamine compound are substantially equimolar in all steps. 4) A method in which an aromatic tetracarboxylic dianhydride is dissolved and / or dispersed in an organic polar solvent, and then polymerized using an aromatic diamine compound in a substantially equimolar amount. 5) A method of polymerizing a mixture of substantially equimolar amounts of an aromatic tetracarboxylic dianhydride and an aromatic diamine by reacting them in an organic polar solvent. These methods may be used alone or in partial combination.
[0029] In the present invention, a polyamic acid obtained by any of the above polymerization methods may be used, and the polymerization method is not particularly limited.
[0030] Examples of the aromatic diamine include, but are not limited to, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 2,2-bis{4-(4-aminophenoxy)phenyl}propane, 2,2-bis{4-(4-aminophenoxy)phenyl}hexafluoropropane, bis{4-(3-aminophenoxy)phenyl}sulfone, bis{4-(4-aminophenoxy)phenyl}sulfone, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, Examples of the amines include 1,4-diaminobenzene (p-phenylenediamine), 1,3-diaminobenzene (m-phenylenediamine), 4,4'-diaminodiphenylsulfone, 3,3'-diaminodiphenylsulfone, 9,9-bis(4-aminophenyl)fluorene, 4,4'-(1,4-phenylenebis(1-methylethylidene))bisaniline, 4,4'-(1,3-phenylenebis(1-methylethylidene))bisaniline, 4,4'-diaminobenzanilide, and the like, or a combination of two or more of these.
[0031] In addition, examples of the aromatic tetracarboxylic dianhydride include, but are not limited to, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 2,2',3,3'-benzophenone tetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, 3,4'-oxyphthalic dianhydride, ethylene bis(trimellitic monoester acid anhydride), bisphenol A bis(trimellitic monoester acid anhydride), pyromellitic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride, 3,3',4, Examples of the aromatic tetracarboxylic acid dianhydride include 4'-dimethyldiphenylsilane tetracarboxylic acid dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic acid dianhydride, 1,2,3,4-furan tetracarboxylic acid dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 4,4'-hexafluoroisopropylidenediphthalic anhydride, 3,3',4,4'-biphenyl tetracarboxylic acid dianhydride, 2,3,3',4'-biphenyl tetracarboxylic acid dianhydride, p-phenylene bis(trimellitic acid monoester anhydride), p-phenylene diphthalic anhydride, and the like, and combinations of two or more of these.
[0032] The aromatic diamine and the aromatic tetracarboxylic dianhydride may be reacted in substantially equimolar amounts, and the order of addition, combination of monomers, and composition are not particularly limited.
[0033] The organic solvent used as the polymerization solvent for producing polyamic acid is not particularly limited as long as it dissolves aromatic diamine, aromatic tetracarboxylic dianhydride, and the resulting polyamic acid. As the polymerization solvent, for example, amide solvents such as N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone are preferable, and by using these, the resulting organic solvent solution of polyamic acid (polyamic acid solution) can be used as it is to prepare a resin solution.
[0034] The reaction temperature for producing polyamic acid is preferably -10°C to 50°C. By controlling the temperature within this range, the reaction proceeds at a good reaction rate, and the productivity is excellent, which is preferable. The reaction time is not particularly limited, but is usually several minutes to several hours.
[0035] In the present invention, the curing agent includes at least one of a dehydrating agent and a catalyst. The dehydrating agent is not particularly limited as long as it can dehydrate the polyamic acid by dehydration ring closure, but examples thereof include aliphatic acid anhydrides, aromatic acid anhydrides, N,N'-dialkylcarbodiimides, lower aliphatic halides, halogenated lower aliphatic acid anhydrides, arylsulfonic acid dihalides, and thionyl halides. These may be used alone or in combination of two or more. Among these, aliphatic acid anhydrides and aromatic acid anhydrides are particularly suitable.
[0036] The catalyst is not particularly limited as long as it is a component that has the effect of promoting the dehydration ring-closing action of the dehydrating agent on the polyamic acid. Specific examples of the catalyst include aliphatic tertiary amines, aromatic tertiary amines, and heterocyclic tertiary amines.
[0037] A filler can be added to the heat-resistant film (A) for the purpose of improving various film properties such as sliding properties, thermal conductivity, electrical conductivity, corona resistance, loop stiffness, etc. Any filler may be used, but preferred examples include silica, titanium oxide, alumina, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc.
[0038] <Thermoplastic resin layer (B)> In the present invention, examples of the thermoplastic resin layer (B) include polycarbonate resins, acrylonitrile-styrene copolymer resins, and thermoplastic polyimide resins, but from the viewpoint of heat resistance, thermoplastic polyimide resins are particularly preferred. The content, molecular structure, and thickness of the thermoplastic polyimide resin contained in the layer are not particularly limited as long as the desired characteristics, such as significant adhesive strength with the metal foil and a suitable linear expansion coefficient, are expressed. However, in order to express the desired characteristics, such as significant adhesive strength and a suitable linear expansion coefficient, it is preferable that the thermoplastic polyimide resin is substantially contained in the thermoplastic resin layer (B) at 50% by weight or more. Furthermore, it is preferable that the thermoplastic polyimide resin contained in the thermoplastic resin layer (B) facing the heat-resistant film is the same type from the viewpoint of the balance of the linear expansion coefficient in the entire adhesive sheet and the simplification of the manufacturing process.
[0039] As the thermoplastic polyimide resin contained in the thermoplastic resin layer (B), for example, a thermoplastic polyamideimide, a thermoplastic polyetherimide, a thermoplastic polyesterimide, etc. can be suitably used.
[0040] The thermoplastic polyimide contained in the thermoplastic resin layer (B) can be obtained by a conversion reaction from its precursor, polyamic acid. As a method for producing the polyamic acid, any known method can be used, as in the case of the precursor of the non-thermoplastic polyimide resin that can be used in the heat-resistant film (A).
[0041] From the viewpoints of exhibiting significant adhesive strength with the metal foil (D) and not impairing the heat resistance of the resulting double-sided flexible metal-clad laminate (G), the thermoplastic polyimide resin used in the present invention preferably has a glass transition temperature (Tg) in the range of 150° C. to 300° C. Note that Tg can be determined from the inflection point value of the storage modulus measured by a dynamic viscoelasticity measuring device (DMA).
[0042] The polyamic acid precursor of the thermoplastic polyimide that can be used in the present invention is not particularly limited, and any known polyamic acid can be used. The polyamic acid solution can also be produced by appropriately selecting the above-mentioned raw materials and production conditions.
[0043] The properties of thermoplastic polyimides can be adjusted by combining various raw materials such as aromatic tetracarboxylic dianhydrides and aromatic diamines, but generally, when the ratio of aromatic diamines having a rigid structure is increased, the glass transition temperature increases, the storage modulus during heating increases, and adhesiveness and processability may decrease. For example, the ratio of aromatic diamines having a rigid structure to the total amount of aromatic diamines is preferably 40 mol% or less, more preferably 30 mol% or less, and particularly preferably 20 mol% or less.
[0044] Specific examples of preferred thermoplastic polyimide resins include aromatic diamines and aromatic tetracarboxylic dianhydrides that can be used in the above-mentioned heat-resistant polyimide film, and more preferably, those obtained by polymerizing an acid dianhydride such as benzophenone tetracarboxylic dianhydride, biphenyl tetracarboxylic dianhydride, oxydiphthalic dianhydride, or biphenyl sulfone tetracarboxylic dianhydride with an aromatic diamine having an aminophenoxy group.
[0045] Furthermore, for the purpose of controlling the slipperiness of the adhesive sheet according to the present invention, inorganic or organic fillers and further other resins may be added as necessary.
[0046] <Adhesive sheet (C)> The adhesive sheet (C) in the present invention is a heat-resistant film (A) having a thermoplastic resin on at least one side thereof. There are no particular limitations as long as the conductive resin layer (B) is included.
[0047] The thickness configuration of each layer of the heat-resistant film (A) and the thermoplastic resin layer (B) of the adhesive sheet (C) in the present invention may be appropriately adjusted so that the total thickness is appropriate for the application. For example, it is preferable to adjust the thickness balance of each thermoplastic resin layer (B) while considering the linear expansion coefficient of each layer so that the adhesive sheet (C) does not warp. When the difference in the linear expansion coefficient of the thermoplastic resin layer (B) facing each other through the heat-resistant film (A) is small, it is easy to achieve a thickness balance. In addition, the total thickness of the adhesive sheet (C) is preferably 5 μm to 50 μm, more preferably 25 μm to 50 μm. If it is within this range, it can be suitably used as a substrate for FPC.
[0048] As the adhesive sheet (C) in the present invention, PIXIO (registered trademark) manufactured by Kaneka Corporation can also be used.
[0049] <Method of manufacturing adhesive sheet (C)> The manufacturing method of the adhesive sheet (C) according to the present invention is not particularly limited, but in the case of an adhesive sheet (C) having a three-layer structure, examples thereof include a method of forming a thermoplastic resin layer (B) on each side of a heat-resistant film (A) that is to be a core layer, or a method of forming the thermoplastic resin layer (B) into a sheet shape and laminating it on the surface of the heat-resistant film (A) that is to be the core layer, etc. Alternatively, the adhesive sheet (C) may be produced by co-extruding the heat-resistant film (A) that is to be a core layer and the thermoplastic resin layer (B) to produce a laminate in substantially one step (also called a co-extrusion film-forming method).
[0050] In addition, for example, when a thermoplastic polyimide resin is used for the thermoplastic resin layer (B), a resin solution obtained by dissolving or dispersing a thermoplastic polyimide resin or a resin composition containing the same in an organic solvent may be applied to the surface of the heat-resistant film (A), or a solution of polyamic acid, which is a precursor of thermoplastic polyimide, may be prepared and applied to the surface of the heat-resistant film, followed by imidization. The conditions for synthesizing polyamic acid and imidizing polyamic acid at this time are not particularly limited, but conventionally known raw materials and conditions can be used. When baking polyamic acid, excessive overheating can reduce tackiness, but problems such as increased moisture absorption and film deterioration may occur. In addition, the polyamic acid solution may contain, for example, a coupling agent, depending on the application.
[0051] <Manufacturing method for laminates with two or more adhesive sheets> The method for producing a laminate of the present invention is characterized in that at least two or more heat-resistant films including at least a polyimide film and an adhesive sheet having a three-layer structure including a thermoplastic resin layer laminated on each of both sides of the heat-resistant film are bonded together, the thickness of the laminate after bonding is 51 μm or more, and at least one of the surfaces of the adhesive sheets to be bonded together during bonding is surface-treated by applying and drying a surface treatment agent.
[0052] The present invention is characterized in that at least one of the surfaces to be bonded to the adhesive sheet is coated with a surface treatment agent and dried to perform a surface treatment. The surface treatment will be described below. Examples of methods for performing surface treatment by coating and drying a surface treatment agent include a method in which a coupling agent is coated directly or diluted with a solvent on a support and / or a polyimide film, dried, and heat-treated; a method in which a support and / or a polyimide film is immersed in a solution of the coupling agent itself or diluted with a solvent, and then dried and heat-treated; A method can be adopted in which the coupling agent is added when the polyimide film is produced, and the coupling agent is treated at the same time as the polyimide film is produced.
[0053] The solvent for diluting the coupling agent may be any solvent that can be made into a homogeneous solution, such as water or alcohol, and among alcohol solvents, it is preferable to use a solvent that is easy to handle when handling the silane coupling agent, such as methanol, ethanol, or 2-propanol. The concentration of the diluted solution of the silane coupling agent is not limited as long as it is easy to handle in the process of applying and drying, but it is preferably 0.01 to 30% by weight, and more preferably 1 to 10% by weight in consideration of increasing the adhesive strength between the laminated films.
[0054] A conventionally known coating method may be used as a method for applying the coupling agent or its diluted solution. For example, a method of printing the entire surface of the coupling agent or its diluted solution by inkjet printing, or a method using other existing printing methods may be used. The amount of the coupling agent applied (adhesion amount or content) and the film thickness of the coupling treatment layer to be formed may be appropriately set. The conditions for the heat treatment are preferably 50 to 250°C, more preferably 75 to 165°C, and even more preferably about 95 to 155°C, and preferably 30 seconds or more, more preferably 2 minutes or more, and even more preferably 5 minutes or more. If the heating temperature is too high, the coupling agent may be decomposed or inactivated, and if it is too low, the fixing may be insufficient. In addition, if the heating time is too long, the same problem may occur, and the upper limit of the heating time is preferably 5 hours, more preferably about 2 hours. In addition, when performing the coupling agent treatment, it is known that the pH during the treatment greatly affects the performance, so it is desirable to adjust the pH appropriately.
[0055] The treatment method of the silane coupling agent in the present invention is a method of applying a solution of the silane coupling agent to a polyimide film, drying the polyimide film and then heat treating the polyimide film, or a method of immersing the polyimide film in a solution of the silane coupling agent. and a method in which the polyimide film is immersed in the copolymer and then dried and heat-treated, or a method in which the copolymer is added during the preparation of the polyimide film and the film is simultaneously treated with the coupling agent.
[0056] (Coupling agent treatment) In the present invention, the coupling agent means a compound that is physically or chemically present between the support and the polyimide film and has the effect of increasing the adhesive strength between them, and includes compounds generally known as silane-based coupling agents, phosphorus-based coupling agents, titanate-based coupling agents, etc.
[0057] The silane coupling agent in the present invention is not particularly limited, but is preferably one having an amino group or an epoxy group. In particular, from the viewpoint of adhesiveness, a silane coupling agent having a trifunctional alkoxyl group or a difunctional alkoxyl group is preferable.
[0058] Specific examples of silane coupling agents include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldiethoxymethylsilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyl ... Trimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltrimethoxysilane hydrochloride, 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatopropyltriethoxysilane, tris-(3- trimethoxysilylpropyl) isocyanurate, chloromethylphenethyltrimethoxysilane, chloromethyltrimethoxysilane, etc.
[0059] Among these, preferred ones include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldiethoxymethylsilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, aminophenyltrimethoxysilane, aminophenethyltrimethoxysilane, aminophenylaminomethylphenethyltrimethoxysilane, etc. When heat resistance is required in the process, it is desirable to use an aromatic bond between Si and the amino group, etc.
[0060] Further, 3-aminopropyltriethoxysilane and 3-aminopropyldiethoxymethylsilane are preferred, with 3-aminopropyldiethoxymethylsilane being particularly preferred.
[0061] <Laminate (adhesive sheet laminate)> The method for producing a laminate of the present invention is characterized in that at least two or more heat-resistant films including at least a polyimide film and an adhesive sheet having a three-layer structure including a thermoplastic resin layer laminated on each of both sides of the heat-resistant film are bonded together, the thickness of the laminate after bonding is 51 μm or more, and at least one of the surfaces of the adhesive sheets to be bonded together during bonding is surface-treated by applying and drying a surface treatment agent.
[0062] For example, two of the above-mentioned adhesive sheets each having a thickness of 25 μm can be coated with a silane coupling agent, dried, and then the coated surfaces can be brought together and laminated at a lamination temperature of 360°C, a lamination pressure of 0.8 tons, and a line speed of 1 m / min, resulting in a laminate thickness of 25 μm x 2 sheets = 50 μm. Similarly, by using three sheets of the adhesive sheet with a thickness of 25 μm, the thickness of the laminate becomes 25 μm×3 sheets=75 μm. At this time, a silane coupling agent is applied to at least one of the surfaces to be bonded, and preferably to each surface to be bonded in order to further improve the adhesion strength, and after drying, the coated surfaces are bonded together. For example, the lamination conditions are a lamination temperature of 360° C., a lamination pressure of 0.8 ton, and a line speed of 1 m / min.
[0063] Similarly, the thickness of the adhesive sheets can be freely combined, such as 50 μm × 4 sheets = 200 μm, 25 μm + 50 μm = 75 μm, and so on, and a thick laminate can be made by laminating them together. The thickness of the adhesive sheets is available in a lineup of 12.5 μm, 18 μm, 25 μm, 50 μm, etc., and can be freely selected and laminated together, and is not limited to this. Also, laminated pieces can be further laminated together. For example, a laminated thickness of 50 μm and a laminated thickness of 50 μm can be made 100 μm by applying a silane coupling agent, drying, and further laminating them. Since the laminate is laminated by applying heat and pressure, the lamination method can also be laminated by pressing other than lamination. It is not limited to this. In addition, a protective film (F) described later can be used so that the adhesive sheet does not come into contact with the heating part of the laminating or pressing device.
[0064] <Metal foil (D)> In the present invention, the metal foil (D) is not particularly limited, but when the single-sided flexible metal-clad laminate (E) and / or the double-sided flexible metal-clad laminate (G) of the present invention is used for electronic equipment and electrical equipment, examples of the metal foil include foils made of copper or copper alloys, stainless steel or its alloys, nickel or nickel alloys (including 42 alloy), and aluminum or aluminum alloys. In general flexible laminates, copper foils such as rolled copper foils and electrolytic copper foils are often used, but they can also be preferably used in the present invention. The surfaces of these metal foils may be coated with an anti-rust layer, a heat-resistant layer, or an adhesive layer. The thickness of the metal foil is not particularly limited, and may be any thickness that can exhibit sufficient functions depending on the application. The thickness of the metal foil (D) is preferably, for example, 3 μm to 30 μm, more preferably 5 μm to 20 μm. The surface roughness (Ra) of the metal foil (D) is preferably 0.01 μm to 1 μm. If the surface roughness (Ra) of the metal foil (D) is outside this range, the adhesion to the thermoplastic resin layer (B) may be poor.
[0065] <Protective film (F)> The specific configuration of the means for carrying out the thermocompression bonding is not particularly limited, but in order to improve the appearance of the resulting single-sided flexible metal-clad laminate (E) and / or double-sided flexible metal-clad laminate (G), the metal foil (D) is laminated on the side on which the metal foil (D) is laminated via a thermoplastic resin layer (B), and a protective film (F) is further laminated in contact with the metal foil (D). Specifically, the protective film (F) is laminated between the pressure surface (e.g., a metal roll) and the adhesive sheet (C) and metal foil (D).
[0066] The protective film (F) is not particularly limited as long as it can withstand the heating temperature in the thermocompression bonding step, and heat-resistant plastics such as non-thermoplastic polyimide films, metal foils such as copper foils, aluminum foils, and SUS foils, etc. can be suitably used. Among them, non-thermoplastic polyimide films are more preferably used because they have an excellent balance between heat resistance, recyclability, etc.
[0067] As the non-thermoplastic polyimide film, various known films can be used, for example, Apical (registered trademark) manufactured by Kaneka Corporation, Upilex (registered trademark) manufactured by Ube Industries, Ltd., Kapton (registered trademark) manufactured by DuPont-Toray Co., Ltd., and the like.
[0068] <Manufacturing method for single-sided flexible metal-clad laminate (E)> The method for producing a single-sided flexible metal-clad laminate of the present invention involves stacking a metal foil / two or more adhesive sheets in the order of a laminate having a thickness of 51 μm or more, or stacking a metal foil / two or more adhesive sheets in the order of a laminate, wherein the adhesive sheet has a three-layer structure having a heat-resistant film containing at least a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film, the thickness after lamination of the adhesive sheet is 51 μm or more, and at least one of the surfaces where the adhesive sheets are to be laminated together during lamination is surface-treated by applying and drying a surface treatment agent.
[0069] The single-sided flexible metal-clad laminate (E) will ultimately be a laminate having a thickness of 51 μm or more, which is made by bonding a metal foil and two or more adhesive sheets. However, it may be a laminate having a thickness of 51 μm or more, which is made by bonding a metal foil and two or more adhesive sheets, or it may be a laminate made by bonding a metal foil and two or more adhesive sheets.
[0070] When laminating a metal foil and two or more adhesive sheets to a thickness of 51 μm or more, the above-mentioned laminate of two or more adhesive sheets may be laminated to copper foil.
[0071] In addition, when bonding a metal foil and two or more adhesive sheets, the adhesive sheet is used, at least one side of which has been coated with a surface treatment agent and dried to perform a surface treatment, and the sheets are laminated in the order of metal foil / two or more adhesive sheets. In this case, the thickness of the adhesive sheets after bonding is 51 μm or more, and the adhesive sheets are bonded such that at least one side of the surface to be bonded has been coated with a surface treatment agent, dried, and surface-treated. Coating both sides of the adhesive sheet with a surface treatment agent and drying to perform a surface treatment tends to improve the adhesion between the adhesive sheets, and is therefore preferred.
[0072] As a method for laminating (bonding), various known methods can be applied, but a thermocompression bonding method for bonding by thermocompression is preferred because it can suppress the occurrence of wrinkles in the single-sided flexible metal-clad laminate (E). Examples of a method for bonding the adhesive sheet (C) and the metal foil (D) include a thermocompression bonding method by batch processing using a single plate press, a thermocompression bonding method by continuous processing using a thermoroll laminator (also called a thermolaminator) or a double belt press (DBP) device, and the like. From the viewpoint of productivity and equipment costs including maintenance costs, a thermocompression bonding method using a thermoroll laminator having one or more pairs of metal rolls is preferred. The "thermoroll laminator having one or more pairs of metal rolls" referred to here may be any device having metal rolls for heating and pressurizing the material, and the specific device configuration is not particularly limited.
[0073] <Manufacturing method 1 for double-sided flexible metal-clad laminate (G)> The method for producing a double-sided flexible metal-clad laminate of the present invention is a method for producing a double-sided flexible metal-clad laminate by laminating a metal foil, a laminate having a thickness of 51 μm or more obtained by laminating two or more adhesive sheets, and a metal foil in this order, or a metal foil, two or more adhesive sheets, and a metal foil in this order, the adhesive sheet has a three-layer structure including a heat-resistant film including at least a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film, The thickness after lamination of the adhesive sheet is 51 μm or more, The adhesive sheet is characterized in that at least one of the surfaces to be bonded to the other adhesive sheet is subjected to a surface treatment by coating and drying a surface treatment agent.
[0074] The double-sided flexible metal-clad laminate (G) will ultimately be a laminate of metal foil / two or more adhesive sheets bonded together to a thickness of 51 μm or more / metal foil; however, it may be bonded by sandwiching a laminate of two or more adhesive sheets bonded together to a thickness of 51 μm or more between the two metal foils mentioned above, or it may be bonded by sandwiching two or more adhesive sheets between two metal foils.
[0075] When sandwiching and bonding a laminate having a thickness of 51 μm or more, which is made by bonding two or more adhesive sheets between two metal foils, the above-mentioned laminate having two or more adhesive sheets bonded together may be bonded to copper foil.
[0076] In addition, when two or more adhesive sheets are sandwiched between two metal foils and bonded together, the adhesive sheet is used, at least one side of which has been coated with a surface treatment agent and dried to perform a surface treatment, and the sheets are laminated in the order of metal foil / two or more adhesive sheets / metal foil. In this case, the thickness of the adhesive sheet after bonding is 51 μm or more, and the adhesive sheets are bonded together such that at least one side of the surface to be bonded has been coated with a surface treatment agent, dried, and surface-treated. It is preferable that both sides of the adhesive sheet are coated with a surface treatment agent and dried to perform a surface treatment, as this tends to improve the adhesion between the adhesive sheets.
[0077] As a lamination method, various known methods can be applied, but a thermocompression bonding method by bonding by thermocompression is preferred because it can suppress the occurrence of appearance defects of the double-sided flexible metal-clad laminate (G). Examples of the bonding method include a thermocompression bonding method by batch processing using a single plate press, a thermocompression bonding method by continuous processing using a thermoroll laminator (also called a thermolaminator) or a double belt press (DBP) device, etc. From the viewpoint of productivity and equipment costs including maintenance costs, a thermocompression bonding method using a thermoroll laminator having one or more pairs of metal rolls is preferred. The "thermoroll laminator having one or more pairs of metal rolls" referred to here may be a device having metal rolls for heating and pressurizing the material, and the specific device configuration is not particularly limited.
[0078] In this thermocompression bonding method, when the metal foil (D) is subjected to high heat treatment twice, during the production of the single-sided flexible metal-clad laminate (E) and the production of the double-sided flexible metal-clad laminate (G), there is a problem that the metal foil (D) is prone to poor appearance due to heat burning and heat deformation. In order to improve the thermal deformation, it is preferable to use a thermocompression bonding method using a heat roll laminating device having one or more pairs of metal rolls in the thermocompression bonding method, and to control the tension of the metal foil (D) and the single-sided flexible metal-clad laminate (E). Specifically, it is preferable to set the tension before thermocompression bonding high, and it is preferable to set the payout tension of the single-sided flexible metal-clad laminate (E) to 40 kgf / 270 mm or more. In addition, in order to improve the heat burning, it is preferable to use a protective film during the heat roll lamination.
[0079] The heating method of the laminated material in the thermocompression bonding means is not particularly limited, and for example, a heating means adopting a conventionally known method capable of heating at a predetermined temperature, such as a heat circulation method, a hot air heating method, an induction heating method, etc. Similarly, the pressurizing method of the laminated material in the thermocompression bonding means is not particularly limited, and for example, a pressurizing means adopting a conventionally known method capable of applying a predetermined pressure, such as a hydraulic method, an air pressure method, an inter-gap pressure method, etc., can be used.
[0080] The heating temperature in the above thermocompression bonding step, i.e., the pressure bonding temperature (lamination temperature), is sufficient for the adhesive sheet (C) on the side in close contact with the metal foil (D) during the production of the single-sided flexible metal-clad laminate, as long as it is the minimum temperature at which it can be adhered, and the adhesive sheet (C) on the side not in close contact with the metal foil (D) is at a temperature at which it does not stick to other materials or processes, so the lamination temperature during the production of the single-sided flexible metal-clad laminate is preferably the glass transition temperature (Tg) of the adhesive sheet (C) used + 20°C to (Tg) + 60°C. On the other hand, during the production of the double-sided flexible metal-clad laminate, it is desirable for all layers to have high adhesion, so lamination is preferably performed at a temperature higher than that of the single-sided flexible metal-clad laminate, and the lamination temperature during the production of the double-sided flexible metal-clad laminate is preferably the glass transition temperature (Tg) of the adhesive sheet (C) used + 20°C to (Tg) + 90°C, more preferably the Tg of the adhesive sheet (C) + 50°C to (Tg) + 80°C.
[0081] In addition to the above-mentioned viewpoint of adhesion with the copper foil, in order to increase the adhesion of the laminated surface after applying and drying the silane coupling agent, the lamination temperature is preferably 340 to 380°C, and most preferably 360 to 380°C. The thickness of the protective film is preferably 50 to 125 μm. When the protective film is thin, the lamination temperature is easily propagated, so the lamination temperature can be lowered, and when a thick protective film is used, the lamination temperature can be raised. There is no limitation to this lamination temperature. Similarly, the pressing temperature is not limited.
[0082] The lamination speed in the thermocompression bonding step is preferably 0.5 m / min or more, and more preferably 1.0 m / min or more. If it is 0.5 m / min or more, sufficient thermocompression bonding can be achieved, and if it is 1.0 m / min or more, productivity can be further improved.
[0083] The pressure in the above-mentioned thermocompression bonding process, i.e., the lamination pressure, has the advantage that the lamination temperature can be lowered and the lamination speed can be increased as the lamination pressure is higher, but generally, if the lamination pressure is too high, the dimensional change of the obtained metal-clad laminate tends to worsen. Conversely, if the lamination pressure is too low, the adhesive strength of the metal foil of the obtained metal-clad laminate tends to be lower. Therefore, the lamination pressure is preferably within the range of 49N / cm to 490N / cm (5kgf / cm to 50kgf / cm), and more preferably within the range of 98N / cm to 294N / cm (10kgf / cm to 30kgf / cm). Within this range, the three conditions of lamination temperature, lamination speed, and lamination pressure can be made good, and productivity can be further improved.
[0084] In order to obtain the laminate, single-sided or double-sided flexible metal-clad laminate (G) according to the present invention, it is preferable to use a thermal roll laminating device that continuously heats and presses the laminated material. In this thermal roll laminating device, a laminated material feeding means for feeding the laminated material may be provided in the upstream of the thermal laminating means, or a laminated material winding means for winding the laminated material may be provided in the downstream of the thermal laminating means. By providing these means, the productivity of the thermal roll laminating device can be further improved. The specific configurations of the laminated material feeding means and the laminated material winding means are not particularly limited, and examples thereof include known roll-shaped winders that can wind the laminate, adhesive sheet, metal foil, or the resulting metal-clad laminate.
[0085] Furthermore, it is more preferable to provide a winding means and a payout means for winding and paying out the protective film (F). If these winding means and payout means are provided, the protective film (F) that has been used once in the thermocompression bonding process can be reused by winding it up and placing it again on the payout side. In addition, an end position detection means and a winding position correction means may be provided to align both ends when winding up the protective film (F). This allows the ends to be accurately aligned when winding up, thereby increasing the efficiency of reuse. The specific configurations of these winding means, payout means, end position detection means, and winding position correction means are not particularly limited, and various conventionally known devices can be used.
[0086] <Method of manufacturing a double-sided flexible metal-clad laminate having a microstrip line structure> A method for manufacturing a double-sided flexible metal-clad laminate having a microstrip line structure is characterized in that the double-sided flexible metal-clad laminate is used to form the laminate so as to have a microstrip line structure, and the total thickness of the two or more overlapping adhesive layers is 75 to 200 μm.
[0087] As shown in Fig. 1, a microstrip line structure can be formed by etching the metal foil on one side of a double-sided flexible metal-clad laminate to form a signal line 3, and using the metal foil on the other side as a ground layer 1. Although Fig. 1 shows an example with one signal line, there may be multiple signal lines.
[0088] It is preferable that the total thickness of the two or more overlapping adhesive layers be 75 μm or more, since this tends to reduce the transmission loss of the double-sided flexible metal-clad laminate having a microstrip line structure, and it is preferable that the total thickness be 200 μm or less, since this allows the laminate to be easily bent and easily mounted on electronic devices.
[0089] <Method of manufacturing a multi-layer flexible metal-clad laminate having a stripline structure> By bonding a single-sided metal-clad laminate having a configuration of ground layer 1 / second polyimide layer 4 to a double-sided flexible metal-clad laminate having the microstrip line structure shown in Figure 1 via an adhesive layer, a multi-layer flexible metal-clad laminate having a strip line structure as shown in Figure 2 can be obtained with a configuration of ground layer 1 / second polyimide layer 4 / adhesive layer 5 / signal line 3 / laminate (first polyimide layer 2) formed by bonding two or more adhesive sheets together / ground layer 1. This configuration is preferable because it tends to reduce transmission loss even more than the microstrip line structure. EXAMPLES
[0090] The manufacturing method of the present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The film thickness, dielectric constant, dielectric loss tangent, laminate inter-film adhesion, FCCL inter-film adhesion, copper foil peel strength, moisture absorption solder heat resistance, FPC transmission characteristics (measurement of microstrip line and strip line transmission characteristics), and copper foil surface roughness were evaluated in the following manner in the examples and comparative examples.
[0091] (film thickness) The thickness of the film was measured using a contact thickness gauge, LASER HOLOGAGE, manufactured by Mitsutoyo Corporation.
[0092] (Measurement of dielectric constant and dielectric tangent) The dielectric constant and dielectric loss tangent of the multilayer polyimide film were measured at the following frequencies using a cavity resonator perturbation method complex dielectric constant evaluation device (manufactured by Kanto Electronics Application Development Co., Ltd.).
[0093] Measurement frequency: 10GHz Measurement conditions: temperature 22℃~24℃, humidity 45%~55% Measurement sample: A sample that had been left to stand for 24 hours under the above measurement conditions was used.
[0094] (Method of measuring adhesion between laminated films and adhesion between FCCL films) The adhesion between the laminates or FCCL films was analyzed according to the "T-type peel test" of JIS K 6854-3. Specifically, a 10mm wide laminate was peeled at 100mm / min with the center of the laminated film exposed, and the load was measured. The adhesion between the films was evaluated as "○" (good) when it was 5N / cm or more, and "×" (bad) when it was less than 5N / cm.
[0095] (Method of measuring copper foil peel strength of metal-clad laminate) FCCL was analyzed according to JIS C6471 "6.5 Peel strength". Specifically, a 1mm wide metal foil portion was peeled at a peel angle of 90 degrees at 100mm / min, and the load was measured. Peel strength of 12N / cm or more was evaluated as "○" (good), and less than 12N / cm was evaluated as "×" (poor).
[0096] (Moisture absorption solder heat resistance test) A specified pattern sample is formed from a copper-clad board made with a thermal laminator, and left in an environmental tester maintained at 85±5°C and 85±5% RH for 24±0.25 hours, then removed and immersed in a solder bath adjusted to 300±5°C for 10±2 seconds. After being removed, the appearance is visually inspected. If there is any swelling, it is rated as ×, and if there is no swelling, it is rated as ○.
[0097] (Fabrication of FCCL, Measurement of transmission characteristics of microstrip line and strip line) A polyimide film and a copper foil were laminated under the following conditions to obtain a double-sided FCCL. Copper foil used: 12 μm thick, roughness of the surface to be bonded to the polyimide film is 0.45 μm or less Polyimide and copper foil lamination conditions: Lamination temperature 360°C, lamination pressure 0.8 tons, lamination speed 1m / min The microstrip line circuit was fabricated by etching one side of a double-sided FCCL to fabricate a microstrip line with a line length of 10 cm, and copper plating was applied to the circuit and terminal parts. The circuit width was calculated from the thickness, dielectric constant, and dielectric loss tangent of the constituent materials so that the characteristic impedance was 50 Ω.
[0098] Then, the microstrip line circuit was bonded to one-sided FCCL with an adhesive layer (bonding sheet) by heating under reduced pressure at 160℃ for 30 minutes to produce an FPC test piece with a strip line structure. The circuit width was calculated from the thickness, dielectric constant, and dielectric tangent of the constituent materials so that the characteristic impedance was 50Ω.
[0099] The following treatment was carried out on the obtained flexible metal-clad laminate having a microstrip line circuit and flexible metal-clad laminate having a strip line circuit. That is, after drying at 150°C for 30 minutes, the humidity was conditioned for 24 hours or more in a test room adjusted to 23°C and 55% RH. Then, the insertion loss S21 parameter was measured using a network analyzer E5071C (Keysight Technologies) and a GSG250 probe, and the transmission loss (dB / 100 mm) at a measurement frequency of 10 GHz was obtained.
[0100] (Copper foil surface roughness Ra) The arithmetic average roughness was measured under the following conditions using an optical interference surface roughness meter (ZYGO NewView5030 system).
[0101] (Measurement conditions) Objective lens: 50x Mirau Image Zoom: 2 FDA Res:Normal Analysis conditions: Remove:Cylinder Filter:High Pass Filter Low Waven: 0.002mm
[0102] Example 1 Heat-resistant double-sided adhesive sheet with a thickness of 50 μm (Pixio (registered trademark) IB made by Kaneka Corporation) A solution of 3-aminopropyltriethoxysilane (sometimes abbreviated as APTS) diluted to 10% by weight with 2-propanol was prepared and applied to one side of the IB film using a bar coater, and then dried at 130°C for 30 minutes. Then, the coated surfaces of the two IBs that had been coated and dried were placed together, and two protective films (Apical (registered trademark) 125AH manufactured by Kaneka Corporation) were placed on the IBs. The IBs were passed through a pair of metal rolls of a hot roll laminator to perform thermal lamination under the conditions of a lamination temperature of 360°C, a lamination pressure of 290 N / cm, and a lamination speed of 1 m / min. Then, the protective films were separated in order to produce a laminate (a laminate of adhesive sheets). The obtained laminate of adhesive sheets was subjected to thickness measurement, dielectric constant measurement, dielectric loss tangent measurement, and adhesion strength measurement between the laminate films.
[0103] A 12 μm thick electrolytic copper foil (CF-T49A-HD2 manufactured by Fukuda Metal Foil and Powder Co., Ltd.) was laminated on the laminate, and a protective film (Apical (registered trademark) 125NPI manufactured by Kaneka Corporation) was arranged so as to sandwich this metal foil with an adhesive sheet, and the laminate was passed between a pair of metal rolls of a hot roll laminator to perform thermal lamination under the conditions of a lamination temperature of 360° C., a lamination pressure of 290 N / cm, and a lamination speed of 1 m / min. Then, the protective film was separated in order to produce a double-sided flexible metal-clad laminate (G). The obtained double-sided flexible metal-clad laminate (G) was evaluated for adhesion between FCCL films, copper foil peel strength of the metal-clad laminate, and moisture absorption solder heat resistance.
[0104] A sheet of electrolytic copper foil (CF-T49A-HD2 manufactured by Fukuda Metal Foil and Powder Co., Ltd.) having a thickness of 12 μm was laminated on the laminate, and a protective film (Apical (registered trademark) 125NPI manufactured by Kaneka Corporation) was arranged so as to sandwich this metal foil with an adhesive sheet. The other protective film was 125AH, and the laminate was passed between a pair of metal rolls of a hot roll laminator to perform thermal lamination under the conditions of a lamination temperature of 360° C., a lamination pressure of 290 N / cm, and a lamination speed of 1 m / min. Then, the protective films were separated in order to produce a single-sided metal-clad laminate (E).
[0105] (Microstrip line) One side of the double-sided flexible metal laminate (G) containing the polyimide layer described above was etched to create a microstrip line with a line length of 10 cm, and the circuit and terminal parts were copper-plated to create a test piece of the flexible metal-clad laminate for the microstrip line (Figure 1). The circuit width was calculated from the thickness, dielectric constant, and dielectric loss tangent of the constituent materials so that the characteristic impedance was 50 Ω.
[0106] (Stripline) One side of the double-sided flexible metal laminate (G) containing the above-mentioned first polyimide layer was etched to prepare a microstrip line with a line length of 10 cm, and copper plating was applied to the circuit and terminal parts. This microstrip line circuit was bonded to a single-sided metal-clad laminate (E) containing a second polyimide laminate via a bonding sheet SAFY manufactured by Nikkan Kogyo Co., Ltd., by heating under reduced pressure at 150°C for 30 minutes at 1 to 2 MPa. In this way, a test piece of a flexible metal-clad laminate with a stripline structure was produced. The circuit width was calculated from the thickness, dielectric constant, and dielectric loss tangent of the constituent materials so that the characteristic impedance was 50 Ω, and the upper and lower grounds were structured to be conductive with vias to reduce noise (Figure 2).
[0107] The following treatment was carried out on the obtained flexible metal-clad laminate having a microstrip line circuit and flexible metal-clad laminate having a strip line circuit. That is, after drying at 150°C for 30 minutes, the humidity was conditioned for 24 hours or more in a test room adjusted to 23°C and 55% RH. Then, the insertion loss S21 parameter was measured using a network analyzer E5071C (Keysight Technologies) and a GSG250 probe, and the transmission loss (dB / 100 mm) at a measurement frequency of 10 GHz was obtained.
[0108] Example 2 The same procedures as in Example 1 were carried out, except that 3-aminopropyldiethoxymethylsilane (sometimes abbreviated as APDE) was used as the silane coupling agent.
[0109] (Reference example 1) The same procedure as in Example 2 was carried out, except that an adhesive sheet was used in combination with a 25 μm polyimide film (both manufactured by Kaneka Corporation, Pixio SR).
[0110] Example 3 The same procedure as in Example 2 was carried out, except that a combination of 50 μm and 25 μm polyimide films (both manufactured by Kaneka Corporation, Pixio SR) was used as the adhesive sheets.
[0111] Example 4 The same procedure as in Example 2 was carried out, except that the adhesive sheet used was a combination of two 50 μm polyimide films (both Pixio SR, manufactured by Kaneka Corporation).
[0112] (Reference example 2) The same procedure as in Example 2 was carried out, except that an adhesive sheet was used in combination with a 25 μm polyimide film (both manufactured by Kaneka Corporation, Pixio FRS).
[0113] Example 5 The same procedure as in Example 2 was carried out, except that a combination of 50 μm and 25 μm polyimide films (both Pixio FRS manufactured by Kaneka Corporation) was used as the adhesive sheets.
[0114] Example 6 The same procedures as in Example 2 were carried out, except that the adhesive sheet used was a combination of two 50 μm polyimide films (both Pixio FRS manufactured by Kaneka Corporation).
[0115] (Reference example 3) The same procedure as in Example 2 was carried out, except that the adhesive sheet used was a combination of two 12.5 μm polyimide films (both Pixio IB, manufactured by Kaneka Corporation).
[0116] (Reference example 4) The same procedure as in Example 2 was carried out, except that the adhesive sheet used was a combination of two 25 μm polyimide films (both Pixio IB, manufactured by Kaneka Corporation).
[0117] Example 7 The same procedure as in Example 2 was carried out, except that a combination of 50 μm and 25 μm polyimide films (both manufactured by Kaneka Corporation, Pixio IB) was used as the adhesive sheets.
[0118] Example 8 The same procedure as in Example 2 was carried out, except that the adhesive sheet used was a combination of three 25 μm polyimide films (all Pixio IB, manufactured by Kaneka Corporation).
[0119] Example 9 The same procedure as in Example 2 was carried out, except that the adhesive sheet used was a combination of three 50 μm polyimide films (all Pixio IB, manufactured by Kaneka Corporation).
[0120] Example 10 The same procedure as in Example 2 was carried out, except that the adhesive sheet used was a combination of four 50 μm polyimide films (all Pixio IB, manufactured by Kaneka Corporation).
[0121] Example 11 In Example 2, except for the stepwise process of obtaining a laminate and laminating it with metal foil, two adhesive sheets to which a silane coupling agent had been applied and dried were stacked, and then laminated together with metal foil to produce a single-sided metal laminate (E) and a double-sided metal laminate (G), the rest of the procedure was the same as in Example 2.
[0122] Example 12 The procedure of Example 2 was repeated, except that the concentration of the solution diluted with 2-propanol was adjusted to 5% by weight.
[0123] Example 13 The procedure of Example 2 was repeated, except that the concentration of the solution diluted with 2-propanol was adjusted to 1% by weight.
[0124] Example 14 The same procedures as in Example 2 were carried out, except that an adhesive sheet on whose surface a silane coupling agent had been applied and dried was bonded to an adhesive sheet on which no surface treatment had been applied.
[0125] Comparative Example 1 The same procedure as in Example 1 was repeated except that the surface treatment of the adhesive sheet was not performed. was carried out in the same manner.
[0126] As a result, the adhesive strength between the adhesive sheets was weak, and the adhesive sheets in the resulting single-sided metal-clad laminate (E) and double-sided metal-clad laminate (G) easily peeled off from each other.
[0127] Comparative Example 2 The same procedure as in Example 1 was repeated except that the surface treatment of the adhesive sheet was atmospheric pressure plasma treatment. A double-sided metal-clad laminate (G) was produced in the same manner as above.
[0128] As a result, the adhesive strength between the adhesive sheets was weak, and the adhesive sheets in the resulting single-sided metal-clad laminate (E) and double-sided metal-clad laminate (G) easily peeled off from each other.
[0129] Comparative Example 3 Except for the surface treatment of the adhesive sheet in Example 1 being embossed, a double-sided metal-clad laminate (G) was produced in the same manner as in Example 1. As a result, the adhesive sheets had weak adhesion to each other, and the adhesive sheets in the obtained single-sided metal-clad laminate (E) and double-sided metal-clad laminate (G) easily peeled off from each other. Comparative Example 4 A double-sided metal-clad laminate (G) was produced in the same manner as in Example 1, except that the surface treatment of the adhesive sheet in Example 1 was a hairline finish. As a result, the adhesive sheets had weak adhesion to each other, and the adhesive sheets in the obtained double-sided metal-clad laminate (G) easily peeled off from each other.
[0130] [Table 1] [Explanation of symbols]
[0131] 1. Ground Layer 2. A laminate (first polyimide layer) made by bonding two or more adhesive sheets together 3. Signal line 4. Laminate made by bonding two or more adhesive sheets (second polyimide layer) 5.Adhesive layer
Claims
1. At least two or more adhesive sheets having a three-layer structure including a heat-resistant film containing at least a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film are bonded together, and the thickness of the laminated sheet is 51 μm or more; A method for producing a laminate, comprising the steps of: applying a surface treatment agent to at least one of the surfaces of the adhesive sheet to be laminated when the adhesive sheets are laminated; and drying the surface treatment agent.
2. The method for producing a laminate according to claim 1 , wherein the surface treatment agent is a silane coupling agent having a trifunctional alkoxyl group or a difunctional alkoxyl group.
3. A method for producing a single-sided flexible metal-clad laminate, comprising laminating a metal foil and a laminate having a thickness of 51 μm or more, the laminate being formed by laminating two or more adhesive sheets, or laminating a metal foil and two or more adhesive sheets, the method comprising the steps of: the adhesive sheet has a three-layer structure including a heat-resistant film including at least a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film, The thickness after lamination of the adhesive sheet is 51 μm or more, A method for producing a single-sided flexible metal-clad laminate, characterized in that at least one of the surfaces where the adhesive sheets are to be laminated together during lamination is subjected to a surface treatment by applying a surface treatment agent and drying it.
4. 4. The method for producing a single-sided flexible metal-clad laminate according to claim 3, wherein the surface treatment agent is a silane coupling agent having a trifunctional alkoxyl group or a difunctional alkoxyl group.
5. A method for producing a double-sided flexible metal-clad laminate, comprising laminating a metal foil, a laminate having a thickness of 51 μm or more obtained by laminating two or more adhesive sheets, and a metal foil in this order, or laminating a metal foil, two or more adhesive sheets, and a metal foil in this order, the adhesive sheet has a three-layer structure including a heat-resistant film including at least a polyimide film and a thermoplastic resin layer laminated on each of both sides of the heat-resistant film, The thickness after lamination of the adhesive sheet is 51 μm or more, A method for producing a double-sided flexible metal-clad laminate, characterized in that at least one of the surfaces to be laminated with the adhesive sheet during lamination is subjected to a surface treatment by coating and drying a surface treatment agent.
6. 6. The method for producing a double-sided flexible metal-clad laminate according to claim 5, wherein the surface treatment agent is a silane coupling agent having a trifunctional alkoxyl group or a difunctional alkoxyl group.
7. A method for producing a double-sided flexible metal-clad laminate having a microstrip line structure, comprising forming the double-sided flexible metal-clad laminate according to claim 5 into a microstrip line structure, and forming the laminate into a microstrip line structure, the total thickness of the two or more superimposed adhesive layers being 75 to 200 μm.
Citation Information
Patent Citations
Manufacturing method of laminated sheet
JP2001129918A
Method of producing double-surface flexible metal-clad laminate sheet
JP2014195947A