Rubber composition for tire cap tread, and tire using the same

A rubber composition for tire treads, combining styrene-butadiene copolymer rubber with carbon black, terpene resin, and ester plasticizer, addresses the challenge of enhancing dry and initial grip performance and wear resistance while maintaining mechanical integrity and environmental friendliness.

JP2024134628APending Publication Date: 2024-10-04THE YOKOHAMA RUBBER CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023044915
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing tire compositions struggle to simultaneously enhance dry grip performance, initial grip performance, and wear resistance, with high glass transition point resins compromising low-temperature grip and liquid plasticizers degrading mechanical strength and abrasion resistance.

Method used

A rubber composition comprising styrene-butadiene copolymer rubber blended with specific amounts of carbon black, terpene resin, and ester plasticizer, with nitrogen adsorption specific surface area between 100-500 m²/g, 50-200 parts by mass of carbon black, 5-80 parts by mass of terpene resin with a softening point of 100°C or higher, and 5-50 parts by mass of ester plasticizer.

Benefits of technology

The composition achieves improved grip performance, initial grip performance, and wear resistance, maintaining environmental sustainability by using biomass oil as a liquid plasticizer without compromising dry grip.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134628000001
    Figure 2024134628000001
  • Figure 2024134628000002
    Figure 2024134628000002
Patent Text Reader

Abstract

To require various performances for a racing tire, especially, dry grip performance, initial grip performance and abrasion resistance.SOLUTION: A rubber composition for a tire cap tread is formed by blending 50 to 200 pts.mass of carbon black having a nitrogen adsorption specific surface area (N2SA) of 100 to 500 m2 / g, 5 to 80 pts.mass of a terpene resin having a softening point of 100°C or higher, and 5 to 50 pts.mass of an ester-based plasticizer, with 100 pts.mass of a styrene-butadiene copolymer rubber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for tire cap treads and a tire using the same, and more particularly, to a rubber composition that can simultaneously improve dry grip performance, initial grip performance and abrasion resistance, and a tire using the same. [Background technology]

[0002] In general, the performance required for racing tires is diverse, and particularly excellent steering stability (dry grip performance) on dry roads during high-speed driving is required. For this reason, in order to improve grip performance, the blending of large amounts of rubber with a high glass transition point (Tg), such as styrene-butadiene copolymer rubber (SBR) or high softening point resin, has been considered. However, while blending high softening point resin with rubber with a high Tg improves grip performance at high temperatures, it also creates temperature dependency in tire performance, which causes problems such as reduced operability (initial grip performance) at low temperatures. On the other hand, there is a method of blending a large amount of liquid plasticizer to improve dry grip performance, but this method has the following problems. (1) The use of a large amount of liquid plasticizer reduces the breaking strength and deteriorates the abrasion resistance. (2) While there is a demand to switch to renewable raw materials for racing tires from an environmental perspective, if biomass oil is used as a liquid plasticizer, the Tg of the compound decreases, deteriorating dry grip performance.

[0003] Patent Document 1 listed below discloses a rubber composition for tires that contains a rubber component having a styrene-butadiene rubber content of 40 to 80 mass% and a butadiene rubber content of 10 to 35 mass%, silica in an amount of 80 parts by mass or more per 100 parts by mass of the rubber component, and a terpene resin in an amount of 10 to 60 parts by mass per 100 parts by mass of the rubber component, and that satisfies the following formula (A). (A) α / β≦3 α: Styrene content of styrene-butadiene rubber [mass%] β: Content of terpene resin per 100 parts by mass of rubber component [parts by mass] However, with the above-mentioned conventional techniques, it has been difficult to simultaneously improve dry grip performance, initial grip performance, and abrasion resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-183010 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a rubber composition for a tire cap tread, which can simultaneously improve dry grip performance, initial grip performance and abrasion resistance, and a tire using the same. [Means for solving the problem]

[0006] As a result of extensive research, the present inventors have found that a rubber composition in which styrene-butadiene copolymer rubber is blended with carbon black having specific properties, a terpene resin, and an ester-based plasticizer in specific amounts can solve the above problems, and have thus completed the present invention.

[0007] That is, the present invention provides a method for producing a styrene-butadiene copolymer rubber having a nitrogen adsorption specific surface area (N 2 SA) is 100~500m 2 The rubber composition for tire cap treads is characterized by blending 50 to 200 parts by mass of carbon black having a molecular weight of 100 / g, 5 to 80 parts by mass of a terpene resin having a softening point of 100°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer. The present invention also provides a tire using the above rubber composition for tire cap tread in a cap tread. Effect of the Invention

[0008] The rubber composition for tire cap tread of the present invention has a nitrogen adsorption specific surface area (N 2 SA) is 100~500m 2 The tire is characterized by a blend of 50 to 200 parts by mass of carbon black having a molecular weight of 100 / g, 5 to 80 parts by mass of a terpene resin having a softening point of 100°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer, thereby making it possible to simultaneously improve dry grip performance, initial grip performance, and abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will now be described in further detail.

[0010] (Rubber component) The rubber component used in the rubber composition for tire cap treads of the present invention (hereinafter, sometimes simply referred to as rubber composition) is styrene-butadiene copolymer rubber (SBR). In the present invention, it is preferable that all of the rubber components are SBR, but if necessary, any diene rubber that can be blended in a normal rubber composition, such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), acrylonitrile-butadiene copolymer rubber (NBR), ethylene-propylene-diene terpolymer (EPDM), etc., can also be used in combination. The SBR used in the present invention is not particularly limited in its molecular weight or microstructure, and may be terminally modified with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl groups, or the like, or may be epoxidized. Moreover, from the viewpoint of improving the effects of the present invention, the SBR used in the present invention preferably contains a styrene content of 25 to 50 mass %.

[0011] (Carbon Black) The carbon black used in the present invention has a nitrogen adsorption specific surface area N 2 SA is 100~500m 2The specific carbon black used in the present invention has a carbon content of N 2 SA is 130~400m 2 / g is preferred. Furthermore, 2 SA shall be measured in accordance with JIS K6217-2.

[0012] (Terpene resin) Examples of the terpene resin used in the present invention include terpene resins such as α-pinene, β-pinene, dipentene, and limonene. From the viewpoint of improving the effects of the present invention, the terpene resin is preferably an aromatic modified terpene resin. The aromatic modified terpene resin can be obtained, for example, by polymerizing the terpene resin with an aromatic compound other than phenol. Examples of the aromatic compound include styrene, α-methylstyrene, vinyltoluene, and indene. The content of the aromatic compound in the aromatic modified terpene resin is preferably 10 to 50% by mass. Moreover, the softening point of the terpene resin used in the present invention is preferably 100°C or higher, and more preferably 120 to 150°C, from the viewpoint of improving the effects of the present invention.

[0013] (Ester plasticizer) Examples of the ester-based plasticizer used in the present invention include vegetable oils, fatty acid esters such as glycerin fatty acid monoesters, glycerin fatty acid diesters, and glycerin fatty acid triesters, processed vegetable oils, etc. Among these, those obtained from processed vegetable oils are preferred.

[0014] Examples of vegetable oils include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil.

[0015] As the fatty acid ester, for example, fatty acid esters represented by the following formula can be suitably used.

[0016] [ka]

[0017] (In the formula, R 11 R represents a linear or branched alkyl group having 1 to 8 carbon atoms, a linear or branched alkenyl group having 1 to 8 carbon atoms, or a linear or branched alkyl group having 2 to 6 carbon atoms substituted with 1 to 5 hydroxyl groups. 12 represents an alkyl group or alkenyl group having 11 to 21 carbon atoms.

[0018] R 11 Examples of R include a methyl group, an ethyl group, a 2-ethylhexyl group, an isopropyl group, an octyl group, and groups in which these groups are substituted with 1 to 5 hydroxyl groups. 12 Examples of the alkyl group include linear or branched alkyl groups and alkenyl groups such as lauryl group, myristyl group, palmityl group, stearyl group, and oleyl group.

[0019] Examples of fatty acid esters include alkyl oleates, alkyl stearates, alkyl linoleates, and alkyl palmitates. Among them, alkyl oleates (methyl oleate, ethyl oleate, 2-ethylhexyl oleate, isopropyl oleate, octyl oleate, and the like) are preferred. In this case, the content of alkyl oleates in 100% by mass of fatty acid ester is preferably 80% by mass or more. Furthermore, modified products are particularly preferred.

[0020] Examples of fatty acid esters include fatty acid monoesters and fatty acid diesters of fatty acids (oleic acid, stearic acid, linoleic acid, palmitic acid, etc.) and alcohols (ethylene glycol, glycerol, trimethylolpropane, pentaerythritol, erythritol, xylitol, sorbitol, dulcitol, mannitol, inositol, etc.). Among these, glycerin fatty acid esters are preferred, and glycerin fatty acid monoesters are more preferred. As the fatty acid, oleic acid is particularly preferred. In this case, the content of oleic acid monoester in the total amount of fatty acid monoesters and fatty acid diesters (100% by mass) is preferably 80% by mass or more.

[0021] (Rubber composition blend ratio) The rubber composition of the present invention is characterized in that it contains 50 to 200 parts by mass of the specific carbon black, 5 to 80 parts by mass of a terpene resin having a softening point of 100°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer, relative to 100 parts by mass of SBR. If the amount of the specific carbon black is less than 50 parts by mass, the dry grip performance and abrasion resistance will decrease, and conversely, if it exceeds 200 parts by mass, the breaking strength will decrease due to deterioration of carbon dispersion, resulting in a decrease in abrasion resistance. If the amount of the terpene resin is less than 5 parts by mass, the amount is too small to achieve the effects of the present invention, whereas if it exceeds 80 parts by mass, the abrasion resistance decreases. If the amount of the ester plasticizer is less than 5 parts by mass, the amount is too small to achieve the effects of the present invention, whereas if it exceeds 50 parts by mass, the grip performance will decrease.

[0022] The blending amount of the specific carbon black is preferably 50 to 200 parts by mass based on 100 parts by mass of SBR. The amount of the terpene resin to be mixed is preferably 5 to 80 parts by mass based on 100 parts by mass of SBR. The amount of the ester plasticizer to be mixed is preferably 5 to 50 parts by mass based on 100 parts by mass of SBR.

[0023] Here, the mass ratio of the ester plasticizer to the terpene resin is preferably 1:0.8 to 3 when the former is taken as 1. With this blending ratio, even if biomass oil is used as the liquid plasticizer from the viewpoint of environmental friendliness, it is possible to suppress a decrease in the Tg of the compound and prevent a deterioration in dry grip performance. The mass ratio of the ester plasticizer:the terpene resin is more preferably 1:1.5-3.

[0024] (Other ingredients) In addition to the above-mentioned components, the rubber composition of the present invention may contain various additives that are generally compounded in rubber compositions, such as vulcanizing or crosslinking agents, vulcanizing or crosslinking accelerators, various fillers such as silica, clay, talc, and calcium carbonate, antioxidants, plasticizers, resins, and curing agents, and these additives can be kneaded in a general manner to form a composition and used for vulcanization or crosslinking. The amounts of these additives may be conventional amounts as long as they do not go against the object of the present invention. The rubber composition for tires of the present invention is preferably in a form that does not contain silica, and even if silica is compounded, it is preferable that the amount of silica is 200 parts by mass or less per 100 parts by mass of the diene rubber.

[0025] (Terpene phenol resin) From the viewpoint of improving the effect, the rubber composition of the present invention preferably contains a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more. Terpene phenol resins are known and are obtained by reacting a terpene compound with phenol, and any terpene phenol resin can be used in the present invention as long as it satisfies the above-mentioned conditions of acid value and hydroxyl value. The aromatic terpene resin described above is a polymer of a terpene compound and an aromatic compound other than phenol, and is distinguished from the above-mentioned terpene phenol resin. The acid value of the terpene phenol resin is more preferably from 40 to 150 mgKOH / g, and the hydroxyl value is more preferably from 10 to 100 mgKOH / g. The softening point of the terpene phenol resin used in the present invention is preferably 85 to 180°C.

[0026] The amount of the terpene phenol resin to be blended is preferably 5 to 50 parts by mass, and more preferably 10 to 40 parts by mass, based on 100 parts by mass of SBR.

[0027] In this specification, the acid value and the hydroxyl value can be measured in accordance with JIS K 0070: 1992. The softening point can be measured in accordance with JIS K 6220-1: 2001.

[0028] The rubber composition of the present invention can improve dry grip performance, initial grip performance and abrasion resistance at the same time, and therefore can be suitably used for tire treads, particularly cap treads, preferably racing tire treads, particularly cap treads. The tire of the present invention is preferably a pneumatic tire, and can be filled with air, an inert gas such as nitrogen, and other gases. EXAMPLES

[0029] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0030] Standard Example, Examples 1-5, Comparative Examples 1-2 In the formulation (parts by mass) shown in Table 1, the components other than the vulcanization system (vulcanization accelerator, sulfur) were kneaded in a 1.7-liter closed Banbury mixer for 5 minutes, then discharged outside the mixer and cooled at room temperature. The composition was then placed back into the same Banbury mixer, and the vulcanization system was added and kneaded to obtain a rubber composition. The obtained rubber composition was then press-vulcanized in a specified mold at 150°C for 30 minutes to prepare a vulcanized rubber test piece. The physical properties of the obtained vulcanized rubber test piece were measured using the test methods shown below.

[0031] Hardness (20° C.): Measured at 20° C. in accordance with JIS K6253. The results are expressed as an index, with the standard example being 100. The smaller the index, the more excellent the initial grip performance.

[0032] Dry grip performance: Based on JIS K6394, tan δ (100°C) was measured using a viscoelasticity spectrometer manufactured by Toyo Seiki Seisakusho Co., Ltd. under the conditions of initial strain = 10%, amplitude = ±2%, and frequency = 20Hz, and the dry grip performance was evaluated based on this value. The results were expressed as an index with the standard example being 100. The higher the index, the better the dry grip performance at high temperatures.

[0033] M300: 300% modulus (M300) at 100°C was measured in accordance with JIS K6251. The results were expressed as an index with the standard example being 100. A larger index indicates better abrasion resistance.

[0034] The results are also shown in Table 1.

[0035] [Table 1]

[0036] *1: SBR (Nipol 1739 manufactured by Zeon Corporation, styrene content = 40% by mass, Tg = -35°C, oil extension amount = 37.5 parts by mass per 100 parts by mass of SBR, Tg of SBR is the Tg of the oil-extended product.) *2: Carbon black: Seast 9, N manufactured by Tokai Carbon Co., Ltd. 2 SA=142m 2 / g) *3: Resin 1 (Yasuhara Chemical Co., Ltd. YS Resin TO-85, aromatic modified terpene resin, softening point = 85°C) *4: Resin 2 (Yasuhara Chemical Co., Ltd. YS Resin TO-125, aromatic modified terpene resin, softening point = 125°C) *5: Resin 3 (Tamanol 803L, terpene phenol resin, acid value = 50 mg KOH / g, hydroxyl value = 15 mg KOH / g, manufactured by Arakawa Chemical Industries, Ltd.) *6: Oil (Showa Shell Sekiyu Co., Ltd. Extract No. 4S, Tg=-41℃) *7: Ester-based plasticizer (H&R Pionier TP130B, glycerin fatty acid monoester of high oleic sunflower oil, Tg=-110℃) *8: Stearic acid (Beads Stearic Acid YR manufactured by NOF Corporation) *9: Zinc oxide (3 types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd.) *10: Anti-aging agent (Flexis 6PPD) *11: Vulcanization accelerator (Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) *12: Sulfur (Kinka-jirushi oil-filled fine sulfur manufactured by Tsurumi Chemical Industry Co., Ltd.)

[0037] From the results in Table 1, the rubber compositions of Examples 1 to 5 have a nitrogen adsorption specific surface area (N 2 SA) is 100~500m 2 The tire contains 50 to 200 parts by mass of carbon black having a viscosity of 100°C or more and 5 to 80 parts by mass of a terpene resin having a softening point of 100°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer, which results in improved dry grip performance, initial grip performance, and abrasion resistance compared to the standard example. On the other hand, since Comparative Example 1 used a plasticizer other than the ester-based plasticizer, it was not possible to simultaneously improve the initial grip performance and abrasion resistance compared to the standard example. In Comparative Example 2, the softening point of the terpene resin was below the lower limit specified in the present invention, so that the dry grip performance and abrasion resistance were deteriorated.

[0038] The present invention includes the following aspects. Embodiment 1: For 100 parts by mass of styrene-butadiene copolymer rubber, Nitrogen adsorption specific surface area (N 2 SA) is 100~500m 2 50 to 200 parts by mass of carbon black having a molecular weight of 1 / g, 5 to 80 parts by mass of a terpene resin having a softening point of 100° C. or higher, and A rubber composition for tire cap treads, comprising 5 to 50 parts by mass of an ester-based plasticizer. Embodiment 2: 2. The rubber composition for tire cap treads according to embodiment 1, wherein a mass ratio of the ester plasticizer:the terpene resin is 1:0.8-3. Embodiment 3: 3. The rubber composition for tire cap treads according to embodiment 1 or 2, wherein the ester plasticizer comprises a glycerin fatty acid ester. Embodiment 4: The rubber composition for tire cap treads according to embodiment 3, wherein the glycerin fatty acid ester is a glycerin fatty acid monoester. Embodiment 5: The rubber composition for tire cap tread according to any one of embodiments 1 to 4, further comprising 5 to 50 parts by mass of a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more, based on 100 parts by mass of the styrene-butadiene copolymer rubber. Embodiment 6: A tire using the rubber composition for a tire cap tread according to any one of the first to fifth embodiments for a cap tread.

Claims

1. For 100 parts by mass of styrene-butadiene copolymer rubber, Nitrogen adsorption specific surface area (N 2 SA) is 100 to 500m 2 50 to 200 parts by mass of carbon black having a molecular weight of 1.0 to 1.0 g / g, 5 to 80 parts by mass of a terpene resin having a softening point of 100° C. or higher, and A rubber composition for tire cap treads, comprising 5 to 50 parts by mass of an ester plasticizer.

2. 2. The rubber composition for tire cap treads according to claim 1, wherein a mass ratio of said ester-based plasticizer: said terpene resin is 1:0.8-3.

3. 2. The rubber composition for a tire cap tread according to claim 1, wherein the ester-based plasticizer includes a glycerin fatty acid ester.

4. 4. The rubber composition for tire cap treads according to claim 3, wherein the glycerin fatty acid ester is a glycerin fatty acid monoester.

5. The rubber composition for tire cap tread according to claim 1, further comprising 5 to 50 parts by mass of a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more, based on 100 parts by mass of the styrene-butadiene copolymer rubber.

6. A tire using the rubber composition for tire cap tread according to claim 1 in the cap tread.

Citation Information

Patent Citations

  • Rubber composition for use in tire tread

    JP2009209262A

  • Rubber composition for tire tread and pneumatic tire obtained using the same

    JP2011111489A

  • Rubber composition for tire outer layer and pneumatic tire

    JP2016204504A

  • Rubber composition for tire, and pneumatic tire

    JP2019183010A