Rubber composition for tire cap tread, and tire using the same
A tire tread composition using styrene-butadiene copolymer rubber, silica, terpene resin, and ester plasticizer addresses the challenge of balancing wet and initial grip with abrasion resistance, improving overall tire performance.
Patent Information
- Application Number
- JP2023044918
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional tire compositions struggle to simultaneously enhance wet grip performance, initial grip performance, and abrasion resistance, often compromising on one or more properties due to the use of high specific surface area fillers, high softening point resins, and liquid plasticizers.
A rubber composition for tire cap treads comprising specific amounts of styrene-butadiene copolymer rubber, silica with a nitrogen adsorption specific surface area of 200 m²/g, terpene resin with a softening point of 60°C or higher, and ester plasticizer, along with optional diene rubbers and additives, to achieve improved grip and wear resistance.
The composition achieves enhanced wet grip, initial grip, and wear resistance by optimizing the blend of silica, terpene resin, and ester plasticizer, balancing performance across various conditions.
Smart Images

Figure 2024134631000001 
Figure 2024134631000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for tire cap treads and a tire using the same, and more particularly to a rubber composition that can simultaneously improve wet grip performance, initial grip performance and abrasion resistance, and a studless tire using the same. [Background technology]
[0002] In general, pneumatic tires for racing are prepared for dry road running and wet road running, and the optimal tire is selected according to the weather and road surface conditions during driving. Here, for racing tires for driving on wet roads, measures such as blending a large amount of high specific surface area filler, high softening point resin, liquid plasticizer, etc. are taken to improve wet grip performance. However, blending a large amount of the high specific surface area filler and high softening point resin has a problem that, for example, operability (initial grip performance) at low temperatures is reduced due to an increase in low temperature hardness. In addition, blending a large amount of liquid plasticizer has a problem that the breaking strength is reduced and the wear resistance is deteriorated.
[0003] Patent Document 1 listed below discloses a rubber composition for tires that contains a rubber component having a styrene-butadiene rubber content of 40 to 80 mass% and a butadiene rubber content of 10 to 35 mass%, silica in an amount of 80 parts by mass or more per 100 parts by mass of the rubber component, and a terpene resin in an amount of 10 to 60 parts by mass per 100 parts by mass of the rubber component, and that satisfies the following formula (A). (A) α / β≦3 α: Styrene content of styrene-butadiene rubber [mass%] β: Content of terpene resin per 100 parts by mass of rubber component [parts by mass] However, with the above-mentioned conventional techniques, it has been difficult to simultaneously improve wet grip performance, initial grip performance, and abrasion resistance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-183010 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a rubber composition for a tire cap tread, which can simultaneously improve wet grip performance, initial grip performance and abrasion resistance, and a tire using the same. [Means for solving the problem]
[0006] As a result of intensive research, the present inventors have found that a rubber composition in which a specific styrene-butadiene copolymer rubber is blended with silica and a terpene resin having specific properties and an ester-based plasticizer in specific amounts can solve the above problems, and have thus completed the present invention.
[0007] That is, the present invention provides a method for producing a rubber composition having a nitrogen adsorption specific surface area (N 2 SA) is 200m 2 The rubber composition for tire cap treads is characterized by comprising 120 to 200 parts by mass of silica having a silica content of less than 1 / g, 15 to 80 parts by mass of a terpene resin having a softening point of 60°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer. The present invention also provides a tire using the above rubber composition for tire cap tread in a cap tread. Effect of the Invention
[0008] The rubber composition for tire cap treads of the present invention has a nitrogen adsorption specific surface area (N 2 SA) is 200m 2The tire is characterized by a blend of 120 to 200 parts by mass of silica having a molecular weight of less than 1 / g, 15 to 80 parts by mass of a terpene resin having a softening point of 60°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer, thereby enabling the tire to simultaneously improve wet grip performance, initial grip performance, and abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will now be described in further detail.
[0010] (Rubber component) The rubber component used in the rubber composition for tire cap treads of the present invention (hereinafter, sometimes simply referred to as rubber composition) is styrene-butadiene copolymer rubber (SBR). In the present invention, it is preferable that all of the rubber components are SBR, but if necessary, any diene rubber that can be blended in a normal rubber composition, such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), acrylonitrile-butadiene copolymer rubber (NBR), ethylene-propylene-diene terpolymer (EPDM), etc., can also be used in combination. The SBR used in the present invention is not particularly limited in its molecular weight or microstructure, and may be terminally modified with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl groups, or the like, or may be epoxidized. In addition, the SBR used in the present invention preferably has a styrene content of 30% by mass or more. By satisfying this styrene content, the wet grip performance, driving stability, and abrasion resistance of the tire can be improved. The styrene content is more preferably 33 to 50% by mass.
[0011] (silica) The silica used in the present invention has a nitrogen adsorption specific surface area N 2 SA is 200m 2 / g (hereinafter referred to as specific silica). Silica N 2 SA is 200m 2 If it exceeds 1 / g, the initial grip performance and abrasion resistance are deteriorated. More preferred N of the silica used in the present invention 2 SA is 120~200m 2 / g. Furthermore, 2 SA shall be measured in accordance with JIS K6217-2.
[0012] (Terpene resin) Examples of the terpene resin used in the present invention include terpene resins such as α-pinene, β-pinene, dipentene, and limonene. From the viewpoint of improving the effects of the present invention, the terpene resin is preferably an aromatic modified terpene resin. The aromatic modified terpene resin can be obtained, for example, by polymerizing the terpene resin with an aromatic compound other than phenol. Examples of the aromatic compound include styrene, α-methylstyrene, vinyltoluene, and indene. The content of the aromatic compound in the aromatic modified terpene resin is preferably 10 to 50% by mass. Moreover, the softening point of the terpene resin used in the present invention is preferably 60°C or higher, and more preferably 80 to 170°C, from the viewpoint of improving the effects of the present invention.
[0013] (Ester plasticizer) Examples of the ester-based plasticizer used in the present invention include vegetable oils, fatty acid esters such as glycerin fatty acid monoesters, glycerin fatty acid diesters, and glycerin fatty acid triesters, processed vegetable oils, etc. Among these, those obtained from processed vegetable oils are preferred.
[0014] Examples of vegetable oils include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil.
[0015] As the fatty acid ester, for example, fatty acid esters represented by the following formula can be suitably used.
[0016] [ka]
[0017] (In the formula, R 11 R represents a linear or branched alkyl group having 1 to 8 carbon atoms, a linear or branched alkenyl group having 1 to 8 carbon atoms, or a linear or branched alkyl group having 2 to 6 carbon atoms substituted with 1 to 5 hydroxyl groups. 12 represents an alkyl group or alkenyl group having 11 to 21 carbon atoms.
[0018] R 11 Examples of R include a methyl group, an ethyl group, a 2-ethylhexyl group, an isopropyl group, an octyl group, and groups in which these groups are substituted with 1 to 5 hydroxyl groups. 12 Examples of the alkyl group include linear or branched alkyl groups and alkenyl groups such as lauryl group, myristyl group, palmityl group, stearyl group, and oleyl group.
[0019] Examples of fatty acid esters include alkyl oleates, alkyl stearates, alkyl linoleates, and alkyl palmitates. Among these, alkyl oleates (methyl oleate, ethyl oleate, 2-ethylhexyl oleate, isopropyl oleate, octyl oleate, and the like) are preferred. In this case, the content of alkyl oleates in 100% by mass of fatty acid ester is preferably 80% by mass or more.
[0020] Examples of fatty acid esters include fatty acid monoesters and fatty acid diesters of fatty acids (oleic acid, stearic acid, linoleic acid, palmitic acid, etc.) and alcohols (ethylene glycol, glycerol, trimethylolpropane, pentaerythritol, erythritol, xylitol, sorbitol, dulcitol, mannitol, inositol, etc.). Among these, glycerin fatty acid esters are preferred, and glycerin fatty acid monoesters are more preferred. As the fatty acid, oleic acid is particularly preferred. In this case, the content of oleic acid monoester in the total amount of fatty acid monoesters and fatty acid diesters (100% by mass) is preferably 80% by mass or more. Furthermore, modified products are particularly preferred.
[0021] (Rubber composition blend ratio) The rubber composition of the present invention is characterized in that it contains 120 to 200 parts by mass of the specific silica, 15 to 80 parts by mass of a terpene resin having a softening point of 60°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer, relative to 100 parts by mass of SBR. If the amount of the specific silica blended is less than 120 parts by mass, the grip performance will decrease, whereas if it exceeds 200 parts by mass, the abrasion resistance will decrease. If the amount of the terpene resin is less than 15 parts by mass, the amount is too small to achieve the effects of the present invention, whereas if it exceeds 80 parts by mass, the initial grip performance decreases. If the amount of the ester plasticizer is less than 5 parts by mass, the amount is too small to achieve the effects of the present invention, whereas if it exceeds 50 parts by mass, the grip performance will decrease.
[0022] The amount of the specific silica to be blended is preferably 120 to 160 parts by mass relative to 100 parts by mass of SBR. The amount of the terpene resin to be mixed is preferably 30 to 80 parts by mass based on 100 parts by mass of SBR. The amount of the ester plasticizer to be mixed is preferably 10 to 40 parts by mass based on 100 parts by mass of SBR.
[0023] Here, the mass ratio of the ester plasticizer to the terpene resin is preferably 1:0.5 to 3 when the former is taken as 1. According to this blending ratio, when biomass oil is used as the liquid plasticizer from the viewpoint of environmental friendliness, it is possible to improve wet grip performance, initial grip performance, and abrasion resistance. The mass ratio of the ester plasticizer:the terpene resin is more preferably 1:1 to 2.5.
[0024] (Other ingredients) In addition to the above-mentioned components, the rubber composition of the present invention may contain various additives that are generally compounded in rubber compositions, such as vulcanizing or crosslinking agents, vulcanizing or crosslinking accelerators, various fillers such as carbon black, clay, talc, and calcium carbonate, antioxidants, plasticizers, resins, and curing agents, and these additives can be kneaded in a general manner to form a composition, which can be used for vulcanization or crosslinking. The amounts of these additives may be conventional amounts, so long as they do not go against the object of the present invention.
[0025] (Terpene phenol resin) From the viewpoint of improving the effect, the rubber composition of the present invention preferably contains a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more. Terpene phenol resins are known and are obtained by reacting a terpene compound with phenol, and any terpene phenol resin can be used in the present invention as long as it satisfies the above-mentioned conditions of acid value and hydroxyl value. The aromatic terpene resin described above is a polymer of a terpene compound and an aromatic compound other than phenol, and is distinguished from the above-mentioned terpene phenol resin. The acid value of the terpene phenol resin is more preferably from 40 to 150 mgKOH / g, and the hydroxyl value is more preferably from 10 to 100 mgKOH / g. The softening point of the terpene phenol resin used in the present invention is preferably 85 to 180°C.
[0026] The amount of the terpene phenol resin to be blended is preferably 5 to 50 parts by mass, and more preferably 10 to 40 parts by mass, based on 100 parts by mass of SBR.
[0027] In this specification, the acid value and the hydroxyl value can be measured in accordance with JIS K 0070: 1992. The softening point can be measured in accordance with JIS K 6220-1: 2001.
[0028] (Aluminum Hydroxide) From the viewpoint of improving the effect, the rubber composition of the present invention is preferably blended with aluminum hydroxide. The blending amount of aluminum hydroxide is, for example, 5 to 50 parts by mass, preferably 10 to 40 parts by mass, per 100 parts by mass of the styrene-butadiene copolymer rubber having a styrene content of 30% by mass or more.
[0029] The rubber composition of the present invention can improve wet grip performance, initial grip performance and abrasion resistance at the same time, and therefore can be suitably used for tire treads, particularly cap treads, preferably racing tire treads, particularly cap treads. The tire of the present invention is preferably a pneumatic tire, and can be filled with air, an inert gas such as nitrogen, and other gases. EXAMPLES
[0030] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0031] Standard Example, Examples 1-6, Comparative Examples 1-3 In the formulation (parts by mass) shown in Table 1, the components other than the vulcanization system (vulcanization accelerator, sulfur) were kneaded in a 1.7-liter closed Banbury mixer for 5 minutes, then discharged outside the mixer and cooled at room temperature. The composition was then placed back into the same Banbury mixer, and the vulcanization system was added and kneaded to obtain a rubber composition. The obtained rubber composition was then press-vulcanized in a specified mold at 150°C for 30 minutes to prepare a vulcanized rubber test piece. The physical properties of the obtained vulcanized rubber test piece were measured using the test methods shown below.
[0032] Hardness (20° C.): Measured at 20° C. in accordance with JIS K6253. The results are expressed as an index, with the standard example being 100. The smaller the index, the more excellent the initial grip performance.
[0033] Wet grip performance: Based on JIS K6394, tan δ (0°C) was measured using a viscoelasticity spectrometer manufactured by Toyo Seiki Seisakusho Co., Ltd. under the conditions of initial strain = 10%, amplitude = ±2%, and frequency = 20Hz, and the wet grip performance was evaluated based on this value. The results were expressed as an index with the standard example being 100. The higher the index, the better the wet grip performance.
[0034] M300: 300% modulus (M300) at 20°C was measured according to JIS K6251. The results were expressed as an index with the standard example being 100. A larger index indicates better abrasion resistance.
[0035] The results are also shown in Table 1.
[0036] [Table 1]
[0037] *1: SBR-1 (Nipol 1739 manufactured by Zeon Corporation, styrene content = 40% by mass, oil extension content = 37.5 parts by mass per 100 parts by mass of SBR.) *2: SBR-2 (Nipol 1723 manufactured by Zeon Corporation, styrene content = 23% by mass, oil extension content = 37.5 parts by mass per 100 parts by mass of SBR) *3: Carbon black (Tokai Carbon Co., Ltd., Seast 9, N 2 SA=142m 2 / g) *4: Aluminum hydroxide (BF013 manufactured by Nippon Light Metal Co., Ltd.) *5: Silica-1 (EVONIK ULTRASIL 9100GR, N 2 SA=237m 2 / g) *6: Silica-2 (EVONIK ULTRASIL 7000GR, N 2 SA=176m 2 / g) *7: Resin-1 (Yasuhara Chemical Co., Ltd. YS Resin TO-125, aromatic modified terpene resin, softening point = 125°C) *8: Resin-2 (Tamanol 803L, terpene phenol resin, acid value = 50 mg KOH / g, hydroxyl value = 15 mg KOH / g, manufactured by Arakawa Chemical Industries, Ltd.) *9: Oil (Showa Shell Sekiyu Co., Ltd. Extract No. 4S, Tg=-41℃) *10: Ester-based plasticizer (H&R Pionier TP130B, glycerin fatty acid monoester of high oleic sunflower oil, Tg=-110℃) *11: Silane coupling agent (EVONIK Si69) *12: Stearic acid (Beads Stearic Acid YR manufactured by NOF Corporation) *13: Zinc oxide (3 types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd.) *14: Anti-aging agent (Flexis 6PPD) *15: Vulcanization accelerator (Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) *16: Sulfur (Kinka-in oil-filled fine sulfur manufactured by Tsurumi Chemical Industry Co., Ltd.)
[0038] From the results in Table 1, the rubber compositions of Examples 1 to 6 have a nitrogen adsorption specific surface area (N2 SA) is 200m 2 The tire contains 120 to 200 parts by mass of silica with a viscosity of less than 1 / g, 15 to 80 parts by mass of a terpene resin with a softening point of 60°C or higher, and 5 to 50 parts by mass of an ester-based plasticizer, which results in improved wet grip performance, initial grip performance, and abrasion resistance compared to the standard example. On the other hand, in Comparative Example 1, the amount of styrene in the SBR was less than the lower limit specified in the present invention, and a plasticizer other than an ester-based plasticizer was used, so that the wet grip performance and abrasion resistance were deteriorated. In Comparative Example 2, the nitrogen adsorption specific surface area (N 2 SA) is 200m 2 / g and the use of plasticizers other than ester-based plasticizers resulted in a deterioration in initial grip performance and abrasion resistance. In Comparative Example 3, a plasticizer other than the ester-based plasticizer was used, and therefore the initial grip performance was deteriorated.
[0039] The present invention includes the following aspects. Embodiment 1: For 100 parts by mass of styrene-butadiene copolymer rubber with a styrene content of 30% by mass or more, Nitrogen adsorption specific surface area (N 2 SA) is 200m 2 120 to 200 parts by mass of silica less than 1 / g, 15 to 80 parts by mass of a terpene resin having a softening point of 60° C. or higher, and A rubber composition for tire cap treads, comprising 5 to 50 parts by mass of an ester-based plasticizer. Embodiment 2: 2. The rubber composition for tire cap treads according to embodiment 1, wherein a mass ratio of the ester plasticizer:the terpene resin is 1:0.5-3. Embodiment 3: 3. The rubber composition for tire cap treads according to embodiment 1 or 2, wherein the ester plasticizer comprises a glycerin fatty acid ester. Embodiment 4: The rubber composition for tire cap treads according to embodiment 3, wherein the glycerin fatty acid ester is a glycerin fatty acid monoester. Embodiment 5: The rubber composition for tire cap tread according to any one of embodiments 1 to 4, further comprising 5 to 50 parts by mass of a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more, based on 100 parts by mass of the styrene-butadiene copolymer rubber. Embodiment 6: The rubber composition for tire cap treads according to any one of embodiments 1 to 5, further comprising 5 to 50 parts by mass of aluminum hydroxide blended with 100 parts by mass of the styrene-butadiene copolymer rubber having a styrene content of 30% by mass or more. Embodiment 7: A tire using the rubber composition for a tire cap tread according to any one of the first to sixth embodiments for a cap tread.
Claims
1. For 100 parts by mass of styrene-butadiene copolymer rubber having a styrene content of 30% by mass or more, Nitrogen adsorption specific surface area (N 2 SA) is 200m 2 / g or less silica, 120 to 200 parts by mass, 15 to 80 parts by mass of a terpene resin having a softening point of 60° C. or higher, and A rubber composition for tire cap treads, comprising 5 to 50 parts by mass of an ester plasticizer.
2. 2. The rubber composition for tire cap treads according to claim 1, wherein a mass ratio of said ester-based plasticizer: said terpene resin is 1:0.5-3.
3. 2. The rubber composition for a tire cap tread according to claim 1, wherein the ester-based plasticizer includes a glycerin fatty acid ester.
4. 4. The rubber composition for tire cap treads according to claim 3, wherein the glycerin fatty acid ester is a glycerin fatty acid monoester.
5. The rubber composition for tire cap tread according to claim 1, further comprising 5 to 50 parts by mass of a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more, based on 100 parts by mass of the styrene-butadiene copolymer rubber.
6. The rubber composition for tire cap treads according to claim 1, further comprising 5 to 50 parts by mass of aluminum hydroxide blended with 100 parts by mass of the styrene-butadiene copolymer rubber having a styrene content of 30% by mass or more.
7. A tire using the rubber composition for tire cap tread according to claim 1 in the cap tread.
Citation Information
Patent Citations
Rubber composition for tire tread and pneumatic tire
JP2011079880A
Rubber composition for tire
JP2018039917A
Pneumatic tire
JP2019026791A
Rubber composition and tire
JP2020094108A
Rubber composition for tire, and pneumatic tire
JP2019183010A
Cited By
Process oil for rubber
WO2026141635A1