Resin composition

The resin composition addresses adhesion and gas barrier issues in EVOH-polyolefin laminates by blending ethylene-vinyl alcohol copolymer into saponified ethylene-vinyl acetate copolymer, enhancing adhesion and moldability while maintaining gas barrier performance.

JP2024134767APending Publication Date: 2024-10-04TOSOH CORP

Patent Information

Application Number
JP2023045121
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing resin compositions for laminates with ethylene-vinyl alcohol copolymer (EVOH) and polyolefins face issues with adhesion, gas barrier properties, and moldability, leading to high equipment costs and poor film appearance due to viscosity increase and gelation during processing.

Method used

A resin composition is developed by blending a specific amount of ethylene-vinyl alcohol copolymer into a saponified ethylene-vinyl acetate copolymer, forming a matrix with layered domains of ethylene-vinyl alcohol copolymer, achieving high gas barrier performance and adhesion without impairing adhesive properties.

Benefits of technology

The resin composition exhibits excellent adhesion to polyolefin resins, maintains gas barrier properties, and improves film appearance and moldability, suitable for use in laminates with reduced equipment costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134767000001_ABST
    Figure 2024134767000001_ABST
Patent Text Reader

Abstract

To provide a resin composition which has excellent gas barrier properties, adhesion, film appearance, moldability and mechanical properties and comprises an ethylene-vinyl acetate copolymer saponification product and an ethylene-vinyl acetate copolymer.SOLUTION: There is provided a resin composition in which an ethylene-vinyl acetate copolymer (B) is present in a matrix of an ethylene-vinyl acetate copolymer saponification product (A) having a vinyl acetate content of 0.3 to 20 mol% and a vinyl alcohol content of 1 to 20 mol% as a domain, 50% or more of the form of (B) has a layered domain or a structure in which a part of the layered domain is three-dimensionally connected and the domain has an aspect ratio of 5 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition containing a saponified ethylene-vinyl acetate copolymer and an ethylene-vinyl alcohol copolymer. [Background technology]

[0002] Ethylene-vinyl alcohol copolymer (hereinafter sometimes referred to as EVOH), which has excellent gas barrier properties, aroma retention, solvent resistance, etc., is used for various purposes in packaging materials made of thermoplastic resins for food, beverages, medicines, etc., to prevent deterioration of the contents. However, EVOH is hydrophilic, and gas barrier properties, etc., decrease due to moisture absorption, so it is generally known to be used as an intermediate layer in laminates with polyolefins such as polyethylene and polypropylene, which have excellent water resistance.

[0003] Since EVOH has many hydroxyl groups in the molecule, it has very low affinity with polyolefins such as polyethylene and polypropylene that do not have polar groups, and the two generally do not adhere to each other. Therefore, for EVOH, which is difficult to adhere to polyolefins, a method has been proposed in which a graft-modified ethylene-based resin composition grafted with an unsaturated carboxylic acid or its derivative (see, for example, Patent Documents 1 and 2) or an ethylene-vinyl acetate copolymer hydrolyzate (see, for example, Patent Document 3) is used as an adhesive between a polyolefin resin layer and an EVOH layer.

[0004] However, the former graft-modified ethylene resin composition grafted with unsaturated carboxylic acid or its derivative has excellent adhesiveness, but due to its high reactivity with EVOH, when it is repeatedly kneaded or added to EVOH, the resin that remains in the extruder or die increases in viscosity and becomes discolored and gelled, resulting in the presence of many fish eyes and gel-like substances in the product, which reduces the commercial value. In addition, the latter ethylene-vinyl acetate copolymer hydrolyzate does not discolor or gel even when it is repeatedly kneaded or added to EVOH, and although the adhesiveness to EVOH is improved by adding a tackifying resin to the ethylene-vinyl acetate copolymer hydrolyzate, the effect is small, and it often peels off when subjected to small impacts or friction during transportation or use, and sufficient adhesiveness was not obtained.

[0005] Furthermore, packaging materials containing EVOH must be configured with at least three types and five layers including a polyolefin resin layer / adhesive layer / EVOH layer / adhesive layer / polyolefin resin layer, or four types and six layers including a polyolefin resin layer / adhesive layer / EVOH layer / adhesive layer / regrind layer / polyolefin resin layer. However, a multilayer molding machine for producing such a multilayer laminate of five or more layers generally has a problem of very high capital investment costs.

[0006] Therefore, there has been a demand for the production of a laminate that can be produced in a three-layer structure using a general-purpose molding machine.For example, Patent Documents 4, 5, and 6 propose a method for producing a three-layer structure by using a hydrolyzate of a melt-kneaded product containing a thermoplastic resin, an ethylene-vinyl ester copolymer having a vinyl ester content 5 mol% or more higher than that of the thermoplastic resin, and a modified product in which the thermoplastic resin and the ethylene-vinyl ester copolymer are grafted, and blending the hydrolyzate with the EVOH layer to improve adhesion with the polyolefin resin layer. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2007-161881 A [Patent Document 2] JP 2000-248128 A [Patent Document 3] JP 2001-200124 A [Patent Document 4] JP 2018-154701 A [Patent Document 5] JP2018-145401 Public Relations [Patent Document 6] Patent Publication No. 2021-154494 Summary of the Invention [Problem to be solved by the invention]

[0008] However, when laminates produced by actual film molding, direct blow molding, etc. using the resin compositions described in Patent Documents 4 and 5 were evaluated, problems occurred in which sufficient adhesive strength and gas barrier properties could not be obtained. In addition, the method described in Patent Document 6 also caused problems such as molding defects such as bubbles shaking during molding, and film appearance was impaired by film streaks, etc. The present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a resin composition that has excellent adhesion to a polyolefin resin layer and also has gas barrier properties, film appearance, moldability, etc. [Means for solving the problem]

[0009] As a result of intensive research aimed at solving the above problems, the inventors have discovered that by blending a specified amount of EVOH with a specific saponified ethylene-vinyl acetate copolymer, it is possible to impart high gas barrier performance to EVOH without impairing the adhesion of the saponified ethylene-vinyl acetate copolymer to polyolefins, and have thus completed the present invention.

[0010] That is, the respective aspects of the present invention are as follows [1] to []. [1] A resin composition comprising a matrix of saponified ethylene-vinyl acetate copolymer (A) having a vinyl acetate content of 0.3-20 mol % and a vinyl alcohol content of 1-20 mol %, in which an ethylene-vinyl alcohol copolymer (B) exists as domains, and 50% or more of the morphology of (B) has a lamellar domain or a structure in which parts of the lamellar domains are three-dimensionally connected, and the aspect ratio of the domains is 5 or more. [2] The resin composition according to [1], wherein a weight ratio (A / B) of the saponified ethylene-vinyl acetate copolymer (A) to the ethylene-vinyl alcohol copolymer (B) is 80 / 20 to 50 / 50. [3] The resin composition according to [1] or [2], wherein the saponified ethylene-vinyl acetate copolymer (A) is a hydrolysate of a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3), and has a melt mass flow rate of 0.3 to 5.0 g / min as measured in accordance with JIS K6922-1: (a1) An ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less (a2) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 45% by weight or more (a3) Compatibilizer [4] The resin composition according to any one of [1] to [3], wherein the ethylene-vinyl alcohol copolymer (B) has an ethylene content of 27 to 48 mol% and a melt mass flow rate measured at 190°C in accordance with JIS K6922-1 of 1.5 to 30 g / min. [5] When the shear rate and apparent shear viscosity of the saponified ethylene-vinyl acetate copolymer (A) and the ethylene-vinyl alcohol copolymer (B) were measured using a capillary rheometer at 200°C and under the conditions of orifice length L / orifice diameter D = 20 / 1, the apparent shear viscosity was measured at a shear rate of 100 to 150 sec -1 The resin composition according to any one of [1] to [4], wherein the viscosity ratio (A / B) is 0.25 to 2.0. [6] The resin composition according to any one of [1] to [5], wherein a melt mass-flow rate ratio (A / B) of the saponified ethylene-vinyl acetate copolymer (A) to the ethylene-vinyl alcohol copolymer (B) measured in accordance with JIS K6922-1 is 0.01 to 3.5. [7] The resin composition according to any one of [1] to [6], wherein the total of the saponified ethylene-vinyl acetate copolymer (A) and the ethylene-vinyl alcohol copolymer (B) contains 1 to 60 parts by weight of polyethylene (C) per 100 parts by weight. [8] A laminate having a gas barrier resin layer made of the resin composition according to any one of [1] to [7], and at least one polyolefin resin layer adjacent to the gas barrier resin layer, wherein the polyolefin resin has a melt mass flow rate of 0.1 to 3.0 g / 10 min. [9] A laminate having a gas barrier resin layer made of the resin composition according to any one of [1] to [7], and a polyolefin resin layer on both sides adjacent to the gas barrier resin layer, wherein the polyolefin resin has a melt mass flow rate of 0.1 to 3.0 g / 10 min.

[10] The laminate according to [8], wherein the polyolefin resin is an ethylene-based polymer or an ionomer resin.

[11] The laminate according to [9], wherein the polyolefin resin is an ethylene-based polymer or an ionomer resin. Effect of the Invention

[0011] When the resin composition of the present invention is made into a film, it has excellent gas barrier properties, adhesive properties, film appearance, moldability and mechanical properties. [Brief description of the drawings]

[0012] [Figure 1] 1A and 1B are a perspective view and a cross-sectional view of a laminate according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below.

[0014] In one embodiment of the resin composition of the present invention, an ethylene-vinyl alcohol copolymer (B) exists as domains in a matrix of a saponified ethylene-vinyl acetate copolymer (A) having a vinyl acetate content of 0.3 to 20 mol % and a vinyl alcohol content of 1 to 20 mol %, and 50% or more of the morphology of (B) has a structure in which lamellar domains are formed or parts of the lamellar domains are three-dimensionally connected, and the aspect ratio of the domains is 5 or more.

[0015] The above-mentioned saponified ethylene-vinyl acetate copolymer (A) (hereinafter sometimes abbreviated as (A), (A) component, or component (A)) is a terpolymer mainly composed of ethylene units, vinyl acetate units, and vinyl alcohol units.

[0016] Component (A) can be obtained, for example, by hydrolyzing (saponifying) a portion of the vinyl acetate constituting an ethylene-vinyl acetate copolymer. The method for hydrolyzing the ethylene-vinyl acetate copolymer is not particularly limited, and for example, an ethylene-vinyl acetate copolymer can be produced according to a known method, and then the copolymer can be hydrolyzed to produce component (A). An acid catalyst or an alkali catalyst can be used for hydrolysis of the ethylene-vinyl acetate copolymer, and examples of such methods include a method in which pellets of the ethylene-vinyl acetate copolymer are directly hydrolyzed in an alkali, and a method in which the ethylene-vinyl acetate copolymer is saponified and extruded in a twin-screw extruder.

[0017] The degree of saponification of component (A) can be calculated from the vinyl acetate content of the ethylene-vinyl acetate copolymer before saponification and the saponified ethylene-vinyl acetate copolymer (A) according to the following formula. Formula: Degree of saponification (mol%) = 100 × {(vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) - (vinyl acetate content of saponified ethylene-vinyl acetate copolymer)} / (vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) If the saponification degree of the component (A) is 10 mol % or more, compatibility with EVOH is good, and it is more preferably 20 mol % or more, and most preferably 30 mol % or more.

[0018] In order to achieve both adhesion to polyolefin and compatibility with EVOH, the (A) component has a vinyl acetate content of 0.3 to 20 mol% and a vinyl alcohol content of 1 to 20 mol%, preferably a vinyl acetate content of 0.5 to 18 mol% and a vinyl alcohol content of 2 to 20 mol%. Of these, the vinyl acetate content is most preferably 1.0 to 15 mol% and a vinyl alcohol content of 3 to 20 mol%. The total value of the ethylene content, the vinyl acetate content and the vinyl alcohol content is 100 mol%. If the vinyl alcohol content is less than 1.0 mol%, the compatibility with EVOH decreases and the mechanical properties of the resin composition are significantly impaired, and if the vinyl acetate content and / or the vinyl alcohol content exceeds 20 mol%, the adhesion to polyolefin decreases, which is not preferable. The (A) component may be used alone or in combination of two or more types.

[0019] From the viewpoint of molding processability, the (A) component has a melt mass flow rate (hereinafter sometimes abbreviated as MFR) measured in accordance with JIS K6924-1 (under conditions of 190°C and a load of 2160 g) of preferably 0.3 to 5.0 g / 10 min, and most preferably 0.5 to 5.0 g / 10 min.

[0020] The component (A) is preferably a hydrolysate of a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3). (a1) An ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less (a2) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 45% by weight or more (a3) Compatibilizer The component (a1) ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less is a copolymer having ethylene units and vinyl acetate units. The method for producing the component (a1) is not particularly limited as long as it is possible to produce an ethylene-vinyl acetate copolymer, and examples of the method include the well-known high-pressure radical polymerization method and ionic polymerization method. Such a resin can be conveniently selected from commercially available products, and an ethylene-vinyl acetate copolymer produced by a high-pressure radical polymerization method is commercially available from Tosoh Corporation under the product name Ultrathene.

[0021] From the viewpoints of molding stability and dispersibility with EVOH, the component (a1) preferably has a melt mass flow rate, measured in accordance with JIS K6924-1 (under conditions of 190°C and a load of 2160 g), of 0.1 to 100 g / 10 min, more preferably 0.1 to 10 g / 10 min, and most preferably 0.5 to 5.0 g / 10 min.

[0022] The component (a2) ethylene-vinyl acetate copolymer has a vinyl acetate content of 45% by weight or more. From the viewpoint of compatibility with the component (a1), the vinyl acetate content is preferably in the range of 45 to 85% by weight, and most preferably in the range of 48 to 80% by weight.

[0023] The method for producing the ethylene-vinyl acetate copolymer in component (a2) is not limited, but examples thereof include known production methods such as high-pressure radical polymerization, solution polymerization, and latex polymerization, and these are commercially available from ARLANXEO under the trade names LEVAPREN and LEVAMELT.

[0024] The compatibilizer constituting the above component (a3) ​​is not particularly limited as long as it can improve the compatibility between (a1) and (a2), and examples thereof include ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-methyl acrylate copolymer, ionomer resin, etc., and is appropriately selected in consideration of the compatibility between (a1) and (a2) and the cost. Among them, it is preferable to use an ethylene-vinyl acetate copolymer having a vinyl acetate content of 21 to 44% by weight from the viewpoint of cost, and one type alone or a combination of two or more types may be used, but using two or more types of ethylene-vinyl acetate copolymers having different vinyl acetate contents reduces the difference in the vinyl acetate content of each component, thereby improving the compatibility between (a1) and (a2). Such ethylene-vinyl acetate copolymers are commercially available from Tosoh Corporation under the trade name Ultrathene, and from ARLANXEO under the trade names LEVAPRENE and LEVAMELT.

[0025] The component (A) is a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3), which is obtained by crosslinking a composition containing the components (a1) to (a3). The method for crosslinking the composition containing the components (a1) to (a3) ​​is not particularly limited as long as it can be modified by crosslinking, and is appropriately selected in consideration of reactivity, etc., but from the viewpoint of productivity, it is preferable to add a crosslinking agent (a4) to the above components (a1) to (a3), and it is preferable to use an organic peroxide as the crosslinking agent (a4).

[0026] The organic peroxide of the crosslinking agent (a4) is not particularly limited as long as it is an organic peroxide, and examples thereof include dicumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 1,1-di(t-butylperoxy)cyclohexane, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, 1,3-bis(t-butylperoxyisopropyl)benzene, 1,1-bis(t-butylperoxy)-3,3,5-trimethylperoxide, and the like. Examples of the peroxides include ethylcyclohexane, 1,3-di-(t-butylperoxy)-diisopropylbenzene, n-butyl-4,4-bis(t-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, t-butyl peroxybenzoate, t-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, t-butylcumyl peroxide, etc. These can be used alone or in combination of two or more.

[0027] Among them, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 1,1-di(t-butylperoxy)cyclohexane are preferably used from the viewpoint of reactivity. In addition, a crosslinking assistant such as triallyl isocyanurate or divinylbenzene may be used together with the above crosslinking agent, if necessary. The amount of the crosslinking agent (a4) is preferably in the range of 0.005 to 1 part by weight per 100 parts by weight of the total of the components (a1) to (a3), which can improve the adhesion of the saponified ethylene-vinyl acetate copolymer (A) of the present invention to polyolefins and the compatibility with EVOH. A specific example of a production process for the component (A), which is a hydrolysate of a kneaded product containing the components (a1) to (a3) ​​and crosslinked products of (a1) to (a3), is as follows.

[0028] A dry blend of the components (a1) to (a3) ​​and the crosslinking agent (a4) is fed into the hopper of an extruder. At least a portion of the components (a1) to (a3) ​​and the crosslinking agent (a4) may be added from a side feeder or the like. Furthermore, two or more extruders may be used to sequentially melt-knead in stages. When mixing in advance, a Henschel mixer, a V blender, a ribbon blender, a tumbler, or the like may be used.

[0029] Furthermore, component (A) may contain additives, such as crosslinking aids, antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, and odor trapping agents, that are typically used in thermoplastic resins, as required.

[0030] The EVOH (B) (hereinafter sometimes abbreviated as (B), (B) component, or component (B)) is a copolymer mainly composed of ethylene units and vinyl alcohol units. The ethylene content of the (B) component is not particularly limited, but is preferably 27 to 48 mol% from the viewpoint of film formation stability and gas barrier properties. The saponification degree of the EVOH is preferably 96 mol% or more. By keeping the ethylene content and saponification degree in the EVOH within the above ranges, good gas barrier properties can be maintained. In addition to the ethylene units and vinyl alcohol units, the EVOH may have other structural units in small amounts, and the (B) component can be used alone or in a mixture of two or more types. Such EVOH is commercially available under the trade name EVAL from Kuraray Co., Ltd. and under the trade name Soarnol from Mitsubishi Chemical Corporation.

[0031] From the viewpoints of high gas barrier property and molding process stability, the MFR of component (B) (value measured at 190° C. under a load of 2160 g) is preferably 1.5 to 30 g / 10 min, and most preferably 1.5 to 20 g / 10 min.

[0032] The resin composition according to one embodiment of the present invention contains the above-mentioned components (A) and (B), and from the viewpoint of maintaining adhesiveness, it is necessary for component (A) to form a matrix (sea component) and component (B) to form domains (island component). Therefore, the weight ratio (A / B) of components (A) and (B) is preferably 80 / 20 to 50 / 50, more preferably 75 / 25 to 50 / 50, and most preferably 70 / 30 to 50 / 50.

[0033] In order to achieve high gas barrier properties, when cut and observed perpendicular to the flow direction (MD) of the resin, it is necessary that the component (A) forming the matrix has a domain in which the component (B) is dispersed in a layered form, or a structure in which parts of the layered domains are three-dimensionally connected. From the viewpoint of maintaining gas barrier properties, it is necessary that 50% or more of the component (B) has a layered domain, or a structure in which parts of the layered domains are three-dimensionally connected. In order to form such a dispersed structure, it is preferable that the component (A) and the component (B) have an appropriate melt viscosity ratio and MFR ratio within the range.

[0034] Specifically, the melt viscosity ratio (A / B) of components (A) and (B) constituting the gas barrier resin layer is preferably 0.25 to 2.0, and more preferably 0.3 to 1.8, when the shear rate and apparent shear viscosity of components (A) and (B) constituting the gas barrier resin layer are measured using a capillary rheometer under conditions of 200°C and orifice length L / orifice diameter D = 20 / 1.

[0035] The MFR ratio, as a melt mass flow rate ratio (A / B) measured in accordance with JIS K6922-1, is preferably 0.01 to 3.5, and more preferably 0.1 to 2.5.

[0036] The aspect ratio (long axis / short axis) of the lamellar domains derived from component (B) formed in the matrix-forming component (A) is 5 or more, more preferably 10 or more, and most preferably 20 or more. An aspect ratio of less than 5 is undesirable since the gas barrier properties are insufficient. From the viewpoint of maintaining the appearance of the film, the short axis of the lamellar domains of component (B) is preferably 10 μm or less, more preferably 5 μm or less, and most preferably 2.5 μm or less.

[0037] The resin composition may contain a component (C) other than the components (A) and (B) as long as the component (B) has a domain dispersed in a layered form or a structure in which the domains of the component (B) are three-dimensionally connected. For example, the component (C) may contain polyethylene. The polyethylene may contain one or more of high-pressure low-density polyethylene, high-density polyethylene, medium-density polyethylene, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, and ethylene-vinyl acetate copolymer. From the viewpoint of maintaining mechanical properties, the amount of the component (C) may be in the range of 1 to 60 parts by weight (the total of (A) and (B) is 100 parts by weight) based on the resin composition of the components (A) and (B) (the total of (A) and (B) is 101 to 160 parts by weight). However, if the blending ratio of component (B) is less than 20% of the total, component (B) may not disperse in a layered form and gas barrier properties may not be exhibited. Therefore, when the blending amount of (C) is large, the blending ratio of (B) is preferably 20% or more.

[0038] Furthermore, since it is necessary to disperse component (B) in a layer form, the MFR of component (C) (value measured at 190°C under a load of 2160 g) is preferably 0.01 to 20 g / 10 min, and more preferably 0.1 to 10 g / 10 min.

[0039] The method of melt-kneading the above resin composition (components (A) and (B) or components (A) and (C)) is not particularly limited as long as it is a melt-kneading device capable of uniformly dispersing each component, and production can be performed using a melt-kneading device that is commonly used for resins. Examples of melt-kneading devices include a single-screw extruder, a multi-screw extruder, a Banbury mixer, a pressure kneader, a rotating roll, and a Labo Plastomill. The melting temperature is preferably about 180 to 260°C. The kneading method of the resin composition (components (A)-(B) or (A)-(C)) does not necessarily have to be melt kneading, and a simple dry blend may also be used. Examples of the dry blending method include a Henschel mixer, a V blender, a ribbon blender, and a tumbler.

[0040] Furthermore, the above resin composition may contain additives, such as crosslinking assistants, antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, odor trapping agents, and the like, which are usually used in thermoplastic resins, as long as the object of the present invention is not impaired.

[0041] A laminate which is one embodiment of the present invention has a gas barrier resin layer made of the above-mentioned resin composition, and at least one polyolefin resin layer adjacent to the gas barrier resin layer, or on both sides adjacent to the gas barrier resin layer.

[0042] Since the resin composition has excellent gas barrier properties, it is possible to use the resin composition as a gas barrier resin layer of a laminate. For example, if necessary, at least one polyolefin resin layer may be disposed on the gas barrier resin layer made of the resin composition, or polyolefin resin layers may be disposed on both sides of the gas barrier resin layer.

[0043] The polyolefin constituting the polyolefin resin layer is not particularly limited as long as it has good adhesion to the component (A), but examples thereof include ethylene-based polymers such as high-pressure low-density polyethylene, high-density polyethylene, medium-density polyethylene, ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-octene copolymer, ethylene-4-methyl-1-pentene copolymer, ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and ethylene-methacrylic acid ester copolymer, and ionomer resins, and it is preferable to use one type alone or two or more types in combination. The ionomer resin is preferably an ethylene-methacrylic acid copolymer crosslinked with metal ions such as zinc or sodium, but the detailed structure is not particularly limited. The polyolefin resin layer can be appropriately selected depending on the required heat seal strength, water vapor barrier property, mechanical properties, and secondary processability.

[0044] The MFR of the polyolefin resin measured according to JIS K6922-1 (under conditions of 190°C and 2160g load) is preferably 0.1 to 3.0g / 10min, more preferably 0.2 to 2.5g / 10min, from the viewpoint of molding processability. If the MFR of the polyolefin resin exceeds 3.0g / 10min, the melt viscosity ratio does not match that of the gas barrier resin layer, which may cause unstable fluidization and deteriorate the appearance of the laminate. If the MFR of the polyolefin resin is less than 0.1g / 10min, the productivity may decrease.

[0045] In addition, the polyolefin resin may contain additives, such as crosslinking aids, antioxidants, lubricants, neutralizing agents, antiblocking agents, surfactants, slip agents, odor trapping agents, etc., which are generally used in thermoplastic resins, as long as the purpose of the present invention is not impaired. In addition, inorganic fillers and dyes and pigments may be contained as necessary for the purpose of reinforcement, weight increase, coloring, etc. Examples of inorganic fillers and dyes and pigments include calcium carbonate, talc, clay, synthetic silicon, titanium oxide, carbon black, and barium sulfate.

[0046] The laminate can be produced by any known method, including, for example, various coextrusion moldings such as coextrusion blow molding, coextrusion sheet molding, coextrusion cast molding, coextrusion inflation molding, coextrusion lamination molding, and coinjection molding, and can be molded into any shape such as a sheet, film, pipe, block, etc. In addition, by adopting a laminate structure with other materials, it is possible to impart the properties of the other materials, such as gas barrier properties, water vapor barrier properties, mechanical properties, oil resistance, and weather resistance, to the laminate.

[0047] A laminate in which the above-mentioned resin composition is used as a gas barrier resin layer can be used in molding machines that have a limit on the number of layers, and can be used not only for food, beverages, pharmaceuticals, agriculture, and cosmetics applications in which high gas barrier properties are required, but also for a wide variety of applications in which it is desirable to avoid releasing odors or fragrance components to the outside. [Explanation of symbols]

[0048] 1 Resin flow direction 2 vertical direction 3 Observation direction 4 Gas barrier resin layer 5 Polyolefin resin layer A: Ethylene-vinyl acetate copolymer saponification product B Ethylene-vinyl alcohol copolymer EXAMPLES

[0049] The resin composition of the present invention will be described in more detail below based on examples carried out to clarify the effects of the resin composition of the present invention. Note that the resin composition of the present invention is not limited by the following examples and comparative examples. <Saponification degree> The vinyl acetate content of the ethylene-vinyl acetate copolymer or saponified ethylene-vinyl acetate copolymer (A) obtained in the examples was measured in accordance with JIS K7192 (1999), and the degree of saponification (mol%) was calculated according to the following formula. Saponification degree (mol%) = 100 × {(vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) - (vinyl acetate content of saponified ethylene-vinyl acetate copolymer)} / (vinyl acetate content of ethylene-vinyl acetate copolymer before saponification) <mfr> The MFR was measured in accordance with JIS K6922-1 (1997), JIS K6924-2 (1997) or ISO1183-3. <Preparation of Laminate> The resin composition constituting the gas barrier resin layer was fed to the extruder (25 mmφ) forming the middle layer of a three-layer cast molding machine (manufactured by Plastics Engineering Research Institute Co., Ltd.) having a screw of 32 / 25 / 25 mmφ, and the polyolefin constituting the polyolefin resin layer was fed to two extruders (32 mmφ and 25 mmφ) forming the inner and outer layers, and all layers were extruded at 220°C and taken up at a take-up speed of 10 m / min to obtain a 55 μm thick laminate (two-kind three-layer film) with a polyolefin resin layer / gas barrier resin layer / polyolefin resin layer=20 μm / 15 μm / 20 μm. The obtained two-kind three-layer film was used to evaluate oxygen permeability, heat seal strength, and film appearance. Note that the / above means adjacent. <Aspect ratio> The obtained laminate (two-type three-layer film) was embedded in a rapid-curing epoxy resin to prepare a block for cutting. A cross section was prepared for each block using a cryomicrotome (-50°C). The cross section was prepared perpendicular to the resin flow direction (MD). The prepared surface was then stained with RuO4 overnight, and a cross section was prepared again. Finally, the prepared surface was coated with osmium, and observed using a SEM (FE-SEM JSM-7100F, manufactured by JEOL Ltd.). The aspect ratio was calculated from the minor and major axes of the observed domains of component (B). Note that cases in which component (B) was not observed as a domain were judged to be ×. <Oxygen permeability> The oxygen permeability was measured in accordance with JIS K7126-2 (2006) at 23°C and 65% humidity using two-type three-layer film (thickness 55μm) obtained in the examples, and the unit was cc / (m2·24h·atm). An oxygen permeability of less than 50 was judged as ◯, less than 100, 50 or more as △, and 100 or more as ×. <Heat seal strength> The heat seal strength of the two-kind three-layer film was measured by cutting the two-kind three-layer film obtained in the examples to 100 mm in the horizontal direction (TD direction) and 200 mm in the vertical direction (MD direction), overlapping the inner layers of the film, and heat sealing was performed with a heat seal tester TP-701B (manufactured by Tester Sangyo Co., Ltd.) at a set temperature of 130°C, double-sided heating, air pressure of 0.2 MPa, and heat seal time of 1 second using a seal bar with a width of 10 mm and a length of 300 mm. This test piece was cut to a width of 15 mm and subjected to a peel test using a tensile tester Tensilon RTE-1210 (manufactured by Orientec Co., Ltd.) under the conditions of a tensile speed of 300 mm / min and T-type peeling, to measure the heat seal strength (N / 15 mm). A heat seal strength of 10 or more was evaluated as ◯, less than 10, 5 or more, △, and less than 5, ×. <Film appearance> The two-type three-layer film was visually observed. If no poor appearance due to unstable fluidization was found, it was rated as ◯, if slight streaks or unevenness were found, it was rated as △, and if clear streaks or unevenness were found, it was rated as ×. <Production Example> [Production example of saponified ethylene-vinyl acetate copolymer (A1)] 70 parts by weight of ethylene-vinyl acetate copolymer (manufactured by Tosoh Corporation, trade name Ultrathene 626) (a1-1) with a melt mass flow rate of 3 g / 10 min and a vinyl acetate content of 15 wt%, 10 parts by weight of ethylene-vinyl acetate copolymer (manufactured by ARLANXEO, trade name LEVAPREN500) (a2-1) with a melt mass flow rate of 5 g / 10 min and a vinyl acetate content of 50 wt%, 20 parts by weight of a compatibilizer (a3) ​​shown below, and 100 ppm of an organic peroxide (manufactured by NOF Corporation, trade name Perhexa 25B) as a crosslinking agent (a4) were dry-blended at a melt resin temperature of 190°C using a twin-screw extruder to obtain a pellet-shaped sample. Next, this sample was hydrolyzed in a 5 wt% sodium hydroxide methanol solution at 65°C for 5 hours to obtain an ethylene-vinyl acetate copolymer saponification product (A1) with a saponification degree of 50 mol% and MFR of 3.0 g / 10 min. Detailed results are shown in Tables 1 and 2. (Constitution of the Compatibilizer (a3)) The following four types of ethylene-vinyl acetate copolymers were dry-blended in equal amounts (1 / 1 / 1 / 1) to prepare the compatibilizer (a3). Ethylene-vinyl acetate copolymer with a melt mass flow rate of 20 g / 10 min and a vinyl acetate content of 20% by weight (manufactured by Tosoh Corporation, product name Ultrathene 633) Ethylene-vinyl acetate copolymer with a melt mass flow rate of 18 g / 10 min and a vinyl acetate content of 28% by weight (manufactured by Tosoh Corporation, product name Ultrathene 710) Ethylene-vinyl acetate copolymer with a melt mass flow rate of 30 g / 10 min and a vinyl acetate content of 32% by weight (manufactured by Tosoh Corporation, product name Ultrathene 750) Ethylene-vinyl acetate copolymer with a melt mass flow rate of 70 g / 10 min and a vinyl acetate content of 42% by weight (manufactured by Tosoh Corporation, product name Ultrathene 760) [Production example of saponified ethylene-vinyl acetate copolymer (A2)] A saponified ethylene-vinyl acetate copolymer (A2) with a saponification degree of 50 mol% and MFR of 0.5 g / 10 min was obtained by dry blending 50 parts by weight of (a1-1), 30 parts by weight of (a2-1), and 150 ppm of crosslinking agent (a4) in the same manner as (A1), except that the hydrolysis treatment was carried out for 7 hours. The detailed results are shown in Tables 1 and 2. [Production example of saponified ethylene-vinyl acetate copolymer (A3)] A saponified ethylene-vinyl acetate copolymer (A3) with a saponification degree of 65 mol% and MFR of 1.5 g / 10 min was obtained in the same manner as (A1), except that 50 parts by weight of (a1-1) and an ethylene-vinyl acetate copolymer (manufactured by ARLANXEO, product name LEVAPREN800) (a2-2) with a melt mass flow rate of 5.0 g / 10 min and a vinyl acetate content of 80 wt% were dry blended. Detailed results are shown in Tables 1 and 2. [Production example of saponified ethylene-vinyl acetate copolymer (A4)] A saponified ethylene-vinyl acetate copolymer (A4) with a saponification degree of 46 mol% and MFR of 14 g / 10 min was obtained by the same method as (A1), except that 65 parts by weight of ethylene-vinyl acetate copolymer (a1-2) with a melt mass flow rate of 30 g / 10 min and a vinyl acetate content of 15 wt%, 12 parts by weight of (a2-1), and 23 parts by weight of (a3) ​​were used, and hydrolysis was carried out for 5 hours at a reaction temperature of 55°C using 1 part by weight of a methanol solution of sodium hydroxide. Detailed results are shown in Tables 1 and 2. [Production example of saponified ethylene-vinyl acetate copolymer (A5)] A saponified ethylene-vinyl acetate copolymer (A5) with a saponification degree of 5 mol% and MFR of 3.5 g / 10 min was obtained in the same manner as (A1), except that 70 parts by weight of (a1-1), 10 parts by weight of (a2-1), and 20 parts by weight of (a3) ​​were dry-blended and hydrolyzed with 1 part by weight of a methanol solution of sodium hydroxide at a reaction temperature of 40°C for 2 hours. Detailed results are shown in Tables 1 and 2. [Production example of saponified ethylene-vinyl acetate copolymer (A6)] A saponified ethylene-vinyl acetate copolymer (A6) with a saponification degree of 80 mol% and MFR of 2.0 g / 10 min was obtained in the same manner as (A1), except that 20 parts by weight of (a1-1), 60 parts by weight of (a2-2), and 20 parts by weight of (a3) ​​were dry-blended. Detailed results are shown in Tables 1 and 2.

[0050] [Table 1]

[0051] [Table 2]

[0052] Example 1 As the resin composition constituting the gas barrier resin layer, 70 parts by weight of saponified ethylene-vinyl acetate copolymer (A1) and 30 parts by weight of an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL C109B) (B1) having a melt mass flow rate of 8.5 and an ethylene content of 35 mol % were dry-blended and then melt-blended at a molten resin temperature of 200°C using a single-screw extruder.

[0053] The polyolefin that constitutes the polyolefin resin layer has a melt mass flow rate of 2.0 g / 10 min and a density of 905 kg / m 3 The copolymer had a melt mass flow rate of 0.3 g / 10 min and a density of 920 kg / m. 3 A dry blend of 30 parts by weight of a high-pressure low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 172) (MFR 1.1 g / 10 min) was used.

[0054] Using the above-mentioned three-layer cast molding machine, the resin composition constituting the gas barrier resin layer was fed to the extruder (25 mmφ) forming the intermediate layer, and the polyolefin resin constituting the polyolefin resin layer was fed to two extruders (32 mmφ and 25 mmφ) forming the inner and outer layers, and molded at 220°C to obtain a 55 μm thick laminate with an inner layer / intermediate layer / outer layer = 20 / 15 / 20 μm. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0055] Example 2 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 50 parts by weight and the amount of ethylene-vinyl alcohol copolymer (B1) was 50 parts by weight. The oxygen permeability, heat seal strength and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0056] Example 3 A laminate was produced in the same manner as in Example 2, except that an ethylene-vinyl alcohol copolymer (manufactured by Kuraray Co., Ltd., product name EVAL F171B) (B2) having a melt mass flow rate of 1.7 g / 10 min and an ethylene content of 32 mol% was used. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0057] Example 4 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A2) was 80 parts by weight and the amount of ethylene-vinyl alcohol copolymer (B1) was 20 parts by weight. The oxygen permeability, heat seal strength and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0058] Example 5 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A3) was 70 parts by weight and the amount of ethylene-vinyl alcohol copolymer (B1) was 30 parts by weight. The oxygen permeability, heat seal strength and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0059] Example 6 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A4) was 50 parts by weight and the amount of ethylene-vinyl alcohol copolymer (B2) was 50 parts by weight. The oxygen permeability, heat seal strength and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0060] Example 7 The polyolefin resin constituting the polyolefin resin layer has a melt mass flow rate of 4.0 g / 10 min and a density of 905 kg / m 3 The copolymer had a melt mass flow rate of 0.3 g / 10 min and a density of 920 kg / m. 3 A laminate was produced in the same manner as in Example 1, except that 20 parts by weight of a dry blend (MFR 2.1 g / 10 min) of high-pressure low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 172) was used. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0061] Example 8 The polyolefin resin constituting the polyolefin resin layer has a melt mass flow rate of 2.0 g / 10 min and a density of 905 kg / m 3 The copolymer had a melt mass flow rate of 0.3 g / 10 min and a density of 920 kg / m. 3 A laminate was produced in the same manner as in Example 1, except that 60 parts by weight of a dry blend (MFR 0.6 g / 10 min) of high-pressure low-density polyethylene (manufactured by Tosoh Corporation, product name Petrothene 172) was used. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0062] Example 9 The polyolefin resin constituting the polyolefin resin layer has a melt mass flow rate of 4.0 g / 10 min and a density of 905 kg / m 3 A laminate was produced in the same manner as in Example 1, except that an ethylene-1-hexene copolymer (manufactured by Tosoh Corporation, trade name Nipolon Z, HF310R) was used. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 3.

[0063] [Table 3]

[0064] Example 10 The mixture was composed of 55 parts by weight of saponified ethylene-vinyl acetate copolymer (A1), 45 parts by weight of ethylene-vinyl alcohol copolymer (B1), and component (C) having a melt mass flow rate of 4.0 g / 10 min and a density of 905 kg / m 3 A laminate was produced in the same manner as in Example 1, except that 30 parts by weight of an ethylene-1-hexene copolymer (manufactured by Tosoh Corporation, product name Nipolon Z, HF310R) (C1) was used. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 4.

[0065] Example 11 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 55 parts by weight, the amount of ethylene-vinyl alcohol copolymer (B1) was 45 parts by weight, and the amount of (C1) was 50 parts by weight. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 4.

[0066] [Table 4]

[0067] Comparative Example 1 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 90 parts by weight and the amount of ethylene-vinyl alcohol copolymer (B1) was 10 parts by weight. The oxygen permeability, heat seal strength and film appearance of the obtained laminate were evaluated, and the results are shown in Table 5. The laminate of this comparative example had poor oxygen permeability.

[0068] Comparative Example 2 A laminate was produced in the same manner as in Example 1, except that the amount of saponified ethylene-vinyl acetate copolymer (A1) was 40 parts by weight and the amount of ethylene-vinyl alcohol copolymer (B1) was 60 parts by weight. The oxygen permeability, heat seal strength and film appearance of the obtained laminate were evaluated, and the results are shown in Table 5. The laminate of this comparative example had poor heat seal strength.

[0069] Comparative Example 3 A laminate was produced in the same manner as in Example 1, except that saponified ethylene-vinyl acetate copolymer (A5) was used. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 5. The laminate of this comparative example had poor heat seal strength.

[0070] Comparative Example 4 A laminate was produced in the same manner as in Example 1, except that saponified ethylene-vinyl acetate copolymer (A6) was used. The oxygen permeability, heat seal strength, and film appearance of the obtained laminate were evaluated, and the results are shown in Table 5. The laminate of this comparative example had poor heat seal strength.

[0071] [Table 5] < / mfr>

Claims

1. A resin composition comprising an ethylene-vinyl alcohol copolymer (B) present as domains in a matrix of a saponified ethylene-vinyl acetate copolymer (A) having a vinyl acetate content of 0.3 to 20 mol % and a vinyl alcohol content of 1 to 20 mol %, wherein 50% or more of the form of (B) has a lamellar domain or a structure in which parts of the lamellar domains are three-dimensionally connected, and the aspect ratio of the domains is 5 or more.

2. 2. The resin composition according to claim 1, wherein a weight ratio (A / B) of the saponified ethylene-vinyl acetate copolymer (A) to the ethylene-vinyl alcohol copolymer (B) is 80 / 20 to 50 / 50.

3. The resin composition according to claim 1, wherein the saponified ethylene-vinyl acetate copolymer (A) is a hydrolyzate of a kneaded product containing the following components (a1) to (a3) ​​and crosslinked products of the (a1) to (a3), and has a melt mass flow rate of 0.3 to 5.0 g / min as measured in accordance with JIS K6922-1: (a1) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 20% by weight or less (a2) Ethylene-vinyl acetate copolymer having a vinyl acetate content of 45% by weight or more (a3) Compatibilizer

4. The ethylene-vinyl alcohol copolymer (B) has an ethylene content of 27 to 48 mol% and a melt mass flow rate measured at 190 ° C. according to JIS K6922-1 of 1.5 to 30 g / min. The resin composition according to claim 1.

5. The shear rate and apparent shear viscosity of the saponified ethylene-vinyl acetate copolymer (A) and the ethylene-vinyl alcohol copolymer (B) were measured using a capillary rheometer under the conditions of 200° C., orifice length L / orifice diameter D=20 / 1. -1 The resin composition according to claim 1, wherein the viscosity ratio (A / B) is 0.25 to 2.

0.

6. The resin composition according to claim 1, wherein the melt mass flow rate ratio (A / B) of the saponified ethylene-vinyl acetate copolymer (A) and the ethylene-vinyl alcohol copolymer (B) is 0.01 to 3.5 as measured in accordance with JIS K6922-1.

7. The resin composition according to claim 1, wherein the total of the saponified ethylene-vinyl acetate copolymer (A) and the ethylene-vinyl alcohol copolymer (B) is 100 parts by weight, and the polyethylene (C) is 1 to 60 parts by weight.

8. A laminate comprising a gas barrier resin layer made of the resin composition according to any one of claims 1 to 7 and at least one polyolefin resin layer adjacent to said gas barrier resin layer, wherein the polyolefin resin has a melt mass flow rate of 0.1 to 3.0 g / 10 min.

9. A laminate having a gas barrier resin layer made of the resin composition according to any one of claims 1 to 7, and polyolefin resin layers on both sides adjacent to said gas barrier resin layer, wherein the polyolefin resin has a melt mass flow rate of 0.1 to 3.0 g / 10 min.

10. The laminate according to claim 8 , wherein the polyolefin resin is an ethylene-based polymer or an ionomer resin.

11. The laminate according to claim 9, wherein the polyolefin resin is an ethylene-based polymer or an ionomer resin.

Citation Information

Patent Citations

  • Spout fitted with pull ring

    JP2000248128A

  • Fuel container

    JP2001200124A

  • Polyethylenic molding material

    JP2007161881A

  • Resin composition and laminate comprising the same

    JP2018145401A

  • Resin composition and laminate formed from the same

    JP2018154701A

Cited By

  • Ethylene-α-olefin copolymer, film, and laminated film

    WO2026191770A1