Powder compact

The application of a silicone resin and silane coupling agent with a glycidoxy group in the insulating coating layer addresses the issue of chipping and cracking in powder magnetic cores, enhancing the structural integrity of the powder compact.

JP2024134791AActive Publication Date: 2024-10-04TAMURA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023045154
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

In pressure molding of powder magnetic cores, weak binding forces between soft magnetic powders lead to chipping and cracking, making it difficult to form the desired shape.

Method used

A powder compact comprising soft magnetic powder coated with an insulating layer containing a silicone resin and a silane coupling agent with a glycidoxy group, such as 3-glycidoxypropylmethyldiethoxysilane, to enhance binding and prevent chipping and cracking.

Benefits of technology

The use of a silane coupling agent with a glycidoxy group in the insulating coating layer effectively reduces chipping and cracking, improving the integrity of the powder compact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134791000005
    Figure 2024134791000005
  • Figure 2024134791000001
    Figure 2024134791000001
  • Figure 2024134791000002
    Figure 2024134791000002
Patent Text Reader

Abstract

To provide a powder compact capable of preventing the occurrence of chips and cracks.SOLUTION: A powder compact includes soft magnetic powder and an insulation coating layer coating around the soft magnetic powder. The insulation coating layer includes a silicone resin and a silane coupling agent, the silicone resin being a methyl phenyl-based resin. The silane coupling agent has a glycidoxy group. Such silane coupling agent having a glycidoxy group can prevent the occurrence of chips and cracks in the powder compact.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a powder compact. [Background technology]

[0002] Coil components such as reactors are used in a variety of applications, including office equipment, solar power generation systems, automobiles, and uninterruptible power supplies. For example, a reactor is an electromagnetic component that converts electrical energy into magnetic energy and stores and releases it. A reactor mainly comprises a core and a coil. The coil is wound around the core. When power is supplied to the coil, it generates magnetic flux. The core is ring-shaped. The core becomes a magnetic path through which the magnetic flux generated by the coil flows.

[0003] Powder magnetic cores are sometimes used as reactor cores. Powder magnetic cores are produced by heat treating a powder compact. Powder compacts are produced, for example, by compacting soft magnetic powder with an insulating coating formed on the surface. In this compacting, a pressure of 10 to 20 ton / cm is generally used. 2 This is done under high pressure. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-125622 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the case of high pressure compaction, if the binding strength between the soft magnetic powder particles is weak, chips and cracks will occur in the compact. In some cases, the legs of the compact may come off, making it impossible to form the compact into the desired shape.

[0006] The present invention has been made to solve the above problems, and an object of the present invention is to provide a powder molded body that can prevent chipping and cracking. [Means for solving the problem]

[0007] The magnetic material comprises a soft magnetic powder and an insulating coating layer that covers the soft magnetic powder, the insulating coating layer containing a silicone resin and a silane coupling agent, the silicone resin being a methylphenyl-based resin, and the silane coupling agent having a glycidoxy group. Effect of the Invention

[0008] According to the present invention, it is possible to obtain a powder molded body that is capable of preventing chipping and cracking. [Brief description of the drawings]

[0009] [Figure 1] 1 is a graph showing the rattle values ​​of Examples 2, 7, and 11, and Comparative Example 2, in which 0.5 wt % of a silane coupling agent was added. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The configuration of the powder molded body of this embodiment will be described below. Note that the present invention is not limited to the embodiment described below.

[0011] Coil components such as reactors have a core containing a magnetic material. Powder magnetic cores are used as the core. Powder magnetic cores are produced by compressing soft magnetic powder into a powder compact and then subjecting the powder compact to a heat treatment called annealing.

[0012] The powder compact of the present embodiment includes a soft magnetic powder and an insulating coating layer. The insulating coating layer covers the surface of the soft magnetic powder. The insulating coating layer contains a silane coupling agent and a silicone resin.

[0013] The soft magnetic powder is mainly composed of iron. As the soft magnetic powder, pure iron powder, permalloy (Fe-Ni alloy) mainly composed of iron, Si-containing iron alloy (Fe-Si alloy), sendust alloy (Fe-Si-Al alloy), or a mixture of two or more of these powders can be used. In addition, amorphous alloy and nanocrystalline alloy powder can be used as the soft magnetic powder. The particle size (median size D50) of the soft magnetic powder is preferably 1 μm or more and 200 μm or less.

[0014] The Fe-Si-Al alloy powder contains, for example, about 7 wt% to 11 wt% of Si and about 4 wt% to 8 wt% of Al relative to Fe. The Fe-Si-Al alloy powder may contain, for example, about 1 wt% to 3 wt% of Ni relative to Fe. Furthermore, the Fe-Si-Al alloy powder may contain Co, Cr, or Mn.

[0015] The Si-containing iron alloy may contain Co, Al, Cr, or Mn. When using permalloy (Fe-Ni alloy), the ratio of Ni to Fe is preferably 50:50 or 25:75, but may be other ratios. For example, Fe-80Ni, Fe-36Ni, Fe-78Ni, or Fe-47Ni may be used. In addition to Fe and Ni, Si, Cr, Mo, Cu, Nb, Ta, etc. may be contained. Examples of Fe-Si alloy powder include Fe-3.5%Si alloy powder and Fe-6.5%Si alloy powder, but the ratio of Si to Fe may be other than 3.5% or 6.5%. Pure iron powder contains Fe at 99% or more.

[0016] The soft magnetic powder may be produced by a pulverization method or an atomization method, which may be any of water atomization, gas atomization, and water gas atomization.

[0017] However, since the pulverized powder produced by the pulverization method is non-circular, the soft magnetic powder particles tend to bond together, and chips and cracks are unlikely to occur in the green compact. On the other hand, the gas atomized powder produced by the atomization method, particularly the gas atomization method, is circular, and therefore has weak binding properties, making the green compact brittle. For this reason, the soft magnetic powder is preferably a gas atomized powder, which significantly exhibits the effect of the present invention of preventing chips and cracks from occurring in the green compact.

[0018] The circularity of the soft magnetic powder is preferably 0.8 or more in terms of the powder with an average particle size (median diameter D50). When the circularity is 0.8 or more, the binding between the soft magnetic powder particles is weak, and the powder compact is easily brittle. Therefore, when the circularity of the soft magnetic powder is 0.8 or more, the effect of the present invention is remarkable. In addition, the Vickers hardness of the soft magnetic powder is preferably 400HV or more. In the case of a hard soft magnetic powder with a Vickers hardness of 400HV or more, the binding between the soft magnetic powder particles is weak, and the powder compact is easily brittle, so the effect of the present invention is remarkable.

[0019] An insulating coating layer is formed on the surface of the soft magnetic powder. The insulating coating layer contains a silane coupling agent and a silicone resin. The insulating coating layer can be applied to the surface of each individual particle of the soft magnetic powder, or to a surface of a bonded particle formed by bonding several particles. It can also be applied to the entire surface or a part of the surface of a particle. In other words, the insulating coating layer does not need to completely cover the surface of the soft magnetic powder, and can be applied to a part of the surface of the soft magnetic powder.

[0020] The silane coupling agent has a glycidoxy group. For example, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, etc. can be used as the silane coupling agent. By having the glycidoxy group in the silane coupling agent, chipping or cracking can be prevented from occurring in the powder compact.

[0021] In particular, the silane coupling agent is preferably 3-glycidoxypropylmethyldiethoxysilane. By using 3-glycidoxypropylmethyldiethoxysilane, the powder compact is prevented from having chips or cracks, and the magnetic properties are improved.

[0022] The amount of the silane coupling agent added is preferably 0.3 wt % or more relative to the soft magnetic powder. When the amount of the silane coupling agent added is 0.3 wt % or more, the effect of preventing chipping and cracks from occurring in the powder compact is significantly observed.

[0023] The upper limit of the amount of the silane coupling agent added is preferably 1.5 wt % relative to the soft magnetic powder, because if the amount of the silane coupling agent added exceeds 1.5 wt %, the core loss deteriorates.

[0024] The silicone resin is made of a methylphenyl-based resin. Although not limited thereto, it is presumed that by combining a methylphenyl-based silicone resin with a silane coupling agent having a glycidoxy group, organic matter is more likely to remain in the insulating coating layer even after heating and drying, resulting in a good Rattra value. As the methylphenyl-based silicone resin, a methylphenyl-based silicone resin or silicone oligomer can be used. When a methylphenyl-based silicone resin is used, it is possible to form an insulating coating layer with little loss in weight due to heating and excellent heat resistance. Also, when a methylphenyl-based silicone oligomer is used, it is possible to form a thick and hard insulating coating layer.

[0025] The amount of silicone resin added is preferably 0.3 wt% or more and 2.0 wt% or less relative to the soft magnetic powder. If the amount added is less than 0.3 wt%, it will not function as an insulating coating layer, and eddy current loss will increase, resulting in reduced magnetic properties. If the amount added is more than 2.0 wt%, it will result in a reduced density of the powder compact.

[0026] After adding and mixing the silane coupling agent and silicone resin to the soft magnetic powder, the powder is heated and dried to form an insulating coating layer on the surface of the soft magnetic powder. The heating and drying conditions are not limited to the above, but are preferably at a temperature of 25°C or higher and 350°C or lower for about 2 hours.

[0027] The insulating coating layer may be a mixed layer of a silane coupling agent and a silicone resin, or a layer of a silane coupling agent and a layer of a silicone resin may be laminated. For example, when the insulating coating layer is laminated in the order of a layer of a silane coupling agent and a layer of a silicone resin, first, a silane coupling agent is added to and mixed with a soft magnetic powder, and then the soft magnetic powder on which the layer of the silane coupling agent has been formed is heated and dried. Then, a silicone resin is added to and mixed with the soft magnetic powder on which the layer of the silane coupling agent has been formed, and the soft magnetic powder is heated and dried to form a layer of the silicone resin on the surface of the layer of the silane coupling agent.

[0028] A lubricant may be added to the soft magnetic powder on which the insulating coating layer is formed. Examples of the lubricant include, but are not limited to, stearic acid, calcium stearate, lithium stearate, aluminum stearate, zinc stearate, ethylene bisstearamide, ethylene bisstearamide, and ethylene bisstearamide. By mixing the lubricant, the soft magnetic powder can slide easily, so that the density of the green compact can be increased. Furthermore, it is possible to reduce the upper punch pressure during compaction and prevent the occurrence of vertical streaks on the core wall surface due to contact between the die and the soft magnetic powder.

[0029] The amount of lubricant added is preferably about 0.2wt% to 0.8wt% of the soft magnetic powder. By setting the amount in this range, the sliding between the soft magnetic powder particles can be further improved. The lubricant may be added twice, before and after the insulating coating layer is formed. That is, the lubricant may be added to the soft magnetic powder before the silane coupling agent and silicone resin are added, and then the lubricant may be added to the soft magnetic powder on which the insulating coating layer has been formed.

[0030] After adding the lubricant, the soft magnetic powder is poured into a die and pressure-molded. This pressure molding produces a green compact. In the pressure molding, the soft magnetic powder is subjected to a pressure of 10 to 20 ton / cm 2 A pressure of about 12 to 15 ton / cm is applied to produce a green compact. 2 degree is more preferable.

[0031] Thereafter, the powder compact produced by the pressure molding is heat-treated in a non-oxidizing atmosphere such as nitrogen gas or a mixed gas of nitrogen and hydrogen, or in air at a temperature of 600°C or higher and lower than the temperature at which the insulating coating layer covering the soft magnetic powder is destroyed (for example, 900°C). By undergoing this heat treatment, a powder magnetic core is produced.

[0032] (Example) The present invention will be described in more detail with reference to the following examples. However, the present invention is not limited to the following examples. Powder compacts of Examples 1 to 13 and Comparative Examples 1 to 2 were produced. The powder compacts of Examples 1 to 13 and Comparative Examples 1 to 2 differ only in the type and amount of the silane coupling agent added.

[0033] First, a powder compact of Example 1 was produced. As the soft magnetic powder, Fe-Si-Al alloy powder produced by gas atomization was used. The particle size and circularity of the Fe-Si-Al alloy powder are shown in Table 1 below.

[0034] [Table 1]

[0035] First, a lubricant was added to the Fe-Si-Al alloy powder. Stearic acid (D50=100 μm, melting point 57° C.) was used as the lubricant. 0.3 wt % of stearic acid was added to the Fe-Si-Al alloy powder and mixed.

[0036] After adding and mixing stearic acid, the silane coupling agent was added and mixed. Then, the silicone resin was added and mixed. As the silane coupling agent, "B 3-glycidoxypropylmethyldiethoxysilane" (product name: KBE-402) shown in Table 2 below was used. 3-glycidoxypropylmethyldiethoxysilane was added at 0.3 wt% to the Fe-Si-Al alloy powder.

[0037] [Table 2]

[0038] A methylphenyl silicone resin was used as the silicone resin. 1.2 wt% of the silicone resin was added to the Fe-Si-Al alloy powder. After adding and mixing the silicone resin, the mixture was dried by heating. The drying temperature was 130°C, and the drying time was 2 hours. As a result, an insulating coating layer was formed around the Fe-Si-Al alloy powder.

[0039] After heating and drying, the Fe-Si-Al alloy powder was passed through a sieve with 850 μm openings to break up the agglomerates. Then, a lubricant was added again and mixed. The lubricant used in this case was aluminum stearate (D50=21 μm, melting point 110°C). Aluminum stearate was added at 0.2 wt% to the Fe-Si-Al alloy powder.

[0040] After adding and mixing the lubricant, the Fe-Si-Al alloy powder with the lubricant was filled into a die and pressed to produce a cylindrical green compact with an outer diameter of 11.3 mm and a height of 10.0 mm (height dimensional tolerance ±0.1 mm). The pressure for the press molding was 12.0 ton / cm. 2 Five powder compacts of Example 1 were produced.

[0041] Examples 2 to 5 differ from Example 1 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same materials, the same manufacturing method, and the same conditions as Example 1. The amount of silane coupling agent added is 0.5 wt% in Example 2, 0.7 wt% in Example 3, 1.0 wt% in Example 4, and 1.5 wt% in Example 5.

[0042] Example 6 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent used in Example 6 was "C3-glycidoxypropylmethyldimethoxysilane" (product name: KBM-402) shown in Table 2 above.

[0043] Examples 7 to 9 differ from Example 6 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same as those in Example 6, using the same materials, manufacturing method, and conditions. The amount of silane coupling agent added is 0.5 wt% in Example 7, 1.0 wt% in Example 8, and 1.5 wt% in Example 9.

[0044] Example 10 differs from Example 1 only in the type of silane coupling agent, and the rest, including the amount of silane coupling agent added, are the same materials, the same manufacturing method, and the same conditions as Example 1. The silane coupling agent used in Example 10 was "D 3-glycidoxypropyltrimethoxysilane" (product name: KBM-403) shown in Table 2 above.

[0045] Examples 11 to 13 differ from Example 10 only in the amount of silane coupling agent added, and the rest, including the type of silane coupling agent, are the same as those in Example 10, using the same materials, manufacturing method, and conditions. The amount of silane coupling agent added is 0.5 wt% in Example 11, 1.0 wt% in Example 12, and 1.5 wt% in Example 13.

[0046] Next, the preparation of the powder compacts of Comparative Examples 1 and 2 will be described. Comparative Example 1 differs from Example 1 only in that no silane coupling agent was added. That is, the insulating coating layer of Comparative Example 1 contains only silicone resin, and does not contain a silane coupling agent. In Comparative Example 1, the materials, manufacturing method, and conditions are otherwise the same as those of Example 1.

[0047] Comparative Example 2 differs from Example 1 only in the type and amount of silane coupling agent, and the rest of the materials, manufacturing method, and conditions are the same as those of Example 1. The silane coupling agent used in Comparative Example 2 was "A Tetraethoxysilane" (product name: TES28) shown in Table 2 above. The amount of silane coupling agent added was 0.5 wt%.

[0048] The rattle values ​​of the green compacts of Examples 1 to 13 and Comparative Examples 1 and 2 prepared as described above were measured. A rattle tester (manufactured by Intesco Co., Ltd.) was used to measure the rattle values. The rattle values ​​were measured based on the Japan Powder Metallurgy Association (JPMA) standard method for measuring the rattle values ​​of metal green compacts (JPMA P11 1992).

[0049] First, the total weight of five powder compacts of Examples 1 to 13 and Comparative Examples 1 to 2 was measured before being put into the Rattler tester. Then, the five powder compacts were put into a cylindrical cage covered with a 14 mesh stainless steel wire mesh and rotated 100 times at a rotation speed of 87 rpm. Finally, the total weight of the five powder compacts taken out of the Rattler tester was measured. Then, the total weight measured after rotation was subtracted from the total weight measured before rotation to obtain the weight reduction rate, thereby calculating the Rattler value. That is, the Rattler value was calculated from the following calculation formula (1). S = ((A-B) / A) × 100 (1) S: Rattler value (%) A: Total weight of the five green compacts before testing (g) B: Total weight of the five compacts after testing (g)

[0050] The calculation results are shown in Table 3 below. Also, a graph showing the rattle values ​​of Examples 2, 7, and 11, in which the silane coupling agent was added at 0.5 wt%, and Comparative Example 2, is shown in FIG.

[0051] [Table 3]

[0052] As shown in Table 3, in Examples 1 to 13 in which a silane coupling agent having a glycidoxy group was added, even the highest Rattler value was 29.2%, which was lower than 30%, and was lower than the values ​​in Comparative Examples 1 and 2. Therefore, it was confirmed that by using a silane coupling agent having a glycidoxy group, the Rattler value can be reduced and chipping and cracking can be prevented in the powder compact.

[0053] In addition, the rattle value is lower in Examples 1, 6 and 10, in which 0.3 wt% of a silane coupling agent having a glycidoxy group is added, compared to Comparative Example 1, in which no silane coupling agent is added. Therefore, it was confirmed that the effect of lowering the rattle value appears by adding 0.3 wt% or more of a silane coupling agent having a glycidoxy group.

[0054] In particular, when comparing Examples 2, 7, and 11, in which 0.5 wt% of a silane coupling agent having a glycidoxy group was added, with Comparative Example 2, in which a silane coupling agent without a glycidoxy group was added, the rattle values ​​of Examples 2, 7, and 11 are less than half that of Comparative Example 2, as shown in Table 3 and Figure 1. From this, it was confirmed that the rattle value is reduced by forming an insulating coating layer using a silane coupling agent having a glycidoxy group.

[0055] Furthermore, in Examples 4, 5, 8, and 9, in which 1.0 wt% or more of 3-glycidoxypropylmethyldiethoxysilane or 3-glycidoxypropylmethyldimethoxysilane was added as a silane coupling agent, the rattle value was lower than 15%, which is an extremely good value. Therefore, it was confirmed that by adding 1.0 wt% or more of 3-glycidoxypropylmethyldiethoxysilane or 3-glycidoxypropylmethyldimethoxysilane as a silane coupling agent, chipping and cracking in the powder compact can be more effectively prevented.

[0056] In addition, the rattler value is an index of the chipping tendency of a molded body, so it does not correlate with strength. In other words, it cannot be said that the rattler value decreases as the strength increases.

[0057] Next, the powder compacts of Example 14 and Comparative Example 3 were further produced. Example 14 differs from Example 2 only in that the powder of Example 14 was a pulverized powder produced by a pulverization method using Fe-Si-Al alloy powder. Other aspects, including the type and amount of the silane coupling agent, were the same as those of Example 2, using the same materials, manufacturing method, and conditions.

[0058] Comparative Example 3 differs from Comparative Example 2 only in that the powder used is a pulverized powder made by pulverizing Fe-Si-Al alloy powder. The rest of the comparison, including the type and amount of silane coupling agent added, is the same as that of Comparative Example 2, and the materials, manufacturing method, and conditions are the same as those of Comparative Example 2.

[0059] Five powder compacts were also prepared for each of Example 14 and Comparative Example 3, and the Rattler values ​​were calculated. The Rattler values ​​were calculated using the same equipment and under the same measurement conditions as above. The calculation results are shown in Table 4 below.

[0060] [Table 4]

[0061] As shown in Table 4, even when the Fe-Si-Al alloy powder is a pulverized powder, it was confirmed that Example 14, to which a silane coupling agent having a glycidoxy group was added, had a lower rattle value than Comparative Example 3. In other words, it was confirmed that the type of soft magnetic powder is not limited to gas atomized powder, and even pulverized powder can have the effect of reducing the rattle value.

[0062] However, looking at Comparative Example 3, the rattler value is 3.9%, which is a low value to begin with, and it is difficult to say that the rattler value of Example 14 is dramatically reduced. On the other hand, the rattler value of Comparative Example 2, which is a gas atomized powder, is a high value of 58.0%. And the rattler value of Example 2 is 29.0%, which is a dramatic reduction to half that of Comparative Example 2. Therefore, it was confirmed that the effect of reducing the rattler value is more pronounced when a silane coupling agent having a glycidoxy group is added to the soft magnetic powder, which is a gas atomized powder.

[0063] (Other embodiments) In this specification, an embodiment of the present invention has been described, but this embodiment is presented as an example and is not intended to limit the scope of the invention. The above-mentioned embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the scope of the invention. The embodiment and its modifications are included in the scope of the invention and its equivalents described in the claims, as well as in the scope and gist of the invention.

Claims

1. A soft magnetic powder; An insulating coating layer that covers the periphery of the soft magnetic powder; Equipped with the insulating coating layer contains a silicone resin and a silane coupling agent, The silicone resin is a methylphenyl-based resin, The silane coupling agent has a glycidoxy group; A powder compact characterized by the above.

2. The amount of the silane coupling agent added is 0.3 wt % or more with respect to the soft magnetic powder; The powder compact according to claim 1 ,

3. The soft magnetic powder is a gas atomized powder; The powder molded body according to claim 1 or 2,

4. The upper limit of the amount of the silane coupling agent added is 1.5 wt % or less with respect to the soft magnetic powder; The powder molded body according to claim 1 or 2,

Citation Information

Patent Citations

  • Powder for powder magnetic core, and powder magnetic core

    JP2022142137A

  • Coil Integrated Inductor

    US20090091412A1

  • Coated metal powder, dust core and method for producing same

    WO2011126120A1

  • Magnetic powder, magnetic-powder composition, molded object of magnetic-powder composition, and processes for producing same

    WO2015008842A1

  • Magnetic powder, compound, molded body, bonded magnet, and powder magnetic core

    WO2022220295A1