Pipe inner surface anticorrosive pipe

A multi-layered coating system with a vinyl ester resin primer and scaly glass flakes addresses the application challenges and protection issues of existing coatings, ensuring durable acid resistance for cast iron pipes in sewer systems.

JP2024134816APending Publication Date: 2024-10-04KURIMOTO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023045201
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing corrosion-resistant coatings for cast iron pipes, such as solvent-free epoxy resin paints and powder coatings, are difficult to apply and may not provide adequate protection against acidic environments, especially in sewer systems where acidic substances can penetrate and deteriorate the mortar lining.

Method used

A multi-layered coating system comprising a mortar lining layer, a vinyl ester resin primer layer, and a coating layer containing scaly glass flakes in a vinyl ester resin paint, which can be applied without heating the entire pipe, providing enhanced acid resistance and durability.

Benefits of technology

The multi-layered coating system effectively prevents penetration of acidic substances into the mortar lining, maintaining pipe integrity and durability even in harsh sewer environments, comparable to conventional powder coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134816000001_ABST
    Figure 2024134816000001_ABST
Patent Text Reader

Abstract

To provide a cast-iron pipe used for sewerage which has workability better than powder coating and for which durability and acid resistance with the similar level to a powder coating film are secured.SOLUTION: An inner surface anticorrosive pipe includes: a mortar lining layer 21; a primer layer 22 formed of a vinyl ester resin; and a coating film layer 23 formed of a vinyl ester resin coating material containing scale-like glass on an inner surface side of a cast-iron pipe 1 in the order from a pipe inner surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This invention relates to corrosion protection of cast iron pipes. [Background technology]

[0002] Ductile iron pipes are stronger than plastic pipes and are widely used for water supply and sewerage pipes, including main water pipes. However, because they are made of cast iron, they will corrode if left in their cast state. Therefore, both the exterior and interior surfaces, including the joints, must be thoroughly anti-corrosive treated before use.

[0003] Due to such demand, mortar linings and the like are applied to the inner surface of cast iron pipes. However, gravity flow systems are often used in sewers, and the pipes are often not filled with water, and liquid and gas phases exist. The liquid phase is an anaerobic environment, where hydrogen sulfide is produced by anaerobic bacteria and diffuses into the gas phase. The gas phase is an aerobic environment, where sulfuric acid is produced from hydrogen sulfide by aerobic bacteria, creating an acidic environment inside the sewer pipe. Here, there is a problem that mortar linings are not sufficiently acid-resistant, making them difficult to apply as is in a sewage environment. In response to this, Patent Document 1 proposes an inner-corrosion-resistant cast iron pipe in which a coating made of a solvent-free epoxy resin paint is formed on the surface of the cement mortar layer on the inner surface of the pipe. This prevents the mortar from coming into direct contact with the acidic environment inside the pipe, and prevents the mortar itself from dissolving in the acid and leaching out.

[0004] Moreover, Patent Document 2 proposes a method of protecting a steel pipe by applying a glass flake paint to the inner surface of the pipe. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-109215 A [Patent Document 2] Japanese Patent Application Publication No. 58-109215 Summary of the Invention [Problem to be solved by the invention]

[0006] However, because solvent-free epoxy resin paints have a high viscosity, the paint itself must be heated and pressurized when applied, making application complicated.

[0007] In addition, in the case of the inner surface corrosion-resistant cast iron pipe in which a coating film is formed on a mortar lining described in Patent Document 1, depending on the environment, acidic substances may penetrate the coating film made of solventless epoxy resin paint, causing the mortar lining to deteriorate. Furthermore, the epoxy resin powder coating generally used on the inner surface of cast iron pipes requires heating the entire pipe to harden the paint, which makes it difficult to apply, especially to large-diameter pipes.

[0008] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a sewer pipe having excellent acid resistance, which is easier to apply than powder coating and can ensure the same level of durability as a powder coating film. [Means for solving the problem]

[0009] The present invention solves the above-mentioned problems by providing an internally corrosion-resistant cast iron pipe which has, on the internal surface of the cast iron pipe, a mortar lining layer, a primer layer formed from vinyl ester resin, and a coating layer formed from vinyl ester resin paint containing glass flakes, in that order from the internal surface of the pipe.

[0010] That is, a coating layer in which glass flakes are contained in a vinyl ester resin paint becomes a protective layer in which glass flakes are laminated in multiple layers within the coating layer. This allows coating to be applied without the need to heat the entire pipe, as is the case with powder coating, and also allows for the production of an internally corrosion-resistant cast iron pipe that exhibits high acid resistance due to the glass flakes.

[0011] The internally corrosion-resistant cast iron pipe according to the present invention may employ an embodiment in which a top coat layer is further provided on the surface side of the coating layer. Effect of the Invention

[0012] In the internally corrosion-protected cast iron pipe of this invention, glass flakes are contained in a vinyl ester resin paint, which can be applied to form a coating layer without heating the entire pipe. This allows the formation of multiple protective layers of glass flakes within the coating layer, preventing acidic substances from penetrating into the mortar lining layer and causing deterioration of the mortar lining layer, even in harsh environments such as acidic sewage. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1A is a cross-sectional view showing an outline of an embodiment of an internally corrosion-resistant cast iron pipe according to the present invention; FIG. 1B is an enlarged cross-sectional view of a straight pipe portion showing a first embodiment of an internally corrosion-resistant cast iron pipe according to the present invention; and FIG. 1C is an enlarged cross-sectional view of a straight pipe portion showing a second embodiment of an internally corrosion-resistant cast iron pipe according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiment of the present invention will be described in detail. The present invention relates to an internally corrosion-protected cast iron pipe in which a corrosion-protective layer 20 is provided on the inner surface of a straight section 13 formed between a spigot 11 and a socket 12 in a straight cast iron pipe 1 as shown in Fig. 1(a). The corrosion-protective layer 20 in a first embodiment of the present invention has a mortar lining layer 21, a primer layer 22, and a coating layer 23, in that order from the inner surface of the cast iron pipe 1, as shown in the enlarged cross-sectional view of Fig. 1(b). The corrosion-protective layer 20 in a second embodiment of the present invention further has a topcoat layer 24 on the coating layer 23, as shown in the enlarged cross-sectional view of Fig. 1(c). The following description will be given mainly of the first embodiment as an example.

[0015] A centrifugal cast cast iron pipe can be suitably used as the cast iron pipe 1 used in the present invention. The type of cast iron pipe is not particularly limited, and a general ductile iron pipe or the like can be used.

[0016] The mortar lining layer 21 is formed by supplying cement mortar to the inner surface of the cast iron pipe 1 while applying centrifugal force and hardening the layer. The cement mortar is a common mixture of aggregate such as sand and cement. The mortar lining layer 21 formed by hardening the cement mortar contains a laitance layer on the surface of the mortar lining layer 21, which is a collection of impurities contained in the cement mortar. Therefore, it is preferable to remove this laitance layer before applying the primer layer 22. In addition, the thickness of the mortar lining layer 21 after removing the laitance layer is preferably 4 to 15 mm. If the thickness is less than 4 mm, the surface of the mortar lining layer 21 will not be smooth due to the unevenness formed on the inner surface of the straight portion 13 after casting, and if the thickness is more than 15 mm, the water flow cross-sectional area on the inner surface of the pipe will be reduced more than necessary.

[0017] The primer layer 22 is a resin layer formed by applying a vinyl ester resin primer to the surface of the mortar lining layer 21. By using a vinyl ester resin as a primer, adhesion can be achieved without using the primer in a high-heat environment as in the case of powder coating. The thickness of the primer layer 22 is preferably 50 μm or more and 100 μm or less. If the thickness is less than 50 μm, the adhesion stabilization effect with the coating layer 23 becomes insufficient, and if the thickness is more than 100 μm, the adhesion stabilization effect does not increase. Although not shown, the primer layer 22 can be applied directly to the inner surface of the cast iron pipe 1 without forming the mortar lining layer 21. However, in this case, since smoothness cannot be ensured by the mortar lining layer 21, processing such as grinding or blasting is required.

[0018] The coating layer 23 is formed by applying a vinyl ester resin paint containing glass flakes onto the primer layer 22. Since the glass flakes are hardened in layers inside, the protective effect of the glass layers is added, and the coating layer 23 exhibits high acid resistance compared to a layer of vinyl ester resin alone. Therefore, the inner surface corrosion-resistant cast iron pipe according to the present invention can prevent the penetration of acidic substances into the mortar lining layer even in an acidic sewage environment, and exhibits high durability by suppressing deterioration of the mortar lining. The thickness of the coating layer 23 is preferably 300 μm or more and 900 μm or less. If the coating layer 23 is less than 300 μm, the amount of glass flakes contained is insufficient, and the protective effect on the mortar lining layer 21 is likely to be insufficient, and if the coating layer is thicker than 900 μm, the water-passing cross-sectional area on the inner surface of the pipe is reduced.

[0019] The topcoat layer 24 in the second embodiment of the present invention is a resin layer formed by further coating a vinyl ester resin on the coating layer 23. The vinyl ester resin used for the topcoat layer 24 does not contain glass flakes. The presence of the topcoat layer 24 provides protection for the coating layer 23 and improves durability. When the topcoat layer 24 is formed, the thickness of the topcoat layer 24 is preferably 100 μm or more and 300 μm or less. If the thickness is less than 100 μm, the effect of concealing the unevenness of the coating layer 23 surface containing glass flakes is not fully exhibited, and even if the thickness is more than 300 μm, the layer of vinyl ester resin paint not containing glass flakes is easily permeated by acid, and the protective effect on the mortar lining layer 21 is not particularly improved, so it is wasted.

[0020] The primer layer 22, the coating layer 23, and the topcoat layer 24 can be formed by, for example, roller coating, brush coating, or spray coating.

[0021] Since the inner surface of the socket 12 and the outer surface of the insertion hole 11, which are not provided with the mortar lining layer 21, are exposed to an acidic environment, these areas can be protected by providing these areas with the primer layer 22 and the coating layer 23. In addition, the surface of the coating layer 23 superimposed on the area without the mortar lining layer 21 can also be provided with a topcoat layer 24. EXAMPLES

[0022] The present invention will be specifically described below with reference to examples in which an internally corrosion-resistant cast iron pipe according to the present invention was actually manufactured.

[0023] (Examples 1 to 3) As a cast iron pipe, a ductile iron pipe with a nominal diameter of 150 manufactured by Kurimoto Iron Works, Ltd. was rotated while applying a mortar lining to the inner surface to form a mortar lining layer 21. After hardening, the portion of the surface that would become the laitance layer was polished off.

[0024] On the inner surface of the mortar lining layer 21 from which the laitance layer had been removed, a vinyl ester resin primer, Tough Barrier #200 Primer RC (manufactured by Nippon Tokushu Toryo Co., Ltd.), was applied with a roller to a film thickness of 80 μm to form a primer layer.

[0025] After the vinyl ester resin primer that would become the primer layer was cured, Tough Barrier #200 flakes (manufactured by Nippon Tokushu Toryo Co., Ltd.) containing scaly glass were applied with a roller to a thickness of 300 μm to form a coating layer (Example 1). In Example 2, similar roller application was performed twice to form a coating layer with a thickness of 600 μm, and in Example 3, similar roller application was performed three times to form a coating layer with a thickness of 900 μm.

[0026] In Examples 1 to 3, after the coating layer had hardened, a vinyl ester resin coating material not containing scaly glass, Tough Barrier #200 topcoat (manufactured by Nippon Tokushu Toryo Co., Ltd.), was applied with a roller to a thickness of 150 μm to form a topcoat layer, thereby obtaining an internally corrosion-resistant cast iron pipe protected by four layers: a mortar lining layer, a primer layer, a coating layer, and a topcoat layer.

[0027] (Comparative Example 1: Conventional Powder Coating) The same cast iron pipe as used in Example 1 was used, and the inner surface of the cast iron pipe was subjected to a primer treatment to produce a clean surface. This polished cast iron pipe was heated to 270°C, and then coated with an epoxy resin powder coating, V-PET#1600 Kurimoto Gray FH (manufactured by Dai Nippon Toryo Co., Ltd.), to a film thickness of 300 μm, and then allowed to cool and harden, yielding an inner-corrosion-resistant cast iron pipe protected by a powder coating layer of the epoxy resin powder coating.

[0028] The coated internally corrosion-resistant cast iron pipes of Examples 1 to 3 and Comparative Example 1 were cut into pieces measuring 150 mm x 90 mm, and the cut surfaces were coated for protection. The following tests were carried out on these test pieces. Each test method was in accordance with the method described in the "Manual for Corrosion Inhibition and Anticorrosion Technology for Sewerage Concrete Structures" (compiled by the Japan Sewage Works Agency, a local joint corporation; hereinafter abbreviated as "Manual").

[0029] <Sulfuric acid immersion test> The test pieces thus prepared were immersed in a 10% by weight aqueous solution of sulfuric acid for 60 days, after which the appearance of the coating was observed. Evaluation was carried out as follows. In the manual, the corrosion protection coating method is a coating-type lining method, the corrosive environment is Class I (an environment in which the annual average hydrogen sulfide gas concentration is 50 ppm or more, and concrete corrosion is extremely common), and the required performance corresponds to Class D. ◯: After 60 days, no cracking, softening, or dissolution was observed in the coating film. ×: After 60 days, the coating film exhibits any of the following abnormalities: cracking, softening, or elution.

[0030] <Sulfur penetration test> The prepared test pieces were immersed in a 10% by weight aqueous solution of sulfuric acid for 120 days, after which elemental analysis of sulfur was performed on the cross section of the coating using an EPMA (EPMA1720, manufactured by Shimadzu Corporation) to investigate the depth of penetration of sulfur from the coating surface. The evaluation was carried out as follows. Similarly, in the manual, the corrosion protection coating method is a paint-type lining method, the corrosive environment is Class I (annual average hydrogen sulfide gas concentration of 50 ppm or more, an environment in which extreme concrete corrosion is observed), and the required performance corresponds to Class D. Good: After 120 days, the depth of sulfur penetration from the surface was 5% or less of the film thickness and 100 μm or less. ×: After 120 days, the sulfur penetration depth from the surface is more than 5% of the film thickness or more than 100 μm.

[0031] <Organic acid immersion resistance test> The prepared test pieces were immersed in a 5% by mass aqueous solution of acetic acid for 60 days, and then the appearance of the coating film was observed. Evaluation was performed as follows. ◯: After 60 days, no cracking, softening, or dissolution was observed in the coating film. ×: After 60 days, the coating film exhibits any of the following abnormalities: cracking, softening, or elution.

[0032] The test results are shown in Table 1. All of the examples showed good test results comparable to those of the comparative examples using conventional powder coating that requires high temperatures.

[0033] [Table 1] [Explanation of symbols]

[0034] 1,1a Cast iron pipe 11 Insertion port 12 socket 13 Straight section 20 Anticorrosive Layer 21 Mortar lining layer 22 Primer layer 23 Coating layer 24 Topcoat

Claims

1. The cast iron pipe has an inner surface that is corrosion-resistant and is provided with, on the inner surface thereof, a mortar lining layer, a primer layer formed from a vinyl ester resin, and a coating layer formed from a vinyl ester resin paint containing glass flakes, in that order from the inner surface of the pipe.

2. 2. The cast iron pipe according to claim 1, further comprising a topcoat layer on the surface side of the coating layer.

3. supplying cement mortar onto the inner surface of the cast iron pipe while rotating the pipe to form a mortar lining layer on the inner surface of the pipe; a step of polishing and removing a laitance layer present on a surface side of the mortar lining layer after the mortar lining layer has hardened; A step of applying a vinyl ester resin primer to a surface layer of the mortar lining layer to form a primer layer; a step of applying a vinyl ester resin paint containing glass flakes to a surface of the primer layer to form a coating layer; This is a manufacturing method for cast iron pipes with internal corrosion protection.

4. 4. The method for producing an internally corrosion-resistant cast iron pipe according to claim 3, further comprising the step of applying a vinyl ester resin paint not containing the glass flakes on the coating layer to form a topcoat layer.

Citation Information

Patent Citations

  • Corrosion-resistant composite pipe

    JP1990038386A

  • Inner surface corrosion-protected cast iron pipe and manufacturing method thereof

    JP2019162737A

  • Finishing method and tool for workpiece