Slurry composition for secondary battery positive electrode, secondary battery positive electrode, and secondary battery

By adding dispersants such as aryl carboxylic acid ester, silicone oil, and N-vinylpyrrolidone-carboxylic acid vinyl ester polymer to the positive electrode slurry of lithium secondary battery, the problem of poor stability of the positive electrode slurry is solved and efficient dispersion is achieved Improved performance and high temperature characteristics, improving battery performance.

CN119069696AActive Publication Date: 2024-12-03JIANGSU BAIKILOMETER NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202310593882.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-03
Estimated Expiration
2043-05-24

AI Technical Summary

Technical Problem

The stability of the positive electrode slurry of the existing lithium secondary batteries is poor, resulting in poor phenomena such as gel, leakage, slope climbing, and burrs, which affects battery performance.

Method used

A slurry composition containing a positive electrode active material, a conductive material and a bonding material is used, and a dispersant, such as aryl carboxylic acid esters, silicone oils and N-vinylpyrrolidone-carboxylic acid vinyl ester polymers are added, stabilized by hydrogen bonding Structure, improve dispersion and high temperature characteristics.

Benefits of technology

It significantly improves the dispersion and high-temperature characteristics of the positive electrode of the secondary battery, reduces the internal resistance, and enhances the stability and performance consistency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a slurry composition for a secondary battery positive electrode, a secondary battery positive electrode, and a secondary battery. The slurry composition for the positive electrode of the secondary battery comprises a positive electrode active material, a conductive material, a binding material and a dispersing agent, the dispersing agent comprises at least two of a component A, a component B and a component C, the component A comprises at least one of aryl carboxylic ester, fatty acid ester and phosphate, the component B comprises silicone oil, and the component C comprises silicone oil. And the component C comprises an N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer. The slurry composition for a positive electrode according to the present application has excellent dispersibility and can produce a positive electrode for a secondary battery and a secondary battery which can exhibit good high-temperature characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of new energy technology, and specifically relates to a slurry composition for a secondary battery positive electrode and its application, a composite material layer for a secondary battery positive electrode, a secondary battery positive electrode and a secondary battery. Background Art

[0002] With the rapid development of secondary batteries, especially lithium secondary batteries, they are widely used in many fields. In the manufacturing process of lithium batteries, the stability of the slurry is one of the important indicators of the slurry properties. The stability of the slurry directly affects the storage time of the slurry. The more stable the slurry is, the more continuity it can provide for production. At the same time, the stability of the slurry will also have a significant impact on the coating effect. The more stable the slurry is, the more stable the coating process is, the more stable the coating surface density is, and the prepared battery performance is stable and consistent.

[0003] However, the positive electrode slurry of lithium secondary batteries currently generally uses polyvinylidene fluoride as a binder, and the interaction between the polyvinylidene fluoride molecular chain and the positive electrode particles is unstable, resulting in a decrease in slurry stability, and the occurrence of adverse phenomena such as gelation, coating leakage, climbing, burrs, etc., which affects battery performance. Summary of the invention

[0004] Problem that the invention aims to solve

[0005] Here, in order to further improve the battery characteristics of the secondary battery, it is usually required to make the electrode active material well dispersed in the slurry composition to form a uniform electrode composite material layer. Therefore, the purpose of the present application is to provide a positive electrode slurry composition for a secondary battery with excellent dispersibility and capable of manufacturing a good high temperature characteristic. In addition, the purpose of the present application is to provide a positive electrode for a secondary battery capable of manufacturing a good high temperature characteristic and a secondary battery capable of performing a good high temperature characteristic.

[0006] In order to solve all or part of the above-mentioned technical problems, one of the objects of the present application is to provide a slurry composition for a secondary battery positive electrode, comprising a positive electrode active material, a conductive material and a binding material, the slurry composition for a secondary battery also comprising a dispersant, the dispersant comprising at least two components of component A, component B or component C, the component A comprising at least one of aromatic carboxylic acid esters, fatty acid esters and phosphate esters, the component B comprising silicone oil, and the component C comprising N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer.

[0007] The second object of the present application is to provide an application of the above-mentioned slurry composition for secondary battery positive electrode in the preparation of a composite material layer for secondary battery positive electrode, a positive electrode for secondary battery or a secondary battery.

[0008] The third object of the present application is to provide a composite material layer for a secondary battery positive electrode, wherein the composite material layer is formed by the slurry composition for a secondary battery positive electrode according to any one of the above technical solutions.

[0009] The third object of the present application is to provide a positive electrode for a secondary battery, wherein the positive electrode for a secondary battery is formed by the slurry composition for a positive electrode of a secondary battery described in any one of the above technical solutions.

[0010] A fourth object of the present application is to provide a secondary battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the positive electrode comprises the positive electrode for a secondary battery described in the above technical solution.

[0011] Solutions for solving problems

[0012] The purpose of the present application is to advantageously solve all or part of the above problems. The secondary battery positive electrode slurry composition of the present application is characterized in that it contains a positive electrode active material, a conductive material, a binding material and a dispersant, the dispersant includes at least two components of component A, component B or component C, the component A includes at least one of aryl carboxylic acid ester, fatty acid ester and phosphate ester, the component B includes silicone oil, and the component C includes N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer. The positive electrode slurry composition having the above-mentioned specified composition has excellent dispersibility, and the secondary battery having a positive electrode formed using the positive electrode slurry composition can exhibit good high temperature characteristics.

[0013] Here, the secondary battery positive electrode slurry composition of the present application preferably comprises at least two of the above-mentioned dispersant component A, component B or component C. The above-mentioned component A includes at least one of aryl carboxylate, fatty acid ester and phosphate, the above-mentioned component B includes silicone oil, and component C includes N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer. This is because a single component is unstable during charging and discharging at high temperatures and is prone to decomposition. When any at least two are used in combination, they stabilize the structure through hydrogen bonding, and the thickness expansion of the secondary battery having the positive electrode formed using the positive electrode slurry composition can be reduced, so that the high temperature characteristics of the secondary battery can be further improved.

[0014] Here, the conductive material in the secondary battery positive electrode slurry composition of the present application preferably includes a fibrous conductive carbon material. This is because if the positive electrode slurry composition includes a fibrous conductive carbon material as a conductive material, the internal resistance of the secondary battery having a positive electrode formed using the positive electrode slurry composition can be well reduced, so the high temperature characteristics of the secondary battery can be further improved.

[0015] In addition, generally, fibrous conductive carbon materials tend to aggregate easily and have poor dispersibility. However, since the slurry composition for positive electrodes of the present application has the above-specified composition, good dispersibility can be achieved.

[0016] In addition, the slurry composition for the secondary battery positive electrode of the present application preferably contains the fibrous conductive carbon material in an amount of 5% by mass or more and 100% by mass or less of the conductive material. This is because if the slurry composition for the positive electrode contains the fibrous conductive carbon material in the above-specified ratio, good dispersibility can be obtained, and the high temperature characteristics of the secondary battery having the positive electrode formed using the slurry composition for the positive electrode are further improved.

[0017] In addition, the secondary battery positive electrode slurry composition of the present application preferably contains the component A in a proportion of 10% by mass or more and 50% by mass or less of the dispersant. This is because if the positive electrode slurry composition contains the component A in an amount within the above range, the dispersibility of the positive electrode slurry composition can be further improved, and the high temperature characteristics of the secondary battery having a positive electrode formed using the positive electrode slurry composition can be further improved.

[0018] In addition, the secondary battery positive electrode slurry composition of the present application preferably contains the component B in a proportion of 10% by mass or more and 80% by mass or less of the dispersant. This is because if the positive electrode slurry composition contains the component B in an amount within the above range, not only can the positive electrode slurry composition have better dispersibility, but also a secondary battery with better high temperature characteristics can be obtained.

[0019] In addition, the secondary battery positive electrode slurry composition of the present application preferably contains the component C in a proportion of 1% by mass or more and 50% by mass or less of the dispersant. This is because if the positive electrode slurry composition contains the component C in an amount within the above range, not only can the positive electrode slurry composition have better dispersibility, but also a secondary battery with better high temperature characteristics can be obtained.

[0020] Furthermore, the secondary battery positive electrode slurry composition of the present application preferably has a shear rate of 10 s -1 The viscosity η 0 Viscosity η at shear rate 1000s-1 1 The ratio (η 0 / η 1 ) is 2 times or more and 20 times or less. This is because if the η of the positive electrode slurry composition is 0 / η 1 When the positive electrode slurry composition is applied on a current collector to form a positive electrode composite material layer within the above range, the coating property of the positive electrode slurry composition becomes good, so that the positive electrode and the secondary battery can be manufactured well.

[0021] In addition, the purpose of the present application is to advantageously solve the above-mentioned problem. The feature of the secondary battery positive electrode of the present application is that it is formed using any of the above-mentioned secondary battery positive electrode slurry compositions. The positive electrode obtained using any of the above-mentioned secondary battery positive electrode slurry compositions can give the secondary battery excellent high temperature characteristics.

[0022] Moreover, the purpose of the present application is to advantageously solve the above-mentioned problem, and the secondary battery of the present application is characterized in that it has a positive electrode, a negative electrode, a separator and an electrolyte, and the above-mentioned positive electrode is the above-mentioned positive electrode for the secondary battery. As such, the secondary battery having the above-mentioned positive electrode for the secondary battery as the positive electrode has excellent high temperature characteristics.

[0023] Effects of the Invention

[0024] The present application provides a positive electrode slurry composition that has excellent dispersibility and can produce a secondary battery that can exhibit good high-temperature characteristics.

[0025] Furthermore, according to the present application, it is possible to provide a positive electrode capable of manufacturing a secondary battery that can exhibit good high-temperature characteristics, and a secondary battery that can exhibit good high-temperature characteristics. DETAILED DESCRIPTION

[0026] Hereinafter, embodiments of the present application are described in detail. However, these embodiments are exemplary and the present application is not limited thereto.

[0027] Here, the secondary battery positive electrode slurry composition of the present application can be used to obtain the positive electrode of a secondary battery such as a lithium ion secondary battery (for example, the secondary battery positive electrode of the present application). Specifically, the secondary battery positive electrode slurry composition of the present application can be used, for example, to form a positive electrode composite material layer of a secondary battery positive electrode. In addition, the secondary battery of the present application is characterized in that it has a secondary battery positive electrode formed using the secondary battery positive electrode slurry composition of the present application.

[0028] Slurry composition for secondary battery positive electrode

[0029] The slurry composition for the positive electrode of the secondary battery of the present application comprises a positive electrode active material, a conductive material, a binding material and a dispersant, wherein the dispersant comprises at least two components of component A, component B or component C, wherein the component A comprises at least one of aryl carboxylic acid ester, fatty acid ester and phosphate ester, wherein the component B comprises silicone oil, and the component C comprises N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer. The slurry composition for the positive electrode of the secondary battery of the present application adopts the above-mentioned prescribed composition, so that the secondary battery having the positive electrode formed by using the slurry composition for the positive electrode can exert excellent high temperature characteristics.

[0030] Positive active material

[0031] As the positive electrode active material for lithium ion secondary batteries, a material capable of absorbing and releasing lithium is generally used. Specifically, it may include one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and a combination thereof. As a specific example, a compound represented by one or more of the following chemical formulas may be used: Li a A 1-b X b D 2 (0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a E 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a E 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05); Li a Ni 1-b-c Co b X c D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<d≤2); Li a Ni 1-b- c Co b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Co b X c O 2-α T 2 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α<2); Li a Ni 1-b-c Mn b X c D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, 0<α≤2); Li a Ni 1-b-c Mnb X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05\0<α<2);Li a Nor 1-b-c Mn b X c O 2-α T 2 (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.05\0<α<2);Li a Nor b E c G d O 2 (0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1);Li a Nor b Co c Mn d GeO 2 (0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0.001≤e≤0.1);Li a NiG b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a CoG b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-b G b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 2 G b O 4 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mn 1-g G g MONTH 4 (0.90≤a≤1.8,0≤g≤0.5);QO 2 ;QS 2 ;LiQS 2 ;V 2 O 5 ;LiV 2 O 5 ;LiZO 2 ;LiLevel 4 ;The (3-f) J2 (PO 4 ) 3 (0≤f≤2);Li (3-f) Fe 2 (PO 4 ) 3 (0≤f≤2);Li a FePO 4 (0.90≤a≤1.8).

[0032] In the above chemical formula, A is selected from Ni, Co, Mn and combinations thereof; X is selected from Al, Ni, Co, Mn, Cr, Fe, Nb, Mg, Sr, V, rare earth elements and combinations thereof; D is selected from O, F, S, P and combinations thereof; E is selected from Co, Mn and combinations thereof; T is selected from F, S, P and combinations thereof; G is selected from Al, Cr, Mn, Fe, Nb, Mg, La, Ce, Sr, V and combinations thereof; Q is selected from Ti, Mo, Mn and combinations thereof; Z is selected from Cr, V, Fe, Sc, Y and combinations thereof; J is selected from V, Cr, Mn, Co, Ni, Cu and combinations thereof.

[0033] The compound may have a coating layer on the surface, or may be mixed with another compound having a coating layer. The coating layer may include at least one coating element compound selected from an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, and a hydroxycarbonate of a coating element. The compound for the coating layer may be amorphous or crystalline. The coating element included in the coating layer may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Nb, Zr, or a mixture thereof. The coating layer may be provided by using these elements in the compound and by a method that has no negative impact on the properties of the positive active material, for example, the method may include any coating method (e.g., spraying, dipping, etc.), but since it is well known to those skilled in the relevant art, it is not described in more detail.

[0034] The amount and particle size of the positive electrode active material are not particularly limited and may be the same as those of the positive electrode active material conventionally used.

[0035] Conductive Materials

[0036] The conductive material is not particularly limited as long as it is a conductive material. As the conductive material, particulate conductive carbon materials such as carbon black, graphite, and carbon flakes can be used; fibrous conductive carbon materials such as carbon fiber, carbon nanotubes, and vapor-grown carbon fiber, and fibers and foils of various metals can be used. Among them, from the viewpoint of reducing the internal resistance of the secondary battery well, as the conductive material, it is preferred to use at least a fibrous conductive carbon material, more preferably carbon black and a fibrous conductive carbon material are used in combination, further preferably acetylene carbon black and a fibrous conductive carbon material are used in combination, and particularly preferably acetylene carbon black and carbon nanotubes are used in combination.

[0037] These can be used individually by 1 type or in combination of 2 or more types.

[0038] In addition, the overall content of the conductive material in the secondary battery positive electrode slurry composition is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, further preferably 1 part by mass or more, particularly preferably more than 3 parts by mass, preferably 10 parts by mass or less, and more preferably 8 parts by mass or less, relative to 100 parts by mass of positive electrode active material. This is because if the overall content of the conductive material is above the above lower limit, in a secondary battery having a positive electrode formed using a positive electrode slurry composition, the internal resistance can be further reduced and the high temperature characteristics can be further improved. In addition, if the overall content of the conductive material is below the above upper limit, the dispersibility of the positive electrode slurry composition can be prevented from decreasing.

[0039] Fibrous conductive carbon materials

[0040] As the fibrous conductive carbon material, a fibrous conductive carbon material containing carbon nanotubes is preferred because the use of a fibrous conductive carbon material containing carbon nanotubes can further reduce the internal resistance of the secondary battery due to the high conductivity of the carbon nanotubes, thereby further improving the high temperature characteristics.

[0041] In addition, in the present application, the "fibrous conductive carbon material" is defined as having an aspect ratio (major diameter / minor diameter) of 5 or more. In addition, the aspect ratio of the fibrous conductive carbon material is preferably greater than 10. Moreover, the "aspect ratio" can be obtained by the following method: observation is performed using a SEM (scanning electron microscope), and for any fibrous conductive carbon material, the maximum diameter (major diameter) and the fiber diameter (minor diameter) in a direction orthogonal to the maximum diameter are measured, and the ratio of the major diameter to the minor diameter (major diameter / minor diameter) is calculated.

[0042] In addition, when using a fibrous conductive carbon material containing carbon nanotubes, the carbon nanotubes in the fibrous conductive carbon material are not particularly limited, and single-layer carbon nanotubes and / or multi-layer carbon nanotubes can be used. Furthermore, from the perspective of reducing the manufacturing cost of the positive electrode slurry composition, at least multi-layer carbon nanotubes can be used. In addition, the fibrous conductive carbon material can be purchased from a commercial product.

[0043] Here, the average fiber diameter of the fibrous conductive carbon material is preferably 0.5 nm or more, more preferably 1 nm or more, usually less than 1 μm, preferably less than 200 nm, more preferably less than 100 nm, and more preferably less than 30 nm. This is because, if the average fiber diameter of the fibrous conductive carbon material is above the above lower limit, the excellent conductivity of the fibrous conductive carbon material can be fully utilized to suppress the increase in the internal resistance of the secondary battery, so that the secondary battery can exert better high temperature characteristics. In addition, if the average fiber diameter of the fibrous conductive carbon material is below the above upper limit, the fibrous conductive carbon material is better stored in the positive electrode slurry composition, for example, the coating property when the positive electrode slurry composition is coated on the current collector to form a positive electrode composite material layer is better, and the high temperature characteristics of the secondary battery can be further improved.

[0044] In addition, in the present application, the "average fiber diameter" can be determined by measuring the diameter of more than 100 randomly selected fibrous conductive carbon materials using SEM (scanning electron microscope) or TEM (transmission electron microscope), and is obtained as a number average diameter. In particular, when the diameter of the fibrous conductive carbon material is small, it is preferably observed using a TEM (transmission electron microscope). In addition, the average fiber diameter of the fibrous carbon nanostructure can be adjusted by changing the manufacturing method and manufacturing conditions of the fibrous conductive carbon material, and can also be adjusted by combining a plurality of fibrous conductive carbon materials obtained by different methods.

[0045] Average fiber length

[0046] In addition, the average fiber length of the fibrous conductive carbon material is preferably 1 μm or more, more preferably 2 μm or more, further preferably 3 μm or more, preferably 200 μm or less, more preferably 100 μm or less, and further preferably 30 μm or less. This is because, if the average fiber length of the fibrous conductive carbon material is above the above lower limit, the excellent conductivity of the fibrous conductive carbon material can be fully utilized to suppress the rise of the internal resistance of the secondary battery, so that the secondary battery can have better high temperature characteristics. In addition, if the average fiber length of the fibrous conductive carbon material is below the above upper limit, the fibrous conductive carbon material can be better stored in the positive electrode slurry composition. In addition, if the average fiber length of the fibrous conductive carbon material is below the above upper limit, for example, the coating property of the positive electrode slurry composition when it is coated on the current collector to form a positive electrode composite material layer is better, and the softness of the formed positive electrode composite material layer is improved, and the high temperature characteristics of the secondary battery can be further improved.

[0047] Bonding material

[0048] Here, as a binding material, as long as it is a binding material that can be used in a secondary battery, it is not particularly limited. For example, as a binding material, a polymer (synthetic polymer, such as an addition polymer obtained by addition polymerization) obtained by polymerizing a monomer composition containing a monomer that can show adhesion can be used. As such a polymer, it can be cited: aliphatic conjugated diene / aromatic vinyl copolymers (polymers mainly containing aliphatic conjugated diene monomer units and aromatic vinyl monomer units), acrylic polymers (polymers mainly containing (methyl) acrylate monomer units), fluorine polymers (polymers mainly containing fluorine-containing monomer units), acrylic acid / acrylamide copolymers (polymers mainly containing (methyl) acrylic acid units and (methyl) acrylamide units), acrylonitrile polymers (polymers mainly containing (methyl) acrylonitrile units), etc. These can be used alone, and more than two kinds can be used in combination at any ratio. And, among these, preferred aliphatic conjugated diene / aromatic vinyl copolymers, acrylic acid / acrylamide copolymers, acrylonitrile polymers. It preferably includes one or more of polyvinylidene fluoride (PVDF), polyacrylate (PAA) and polyacrylonitrile (PAN), for example, more preferably polyvinylidene fluoride (PVDF), polyacrylate (PAA) or polyacrylonitrile (PAN).

[0049] Among them, the aliphatic conjugated diene monomer that can form the aliphatic conjugated diene monomer unit in the aliphatic conjugated diene / aromatic vinyl copolymer, the aromatic vinyl monomer that can form the aromatic vinyl monomer unit in the aliphatic conjugated diene / aromatic vinyl copolymer, the (meth)acrylate monomer that can form the (meth)acrylate monomer unit in the acrylic polymer, and the fluorine-containing monomer that can form the fluorine-containing monomer unit in the fluorine-based polymer, known ones can be used.

[0050] Dispersants

[0051] The dispersant contained in the secondary battery positive electrode slurry composition of the present application needs to include at least two components of component A, component B or component C, wherein the above-mentioned component A includes at least one of aryl carboxylate, fatty acid ester and phosphate, the above-mentioned component B includes silicone oil, and component C includes N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer. If a single component is used, the dispersibility of the positive electrode slurry composition cannot be made good. A single component is unstable during charging and discharging at high temperatures and is prone to decomposition. When any at least two are used in combination, they stabilize the structure through hydrogen bonding, and the thickness expansion of the secondary battery having the positive electrode formed using the positive electrode slurry composition can be reduced, so that the high temperature characteristics of the secondary battery can be further improved.

[0052] The component A mentioned above includes at least one of aryl carboxylic acid ester, fatty acid ester and phosphate ester.

[0053] The above-mentioned aromatic carboxylic acid ester can be an ester formed by a monohydric alcohol or polyhydric alcohol having 1 to 10 carbon atoms and phthalic acid, for example, it can be one or more of dimethyl phthalate, diethyl phthalate, dipropyl phthalate, dibutyl phthalate, dipentyl phthalate, dihexyl phthalate, diheptyl phthalate, dioctyl phthalate, dinonyl phthalate and didecyl phthalate.

[0054] The above-mentioned fatty acid ester can be an ester formed by a monohydric alcohol or polyhydric alcohol having 1 to 10 carbon atoms and a monohydric or polybasic carboxylic acid having 3 to 12 carbon atoms, for example, it can be one or more of diethyl adipate, dipropyl adipate, dibutyl adipate, dipentyl adipate, dihexyl adipate, diheptyl adipate, dioctyl adipate, diisooctyl adipate, diethyl sebacate, dipropyl sebacate, dibutyl sebacate, dipentyl sebacate, dihexyl sebacate, diheptyl sebacate and dioctyl sebacate.

[0055] The above-mentioned phosphate ester can be an ester formed by a monohydric alcohol or polyhydric alcohol having a carbon number of 1 to 10 and phosphoric acid, for example, it can be one or more of tricresyl phosphate, trioctyl phosphate, tributyl phosphate and triphenyl phosphate. Preferably, the phthalate ester is dibutyl phthalate (DBP) and / or dioctyl phthalate (DOP), the phosphate ester is tricresyl phosphate (TCP) and / or trioctyl phosphate (TOP), and the fatty acid ester is dioctyl sebacate (DOS) and / or dioctyl adipate (DOA).

[0056] In addition, the component A content ratio in the dispersant is preferably 10% by mass or more, more preferably 15% by mass or more, further preferably 20% by mass or more, preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less. This is because, if the dispersant contains component A above the above lower limit, the dispersibility of the positive electrode slurry composition can be made better, so that, for example, the coating of the positive electrode slurry composition on the current collector to form a positive electrode composite material layer is better. In addition, if the dispersant contains component A below the above upper limit, the dispersibility and viscosity stability of the positive electrode slurry composition can be improved, so that, for example, the coating of the positive electrode slurry composition on the current collector to form a positive electrode composite material layer is better. And because, if the content ratio of component A in the dispersant is within the above range, the high temperature characteristics of the secondary battery can be further improved.

[0057] The above-mentioned component B includes silicone oil, for example, dimethyl polysiloxane (INCI name: dimethicone oil), dimethyl polysiloxane having a hydroxyl terminal group (INCI name: dimethiconol), methylphenyl polysiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, silicone oil, polyether-modified siloxane, high-polymer siloxane with an average degree of polymerization of 650-10000, amino-modified siloxane, betaine-modified siloxane, alkyl-modified siloxane, alkoxy-modified siloxane, mercapto-modified siloxane, carboxyl-modified siloxane, fluorine-modified siloxane, etc. can be listed.

[0058] Among the above, examples of the amino-modified silicone include aminopropyl methylsiloxane-dimethylsiloxane copolymer (INCI name: aminopropyl dimethicone), aminoethylaminopropyl methylsiloxane-dimethylsiloxane copolymer (INCI name: amodimethicone), and aminoethylaminopropyl methylsiloxane-dimethylsiloxane copolymer (INCI name: trimethylsilyl amodimethicone).

[0059] In addition, the content ratio of component B in the dispersant is preferably 10% by mass or more, more preferably 20% by mass or more, further preferably 30% by mass or more, preferably 80% by mass or less, more preferably 70% by mass or less, and further preferably 60% by mass or less. This is because if the dispersant contains component B above the above lower limit, the dispersibility of the positive electrode slurry composition can be better, and the decomposition of component A can be inhibited during high-temperature charge and discharge, thereby further improving the high-temperature characteristics of the secondary battery.

[0060] The above-mentioned component C includes N-vinyl pyrrolidone-carboxylic acid vinyl ester polymers, for example, N-vinyl pyrrolidone-vinyl acetate, N-vinyl pyrrolidone-vinyl propionate, N-vinyl pyrrolidone-vinyl butyrate, etc. A large number of hydrogen bonds will be formed between component C and component A or B, which plays a great role in maintaining the structural stability of component A or B at high temperatures. The content ratio of component C in the dispersant is preferably 1% by mass or more, more preferably 5% by mass or more, further preferably 10% by mass or more, preferably 50% by mass or less, more preferably 40% by mass or less, and further preferably 30% by mass or less. This is because, if the dispersant contains component B above the above lower limit, the dispersibility of the positive electrode slurry composition can be made better, and the decomposition of component A or B can be inhibited during high-temperature charging and discharging, thereby further improving the high-temperature characteristics of the secondary battery.

[0061] Other ingredients

[0062] In addition, the secondary battery positive electrode slurry composition may further contain other components in addition to the above-mentioned components. Moreover, as other components that may be included in the positive electrode slurry composition, any other components such as reinforcing materials, leveling agents, viscosity modifiers, electrolyte additives, etc. may be cited. These are not particularly limited as long as they do not affect the battery reaction, and known components can be used. These components can be used alone, or two or more can be used in combination at any ratio.

[0063] Solvents

[0064] The solvent of the secondary battery positive electrode slurry composition is not particularly limited, and a known storage medium, water or N-methylpyrrolidone (NMP) can be used.

[0065] Method for preparing slurry composition for positive electrode

[0066] The slurry composition for secondary battery positive electrode can be prepared by storing the above components in a solvent at the same time or in any order. Specifically, the slurry composition for positive electrode can be prepared by mixing the above components and the solvent using a ball mill, a sand mill, a bead mill, or a planetary mixer.

[0067] Positive electrode for secondary battery

[0068] The positive electrode for secondary battery of the present application is characterized in that it is formed using any of the above-mentioned slurry compositions for secondary battery, and generally has a structure in which a positive electrode composite material layer formed using the above-mentioned slurry composition for positive electrode is formed on a current collector. Moreover, the positive electrode for secondary battery of the present application is obtained using the above-mentioned slurry composition for positive electrode, so when used as a positive electrode of a secondary battery, the secondary battery can exert excellent high temperature characteristics.

[0069] current collector

[0070] As the current collector, a material having conductivity and electrochemical durability can be used. Specifically, as the current collector, a current collector formed of a metal material such as aluminum, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. can be used. In addition, the above materials can be used alone or in combination of two or more in any ratio.

[0071] Positive electrode composite material layer

[0072] The positive electrode mixture layer is formed through the steps of applying the slurry composition for secondary battery positive electrodes (coating step) and drying the applied slurry composition for secondary battery positive electrodes (drying step).

[0073] Coating process

[0074] As a method for applying the slurry composition for the positive electrode of a secondary battery on a current collector, for example, there is no particular limitation, and a known method can be used. Specifically, as a coating method, a scraping coating method, an immersion method, a reverse roll coating method, a direct roll coating method, a gravure printing method, an extrusion method, a brush coating method, etc. can be used. At this time, the positive electrode slurry composition can be applied only on one side of the current collector, or on both sides. In addition, the thickness of the positive electrode slurry composition film on the current collector before drying after coating can be appropriately set according to the thickness of the positive electrode composite material layer obtained by drying.

[0075] Drying process

[0076] There is no particular limitation on the method for drying the positive electrode slurry composition applied on the current collector, and a known method can be used, for example, a drying method based on warm air, hot air, low-humidity air, a vacuum drying method, a drying method based on irradiation with infrared rays, electron beams, etc. By drying the positive electrode slurry composition applied on the current collector in this way, a positive electrode composite material layer can be formed on the current collector, and a positive electrode having a current collector and a positive electrode composite material layer can be obtained.

[0077] In addition, after the drying process, the positive electrode composite material layer can be subjected to pressure treatment by mold pressing or roller pressing. By pressure treatment, the adhesion between the positive electrode composite material layer and the current collector can be improved. Here, if the positive electrode composite material layer is formed using the secondary battery positive electrode slurry composition of the present application, a positive electrode having excellent softness even after pressure treatment can be obtained.

[0078] Secondary battery

[0079] Furthermore, the secondary battery of the present application is characterized in that it has a positive electrode, a negative electrode, a separator and an electrolyte, and the positive electrode is the positive electrode for the secondary battery of the present application described above. In addition, the negative electrode can be set to a known negative electrode. Furthermore, the secondary battery of the present application has the positive electrode for the secondary battery of the present application as the positive electrode, so it has excellent high temperature characteristics.

[0080] In addition, in the following, a case where the secondary battery is a lithium ion secondary battery will be described as an example, but the present application is not limited to the following example.

[0081] negative electrode

[0082] The negative electrode can usually be set as a known negative electrode. The composition of the negative electrode is well known to those skilled in the art. In general, the negative electrode includes a conductive substrate and a negative electrode material coated or filled on the conductive substrate, and the negative electrode material includes a negative electrode active substance and a binder. The negative electrode active material is not particularly limited, and conventional negative electrode active materials that can be embedded and released lithium in the art can be used, such as carbon materials and silicon-based materials. The carbon material is selected from one or more of non-graphitized carbon, graphite, or carbon or pyrolytic carbon obtained by high-temperature oxidation of polyacetylene polymer materials, coke, organic polymer sintered products, and activated carbon. The organic polymer sintered product can be a product obtained by sintering and carbonizing phenolic resin, epoxy resin, etc. The silicon-based material includes silicon oxide or silicon carbide.

[0083] The type and content of the negative electrode binder are well known to those skilled in the art, such as fluorine-containing resins and polyolefin compounds such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), styrene-butadiene rubber (SBR), hydroxypropyl methylcellulose, sodium carboxymethylcellulose, hydroxyethyl cellulose, and polyvinyl alcohol. The negative electrode material may also include a conductive agent to increase the conductivity of the electrode and reduce the internal resistance of the battery. The conductive agent is not particularly limited and may be a conventional negative electrode conductive agent in the art, such as one or more of carbon black, nickel powder, and copper powder. The negative electrode conductive substrate may be a conventional negative electrode conductive substrate in a lithium ion battery, such as stamped metal, metal foil, mesh metal, and foamed metal. In a specific embodiment of the present invention, copper foil is used as the negative electrode conductive substrate.

[0084] The negative electrode can be prepared by a conventional preparation method. For example, the negative electrode material is mixed with a solvent, coated on the conductive substrate, dried, and rolled or not rolled to obtain the negative electrode. The drying and rolling methods and conditions are well known to those skilled in the art.

[0085] Diaphragm

[0086] As a diaphragm, there is no particular limitation, and examples include: a microporous membrane using a resin of a polyolefin system (polyethylene, polypropylene, polybutene, polyvinyl chloride), a microporous membrane using a resin such as polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimide amide, polyarylamide, polycycloolefin, nylon, polytetrafluoroethylene, a woven or nonwoven fabric using polyolefin fibers, an aggregate of particles formed by an insulating material, etc. Among these, from the aspect of being able to thin the overall thickness of the diaphragm, thereby being able to increase the ratio of the electrode composite material layer in the secondary battery and increase the capacity per unit volume, it is preferred to use a microporous membrane of a resin of a polyolefin system (polyethylene, polypropylene, polybutene, polyvinyl chloride). Among them, a microporous membrane formed by a polyethylene resin is more preferably used.

[0087] Electrolyte

[0088] As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent can be generally used. As the supporting electrolyte, for example, a lithium salt can be used in a lithium ion secondary battery. Examples of the lithium salt include LiPF 6 、LiAsF 6 , LiBF 4 、LiSbF 6 、LiAlCl 4 、LiClO 4 CF 3 SO 3 Li, C 4 F 9 SO 3 Li, CF 3 COOLi, (CF 3 CO) 2 NLi, (CF 3 SO 2 ) 2 NLi, (C 2 F 5 SO 2 )NLi, etc. Among them, LiPF 6 、LiClO 4 CF 3 SO 3 Li is preferred because it is easily dissolved in a solvent and shows a high degree of dissociation. In addition, the electrolyte can be used alone or in combination with two or more. Because there is usually a tendency that the higher the degree of dissociation of the supporting electrolyte, the higher the lithium ion conductivity, the lithium ion conductivity can be adjusted according to the type of supporting electrolyte.

[0089] As an organic solvent used in the electrolyte, there is no particular limitation as long as it can dissolve the supporting electrolyte. For example, in lithium-ion secondary batteries, carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and ethyl methyl carbonate (EMC) can be preferably used; esters such as γ-butyrolactone, methyl formate, ethyl acetate, propyl propionate, and ethyl propionate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, a mixed solution of these solvents can also be used. Among them, carbonates are preferred because of their high dielectric constant and wide stable potential region. Because there is usually a tendency that the lower the viscosity of the solvent used, the higher the lithium ion conductivity, the lithium ion conductivity can be adjusted according to the type of solvent. In addition, the concentration of the electrolyte in the electrolyte can be appropriately adjusted.

[0090] Battery Assembly

[0091] Moreover, the secondary battery of the present application is not particularly limited and can be manufactured using a known assembly method. Specifically, the secondary battery of the present application can be manufactured by, for example, the following method: the positive electrode, negative electrode and separator obtained above are wound, folded, etc. as needed to make them into a battery shape and placed in a battery container, and an electrolyte is injected into the battery container and sealed. Here, in order to prevent the internal pressure of the secondary battery from rising, overcharging and discharging, etc., overcurrent protection elements such as fuses, PTC elements, porous metal meshes, guide plates, etc. can also be provided as needed. In addition, the shape of the secondary battery can be, for example, any of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc.

[0092] Example

[0093] The present application will be specifically described below based on examples, but the present application is not limited to these examples. In addition, in the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.

[0094] The viscosity, viscosity ratio, dispersibility and coating properties of the slurry composition for secondary battery positive electrodes, the flexibility of the positive electrode, and the high-temperature characteristics of the lithium ion secondary battery were measured and evaluated by the following methods.

[0095] (1) Dispersibility

[0096] The dispersibility of the slurry composition for secondary battery positive electrodes described in the present application was measured using a fineness meter (groove depth: 0 μm to 100 μm) in accordance with JIS K5600-2-5. Then, the dispersibility was evaluated according to the following criteria.

[0097] The smaller the particle size measured above, the higher the storage capacity of the secondary battery positive electrode slurry composition and the better the dispersibility. A, B, C, and D in the "Dispersibility" column in Table 1 represent:

[0098] A: Particle size less than 30μm

[0099] B: Particle size is 30 μm or more and less than 50 μm

[0100] C: Particle size is 50 μm or more and less than 70 μm

[0101] D: Particle size is 70μm or more

[0102] (2) Coating properties

[0103] In the present application, the coating property of the slurry composition for secondary battery positive electrodes is evaluated by the smoothness index of the positive electrode composite material layer formed using the positive electrode slurry composition.

[0104] Specifically, a positive electrode slurry composition is used to form a positive electrode composite material layer on a current collector. For the positive electrode raw material before roller pressing with the positive electrode composite material layer, a smoothness index is calculated from the thickness (layer thickness), and the smoothness index is evaluated. More specifically, first, for any 10 points of the end within 2 cm from both ends of the width direction of the positive electrode raw material before roller pressing, the layer thickness is measured, and the average value (the average thickness of the end) is calculated. In addition, as described above, for any 10 points of the central part within 2 cm from the center of the width direction of the positive electrode raw material before roller pressing to both sides, the layer thickness is measured, and the average value (the average thickness of the central part) is calculated. Then, the smoothness index (that is, the absolute value of the difference between the average layer thickness of the end and the average layer thickness of the central part is expressed as a percentage of the average layer thickness of the central part) is calculated according to the following formula (1), and the following benchmarks are used for evaluation.

[0105] Smoothness index (%) = (|average layer thickness at the end portion - average layer thickness at the center portion| / average layer thickness at the center portion) × 100 (1)

[0106] The smaller the smoothness index, the higher the smoothness of the positive electrode composite material layer, and the better the coating property of the positive electrode slurry composition. A, B, and C in the "Coating Property" column in Table 1 represent:

[0107] A: Smoothness index is less than 3%

[0108] B: Smoothness index is 3% or more and less than 8%

[0109] C: Smoothness index is 8% or more

[0110] (3) Softness

[0111] The flexibility of the positive electrode was evaluated by the presence or absence of cracks and ruptures in the positive electrode raw material before roll pressing. Specifically, the state of cracks and ruptures in the positive electrode raw material was observed according to the evaluation criteria of JIS K5600-8-4 shown below.

[0112] The harder it is to observe cracks and fissures, the better the flexibility of the positive electrode. In the "Flexibility" column of Table 1, A, B, C, D, and E represent:

[0113] A: Even if it is enlarged by 2 times, it cannot be visually perceived.

[0114] B: A 2-fold enlargement is visually perceptible on less than 5% of the surface.

[0115] C: Barely recognizable with normal corrected vision.

[0116] D: Can be clearly identified with normal corrected vision.

[0117] E: Large cracks with a width of usually up to 1 mm.

[0118] (4)High temperature characteristics

[0119] After the electrolyte was injected, the prepared lithium-ion secondary battery was left to stand at a temperature of 25°C for 5 hours. Then, the battery cell voltage was 3.65V by a constant current method at a temperature of 25°C and 0.2C, and then an aging treatment was performed at a temperature of 60°C for 12 hours. Then, the battery cell voltage was 3.00V by a constant current method at a temperature of 25°C and 0.2C. After that, CC-CV charging was performed at a constant current of 0.2C (the upper limit battery cell voltage was 4.50V), and CC discharge was performed at a constant current of 0.2C until the battery cell voltage was 3.00V. Repeat the charge and discharge at 0.2C three times. The third discharge capacity at 0.2C is set as the initial capacity CX. After that, CC-CV charging was performed at a constant current of 0.2C (the upper limit battery cell voltage was 4.50V). Next, the lithium-ion secondary battery was stored for 4 weeks in an inert oven with a nitrogen environment of 60°C in the treatment chamber. After that, discharge by constant current method at 0.2C until the battery cell voltage is 3.00V, and set the discharge capacity at this time as CY. Calculate the high temperature capacity retention rate represented by (CY / CX)×100(%) and evaluate it by the following criteria. The greater the high temperature capacity retention rate, the less deterioration of the lithium ion secondary battery under high temperature storage (that is, the better the high temperature storage characteristics). A, B, C, and D in the "High Temperature Performance" column in Table 1 represent:

[0120] A: High temperature capacity retention rate is more than 90%

[0121] B: High temperature capacity retention rate is 85% or more and less than 90%

[0122] C: High temperature capacity retention rate is 80% or more and less than 85%

[0123] D: High temperature capacity retention rate is less than 80%

[0124] Example 1

[0125] Preparation of slurry composition for positive electrode

[0126] In a double planetary mixer with a storage device, 97 parts of lithium cobalt oxide (4.5VLCO, Xiatung New Energy) as a positive electrode active material, 1 part of a dispersant (30wt% of component A01, 70wt% of component B01) calculated as solid content, 1 part of polyvinylidene fluoride, and 1 part of acetylene black were added, and the powder was mixed at a temperature of 25°C for 20 minutes, and then the solvent N-methylpyrrolidone (NMP) was added to adjust the solid content and slurry viscosity, and then mixed for 20 minutes to obtain a storage solution. The obtained storage solution was degassed under reduced pressure to obtain a slurry composition for the positive electrode of a lithium-ion secondary battery. Then, the dispersibility of the obtained positive electrode slurry composition was evaluated according to the above method. The results are shown in Table 1.

[0127] Cathode Manufacturing

[0128] The obtained positive electrode slurry composition is coated on a 9 μm thick aluminum foil as a current collector in such a manner that the thickness of the dried positive electrode composite material layer is about 60 μm. Next, the aluminum foil coated with the positive electrode slurry composition is transported in an oven at a temperature of 60 ° C and a speed of 0.5 m / min for 2 minutes, and then transported in an oven at a temperature of 120 ° C for 2 minutes, and heat-treated to obtain a positive electrode raw material before roller pressing. Then, the coating property of the obtained positive electrode raw material before roller pressing is evaluated according to the above method. The results are shown in Table 1.

[0129] Next, the obtained positive electrode raw material was rolled by roller pressing to produce a positive electrode for a lithium ion secondary battery having a positive electrode composite material layer with a thickness of 45 μm. Then, the flexibility of the obtained positive electrode for a lithium ion secondary battery was evaluated according to the above method. The results are shown in Table 1.

[0130] Negative electrode manufacturing

[0131] In a double planetary mixer with a storage machine, 97 parts of artificial graphite as a negative electrode active material and 1.0 part of carboxymethyl cellulose as a viscosity modifier in terms of solid content were added, and an appropriate amount of ion exchange water was added, and mixed at a temperature of 25°C for 60 minutes. Furthermore, after adjusting the solid content concentration to 52% with ion exchange water, a mixed solution was obtained by mixing at a temperature of 25°C for 15 minutes. To the obtained mixed solution, 2 parts of a styrene-butadiene copolymer solution with a solid content concentration of 40% and ion exchange water were added, and the final solid content concentration was adjusted to 42%, and then mixed for 10 minutes to obtain a storage solution. The obtained storage solution was degassed under reduced pressure to obtain a slurry composition for a negative electrode of a lithium-ion secondary battery.

[0132] Next, the above-obtained slurry composition for the negative electrode of the lithium ion secondary battery is applied to the copper foil (thickness 5 μm) as the current collector in such a manner that the thickness of the negative electrode composite material layer after drying is about 70 μm. In addition, the copper foil coated with the slurry composition for the negative electrode of the lithium ion secondary battery is transported in an oven at a temperature of 60 ° C and a speed of 0.5 m / min for 2 minutes, and then at a temperature of 120 ° C, It took 2 minutes to transport in the oven and heat-treated to obtain the negative electrode raw material before roller pressing. Then, the obtained negative electrode raw material is rolled by roller pressing to prepare a negative electrode for a lithium ion secondary battery with a thickness of 50 μm of the negative electrode composite material layer.

[0133] Manufacturing of lithium-ion secondary batteries

[0134] The lithium ion secondary battery positive electrode obtained above is arranged in a manner that the current collector surface is in contact with the aluminum plastic film outer packaging. In addition, a single-layer polyethylene diaphragm (width 65mm, length 500mm, thickness 7μm, porosity 53%) manufactured by a dry method is arranged on the surface of the positive electrode composite material layer side of the positive electrode. Furthermore, the lithium ion secondary battery negative electrode obtained above is arranged on the arranged diaphragm in a manner that the surface of the negative electrode composite material layer is opposite to the diaphragm. Next, a concentration of 12% by mass of LiPF 6 The solution is filled in the aluminum plastic film material as an electrolyte, wherein the solvent of the electrolyte is a mixed solvent of ethylene carbonate / ethyl methyl carbonate / propylene carbonate / ethyl propionate / propyl propionate=1 / 1 / 1 / 1 / 1 (mass ratio), and the additives of the electrolyte are: 2% by mass of vinyl sulfate and 4% by mass of succinonitrile. Then, heat sealing at a temperature of 150° C. is performed to seal the opening of the aluminum packaging material to manufacture a lithium ion secondary battery.

[0135] The high temperature characteristics of the obtained lithium ion secondary battery were evaluated according to the above method.

[0136] Embodiments 2 to 17:

[0137] The difference between Examples 2 to 17 and Example 1 is that the conductive material, binder and dispersant used in Examples 2 to 17 are changed as shown in Table 1. Otherwise, the slurry composition for secondary battery is prepared, the separator is prepared, the negative electrode, the positive electrode and the secondary battery are manufactured in the same manner as in Example 1. Then, various evaluations are performed in the same manner as in Example 1. The results are shown in Table 1.

[0138] Comparative Examples 1 to 7:

[0139] The difference between Comparative Examples 1 to 7 and Example 1 is that the conductive material, binder and dispersant used in Comparative Examples 1 to 7 are changed as shown in Table 1. Otherwise, the slurry composition for secondary battery is prepared, the separator is prepared, and the negative electrode, positive electrode and secondary battery are manufactured in the same manner as in Example 1. Then, various evaluations are performed in the same manner as in Example 1. The results are shown in Table 1.

[0140] Table 1 Addition of relevant components and performance test results in Examples 1 to 17 and Comparative Examples 1 to 7

[0141]

[0142]

[0143] The abbreviations of component A and component B of the dispersant in Table 1 are shown in Table 2 below, wherein C01 in Table 1 is N-vinyl pyrrolidone-vinyl acetate polymer. Component A includes at least one of aromatic carboxylic acid ester, fatty acid ester and phosphate ester, component B includes silicone oil, and component C includes N-vinyl pyrrolidone-vinyl acetate polymer (C01), and the above substances can be purchased commercially.

[0144] Table 2 Abbreviations of component A and component B of the dispersant in Table 1

[0145] Component A abbreviation Component B abbreviation Dimethyl phthalate A01 Polyether modified siloxane B01 Dioctyl adipate A02 Dimethicone B02 Dibutyl adipate A03 Dodecamethylcyclohexasiloxane B03 Tributyl phosphate A04 Fluorine-modified siloxane B04

[0146] The technical solution of this application is analyzed in combination with Table 1 and Table 2:

[0147] (1) By comparing Example 1 and Comparative Example 1, it can be seen that when no dispersant is used, the dispersibility of the positive electrode slurry composition is poor, and the electrode sheet cracks are obvious, reaching a level that makes it difficult to manufacture the positive electrode and the secondary battery.

[0148] (2) By comparing Comparative Example 1 with Comparative Examples 2 to 7, it can be seen that, compared with not using a dispersant, using a single-component dispersant can improve the dispersibility and coating properties of the positive electrode slurry composition to a certain extent. However, the softness of the positive electrode prepared using the positive electrode slurry composition is still poor, and the high-temperature performance of the secondary battery assembled with the positive electrode is still poor.

[0149] (3) By comparing Examples 1 to 17 and Comparative Examples 2 to 7, it can be seen that compared with a single-component dispersant, the positive electrode slurry composition obtained by using at least two dispersant components has significantly better dispersibility and coating properties, the positive electrode prepared by the positive electrode slurry has better softness, and the high-temperature performance of the secondary battery assembled with the positive electrode is significantly excellent; and it has excellent effects in the binder material polyvinylidene fluoride (PVDF), polyacrylate (PAA) or polyacrylonitrile (PAN) system. It shows that when the dispersant contains at least two of component A, component B and component C, it can stabilize the structure by forming abundant hydrogen bonds, thereby reducing the thickness expansion of the secondary battery of the positive electrode formed by the positive electrode slurry composition, thereby further improving the high-temperature characteristics of the secondary battery.

[0150] (4) By comparing Example 3 and Example 5, and Example 6 and Example 7, it can be seen that compared with a dispersant having any two of Component A, Component B and Component C, the dispersibility and coating properties of the positive electrode slurry composition containing a dispersant of Component A, Component B and Component C are further improved, and thus the high temperature performance of the secondary battery prepared is further improved.

[0151] (5) By comparing Comparative Examples 1 to 4 and Comparative Examples 5 to 7, it can be seen that when the conductive material includes carbon nanotubes (CNTs), the high-temperature performance of the secondary battery prepared is better. This is because the positive electrode slurry composition containing the fibrous conductive carbon material can well reduce the internal resistance of the secondary battery assembled with the positive electrode formed therefrom, thereby further improving the high-temperature characteristics of the secondary battery.

[0152] (6) By comparing Example 1 and Example 4, and Example 13 and Example 14, it can be seen that when the dispersant contains two of Component A, Component B, and Component C, the dispersant having Component C has better dispersibility and coating performance, and the high-temperature performance of the secondary battery prepared may be better.

[0153] In summary, the positive electrode slurry composition having the above-described predetermined composition has excellent dispersibility and coating properties, and a secondary battery having a positive electrode formed using the positive electrode slurry composition can exhibit good high-temperature characteristics.

[0154] The present application has industrial applicability: According to the present application, a positive electrode slurry composition that has excellent dispersibility and can produce a secondary battery that can exhibit good high-temperature characteristics can be provided.

[0155] Furthermore, according to the present application, it is possible to provide a positive electrode capable of manufacturing a secondary battery that can exhibit good high-temperature characteristics, and a secondary battery that can exhibit good high-temperature characteristics.

[0156] The above embodiments are merely illustrative of the principles and effects of the present application and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.

Claims

1. A slurry composition for a secondary battery positive electrode, comprising a positive electrode active material, a conductive material and a binding material, Features: The slurry composition also includes a dispersant, which includes at least two components of component A, component B or component C, wherein component A includes at least one of aromatic carboxylic acid ester, fatty acid ester and phosphate ester, component B includes silicone oil, and component C includes N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer.

2. The slurry composition for secondary battery positive electrode according to claim 1, Features: The content ratio of the component A is 10wt% to 50wt% of the dispersant; preferably 15wt% to 40wt%; more preferably 20wt% to 30wt%; And / or, the content ratio of the component B is 10wt% to 80wt% of the dispersant; preferably 20wt% to 70wt%; more preferably 30wt% to 60wt%; And / or, the content ratio of the component C is 1wt% to 50wt% of the dispersant; preferably 5wt% to 40wt%; more preferably 10wt% to 30wt%; And / or, the content ratio of the conductive material is 0.1 wt % to 10 wt % of the positive electrode active material.

3. The slurry composition for secondary battery positive electrode according to claim 1, Features: The aromatic carboxylic acid ester includes one or more of dimethyl phthalate, diethyl phthalate, dipropyl phthalate, dibutyl phthalate, dipentyl phthalate, dihexyl phthalate, diheptyl phthalate, dioctyl phthalate, dinonyl phthalate and didecyl phthalate; And / or, the fatty acid ester comprises one or more of diethyl adipate, dipropyl adipate, dibutyl adipate, dipentyl adipate, dihexyl adipate, diheptyl adipate, dioctyl adipate, diisooctyl adipate, diethyl sebacate, dipropyl sebacate, dibutyl sebacate, dipentyl sebacate, dihexyl sebacate, diheptyl sebacate and dioctyl sebacate; And / or, the phosphate ester includes one or more of tricresyl phosphate, trioctyl phosphate, tributyl phosphate and triphenyl phosphate; Preferably, the component A includes one or more of dibutyl phthalate, dioctyl phthalate, tricresyl phosphate, trioctyl phosphate, dioctyl sebacate or dioctyl adipate.

4. The slurry composition for secondary battery positive electrode according to claim 1, Features: The silicone oil includes a synthetic polymer substance in which silicon and oxygen connected by organic groups are chemically bonded to each other; Preferably, the silicone oil includes one or more of dimethylpolysiloxane, polydimethylsiloxane alcohol, methylphenylpolysiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, polyether-modified siloxane, high-polymer siloxane with an average degree of polymerization of 650-10000, amino-modified siloxane, betaine-modified siloxane, alkyl-modified siloxane, alkoxy-modified siloxane, mercapto-modified siloxane, carboxyl-modified siloxane or fluorine-modified siloxane; wherein the amino-modified siloxane includes one or more of aminopropylmethylsiloxane-dimethylsiloxane copolymer, aminoethylaminopropylsiloxane-dimethylsiloxane copolymer and aminoethylaminopropylmethylsiloxane-dimethylsiloxane copolymer.

5. The slurry composition for secondary battery positive electrode according to claim 1, Features: The N-vinyl pyrrolidone-carboxylic acid vinyl ester polymer includes one or more of N-vinyl pyrrolidone-vinyl acetate, N-vinyl pyrrolidone-vinyl propionate and N-vinyl pyrrolidone-vinyl butyrate.

6. The slurry composition for secondary battery positive electrode according to claim 1, Features: The conductive material comprises a fibrous conductive carbon material; Preferably, the fibrous conductive carbon material comprises carbon nanotubes; Preferably, the content ratio of the fibrous conductive carbon material is 5wt% to 100wt% of the conductive material; Preferably, the aspect ratio of the fibrous conductive carbon material is greater than 5; preferably, the aspect ratio is greater than 10; Preferably, the average fiber diameter of the fibrous conductive carbon material is 0.5 nm to 1 μm; Preferably, the average fiber length of the fibrous conductive carbon material is 1 μm to 200 μm.

7. The slurry composition for secondary battery positive electrode according to claim 1, Features: The bonding material comprises one or more of polyvinylidene fluoride, polyacrylate and polyacrylonitrile.

8. The slurry composition for secondary battery positive electrode according to claim 1, Features: The dispersant comprises component A, component B and component C.

9. The slurry composition for secondary battery positive electrode according to claim 1, Features: The secondary battery positive electrode slurry composition is subjected to a shearing speed of 10 s -1 The viscosity η 0 At a shear rate of 1000s -1 The viscosity η 1 The ratio is 2 to 20.

10. Use of the slurry composition for a secondary battery positive electrode according to any one of claims 1 to 9 in preparing a composite material layer for a secondary battery positive electrode, a secondary battery positive electrode or a secondary battery.

11. A composite material layer for a secondary battery positive electrode, Features: The positive electrode composite material layer is formed from the slurry composition for a secondary battery positive electrode according to any one of claims 1 to 9.

12. A positive electrode for a secondary battery, Features: The positive electrode for a secondary battery is formed from the slurry composition for a positive electrode for a secondary battery according to any one of claims 1 to 9.

13. A secondary battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, Features: The positive electrode includes the positive electrode for a secondary battery according to claim 12.

Citation Information

Patent Citations

  • Binder resin composition for secondary battery electrodes, slurry for secondary battery electrodes, electrode for secondary batteries, and lithium ion secondary battery

    CN104081567A

  • Water-based solid electrolyte membrane, preparation method thereof, and secondary battery

    CN108598563A

  • Ion conductor slurry and preparation method and application thereof

    CN109817871A

  • Slurry composition for positive electrode of lithium secondary battery, and positive electrode and lithium secondary battery comprising same

    CN114930581A

  • High-solid-content graphene composite conductive paste, preparation method and application thereof

    CN115101750A

Cited By

  • Modified positive electrode sheet, preparation method therefor and use thereof

    WO2026149092A1