Polyester and molded product composed of the same

By adding specific compounds like polyoxyethylene sorbitan monolaurate and hindered phenolic antioxidants to the polyester, gel formation and coloring are suppressed, enabling high-temperature polycondensation and producing safe, high-quality molded products.

JP2024134860AInactive Publication Date: 2024-10-04KURARAY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023045281
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing crosslinked polyesters are prone to gel formation and coloring due to the use of crosslinking agents with small molecular weights or those that decompose at high polycondensation temperatures, compromising their suitability for extrusion molding.

Method used

Incorporating 0.001 to 0.2 mol% of units derived from a specific compound represented by formula (I), such as polyoxyethylene sorbitan monolaurate, and optionally 0.0005 to 0.2 mol% of hindered phenolic antioxidant units, into the polyester composition to suppress gel formation and coloring, while maintaining non-Newtonian properties suitable for extrusion molding.

Benefits of technology

The solution results in a polyester with suppressed gel formation and coloring, even at high polycondensation temperatures, ensuring high safety and excellent appearance in molded products, suitable for extrusion blow molding and profile extrusion molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134860000001
    Figure 2024134860000001
  • Figure 2024134860000002
    Figure 2024134860000002
  • Figure 2024134860000003
    Figure 2024134860000003
Patent Text Reader

Abstract

To provide a slightly crosslinked polyester resin with high safety that has a predetermined non-Newtonian behavior and suppresses gel formation and coloration even during polycondensation at high temperatures.SOLUTION: The present invention provides a polyester comprising 0.001-0.2 mol% of a unit derived from a compound represented by formula (I). [In formula (I), the total of x, y, z, and w is 1-50, and R1-R4 independently represent a hydrogen atom or a C1-18 acyl group].SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a slightly crosslinked polyester in which the generation of gel and coloring are suppressed, and a method for producing the same. [Background technology]

[0002] Polyesters are excellent in various properties such as transparency, mechanical properties, gas barrier properties, flavor barrier properties, etc., and furthermore, when molded into articles, there is little concern about residual monomers or harmful additives, and they are excellent in hygiene and safety. For these reasons, polyesters have been widely used in recent years as hollow containers for filling juices, soft drinks, seasonings, oils, cosmetics, detergents, and other products, as an alternative to the conventionally used polyvinyl chloride resins.

[0003] Incidentally, a slightly crosslinked polyester in which molecular chains are crosslinked by adding a multifunctional crosslinking agent is used in extrusion blow molding, profile extrusion molding, and the like. By appropriately crosslinking the molecular chains of polyester, non-Newtonian properties suitable for extrusion blow molding and the like are expressed. Patent Documents 1 and 2 describe copolymerized polyesters obtained using trimellitic anhydride, pyromellitic anhydride, trimethylolpropane, tetramethylolmethane, pentaerythritol, trimesic acid, and the like as crosslinking agents. However, these crosslinking agents have a small molecular weight and a small minimum molecular weight between crosslinking points, so there is a problem that gels are easily generated. On the other hand, when a crosslinking agent with a large molecular weight is used to increase the minimum molecular weight between crosslinking points, the amount of crosslinking agent added required to express the required non-Newtonian properties increases. Polycondensation of polyester is carried out at a high temperature compared to other resins, and when such a crosslinking agent is used, the polyester is colored due to its decomposition, which has been a problem. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Unexamined Patent Publication No. 7-179581 [Patent Document 2] Japanese Patent Application Publication No. 9-157365 Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made in order to solve the above problems, and an object of the present invention is to provide a slightly crosslinked polyester in which gel formation and coloration are suppressed. [Means for solving the problem]

[0006] The above-mentioned problems can be solved by providing a polyester containing units derived from a compound represented by the following formula (I) in an amount of 0.001 to 0.2 mol % based on the total monomer units.

[0007] [ka] [In formula (I), the sum of x, y, z and w is 1 to 50, and R 1 ~R 4 each independently represents a hydrogen atom or an acyl group having 1 to 18 carbon atoms.] This is solved by providing

[0008] In this case, it is preferable that the compound represented by the above formula (I) is at least one selected from the group consisting of polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monopalmitate, and polyoxyethylene sorbitan trioleate.

[0009] It is also preferred that the polyester further contains 0.0005 to 0.2 mol % of units derived from a hindered phenol-based antioxidant based on the total monomer units.The polyester is preferably at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene furanoate, and polylactic acid, and is more preferably polyethylene terephthalate containing 1.5 to 25 mol % of cyclohexanedimethanol units or isophthalic acid units.It is also preferred that the polyester has an intrinsic viscosity of 0.7 dl / g or more.

[0010] A molded article obtained by extrusion molding of the polyester is a preferred embodiment of the present invention, and a molded article obtained by extrusion blow molding or profile extrusion molding is a more preferred embodiment. A film or sheet made of the molded article is a more preferred embodiment of the present invention, and a thermoformed article obtained by thermoforming the film or sheet is a further preferred embodiment. A container made of the molded article is also a more preferred embodiment of the present invention.

[0011] The above-mentioned problems can also be solved by providing a method for producing the polyester, which comprises polycondensing an ester-forming monomer and a compound represented by the above formula (I). Effect of the Invention

[0012] The polyester of the present invention has non-Newtonian properties suitable for extrusion molding, and is suppressed in gel formation and coloration, even though polycondensation is carried out at high temperatures, as compared with other resins. Moreover, the polyester is highly safe. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The polyester of the present invention contains 0.001 to 0.2 mol % of units derived from the compound represented by the following formula (I) based on the total monomer units. By using the compound represented by the following formula (I) as a crosslinking agent, a polyester is obtained that has non-Newtonian properties suitable for extrusion molding and the like, and suppresses gel formation and coloration, even though polycondensation is carried out at a higher temperature than other resins. Moreover, the compound represented by the following formula (I) is widely used internationally as a food additive and is highly safe, so the polyester is highly safe.

[0014] [ka] [In formula (I), the sum of x, y, z and w is 1 to 50, and R 1 ~R 4 each independently represents a hydrogen atom or an acyl group having 1 to 18 carbon atoms.]

[0015] The polyester of the present invention contains 0.001 to 0.2 mol% of the unit derived from the compound represented by the above formula (I) based on the total monomer units. When the content of the unit derived from the compound represented by the above formula (I) is less than 0.001 mol%, the above effect is not achieved. The content is preferably 0.002 mol% or more, more preferably 0.005 mol% or more, even more preferably 0.007 mol% or more, and particularly preferably 0.008 mol% or more. From the viewpoint of obtaining a polyester with high melt tension, the content is preferably 0.01 mol% or more, more preferably 0.03 mol% or more, even more preferably 0.05 mol% or more, particularly preferably 0.08 mol% or more, and most preferably 0.1 or more. On the other hand, when the content exceeds 0.2 mol%, the required non-Newtonian property is not obtained and the obtained polyester is colored. The content is preferably 0.15 mol% or less. In order to obtain a polyester in which coloration is extremely suppressed, the content is preferably 0.1 mol % or less, and particularly preferably 0.02 mol % or less.

[0016] In the above formula (I), the sum of x, y, z and w is 1 to 50. If the sum is less than 1, the minimum molecular weight between crosslinks is reduced, causing gelation in the resulting polyester. The sum is preferably 4 or more, more preferably 8 or more, even more preferably 12 or more, particularly preferably 16 or more, and most preferably 18 or more. On the other hand, if the sum exceeds 50, the required non-Newtonian properties are not obtained, and the resulting polyester is colored. The sum is preferably 40 or less, more preferably 32 or less, even more preferably 28 or less, particularly preferably 24 or less, and most preferably 22 or less.

[0017] In the above formula (I), R 1 ~R 4 each independently represents a hydrogen atom or an acyl group having 1 to 18 carbon atoms. From the viewpoint of suppressing gel formation, the number of carbon atoms in the acyl group is preferably 2 or more, more preferably 4 or more, even more preferably 6 or more, particularly preferably 7 or more, and most preferably 8 or more. On the other hand, from the viewpoint of availability, the number of carbon atoms is 18 or less, preferably 16 or less, more preferably 14 or less, and most preferably 12 or less. The acyl group may be a straight chain or a branched chain, but the former is preferred.

[0018] The compound represented by the above formula (I) is preferably at least one selected from the group consisting of polyoxyethylene sorbitan monolaurate (polysorbate 20), polyoxyethylene sorbitan monostearate (polysorbate 60), polyoxyethylene sorbitan monooleate (polysorbate 80), polyoxyethylene sorbitan tristearate (polysorbate 65), polyoxyethylene sorbitan monopalmitate (polysorbate 40) and polyoxyethylene sorbitan trioleate (polysorbate 85), and among these, polyoxyethylene sorbitan monolaurate is more preferred.

[0019] The reason why the use of the compound represented by the above formula (I) as a crosslinking agent produces the above-mentioned effects is unclear, but it is considered that the compound is difficult to decompose even when polycondensation is carried out at high temperatures, and the tetrahydrofuran ring contained in the compound is flexible, so that the generation of gel is suppressed even when a crosslinked structure is formed.

[0020] It is preferable that the polyester of the present invention contains dicarboxylic acid units, diol units, and units derived from the compound represented by the above formula (I), which are obtained by polycondensation of ester-forming monomers, i.e., dicarboxylic acid and diol, with the compound represented by the above formula (I).

[0021] The dicarboxylic acid is not particularly limited as long as it can be polycondensed with a diol, and examples thereof include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, biphenyl dicarboxylic acid, diphenyl ether dicarboxylic acid, diphenyl sulfone dicarboxylic acid, diphenyl ketone dicarboxylic acid, sodium sulfoisophthalate, 2,6-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, and 2,7-naphthalenedicarboxylic acid; aliphatic dicarboxylic acids such as glutaric acid, adipic acid, azelaic acid, sebacic acid, and dimer acid (and hydrogenated products thereof); alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid, norbornene dicarboxylic acid, and tricyclodecane dicarboxylic acid; and heterocyclic aromatic dicarboxylic acids such as 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, and 3,4-furandicarboxylic acid. These may be used alone or in combination of two or more. In addition, an ester-forming derivative thereof may be used instead of the dicarboxylic acid. Among them, it is preferable that the polyester contains an aromatic dicarboxylic acid unit as a dicarboxylic acid unit, and it is more preferable that the polyester contains a terephthalic acid unit.

[0022] The polyester preferably contains aromatic dicarboxylic acid units in an amount of 25 mol % or more based on the total monomer units, and the content of aromatic dicarboxylic acid units in this case is preferably 50 mol % or less based on the total monomer units.

[0023] The diol is not particularly limited as long as it can be polycondensed with a dicarboxylic acid, and examples thereof include aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, and methylpentanediol; and alicyclic diols such as cyclohexanedimethanol, norbornene dimethanol, and tricyclodecane dimethanol. A diol in which one or more molecules of ethylene oxide are added to each of two hydroxyl groups of an aromatic diol can also be used. For example, a diol in which 1 to 8 molecules of ethylene oxide are added to each of two phenolic hydroxyl groups of bisphenol A can be exemplified. These may be used alone or in combination of two or more kinds. In addition, an ester-forming derivative thereof may be used instead of a diol. Among them, it is preferable that the polyester contains an aliphatic diol unit as a diol unit, more preferably an ethylene glycol unit, a 1,3-propanediol unit, or a 1,4-butaneol unit, and even more preferably an ethylene glycol unit.

[0024] The polyester preferably contains 40 mol % or more of aliphatic diol units based on the total monomer units, and the content of the aliphatic diol units in this case is preferably 55 mol % or less based on the total monomer units.

[0025] It is also preferable that the polyester of the present invention contains a hydroxycarboxylic acid unit and a unit derived from the compound represented by the above formula (I), the unit being obtained by polycondensation of a hydroxycarboxylic acid, which is an ester-forming monomer, with the compound represented by the above formula (I).

[0026] In this case, the content of the hydroxycarboxylic acid unit in the polyester is usually 50 mol % or more, preferably 70 mol % or more, more preferably 80 mol % or more, and further preferably 90 mol % or more.

[0027] Examples of the hydroxycarboxylic acid include lactic acid, glycolic acid, 2-hydroxybutyric acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxyisobutyric acid, 2-hydroxy-2-methylbutyric acid, 2-hydroxyvaleric acid, 3-hydroxyvaleric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, 6-hydroxycaproic acid, 10-hydroxystearic acid, 4-hydroxyphenylstearic acid, and 4-(β-hydroxy)ethoxybenzoic acid. Of these, lactic acid is preferred.

[0028] The polyester of the present invention is preferably at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene furanoate, and polylactic acid, and more preferably polyethylene terephthalate. Polyethylene terephthalate, polybutylene terephthalate, and polytrimethylene terephthalate are obtained by polycondensation of terephthalic acid as the aromatic dicarboxylic acid, ethylene glycol, 1,4-butanol, or 1,3-propanediol as the aliphatic diol, and the compound represented by the above formula (I). Polylactic acid is obtained by polycondensation of lactic acid as the hydroxycarboxylic acid, and the compound represented by the above formula (I).

[0029] The polyester of the present invention is preferably a polyethylene terephthalate containing 1.5 to 25 mol % of cyclohexanedimethanol units or isophthalic acid units based on the total monomer units. From the viewpoint of strength of the molded product, it is preferable that the polyethylene terephthalate contains cyclohexanedimethanol units, and from the viewpoint of polymerization rate, it is preferable that the polyethylene terephthalate contains isophthalic acid units. The content of cyclohexanedimethanol units or isophthalic acid units is more preferably 1.6 mol % or more, and even more preferably 1.8 mol % or more. On the other hand, the content is more preferably 20 mol % or less, and even more preferably 10 mol % or less.

[0030] In recent years, the disposal of plastic molded products after use has become a social issue, and recycling treatments in which collected molded products are reprocessed and reused are desired. In the recycling of polyesters, a mechanical recycling method is generally adopted in which the collected polyesters are returned to a reusable form by separation, washing, and granulation from the viewpoint of the required energy amount and cost. In such a method, a drying step at a temperature equal to or higher than the melting temperature may be required to reduce the water content of the collected polyesters, but depending on the type of polyester, there is a problem that the polyesters are fused together in the drying step. The polyethylene terephthalate containing 1.5 to 25 mol % of the cyclohexanedimethanol unit or isophthalic acid unit relative to the total monomer units is an example of a preferred embodiment of the polyester of the present invention, since the polyesters are unlikely to be fused together even in the drying step.

[0031] When the polyethylene terephthalate contains cyclohexanedimethanol units, the content of ethylene glycol units in the polyethylene terephthalate is preferably 25 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more, based on the total monomer units, while the content is preferably 55 mol% or less, more preferably 52 mol% or less, and even more preferably 51 mol% or less.

[0032] When the polyethylene terephthalate contains isophthalic acid units, the content of the terephthalic acid units in the polyethylene terephthalate is preferably 25 mol% or more, more preferably 30 mol% or more, and even more preferably 40 mol% or more, based on the total monomer units, while the content is preferably 50 mol% or less, more preferably 49.99 mol% or less, and even more preferably 49.98 mol% or less.

[0033] The polyester of the present invention preferably further contains 0.0005 to 0.2 mol % of units derived from a hindered phenol-based antioxidant based on the total monomer units. Here, the units derived from a hindered phenol-based antioxidant are those contained in the polyester by polycondensing the hindered phenol-based antioxidant together with an ester-forming monomer and a compound represented by the above formula (I). The polyol units of the hindered phenol-based antioxidant and the carboxylic acid units having a hindered phenol group are contained in the polyester by transesterification. By containing the units derived from the hindered phenol-based antioxidant in the polyester, coloration of the polyester is further suppressed. Examples of the hindered phenol-based antioxidant include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and 1,3,5-tris[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanoyloxy]ethyl]hexahydro-1,3,5-triazine-2,4,6-trione.

[0034] The content of the units derived from the hindered phenol-based antioxidant in the polyester of the present invention is preferably 0.0005 to 0.2 mol% based on the total monomer units. If the content is less than 0.0005 mol%, the effect may not be achieved. The content is more preferably 0.0006 mol% or more, even more preferably 0.0007 mol% or more, and most preferably 0.0008 mol% or more. On the other hand, if the content exceeds 0.2 mol%, the crystallinity may decrease, resulting in a decrease in physical properties. The content is more preferably 0.190 mol% or less, even more preferably 0.150 mol% or less, particularly preferably 0.100 mol% or less, and most preferably 0.050 mol% or less.

[0035] From the viewpoint of further suppressing coloration, the molar ratio of the units derived from the hindered phenol antioxidant to the units derived from the compound represented by formula (I) in the polyester of the present invention (units derived from the hindered phenol antioxidant / units derived from the compound represented by formula (I)) is preferably 0.001 to 0.1. The molar ratio (units derived from the hindered phenol antioxidant / units derived from the compound represented by formula (I)) is more preferably 0.005 or more. From the viewpoint of obtaining a polyester in which coloration is extremely suppressed, the molar ratio (units derived from the hindered phenol antioxidant / units derived from the compound represented by formula (I)) is more preferably 0.01 or more, and even more preferably 0.05 or more. On the other hand, the molar ratio (units derived from the hindered phenol antioxidant / units derived from the compound represented by formula (I)) is more preferably 0.095 or less, even more preferably 0.090 or less, and particularly preferably 0.085 or less. In order to obtain a polyester having high melt tension, the molar ratio (units derived from the hindered phenol antioxidant / units derived from the compound represented by formula (I)) is preferably 0.05 or less, more preferably 0.02 or less, and even more preferably 0.01 or less.

[0036] The polyester of the present invention may contain units derived from other ester-forming monomers other than the dicarboxylic acid, the dicarboxylic acid and the compound represented by the above formula (I), and the hindered phenol-based antioxidant, as long as the effects of the present invention are not impaired. Examples of the other ester-forming monomers include monocarboxylic acids, monoalcohols and their ester-forming derivatives; and polyfunctional compounds having three or more carboxyl groups, hydroxyl groups and / or ester-forming groups other than the compound represented by the above formula (I). Examples of the polyfunctional compounds include trimellitic anhydride, pyromellitic anhydride, trimethylolpropane, tetramethylolmethane, pentaerythritol, trimesic acid, and the like. The content of the other ester-forming monomer units in the polyfunctional compound is preferably 5 mol% or less, more preferably 3 mol% or less, even more preferably 1 mol% or less, based on the total monomer units, and particularly preferably is not substantially contained.

[0037] From the viewpoint of further improving the melt moldability of the polyester of the present invention and the production stability of the obtained molded article, the intrinsic viscosity of the polyester is preferably 0.67 dl / g or more, more preferably 0.7 dl / g or more, even more preferably 0.8 dl / g or more, even more preferably 0.9 dl / g or more, and particularly preferably 1.0 dl / g or more, while the intrinsic viscosity is preferably 1.5 dl / g or less, more preferably 1.4 dl / g or less, and even more preferably 1.3 dl / g or less.

[0038] From the viewpoint of improving heat resistance, the glass transition temperature of the polyester is preferably 75° C. or higher, more preferably 77° C. or higher. On the other hand, the glass transition temperature is preferably 100° C. or lower. In this case, it is preferable because there is no need to heat the mold to room temperature or higher when extrusion blow molding the polyester.

[0039] From the viewpoint of further improving the drawdown resistance during extrusion blow molding, the melting point of the polyester is preferably 225° C. or higher, more preferably 230° C. or higher, and even more preferably 235° C. or higher. On the other hand, from the viewpoint of further improving the color tone of the molded product by keeping the cylinder temperature low during extrusion blow molding, the melting point of the polyester is preferably 260° C. or lower.

[0040] The polyester is preferably produced by polycondensing an ester-forming monomer and a compound represented by the formula (I) above. As the ester-forming monomer, it is preferable to use both the above-mentioned dicarboxylic acid and diol, or to use the above-mentioned hydroxycarboxylic acid.

[0041] The method of polycondensing the ester-forming monomer and the compound represented by the formula (I) is not particularly limited, but when the above-mentioned dicarboxylic acid and diol are used as the ester-forming monomer, a method of melt-kneading the dicarboxylic acid, the diol, and the compound represented by the formula (I) to perform condensation polymerization is preferable. Specifically, the dicarboxylic acid, the diol, and the compound represented by the formula (I) are used as raw materials, and then the obtained polyester oligomer is melt-polycondensed after the esterification reaction or the ester exchange reaction is performed. The compound represented by the formula (I) may be added before the esterification reaction or the ester exchange reaction, or after the reaction. In addition, raw materials other than the compound represented by the formula (I) may be added before the esterification reaction or the ester exchange reaction, or after the reaction.

[0042] The above-mentioned esterification reaction or transesterification reaction is preferably carried out by charging the above-mentioned raw materials, polymerization catalyst, and, where necessary, additives such as the hindered phenol-based antioxidant into a reactor, under an absolute pressure of about 0.5 MPa or less or under normal pressure, at a temperature of 160 to 280°C, while distilling off the water or alcohol produced.

[0043] The melt polycondensation reaction following the esterification reaction or transesterification reaction is preferably carried out by adding the above-mentioned raw materials, polycondensation catalyst, and additives such as the hindered phenol-based antioxidant to the obtained polyester oligomer as necessary, and performing the reaction at a temperature of 260 to 290°C under a reduced pressure of 1 kPa or less until a polyester with a desired viscosity is obtained. If the reaction temperature of the melt polycondensation reaction is less than 260°C, the polymerization activity of the polymerization catalyst is low, and a polyester with a target polymerization degree may not be obtained. On the other hand, if the reaction temperature of the melt polymerization reaction is more than 290°C, the decomposition reaction is likely to proceed, and as a result, a polyester with a target polymerization degree may not be obtained. The melt polycondensation reaction can be carried out using, for example, a tank-type batch polycondensation apparatus or a continuous polycondensation apparatus consisting of a two-axis rotating horizontal reactor.

[0044] As the polymerization catalyst used in the condensation polymerization, any catalyst that can be used in the production of polyester can be selected, but compounds containing metal elements such as germanium, titanium, zirconium, hafnium, antimony, tin, magnesium, calcium, zinc, aluminum, cobalt, lead, cesium, manganese, lithium, potassium, sodium, copper, barium, and cadmium are suitable. Among them, compounds containing germanium, antimony, and titanium are preferred. As compounds containing antimony, antimony trioxide, antimony chloride, and antimony acetate are used, and as compounds containing germanium, germanium dioxide, germanium tetrachloride, and germanium tetraethoxide are used, and as compounds containing titanium, tetraisopropyl titanate, tetrabutyl titanate, and the like are used. In addition, composite particles of hydrotalcite and titanium dioxide can also be used as the polymerization catalyst. Among these, antimony trioxide and germanium dioxide are preferred from the viewpoints of polymerization catalyst activity, physical properties of the resulting polyester, and cost. When a polycondensation catalyst is used, the amount added is preferably within a range of 0.002 to 0.8% by mass based on the mass of the dicarboxylic acid component.

[0045] In the above condensation polymerization, an antioxidant other than the hindered phenol-based antioxidant, such as phosphorous acid or other phosphoric acid compounds or esters thereof, may be used as long as it does not impair the effects of the present invention. These may be used alone or in combination of two or more. Examples of phosphoric acid compounds include phosphorous acid, phosphorous acid esters, phosphoric acid, trimethyl phosphate, and triphenyl phosphate. The amount of the coloring inhibitor used is preferably within the range of 20 to 1000 ppm based on the total amount of the dicarboxylic acid component and the diester component. In addition, in order to suppress coloring due to thermal decomposition of the polyester, a cobalt compound such as cobalt acetate may be added, and the amount used is more preferably within the range of 20 to 1000 ppm based on the total amount of the dicarboxylic acid component and the diester component.

[0046] In the condensation polymerization, a dicarboxylate may be used to form the dicarboxylate unit. The alcohol portion of the dicarboxylate is not particularly limited, and examples thereof include monools such as methanol and ethanol; and polyols such as the diols that are structural units of the polyester.

[0047] In the condensation polymerization, a monoester or diester of a linear aliphatic diol may be used to form the diol unit. The carboxylic acid portion of the carboxylic acid ester is not particularly limited, and examples of the monocarboxylic acid include formic acid, acetic acid, and propionic acid.

[0048] The intrinsic viscosity of the polyester obtained by melt polycondensation is preferably 0.4 dl / g or more. This improves the handling property, and also improves the productivity since the polyester obtained by melt polycondensation can be further polymerized in a solid phase to have a high molecular weight in a short time. The intrinsic viscosity is more preferably 0.55 dl / g or more, and even more preferably 0.65 dl / g or more. On the other hand, in terms of being able to easily take out the polyester from the reactor and suppressing coloration due to thermal degradation, the intrinsic viscosity is preferably 0.9 dl / g or less, more preferably 0.85 dl / g or less, and even more preferably 0.8 dl / g or less.

[0049] The polyester thus obtained is suitably used as a raw material for extrusion molding, etc. It is also preferred that the polyester obtained by melt polycondensation is further subjected to solid-phase polymerization. The solid-phase polymerization is described below.

[0050] The polyester obtained as described above is extruded into a shape such as a strand or a sheet, cooled, and then cut with a strand cutter, a sheet cutter, or the like to produce intermediate pellets having a shape such as a cylinder, an elliptical cylinder, a disk, a die, etc. The cooling after the extrusion can be carried out by, for example, a water cooling method using a water tank, a method using a cooling drum, an air cooling method, or the like.

[0051] In order to further increase the degree of polymerization of the intermediate pellets thus obtained, solid-phase polymerization is carried out. It is preferable to heat the intermediate pellets before solid-phase polymerization to crystallize a part of the polyester. By doing so, it is possible to prevent the pellets from sticking together during solid-phase polymerization. The crystallization temperature is preferably 100 to 180°C. As a crystallization method, the intermediate pellets may be crystallized in a vacuum tumbler, or may be crystallized by heating in an air-circulating heating device. When heating in an air-circulating heating device, the internal temperature is preferably 100 to 160°C. When heating using an air-circulating heating device, the heat conduction is good compared to when crystallizing using a vacuum tumbler, so the time required for crystallization can be shortened, and the device is inexpensive. The time required for crystallization is not particularly limited, but is usually about 30 minutes to 24 hours. Prior to crystallization, the pellets may be dried at a temperature less than 100°C.

[0052] The temperature of the solid-state polymerization is preferably 170 to 250°C. If the temperature of the solid-state polymerization is less than 170°C, the time of the solid-state polymerization may be long, and the productivity may decrease. The temperature of the solid-state polymerization is more preferably 175°C or higher, and even more preferably 180°C or higher. On the other hand, if the temperature of the solid-state polymerization exceeds 250°C, the pellets may stick together. The temperature of the solid-state polymerization is more preferably 240°C or lower, and even more preferably 230°C or lower. The time of the solid-state polymerization is usually about 5 to 70 hours. In addition, the catalyst used in the melt polymerization may be present during the solid-state polymerization.

[0053] The solid-state polymerization is preferably carried out under reduced pressure or in an inert gas such as nitrogen gas. In order to prevent the pellets from sticking together, the solid-state polymerization is preferably carried out while moving the pellets by a suitable method such as a rolling method or a gas fluidized bed method. When the solid-state polymerization is carried out under reduced pressure, the pressure is preferably 1 kPa or less.

[0054] The polyester thus obtained by solid phase polymerization is suitably used as a raw material for extrusion molding, particularly extrusion blow molding.

[0055] As described above, the polyester obtained by carrying out melt polycondensation and further carrying out solid-phase polymerization may contain other additives within a range that does not impair the effects of the present invention, such as colorants such as dyes and pigments, stabilizers such as ultraviolet absorbers, antistatic agents, flame retardants, flame retardant assistants, lubricants, plasticizers, inorganic fillers, etc. The content of these additives in the polyester is preferably 10% by mass or less, more preferably 5% by mass or less.

[0056] The intrinsic viscosity of the polyester obtained by solid-phase polymerization is preferably 0.9 dl / g or more. This further improves the drawdown resistance when the polyester is extrusion blow molded. The intrinsic viscosity is more preferably 1.0 dl / g or more, and even more preferably 1.05 dl / g or more. On the other hand, the intrinsic viscosity is preferably 1.5 dl / g or less.

[0057] The method for producing the polylactic acid is not particularly limited, and a general method for producing polylactic acid can be adopted. Specifically, a one-step direct polymerization method can be adopted in which lactic acid and the compound represented by the above formula (I) are subjected to dehydration polycondensation in a solvent.

[0058] Examples of the catalyst include metals such as tin, zinc, lead, titanium, bismuth, zirconium, germanium, antimony, and aluminum, and derivatives thereof. Derivatives include metal alkoxides, carboxylates, carbonates, oxides, and halides. Specific examples include tin chloride, tin acetate, tin octoate, zinc chloride, lead oxide, lead carbonate, titanium chloride, alkoxytitanium, germanium oxide, and zirconium oxide. Among these, tin compounds are preferred, and tin acetate or tin octoate is more preferred.

[0059] The polymerization reaction can be carried out in the presence of the above catalyst, usually at a temperature of 100 to 200° C., although this varies depending on the type of catalyst. In order to remove water produced during the polymerization reaction, the polymerization reaction is desirably carried out under reduced pressure conditions, preferably 7 kPa or less, more preferably 1.5 kPa or less.

[0060] In addition, a compound having two or more hydroxyl groups or amino groups in the molecule may be used as a polymerization initiator during the polymerization reaction. Here, examples of the compound having two or more hydroxyl groups or amino groups in the molecule used as a polymerization initiator include polyhydric alcohols such as ethylene glycol, propylene glycol, butanediol, hexanediol, octanediol, neopentyl glycol, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, glycerin, trimethylolpropane, pentaerythritol, dipentaerythritol, tripentaerythritol, sorbitol, poly(vinyl alcohol), poly(hydroxyethyl methacrylate), and poly(hydroxypropyl methacrylate), and polyhydric amines such as ethylenediamine, propylenediamine, butanediamine, hexanediamine, diethylenetriamine, and melamine, and among these, polyhydric alcohols are more preferred.

[0061] The amount of the polymerization initiator added is not particularly limited, but is preferably 0.001 to 5 parts by mass, and more preferably 0.01 to 3 parts by mass, per 100 parts by mass of the raw materials (L-lactic acid, D-lactic acid) used.

[0062] The solvent to be used is not particularly limited as long as it does not affect the polymerization, and water or an organic solvent can be used. In the case of an organic solvent, for example, aromatic hydrocarbons can be mentioned. Examples of aromatic hydrocarbons include toluene, xylene, naphthalene, chlorobenzene, and diphenyl ether. In addition, the polymerization can be promoted by discharging water generated in the condensation reaction out of the system. As a method for discharging water out of the system, it is preferable to carry out the polymerization under reduced pressure conditions, specifically, 7 kPa or less, more preferably 1.5 kPa or less.

[0063] Various molded articles can be obtained by melt molding the polyester obtained. In the polyester of the present invention, the occurrence of gels and coloring is suppressed, so molded articles having excellent appearance can be obtained. The b value of the polyester (pellets) of the present invention is usually 0 to 20, and the lower the value, the less yellowish it is, and the more beautiful the appearance of the molded article obtained is, which is preferable. Therefore, the b value is preferably 10 or less, more preferably 5 or less, and particularly preferably 3 or less. The b value of the polyester of the present invention is measured by the method described in the examples.

[0064] The molding method is not particularly limited, but an extrusion molding method is preferably used. The polyester of the present invention has non-Newtonian properties suitable for extrusion molding and the like, and is therefore preferably used in such a molding method. A molded product obtained by extruding the polyester is a preferred embodiment of the present invention. A film or sheet obtained by extruding the polyester is a more preferred embodiment of the present invention. A container obtained by extruding the polyester is also a more preferred embodiment of the present invention. The polyester has non-Newtonian properties suitable for extrusion molding. The temperature of the resin composition during extrusion molding is preferably within the range of (melting point of polyester + 10°C) to (melting point of polyester + 70°C), and more preferably within the range of (melting point of polyester + 10°C) to (melting point of polyester + 40°C). By extruding at a temperature relatively close to the melting point, drawdown can be suppressed.

[0065] When the polyester is used to produce a sheet or film by extrusion molding such as the T-die method or the inflation method, a high-quality sheet or film can be produced with good productivity without drawdown, neck-in, film shaking, or gel generation. When the sheet or film thus obtained is used for secondary processing such as thermoforming, the desired molded product can be obtained with good shaping properties when forming a deep-draw molded product or a large molded product. Such a thermoformed product obtained by thermoforming a sheet or film, especially a container obtained by thermoforming the sheet or film, is also a preferred embodiment of the present invention.

[0066] Among the extrusion moldings, the polyester is particularly suitable for use in extrusion blow molding. The method of extrusion blow molding is not particularly limited, and can be carried out in the same manner as the conventionally known extrusion blow molding. For example, the polyester is melt-extruded to form a cylindrical parison, and while the parison is in a softened state, it is sandwiched between a blow mold and gas such as air is blown in to expand the parison into a predetermined hollow shape that conforms to the shape of the mold cavity. When the polyester is used, the extruded parison has good drawdown resistance, and hollow molded products can be produced with good productivity.

[0067] As the extrusion molding, profile extrusion molding is also preferred. The polyester is suitable for use in profile extrusion molding because gel formation and coloring are suppressed even when the melt tension is high. The profile extrusion molding method is not particularly limited, and can be performed in the same manner as the conventional profile extrusion molding method. For example, the polyester can be shaped by melt extruding it from a die of a predetermined shape. The polyester is suitable for use in profile extrusion molding because gel formation and coloring are suppressed even when the intrinsic viscosity and melt tension are high, and profile extrusion molded products having a predetermined cross-sectional shape can be produced with good productivity.

[0068] Molded articles obtained by extrusion blow molding the polyester and molded articles obtained by profile extrusion molding are also suitable embodiments of the present invention. The polyester of the present invention has non-Newtonian properties suitable for extrusion blow molding, and compared with other resins, gel formation and coloring are suppressed even though polycondensation is performed at high temperatures, so that molded articles with excellent appearance can be obtained. In addition, since the polyester suppresses gel formation and coloring even when the melt tension is high, molded articles obtained by profile extrusion molding the polyester also have excellent appearance. Moreover, the polyester of the present invention is safe. Therefore, these molded articles can be used for various applications. A container made of the extrusion blow molding is a suitable embodiment of the molded article. Such a container is suitably used as a container for filling soft drinks, seasonings, oils, cosmetics, detergents, and other products. A price rail made of the profile extrusion molding is a suitable embodiment of the molded article. In addition, a molded article having a laminated structure of the polyester and other thermoplastic resins can also be obtained.

[0069] Molded products obtained by extrusion molding of the polyester of the present invention can also be recycled. Specific examples of the recycled molded products include chips obtained by crushing the molded product, recycled polyesters containing the chips, recycled polyesters containing unadopted polyesters generated in the process of manufacturing the molded product, molded products obtained by extrusion molding (e.g., extrusion blow molding, profile extrusion molding) of these recycled polyesters, containers made of the molded products, films or sheets made of the molded products, and thermoformed products obtained by thermoforming the films or sheets. In addition, a manufacturing method of a molded product including a step of extrusion molding recycled polyesters containing chips obtained by crushing the molded product obtained by extrusion molding of the polyester of the present invention, and / or recycled polyesters containing unadopted polyesters generated in the process of manufacturing the molded product, can be mentioned as an embodiment of the recycled polyester. The manufacturing method may include a step of drying the recycled polyester before extrusion molding. The recycled polyester may contain virgin polyester. When virgin polyester is contained, the mixing method is not particularly limited, and a method using a tumbler mixer, a universal mixer, or the like that is generally used to mix resin and recycled material can be mentioned. EXAMPLES

[0070] The present invention will now be described in more detail with reference to examples.

[0071] (1) Intrinsic viscosity The intrinsic viscosities of the polyester pellets after melt polymerization and the polyester after solid-phase polymerization were measured at a temperature of 30° C. using an equal mass mixture of phenol and 1,1,2,2-tetrachloroethane as a solvent.

[0072] (2) Melting point Tm and glass transition temperature Tg The melting point Tm and glass transition temperature Tg of the polyester were measured using a differential scanning calorimeter (TA Instruments, TA Q2000). The melting point Tm and glass transition temperature Tg were calculated from the data obtained by heating the sample from 30°C to 280°C at a heating rate of 10°C / min, then quenching to 30°C at -50°C / min, and then heating it again at a heating rate of 10°C / min.

[0073] (3) Composition The ratio (mol%) of each monomer unit constituting the polyester is 1 The H-NMR spectrum was determined (apparatus: JNM-GX-500 manufactured by JEOL, solvent: deuterated trifluoroacetic acid).

[0074] (4) b value The b value of the resin pellets was measured using a Hunter Lab colorimeter "LabScan XE." The resin pellets were placed in a quartz cell, the container was filled while tapping the side, and the cell was covered with a black cup. The cell was then measured five times and the average value was calculated. The lower the b value (0-20), the less yellowish the color, and the more beautiful the appearance of the molded product obtained.

[0075] (5) Making the bottle Using an electric blow molding machine MSE-40E / 32M-A(T1) manufactured by Tahara Corporation, the obtained polyester was extrusion blow molded at a maximum cylinder temperature of 280°C, a die temperature of 250°C, a molding cycle of 15 seconds, a screw rotation speed of 22 rpm, an extrusion resin pressure of 26 MPa, and a mold temperature of 30°C to obtain a transparent bottle with a volume of 220 ml (27.5 g±0.5 g).

[0076] (6) Melt tension Using a Capillograph 1D manufactured by Toyo Seiki Seisakusho Co., Ltd., polyester was extruded in the form of a strand at a measurement temperature of 290°C, a capillary length of 10 mm, a capillary diameter of 1 mm, and a piston descending speed of 10 mm / min to measure the melt tension (mN). The melt tension was evaluated according to the following criteria. AA: More than 0.63mN A: More than 0.6mN and less than 0.63mN B: 0.6mN or less

[0077] (7) Sawing speed Using an electric blow molding machine MSE-40E / 32M-A(T1) manufactured by Tahara Corporation, polyester was extruded with a lip opening of 0.8 mm, and the time it took for the formed parison to reach 277 mm from the lip tip was measured to calculate the sagging speed (mm / s). AA: Less than 18.0 mm / s A: 18.0mm / s or more and less than 20.0mm / s B: 20.0mm / s or more and less than 25.0mm / s C:25.0mm / s or more

[0078] (8) Number of items Using a single-screw extruder D2020 manufactured by Toyo Seiki, a 100 μm sheet was produced at a maximum cylinder temperature of 280°C, a screw rotation speed of 65 rpm, a take-up speed of 1.6 m / min, and a take-up roll temperature of 70°C. Using a defect detector, the number of bumps with a diameter (equivalent circle diameter) of 50 μm or more where the boundary between the bumps and normal parts could be seen with a microscope with a 25x lens was counted at 0.5 m. 2 It was counted against. A: Less than 3,000 units B: More than 3,000 pieces

[0079] Example 1 A slurry containing 50.97 parts by mass of terephthalic acid, 22.86 parts by mass of ethylene glycol, and 2.16 parts by mass of cyclohexane-1,4-dimethanol [CHDM, a mixture ratio of cis and trans isomers (cis / trans isomers) of 30 / 70] was prepared, and polyoxyethylene (20) sorbitan monolaurate (a compound represented by formula (I), in which the sum of x, y, z, and w is 20, and R 2 ~R 4 is a hydrogen atom, and R 1 is C=O(CH2) 10The mixture was heated to 250°C under pressure (absolute pressure 0.25MPa) to carry out an esterification reaction to produce a low polymer. The low polymer was melt-polycondensed at 280°C under reduced pressure of 1hPa to obtain a polyester with an intrinsic viscosity of 0.76dl / g. The polyester obtained was extruded from a nozzle in the form of a strand, cooled with water, and then cut into a cylindrical shape (diameter about 2.5mm, length about 2.5mm) to obtain polyester pellets (melt-polycondensed pellets). The evaluation results of the obtained polyester pellets are shown in Table 2.

[0080] Example 2 Except for using 0.006 parts by mass of phosphorous acid and 0.006 parts by mass of pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] as antioxidants, polyester pellets (melt polycondensation pellets) were obtained in the same manner as in Example 1. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0081] Example 3 Polyester pellets (melt polycondensation pellets) were obtained in the same manner as in Example 2, except that a slurry consisting of 48.9 parts by mass of terephthalic acid, 19.63 parts by mass of ethylene glycol, and 7.42 parts by mass of cyclohexane-1,4-dimethanol [CHDM, a mixing ratio of cis isomer and trans isomer (cis isomer / trans isomer) of 30 / 70] was used. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0082] Example 4 Except for using a slurry consisting of 49.23 parts by mass of terephthalic acid, 24.19 parts by mass of ethylene glycol, and 2.59 parts by mass of isophthalic acid, polyester pellets (melt polycondensation pellets) were obtained in the same manner as in Example 2. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0083] Example 5 150 parts by mass of lactic acid was heated at 800 Pa, 160 ° C. for 3.5 hours in a reaction vessel equipped with a stirrer to obtain an oligomer. Then, 0.12 parts by mass of tin (II) acetate (Kanto Chemical Co., Ltd.), 0.33 parts by mass of methanesulfonic acid (Wako Pure Chemical Industries, Ltd.), and 0.199 parts by mass of polyoxyethylene (20) sorbitan monolaurate were added to the oligomer and heated at 500 Pa, 180 ° C. for 7 hours to obtain a prepolymer. Next, the prepolymer was heated in an oven at 120 ° C. for 2 hours to crystallize. The obtained prepolymer was crushed using a hammer crusher and sieved to obtain a powder with an average particle size of 0.1 mm. In the solid-phase polymerization, 150 parts by mass of the prepolymer was taken and introduced into an oven connected to an oil rotary pump, and subjected to a heating and decompression treatment. The pressure was 50 Pa, and the heating temperatures and heating times were 140° C.: 10 hours, 150° C.: 10 hours, and 160° C.: 20 hours. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0084] Comparative Example 1 Polyester pellets were obtained in the same manner as in Example 1, except that polyoxyethylene (20) sorbitan monolaurate was not added and the amount of the ingredients was changed as shown in Table 1. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0085] Comparative Example 2 Polyester pellets were obtained in the same manner as in Example 1, except that polyoxyethylene (20) sorbitan monolaurate was not added and the amount of the ingredients was changed as shown in Table 1. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0086] Comparative Example 3 Polyester pellets were obtained in the same manner as in Example 1, except that polyoxyethylene (20) sorbitan monolaurate was not added and the amount of the ingredients was changed as shown in Table 1. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0087] Comparative Example 4 Polyester pellets were obtained in the same manner as in Example 1, except that polyoxyethylene (20) sorbitan monolaurate was not added and the amount of the ingredients was changed as shown in Table 1. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0088] Example 6 The polyester pellets obtained in Example 1 were charged into a universal mixer and heated at 120° C. for 2 hours while stirring to obtain a pre-crystallized polyester.

[0089] The above pre-crystallized polyester was charged into a rotary vacuum solid-phase polymerization apparatus and subjected to solid-phase polymerization at 200° C. under 1 torr for 107 hours to obtain polyester pellets (solid-phase polymerized pellets). The evaluation results of the obtained polyester pellets are shown in Table 2.

[0090] Example 7 Polyester pellets (solid-phase polymerized pellets) were obtained in the same manner as in Example 6, except for using the polyester pellets obtained in Example 2. The evaluation results of the obtained solid-phase polymerized pellets are shown in Table 2.

[0091] Example 8 Polyester pellets (solid-phase polymerized pellets) were obtained in the same manner as in Example 6, except for using the polyester pellets obtained in Example 3. The evaluation results of the obtained solid-phase polymerized pellets are shown in Table 2.

[0092] Example 9 Polyester pellets (solid-phase polymerized pellets) were obtained in the same manner as in Example 6, except for using the polyester pellets obtained in Example 4. The evaluation results of the obtained solid-phase polymerized pellets are shown in Table 2.

[0093] Comparative Example 5 Polyester pellets (melt polycondensation pellets) were obtained in the same manner as in Example 1, except that a slurry consisting of 51.00 parts by mass of terephthalic acid, 22.89 parts by mass of ethylene glycol, and 2.16 parts by mass of cyclohexane-1,4-dimethanol [CHDM, a mixing ratio of cis isomer and trans isomer (cis isomer / trans isomer) of 30 / 70] was used, and 0.02 parts by mass of trimellitic anhydride was used as a crosslinking agent.

[0094] Except for using the obtained polyester pellets (melt polycondensation pellets), polyester pellets (solid-phase polymerization pellets) were obtained in the same manner as in Example 6. The evaluation results of the obtained solid-phase polymerization pellets are shown in Table 2.

[0095] Comparative Example 6 Polyester pellets (melt polycondensation pellets) were obtained in the same manner as in Example 1, except that a slurry consisting of 50.98 parts by mass of terephthalic acid, 22.87 parts by mass of ethylene glycol, and 2.16 parts by mass of cyclohexane-1,4-dimethanol [CHDM, a mixing ratio of cis isomer and trans isomer (cis isomer / trans isomer) of 30 / 70] was used, and 0.07 parts by mass of trimethylolpropane was used as a crosslinking agent.

[0096] Except for using the obtained polyester pellets (melt polycondensation pellets), polyester pellets (solid-phase polymerization pellets) were obtained in the same manner as in Example 6. The evaluation results of the obtained solid-phase polymerization pellets are shown in Table 2.

[0097] Example 10 Polyester pellets (melt polycondensation pellets) were obtained in the same manner as in Example 2, except that a slurry consisting of 50.50 parts by mass of terephthalic acid, 22.61 parts by mass of ethylene glycol, and 2.14 parts by mass of cyclohexane-1,4-dimethanol [CHDM, mixing ratio of cis isomer and trans isomer (cis isomer / trans isomer) is 30 / 70] was used and 0.817 parts by mass of a crosslinking agent was added. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0098] Comparative Example 7 Polyester pellets (melt polycondensation pellets) were obtained in the same manner as in Example 2, except that a slurry consisting of 50.01 parts by mass of terephthalic acid, 22.36 parts by mass of ethylene glycol, and 2.12 parts by mass of cyclohexane-1,4-dimethanol [CHDM, mixing ratio of cis isomer and trans isomer (cis isomer / trans isomer) was 30 / 70] was used and 1.565 parts by mass of a crosslinking agent was added. The intrinsic viscosity of the obtained polyester and the evaluation results of the polyester pellets are shown in Table 2.

[0099] [Table 1]

[0100] [Table 2]

[0101] Example 11 The polyester pellets (solid-phase polymerization pellets) obtained in Example 6 were used to obtain an extrusion blow molded bottle. The bottle was crushed using a DAS-28 crusher manufactured by Daiko Seiki Co., Ltd., and passed through a φ4 mm mesh, and then dried and crystallized at 120°C to obtain recovered chips. 20 parts by mass of the recovered chips and 80 parts by mass of the virgin polyester pellets (solid-phase polymerization pellets) obtained in Example 6 were placed in a PE bag and dry-blended using a tumbler to obtain recycled polyester pellets. The evaluation results of the moldability of the pellets are shown in Table 3.

[0102] Example 12 Recycled polyester pellets were produced and evaluated in the same manner as in Example 11, except that the amount of the recovered chips used was 40 parts by mass, and the amount of the virgin polyester pellets obtained in Example 6 used was 60 parts by mass. The evaluation results are shown in Table 3.

[0103] [Table 3]

Claims

1. A polyester containing 0.001 to 0.2 mol % of units derived from a compound represented by the following formula (I) based on all monomer units: 【Chemistry 1】 [In formula (I), the sum of x, y, z and w is 1 to 50, and R 1 ~R 4 each independently represents a hydrogen atom or an acyl group having 1 to 18 carbon atoms.

2. 2. The polyester according to claim 1, wherein the compound represented by formula (I) is at least one selected from the group consisting of polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monopalmitate, and polyoxyethylene sorbitan trioleate.

3. 2. The polyester according to claim 1, further comprising 0.0005 to 0.2 mol % of units derived from a hindered phenol-based antioxidant based on the total monomer units.

4. The polyester according to claim 1 , wherein the polyester is at least one selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene furanoate, and polylactic acid.

5. 2. The polyester according to claim 1, which is a polyethylene terephthalate containing 1.5 to 25 mol % of cyclohexanedimethanol units or isophthalic acid units based on the total monomer units.

6. 2. The polyester according to claim 1, having an intrinsic viscosity of 0.70 dl / g or more.

7. A molded article obtained by extrusion molding the polyester according to any one of claims 1 to 6.

8. 8. The molded article according to claim 7, which is obtained by extrusion blow molding the polyester.

9. 8. The molded article according to claim 7, which is obtained by profile extrusion of the polyester.

10. A film or sheet comprising the molded article according to claim 7.

11. A thermoformed article obtained by thermoforming the film or sheet according to claim 10.

12. A container comprising the molded article according to claim 7.

13. The method for producing the polyester according to any one of claims 1 to 6, comprising polycondensing an ester-forming monomer and the compound represented by formula (I).

Citation Information

Patent Citations

  • Copolymerized polyester, hollow vessel made thereof and its production