Positive electrode active material layer for solid-state battery and solid-state battery
By employing a positive electrode active material layer with a specific composition and particle size ratio of sulfide solid electrolytes, the structural changes in solid-state batteries are mitigated, resulting in reduced resistance increase during charging and discharging.
Patent Information
- Application Number
- JP2023045286
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Solid-state batteries using lithium composite oxides with a layered rock salt structure experience significant structural changes during charging and discharging, leading to high resistance increases due to expansion and contraction.
A positive electrode active material layer comprising a positive electrode active material with a composition of Li1-xM2O2, where M includes Ni, Co, or Al, and a specific ratio of two types of sulfide solid electrolytes with different particle sizes is used to mitigate structural changes, reducing resistance increase.
The proposed solution effectively reduces the resistance increase rate in solid-state batteries by using a positive electrode active material layer with a layered rock salt structure that expands and contracts during charging and discharging.
Smart Images

Figure 2024134864000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode active material layer for a solid-state battery and a solid-state battery. [Background technology]
[0002] In recent years, various developments have been made regarding solid-state batteries.
[0003] For example, Patent Document 1 discloses a positive electrode active material layer for an all-solid-state battery having a good specific capacitance. More specifically, the positive electrode active material layer of Patent Document 1 is a positive electrode active material layer used in an all-solid-state lithium ion battery, and the positive electrode active material layer contains a positive electrode active material and a solid electrolyte. The positive electrode active material is Li a Ni b Mn c O2 (0.90≦a≦1.15, 0.45≦b≦0.55, 0.45≦c≦0.55), the crystallite size determined from the peak of the (110) plane belonging to the space group R-3m in X-ray diffraction using Cu-Kα radiation is 380 Å or more and 530 Å or less, and the average primary particle size of the solid electrolyte is 2.0 μm or less. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-173993 A Summary of the Invention [Problem to be solved by the invention]
[0005] There is a demand for further reduction in resistance in solid-state batteries. However, lithium composite oxides having a layered rock-salt structure used as positive electrode active materials undergo large structural changes due to charging and discharging, which can lead to large expansion and contraction due to charging and discharging. In such cases, the resistance of the battery may increase after repeated charging and discharging.
[0006] An object of the present disclosure is to provide a positive electrode active material layer for a solid-state battery with a reduced rate of increase in resistance, and a solid-state battery using the same. [Means for solving the problem]
[0007] The present disclosure, which achieves the above objectives, includes the following aspects:
[0008] <Aspect 1> A positive electrode active material layer for a solid-state battery comprising a positive electrode active material, a first sulfide solid electrolyte, and a second sulfide solid electrolyte, The positive electrode active material has a composition Li 1-x It has a layered rock-salt structure of MO2 (wherein M contains at least one element selected from the group consisting of Ni, Co, Mn, and Al), and as a result of Rietveld analysis of the XRD profile, the change in lattice volume when x = 0.72 relative to the lattice volume when x = 0 is 3.0% or more, and a ratio of a particle size of the second sulfide solid electrolyte to a particle size of the first sulfide solid electrolyte (particle size of the second sulfide solid electrolyte / particle size of the first sulfide solid electrolyte) is 1 / 5 or less; Positive electrode active material layer for solid-state batteries. <Aspect 2> 2. The positive electrode active material layer for a solid battery according to aspect 1, wherein the ratio is 1 / 10 or less. <Aspect 3> A solid-state battery comprising the positive electrode active material layer for a solid-state battery according to aspect 1 or 2. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a positive electrode active material layer for a solid-state battery in which the rate of increase in resistance is reduced even when a positive electrode active material having a layered rock salt structure that expands and contracts greatly due to charging and discharging is used, and a solid-state battery using the same. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a graph showing the relationship between the amount of shrinkage due to charging in Reference Examples 1 and 2. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of a solid-state battery according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0012] 《Cathode active material layer for solid battery》 The positive electrode active material layer for a solid battery according to the present disclosure is A positive electrode active material layer for a solid-state battery comprising a positive electrode active material, a first sulfide solid electrolyte, and a second sulfide solid electrolyte, The positive electrode active material has the composition Li 1-x It has a layered rock-salt structure of MO2 (wherein M contains at least one element selected from the group consisting of Ni, Co, Mn, and Al), and as a result of Rietveld analysis of the XRD profile, the change in lattice volume when x = 0.72 relative to the lattice volume when x = 0 is 3.0% or more, and a ratio of a particle size of the second sulfide solid electrolyte to a particle size of the first sulfide solid electrolyte (particle size of the second sulfide solid electrolyte / particle size of the first sulfide solid electrolyte) is 1 / 5 or less; Cathode active material layer for solid-state batteries It is.
[0013] Through intensive research by the present inventors, it has been found that for the above-mentioned positive electrode active material having a layered rock salt structure, i.e., for a solid-state battery that undergoes a large degree of expansion and contraction due to charging and discharging, the resistance increase rate of the solid-state battery can be reduced by using two types of sulfide solid electrolytes that have a specific particle size ratio.
[0014] In the present disclosure, a "solid-state battery" refers to a battery that uses at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. Also, the solid-state battery of the present disclosure may be an all-solid-state battery, i.e., a battery that uses only a solid electrolyte as an electrolyte.
[0015] <Cathode active material> The positive electrode active material layer for a solid-state battery according to the present disclosure includes a positive electrode active material. 1-x It has a layered rock-salt structure, which is MO2 (wherein M includes at least one element selected from the group consisting of Ni, Co, Mn, and Al).
[0016] Here, the layered rock-salt structure refers to a layered crystal structure in which lithium ions and transition metal ions are arranged alternately, and the crystal structure can be confirmed, for example, by powder X-ray diffraction (XRD) measurement. The amount of change in the layered rock-salt structure due to charging and discharging can also be confirmed by Rietveld analysis of the measured XRD profile.
[0017] In the composition of the positive electrode active material according to the present disclosure, Li 1-x The "x" in MO2 represents the degree of extraction of lithium ions upon charging, and the layered rock-salt structure of the positive electrode active material shrinks and changes in accordance with the degree of extraction of lithium ions.
[0018] In this disclosure, the positive electrode active material (composition Li 1-x The Rietveld analysis of the XRD profile of the layered rock-salt structure of MO2 has the following characteristics: the lattice volume when x = 0 (a state in which no lithium ions have been extracted) is defined as "V0", and the lattice volume when x = 0.72 (a state in which some lithium ions have been extracted and the layered rock-salt structure has shrunk) is defined as "V 0.72 " Then, V for V0 0.72 The change (shrinkage) in is 3.0% or more. More specifically, the shrinkage may be, for example, 3.0% or more, 3.1% or more, 3.2% or more, 3.3% or more, 3.4% or more, 3.5% or more, or 3.6% or more. The upper limit of the shrinkage may be, for example, 10.0% or less, 9.0% or less, 8.0% or less, 7.0% or less, 6.0% or less, or 5.0% or less, from the viewpoint of maintaining the crystal structure.
[0019] In the present disclosure, the shape of the positive electrode active material is not particularly limited, but may be, for example, particulate. The average particle diameter (D50) of the primary particles of the positive electrode active material is, for example, 50 nm or more, may be 100 nm or more, or may be 300 nm or more. On the other hand, the average particle diameter (D50) of the primary particles of the positive electrode active material is, for example, 1 μm or less, may be 700 nm or less, or may be 500 nm or less. The average particle diameter (D50) of the positive electrode active material can be determined, for example, from the results of particle size distribution measurement by a laser diffraction scattering method.
[0020] In the present disclosure, specific examples of the positive electrode active material are not particularly limited, and include, for example, Li(Ni 0.50 Mn 0.50 )O2, Li(Ni 0.82 Co 0.15 Al 0.03 )O2, LiMn2O4, or Li(Ni 0.5 Mn 1.5 )O4, etc.
[0021] The surface of the positive electrode active material according to the present disclosure may be coated with a coating layer of an oxide having Li-ion conductivity. Examples of such oxides include Li3BO3, LiBO2, Li2CO3, LiAlO2, Li4SiO4, Li2SiO3, Li3PO4, Li2SO4, Li2TiO3, and Li4Ti5O 12 , Li2Ti2O5, Li2ZrO3, LiNbO3, Li2MoO4, Li2WO4, etc. Among them, lithium niobate (LiNbO3) is preferable. The thickness of the coating layer is not particularly limited, but can be, for example, 1 nm to 100 nm. The coating layer can be formed by coating the above oxide on the surface of the active material using a tumbling fluidization device.
[0022] In the positive electrode active material layer for a solid battery according to the present disclosure, the content of the positive electrode active material is not particularly limited, and may be, for example,
[0023] <Sulfide solid electrolyte> The positive electrode active material layer for a solid battery according to the present disclosure includes a first sulfide solid electrolyte and a second sulfide solid electrolyte. Here, the "first sulfide solid electrolyte" and the "second sulfide solid electrolyte" simply mean two types of sulfide solid electrolytes that are relatively different in particle size, and may be the same or different in constituent components.
[0024] In the present disclosure, the ratio of the particle size of the second sulfide solid electrolyte to the particle size of the first sulfide solid electrolyte (particle size of the second sulfide solid electrolyte / particle size of the first sulfide solid electrolyte) is 1 / 5 or less. More specifically, this ratio may be, for example, 1 / 5 or less, 1 / 8 or less, or 1 / 10 or less, and may be 1 / 50 or more, 1 / 30 or more, or 1 / 10 or more.
[0025] In addition, in the present disclosure, the specific value of the particle size of the first sulfide solid electrolyte is not particularly limited, and may be, for example, 0.5 μm or more, 0.6 μm or more, 0.7 μm or more, 0.8 μm or more, 0.9 μm or more, 1.0 μm or more, 1.1 μm or more, 1.2 μm or more, 1.3 μm or more, 1.4 μm or more, or 1.5 μm or more, and may be 2.5 μm or less, 2.0 μm or less, 1.9 μm or less, 1.8 μm or less, 1.7 μm or less, 1.6 μm or less, 1.5 μm or less, 1.4 μm or less, 1.3 μm or less, 1.2 μm or less, 1.1 μm or less, or 1.0 μm or less.
[0026] In addition, in the present disclosure, the specific value of the particle size of the second sulfide solid electrolyte is not particularly limited, and may be, for example, 0.01 μm or more, 0.05 μm or more, 0.1 μm or more, 0.2 μm or more, 0.3 μm or more, 0.4 μm or more, or 0.5 μm or more, and may be 0.5 μm or less, 0.4 μm or less, 0.3 μm or less, 0.2 μm or less, or 0.1 μm or less.
[0027] In the present disclosure, the particle size of the sulfide solid electrolyte is the median diameter (D50) calculated from the volume-based average particle size, where the average particle size is measured by a laser diffraction method using a MALVERN Mastersizer 200. More specifically, the measuring apparatus uses a Mastersizer 2000 manufactured by Malvern Instruments Ltd. 110 ml of dehydrated toluene (manufactured by Wako Pure Chemical Industries, Ltd., product name: special grade) is placed in the dispersion tank of the apparatus, and 6% of dehydrated tertiary butyl alcohol (manufactured by Wako Pure Chemical Industries, Ltd., special grade) is further added as a dispersant. After thoroughly mixing the above mixture, the first or second sulfide solid electrolyte is added to measure the particle size.
[0028] In the present disclosure, specific examples of the first and second sulfide solid electrolytes are not particularly limited, and each independently preferably contains sulfur (S) as a main component of the anion element, and more preferably contains, for example, Li element, A element, and S element. Here, the A element may be at least one selected from the group consisting of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In. Further, the sulfide solid electrolyte may further contain at least one of O and a halogen element. Examples of the halogen element (X) include F, Cl, Br, I, etc.
[0029] Also, in the present disclosure, the compositions of the first and second sulfide solid electrolytes are not particularly limited, and each independently includes, for example, xLi2S·(100 - x)P2S5 (70 ≤ x ≤ 80), yLiI·zLiBr·(100 - y - z)(xLi2S·(1 - x)P2S5) (0.7 ≤ x ≤ 0.8, 0 ≤ y ≤ 30, 0 ≤ z ≤ 30), etc. Further, the compositions of the first and second sulfide solid electrolytes may each independently have a composition represented by the following general formula (1): Li 4-x Ge 1-x P x S4(0 < x < 1) ··· Formula (1) In formula (1), at least a portion of Ge may be substituted with at least one selected from the group consisting of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. At least a portion of P may be substituted with at least one selected from the group consisting of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. At least a portion of Li may be substituted with at least one selected from the group consisting of Na, K, Mg, Ca, and Zn. At least a portion of S may be substituted with a halogen. The halogen is at least one of F, Cl, Br, and I.
[0030] <Content of positive electrode active material and sulfide solid electrolyte> In the positive electrode active material layer for a solid battery of the present disclosure, the total volume of the first and second sulfide solid electrolytes may be, for example, 10 vol.% or more, 15 vol.% or more, 20 vol.% or more, 22 vol.% or more, or 25 vol.% or more, and may be 60 vol.% or less, 50 vol.% or less, 40 vol.% or less, 38 vol.% or less, or 35 vol.% or less, relative to the total volume of the positive electrode active material and the first and second sulfide solid electrolytes.
[0031] In addition, in the positive electrode active material layer for a solid battery of the present disclosure, the content of the second sulfide solid electrolyte may be, for example, 5.0 mass% or more, 8.0 mass% or more, 10 mass% or more, or 15 mass% or more, and may be 20 mass% or less, 15 mass% or less, or 10 mass% or less, relative to the total content of the first and second sulfide solid electrolytes.
[0032] <Other Ingredients> The positive electrode active material layer for a solid battery according to the present disclosure may further contain other components in addition to the above-mentioned positive electrode active material and sulfide solid electrolyte.
[0033] Examples of other components include, but are not limited to, a conductive assistant, a binder, and other optional components.
[0034] More specifically, examples of the conductive assistant include, but are not limited to, carbon materials, metal materials, and conductive polymer materials.
[0035] Examples of binders include, but are not limited to, vinyl halide resins, rubbers, polyolefin resins, and the like.
[0036] Examples of other optional components include, but are not limited to, oxide solid electrolytes, halide solid electrolytes, thickeners, surfactants, dispersants, wetting agents, antifoaming agents, and solvents.
[0037] <Method for producing positive electrode active material layer> In the present disclosure, the method for producing the positive electrode active material layer is not particularly limited and may be a conventionally known method. For example, a method may be used in which a positive electrode active material, first and second sulfide solid electrolytes, and a dispersion medium such as heptane are mixed to prepare a slurry, and the prepared slurry is applied to a substrate and dried.
[0038] In the present disclosure, the thickness of the positive electrode active material layer is not particularly limited, and may be within the range of, for example, 0.1 μm to 1000 μm.
[0039] 《Solid-state battery》 The present disclosure can also provide a solid-state battery. The solid-state battery of the present disclosure has the above-mentioned positive electrode active material layer. The solid-state battery of the present disclosure may be a so-called solid-state lithium ion battery, and is preferably a sulfide solid-state lithium ion battery. The solid-state battery of the present disclosure may be a primary battery or a secondary battery, and is preferably a secondary battery. This is because the battery can be repeatedly charged and discharged, and is useful, for example, as an in-vehicle battery. Examples of the shape of the battery include a coin type, a laminate type, a cylindrical type, and a square type.
[0040] FIG. 2 is a schematic cross-sectional view showing an example of a solid-state battery according to the present disclosure.
[0041] As shown in FIG. 2, the solid state battery 1 has a positive electrode current collector layer 11, a positive electrode active material layer 12, a solid electrolyte layer 13, a negative electrode active material layer 14, and a negative electrode current collector layer 15 in this order.
[0042] Hereinafter, each of the components that may be included in the solid-state battery of the present disclosure will be described. Note that since the positive electrode active material layer is as described above, a description thereof will be omitted here.
[0043] <Positive electrode current collector layer> The positive electrode current collector layer collects the current from the positive electrode active material layer. Examples of the positive electrode current collector layer include stainless steel, aluminum, copper, nickel, iron, titanium, and carbon, and aluminum alloy foil or aluminum foil is preferable. The shape of the positive electrode current collector layer may be, for example, a foil shape or a mesh shape.
[0044] <Negative electrode current collector layer> The negative electrode current collector layer collects current from the negative electrode active material layer. Examples of the negative electrode current collector layer include stainless steel, aluminum, copper, nickel, iron, titanium, and carbon, and copper is preferred. The negative electrode current collector layer may be in the form of, for example, a foil or a mesh.
[0045] <Solid electrolyte layer> The solid electrolyte layer contains at least a solid electrolyte, and may further contain a binder, etc., as necessary. The above-mentioned sulfide solid electrolyte can be used as the solid electrolyte. The binder can be appropriately referred to as the "binder" that can be contained in the above-mentioned positive electrode active material layer, and therefore the description thereof will be omitted here.
[0046] The thickness of the solid electrolyte layer is not particularly limited, but may be, for example, 0.1 μm or more and 1000 μm or less.
[0047] <Negative electrode active material layer> The negative electrode active material layer contains at least a negative electrode active material, and may further contain at least one of a conductive assistant, a solid electrolyte, and a binder as necessary. The above-mentioned sulfide solid electrolyte can be used as the solid electrolyte. For other components such as the conductive assistant and the binder, the "other components" that may be contained in the above-mentioned positive electrode active material layer can be appropriately referred to, and therefore the description here is omitted.
[0048] The negative electrode active material is not particularly limited, and any negative electrode active material used in conventional solid-state lithium ion batteries can be used. Examples of the negative electrode active material include metal active materials and carbon active materials. Examples of the metal active material include In, Al, Si, Sn, etc. On the other hand, examples of the carbon active material include mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. In addition, lithium titanate (Li4Ti5O 12 The negative electrode active material may be in the form of, for example, a particle or a thin film. When the negative electrode active material is in the form of a particle, the negative electrode active material may be in the form of a primary particle or a secondary particle.
[0049] The thickness of the negative electrode active material layer is not particularly limited, but may be, for example, 0.1 μm or more and 1000 μm or less.
[0050] <<Method for manufacturing solid-state batteries>> In the present disclosure, the method for producing the solid-state battery is not particularly limited, and the solid-state battery can be produced by a conventionally known method. An example of the method for producing the solid-state battery of the present disclosure will be described below.
[0051] The method for producing a solid-state battery according to the present disclosure includes, for example, A step of preparing a positive electrode, a negative electrode, and a solid electrolyte layer (preparation step); a step of stacking a positive electrode, a solid electrolyte layer, and a negative electrode in this order (a stacking step); may have
[0052] Here, the positive electrode includes a positive electrode current collector layer and a positive electrode active material layer, and the negative electrode includes a negative electrode current collector layer and a negative electrode active material layer.
[0053] The method for producing the positive electrode, the negative electrode, and the solid electrolyte layer is not particularly limited, and it is preferable to produce them by kneading components that can be contained in the positive electrode active material layer, the negative electrode active material layer, and the solid electrolyte layer to obtain a slurry, applying the slurry to a substrate, and drying the resulting dried film, and pressing the resulting film.
[0054] Techniques for pressing the dried film include, but are not limited to, roll pressing, cold isostatic pressing (CIP), and the like.
[0055] The lamination step is a step of laminating a positive electrode, a solid electrolyte layer, and a negative electrode in this order. In the lamination step, the positive electrode, the solid electrolyte layer, and the negative electrode prepared in the preparation step are laminated in this order, and pressed as necessary to obtain a laminate (electrode body).
[0056] 《Charging and discharging method》 The present disclosure also provides a method for charging and discharging a solid-state battery. The method for charging and discharging a solid-state battery includes the steps of: The solid-state battery has a positive electrode active material layer including a positive electrode active material, a first sulfide solid electrolyte, and a second sulfide solid electrolyte, The change in lattice volume of the positive electrode active material due to charging and discharging is 3.0% or more, and a ratio of a particle size of the second sulfide solid electrolyte to a particle size of the first sulfide solid electrolyte (particle size of the second sulfide solid electrolyte / particle size of the first sulfide solid electrolyte) is 1 / 5 or less; method It is. EXAMPLES
[0057] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.
[0058] Examples 1 to 5 and Comparative Examples 1 to 4 <Common operation part> (Preparation of coated positive electrode active material) 53.7 g of the coating liquid was added to 50.0 g of the positive electrode active material to form a slurry, which was then spray-dried to coat the positive electrode active material. The coating liquid used was LiNbO3.
[0059] (Preparation of negative electrode) A sulfide solid electrolyte (Li2S-P2S5-based glass ceramics containing LiI, D50 = 0.8 μm), 1 mass% of vapor grown carbon fiber (VGCF) as a conductive additive, 2 mass% of butadiene rubber as a binder, and heptane were added to the kneading vessel of a Filmix device (30-L model manufactured by Primix) and stirred at 20,000 rpm for 30 minutes.
[0060] Next, the negative electrode active material (Li4Ti5O 12 The negative electrode mixture was prepared by mixing the mixture in a kneading vessel so that the volume ratio of the sulfide solid electrolyte was 7:3 and stirring at 15,000 rpm for 60 minutes with a Filmix device. The negative electrode mixture was applied to copper foil and dried at 100°C for 30 minutes. After that, the negative electrode mixture was applied to a copper foil of 1 cm 2 A negative electrode was obtained by punching out a piece of the material having a size of 10 mm.
[0061] (Preparation of solid electrolyte layer) Inner diameter cross-sectional area 1cm 2 64.8 mg of sulfide solid electrolyte (Li2S-P2S5 glass ceramics containing LiI, D50 = 2.5 μm) was placed in the cylindrical ceramic, smoothed, and then 1 ton / cm 2 The mixture was pressed with a pressure of 1000 V to form a solid electrolyte layer.
[0062] (Production of all-solid-state batteries) The above-prepared positive electrode was placed on one side of the solid electrolyte layer, and the above-prepared negative electrode was placed on the other side. 2 Then, stainless steel rods were inserted into both electrodes and restrained at 1 ton to obtain an all-solid-state lithium-ion battery.
[0063] <evaluation> (Battery characteristics - Evaluation of resistance increase rate) For each solid-state lithium-ion battery, constant current-constant voltage charging and discharging were performed at 1 / 3C rate for 2 cycles so that the initial charge specific capacity was the specific capacity in Table 1, and then the SOC was adjusted to 50% at 1 / 3C rate. The AC impedance was measured at 10mV and 0.1-106Hz, and an arc was fitted to the Cole-Cole plot. The distance between the two intersection points of the fitted arc and the real axis was taken as the interface resistance. Next, a cycle test was performed at 60°C, 1C, SOC 0-100%, and 100 cycles. After the cycle test, the interface resistance was measured again by AC impedance, and the resistance increase rate before and after the cycle test was evaluated. The results obtained are shown in Table 1.
[0064] (Measurement of shrinkage of positive electrode active material) The amount of shrinkage of each positive electrode active material was obtained by measuring the positive electrode active material layer charged in a coin cell of a liquid battery with an X-ray diffraction device (SmartLab, manufactured by Rigaku Corporation) and subjecting the obtained profile to Rietveld analysis using Fullprof.
[0065] The positive electrode active material layer was charged as follows: In other words, in a coin cell CR2032 specification, the positive electrode active material shown in Table 1 and metallic lithium as the negative electrode active material layer were used to charge the battery to the specific capacity shown in Table 1, and then the coin cell was disassembled and the positive electrode active material layer was washed and dried with EMC to obtain a positive electrode active material layer in a charged state.
[0066] Comparative Example 1 Coated positive electrode active material Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3)O2 and a first sulfide solid electrolyte (Li2S-P2S5-based glass ceramics containing LiI, D50 = 1.0 μm) were weighed out to a volume ratio of 7:3, and these were put into tetralin together with 3 mass% of vapor grown carbon fiber (VGCF) as a conductive additive and 0.7 mass% of butadiene rubber as a binder. Next, these were mixed to prepare a positive electrode mixture. The prepared positive electrode mixture was thoroughly dispersed using an ultrasonic homogenizer (UH-50 manufactured by SMT), then coated on aluminum foil and dried at 100°C for 30 minutes. After that, 1 cm 2 A positive electrode was obtained by punching out a piece of the material having a size of 10 mm.
[0067] Then, using this positive electrode, an all-solid-state battery of Comparative Example 1 was produced according to the common procedure described above.
[0068] Comparative Example 2 A positive electrode was obtained in the same manner as in Comparative Example 1, except that a second sulfide solid electrolyte (Li2S-P2S5-based glass ceramics containing LiI, D50=0.1 μm) was added to the total amount of the solid electrolyte to be 10 mass %. Then, the all-solid-state battery of Comparative Example 2 was produced.
[0069] Comparative Example 3 Coated positive electrode active material Li(Ni 0.5 Mn 0.5 An all-solid-state battery of Comparative Example 3 was produced in the same manner as in Comparative Example 1, except that 02 was used and the specific capacity was set to 202 mAh / g.
[0070] Examples 1 to 3 The all-solid-state batteries of Examples 1 to 3 were each produced in the same manner as in Comparative Example 3, except that the second sulfide solid electrolyte (Li2S-P2S5-based glass ceramics containing LiI, D50=0.1 μm) was added in amounts of 5 mass %, 10 mass %, and 20 mass %, respectively, relative to the total mass of the solid electrolyte.
[0071] Example 4 An all-solid-state battery of Example 4 was produced in the same manner as in Comparative Example 3, except that a second sulfide solid electrolyte (Li2S-P2S5-based glass ceramics containing LiI, D50 = 0.2 μm) was added to the entire solid electrolyte in an amount of 10 mass %.
[0072] Comparative Example 4 Coated positive electrode active material Li(Ni 0.82 Co 0.15 Al 0.03 An all-solid-state battery of Comparative Example 4 was produced in the same manner as in Comparative Example 1, except that 02 was used and the specific capacity was set to 201 mAh / g.
[0073] Example 5 An all-solid-state battery of Example 5 was produced in the same manner as in Comparative Example 4, except that a second sulfide solid electrolyte (Li2S-P2S5-based glass ceramics containing LiI, D50 = 0.1 μm) was added to the entire solid electrolyte in an amount of 10 mass %.
[0074] [Table 1]
[0075] As is clear from Table 1, it was found that all of the Examples had a resistance increase suppression effect compared to the Comparative Example (Comparative Example) in which the positive electrode active material had the same composition but no second sulfide solid electrolyte was added.
[0076] Reference Examples 1 and 2 In Reference Examples 1 and 2, the positive electrode active material was Li 1-x (Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2, and Li 1-x (Ni 0.5 Mn 0.5 The relationship between the amount of shrinkage due to charging and the amount of shrinkage when O2 was used was investigated. In Reference Examples 1 and 2, the same first sulfide solid electrolyte as in Comparative Example 1 was added to the positive electrode active material layer. The results are shown in FIG.
[0077] As is clear from the results of FIG. 1, in Reference Examples 1 and 2, when lithium ions were similarly extracted up to x=0.72, the positive electrode active material was 1-x (Ni 0.5 Mn 0.5 The amount of volumetric shrinkage was larger when O2 was used. [Explanation of symbols]
[0078] 1 solid state battery 11 Positive electrode current collector layer 12 Cathode active material layer 13 Solid electrolyte layer 14 Negative electrode active material layer 15 Negative electrode current collector layer
Claims
1. A positive electrode active material layer for a solid-state battery comprising a positive electrode active material, a first sulfide solid electrolyte, and a second sulfide solid electrolyte, The positive electrode active material has a composition Li 1-x M.O. 2 (wherein M contains at least one element selected from the group consisting of Ni, Co, Mn, and Al), and as a result of Rietveld analysis of the XRD profile, the amount of change in lattice volume when x = 0.72 relative to the lattice volume when x = 0 is 3.0% or more; and A ratio of a particle size of the second sulfide solid electrolyte to a particle size of the first sulfide solid electrolyte (particle size of the second sulfide solid electrolyte / particle size of the first sulfide solid electrolyte) is 1 / 5 or less; Positive electrode active material layer for solid-state batteries.
2. The positive electrode active material layer for a solid battery according to claim 1 , wherein the ratio is 1 / 10 or less.
3. A solid-state battery comprising the positive electrode active material layer for a solid-state battery according to claim 1 or 2.
Citation Information
Patent Citations
Positive electrode active material layer
JP2020173993A