Emulsion composition and coating agent

By controlling the minimum film forming temperature and incorporating specific resins, the emulsion composition addresses issues of tensile strength and oil resistance, enhancing its stability and performance in film formation.

JP2024134869AInactive Publication Date: 2024-10-04MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023045293
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional emulsion compositions containing aliphatic polyester resins suffer from insufficient tensile strength and oil resistance after film formation, limiting their applications, and there is a lack of progress in improving sedimentation stability.

Method used

The emulsion composition includes an aliphatic polyester resin with specific aliphatic polyhydric alcohol and aliphatic polycarboxylic acid units, controlled to a minimum film forming temperature (MFT) of 75°C or less, along with a polyvinyl alcohol resin and a plasticizer, to enhance sedimentation stability, tensile strength, and oil resistance.

Benefits of technology

The composition achieves excellent sedimentation stability, tensile strength, and oil resistance, making it suitable for various applications including coatings and adhesives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134869000001
    Figure 2024134869000001
Patent Text Reader

Abstract

To provide an emulsion composition which is excellent in sedimentation stability, and is also excellent in tensile strength and oil resistance after film formation.SOLUTION: An emulsion composition contains an aliphatic polyester-based resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polyvalent carboxylic acid unit as main constitutional units, wherein a lowest film forming temperature of the emulsion composition is 75°C or lower.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an emulsion composition containing a biodegradable resin, and more particularly to an emulsion composition and a coating agent containing an aliphatic polyester resin. [Background technology]

[0002] In recent years, research and development of various biodegradable resins has been progressing against the background of demands for reducing the environmental burden. In particular, from the viewpoint of promoting the elimination of organic solvents, a resin composition for emulsion containing a biodegradable resin has attracted attention.

[0003] For example, as a resin composition for emulsion having excellent biodegradability, an emulsion composition has been proposed in which an aliphatic polyester resin such as polylactic acid or polybutylene succinate is emulsified using a dispersant such as polyvinyl alcohol, and it is expected that this composition will be used in various applications such as adhesives, paints, and coating agents (e.g., Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-204038 A [Patent Document 2] JP 2004-238579 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, conventional emulsion compositions containing aliphatic polyester resins may have insufficient tensile strength and oil resistance after film formation, and their applications may be limited, so further improvement is required. Furthermore, research and development into emulsion compositions that have improved tensile strength and oil resistance while also having excellent sedimentation stability, which is one of the important required properties, has not yet progressed sufficiently. [Means for solving the problem]

[0006] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide an emulsion composition and the like which is excellent in sedimentation stability and also in tensile strength and oil resistance after film formation.

[0007] Means for Solving the Problems The present inventors have conducted extensive research in light of the above circumstances and have found that by using a specific aliphatic polyester resin and controlling the minimum film formation temperature (MFT) of the emulsion composition within a specific range, it is possible to provide an emulsion composition and the like which has excellent sedimentation stability and also has excellent tensile strength and oil resistance after film formation, and have completed the present invention.

[0008] The present invention provides the following [1] to

[16] . [1] An emulsion composition comprising an emulsion resin composition containing an aliphatic polyester resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polycarboxylic acid unit as main constituent units, wherein the emulsion composition has a minimum film-forming temperature of 75°C or lower. [2] The emulsion composition according to [1], further comprising a polyvinyl alcohol-based resin (B1). [3] The emulsion composition according to [2], wherein a mass ratio (B1 / A) of the polyvinyl alcohol-based resin (B1) to the aliphatic polyester-based resin (A) is 0.1 or less. [4] The emulsion composition according to [2] or [3], wherein a mass ratio of the polyvinyl alcohol-based resin (B1) to the solid content (B1 / solid content) is 0.15 or less. [5] The emulsion composition according to any one of [1] to [4], further comprising a plasticizer (C), wherein a mass ratio (C / A) of the plasticizer (C) to the aliphatic polyester resin (A) is 0.002 to 0.5. [6] The emulsion composition according to any one of [1] to [5], wherein the dispersed particle size is 10 μm or less. [7] A coating agent comprising the emulsion composition according to any one of [1] to [6]. [8] The coating agent according to [7], wherein the substrate to be coated is a paper substrate. [9] The coating agent according to [7], wherein the object to be coated is a plastic substrate.

[10] A molded article obtained by using the emulsion composition according to any one of [1] to [6].

[11] A film obtained by using the emulsion composition according to any one of [1] to [6].

[12] A cosmetic preparation comprising the emulsion composition according to any one of [1] to [6].

[13] An agricultural composition comprising the emulsion composition according to any one of [1] to [6].

[14] A paint comprising the emulsion composition according to any one of [1] to [6].

[15] An ink containing the emulsion composition according to any one of [1] to [6].

[16] A pressure-sensitive adhesive comprising the emulsion composition according to any one of [1] to [6]. Effect of the Invention

[0009] According to the present invention, it is possible to provide an emulsion composition and the like which is excellent in sedimentation stability and also in tensile strength and oil resistance after film formation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in more detail below based on the embodiments of the present invention, but the present invention is not limited to these embodiments.

[0011] In this specification, when expressed as "X to Y" (X and Y are arbitrary numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "it is preferably greater than X" or "it is preferably less than Y". Furthermore, "X and / or Y (X and Y are optional)" means at least one of X and Y, and means the following three cases: X only, Y only, and X and Y.

[0012] An emulsion composition according to an embodiment of the present invention (hereinafter, sometimes referred to as "the emulsion composition") is an emulsion composition containing a resin composition for emulsions, the resin composition for emulsions being a resin composition for emulsions containing an aliphatic polyester resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polycarboxylic acid unit as main constituent units (hereinafter, sometimes referred to as "the emulsion resin composition"), characterized in that the minimum film-forming temperature (MFT) of the emulsion composition is 75° C. or less. By setting the minimum film-forming temperature (MFT) within the above range, it is possible to provide an emulsion composition that is excellent in sedimentation stability and also excellent in tensile strength and oil resistance after film formation.

[0013] As an example of an embodiment of the present emulsion composition, for example, an emulsion composition containing a resin composition for emulsions containing the component (A), a dispersant (B) such as a polyvinyl alcohol-based resin (B1), and a dispersion medium (D) such as water is suitable. As an example of an embodiment of the emulsion composition of the present invention, for example, an emulsion composition containing an aqueous emulsion resin composition containing component (A), a dispersant (B) such as a polyvinyl alcohol-based resin, a plasticizer (C), and a dispersion medium (D) such as water is suitable. The present emulsion composition is obtained by using the present emulsion resin composition, specifically, by a known production method such as a phase inversion emulsification method using the present emulsion resin composition. The present resin composition for emulsion and the present emulsion composition will be described in detail below.

[0014] It is important that the present emulsion composition uses component (A) and that the minimum film-forming temperature (MFT) of the emulsion composition is 75° C. or lower. By setting the minimum film-forming temperature (MFT) in the above range, it is possible to provide an emulsion composition etc. that is excellent in sedimentation stability and also in tensile strength and oil resistance after film formation. If the minimum film-forming temperature (MFT) exceeds the above range, the sedimentation stability tends to decrease and the tensile strength after film formation tends to decrease.

[0015] The minimum film-forming temperature (MFT) of the present emulsion composition is preferably 72°C or lower, more preferably 5 to 70°C, and even more preferably 5 to 40°C, from the viewpoint of achieving both the above-mentioned sedimentation stability and the above-mentioned tensile strength.

[0016] Methods for adjusting the minimum film formation temperature (MFT) of the present emulsion composition within the above range include, but are not limited to, methods for adjusting the types of component (A), component (C), etc., the melt flow rates of component (A), component (C), etc., and the content ratios of component (A), component (B) and component (C). The minimum film-forming temperature (MFT) of the present emulsion composition can be measured in accordance with JIS K6828 5.11.

[0017] [Component (A)] The component (A) is, for example, an aliphatic polyester resin having, as main constituent units, an aliphatic polyhydric alcohol unit represented by the following formula (1) and an aliphatic polycarboxylic acid unit represented by the following formula (2).

[0018] -OR 11 -O- (1) [In formula (1), R11 represents a divalent chain aliphatic hydrocarbon group, and when copolymerized, the number of types is not limited to one.

[0019] -OC-R 21 -CO- (2) [In formula (2), R 21 represents a divalent chain aliphatic hydrocarbon group, and when copolymerized, the number of types is not limited to one.

[0020] The term "unit" means a structural unit contained in the aliphatic polyester resin derived from a monomer component used in the production of the aliphatic polyester resin, and the term "main structural unit" means that the structural unit derived from the target monomer component is contained in the total structural units of the component (A) at 50 mol% or more. The content of the structural unit derived from the target monomer is preferably 60 mol% or more, more preferably 70 mol% or more, and even more preferably 80 to 100 mol%. For example, it is preferable that the aliphatic polyester resin is produced by polymerizing a raw material containing an aliphatic polyhydric alcohol and an aliphatic polycarboxylic acid component at 50 mol% or more, preferably 60 mol% or more, more preferably 70 mol% or more, and even more preferably 80 to 100 mol% of the total monomer components used in the polymerization reaction of the aliphatic polyester resin.

[0021] The aliphatic polyhydric alcohol that gives the polyhydric alcohol unit of formula (1) is not particularly limited, but for example, an aliphatic polyhydric alcohol having 2 to 10 carbon atoms is preferable, and an aliphatic polyhydric alcohol having 4 to 6 carbon atoms is more preferable. Specific examples include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, neopentyl glycol, diethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc. Among them, 1,4-butanediol is preferable. The aliphatic polyhydric alcohol may be used alone or in combination of two or more kinds.

[0022] The aliphatic polycarboxylic acid component that gives the aliphatic polycarboxylic acid unit of formula (2) is an aliphatic polycarboxylic acid or an aliphatic polycarboxylic acid derivative such as an alkyl ester thereof, and the aliphatic polycarboxylic acid is not particularly limited, but is preferably an aliphatic polycarboxylic acid having 2 to 40 carbon atoms, more preferably an aliphatic polycarboxylic acid having 4 to 10 carbon atoms. Specific examples include succinic acid, adipic acid, suberic acid, sebacic acid, and dodecanedioic acid. Among them, succinic acid, adipic acid, and sebacic acid are preferred, and succinic acid and adipic acid are more preferred. The aliphatic polycarboxylic acid components may be used alone or in combination of two or more.

[0023] Specific examples of the (A) component include, for example, an aliphatic polyester resin containing 1,4-butanediol and succinic acid, and an aliphatic polyester resin containing 1,4-butanediol, adipic acid, and succinic acid. More specifically, from the viewpoint of significantly achieving the effects of the present invention, suitable examples include polybutylene succinate and polybutylene succinate adipate. Among these, polybutylene succinate adipate is preferred.

[0024] When the aliphatic polycarboxylic acid is succinic acid, the proportion of constituent units derived from succinic acid in all polycarboxylic acid units of the aliphatic polyester resin is usually 50 to 100 mol %, preferably 80 to 100 mol %, and more preferably 90 to 100 mol %.

[0025] Furthermore, when the aliphatic polycarboxylic acid is succinic acid and adipic acid, the proportion of the succinic acid-derived constituent units in all polycarboxylic acid units of the aliphatic polyester resin is usually 50 to 95 mol%, preferably 60 to 93 mol%, and more preferably 70 to 90 mol%, and the proportion of the adipic acid-derived constituent units in all polycarboxylic acid units is usually 5 to 50 mol%, preferably 7 to 40 mol%, and more preferably 10 to 30 mol%.

[0026] The component (A) preferably has the following physical properties:

[0027] The weight average molecular weight (Mw) of the component (A) is preferably 10,000 or more, more preferably 20,000 or more, and even more preferably 50,000 or more, and is preferably 1,000,000 or less, more preferably 500,000 or less, and even more preferably 400,000 or less. The weight average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0028] The melt flow rate (MFR) of component (A), when measured at 190°C and 2.16 kg, is usually 0.1 g / 10 min or more, preferably 0.5 g / 10 min or more, more preferably 1 g / 10 min or more, and usually 1,000 g / 10 min or less, preferably 500 g / 10 min or less, more preferably 100 g / 10 min or less, even more preferably 50 g / 10 min or less, and particularly preferably 30 g / 10 min or less.

[0029] The melting point of component (A) is preferably 70° C. or higher, more preferably 75° C. or higher, and is preferably 250° C. or lower, more preferably 200° C. or lower, and particularly preferably 150° C. or lower. When there are multiple melting points, it is preferable that at least one of the melting points is within the above range.

[0030] In the present emulsion composition, the component (A) may be used alone or in combination of two or more kinds. For example, two or more kinds of aliphatic polyester resins having different polyhydric alcohol units or polyvalent carboxylic acid units may be mixed and used.

[0031] The content of the component (A) is not particularly limited, but is preferably 15% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the total amount of the emulsion composition, and is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 60% by mass or less.

[0032] [(B) Dispersant] The dispersant (B) that can be used in the present emulsion resin composition can be any commonly used known dispersant. For example, water-soluble polymers, various surfactants, etc. can be mentioned. These can be used alone or in combination of two or more kinds.

[0033] Examples of water-soluble polymers include, but are not limited to, polyvinyl alcohol resins (hereinafter referred to as "PVA resins"), cellulose derivatives such as methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxybutyl methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, aminomethyl hydroxypropyl cellulose, and aminoethyl hydroxypropyl cellulose, starch, tragacanth, pectin, glue, alginic acid or a salt thereof, gelatin, polyvinylpyrrolidone, polyacrylic acid or a salt thereof, polymethacrylic acid or a salt thereof, polyacrylamide, polymethacrylamide, copolymers of vinyl acetate and unsaturated acids such as maleic acid, maleic anhydride, acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and crotonic acid, copolymers of styrene and the above unsaturated acids, copolymers of vinyl ethers and the above unsaturated acids, and salts of the above copolymers. Examples of the surfactant include nonionic surfactants, cationic surfactants, anionic surfactants, etc. Specific examples include, but are not limited to, polyoxyethylene nonylphenyl ether, polyoxyethylene octylnonyl ether, polyoxyethylene dodecylphenyl ether, polyoxyethylene alkyl allyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monooleate, polyoxyalkylene alkyl ether phosphate monoethanolamine salt, polyoxyethylene lauryl amino ether, polyoxyethylene stearyl amino ether, and other polyoxyethylene alkyl amino ethers. Among these, the PVA-based resin (B1) is preferably used from the viewpoint of achieving the remarkable effects of the present invention.

[0034] [PVA resin (B1)] The PVA resin (B1) that can be used in the present resin composition for emulsion includes unmodified PVA resins and modified PVA resins.

[0035] The unmodified PVA resin can be produced by saponifying a vinyl ester polymer obtained by polymerizing a vinyl ester compound.

[0036] Examples of such vinyl ester compounds include vinyl formate, vinyl acetate, vinyl trifluoroacetate, vinyl propionate, vinyl butyrate, vinyl caprate, vinyl laurate, vinyl versatate, vinyl palmitate, vinyl stearate, etc., with vinyl acetate being preferred. The vinyl ester compounds may be used alone or in combination of two or more.

[0037] The modified PVA resin can be produced by copolymerizing the vinyl ester compound with an unsaturated monomer copolymerizable with the vinyl ester compound, followed by saponification.

[0038] Examples of the unsaturated monomer copolymerizable with the vinyl ester compound include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, α-octadecene, etc., hydroxyl group-containing α-olefins such as 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, etc., and derivatives such as acylated products thereof; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, undecylenic acid, etc., salts thereof, monoesters, or dialkyl esters thereof; amides such as diacetone acrylamide, acrylamide, methacrylamide, etc.; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, etc., or salts thereof. These can be used alone or in combination of two or more kinds.

[0039] The modified PVA resin may have a primary hydroxyl group in the side chain, for example, a number of primary hydroxyl groups in the side chain is usually 1 to 5, preferably 1 to 2, and particularly preferably 1. Furthermore, the modified PVA resin may preferably have a secondary hydroxyl group in addition to the primary hydroxyl group. Examples of such modified PVA resins include PVA resins having a hydroxyalkyl group in the side chain, PVA resins having a 1,2-diol structural unit in the side chain, and the like.

[0040] The average saponification degree of the PVA resin (B1) is preferably 70 mol% or more, more preferably 75 to 99 mol%, even more preferably 78 to 95 mol%, and particularly preferably 82 to 90 mol%. If the average saponification degree is too low, the water resistance of the film obtained by using the resin composition for emulsion tends to decrease.

[0041] In particular, when an unmodified PVA resin is used as the PVA resin (B1), the average saponification degree is preferably 75 mol% or more, more preferably 78 to 95 mol%, and even more preferably 82 to 90 mol%. If the average saponification degree is too low, the water resistance of the film obtained by using the resin composition for emulsion tends to decrease.

[0042] When a modified PVA resin is used as the PVA resin (B1), the average saponification degree is preferably 72 mol% or more, more preferably 75 to 99 mol%, and even more preferably 80 to 95 mol%. If the average saponification degree is too low, the water resistance of the film obtained by using the resin composition for emulsion tends to decrease.

[0043] The average degree of saponification is measured in accordance with JIS K 6726 3.5.

[0044] The viscosity of a 4% by mass aqueous solution of the PVA resin (B1) at 20° C. is preferably 10 to 70 mPa s, more preferably 13 to 45 mPa s, and even more preferably 17 to 40 mPa s. If the viscosity is too low, the stability of the emulsion composition tends to decrease.

[0045] When an unmodified PVA resin is used as the PVA resin (B1), the viscosity of a 4 mass% aqueous solution of the unmodified PVA resin at 20° C. is preferably 5 to 50 mPa s, more preferably 13 to 45 mPa s, and even more preferably 17 to 40 mPa s. If the viscosity is too low, the stability of the emulsion composition tends to decrease.

[0046] When a modified PVA resin is used as the PVA resin (B1), the viscosity of a 4% by mass aqueous solution of the modified PVA resin at 20° C. is preferably 5 to 50 mPa s, more preferably 13 to 40 mPa s, and even more preferably 17 to 30 mPa s. If the viscosity is too low, the stability of the emulsion composition tends to decrease.

[0047] The viscosity of the 4 mass % aqueous solution is measured in accordance with JIS K 6726 3.11.2.

[0048] The average degree of polymerization of the PVA resin (B1) is preferably from 50 to 5,000, more preferably from 150 to 4,000, and even more preferably from 300 to 3,000. The average degree of polymerization can be determined according to the method for calculating the average degree of polymerization described in JIS K 6726.

[0049] In the present resin composition for emulsion, the PVA-based resins (B1) can be used alone, or unmodified PVA-based resins can be used in combination, modified PVA-based resins can be used in combination, or an unmodified PVA resin can be used in combination with a modified PVA-based resin. Furthermore, two or more types of PVA-based resins having different average saponification degrees, viscosities, modified species, modification amounts, etc. can also be used in combination.

[0050] The mass ratio (B / A) of the (B) component to the (A) component is not particularly limited, but from the viewpoint of significantly exhibiting the effects of the present invention, it is, for example, 0.002 to 0.4, preferably 0.01 to 0.3, more preferably 0.02 to 0.24, and even more preferably 0.03 to 0.2. It is particularly preferably 0.1 or less, and particularly preferably 0.035 to 0.1, 0.035 to 0.09, or 0.035 to 0.08. The mass ratio (B1 / A) is also preferably in the same range as above.

[0051] The content of the (B) component is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and particularly preferably 3% by mass or more, based on the total amount of the emulsion composition. Also, it is preferably 20% by mass or less, more preferably 15% by mass or less, even more preferably 12% by mass or less, and particularly preferably 10% by mass or less. Outside this range, the stability of the emulsion composition tends to decrease.

[0052] [(C) Plasticizer] The plasticizer (C) that can be used in the present emulsion resin composition includes, for example, plasticizers having an ester bond in the molecule. For example, aliphatic dibasic acid ester plasticizers such as adipate ester plasticizers, sebacate ester plasticizers, and azelaate ester plasticizers, phthalate ester plasticizers, phosphate ester plasticizers, citrate ester plasticizers, glycolate ester plasticizers, trimellitate ester plasticizers, ricinoleate ester plasticizers, benzoate ester plasticizers, and acetate ester plasticizers can be used alone or in combination of two or more.

[0053] Examples of the adipate plasticizer include dimethyl adipate, dibutyl adipate, dioctyl adipate, isobutyl adipate, isodecyl adipate, diisononyl adipate, divinyl adipate, dibenzyl adipate, and mixed esters of adipic acid with aromatic alcohols and aliphatic alcohols.

[0054] Examples of mixed esters of adipic acid with aromatic alcohols and aliphatic alcohols include benzyl alkyl diglycol adipate. The alkyl group in the benzyl alkyl diglycol adipate may be either linear or branched, and the number of carbon atoms in the alkyl group is not particularly limited, but is usually about 1 to 20. Among these, linear alkyl groups are preferred, more preferably linear alkyl groups having 1 to 8 carbon atoms, and even more preferably linear alkyl groups having 1 to 4 carbon atoms. More specific examples include benzyl methyl diglycol adipate, benzyl ethyl diglycol adipate, benzyl propyl diglycol adipate, and benzyl butyl diglycol adipate.

[0055] Examples of the sebacate plasticizer include dimethyl sebacate, dibutyl sebacate, di-2-ethylhexyl sebacate, dioctyl sebacate, and diisooctyl sebacate.

[0056] Examples of the azelaic acid ester plasticizer include dioctyl azelate, 2-ethylhexyl azelate, isobutyl azelate, isodecyl azelate, diisononyl azelate, dihexyl azelate, divinyl azelate, and dibenzyl azelate.

[0057] Examples of phthalate plasticizers include dimethyl phthalate, diethyl phthalate, dibutyl phthalate, diheptyl phthalate, dioctyl phthalate, diisooctyl phthalate, di-2-ethylhexyl phthalate, di-2-ethylhexyl isophthalate, dinonyl phthalate, diisononyl phthalate, diisodecyl phthalate, ditridecyl phthalate, dibutylpentyl phthalate, dicyclohexyl phthalate, diundecyl phthalate, and diphenyl phthalate.

[0058] Examples of the phosphate plasticizer include trimethyl phosphate, triethyl phosphate, tributyl phosphate, tri-2-ethylhexyl phosphate, 2-ethylhexyl diphenyl phosphate, triphenyl phosphate, tricresyl phosphate, and diphenylethyl phosphate.

[0059] Examples of the citrate ester plasticizer include triethyl citrate, triethyl acetyl citrate, tributyl citrate, tributyl acetyl citrate, and tri-2-ethylhexyl acetyl citrate.

[0060] Examples of glycolic acid ester plasticizers include triacetin, tributyrin, methylphthalyl ethylglycolate, ethylphthalyl ethylglycolate, and butylphthalyl butylglycolate.

[0061] Examples of trimellitic acid ester plasticizers include trioctyl trimellitate, tri-2-ethylhexyl trimellitate, diisooctyl monoisodecyl trimellitate, and triisononyl trimellitate.

[0062] Examples of the ricinoleic acid ester plasticizer include methylacetyl ricinoleate and butylacetyl ricinoleate.

[0063] Examples of the benzoate plasticizer include diethylene glycol dibenzoate, dipropylene glycol dibenzoate, triethylene glycol dibenzoate, and polyethylene glycol dibenzoate.

[0064] Of these components (C), from the viewpoint of enhancing the stability of the emulsion composition, aliphatic dibasic acid ester plasticizers are preferred, adipate ester plasticizers are more preferred, and benzyl alkyl diglycol adipate is even more preferred.

[0065] The weight average molecular weight (Mw) of the component (C) is not particularly limited, but is, for example, preferably at least 100, more preferably at least 200, and even more preferably at least 300. Also, it is preferably at most 2,000, more preferably at most 1,500, and even more preferably at most 1,000. The weight average molecular weight (Mw) is a value measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0066] The mass ratio (C / A) of the component (C) to the component (A) is not particularly limited, but from the viewpoint of significantly exhibiting the effects of the present invention, it is, for example, 0.002 to 0.5, preferably 0.01 to 0.4, more preferably 0.02 to 0.3, and even more preferably 0.04 to 0.24.

[0067] The content of the (C) component is not particularly limited, but is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, and particularly preferably 2% by mass or more, based on the total amount of the emulsion composition. Also, it is preferably 25% by mass or less, more preferably 20% by mass or less, even more preferably 15% by mass or less, and particularly preferably 12% by mass or less.

[0068] [(D) Dispersion medium] The dispersion medium (D) that can be used in the present emulsion resin composition is not particularly limited as long as it is a water-soluble component in the substance and concentration range that does not affect the stability of the emulsion composition, and may be an aqueous solution containing the component, such as water alone, an aqueous solution of a polysaccharide, an aqueous solution of cellulose (CNF), etc., and may be used in combination with a small amount of a water-soluble organic solvent. Examples of the organic solvent include methanol, ethanol, acetone, etc. Among these, water is the most preferable as the dispersion medium.

[0069] The mass ratio (D / A) of the component (D) to the component (A) is not particularly limited, but from the viewpoint of significantly exhibiting the effects of the present invention, it is, for example, 0.5 to 1.6, preferably 0.7 to 1.4, and more preferably 0.8 to 1.2.

[0070] The content of the (D) component is not particularly limited, but is preferably 25% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more, based on the total amount of the emulsion composition, and is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less.

[0071] When the dispersion medium is a combination of water and an organic solvent, the content of water in the total amount of the dispersion medium is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 90% by mass or more. Among these, it is most preferable to use only water as the dispersion medium.

[0072] [Other ingredients] The present emulsion resin composition preferably does not contain any other components in addition to the above-mentioned components, but as long as the other components are within a range that does not impair the effects of the present invention (for example, 10 mass% or less based on the total amount of the emulsion composition), components that have been commonly used in conventional resin compositions may be included. Such components are not particularly limited, but examples thereof include polyester resins other than the polyester resin (A), preservatives, antifungal agents, antibacterial agents, thermoplastic resins, various stabilizers, ultraviolet absorbers, light stabilizers, antioxidants, antistatic agents, rust inhibitors, curing agents, fillers, etc.

[0073] (Polyester resins other than polyester resin (A)) Examples of polyester resins other than the polyester resin (A) include aliphatic polyester resins having aliphatic oxycarboxylic acid units as the main structural unit. Specific examples of aliphatic oxycarboxylic acid components that provide aliphatic oxycarboxylic acid units include lactic acid, glycolic acid, 2-hydroxy-n-butyric acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxycaproic acid, 6-hydroxycaproic acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-hydroxyisocaproic acid, 3-hydroxyvaleric acid, malic acid, citric acid, and the like, or lower alkyl esters or intramolecular esters thereof. In addition, lactone compounds such as ε-caprolactone are also included in the aliphatic oxycarboxylic acid in the present invention. When optical isomers exist in these, they may be D-form, L-form, or racemic form, and may be in the form of a solid, liquid, or aqueous solution. Among these, lactic acid, glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 6-hydroxycaproic acid, and 3-hydroxyvaleric acid are preferred. These aliphatic oxycarboxylic acids may be used alone or in combination of two or more.

[0074] Specific examples of the aliphatic polyester resin having the aliphatic oxycarboxylic acid unit as the main constituent unit include polylactic acid, polyglycolic acid, poly 3-hydroxybutyrate, poly 4-hydroxybutyrate, poly(3-hydroxybutyrate-co-3-hydroxyvalerate), polycaprolactone, etc.

[0075] The composition of lactic acid contained in polylactic acid is, for example, a molar ratio of D-lactic acid:L-lactic acid=100:0-85:15, or 0:100-15:85. It is also possible to blend other polylactic acids having different composition ratios of D-lactic acid and L-lactic acid.

[0076] Furthermore, the polylactic acid may be a copolymer of the above-mentioned polylactic acid and other oxycarboxylic acids, or may contain a small amount of units derived from a chain extender. Examples of other oxycarboxylic acids include optical isomers of lactic acid (D-lactic acid for L-lactic acid, and L-lactic acid for D-lactic acid), glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 2-hydroxy-n-butyric acid, 2-hydroxy-3,3-dimethylbutyric acid, 2-hydroxy-3-methylbutyric acid, 2-methyllactic acid, and bifunctional aliphatic oxycarboxylic acids such as 2-hydroxycaproic acid, and lactones such as caprolactone, butyrolactone, and valerolactone. Units derived from such other oxycarboxylic acids can be used in an amount of less than 15 mol% of the total structural units of the polylactic acid.

[0077] In addition, examples of polyester resins other than the polyester resin (A) include aliphatic-aromatic polyester resins having aliphatic polyhydric alcohol units, aliphatic polycarboxylic acid units, and aromatic polycarboxylic acid units as main constituent units. The aliphatic-aromatic polyester resin having an aliphatic polyhydric alcohol unit, an aliphatic polycarboxylic acid unit, and an aromatic polycarboxylic acid unit as main constituent units has, for example, an aliphatic polyhydric alcohol unit represented by the above formula (1), an aliphatic polycarboxylic acid unit represented by the above formula (2), and an aromatic polycarboxylic acid unit represented by the following formula (3) as main constituent units. It may further have the above-mentioned oxycarboxylic acid unit.

[0078] -OC-R 31 -CO- (3) [In formula (3), R 31 represents a divalent aromatic hydrocarbon group, and when copolymerized, the number of types is not limited to one.

[0079] The aliphatic polyhydric alcohol that provides the polyhydric alcohol unit of formula (1) and the aliphatic polycarboxylic acid component that provides the aliphatic polycarboxylic acid unit of formula (2) are the same as those exemplified in the description of component (A) above.

[0080] The aromatic polycarboxylic acid component that gives the aromatic polycarboxylic acid unit of formula (3) is not particularly limited, but examples thereof include terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, etc. These may be acid anhydrides. In addition, examples of derivatives of aromatic polycarboxylic acids include lower alkyl esters of these aromatic polycarboxylic acids.

[0081] Specific examples of the aliphatic-aromatic polyester resin include polybutylene alkylate terephthalates such as polybutylene adipate terephthalate and polybutylene succinate terephthalate. These can be used alone or in combination of two or more.

[0082] [Resin composition for emulsion and method for producing emulsion composition] The resin composition for emulsion and the method for producing the emulsion composition can employ known methods in the art. For example, the composition is produced by a phase inversion emulsification step of mixing component (A), dispersant (B), and dispersion medium (D). Alternatively, the composition can be produced by a phase inversion emulsification step of melt-kneading a composition containing component (A) and plasticizer (C), and adding dispersant (B) and dispersion medium (D) to the melt-kneaded composition and mixing them.

[0083] The melt flow rate (MFR) of the composition obtained by the step of melt-kneading the (A) component and the (C) plasticizer is preferably 8 g / 10 min or more, more preferably 9 g / 10 min or more, and even more preferably 10 g / 10 min or more, when measured at 190°C and 2.16 kg. It is also preferably 50 g / 10 min or less, more preferably 45 g / 10 min or less, even more preferably 42 g / 10 min or less, and particularly preferably 40 g / 10 min or less. When the melt flow rate is within the above range, the stability of the emulsion composition tends to be high. When a resin component other than the (A) component is contained, the melt flow rate (MFR) of the composition obtained by the step of melt-kneading the resin component, the (A) component, and the (C) plasticizer is preferably within the above-mentioned range when measured at 190°C and 2.16 kg.

[0084] Specifically, the emulsion composition is produced by, for example, adding component (A) (with optional addition of plasticizer (C)) to a kneader, optionally adding a solvent, melt-kneading under heating conditions, adding dispersant (B) such as PVA resin (B1) and dispersion medium (D) such as water, and mixing and phase-inversion emulsifying these components. The heating temperature is usually 40 to 250°C, preferably 60 to 200°C, more preferably 60 to 160°C, and even more preferably 80 to 150°C. The heating time is usually 10 to 1,800 seconds, preferably 10 to 600 seconds, and more preferably 20 to 300 seconds.

[0085] Examples of the kneading machine include an extruder, a homogenizer (high pressure), a roll mill, a kneader, an ink roll, a Banbury mixer, etc. Among these, from the viewpoint of productivity, an extruder is preferred, and a multi-screw extruder having two or more screws such as a twin-screw extruder is particularly preferred.

[0086] When producing using an extruder, for example, component (A) (with addition of plasticizer (C) as necessary) is continuously fed from a hopper of the extruder or a separate supply port and melt-kneaded under heating conditions, a dispersant (B) such as a PVA-based resin (B1) and a dispersion medium (D) such as water are added from another supply port provided in the extruder, kneaded and dispersed to effect phase inversion emulsification, and then continuously extruded from a die to obtain an emulsion composition according to an embodiment of the present invention.

[0087] In addition, the emulsion composition can be obtained by using pellets obtained by melt-kneading the component (A) (with the addition of the plasticizer (C) as necessary) under heating conditions using an extruder, etc. Specifically, the pellets of the component (A) (containing the plasticizer (C) as necessary) are continuously fed from a hopper of the extruder and melt-kneaded under heating conditions, and a dispersant (B) such as a PVA-based resin (B1) and a dispersion medium (D) such as water are added from another feed port provided in the same extruder, and the mixture is kneaded and dispersed to undergo phase inversion emulsification, and then continuously extruded from a die to obtain an emulsion composition according to an embodiment of the present invention.

[0088] [Resin composition for emulsion and emulsion composition] The present emulsion composition obtained as described above is an aqueous emulsion composition. An aqueous emulsion composition is an emulsion in which particulate matter is dispersed in an aqueous solvent and emulsified, specifically, an emulsion system in which the dispersion medium (i.e., continuous phase) is an aqueous liquid such as water and / or an organic solvent in which the dispersoid is substantially insoluble or has a significantly low solubility. In the present emulsion composition, the mixed composition of the (A) component and the (C) plasticizer is the dispersoid, and the aqueous emulsion composition is one in which these are dispersed in an aqueous solvent.

[0089] The mass ratio of the dispersant (B) to the solid content contained in the resin composition for emulsion [content of (B) / content of solid content] is preferably 0.015 or more, more preferably 0.02 or more, and even more preferably 0.03 or more. The mass ratio [content of (B) / content of solid content] is not particularly limited, but is preferably 0.3 or less, more preferably 0.2 or less, and even more preferably 0.15 or less. Outside this range, the stability of the emulsion composition tends to decrease.

[0090] Specifically, for example, when the composition contains the (A) component, the (B) component is a polyvinyl alcohol resin (B1), and the (C) component is an ester plasticizer, the mass ratio of the content of the (B1) component to the total content of these components [(B1) / [(A)+(B1)+(C)]] is preferably 0.015 or more, more preferably 0.02 or more, and even more preferably 0.03 or more. The mass ratio [(B1) / [(A)+(B1)+(C)]] is not particularly limited, but is preferably 0.3 or less, more preferably 0.2 or less, and even more preferably 0.15 or less. The term "solid content" refers to components other than volatile components contained in the emulsion composition. Specifically, for example, the term refers to components that remain on a support as a coating film when the emulsion composition is applied to a support and dried.

[0091] The emulsion composition obtained as described above has excellent sedimentation stability. The sedimentation stability of the emulsion composition can be evaluated, for example, by the method described in the Examples below. For example, the sedimentation rate measured by the method described in the Examples below is preferably 10% or less, more preferably 8% or less, even more preferably 6% or less, and particularly preferably 3% or less.

[0092] From the viewpoint of sedimentation stability, the dispersed particle size of the dispersoid in the present emulsion composition is 10 μm or less, preferably 5 μm or less, more preferably 2.5 μm or less, and even more preferably 3 μm or less. The lower limit is usually about 0.01 μm. The dispersed particle size is the median size (d50) corresponding to 50% of the cumulative particle size distribution value on a volume basis, and can be measured, for example, by a laser diffraction particle size measuring device (e.g., model number LA-950V2, manufactured by Horiba, Ltd.).

[0093] The present emulsion composition has excellent oil resistance. The oil resistance can be evaluated by JAPAN TAPPI, Paper and Pulp Testing Method, No. 41, KITT method. In the present emulsion composition, the KIT value obtained by such a method is preferably 4 or more, more preferably 5 or more, even more preferably 6 or more, and particularly preferably 7 or more.

[0094] Films and the like obtained from the present emulsion composition have excellent tensile strength, specifically, for example, a tensile strength (MPa) of 5 MPa or more as measured by the method described in the Examples below.

[0095] In the present emulsion composition, it is preferable to use a biodegradable component as the dispersant (B), and in particular it is more preferable to use a PVA-based resin (B1) as the dispersant (B).

[0096] [Application] The present resin composition for emulsion or the present emulsion composition can be used in the form of a molded article (film or the like) obtained by a known molding method, although the form is not limited thereto. Furthermore, the present resin composition for emulsions or the present emulsion composition can be used, for example, as an adhesive, pressure sensitive adhesive, a modifier thereof, a coating agent, a heat sealing agent, a paint, a primer for paint, an ink, a binder, etc., in paper, a film, a sheet, a structural material, a building material, an automobile part, an electric / electronic product, a packaging material, clothing, a medicine, a cosmetic (shampoo, rinse, emulsion, lotion, perfume, etc.), an agricultural composition (pesticide emulsion, etc.), a health food, a food, etc. Among them, a cosmetic, an agricultural composition, a paint, an ink, or an adhesive containing the present resin composition for emulsions or the present emulsion composition is preferable. The present resin composition for emulsion or the present emulsion composition is also suitably used as a coating agent for an object to be coated (an object to be coated).

[0097] The object to be coated with the present resin composition for emulsion is not particularly limited, but is preferably, for example, a paper substrate, and examples of the paper substrate include thermal recording paper, release paper, peeling paper, inkjet paper, carbon paper, non-carbon paper, base paper for paper cups, greaseproof paper, paperboard such as Manila board, white board and liner, printing paper such as general fine paper, medium quality paper and gravure paper, high-grade, medium-grade and low-grade paper, newsprint, etc. For example, a laminate including a layer made of a paper substrate and a layer made of the resin composition for emulsion or the present emulsion composition coated on the paper substrate is also suitable.

[0098] The object to be coated is preferably a plastic substrate, and examples of the plastic substrate include polyethylene terephthalate (PET) resin, polypropylene (PP) resin [biaxially oriented polypropylene (OPP), non-axially oriented polypropylene (CPP)], nylon resin, various biodegradable resins, polyethylene (PE) resin [low density polyethylene (LDPE), high density polyethylene (HDPE)], etc. For example, a laminate including a layer made of a plastic substrate and a layer made of a resin composition for emulsions coated on the plastic substrate is also suitable.

[0099] The coating method using the present resin composition for emulsion or the present emulsion composition is not particularly limited, and examples thereof include roll coating, dip coating, bar coating, nozzle coating, die coating, spray coating, spin coating, curtain coating, and flow coating. EXAMPLES

[0100] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are based on mass.

[0101] First, the following ingredients were prepared: <Component (A)> (a1) Polybutylene succinate adipate 1 (PBSA) [BiOPBS (FD72PM) manufactured by PTT MCC Biochem, melt flow rate (MFR) 22g / 10min (190℃, 2.16kg), melting point 86℃] (a2) Polybutylene succinate adipate 2 (PBSA) [BiOPBS (FD92PM) manufactured by PTT MCC Biochem, melt flow rate (MFR) 4g / 10min (190℃, 2.16kg), melting point 84℃]

[0102] Polylactic acid [Natureworks' Ingeo4032D]

[0103] <(B) component> (b1) Polyvinyl alcohol resin (PVA resin) [Unmodified PVA resin, average degree of polymerization 1,700, degree of saponification 87-89%, 4% viscosity at 20°C 20.5-24.5 mPa s]

[0104] <(C) component> (c1) Adipate plasticizers [DAIFATTY-101 (mixed dibasic acid ester, adipate-containing compound) manufactured by Daihachi Chemical Industry Co., Ltd., weight average molecular weight of the adipate ester is 338]

[0105] <(D) component> ·(d1)Water

[0106] [Example 1] Polybutylene succinate adipate 1 (a1) was continuously fed from the hopper of a twin-screw extruder [KZW15TW-60MG, Technobel, L / D=60], and a PVA-based resin (b1) as a dispersant and water (d1) as a dispersion medium were continuously fed from a feed port provided in the extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0107] [Example 2] Polybutylene succinate adipate 1 (a1) and an adipate ester plasticizer (c1) were continuously fed from the hopper of a twin-screw extruder [product number KZW15TW-60MG, Technobel Co., Ltd., L / D=60] in a mass ratio of 45:5 (a1:c1), and melt-kneaded under 140°C conditions to obtain a mixed composition. Then, while continuously feeding PVA resin (b1) as a dispersant and water (d1) as a dispersion medium from a feed port provided in the extruder, the mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0108] [Example 3] Polybutylene succinate adipate 2 (a2) and an adipate ester plasticizer (c1) were continuously fed from the hopper of a twin-screw extruder [product number KZW15TW-60MG, Technobel Co., Ltd., L / D=60] in a mass ratio of 40:10 (a2:c1), and melt-kneaded under 140°C conditions to obtain a mixed composition. Then, while continuously feeding PVA resin (b1) as a dispersant and water (d1) as a dispersion medium from a feed port provided in the extruder, the mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0109] [Example 4] Polybutylene succinate adipate 2 (a2) and an adipate ester plasticizer (c1) were continuously fed from the hopper of a twin-screw extruder [product number KZW15TW-60MG, Technovel Co., Ltd., L / D=60] in a mass ratio of 45:5 (a2:c1), and melt-kneaded under conditions of 140°C to obtain a mixed composition. Then, while continuously feeding PVA resin (b1) as a dispersant and water (d1) as a dispersion medium from a feed port provided in the extruder, the mixture was continuously extruded (screw rotation speed: 300 rpm) under conditions of a heating temperature (cylinder temperature) of 90 to 105°C and a heating time of 180 seconds, to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0110] [Example 5] Polybutylene succinate adipate 1 (a1) was continuously fed from the hopper of a twin-screw extruder [KZW15TW-60MG, Technobel, L / D=60], and a PVA-based resin (b1) as a dispersant and water (d1) as a dispersion medium were continuously fed from a feed port provided in the extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0111] [Example 6] Polybutylene succinate adipate 1 (a1) was continuously fed from the hopper of a twin-screw extruder [KZW15TW-60MG, Technobel, L / D=60], and a PVA-based resin (b1) as a dispersant and water (d1) as a dispersion medium were continuously fed from a feed port provided in the extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0112] [Example 7] Polybutylene succinate adipate 1 (a1) was continuously fed from the hopper of a twin-screw extruder [KZW15TW-60MG, Technobel, L / D=60], and a PVA-based resin (b1) as a dispersant and water (d1) as a dispersion medium were continuously fed from a feed port provided in the extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0113] [Comparative Example 1] Polybutylene succinate adipate 2 (a2) was continuously fed from the hopper of a twin-screw extruder [KZW15TW-60MG, Technobel, L / D=60], and a PVA-based resin (b1) as a dispersant and water (d1) as a dispersion medium were continuously fed from a feed port provided in the extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0114] [Comparative Example 2] Polybutylene succinate adipate 2 (a2) was continuously fed from the hopper of a twin-screw extruder [KZW15TW-60MG, Technobel, L / D=60], and a PVA-based resin (b1) as a dispersant and water (d1) as a dispersion medium were continuously fed from a feed port provided in the extruder. The mixture was continuously extruded (screw rotation speed: 300 rpm) at a heating temperature (cylinder temperature) of 90 to 105°C for a heating time of 180 seconds to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0115] [Comparative Example 3] Polylactic acid and an adipic acid ester-based plasticizer (c1) were continuously fed from the hopper of a twin-screw extruder [product number KZW15TW-60MG, Technovel Co., Ltd., L / D=60] in a mass ratio of 40:10 (polylactic acid:c1), and melt-kneaded under conditions of 140°C to obtain a mixed composition. Then, while continuously feeding PVA-based resin (b1) as a dispersant and water (d1) as a dispersion medium from a feed port provided in the extruder, the mixture was continuously extruded (screw rotation speed: 300 rpm) under conditions of a heating temperature (cylinder temperature) of 90 to 105°C and a heating time of 180 seconds, to obtain an emulsion composition having the mass ratio shown in Table 1 below.

[0116] [Minimum film formation temperature (MFT) measurement test] The minimum film-forming temperature of the emulsion compositions according to the examples and comparative examples was measured using a film-forming temperature measuring device (Yoshimitsu Seiki Co., Ltd., film-forming temperature measuring device) in accordance with JIS K 6828 5.11. Specifically, when each emulsion composition was applied to a test plate with a 0.1 mm applicator and dried, the temperature of the boundary where a transparent coating was formed was measured. The results are shown in Table 1.

[0117] [Tensile strength measurement test] The tensile strength was measured according to JIS K7161. Specifically, the emulsion compositions according to the examples and comparative examples were first applied onto a Teflon (registered trademark) sheet and heated at 105°C for 5 minutes to prepare a test film. The tensile strength (MPa) of the obtained test film was measured using a tensile tester (Shimadzu Corporation, Autograph AG-IS) under the following test conditions. The results are shown in Table 1. [Test conditions] Test speed: 100mm / min Distance between gauge lines 15mm Grip distance: 150 mm

[0118] [Oil resistance test] The oil resistance was evaluated according to JAPAN TAPPI, Paper and Pulp Testing Method, No. 41, KITT method. Specifically, kraft paper (basis weight 80 g / m2) cut into small pieces of 50 mm x 50 mm was used. 2) The emulsion compositions of the Examples and Comparative Examples were diluted with water to adjust the solid content to 30% by mass, and coated with a bar coater at a coating amount of 6 g / m 2 The test pieces were then coated and dried so that the oil resistance was such that the oil resistance was within the range of 100%. The oil resistance of the test pieces was evaluated (kit number). The higher the oil resistance (kit number), the better the oil resistance.

[0119] [Settling stability test (settling rate)] The emulsion compositions of the Examples and Comparative Examples were placed in a settling tube (bottom area 9.62 cm 2 The sedimentation rate was calculated based on the reading of the scale on the sedimentation tube (height of the separated layer). The sedimentation rate is calculated based on the following formula. [Formula] Sedimentation rate = height of separated layer (cm) / height of total emulsion composition (cm) x 100

[0120] [Dispersed particle size measurement test] The dispersed particle diameter (median diameter) in the emulsion compositions according to the examples and comparative examples was measured using a laser diffraction particle diameter measuring device (LA-950V2, manufactured by Horiba, Ltd.). The results are shown in Table 1.

[0121] [Melt flow rate (MFR) measurement test] The melt flow rate (MFR) of the base resin contained in each of the resin compositions according to the examples and comparative examples was measured at a temperature of 190° C. and a load of 2.16 kg in accordance with JIS K7210. The results are shown in Table 1. The base resin means either the component (A) or the component (C) contained in each resin composition or a mixed composition thereof. For example, in Example 1, the base resin means the component (a1), and in Example 2, the base resin means a mixed composition consisting of the components (a1) and (c1). Moreover, the base resin means, for example, in Comparative Example 3, a mixed composition consisting of polylactic acid and the component (c1).

[0122] [Table 1]

[0123] As shown in Table 1, Examples 1 to 7, which are emulsion compositions containing an aliphatic polyester resin (A) having an aliphatic polyhydric alcohol and an aliphatic polycarboxylic acid unit as the main structural unit and having a minimum film formation temperature (MFT) of 75°C or less, had excellent sedimentation stability, tensile strength after film formation, and oil resistance. On the other hand, the emulsion compositions of Comparative Examples 1 and 2, which have a minimum film-forming temperature above the range specified in the present invention, were inferior to the Examples in both sedimentation stability and tensile strength after film formation. Furthermore, Comparative Example 3, which is an emulsion composition containing polylactic acid instead of component (A) of the present invention, was inferior to the Examples in both sedimentation stability and tensile strength after film formation.

[0124] From the above, it was confirmed that the present invention can provide an emulsion composition and the like that is excellent in sedimentation stability, tensile strength after film formation, and oil resistance. [Industrial Applicability]

[0125] The emulsion composition of the present invention is particularly useful as a variety of coating agents, for example, as a coating agent for paper substrates, a coating agent for plastic substrates, and the like.

Claims

1. An emulsion composition comprising an emulsion resin composition containing an aliphatic polyester-based resin (A) having an aliphatic polyhydric alcohol unit and an aliphatic polycarboxylic acid unit as main constituent units, wherein the emulsion composition has a minimum film-forming temperature of 75° C. or lower.

2. The emulsion composition according to claim 1 , further comprising a polyvinyl alcohol-based resin (B1).

3. 3. The emulsion composition according to claim 2, wherein a mass ratio (B1 / A) of the polyvinyl alcohol-based resin (B1) to the aliphatic polyester-based resin (A) is 0.1 or less.

4. The emulsion composition according to claim 2, wherein a mass ratio of the polyvinyl alcohol-based resin (B1) to the solid content (B1 / solid content) is 0.15 or less.

5. 3. The emulsion composition according to claim 1, further comprising a plasticizer (C), wherein a mass ratio (C / A) of the plasticizer (C) to the aliphatic polyester resin (A) is 0.002 to 0.

5.

6. 3. The emulsion composition according to claim 1, wherein the dispersed particle size is 10 μm or less.

7. A coating agent comprising the emulsion composition according to claim 1 or 2.

8. The coating agent according to claim 7, wherein the substrate to be coated is a paper substrate.

9. 8. The coating agent according to claim 7, wherein the object to be coated is a plastic substrate.

10. A molded article obtained by using the emulsion composition according to claim 1 or 2.

11. A film obtained by using the emulsion composition according to claim 1 or 2.

12. A cosmetic comprising the emulsion composition according to claim 1 or 2.

13. 3. An agricultural composition comprising the emulsion composition according to claim 1 or 2.

14. A paint comprising the emulsion composition according to claim 1 or 2.

15. 3. An ink comprising the emulsion composition according to claim 1 or 2.

16. A pressure-sensitive adhesive comprising the emulsion composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Biodegradable water dispersion