Fiber-reinforced resin molding
A fiber-reinforced resin molded article with optimized epoxy resin and acid anhydride composition addresses workability and bending strength issues, ensuring crack resistance and suitability for building materials.
Patent Information
- Application Number
- JP2023045532
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Fiber-reinforced resin materials face issues with workability and bending properties when used as base materials in ceiling structures, leading to cracks and poor processability during fixation, especially when replacing traditional aluminum materials.
A fiber-reinforced resin molded article is developed using a resin composition containing specific ratios of epoxy resin, epoxy diluent, and acid anhydride, with compounds like difunctional glycidyl compounds and polyacid polyanhydrides, to achieve a viscosity of 1000 mPa·s or less and a glass transition temperature of 110°C or less, ensuring excellent processability and bending strength.
The solution provides a fiber-reinforced resin molded article with improved workability and bending strength, reducing the likelihood of cracks and burrs during fixation, making it suitable for use in building materials like field edge supports and ceiling boards.
Smart Images

Figure 2024135040000001 
Figure 2024135040000002 
Figure 2024135040000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fiber-reinforced resin molding that is used particularly as a building material. [Background technology]
[0002] Fiber-reinforced resin composite materials are lightweight, high-strength, and high-rigidity, and therefore have a wide range of applications, from sports and leisure applications to industrial applications such as vehicles, aircraft, architecture, and civil engineering. Such molded bodies of fiber-reinforced resin composite materials (hereinafter also referred to as "fiber-reinforced resin molded bodies") are molded using a mold. For example, as an example of such fiber-reinforced resin molded bodies, Patent Document 1 describes a fiber-reinforced resin molded body that has flame retardancy and good moldability.
[0003] Meanwhile, in the field of building materials, aluminum or steel plate base materials are used for the base of the walls or ceilings of buildings. In the ceiling base structure of a building or the like using base materials, for example, a hanging bolt is hung from the floor slab of the upper floor, and the hanging bolt and the rafter are attached via a hanger. Furthermore, a rafter for fixing the ceiling board is fixed to the indoor side of the rafter (i.e., the lower side opposite to the upper floor). In addition, braces and the like are also fixed to the ceiling base structure in order to increase the rigidity of the ceiling. Such rafter supports and rafters or these and braces are usually fixed using screws. Note that in the field of architecture, various ceiling structures with excellent functions have been developed. For example, Patent Document 2 describes a ceiling structure that can reduce floor impact sound propagating from the upper floors of a building to the lower floors. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2022-158205 [Patent Document 2] Patent No. 6504966 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been a demand for weight reduction in the entire ceiling foundation structure of high-rise buildings, etc. Specifically, there has been a demand for weight reduction in foundation materials in the ceiling structure, such as joist supports, joists, ceiling panels, braces, etc.
[0006] In view of the above circumstances, it was considered to use a relatively lightweight fiber-reinforced resin molded body as a base material for ceiling structures and the like, in place of an aluminum base material. However, when fiber-reinforced resin base materials are fixed to each other, or when a fiber-reinforced resin base material is fixed to an aluminum base material by screwing, cracks and burrs occur in the base material. Thus, it was found that fiber-reinforced resin base materials have problems with processability. On the other hand, when using a fiber-reinforced resin base material as a substitute for an aluminum base material, it is also required that the base material have good bending properties.
[0007] Therefore, an object of the present invention is to provide a fiber-reinforced resin molding that has excellent processability while maintaining good bending strength and bending modulus. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention includes the following preferred embodiments.
[0009] The fiber-reinforced resin molded product according to the present invention is a fiber-reinforced resin molded product obtained by impregnating reinforcing fibers with a resin composition containing an epoxy resin, an epoxy diluent, and a curing agent, and curing the resin composition. the resin composition contains 30 parts by mass or more and 80 parts by mass or less of the epoxy resin and 20 parts by mass or more and 70 parts by mass or less of the epoxy diluent relative to 100 parts by mass in total of the epoxy resin and the epoxy diluent, contains an acid anhydride as the curing agent, has a viscosity of 1000 mPa s or less, and has a glass transition temperature Tg of 110° C. or less; The epoxy diluent contains a bifunctional glycidyl compound having a total of 7 or more carbon atoms and oxygen atoms constituting the main chain between the glycidyl groups, and / or the acid anhydride contains a polyacid polyanhydride having 7 or more carbon atoms in the main chain.
[0010] In the fiber-reinforced resin molded product, the ratio of the hydroxyl equivalent of the acid anhydride to the total epoxy equivalent of the epoxy resin and the epoxy diluent is preferably 0.8 to 1.1.
[0011] In the fiber reinforced resin molding, it is more preferable that the flexural modulus is 130 GPa or more and the flexural strength is 1000 MPa or more.
[0012] The fiber-reinforced resin molding is more preferably a building material. Effect of the Invention
[0013] According to the present invention, it is possible to provide a fiber-reinforced resin molding having excellent processability while maintaining good bending strength and bending modulus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present inventors have conducted extensive research into fiber-reinforced resin moldings that have excellent processability while maintaining good bending strength and bending modulus. As a result, the present invention has been achieved. Specifically, in the fiber-reinforced resin molding, the epoxy resin and the epoxy diluent are contained in a resin composition within a specific ratio range, and at least one of the epoxy diluent and the acid anhydride as the curing agent each contains a specific compound, so that the fiber-reinforced resin molding described above can be provided.
[0015] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.
[0016] 1. Components of fiber-reinforced plastic moldings The fiber-reinforced resin molded body of the present embodiment is obtained by impregnating reinforcing fibers with a resin composition and curing the resin composition. First, the components of the fiber-reinforced resin molded body of the present embodiment will be described.
[0017] <Resin composition> The resin composition includes an epoxy resin, an epoxy diluent, and a curing agent. The resin composition may also include other additives. Each component of the resin composition, a method for preparing the resin composition, and physical properties of the resin composition will be described in detail below.
[0018] (Epoxy resin) The epoxy resin is a resin that is the main component of the resin composition. The type of the epoxy resin is not particularly limited as long as it does not impair the effects of bending properties and processability in the fiber-reinforced resin molded body of this embodiment. For example, the epoxy resin is preferably a resin selected from bisphenol F type epoxy resin and bisphenol A type epoxy resin.
[0019] The epoxy resin is contained in the resin composition in an amount of 30 parts by mass or more and 80 parts by mass or less, based on 100 parts by mass of the total of the epoxy resin and the epoxy diluent. When the epoxy resin is contained in an amount of 30 parts by mass or more, a fiber-reinforced resin molded product that can maintain good bending strength can be obtained. When the epoxy resin is contained in an amount of 80 parts by mass or less, the viscosity of the resin composition can be prevented from becoming too high, which makes it difficult to impregnate the reinforcing fibers. As a result, a fiber-reinforced resin molded product that is less likely to crack or break and has excellent processability can be obtained.
[0020] The epoxy resin is preferably contained in an amount of 35 parts by mass or more, more preferably 40 parts by mass or more, based on the total amount of the epoxy resin and the epoxy diluent, and is preferably contained in an amount of 70 parts by mass or less, more preferably 65 parts by mass or less, based on the total amount of the epoxy resin and the epoxy diluent.
[0021] (Epoxy Diluent) The epoxy diluent dilutes the epoxy resin and gives the resin composition an appropriate viscosity.
[0022] The type of epoxy diluent is not particularly limited as long as it does not impair the effects of bending properties and processability in the fiber-reinforced resin molded body of this embodiment, and any epoxy diluent known to those skilled in the art can be used. For example, the epoxy diluent may be a glycidyl-based compound such as a glycidyl ester compound or a glycidyl ether compound. The glycidyl-based compound such as a glycidyl ester compound or a glycidyl ether compound may be monofunctional, bifunctional, or polyfunctional (three or more).
[0023] In this specification, the term "glycidyl compound" refers to all glycidyl compounds, including glycidyl compounds whose main chain is composed of CC bonds, glycidyl compounds whose main chain is composed of CO bonds, and glycidyl compounds whose main chain is composed of CC bonds and CO bonds.
[0024] Here, in the fiber-reinforced resin molded body of this embodiment, the epoxy diluent contains a bifunctional glycidyl-based compound having 7 or more carbon atoms and oxygen atoms constituting the main chain between the glycidyl groups, and / or the acid anhydride described later contains a polyacid polyanhydride having 7 or more carbon atoms in the main chain. When the epoxy diluent contains a bifunctional glycidyl-based compound having 7 or more carbon atoms and oxygen atoms constituting the main chain between the glycidyl groups, toughness can be effectively imparted to the cured product. Therefore, a fiber-reinforced resin molded body having excellent processability and less susceptible to cracks and burrs can be obtained. In addition, when the epoxy diluent contains a bifunctional glycidyl-based compound having 7 or more carbon atoms and oxygen atoms constituting the main chain between the glycidyl groups, it is preferable that the epoxy diluent is made of a bifunctional glycidyl-based compound having 7 or more carbon atoms and oxygen atoms constituting the main chain between the glycidyl groups. Furthermore, the total number of carbon atoms and oxygen atoms in the main chain of the bifunctional glycidyl-based compound is preferably 10 or more, more preferably 15 or more, and even more preferably 18 or more.
[0025] Furthermore, when the epoxy diluent contains a bifunctional glycidyl-based compound in which the total number of carbon atoms and oxygen atoms constituting the main chain between the glycidyl groups is 7 or more, the epoxy diluent preferably contains a bifunctional glycidyl-based compound in which the total number of carbon atoms constituting the main chain between the glycidyl groups is 7 or more, and more preferably consists of a bifunctional glycidyl-based compound in which the total number of carbon atoms constituting the main chain between the glycidyl groups is 7 or more. In this case, the number of carbon atoms in the main chain of the bifunctional glycidyl-based compound is preferably 10 or more, more preferably 15 or more, and even more preferably 18 or more.
[0026] Examples of bifunctional glycidyl compounds having a total of 7 or more carbon atoms and oxygen atoms constituting the main chain between glycidyl groups include, but are not limited to, bis(2,3-epoxypropyl) isoeicosadienedioate, bis(2,3-epoxypropyl) isoeicosadienedioate, polyethylene glycol diglycidyl ether, and polypropylene glycol diglycidyl ether.
[0027] The bifunctional glycidyl compound having a total number of carbon atoms and oxygen atoms constituting the main chain between glycidyl groups of 7 or more may be a commercially available product. Examples of commercially available products include dibasic acid glycidyl ester "SB-20G" (manufactured by Okamura Oil Mills, Ltd.), dibasic acid glycidyl ester "IPU-22G" (manufactured by Okamura Oil Mills, Ltd.), Denacol "EX-832" (manufactured by Nagase ChemteX Corporation), and Denacol "EX-931" (manufactured by Nagase ChemteX Corporation).
[0028] The epoxy diluent is contained in the resin composition in an amount of 20 parts by mass or more and 70 parts by mass or less, based on 100 parts by mass of the total of the epoxy resin and the epoxy diluent. When the epoxy diluent is contained in an amount of 20 parts by mass or more, it is possible to prevent the reinforcing fibers from being difficult to impregnate. As a result, it is possible to obtain a fiber-reinforced resin molded product having excellent processability and being less susceptible to cracks and fraying. When the epoxy diluent is contained in an amount of 70 parts by mass or less, it is possible to obtain a fiber-reinforced resin molded product that maintains good bending strength.
[0029] The epoxy diluent is preferably contained in an amount of 30 parts by mass or more, more preferably 35 parts by mass or more, based on the total amount of the epoxy resin and the epoxy diluent, and is preferably contained in an amount of 65 parts by mass or less, more preferably 60 parts by mass or less, based on the total amount of the epoxy resin and the epoxy diluent.
[0030] In addition, two or more kinds of epoxy diluents may be included. For example, the epoxy diluent may include a bifunctional glycidyl compound having a total of 7 or more carbon atoms and oxygen atoms constituting the main chain between glycidyl groups, and one or more other epoxy diluents.
[0031] (hardening agent) The curing agent cures the epoxy resin and imparts suitable moldability and bending properties to the finally obtained fiber-reinforced resin molded article. The resin composition of the present embodiment contains an acid anhydride as a curing agent.
[0032] The type of acid anhydride is not particularly limited as long as it does not impair the bending properties and processability of the fiber-reinforced resin molded body of this embodiment. For example, examples of the acid anhydride include phthalic anhydride compounds, maleic anhydride compounds, and Nadic anhydride. Of these, the acid anhydride is preferably a phthalic anhydride compound from the viewpoint of viscosity. In addition, when a phthalic anhydride compound is included as the acid anhydride, it is easy to impart good moldability to the fiber-reinforced resin molded body finally produced. Examples of the phthalic anhydride compound include, but are not limited to, methyltetrahydrophthalic anhydride, tetrahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, hexahydrophthalic anhydride, and the like. Of these, the phthalic anhydride compound is preferably liquid low-viscosity methyltetrahydrophthalic anhydride from the viewpoint of easily realizing a low viscosity of the resin composition.
[0033] When the above-mentioned types of acid anhydrides such as phthalic anhydride compounds are included as the acid anhydride, the content of the acid anhydride is preferably blended so as to satisfy the ratio of the hydroxyl group equivalent of the acid anhydride to the epoxy equivalent described below. When the acid anhydride is blended so as to satisfy the equivalent ratio, it is possible to easily suppress the occurrence of surface defects such as poor curing and cracks in the fiber reinforced resin molding finally produced.
[0034] Here, in the fiber-reinforced resin molding of this embodiment, as described above, the epoxy diluent contains a bifunctional glycidyl-based compound in which the total number of carbon atoms and oxygen atoms constituting the main chain between the glycidyl groups is 7 or more, and / or the acid anhydride contains a polyacid polyanhydride in which the main chain has 7 or more carbon atoms. When the acid anhydride contains a polyacid polyanhydride in which the main chain has 7 or more carbon atoms, a fiber-reinforced resin molding having excellent processability in which cracks and burrs are unlikely to occur can be obtained. In addition, when the acid anhydride contains a polyacid polyanhydride in which the main chain has 7 or more carbon atoms, it is preferable that the acid anhydride contained as a curing agent is made of a polyacid polyanhydride in which the main chain has 7 or more carbon atoms. Furthermore, the number of carbon atoms in the main chain of the polyacid polyanhydride is preferably 10 or more, more preferably 15 or more, and even more preferably 18 or more.
[0035] The polyacid polyanhydride having 7 or more carbon atoms in the main chain is not particularly limited, and examples thereof include eicosane diacid, tetradecane diacid, etc. In addition, the polyacid polyanhydride having 7 or more carbon atoms in the main chain may be a commercially available product. Examples of commercially available products include branched long-chain dibasic acid polyacid polyanhydrides "IPU-22AH" (manufactured by Okamura Oil Mills, Ltd.), "SB-20AH" (manufactured by Okamura Oil Mills, Ltd.), "SB-12AL" (manufactured by Okamura Oil Mills, Ltd.), etc.
[0036] Even when a polyacid polyanhydride having 7 or more carbon atoms in the main chain is used as the acid anhydride instead of the acid anhydride such as the above-mentioned phthalic anhydride compound, the content of the polyacid polyanhydride is preferably blended so as to satisfy the ratio of the hydroxyl group equivalent of the acid anhydride to the epoxy equivalent described below. When the polyacid polyanhydride is blended so as to satisfy the equivalent ratio, it is possible to easily suppress the occurrence of surface defects such as poor curing and cracks in the finally produced fiber-reinforced resin molding.
[0037] In addition, two or more kinds of acid anhydrides may be included. For example, the acid anhydride may include a polyacid polyanhydride having 7 or more carbon atoms in the main chain and one or more other acid anhydrides. In this case, it is preferable to adjust the content of the acid anhydride relative to the total of the epoxy resin and the epoxy diluent so as to satisfy the ratio of the hydroxyl group equivalent of the acid anhydride to the epoxy equivalent described later.
[0038] In the fiber-reinforced resin molded product of this embodiment, the ratio of the hydroxyl equivalent of the acid anhydride to the total epoxy equivalent of the epoxy resin and the epoxy diluent is preferably 0.8 to 1.1. By setting the ratio of the hydroxyl equivalent of the acid anhydride to 0.8 or more, it is possible to prevent the fiber-reinforced resin molded product from being insufficiently cured or the viscosity of the resin composition from being excessively increased. In addition, by setting the ratio of the hydroxyl equivalent of the acid anhydride to 1.1 or less, it is possible to prevent defects such as cracks from occurring in the fiber-reinforced resin molded product that is finally produced.
[0039] In this specification, the "hydroxyl group equivalent of the acid anhydride" means the total hydroxyl group equivalent when the acid anhydride contains both a polyacid polyanhydride having 7 or more carbon atoms in the main chain and one or more other acid anhydrides, or when two or more types of acid anhydrides are contained.
[0040] The ratio of the hydroxyl equivalent of the acid anhydride to the total epoxy equivalent of the epoxy resin and the epoxy diluent is more preferably 0.9 or more, and even more preferably 0.95 or more. The ratio of the hydroxyl equivalent of the acid anhydride to the total epoxy equivalent of the epoxy resin and the epoxy diluent is more preferably 1.05 or less, and even more preferably 1 or less.
[0041] The resin composition of the present embodiment may contain a curing agent other than the acid anhydride. Examples of the curing agent other than the acid anhydride include aromatic polyamines and phenolic resins.
[0042] (Other additives) The resin composition according to the present embodiment may contain, in addition to the epoxy resin, the epoxy diluent and the curing agent, other additives such as a curing accelerator, a release agent, a filler, a pigment, an ultraviolet absorber, and an antioxidant.
[0043] Among these additives, the resin composition preferably contains a curing accelerator. When the resin composition contains a curing accelerator, it is possible to achieve a curing time suitable for pultrusion molding, which will be described later, for example, a curing time of about 2 minutes.
[0044] The curing accelerator is not particularly limited, but examples thereof include imidazole derivatives, tertiary amines, phosphorus compounds, Lewis acids, and the like. Of these, from the viewpoint of viscosity stability, the curing accelerator is preferably an imidazole derivative. Examples of imidazole derivatives include 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-4-methylimidazole, and the like. In addition, the curing accelerator may be a commercially available product. Examples of commercially available products include Curazole (registered trademark) "2E4MZ-CN" (manufactured by Shikoku Chemical Industry Co., Ltd.), Curazole (registered trademark) "2E4MZ" (manufactured by Shikoku Chemical Industry Co., Ltd.), Curazole (registered trademark) "2P4MZ" (manufactured by Shikoku Chemical Industry Co., Ltd.), and the like.
[0045] The curing accelerator is preferably contained in the resin composition in an amount of 0.5 parts by mass or more and 5 parts by mass or less, based on 100 parts by mass of the epoxy resin and the epoxy diluent in total. By containing 0.5 parts by mass or more of the curing accelerator, the above-mentioned action of the curing accelerator can be effectively exerted. By containing 5 parts by mass or less of the curing accelerator, the viscosity increase of the resin composition in a short period of time can be suppressed.
[0046] The curing accelerator is preferably contained in an amount of 1 part by mass or more, more preferably 1.5 parts by mass or more, based on the total amount of the epoxy resin and the epoxy diluent, and more preferably 4 parts by mass or less, more preferably 3 parts by mass or less, based on the total amount of the epoxy resin and the epoxy diluent.
[0047] Furthermore, among these additives, the resin composition preferably contains a release agent. The release agent is not particularly limited, and may be any release agent known to those skilled in the art, such as fatty acid amine-based release agents and fatty acid ester-based release agents. Two or more of these release agents may be included. In addition, the release agent may be a commercially available product. Examples of commercially available products include MoldWiz (registered trademark) "INT-1888LE" (manufactured by Axel Plastics Research Laboratories), MoldWiz (registered trademark) "INT-1846N2" (manufactured by Axel Plastics Research Laboratories), and MoldWiz (registered trademark) "INT-1324B" (manufactured by Axel Plastics Research Laboratories).
[0048] The release agent is preferably contained in the resin composition in an amount of 0.1 to 15 parts by mass relative to 100 parts by mass of the total of the epoxy resin and the epoxy diluent. By containing 0.1 parts by mass or more of the release agent, the fiber reinforced resin molded body can be easily pulled out from the mold. By containing 15 parts by mass or less of the release agent, the deterioration of the heat resistance and strength of the fiber reinforced resin molded body can be suppressed.
[0049] The release agent is contained in an amount of preferably 1 part by mass or more, and more preferably 3 parts by mass or more, based on the total amount of the epoxy resin and the epoxy diluent, and more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, based on the total amount of the epoxy resin and the epoxy diluent.
[0050] (Method for preparing resin composition) In the method for preparing the resin composition, first, the above-mentioned epoxy resin, epoxy diluent, curing agent, and other optional additives are weighed out so as to obtain the above-mentioned predetermined mass ratio. Then, the weighed components are kneaded using any device known to those skilled in the art to obtain the resin composition.
[0051] (Physical Properties of Resin Composition) The viscosity of the resin composition is 1000 mPa·s or less. When the viscosity of the resin composition is 1000 mPa·s or less, the reinforcing fibers can be impregnated with the resin composition well, and after curing, a well-formed fiber-reinforced resin molding can be obtained.
[0052] The viscosity of the resin composition is preferably 900 mPa·s or less, more preferably 800 mPa·s or less, and even more preferably 700 mPa·s or less. The lower limit of the viscosity of the resin composition is not particularly limited as long as a fiber-reinforced resin molded product can be finally obtained, but may be, for example, 100 mPa·s or more.
[0053] In this specification, the term "viscosity of a resin composition" refers to the initial viscosity of the resin composition. Specifically, as described in detail in the Examples below, the term "viscosity of a resin composition" refers to the viscosity at 25° C. measured immediately after the preparation of the resin composition.
[0054] The glass transition temperature Tg of the resin composition is 110° C. or lower. If the glass transition temperature Tg of the resin composition is 110° C. or lower, the crosslink density is reduced, resulting in toughness, which is preferable because cracks and burrs are prevented when a drill screw is screwed in. In this specification, the "glass transition temperature Tg" refers to a temperature measured using a differential scanning calorimeter (DSC), as will be described in detail in the following examples.
[0055] The glass transition temperature Tg of the resin composition is preferably 100° C. or lower, and more preferably 80° C. or lower. The lower limit of the glass transition temperature Tg of the resin composition is not particularly limited, but may be, for example, 50° C. or higher.
[0056] <Reinforced fiber> The reinforcing fibers are used to improve the strength of the fiber-reinforced resin molded product. Specifically, the reinforcing fibers are impregnated with the above-mentioned resin composition, and after curing, the resin composition and the reinforcing fibers are integrated together.
[0057] The type of reinforcing fiber is not particularly limited as long as it is any fiber known to those skilled in the art as a reinforcing fiber constituting a fiber-reinforced resin molded body. Examples of reinforcing fibers include carbon fiber, glass fiber, boron fiber, alumina fiber, silicon nitride fiber, basalt fiber, etc. These reinforcing fibers may be used in combination of one or more types. Among these, from the viewpoint of specific strength and specific elasticity, it is preferable that the reinforcing fiber contains one or more of carbon fiber, glass fiber, boron fiber, alumina fiber, and silicon nitride fiber. Furthermore, since the strength and corrosion resistance of the fiber-reinforced resin molded body can be further improved, it is more preferable that the reinforcing fiber is carbon fiber. As the carbon fiber, PAN (polyacrylonitrile)-based carbon fiber, pitch-based carbon fiber, etc. can be used. Among these, it is particularly preferable to use PAN-based carbon fiber as the carbon fiber from the viewpoint of particularly high strength. In addition, when carbon fiber is used as the reinforcing fiber, the carbon fiber may be surface-treated with a metal.
[0058] In the fiber reinforced resin molded body of this embodiment, the volume fraction Vf of the reinforcing fibers relative to the entire fiber reinforced resin molded body is preferably 70% or less. If the volume fraction Vf of the reinforcing fibers is 70% or less, it is possible to avoid the occurrence of cracks due to the resin ratio in the fiber reinforced resin molded body becoming too low. The volume fraction Vf of the reinforcing fibers is more preferably 68% or less, and even more preferably 65% or less.
[0059] The lower limit of the volume fraction Vf of the reinforcing fibers is not particularly limited as long as the fiber-reinforced resin molding has sufficient strength, but may be about 45%. If the volume fraction Vf of the reinforcing fibers is 45% or more, the fiber-reinforced resin molding is sufficiently reinforced by the reinforcing fibers, so that excessive reduction in strength such as bending strength of the fiber-reinforced resin molding can be avoided. The volume fraction Vf of the reinforcing fibers is preferably 48% or more, and more preferably 50% or more.
[0060] In this specification, the "volume fraction Vf of reinforcing fibers" is a value measured by a combustion method.
[0061] 2. Manufacturing method of fiber-reinforced resin molding The fiber-reinforced resin molded article in this embodiment can be produced by curing the resin composition impregnated with the reinforcing fibers described above at a mold temperature of 65° C. to 300° C. for 1 minute to 10 minutes.
[0062] The method of impregnating the reinforcing fiber with the resin composition is not particularly limited, and any method known to those skilled in the art can be adopted. For example, the bundle of reinforcing fibers may be immersed in a container containing the resin composition, or the bundle of reinforcing fibers may be coated with the resin composition.
[0063] The mold used for curing is not particularly limited. For example, a die having a through hole into which the resin composition can be poured and through which a bundle of reinforcing fibers can pass, or a mold such as an injection mold into which reinforcing fibers and resin fibers can be poured can be used.
[0064] More specifically, the fiber-reinforced resin molded body in this embodiment can be manufactured by applying a pultrusion method, a VaRTM (Vacuum assisted Resin Transfer Molding) molding method, or the like.
[0065] In the pultrusion molding method, first, a mixture in which the reinforcing fiber, which is a base material, is impregnated with the resin composition is drawn into the inside of a mold, or the reinforcing fiber is impregnated with the resin composition in the mold. Next, the resin composition is heated and cured in the mold or at a place where it is removed from the mold, and the obtained cured product is pulled out from the mold. When the pultrusion molding method is applied in the production of the fiber-reinforced resin molded body in this embodiment, the mold temperature is preferably 100°C to 250°C. When the mold temperature is 100°C or higher, the resin composition can be quickly cured within a moldable time. When the mold temperature is 250°C or lower, the deterioration of physical properties due to thermal decomposition of the resin can be avoided. In addition, by applying the pultrusion molding method in this temperature range, the curing can be completed in about 1 minute to 10 minutes.
[0066] The VaRTM molding method is a molding method using a mold to which a plastic film is attached. In the VaRTM molding method, first, the laminated reinforcing fibers are sealed between the mold and the plastic film, and the air between them is discharged by a vacuum pump. Next, a resin composition is injected into the space from which the air has been discharged using negative pressure, and the reinforcing fibers are impregnated with the resin composition. Thereafter, the reinforcing fibers and the resin composition are sandwiched between the mold and the plastic film, and cured into a desired shape. In the production of the fiber-reinforced resin molded body in this embodiment, when the VaRTM molding method is applied, the mold temperature (mold temperature) is preferably 65°C to 300°C. In addition, curing can be completed in about 1 minute to 15 minutes after the reinforcing fibers are impregnated with the resin composition.
[0067] 3. Physical properties of fiber-reinforced plastic moldings The fiber reinforced resin molded product in this embodiment preferably has a flexural modulus of 130 GPa or more. In this specification, "flexural modulus of (fiber reinforced resin molded product) 130 GPa or more" means that the flexural modulus measured by carrying out a three-point bending test in accordance with JIS K 7074-1988 is 130 GPa or more, as will be described in detail in the examples below.
[0068] Furthermore, the fiber reinforced resin molding in this embodiment preferably has a bending strength of 1000 MPa or more. In this specification, "(fiber reinforced resin molding) bending strength of 1000 MPa or more" means that the bending strength measured by carrying out a three-point bending test in accordance with JIS K 7074-1988 is 1000 MPa or more, as will be described in detail in the examples below.
[0069] In this way, the fiber-reinforced resin molded body in this embodiment has excellent processability while maintaining good bending strength and bending modulus because the epoxy resin and the epoxy diluent are adjusted within a specific ratio range, and at least one of the epoxy diluent and the acid anhydride each contains a specific compound. Therefore, even if the fiber-reinforced resin molded body is fixed to another fiber-reinforced resin molded body or to another material by screwing, or even if a hole is drilled in the fiber-reinforced resin molded body, cracks and burrs are unlikely to occur. Therefore, the fiber-reinforced resin molded body in this embodiment can be suitably used in actual construction sites as a building material such as a siding support, a siding, a ceiling board, and a brace, just like an aluminum base material. EXAMPLES
[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0071] In this example, various resin compositions were prepared by changing the types of epoxy resin, epoxy diluent, and curing agent contained in the resin composition and their blending amounts. Then, test pieces of various fiber-reinforced resin molded bodies were prepared. Furthermore, the physical properties (initial viscosity and glass transition temperature Tg) of the resin composition were measured, and bending tests and processability tests (screw driving tests and hole drilling tests) were performed using the test pieces of the fiber-reinforced resin molded bodies. In addition, although it is not related to the problem to be solved by the present invention, the moldability of the fiber-reinforced resin molded body was also evaluated by observing the test pieces as a reference test.
[0072] In this example, the glass transition temperature Tg of the resin composition was measured by a differential scanning calorimeter (DSC). The initial viscosity of the resin composition was measured at 25°C immediately after the preparation of the resin composition using a B-type viscometer. The volume content (%) of carbon fiber was measured by a combustion method.
[0073] First, the materials used in preparing the test pieces of the fiber-reinforced resin moldings of the respective Examples and Comparative Examples and the method of preparing the test pieces will be described in detail below.
[0074] <Materials for test pieces of fiber-reinforced resin moldings and method for preparing test pieces> (material) The materials used in producing the test pieces of the fiber-reinforced resin moldings and shown in Tables 1 and 2 below are as follows. Bisphenol F type epoxy resin: "EPICLON830" (registered trademark), manufactured by DIC Corporation (epoxy equivalent: 171) Bisphenol A epoxy resin: "EPICLON850" (registered trademark), manufactured by DIC Corporation (epoxy equivalent: 189) Epoxy diluent 1: Dibasic acid glycidyl ester with 18 carbon atoms (specifically, isoeicosanedioic acid bis(2,3-epoxypropyl)), "SB-20G", manufactured by Okamura Oil Mills Co., Ltd. (epoxy equivalent: 285) Epoxy diluent 2: Dibasic acid glycidyl ester having 20 carbon atoms (specifically, isodocosadienedioic acid bis(2,3-epoxypropyl)), "IPU-22G", manufactured by Okamura Oil Mills Co., Ltd. (epoxy equivalent: 290) Epoxy diluent 3: 1,6-hexanediol glycidyl ether with 6 carbon atoms, Denacol "EX-212", manufactured by Nagase ChemteX Corporation (epoxy equivalent: 151) Hardener 1: Methyltetrahydrophthalic anhydride, "HN-2200", manufactured by Resonac Co., Ltd. (hydroxyl equivalent: 168) Hardener 2: Polyanhydride of a branched long-chain dibasic acid having 20 carbon atoms between ester groups, "IPU-22AH" manufactured by Okamura Oil Mills (hydroxyl equivalent: 290) Curing accelerator: 1-cyanoethyl-2-ethyl-4-methylimidazole, Curesol (registered trademark) "2E4MZ-CN", manufactured by Shikoku Chemical Industry Co., Ltd. Release agent: Aliphatic amine-based release agent, MoldWiz (registered trademark) "INT-1888LE", manufactured by Axel Plastics Research Laboratories Carbon fiber: TORAYCA (registered trademark) "T700S-24K" (fiber diameter 7 μm, fineness: 1650 tex), manufactured by Toray Industries, Inc. Vinyl ester resin: Lipoxy R-806, manufactured by Showa Denko K.K.
[0075] Example 1 In Example 1, a resin composition was prepared by mixing bisphenol F type epoxy resin, epoxy diluent 1, curing agent 1, curing accelerator, and release agent in the ratio shown in Table 1 below. The initial viscosity and glass transition temperature Tg of the obtained resin composition were measured. The measurement results are also shown in Table 1 below.
[0076] Carbon fibers were used as the reinforcing fibers. The resin composition prepared as above was impregnated with reinforcing fibers, and the resin composition and reinforcing fibers were filled in a mold and held for a predetermined time. The resin composition was cured and then pulled out to obtain a fiber-reinforced resin molded body (pultrusion molding method). The mold temperature was 180°C, and the holding time in the mold was 2 minutes. The obtained rectangular fiber-reinforced resin molded body was cut to prepare test pieces of fiber-reinforced resin molded bodies (for example, test pieces with a size of 100 mm (length) x 15 mm (width) x 2 mm (thickness)) to be used in each test later.
[0077] The volume fraction Vf of the reinforcing fiber (carbon fiber) in the test piece of the fiber-reinforced resin molding produced was 65%. In all examples and comparative examples, the amount of reinforcing fiber impregnated into the resin composition was adjusted so that the volume fraction Vf of the reinforcing fiber was 65%.
[0078] (Examples 2 to 7) In Examples 2 to 7, the materials were mixed in the ratios shown in Table 1 below to prepare resin compositions. Thereafter, similarly to Example 1, the initial viscosity and glass transition temperature Tg of the resin compositions were measured. The measurement results are also shown in Table 1 below. Furthermore, in the same manner as in Example 1, the resin compositions impregnated with the reinforcing fibers were cured, and finally, test pieces of fiber-reinforced resin moldings of the same size as in Example 1 were obtained.
[0079] (Comparative Examples 1 to 5) In Comparative Examples 1 to 5, the materials were mixed in the ratios shown in Table 2 below to prepare resin compositions. Thereafter, similarly to Example 1, the initial viscosity and glass transition temperature Tg of the resin compositions were measured. The measurement results are also shown in Table 2 below. Furthermore, in the same manner as in Example 1, the resin compositions impregnated with the reinforcing fibers were cured, and finally, test pieces of fiber-reinforced resin moldings of the same size as in Example 1 were obtained.
[0080] (Example for comparison) As a comparative reference example, a vinyl ester resin composition was prepared by blending 100 parts by mass of a vinyl ester resin ("Lipoxy R-806", Showa Denko K.K.), 1 part by mass of another curing agent ("Trigonox 121-50E"), 1 part by mass of yet another curing agent ("Trigonox 129-75"), and 0.5 parts by mass of another mold release agent (MoldWiz (registered trademark) "INT-PUL24", Axel Plastics Research Laboratories) in the ratio shown in Table 2 below. In addition, fiber-reinforced resin molded bodies using vinyl ester resins are generally often used as building materials such as undercoats for ceiling structures, as with epoxy resins. Therefore, they were used as a reference when evaluating bending tests and processability tests. As in Example 1, the initial viscosity and glass transition temperature Tg of the resin composition were measured. The measurement results are also shown in Table 2 below. Furthermore, the resin composition impregnated with the reinforcing fibers was cured in the same manner as in Example 1, and finally test pieces of various fiber-reinforced resin moldings of the same size as in Example 1 were obtained.
[0081] (Reference Example 1 and Reference Example 2) As a reference example, a resin composition was prepared in which the ratio of the hydroxyl equivalent of the acid anhydride to the epoxy equivalent was changed compared to other examples and comparative examples. Specifically, the materials were mixed in the ratios shown in Table 2 below to prepare a resin composition. Thereafter, the initial viscosity and glass transition temperature Tg of the resin composition were measured in the same manner as in Example 1. The measurement results are also shown in Table 2 below. Furthermore, the resin composition impregnated with the reinforcing fibers was cured in the same manner as in Example 1, and finally a test piece of a fiber-reinforced resin molding of the same size as in Example 1 was obtained.
[0082] The following Tables 1 and 2 show the compounding ratios and physical properties of the resin compositions of the above-mentioned Examples and Comparative Examples, as well as the physical properties of the fiber-reinforced resin molded articles.
[0083] [Table 1]
[0084] [Table 2]
[0085] In Table 2, the "60 downward arrow" indicates that the glass transition temperature Tg was too low, so that no peak was observed in DSC and the value of the glass transition temperature Tg could not be calculated accurately. Specifically, it means that the glass transition temperature Tg was determined to be lower than 60°C of Example 1, which was the lowest value among the measured examples.
[0086] Next, a bending test method using test pieces of a fiber-reinforced resin molded body, a processability test method (screw driving test method and hole drilling test method), and a method for evaluating moldability as a reference evaluation will be described in detail below.
[0087] <Bending test method> Using test pieces of the fiber-reinforced resin molded body having a size of 100 mm (length) × 15 mm (width) × 2 mm (thickness) produced in each of the above examples and comparative examples, a three-point bending test was carried out in accordance with JIS K 7074-1988 to measure the bending strength and bending modulus of the fiber-reinforced resin molded body. As long as there was no significant difference in the numerical values compared to the bending strength and bending modulus of the comparative reference example, it was evaluated that the fiber-reinforced resin molded body maintained good bending strength and bending modulus.
[0088] <Processability test method> (Screw driving test method) The screw driving test was carried out by the following method. A drill screw was screwed into a test piece of a fiber-reinforced resin molding having a size of 500 mm (length) × 30 mm (width) × 2 mm (thickness) produced in each of the above examples and comparative examples. The vicinity of the protruding tip of the screw of the test piece was then observed. A test piece without cracks or burrs was judged as "◯" (excellent workability), and a test piece with cracks or burrs was judged as "×" (poor workability).
[0089] (Drilling test method) The hole drilling test was carried out by the following method. A hole with a diameter of 3 mm was drilled in a test piece of a fiber-reinforced resin molding having a size of 500 mm (length) × 30 mm (width) × 2 mm (thickness) produced in each of the above examples and comparative examples. After that, the vicinity of the opening of the test piece was observed. When no cracks or burrs occurred in the test piece, it was judged as "◯" (excellent workability), and when cracks or burrs occurred in the test piece, it was judged as "×" (poor workability).
[0090] <Method of evaluating moldability> The moldability of the fiber-reinforced resin molding (or its test piece) as a reference evaluation was evaluated by the following method. The fiber-reinforced resin molding (or its test piece) produced in each of the above examples and comparative examples was visually observed to check for the presence or absence of defects such as surface defects due to poor curing, cracks, etc. If no defects were found, the moldability of the fiber-reinforced resin molding (or its test piece) was evaluated as "good", and if defects were found, the moldability of the fiber-reinforced resin molding (or its test piece) was evaluated as "not good".
[0091] The following Tables 3 and 4 summarize the results of the bending test, the processability test (screw driving test and hole drilling test) and the moldability evaluation as a reference evaluation of the fiber-reinforced resin molded bodies of the above-mentioned respective Examples and Comparative Examples.
[0092] [Table 3]
[0093] [Table 4]
[0094] <Consideration> As shown in Table 3 above, the fiber-reinforced resin moldings of Examples 1 to 7 all had excellent processability while maintaining good flexural modulus and flexural strength. Furthermore, the moldability as a reference evaluation was also good.
[0095] On the other hand, as shown in Table 4 above, the processability of the fiber-reinforced resin moldings was poor in Comparative Examples 1 and 2. This is presumably because Comparative Examples 1 and 2 did not contain an epoxy diluent in the resin composition, and did not contain a polyacid polyanhydride having 7 or more carbon atoms in the main chain as a curing agent.
[0096] The processability of the fiber-reinforced resin molding was poor in Comparative Example 3. This is presumably because the amount of epoxy diluent 1, i.e., the amount of dibasic acid glycidyl ester having 18 carbon atoms, in the resin composition in Comparative Example 3 was too small.
[0097] The bending strength of the fiber-reinforced resin molding was significantly poor in Comparative Example 4. This is presumably because the amount of epoxy diluent 1, i.e., the amount of dibasic acid glycidyl ester having 18 carbon atoms, in the resin composition in Comparative Example 4 was excessively large.
[0098] The processability of the fiber-reinforced resin molding was poor in Comparative Example 5. This is presumably because Comparative Example 5 contains only epoxy diluent 3, which is not a bifunctional glycidyl-based compound having 7 or more carbon atoms and oxygen atoms constituting the main chain between glycidyl groups, as the epoxy diluent in the resin composition, and does not contain a polyacid polyanhydride having 7 or more carbon atoms in the main chain as the curing agent.
[0099] In Reference Example 1, the moldability was not good as a reference evaluation, and curing failure occurred. This is presumably because the ratio of the hydroxyl group equivalent of the acid anhydride to the epoxy equivalent in Reference Example 1 was less than 0.8.
[0100] In Reference Example 2, the moldability was not good as a reference evaluation, and surface defects occurred. This is presumably because the ratio of the hydroxyl group equivalent of the acid anhydride to the epoxy equivalent in Reference Example 2 was more than 1.1.
Claims
1. A fiber-reinforced resin molded body is obtained by impregnating reinforcing fibers with a resin composition containing an epoxy resin, an epoxy diluent, and a curing agent, and curing the resin composition. the resin composition contains 30 parts by mass or more and 80 parts by mass or less of the epoxy resin and 20 parts by mass or more and 70 parts by mass or less of the epoxy diluent relative to 100 parts by mass in total of the epoxy resin and the epoxy diluent, contains an acid anhydride as the curing agent, has a viscosity of 1000 mPa s or less, and has a glass transition temperature Tg of 110° C. or less; The fiber-reinforced resin molding, wherein the epoxy diluent contains a bifunctional glycidyl compound having a total number of carbon atoms and oxygen atoms constituting the main chain between glycidyl groups of 7 or more, and / or the acid anhydride contains a polyacid polyanhydride having a main chain of 7 or more carbon atoms.
2. The fiber-reinforced resin molding according to claim 1, wherein the ratio of the hydroxyl equivalent of the acid anhydride to the total epoxy equivalent of the epoxy resin and the epoxy diluent is 0.8 to 1.
1.
3. The fiber-reinforced resin molding according to claim 1 or 2, having a flexural modulus of 130 GPa or more and a flexural strength of 1000 MPa or more.
4. The fiber-reinforced resin molding according to claim 1 or 2, which is a building material.
Citation Information
Patent Citations
Epoxy resin composition
JP1998036638A
Fiber-reinforced resin molding and method for manufacturing the same
JP2022158205A
Ceiling structure
JP6504966B2