Release agent composition, laminate, and method for manufacturing processed semiconductor substrate or electronic device layer
A release agent composition with branched polysilane and antioxidants enhances storage stability and releasability, addressing the challenges of wafer deformation during polishing for three-dimensional semiconductor stacking.
Patent Information
- Application Number
- JP2023045580
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing release agent compositions for semiconductor wafers lack sufficient storage stability and effective releasability after polishing, leading to potential deformation or damage during the polishing process for three-dimensional stacking.
A release agent composition comprising an organic resin, branched polysilane, and antioxidants, such as phenolic, amine, phosphoric acid, and sulfide antioxidants, is used to form a laminate with a release layer that maintains adhesion during polishing and ensures easy separation post-polishing, while enhancing storage stability.
The composition provides a release agent with improved storage stability and effective releasability, allowing for the successful separation of semiconductor wafers without deformation, thus facilitating the manufacturing of processed semiconductor substrates.
Smart Images

Figure 2024135070000065 
Figure 2024135070000066 
Figure 2024135070000067
Abstract
Description
[Technical field]
[0001] The present invention relates to stripper compositions, laminates, and methods for producing processed semiconductor substrates or electronic device layers. [Background technology]
[0002] Conventionally, semiconductor wafers have been integrated in a two-dimensional plane, but for the purpose of further integration, there is a demand for semiconductor integration technology that integrates (stacks) the plane in a three-dimensional direction. This three-dimensional stacking is a technology that integrates multiple layers while connecting them with through silicon vias (TSVs). When integrating multiple layers, each wafer to be integrated is thinned by polishing the side opposite the circuit surface (i.e., the back side), and the thinned semiconductor wafers are stacked.
[0003] Semiconductor wafers before thinning (also simply referred to as wafers here) are bonded to a support in order to be polished by a polishing device. The bond at this time must be easily peeled off after polishing, and is therefore called temporary bonding. This temporary bonding must be easily removed from the support, and if a large force is applied to remove it, the thinned semiconductor wafer may be cut or deformed, so it is easily removed to prevent such things from happening. However, it is undesirable for the semiconductor wafer to become dislodged or shifted due to the polishing stress when the back surface of the semiconductor wafer is polished. Therefore, the performance required of the temporary bonding is to withstand the stress during polishing and to be easily removed after polishing.
[0004] Patent Document 1 discloses a laminate having a release layer used for the above-mentioned temporary adhesion, in which a branched chain polysilane is used in a release composition that provides the release layer. A laminate formed from such a release composition can maintain good adhesion during polishing, while exhibiting good releasability after cleaning or the like after polishing. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2022 / 019211 Brochure Summary of the Invention [Problem to be solved by the invention]
[0006] As a further required property of the above-mentioned release agent composition, for example, improved storage stability is expected, such as little increase in molecular weight even when stored for a long period of time, etc. Therefore, an object of the present invention is to provide a release agent composition which maintains the above-mentioned adhesion during polishing and good releasability after polishing, while also improving storage stability. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems, and as a result have found that the above problems can be solved, and have completed the present invention having the following gist.
[0008] That is, the present invention includes the following. [1] A semiconductor substrate; A support substrate; A release agent composition for forming a release layer of a laminate having an adhesive layer and a release layer provided between the semiconductor substrate and the support substrate, comprising: A stripping agent composition comprising an organic resin, a branched polysilane, an antioxidant, and a solvent. [2] The stripping agent composition according to [1], wherein the antioxidant is at least one of a phenol-based antioxidant, an amine-based antioxidant, a phosphoric acid-based antioxidant, and a sulfide-based antioxidant. [3] The stripping composition according to [2], wherein the phenol-based antioxidant is a compound having a group represented by formula (1). [ka] (In the formula, R 1 represents an alkyl group having 1 to 10 carbon atoms, R 2 ~R 4each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and * represents a bond.) [4] The stripping composition according to [2] or [3], wherein the amine-based antioxidant is a compound having a group represented by formula (2). [ka] (In the formula, R 5 represents a hydrogen atom, an oxy radical group, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms, and * represents a bond. [5] The stripping agent composition according to any one of [2] to [4], wherein the phosphoric acid-based antioxidant is a compound represented by the following formula (3) or (4), and the sulfide-based antioxidant is a compound represented by the following formula (5) or (6): [ka] (In the formula, R 6 ~R 8 represents an alkyl group having 1 to 12 carbon atoms, or an aryl group which may be substituted with an alkyl group. [ka] (In the formula, R 9 ~R 10 represents an alkyl group having 1 to 12 carbon atoms, or an aryl group which may be substituted with an alkyl group. [ka] (In the formula, R 11 ~R 12 represents an alkyl group having 1 to 12 carbon atoms. [ka] (In the formula, R 13 ~R 16 represents an alkyl group having 1 to 12 carbon atoms. [6] The stripping composition according to any one of [1] to [5], wherein the branched chain polysilane has a structure represented by formula (B): [ka] (In the formula, R B represents a hydrogen atom, a hydroxyl group, a silyl group, or an organic group. [7] R B is a phenyl group. [8] The stripping composition according to any one of [1] to [7], wherein the organic resin is a novolak resin. [9] The stripping composition according to [8], wherein the novolak resin is a polymer containing one or more units selected from the group consisting of units represented by formula (C1-1), units represented by formula (C1-2), and units represented by formula (C1-3). [ka] (In the formula, C 1 represents a group derived from an aromatic compound containing a nitrogen atom, C 2 represents a group containing a tertiary carbon atom having at least one member selected from the group consisting of a secondary carbon atom, a quaternary carbon atom, and an aromatic ring in a side chain, 3 represents a group derived from an aliphatic polycyclic compound, C 4 represents a group derived from phenol, a group derived from bisphenol, a group derived from naphthol, a group derived from biphenyl, or a group derived from biphenol.
[10] The stripping composition according to any one of [1] to [9], which contains a crosslinking agent.
[11] A semiconductor substrate or an electronic device layer; A support substrate; a release agent layer provided between the semiconductor substrate or the electronic device layer and the support substrate; The release agent layer is a laminate formed from the release agent composition according to any one of [1] to
[10] .
[12] The laminate according to
[11] , further comprising an adhesive layer provided between the semiconductor substrate or the electronic device layer and the supporting substrate.
[13] A method for producing a processed semiconductor substrate or electronic device layer, comprising the steps of: A step 5A in which the semiconductor substrate of the laminate according to
[11] or
[12] is processed, or a step 5B in which the electronic device layer of the laminate according to
[11] is processed; a step 6A in which the semiconductor substrate processed in the step 5A is separated from the support substrate, or a step 6B in which the electronic device layer processed in the step 5B is separated from the support substrate; 2. A method for producing a processed semiconductor substrate or electronic device layer, comprising:
[14] The method for producing a processed semiconductor substrate or electronic device layer according to
[13] , wherein the supporting substrate is optically transparent, and step 6A or step 6B includes a step of irradiating the laminate with a laser from the supporting substrate side. Effect of the Invention
[0009] According to the present invention, it is possible to provide a release agent composition having good release properties and excellent long-term storage stability, as well as a method for producing a laminate and a processed semiconductor using the release agent composition. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of an example of a laminate according to the first embodiment. [Figure 2A] FIG. 2A is a schematic cross-sectional view (part 1) illustrating a method for producing a laminate showing one example of the first embodiment. [Figure 2B] FIG. 2B is a schematic cross-sectional view (part 2) illustrating a method for producing a laminate showing one example of the first embodiment. [Figure 2C] FIG. 2C is a schematic cross-sectional view (part 3) illustrating an example of a method for producing a laminate according to the first embodiment. [Diagram 3] FIG. 3 is a schematic cross-sectional view of an example of a laminate in the second embodiment. [Figure 4] FIG. 4 is a schematic cross-sectional view of another example of the laminate in the second embodiment. [Figure 5A]FIG. 5A is a schematic cross-sectional view (part 1) illustrating a method for producing a laminate showing one example of the second embodiment. [Figure 5B] FIG. 5B is a schematic cross-sectional view (part 2) illustrating a method for producing a laminate showing one example of the second embodiment. [Figure 5C] FIG. 5C is a schematic cross-sectional view (part 3) illustrating an example of the method for producing a laminate according to the second embodiment. [Figure 5D] FIG. 5D is a schematic cross-sectional view (part 4) illustrating a method for producing a laminate showing one example of the second embodiment. [Figure 6A] FIG. 6A is a schematic cross-sectional view (part 1) illustrating a method for processing a laminate showing one example of the first embodiment. [Figure 6B] FIG. 6B is a schematic cross-sectional view (part 2) illustrating a method for processing the laminate showing one example of the first embodiment. [Figure 6C] FIG. 6C is a schematic cross-sectional view (part 3) illustrating a method for processing a laminate showing one example of the first embodiment. [Figure 6D] FIG. 6D is a schematic cross-sectional view (part 4) illustrating a method for processing a laminate showing one example of the first embodiment. [Figure 7A] FIG. 7A is a schematic cross-sectional view (part 1) illustrating a method for processing a laminate showing one example of the second embodiment. [Figure 7B] FIG. 7B is a schematic cross-sectional view (part 2) illustrating a method for processing a laminate showing one example of the second embodiment. [Figure 7C] FIG. 7C is a schematic cross-sectional view (part 3) illustrating a method for processing a laminate showing one example of the second embodiment. [Figure 7D] FIG. 7D is a schematic cross-sectional view (part 4) illustrating a method for processing a laminate showing one example of the second embodiment. [Figure 7E] FIG. 7E is a schematic cross-sectional view (part 5) illustrating a method for processing a laminate showing one example of the second embodiment. [Figure 7F]FIG. 7F is a schematic cross-sectional view (part 6) illustrating a method for processing a laminate showing one example of the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] (Removal agent composition) The release agent composition of the present invention contains an organic resin, a branched polysilane, an antioxidant, and a solvent. The release agent composition is a release agent composition for forming a release layer of a laminate having a semiconductor substrate, a support substrate, and an adhesive layer and a release layer provided between the semiconductor substrate and the support substrate.
[0012] <Antioxidants> The antioxidant may be appropriately selected depending on the type of organic resin, the storage temperature of the stripping composition, etc. One or more types of antioxidant may be contained, and two or more types may be used. Examples of the antioxidant include at least one of phenol-based antioxidants, amine-based antioxidants, phosphoric acid-based antioxidants, and sulfide-based antioxidants. The stripping composition of the present invention containing an antioxidant exhibits good stability even when stored for a long period of time, such as 2 weeks to 1 month, without a significant increase in the molecular weight of the stripping composition.
[0013] The amount of the antioxidant in the stripping composition of the present invention can be appropriately determined. The amount of the antioxidant may be, for example, 0.001 to 80 mass% relative to the amount of the branched chain polysilane, and from the viewpoint of further suppressing the increase in the molecular weight of the branched chain polysilane, it is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and even more preferably 0.5 mass% or more. It is also good to have it 30 mass% or less, preferably 25 mass% or less, more preferably 20 mass% or less, even more preferably 15 mass% or less, and even more preferably 10 mass% or less.
[0014] <<Phenol-based antioxidants>> The phenol-based antioxidant is a compound having a phenol group, and examples thereof include compounds having a group represented by formula (1). [ka] (In the formula, R 1 represents an alkyl group having 1 to 10 carbon atoms, R 2 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and * represents a bond.) In addition, the bond * in the formula may be bonded to a hydrogen atom, or to an atom or group other than a hydrogen atom.
[0015] In formula (1), R 1 ~R 4 Examples of the alkyl group having 1 to 10 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isoamyl group, a neopentyl group, a tert-amyl group, a sec-isoamyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. R 1 As the alkyl group, a tert-butyl group is preferable. Examples of such a group represented by formula (1) include a 3-tert-butyl-4-hydroxy-5-methylphenyl group, a 3-tert-butyl-4-hydroxy-6-methylphenyl group, a 3,5-di-tert-butyl-4-hydroxyphenyl group, etc. The phenol-based antioxidant is different from the phenol-based crosslinking agent described later.
[0016] The molecular weight of the phenol-based antioxidant is not particularly limited, but is preferably 50 to 1,000, and more preferably 100 to 300.
[0017] Examples of phenolic antioxidants include compounds having the following structures: [ka] [ka] [ka]
[0018] <<Amine-based antioxidants>> Amine antioxidants are N, NH or NO · Examples of the compound include a group represented by hindered amine and a compound having a nitroxyl radical group called TEMPO. The amine-based antioxidant includes, for example, a compound having a group represented by formula (2). [ka] (In the formula, R 5 represents a hydrogen atom, an oxy radical group (-O·), an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms, and * represents a bond. In addition, the bond * in the formula may be bonded to a hydrogen atom, or to an atom or group other than a hydrogen atom.
[0019] In formula (2), R 5 Examples of the alkyl group having 1 to 10 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isoamyl group, a neopentyl group, a tert-amyl group, a sec-isoamyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. R 5Examples of the alkoxy group having 1 to 12 carbon atoms represented by the formula (I) include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, a tert-butoxy group, an n-pentyloxy group, an isoamyloxy group, a neopentyloxy group, a tert-amyloxy group, a sec-isoamyloxy group, a cyclopentyloxy group, an n-hexyloxy group, a cyclohexyloxy group, an n-heptyloxy group, an n-octyloxy group, an n-nonyloxy group, an n-decyloxy group, and an n-undecyloxy group. R 5 is preferably a hydrogen atom, an oxy radical group, a methyl group, a cyclohexyloxy group, or an n-octyloxy group, and particularly preferably a hydrogen atom, an oxy radical group, or a methyl group.
[0020] The molecular weight of the amine-based antioxidant is not particularly limited, but is preferably 50 to 1,000, and more preferably 100 to 600.
[0021] Examples of the amine-based antioxidant include compounds having the following structures: [ka] [ka]
[0022] <<Phosphate-based antioxidants>> The phosphoric acid-based antioxidant is a compound having phosphoric acid or a phosphoric acid such as phosphoric acid, polyphosphoric acid, or metaphosphoric acid, and examples thereof include compounds having a group represented by formula (3) or (4). [ka] (In the formula, R 6 ~R 8 represents an alkyl group having 1 to 12 carbon atoms, or an aryl group which may be substituted with an alkyl group. [ka] (In the formula, R 9 ~R 10 represents an alkyl group having 1 to 12 carbon atoms, or an aryl group which may be substituted with an alkyl group.
[0023] R in Equation (3) 6 ~R 8 , and R in formula (4) 9 ~R 10 Examples of the alkyl group having 1 to 12 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isoamyl group, a neopentyl group, a tert-amyl group, a sec-isoamyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. R 6 ~R 10 The aryl group which may be substituted with an alkyl group represented by the formula (I) may have at least one aromatic ring, and examples thereof include a phenyl group, a methylphenyl group, a tert-butylphenyl group, and a di-tert-butylphenyl group.
[0024] Examples of the phosphoric acid-based antioxidant include compounds having the following structures: [ka] [ka]
[0025] <<Sulfide-based antioxidants>> The sulfide-based antioxidant is a compound having a group represented by sulfide (thioether), and examples thereof include compounds having a group represented by formula (5) or formula (6). [ka] (In the formula, R 11 ~R 12represents an alkyl group having 1 to 12 carbon atoms. [ka] (In the formula, R 13 ~R 16 represents an alkyl group having 1 to 12 carbon atoms.
[0026] R in Equation (5) 11 ~R 12 , and R in formula (6) 13 ~R 16 Examples of the alkyl group having 1 to 12 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isoamyl group, a neopentyl group, a tert-amyl group, a sec-isoamyl group, a cyclopentyl group, an n-hexyl group, a cyclohexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, and an n-dodecyl group. The above R 11 ~R 16 As the alkyl group, an n-dodecyl group is preferable.
[0027] Examples of the sulfide-based antioxidant include compounds having the following structure: [ka]
[0028] <Organic resin> The release agent composition contains an organic resin. Such an organic resin is preferably one that can exhibit suitable release ability, and when the semiconductor substrate and the support substrate are separated by irradiating the release layer with light, the organic resin is one that absorbs light and preferably undergoes a change in quality, such as decomposition, required for improving the release ability.
[0029] A preferred example of the organic resin is a novolac resin. When the release layer of the laminate of the present invention is irradiated with light to perform peeling, a novolac resin that absorbs and changes its properties when exposed to light having a wavelength of 190 nm to 600 nm is preferred, and a novolac resin that changes its properties when exposed to light such as a laser having a wavelength of 308 nm, 343 nm, 355 nm, or 365 nm is more preferred. Novolac resins have at least one of a hydroxy group directly bonded to an aromatic ring and a carboxy group directly bonded to an aromatic ring. Novolac resins are resins obtained by, for example, subjecting at least one of a phenolic compound, a carbazole compound, and an aromatic amine compound to a condensation reaction with at least one of an aldehyde compound, a ketone compound, and a divinyl compound in the presence of an acid catalyst.
[0030] Examples of phenolic compounds include phenols, naphthols, anthrols, and hydroxypyrenes. Examples of phenols include phenol, cresol, xylenol, resorcinol, bisphenol A, p-tert-butylphenol, p-octylphenol, 9,9-bis(4-hydroxyphenyl)fluorene, and 1,1,2,2-tetrakis(4-hydroxyphenyl)ethane. Examples of naphthols include 1-naphthol, 2-naphthol, 1,5-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, and 9,9-bis(6-hydroxynaphthyl)fluorene. Examples of anthrols include 9-anthrol. Examples of hydroxypyrenes include 1-hydroxypyrene and 2-hydroxypyrene. Examples of the carbazole compound include carbazole, 1,3,6,8-tetranitrocarbazole, 3,6-diaminocarbazole, 3,6-dibromo-9-ethylcarbazole, 3,6-dibromo-9-phenylcarbazole, 3,6-dibromocarbazole, 3,6-dichlorocarbazole, 3-amino-9-ethylcarbazole, 3-bromo-9-ethylcarbazole, 4,4'bis(9H-carbazol-9-yl)biphenyl, 4-glycidylcarbazole, 4-hydroxycarbazole, 9-(1H-benzotriazol-1-yl)methylcarbazole, 4 ... N-((9-ethylcarbazole-3-yl)methylene)-9H-carbazole, 9-acetyl-3,6-diiodocarbazole, 9-benzoylcarbazole, 9-benzoylcarbazole-6-dicarboxaldehyde, 9-benzylcarbazole-3-carboxaldehyde, 9-methylcarbazole, 9-phenylcarbazole, 9-vinylcarbazole, potassium carbazole, carbazole-N-carbonyl chloride, N-ethylcarbazole-3-carboxaldehyde, N-((9-ethylcarbazole-3-yl)methylene)-2-methyl-1-indolinylamine, and the like. Examples of the aromatic amine compound include diphenylamine and N-phenyl-1-naphthylamine. These may be used alone or in combination of two or more. These may have a substituent, for example, a substituent on the aromatic ring.
[0031] Examples of aldehyde compounds include formaldehyde, paraformaldehyde, acetaldehyde, propylaldehyde, butylaldehyde, isobutyraldehyde, valeraldehyde, capronaldehyde, 2-methylbutyraldehyde, hexylaldehyde, undecanealdehyde, 7-methoxy-3,7-dimethyloctylaldehyde, cyclohexanealdehyde, 3-methyl-2-butyraldehyde, glyoxal, malonaldehyde, succinaldehyde, glutaraldehyde, and adipaldehyde. Examples of the aldehyde include saturated aliphatic aldehydes such as benzene aldehyde, unsaturated aliphatic aldehydes such as acrolein and methacrolein, heterocyclic aldehydes such as furfural and pyridine aldehyde, and aromatic aldehydes such as benzaldehyde, naphthyl aldehyde, anthryl aldehyde, phenanthryl aldehyde, salicyl aldehyde, phenylacetaldehyde, 3-phenylpropionaldehyde, tolyl aldehyde, (N,N-dimethylamino)benzaldehyde, and acetoxybenzaldehyde. Among these, aromatic aldehydes are preferred. Examples of the ketone compound include diaryl ketone compounds such as diphenyl ketone, phenyl naphthyl ketone, dinaphthyl ketone, phenyl tolyl ketone, and ditolyl ketone. Examples of the divinyl compound include divinylbenzene, dicyclopentadiene, tetrahydroindene, 4-vinylcyclohexene, 5-vinylnoborna-2-ene, divinylpyrene, limonene, and 5-vinylnorbornadiene. These may be used alone or in combination of two or more.
[0032] The novolac resin is, for example, a novolac resin that absorbs light irradiated from the support substrate side and changes in quality, for example, by photolysis.
[0033] The novolac resin contains, for example, at least one of a structural unit represented by the following formula (C1-1), a structural unit represented by the following formula (1-2), and a structural unit represented by the following formula (C1-3).
[0034] [ka]
[0035] In the formula, C 1 represents a group derived from an aromatic compound containing a nitrogen atom, C 2 represents a group containing a tertiary carbon atom having at least one member selected from the group consisting of a secondary carbon atom, a quaternary carbon atom, and an aromatic ring in a side chain, 3 represents a group derived from an aliphatic polycyclic compound, C 4 represents a group derived from phenol, a group derived from bisphenol, a group derived from naphthol, a group derived from biphenyl, or a group derived from biphenol.
[0036] That is, the novolac resin contains, for example, one or more of the following structural units: A structural unit having a bond between a group derived from an aromatic compound containing a nitrogen atom and a group containing a tertiary carbon atom having at least one member selected from the group consisting of a secondary carbon atom, a quaternary carbon atom, and an aromatic ring in its side chain (formula (C1-1)). Structural units having a bond between a group derived from an aromatic compound containing a nitrogen atom and a group derived from an aliphatic polycyclic compound (formula (C1-2)) A structural unit having a bond between a group derived from a phenol, a group derived from a bisphenol, a group derived from a naphthol, a group derived from a biphenyl, or a group derived from a biphenol and a group containing a tertiary carbon atom having at least one member selected from the group consisting of a quaternary carbon atom and an aromatic ring in the side chain ((Formula (C1-3))
[0037] In a preferred embodiment, the novolak resin contains either or both of a structural unit (formula (C1-1)) having a bond between a group derived from an aromatic compound containing a nitrogen atom and a group containing a tertiary carbon atom having at least one kind selected from the group consisting of a secondary carbon atom, a quaternary carbon atom, and an aromatic ring in its side chain, and a structural unit (formula (C1-2)) having a bond between a group derived from an aromatic compound containing a nitrogen atom and a group derived from an aliphatic polycyclic compound.
[0038] C 1 Examples of the group derived from an aromatic compound containing a nitrogen atom include, but are not limited to, a group derived from carbazole, a group derived from N-phenyl-1-naphthylamine, a group derived from N-phenyl-2-naphthylamine, and the like. C 2 The group containing a tertiary carbon atom having at least one selected from the group consisting of a secondary carbon atom, a quaternary carbon atom, and an aromatic ring in a side chain thereof can be, for example, a group derived from 1-naphthaldehyde, a group derived from 1-pyrenecarboxaldehyde, a group derived from 4-(trifluoromethyl)benzaldehyde, a group derived from acetaldehyde, etc., but is not limited to these. C 3 The group derived from an aliphatic polycyclic compound may be, but is not limited to, a group derived from dicyclopentadiene. C 4 is a group derived from phenol, a group derived from bisphenol, a group derived from naphthol, a group derived from biphenyl, or a group derived from biphenol.
[0039] In a preferred embodiment, the novolak resin contains, as the structural unit represented by formula (C1-1), for example, a structural unit represented by the following formula (C1-1-1).
[0040] [ka]
[0041] In formula (C1-1-1), R 901 and R 902 represents a substituent substituted on the ring, and each independently represents a halogen atom, a nitro group, a cyano group, an amino group, a hydroxy group, a carboxy group, an optionally substituted alkyl group, an optionally substituted alkenyl group, or an optionally substituted aryl group. R 903 represents a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkenyl group, or an optionally substituted aryl group. R904 represents a hydrogen atom, an optionally substituted aryl group, or an optionally substituted heteroaryl group. R 905 represents an optionally substituted alkyl group, an optionally substituted aryl group, or an optionally substituted heteroaryl group. R 904 Group and R 905 may be bonded to each other to form a divalent group. Substituents for the alkyl and alkenyl groups include halogen atoms, nitro groups, cyano groups, amino groups, hydroxy groups, carboxy groups, aryl groups, and heteroaryl groups. Substituents for the aryl group and heteroaryl group include a halogen atom, a nitro group, a cyano group, an amino group, a hydroxy group, a carboxy group, an alkyl group, and an alkenyl group. h 1 and h 2 each independently represents an integer of 0 to 3.
[0042] The number of carbon atoms in the optionally substituted alkyl group and the optionally substituted alkenyl group is usually 40 or less, and from the viewpoint of solubility, it is preferably 30 or less, and more preferably 20 or less. The number of carbon atoms in the optionally substituted aryl group and heteroaryl group is usually 40 or less, and from the viewpoint of solubility, it is preferably 30 or less, and more preferably 20 or less.
[0043] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0044] Specific examples of the optionally substituted alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2-methyl-n-pentyl group, a 3-methyl-n-pentyl group, Examples of the aryl group include, but are not limited to, a 4-methyl-n-pentyl group, a 1,1-dimethyl-n-butyl group, a 1,2-dimethyl-n-butyl group, a 1,3-dimethyl-n-butyl group, a 2,2-dimethyl-n-butyl group, a 2,3-dimethyl-n-butyl group, a 3,3-dimethyl-n-butyl group, a 1-ethyl-n-butyl group, a 2-ethyl-n-butyl group, a 1,1,2-trimethyl-n-propyl group, a 1,2,2-trimethyl-n-propyl group, a 1-ethyl-1-methyl-n-propyl group, and a 1-ethyl-2-methyl-n-propyl group.
[0045] Specific examples of the optionally substituted alkenyl group include ethenyl, 1-propenyl, 2-propenyl, 1-methyl-1-ethenyl, 1-butenyl, 2-butenyl, 3-butenyl, 2-methyl-1-propenyl, 2-methyl-2-propenyl, 1-ethylethenyl, 1-methyl-1-propenyl, 1-methyl-2-propenyl, 1-pentenyl, 2-pentenyl, 3-pentenyl, 4-pentenyl, 1-n-propylethenyl, 1-methyl-1-butenyl, 1-methyl-2-butenyl, and 1-methyl-3-butenyl. 2-ethyl-2-propenyl group, 2-methyl-1-butenyl group, 2-methyl-2-butenyl group, 2-methyl-3-butenyl group, 3-methyl-1-butenyl group, 3-methyl-2-butenyl group, 3-methyl-3-butenyl group, 1,1-dimethyl-2-propenyl group, 1-i-propylethenyl group, 1,2-dimethyl-1-propenyl group, 1,2-dimethyl-2-propenyl group, 1-cyclopentenyl group, 2-cyclopentenyl group, 3-cyclopentenyl group, 1-hexenyl group, 2-hexenyl group, 3-hexenyl group, 4-hexenyl group, 5-hexenyl group, xenyl group, 1-methyl-1-pentenyl group, 1-methyl-2-pentenyl group, 1-methyl-3-pentenyl group, 1-methyl-4-pentenyl group, 1-n-butylethenyl group, 2-methyl-1-pentenyl group, 2-methyl-2-pentenyl group, 2-methyl-3-pentenyl group, 2-methyl-4-pentenyl group, 2-n-propyl-2-propenyl group, 3-methyl-1-pentenyl group, 3-methyl-2-pentenyl group, 3-methyl-3-pentenyl group, 3-methyl-4-pentenyl group, 3-ethyl-3-butenyl group, 4-methyl-1-pentenyl group, 4-methyl-2-pentenyl group, 4-methyl-3-pentenyl group, 4-methyl-4-pentenyl group, 1,1-dimethyl-2-butenyl group, 1,1-dimethyl-3-butenyl group, 1,2-dimethyl-1-butenyl group, 1,2-dimethyl-2-butenyl group, 1,2-dimethyl-3-butenyl group, 1-methyl-2-ethyl-2-propenyl group, 1-s-butylethenyl group, 1,3-dimethyl-1-butenyl group, 1,3-dimethyl-2-butenyl group, 1,3-dimethyl-3-butenyl group, 1-i-butylethenyl group, 2,2-dimethyl-3-butenyl group, 2,3-dimethyl-1-butenyl group, 2,3-dimethyl-2-butenyl group, 2,3-dimethyl-3-butenyl group, 2-i-propyl-2-propenyl group, 3,3-dimethyl-1-butenyl group, 1-ethyl-1-butenyl group, 1-ethyl-2-butenyl group, 1-ethyl-3-butenyl group, 1-n-propyl-1-propenyl group, 1-n-propyl-2-propenyl group, 2-ethyl-1-butenyl group, 2-ethyl-2-butenyl group, 2-ethyl-3-butenyl group, 1,1,2-trimethyl-2-propenyl group, 1-tert-butylethenyl group, 1-methyl-1-ethyl-2-propenyl group, 1-ethyl-2-methyl-1-propenyl group, 1-ethyl-2-methyl-2-propenyl group, 1-i-propyl-1-propenyl group , 1-i-propyl-2-propenyl group, 1-methyl-2-cyclopentenyl group, 1-methyl-3-cyclopentenyl group, 2-methyl-1-cyclopentenyl group, 2-methyl-2-cyclopentenyl group, 2-methyl-3-cyclopentenyl group, 2-methyl-4-cyclopentenyl group, 2-methyl-5-cyclopentenyl group, 2-methylene-cyclopentyl group, 3-methyl-1-cyclopentenyl group, 3-methyl-2-cyclopentenyl group, 3-methyl-3-cyclopentenyl group, 3-methyl-4-cyclopentenyl group, 3-methyl-5-cyclopentenyl group, 3-methylene-cyclopentyl group, 1-cyclohexenyl group, 2-cyclohexenyl group, 3-cyclohexenyl group, and the like, but are not limited thereto.
[0046] Specific examples of the optionally substituted aryl group include, but are not limited to, a phenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 2-chlorophenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 2-fluorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-nitrophenyl group, a 4-cyanophenyl group, a 1-naphthyl group, a 2-naphthyl group, a biphenyl-4-yl group, a biphenyl-3-yl group, a biphenyl-2-yl group, a 1-anthryl group, a 2-anthryl group, a 9-anthryl group, a 1-phenanthryl group, a 2-phenanthryl group, a 3-phenanthryl group, a 4-phenanthryl group, and a 9-phenanthryl group.
[0047] Specific examples of optionally substituted heteroaryl groups include, but are not limited to, a 2-thienyl group, a 3-thienyl group, a 2-furanyl group, a 3-furanyl group, a 2-oxazolyl group, a 4-oxazolyl group, a 5-oxazolyl group, a 3-isoxazolyl group, a 4-isoxazolyl group, a 5-isoxazolyl group, a 2-thiazolyl group, a 4-thiazolyl group, a 5-thiazolyl group, a 3-isothiazolyl group, a 4-isothiazolyl group, a 5-isothiazolyl group, and the like.
[0048] Specific examples of the structural unit represented by formula (C1-1-1) are listed below, but the structural unit is not limited thereto.
[0049] [ka]
[0050] In a preferred embodiment, the novolak resin contains, as the structural unit represented by formula (C1-1), for example, a structural unit represented by the following formula (C1-1-2).
[0051] [ka]
[0052] In formula (C1-1-2), Ar 901 and Ar 902 each independently represents an aromatic ring such as a benzene ring or a naphthalene ring; R 901 ~R 905 And h 1 and h 2 has the same meaning as above.
[0053] Specific examples of the structural unit represented by formula (C1-1-2) are listed below, but the structural unit is not limited thereto.
[0054] [ka]
[0055] In a preferred embodiment, the novolak resin contains, as the structural unit represented by formula (C1-2), for example, a structural unit represented by the following formula (C1-2-1) or (1-2-2).
[0056] [ka]
[0057] In the above formula, R 906 ~R 909 are substituents bonded to the ring, each independently representing a halogen atom, a nitro group, a cyano group, an amino group, a hydroxy group, a carboxy group, an optionally substituted alkyl group, an optionally substituted alkenyl group, or an optionally substituted aryl group; specific examples and preferred carbon numbers of the halogen atom, the optionally substituted alkyl group, the optionally substituted alkenyl group, and the optionally substituted aryl group are the same as those mentioned above; 3 ~h 6 each independently represents an integer of 0 to 3; R 901 ~R 903 And h 1 and h 2 has the same meaning as above.
[0058] Specific examples of the structural units represented by formulae (C1-2-1) and (C1-2-2) are listed below, but are not limited to these.
[0059] [ka]
[0060] Specific examples of the structural unit represented by formula (C1-3) are listed below, but the structural unit is not limited thereto.
[0061] [ka]
[0062] As described above, the novolac resin is a resin obtained by, for example, subjecting at least one of a phenolic compound, a carbazole compound, and an aromatic amine compound to a condensation reaction with at least one of an aldehyde compound, a ketone compound, and a divinyl compound in the presence of an acid catalyst. In this condensation reaction, for example, the aldehyde compound or ketone compound is usually used in a ratio of 0.1 to 10 equivalents per equivalent of the benzene ring constituting the ring of the carbazole compound.
[0063] <Branched chain polysilane> The stripping composition of the present invention contains a branched polysilane. The branched polysilane has a Si-Si bond and a branched structure. By containing the branched polysilane in the above-mentioned release agent composition, the release agent layer formed of the obtained film cannot be suitably removed by any of organic solvents, acids, and chemical solutions (such as alkaline developer and hydrogen peroxide solution) used in the manufacture of semiconductor elements, but can be suitably removed by the cleaning agent composition. As a result, the semiconductor substrate and the support substrate of the laminate are separated, and then the respective substrates are cleaned with the cleaning agent composition, whereby the residue of the release agent layer on the substrate can be suitably removed. Although the reason for this is not clear, depending on the type of terminal group (terminal substituent (atom)) of the polysilane, the polysilane can react with an organic resin to form crosslinks. Also, since a branched-chain polysilane has more terminal groups (terminal substituent (atom)) than a linear polysilane, the branched-chain polysilane is considered to have more crosslinking points than a linear polysilane. It is speculated that moderate and suitable curing via such a larger number of crosslinking points in the branched-chain polysilane can achieve both the property of being not suitably removed by organic solvents, acids, and chemical solutions used in the production of semiconductor elements (such as alkaline developing solutions and hydrogen peroxide solutions) and the property of being suitably removed by a cleaning composition.
[0064] The branched polysilane preferably contains a structural unit represented by formula (B).
[0065] [ka]
[0066] In formula (B), R Brepresents a hydrogen atom, a hydroxyl group, a silyl group, or an organic group, and specific examples of such an organic group include a hydrocarbon group (an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted aryl group, an optionally substituted aralkyl group), and an ether group corresponding to these hydrocarbon groups (an optionally substituted alkoxy group, an optionally substituted aryloxy group, an optionally substituted aralkyloxy group, etc.), and the organic group is usually often a hydrocarbon group such as an alkyl group, an alkenyl group, an aryl group, or an aralkyl group. In addition, a hydrogen atom, a hydroxyl group, an alkoxy group, a silyl group, etc. are often substituted at the terminal.
[0067] The optionally substituted alkyl group may be linear, branched, or cyclic. Specific examples of the optionally substituted straight-chain or branched-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a tertiary butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2-methyl-n-pentyl group, a 3-methyl-n-pentyl group, a 4-methyl-n-pentyl group, a 5-methyl-n-pentyl group, a 6-methyl-n-pentyl group, a 7-methyl-n-pentyl group, a 8-methyl-n-pentyl group, a 9-methyl-n-pentyl group, a 10-methyl-n-pentyl group, a 11-methyl-n-pentyl group, a 12-methyl-n-pentyl group, a 13-methyl-n-pentyl group, a 14-methyl-n-pentyl group, a 15-methyl-n-pentyl group, a 16-methyl-n-pentyl group, a 17-methyl-n-pentyl group, a 18-methyl-n-pentyl group, a 19-methyl-n-pentyl group, a 20-methyl-n-pentyl group, a 21-methyl-n-pentyl group, a 22-methyl-n-pentyl group, a 23-methyl-n-pentyl group, a 24-methyl-n-pentyl group, a 25-methyl-n-pentyl group, a 26-methyl-n-pentyl group, a 27-methyl-n-pentyl group, a 2 Examples of such aryl groups include, but are not limited to, an ethyl group, a 1,1-dimethyl-n-butyl group, a 1,2-dimethyl-n-butyl group, a 1,3-dimethyl-n-butyl group, a 2,2-dimethyl-n-butyl group, a 2,3-dimethyl-n-butyl group, a 3,3-dimethyl-n-butyl group, a 1-ethyl-n-butyl group, a 2-ethyl-n-butyl group, a 1,1,2-trimethyl-n-propyl group, a 1,2,2-trimethyl-n-propyl group, a 1-ethyl-1-methyl-n-propyl group, and a 1-ethyl-2-methyl-n-propyl group. The number of carbon atoms in the aryl group is usually 1 to 14, preferably 1 to 10, and more preferably 1 to 6. Specific examples of the optionally substituted cyclic alkyl group include a cyclopropyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, a cyclopentyl group, a 1-methyl-cyclobutyl group, a 2-methyl-cyclobutyl group, a 3-methyl-cyclobutyl group, a 1,2-dimethyl-cyclopropyl group, a 2,3-dimethyl-cyclopropyl group, a 1-ethyl-cyclopropyl group, a 2-ethyl-cyclopropyl group, a cyclohexyl group, a 1-methyl-cyclopentyl group, a 2-methyl-cyclopentyl group, a 3-methyl-cyclopentyl group, a 1-ethyl-cyclobutyl group, a 2-ethyl-cyclobutyl group, a 3-ethyl-cyclobutyl group, a 1,2-dimethyl-cyclobutyl group, a 1,3-dimethyl-cyclobutyl group, a 2,2-dimethyl-cyclobutyl group, a 2,3-dimethyl-cyclobutyl group, a 2,4-dimethyl-cyclobutyl group, a 3,3- Examples of cycloalkyl groups include dimethyl-cyclobutyl group, 1-n-propyl-cyclopropyl group, 2-n-propyl-cyclopropyl group, 1-i-propyl-cyclopropyl group, 2-i-propyl-cyclopropyl group, 1,2,2-trimethyl-cyclopropyl group, 1,2,3-trimethyl-cyclopropyl group, 2,2,3-trimethyl-cyclopropyl group, 1-ethyl-2-methyl-cyclopropyl group, 2-ethyl-1-methyl-cyclopropyl group, 2-ethyl-2-methyl-cyclopropyl group, and 2-ethyl-3-methyl-cyclopropyl group; and bicycloalkyl groups such as bicyclobutyl group, bicyclopentyl group, bicyclohexyl group, bicycloheptyl group, bicyclooctyl group, bicyclononyl group, and bicyclodecyl group, but are not limited thereto. The number of carbon atoms is usually 3 to 14, preferably 4 to 10, and more preferably 5 to 6.
[0068] The alkenyl group may be straight-chain, branched-chain, or cyclic. Specific examples of the optionally substituted linear or branched alkenyl group include, but are not limited to, a vinyl group, an allyl group, a butenyl group, and a pentenyl group, and the number of carbon atoms is usually 2 to 14, preferably 2 to 10, and more preferably 1 to 6. Specific examples of the optionally substituted cyclic alkenyl group include, but are not limited to, cyclopentenyl and cyclohexenyl. The number of carbon atoms is usually 4 to 14, preferably 5 to 10, and more preferably 5 to 6.
[0069] Specific examples of the optionally substituted aryl group include, but are not limited to, a phenyl group, a 4-methylphenyl group, a 3-methylphenyl group, a 2-methylphenyl group, a 3,5-dimethylphenyl group, a 1-naphthyl group, and a 2-naphthyl group. The number of carbon atoms is usually 6 to 20, preferably 6 to 14, and more preferably 6 to 12.
[0070] Specific examples of the aralkyl group which may be substituted include, but are not limited to, a benzyl group, a phenethyl group, a phenylpropyl group, etc. The aralkyl group which may be substituted is preferably a group in which one hydrogen atom of an alkyl group having 1 to 4 carbon atoms is substituted with an aryl group having 6 to 20 carbon atoms.
[0071] The alkyl moiety of the optionally substituted alkoxy group may be straight-chain, branched-chain, or cyclic. Specific examples of the optionally substituted linear or branched alkoxy group include, but are not limited to, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a t-butoxy group, and a pentyloxy group. The number of carbon atoms is usually 1 to 14, preferably 1 to 10, and more preferably 1 to 6. Specific examples of the optionally substituted cyclic alkoxy group include, but are not limited to, cyclopentyloxy and cyclohexyloxy. The number of carbon atoms is usually 3 to 14, preferably 4 to 10, and more preferably 5 to 6.
[0072] Specific examples of the optionally substituted aryloxy group include, but are not limited to, phenoxy, 1-naphthyloxy, and 2-naphthyloxy. The number of carbon atoms is usually 6 to 20, preferably 6 to 14, and more preferably 6 to 10.
[0073] Specific examples of the optionally substituted aralkyloxy group include, but are not limited to, benzyloxy, phenethyloxy, phenylpropyloxy, etc. The optionally substituted aralkyloxy group is preferably a group in which one hydrogen atom of an alkyloxy group having 1 to 4 carbon atoms is substituted with an aryl group having 6 to 20 carbon atoms.
[0074] Specific examples of the silyl group include, but are not limited to, a silyl group, a disilanyl group, and a trisilanyl group. The number of silicon atoms is usually 1 to 10, and preferably 1 to 6.
[0075] R B When is the above organic group or silyl group, at least one of the hydrogen atoms may be substituted with a substituent, specific examples of which include a hydroxy group, an alkyl group, an aryl group, and an alkoxy group.
[0076] From the viewpoint of suppressing unintended peeling when the laminate is brought into contact with any of organic solvents, acids, and chemical solutions used in the manufacture of semiconductor elements (such as alkaline developing solutions and hydrogen peroxide solutions), and from the viewpoint of suitably removing residues of the release agent layer on the substrate when the semiconductor substrate and the support substrate of the laminate are separated and then washed with the cleaning agent composition, R B is preferably an alkyl group or an aryl group, more preferably an aryl group, even more preferably a phenyl group, a 1-naphthyl group or a 2-naphthyl group, and even more preferably a phenyl group.
[0077] The branched-chain polysilane may contain a structural unit represented by the following formula (S) or a structural unit represented by the following formula (N) in addition to the structural unit represented by formula (B). From the viewpoint of suppressing unintended peeling when the laminate is brought into contact with any of an organic solvent, an acid, or a chemical solution used in the production of semiconductor elements (such as an alkaline developer or hydrogen peroxide solution), and from the viewpoint of suitably removing residue of the release agent layer on the substrate when the semiconductor substrate and the support substrate of the laminate are separated and then each substrate is washed with a cleaning agent composition, the content of the structural unit represented by formula (B) in the branched-chain polysilane is usually 50 mol % or more, preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, even more preferably 90 mol % or more, and even more preferably 95 mol % or more of all structural units.
[0078] [ka] (R S1 and S2 is R B It has the same meaning as
[0079] The terminal group (terminal substituent (atom)) of the branched chain polysilane may usually be a hydrogen atom, a hydroxy group, a halogen atom (such as a chlorine atom), an alkyl group, an aryl group, an alkoxy group, a silyl group, etc. Among these, a hydroxy group, a methyl group, or a phenyl group is often used, and a methyl group is preferred, and the terminal group may be a trimethylsilyl group.
[0080] In one embodiment, the average degree of polymerization of the branched polysilane is usually 2 to 100, preferably 3 to 80, more preferably 5 to 50, and even more preferably 10 to 30, in terms of silicon atoms (that is, the average number of silicon atoms per molecule). In one embodiment, the upper limit of the weight average molecular weight of the branched polysilane is usually 30,000, preferably 20,000, more preferably 10,000, even more preferably 5,000, even more preferably 2,000, even more preferably 1,500, and the lower limit is usually 50, preferably 100, more preferably 150, even more preferably 200, even more preferably 300, even more preferably 500. The average degree of polymerization and the weight average molecular weight of the branched polysilane can be measured, for example, using a GPC apparatus (EcoSEC, HLC-8220GPC manufactured by Tosoh Corporation) and GPC columns (Shodex KF-803L, KF-802, and KF-801 manufactured by Showa Denko K.K., in this order), at a column temperature of 40° C., using tetrahydrofuran as an eluent (elution solvent), at a flow rate (flow velocity) of 1.00 mL / min, and using polystyrene (manufactured by Sigma-Aldrich Co.) as a standard sample. If the degree of polymerization and weight average molecular weight of the branched-chain polysilane used are too small, the branched-chain polysilane may be vaporized by heating when forming a film that is a release agent layer or when processing a laminate having the obtained release agent layer, or defects may occur due to poor strength of the film. On the other hand, if the degree of polymerization and molecular weight of the branched-chain polysilane used are too large, sufficient solubility may not be ensured depending on the type of solvent used in preparing the release agent composition, causing precipitation in the composition, or mixing with the resin may be insufficient, making it difficult to reproducibly obtain a highly uniform film. Therefore, from the viewpoint of obtaining with even greater reproducibility a laminate having a release agent layer that contributes to favorable production of semiconductor elements, it is desirable for the degree of polymerization and weight average molecular weight of the branched-chain polysilane to satisfy the above-mentioned ranges.
[0081] From the viewpoint of reproducibly obtaining a release agent layer having excellent heat resistance, the 5% weight loss temperature of the branched polysilane is usually 300°C or higher, preferably 350°C or higher, more preferably 365°C or higher, even more preferably 380°C or higher, even more preferably 395°C or higher, and even more preferably 400°C or higher. The 5% weight loss temperature of the branched polysilane can be measured, for example, by raising the temperature from room temperature (25° C.) to 400° C. at a rate of 10° C. / min in air using a 2010SR manufactured by NETZSCH.
[0082] In the case where the semiconductor substrate and the support substrate of the laminate are separated and then each substrate is washed with a cleaning composition, from the viewpoint of suitably removing the residue of the release agent layer on the substrate and from the viewpoint of reproducibly preparing a release agent composition having excellent uniformity, the branched chain polysilane is preferably soluble in any one of ether compounds such as tetrahydrofuran, aromatic compounds such as toluene, glycol ether ester compounds such as propylene glycol monomethyl ether acetate, ketone compounds such as cyclohexanone and methyl ethyl ketone, and glycol ether compounds such as propylene glycol monomethyl ether. In this case, dissolution means a case where dissolution can be visually confirmed within 1 hour when dissolution is attempted using a shaker at room temperature (25°C) to obtain a 10% by mass solution.
[0083] The branched chain polysilane may be in either a solid or liquid state at room temperature.
[0084] The branched chain polysilane can be produced by referring to known methods described in, for example, JP2011-208054A, JP2007-106894A, JP2007-145879A, WO2005 / 113648A, etc., or can be obtained as a commercially available product. Specific examples of commercially available products include, but are not limited to, silicon material polysilane OGSOL SI-20-10, SI-20-14, etc., manufactured by Osaka Gas Chemicals Co., Ltd.
[0085] Suitable examples of branched polysilanes include, but are not limited to, the following: [ka] (Ph represents a phenyl group, R E each independently represents a terminal substituent, represents an atom or a group, nb indicates the number of repeating units.)
[0086] The content of the branched-chain polysilane in the stripper composition is usually 10 to 90% by mass based on the film-constituting components. From the viewpoint of reproducibly realizing a film that cannot be suitably removed by organic solvents, acids, or chemical solutions used in the production of semiconductor elements (such as alkaline developing solutions and hydrogen peroxide solutions) but can be suitably removed by the cleaning composition, the content is preferably 15 to 80% by mass, more preferably 20 to 70% by mass, even more preferably 25 to 60% by mass, and even more preferably 30 to 50% by mass.
[0087] <Crosslinking agent> The stripper composition may include a crosslinker. The crosslinking agent may undergo a crosslinking reaction due to self-condensation, but when crosslinkable substituents are present in the novolak resin, it can undergo a crosslinking reaction with the crosslinkable substituents.
[0088] Specific examples of the crosslinking agent are not particularly limited, but typically include phenol-based crosslinking agents, melamine-based crosslinking agents, urea-based crosslinking agents, and thiourea-based crosslinking agents, each of which has a crosslinking-forming group in the molecule, such as an alkoxymethyl group (e.g., a hydroxymethyl group, a methoxymethyl group, or a butoxymethyl group), and these may be low molecular weight compounds or high molecular weight compounds. The crosslinking agent contained in the release agent composition usually has two or more crosslinking groups. From the viewpoint of realizing more suitable curing with good reproducibility, the number of crosslinking groups contained in the compound that is the crosslinking agent is preferably 2 to 10, and more preferably 2 to 6. From the viewpoint of realizing higher heat resistance, the crosslinking agent contained in the release agent composition preferably has an aromatic ring (e.g., a benzene ring, a naphthalene ring) in the molecule, and a typical example of such a crosslinking agent includes, but is not limited to, a phenol-based crosslinking agent.
[0089] A phenol-based crosslinking agent having a crosslinking group is a compound having a crosslinking group bonded to an aromatic ring and having at least one of a phenolic hydroxy group and an alkoxy group derived from a phenolic hydroxy group. Examples of the alkoxy group derived from such a phenolic hydroxy group include, but are not limited to, a methoxy group and a butoxy group. The aromatic ring to which the cross-linking group is bonded and the aromatic ring to which the phenolic hydroxy group and / or the alkoxy group derived from the phenolic hydroxy group is bonded are not limited to non-condensed aromatic rings such as a benzene ring, but may also be condensed aromatic rings such as a naphthalene ring, anthracene ring, etc. When a plurality of aromatic rings are present in the molecule of the phenol-based crosslinking agent, the crosslinking group, the phenolic hydroxy group, and the alkoxy group derived from the phenolic hydroxy group may be bonded to the same aromatic ring or different aromatic rings in the molecule. The aromatic ring to which the crosslinking group, the phenolic hydroxy group, or the alkoxy group derived from the phenolic hydroxy group is bonded may be further substituted with a hydrocarbon group such as an alkyl group (e.g., methyl, ethyl, butyl, etc.) or an aryl group (e.g., phenyl, etc.) or a halogen atom (e.g., fluorine, etc.).
[0090] For example, specific examples of the phenol-based crosslinking agent having a crosslinking group include compounds represented by any of formulas (L1) to (L4).
[0091] [ka]
[0092] In each formula, each R' independently represents a fluorine atom, an aryl group, or an alkyl group, each R'' independently represents a hydrogen atom, an alkyl group, or an alkoxyalkyl group, and L 1 and L 2 each independently represents a single bond, a methylene group, or a propane-2,2-diyl group; L 3is determined according to q1 and represents a single bond, a methylene group, a propane-2,2-diyl group, a methanetriyl group, or an ethane-1,1,1-triyl group; t11, t12, and t13 are integers satisfying 2≦t11≦5, 1≦t12≦4, 0≦t13≦3, and t11+t12+t13≦6; t21, t22, and t23 are integers satisfying 2≦t21≦4, t24, t25, and t26 are integers that satisfy 2≦t24≦4, 1≦t25≦3, 0≦t26≦2, and t24+t25+t26≦5; t27, t28, and t29 are integers that satisfy 0≦t27≦4, 0≦t28≦4, 0≦t29≦4, and t27+t28 and t41+t42+t43≦4; t31, t32, and t33 are integers satisfying 2≦t31≦4, 1≦t32≦3, 0≦t33≦2, and t31+t32+t33≦5; t41, t42, and t43 are integers satisfying 2≦t41≦3, 1≦t42≦2, 0≦t43≦1, and t41+t42+t43≦4; q1 is 2 or 3, q2 represents the number of repetitions and is an integer of 0 or more; specific examples of the aryl group and alkyl group include the same as the specific examples below, but the aryl group is preferably a phenyl group, the alkyl group is preferably a methyl group or a t-butyl group, and the alkoxyalkyl group is preferably a 2-methoxy-1-methylethyl group.
[0093] Specific examples of the compounds represented by formulas (L1) to (L4) are listed below, but are not limited thereto. These compounds may be synthesized by known methods, and are also available as products from, for example, Asahi Yukizai Kogyo Co., Ltd. or Honshu Chemical Industry Co., Ltd.
[0094] [ka]
[0095] [ka]
[0096] [ka]
[0097] [ka] TIFF2024135070000039.tif4364
[0098] The melamine-based crosslinking agent having a crosslinking group is a melamine derivative, a 2,4-diamino-1,3,5-triazine derivative or a 2-amino-1,3,5-triazine derivative in which at least one hydrogen atom of the amino group bonded to the triazine ring is substituted with a crosslinking group, and the triazine ring may further have a substituent such as an aryl group such as a phenyl group. Specific examples of melamine-based crosslinking agents having a crosslinking group include mono-, bis-, tris-, tetrakis-, pentakis- or hexakisalkoxymethylmelamines such as N,N,N',N',N",N"-hexakis(methoxymethyl)melamine and N,N,N',N',N",N"-hexakis(butoxymethyl)melamine; mono-, bis-, tris- or tetrakisalkoxymethylbenzoguanamines such as N,N,N',N'-tetrakis(methoxymethyl)benzoguanamine and N,N,N',N'-tetrakis(butoxymethyl)benzoguanamine, but are not limited to these.
[0099] The urea-based crosslinking agent having a crosslinking group is a derivative of a compound containing a urea bond, and has a structure in which at least one hydrogen atom of the NH group constituting the urea bond is substituted with a crosslinking group. Specific examples of urea-based crosslinking agents having a crosslinking group include mono-, bis-, tris-, or tetrakisalkoxymethylglycolurils such as 1,3,4,6-tetrakis(methoxymethyl)glycoluril and 1,3,4,6-tetrakis(butoxymethyl)glycoluril; and mono-, bis-, tris-, or tetrakisalkoxymethylureas such as 1,3-bis(methoxymethyl)urea and 1,1,3,3-tetrakismethoxymethylurea, but are not limited to these.
[0100] A thiourea-based crosslinking agent having a crosslinking group is a derivative of a compound containing a thiourea bond, and has a structure in which at least one hydrogen atom of the NH group constituting the thiourea bond is substituted with a crosslinking group. Specific examples of thiourea-based crosslinking agents having a crosslinking group include mono-, bis-, tris-, or tetrakisalkoxymethylthioureas such as 1,3-bis(methoxymethyl)thiourea and 1,1,3,3-tetrakismethoxymethylthiourea, but are not limited to these.
[0101] The amount of crosslinking agent contained in the release agent composition cannot be generally defined because it varies depending on the coating method used, the desired film thickness, etc., but is usually 0.01 to 50% by mass with respect to the organic resin or polynuclear phenol derivative. From the viewpoint of achieving suitable curing and reproducibly obtaining a laminate from which the semiconductor substrate and the support substrate can be satisfactorily separated, the amount is preferably 0.1% by mass or more, more preferably 1% by mass or more, even more preferably 3% by mass or more, and still more preferably 5% by mass or more, and is preferably 45% by mass or less, more preferably 40% by mass or less, even more preferably 35% by mass or less, and still more preferably 30% by mass or less.
[0102] <Acid generator and acid> For the purpose of promoting the crosslinking reaction, the stripping composition may contain an acid generator or an acid.
[0103] Examples of the acid generator include a thermal acid generator and a photoacid generator. The thermal acid generator is not particularly limited as long as it generates an acid by heat, and specific examples thereof include 2,4,4,6-tetrabromocyclohexadienone, benzoin tosylate, 2-nitrobenzyl tosylate, K-PURE (registered trademark) CXC-1612, CXC-1614, TAG-2172, TAG-2179, TAG-2678, TAG2689, and TAG2700 (manufactured by King Industries), as well as SI-45, SI-60, SI-80, SI-100, SI-110, and SI-150 (manufactured by Sanshin Chemical Industry Co., Ltd.), and other organic sulfonic acid alkyl esters, but are not limited thereto.
[0104] Examples of the photoacid generator include an onium salt compound, a sulfonimide compound, and a disulfonyldiazomethane compound.
[0105] Specific examples of the onium salt compound include iodonium salt compounds such as diphenyliodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoronormal butanesulfonate, diphenyliodonium perfluoronormal octanesulfonate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, and bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate; and sulfonium salt compounds such as triphenylsulfonium nitrate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoronormal butanesulfonate, triphenylsulfonium camphorsulfonate, and triphenylsulfonium trifluoromethanesulfonate, but are not limited to these.
[0106] Specific examples of the sulfonimide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoronormalbutanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, N-(trifluoromethanesulfonyloxy)naphthalimide, and the like, but are not limited thereto.
[0107] Specific examples of the disulfonyldiazomethane compound include, but are not limited to, bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, methylsulfonyl-p-toluenesulfonyldiazomethane, and the like.
[0108] Specific examples of acids include arylsulfonic acids and pyridinium salts such as p-toluenesulfonic acid, pyridinium p-toluenesulfonate (pyridinium paratoluenesulfonate), pyridinium trifluoromethanesulfonate, pyridinium phenolsulfonic acid, 5-sulfosalicylic acid, 4-phenolsulfonic acid, 4-chlorobenzenesulfonic acid, benzenedisulfonic acid, and 1-naphthalenesulfonic acid, and salts thereof; arylcarboxylic acids and salts thereof such as salicylic acid, benzoic acid, hydroxybenzoic acid, and naphthalenecarboxylic acid; linear or cyclic alkylsulfonic acids and salts thereof such as trifluoromethanesulfonic acid and camphorsulfonic acid; linear or cyclic alkylcarboxylic acids and salts thereof such as citric acid, but are not limited thereto.
[0109] The amounts of the acid generator and acid contained in the stripping composition cannot be generally defined because they vary depending on the type of crosslinking agent used and the heating temperature when forming the film, but are usually 0.01 to 5 mass % based on the film constituent components.
[0110] <Surfactant> The stripping agent composition may contain a surfactant for the purposes of adjusting the liquid properties of the composition itself and the film properties of the resulting film, and for the purpose of preparing a highly uniform stripping agent composition with good reproducibility. Examples of surfactants include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether; polyoxyethylene alkyl allyl ethers such as polyoxyethylene octyl phenol ether and polyoxyethylene nonyl phenol ether; polyoxyethylene-polyoxypropylene block copolymers; sorbitan fatty acid esters such as sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate; polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, Examples of suitable surfactants include nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters, such as polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate; fluorosurfactants such as EFTOP EF301, EF303, and EF352 (trade names, manufactured by Tochem Products Co., Ltd.), Megafac F171, F173, R-30, and R-30N (trade names, manufactured by DIC Corporation), Fluorad FC430 and FC431 (trade names, manufactured by Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, and SC106 (trade names, manufactured by Asahi Glass Co., Ltd.); and organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.). The surfactants can be used alone or in combination of two or more. The amount of the surfactant is usually 2% by mass or less based on the film-constituting components of the stripping composition.
[0111] <Solvent> The stripper composition preferably includes a solvent. As such a solvent, for example, a high polarity solvent capable of dissolving well the film constituent components such as the organic resin, polynuclear phenol derivative, branched polysilane, and crosslinking agent can be used, and a low polarity solvent may be used as necessary for the purpose of adjusting viscosity, surface tension, etc. In the present invention, a low polarity solvent is defined as a solvent having a relative dielectric constant of less than 7 at a frequency of 100 kHz, and a high polarity solvent is defined as a solvent having a relative dielectric constant of 7 or more at a frequency of 100 kHz. The solvents can be used alone or in combination of two or more.
[0112] Examples of highly polar solvents include amide-based solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N,N-dimethylisobutyramide, N-methylpyrrolidone, and 1,3-dimethyl-2-imidazolidinone; ketone-based solvents such as ethyl methyl ketone, isophorone, and cyclohexanone; cyano-based solvents such as acetonitrile and 3-methoxypropionitrile; polyhydric alcohol-based solvents such as ethylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, 1,3-butanediol, and 2,3-butanediol; monohydric alcohol-based solvents other than aliphatic alcohols such as propylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monophenyl ether, triethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, benzyl alcohol, 2-phenoxyethanol, 2-benzyloxyethanol, 3-phenoxybenzyl alcohol, and tetrahydrofurfuryl alcohol; and sulfoxide-based solvents such as dimethyl sulfoxide.
[0113] Examples of low polarity solvents include chlorine-based solvents such as chloroform and chlorobenzene; aromatic hydrocarbon-based solvents such as alkylbenzenes such as toluene, xylene, tetralin, cyclohexylbenzene, and decylbenzene; aliphatic alcohol-based solvents such as 1-octanol, 1-nonanol, and 1-decanol; ether-based solvents such as tetrahydrofuran, dioxane, anisole, 4-methoxytoluene, 3-phenoxytoluene, dibenzyl ether, diethylene glycol dimethyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, and triethylene glycol butyl methyl ether; and ester-based solvents such as methyl benzoate, ethyl benzoate, butyl benzoate, isoamyl benzoate, bis(2-ethylhexyl) phthalate, dibutyl maleate, dibutyl oxalate, hexyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate.
[0114] The content of the solvent is appropriately determined taking into consideration the viscosity of the desired composition, the coating method to be used, the thickness of the film to be produced, and the like, but is 99% by mass or less of the entire composition, and preferably 70 to 99% by mass with respect to the entire composition, i.e., the amount of the film constituent components in this case is 1 to 30% by mass with respect to the entire composition.
[0115] The viscosity and surface tension of the stripping composition are appropriately adjusted by changing the types of solvents used, their ratios, the concentrations of the film constituent components, etc., taking into consideration various factors such as the coating method used and the desired film thickness.
[0116] In one embodiment of the present invention, the stripping agent composition contains a glycol-based solvent from the viewpoint of reproducibly obtaining a composition with high uniformity, from the viewpoint of reproducibly obtaining a composition with high storage stability, from the viewpoint of reproducibly obtaining a composition that gives a film with high uniformity, etc. Note that the "glycol-based solvent" referred to here is a general term for glycols, glycol monoethers, glycol diethers, glycol monoesters, glycol diesters, and glycol ester ethers.
[0117] An example of a preferred glycol solvent is represented by formula (G).
[0118] [ka]
[0119] In formula (G), R G1 each independently represents a linear or branched alkylene group having 2 to 4 carbon atoms; R G2 and R G3 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 8 carbon atoms, or an alkylacyl group in which the alkyl portion is a linear or branched alkyl group having 1 to 8 carbon atoms; n g is an integer from 1 to 6.
[0120] Specific examples of the linear or branched alkylene group having 2 to 4 carbon atoms include, but are not limited to, an ethylene group, a trimethylene group, a 1-methylethylene group, a tetramethylene group, a 2-methylpropane-1,3-diyl group, a pentamethylene group, and a hexamethylene group. Of these, from the viewpoint of reproducibly obtaining a composition having high uniformity, from the viewpoint of reproducibly obtaining a composition having high storage stability, from the viewpoint of reproducibly obtaining a composition that gives a film having high uniformity, etc., a linear or branched alkylene group having 2 to 3 carbon atoms is preferred, and a linear or branched alkylene group having 3 carbon atoms is more preferred.
[0121] Specific examples of the linear or branched alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a tertiary butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2-methyl-n-pentyl group, a 3-methyl Examples of such aryl groups include, but are not limited to, -n-pentyl group, 4-methyl-n-pentyl group, 1,1-dimethyl-n-butyl group, 1,2-dimethyl-n-butyl group, 1,3-dimethyl-n-butyl group, 2,2-dimethyl-n-butyl group, 2,3-dimethyl-n-butyl group, 3,3-dimethyl-n-butyl group, 1-ethyl-n-butyl group, 2-ethyl-n-butyl group, 1,1,2-trimethyl-n-propyl group, 1,2,2-trimethyl-n-propyl group, 1-ethyl-1-methyl-n-propyl group, and 1-ethyl-2-methyl-n-propyl group. Of these, from the viewpoint of reproducibly obtaining a composition that is highly uniform, from the viewpoint of reproducibly obtaining a composition that has high storage stability, and from the viewpoint of reproducibly obtaining a composition that gives a film that is highly uniform, a methyl group and an ethyl group are preferred, and a methyl group is more preferred.
[0122] Specific examples of the linear or branched alkyl group having 1 to 8 carbon atoms in the alkyl acyl group in which the alkyl portion is a linear or branched alkyl group having 1 to 8 carbon atoms include the same as the specific examples mentioned above. Of these, from the viewpoint of reproducibly obtaining a composition having high uniformity, from the viewpoint of reproducibly obtaining a composition having high storage stability, from the viewpoint of reproducibly obtaining a composition that gives a film having high uniformity, etc., a methylcarbonyl group and an ethylcarbonyl group are preferred, and a methylcarbonyl group is more preferred.
[0123] n gis preferably 4 or less, more preferably 3 or less, even more preferably 2 or less, and most preferably 1, from the viewpoint of reproducibly obtaining a highly uniform composition, from the viewpoint of reproducibly obtaining a composition that gives a highly uniform film, and the like.
[0124] From the viewpoint of reproducibly obtaining a composition having high uniformity, a composition having high storage stability, and a composition that gives a film having high uniformity, it is preferable that R G2 and R G3 At least one of R is a linear or branched alkyl group having 1 to 8 carbon atoms, and more preferably R G2 and R G3 One of these is a linear or branched alkyl group having 1 to 8 carbon atoms, and the other is a hydrogen atom or an alkylacyl group in which the alkyl portion is a linear or branched alkyl group having 1 to 8 carbon atoms.
[0125] From the viewpoint of reproducibly obtaining a highly uniform composition, from the viewpoint of reproducibly obtaining a composition with high storage stability, from the viewpoint of reproducibly obtaining a composition that gives a highly uniform film, etc., the content of the glycol-based solvent is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 95% by mass or more, of the solvent contained in the stripping agent composition. From the viewpoint of reproducibly obtaining a composition having high uniformity, from the viewpoint of reproducibly obtaining a composition having high storage stability, from the viewpoint of reproducibly obtaining a composition that gives a film having high uniformity, and the like, in the stripper composition, the film constituent components are uniformly dispersed or dissolved in the solvent, and preferably dissolved.
[0126] <Laminate> The laminate according to the present invention comprises a semiconductor substrate or an electronic device layer, a supporting substrate, and a release agent layer. The laminate according to the present invention preferably further comprises an adhesive layer, and has a configuration including a semiconductor substrate or an electronic device layer, a support substrate, a release agent layer, and an adhesive layer. The release agent layer is preferably a release agent layer for peeling by light irradiation. When the release agent layer according to the present invention is formed so as to have both a release function of peeling off the semiconductor substrate or electronic device layer from the supporting substrate by light irradiation, and an adhesive function of bonding the semiconductor substrate or electronic device layer to the supporting substrate (i.e., when the release agent layer is formed using a release agent composition containing components that exhibit both functions), the laminate may be formed of a single layer structure of the release agent layer having adhesive properties, rather than a two-layer structure of the release agent layer and the adhesive layer.
[0127] The supporting substrate preferably has optical transparency. When the release agent layer is a release agent layer for peeling by light irradiation, the release agent layer for peeling by light irradiation is provided between the semiconductor substrate or electronic device layer and the supporting substrate. The laminate is used in such a manner that the semiconductor substrate or electronic device layer and the supporting substrate are peeled off after the release agent layer absorbs light irradiated from the supporting substrate side. The release agent layer is a layer formed from the above-mentioned release agent composition of the present invention.
[0128] The laminate of the present invention is used for temporary bonding for processing a semiconductor substrate or an electronic device layer, and can be suitably used for processing such as thinning a semiconductor substrate or an electronic device layer. During the processing such as thinning of the semiconductor substrate, the semiconductor substrate is supported by the support substrate. On the other hand, after processing of the semiconductor substrate, for example, the release agent layer is irradiated with light, and then the support substrate and the semiconductor substrate are separated. In the release agent layer formed from the release agent composition, the organic resin contained in the release agent composition causes the novolac resin to absorb light (e.g., laser light) and alter (e.g., separate or decompose) the release agent layer. As a result, after the release agent layer is irradiated with light, the semiconductor substrate and the support substrate are easily peeled off. In addition to light irradiation, the semiconductor substrate and the support substrate may be peeled off by peeling between the layers. In addition, while the electronic device layer is being processed, such as being thinned, the electronic device layer is supported by the support substrate. After the electronic device layer is processed, for example, the release agent layer is irradiated with light, and then the support substrate and the electronic device layer are separated from each other. The release agent layer according to the present invention allows residues of the release agent layer or adhesive layer remaining on the semiconductor substrate, electronic device layer, or supporting substrate after the semiconductor substrate or electronic device layer is peeled from the supporting substrate to be removed, for example, with a cleaning composition for cleaning semiconductor substrates, etc. Furthermore, the release layer for light irradiation peeling makes it easier to peel the semiconductor substrate or electronic device layer from the supporting substrate after irradiation with light.
[0129] The wavelength of the light used for peeling is, for example, preferably 250 to 600 nm, more preferably 250 to 370 nm. More preferably, the wavelength is 308 nm, 343 nm, 355 nm, 365 nm, or 532 nm. The amount of light required for peeling is an amount that can cause suitable alteration, such as decomposition, of the novolac resin. The light used for the peeling may be laser light or non-laser light emitted from a light source such as an ultraviolet lamp.
[0130] The laminated body will be described in detail below, with respect to the case where the laminated body includes a semiconductor substrate and the case where the laminated body includes an electronic device layer. The case where the laminate has a semiconductor substrate is described below in the <First embodiment>, and the case where the laminate has an electronic device layer is described below in the <Second embodiment>.
[0131] <First embodiment> The laminate having the semiconductor substrate is used for processing the semiconductor substrate. During the processing of the semiconductor substrate, the semiconductor substrate is adhered to the support substrate. After the processing of the semiconductor substrate, for example, after irradiating the release agent layer with light, the semiconductor substrate is separated from the support substrate.
[0132] <<Semiconductor substrate>> The main material constituting the entire semiconductor substrate is not particularly limited as long as it is used for this type of application, but examples thereof include silicon, silicon carbide, and compound semiconductors. The shape of the semiconductor substrate is not particularly limited, but may be, for example, a disk shape. Note that the disk-shaped semiconductor substrate does not need to have a perfectly circular surface, and for example, the outer periphery of the semiconductor substrate may have a straight line portion called an orientation flat, or may have a cut called a notch. The thickness of the disk-shaped semiconductor substrate may be appropriately determined depending on the intended use of the semiconductor substrate, and is not particularly limited, but is, for example, 500 to 1,000 μm. The diameter of the disk-shaped semiconductor substrate may be appropriately determined depending on the intended use of the semiconductor substrate, and is not particularly limited, but is, for example, 100 to 1,000 mm.
[0133] The semiconductor substrate may have bumps, which are protruding terminals. In the laminate, when the semiconductor substrate has bumps, the semiconductor substrate has the bumps on the supporting substrate side. In a semiconductor substrate, bumps are usually formed on a surface on which a circuit is formed. The circuit may be a single layer or a multilayer. There is no particular limitation on the shape of the circuit. In the semiconductor substrate, the surface opposite to the surface having the bumps (back surface) is the surface to be processed. The material, size, shape, structure, and density of the bumps on the semiconductor substrate are not particularly limited. Examples of the bump include a ball bump, a printed bump, a stud bump, and a plated bump. Usually, the height, radius and pitch of the bumps are appropriately determined based on the conditions of a bump height of about 1 to 200 μm, a bump radius of 1 to 200 μm and a bump pitch of 1 to 500 μm. Examples of materials for the bump include low melting point solder, high melting point solder, tin, indium, gold, silver, copper, etc. The bump may be composed of only a single component, or may be composed of multiple components. More specifically, examples of the bump include alloy plating mainly composed of Sn, such as SnAg bump, SnBi bump, Sn bump, and AuSn bump. The bump may have a laminated structure including a metal layer made of at least one of these components.
[0134] An example of a semiconductor substrate is a silicon wafer having a diameter of about 300 mm and a thickness of about 770 μm.
[0135] <<Support substrate>> The support substrate is preferably a member that is optically transparent to the light irradiated to the release agent layer and can support the semiconductor substrate when the semiconductor substrate is processed. The support substrate is not particularly limited, but examples thereof include a glass support substrate.
[0136] The shape of the support substrate is not particularly limited, but may be, for example, a disk shape. The thickness of the disk-shaped support substrate may be appropriately determined depending on the size of the semiconductor substrate, and is not particularly limited, but is, for example, 500 to 1,000 μm. The diameter of the disk-shaped support substrate may be appropriately determined depending on the size of the semiconductor substrate, and is not particularly limited, but is, for example, 100 to 1,000 mm.
[0137] An example of the support substrate is a glass wafer having a diameter of about 300 mm and a thickness of about 700 μm.
[0138] <<Release agent layer>> The release agent layer is a layer formed from a release agent composition. The release agent layer is provided between the semiconductor substrate and the supporting substrate. The release agent layer may be in contact with either the supporting substrate or the semiconductor substrate.
[0139] The release agent composition of the present invention can be suitably used for forming a release agent layer of a laminate having a semiconductor substrate, a support substrate, and a release agent layer provided between the semiconductor substrate and the support substrate. The laminate is used for peeling off the semiconductor substrate and the support substrate. The release agent layer obtained from the release agent composition of the present invention makes it possible to easily peel the semiconductor substrate from the supporting substrate after irradiation with light.
[0140] It is believed that when the release agent layer is formed from the release agent composition, the novolac resin reacts with the siloxane skeleton-containing epoxy resin.
[0141] The thickness of the release agent layer is not particularly limited, but is usually 0.01 to 10 μm. From the viewpoint of maintaining film strength, the thickness is preferably 0.03 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more, and from the viewpoint of avoiding non-uniformity due to a thick film, the thickness is preferably 8 μm or less, more preferably 5 μm or less, even more preferably 2 μm or less, and even more preferably 1 μm or less. The method for forming the release agent layer from the release agent composition will be described in detail in the description of <<An example of a method for producing the laminate in the first embodiment>> below.
[0142] <<Adhesive layer>> The adhesive layer is provided between the support substrate and the semiconductor substrate. The adhesive layer may be in contact with, for example, a semiconductor substrate. The adhesive layer may be in contact with, for example, a support substrate. The adhesive layer is not particularly limited, but is preferably a layer formed from an adhesive composition.
[0143] <<Adhesive composition>> Examples of adhesive compositions include, but are not limited to, polysiloxane-based adhesives, acrylic resin-based adhesives, epoxy resin-based adhesives, polyamide-based adhesives, polystyrene-based adhesives, polyimide adhesives, and phenolic resin-based adhesives. Among these, polysiloxane-based adhesives are preferred as the adhesive composition, because they exhibit suitable adhesive performance during processing of semiconductor substrates and the like, can be easily peeled off after processing, have excellent heat resistance, and can be easily removed by a cleaning composition.
[0144] In a preferred embodiment, the adhesive composition contains a polyorganosiloxane. In another preferred embodiment, the adhesive composition includes a component that cures via a hydrosilylation reaction.
[0145] For example, the adhesive composition used in the present invention contains a curable component (A) that becomes an adhesive component. The adhesive composition used in the present invention may contain a curable component (A) that becomes an adhesive component and a component (B) that does not undergo a curing reaction. Here, an example of the component (B) that does not undergo a curing reaction is polyorganosiloxane. In the present invention, "does not undergo a curing reaction" does not mean that any curing reaction does not occur, but means that the curing reaction occurring in the curable component (A) does not occur. In a preferred embodiment, component (A) may be a component that cures by a hydrosilylation reaction, or may be a polyorganosiloxane component (A') that cures by a hydrosilylation reaction. In another preferred embodiment, the component (A) contains, for example, a polyorganosiloxane (a1) having an alkenyl group having 2 to 40 carbon atoms bonded to a silicon atom, as an example of the component (A'), a polyorganosiloxane (a2) having a Si-H group, and a platinum group metal catalyst (A2). Here, the alkenyl group having 2 to 40 carbon atoms may be substituted. Examples of the substituent include a halogen atom, a nitro group, a cyano group, an amino group, a hydroxyl group, a carboxyl group, an aryl group, and a heteroaryl group.
[0146] In another preferred embodiment, the polyorganosiloxane component (A') that cures by a hydrosilylation reaction comprises siloxane units (Q units) represented by SiO2, R 1 R2 R 3 SiO 1 / 2 Siloxane unit (M unit) represented by R 4 R 5 SiO 2 / 2 Siloxane units (D units) represented by the formula 6 SiO 3 / 2 and a platinum group metal catalyst (A2). The polysiloxane (A1) contains one or more units selected from the group consisting of siloxane units (T units) represented by the following formula: 1 'R 2 'R 3 'SiO 1 / 2 Siloxane unit (M' unit) represented by R 4 'R 5 'SiO 2 / 2 Siloxane units (D' units) represented by the formula 6 'SiO 3 / 2 and at least one unit selected from the group consisting of M' units, D' units and T' units; and a polyorganosiloxane (a1') containing one or more units selected from the group consisting of siloxane units (T' units) represented by the following formula: 1 "R 2 "R 3 "SiO 1 / 2 Siloxane unit (M” unit) represented by R 4 "R 5 "SiO 2 / 2 Siloxane units (D" units) represented by the formula 6 "SiO 3 / 2 and a polyorganosiloxane (a2') containing one or more units selected from the group consisting of siloxane units (T" units) represented by the following formula: Note that (a1') is an example of (a1), and (a2') is an example of (a2).
[0147] R 1 ~R 6are groups or atoms bonded to silicon atoms, each independently representing an optionally substituted alkyl group, an optionally substituted alkenyl group, or a hydrogen atom. Examples of the substituent include a halogen atom, a nitro group, a cyano group, an amino group, a hydroxyl group, a carboxyl group, an aryl group, and a heteroaryl group.
[0148] R 1 '~R 6 Each of R ′ is a group bonded to a silicon atom, and each independently represents an optionally substituted alkyl group or an optionally substituted alkenyl group. 1 '~R 6 At least one of the groups ' is an alkenyl group which may be substituted. Examples of the substituent include a halogen atom, a nitro group, a cyano group, an amino group, a hydroxyl group, a carboxyl group, an aryl group, and a heteroaryl group.
[0149] R 1 ”~R 6 " are groups or atoms bonded to the silicon atom, each independently representing an optionally substituted alkyl group or a hydrogen atom, R 1 ”~R 6 At least one of " is a hydrogen atom. Examples of the substituent include a halogen atom, a nitro group, a cyano group, an amino group, a hydroxyl group, a carboxyl group, an aryl group, and a heteroaryl group.
[0150] The alkyl group may be linear, branched, or cyclic, but is preferably a linear or branched alkyl group. The number of carbon atoms is not particularly limited, but is usually 1 to 40, preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less.
[0151] Specific examples of the optionally substituted straight-chain or branched-chain alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a tertiary butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl-n-propyl group, an n-hexyl group, a 1-methyl-n-pentyl group, a 2-methyl-n-pentyl group, a 3-methyl-n-pentyl group, a 4-methyl-n-pentyl group, Examples of the alkyl group include, but are not limited to, a 1,1-dimethyl-n-butyl group, a 1,2-dimethyl-n-butyl group, a 1,3-dimethyl-n-butyl group, a 2,2-dimethyl-n-butyl group, a 2,3-dimethyl-n-butyl group, a 3,3-dimethyl-n-butyl group, a 1-ethyl-n-butyl group, a 2-ethyl-n-butyl group, a 1,1,2-trimethyl-n-propyl group, a 1,2,2-trimethyl-n-propyl group, a 1-ethyl-1-methyl-n-propyl group, and a 1-ethyl-2-methyl-n-propyl group, and the number of carbon atoms is usually 1 to 14, preferably 1 to 10, and more preferably 1 to 6. Among these, a methyl group is particularly preferable.
[0152] Specific examples of the optionally substituted cyclic alkyl group include a cyclopropyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, a cyclopentyl group, a 1-methyl-cyclobutyl group, a 2-methyl-cyclobutyl group, a 3-methyl-cyclobutyl group, a 1,2-dimethyl-cyclopropyl group, a 2,3-dimethyl-cyclopropyl group, a 1-ethyl-cyclopropyl group, a 2-ethyl-cyclopropyl group, a cyclohexyl group, a 1-methyl-cyclopentyl group, a 2-methyl-cyclopentyl group, a 3-methyl-cyclopentyl group, a 1-ethyl-cyclobutyl group, a 2-ethyl-cyclobutyl group, a 3-ethyl-cyclobutyl group, a 1,2-dimethyl-cyclobutyl group, a 1,3-dimethyl-cyclobutyl group, a 2,2-dimethyl-cyclobutyl group, a 2,3-dimethyl-cyclobutyl group, a 2,4-dimethyl-cyclobutyl group, a 3,3-dimethyl-cyclobutyl group, a cyclopropyl ... Examples of cycloalkyl groups include cycloalkyl groups such as 1-n-cyclobutyl group, 1-n-propyl-cyclopropyl group, 2-n-propyl-cyclopropyl group, 1-i-propyl-cyclopropyl group, 2-i-propyl-cyclopropyl group, 1,2,2-trimethyl-cyclopropyl group, 1,2,3-trimethyl-cyclopropyl group, 2,2,3-trimethyl-cyclopropyl group, 1-ethyl-2-methyl-cyclopropyl group, 2-ethyl-1-methyl-cyclopropyl group, 2-ethyl-2-methyl-cyclopropyl group, and 2-ethyl-3-methyl-cyclopropyl group; and bicycloalkyl groups such as bicyclobutyl group, bicyclopentyl group, bicyclohexyl group, bicycloheptyl group, bicyclooctyl group, bicyclononyl group, and bicyclodecyl group, but are not limited to these. The number of carbon atoms is usually 3 to 14, preferably 4 to 10, and more preferably 5 to 6.
[0153] The alkenyl group may be either linear or branched, and the number of carbon atoms therein is not particularly limited, but is usually 2 to 40, preferably 30 or less, more preferably 20 or less, and even more preferably 10 or less.
[0154] Specific examples of the optionally substituted linear or branched alkenyl group include, but are not limited to, a vinyl group, an allyl group, a butenyl group, a pentenyl group, and the like, and the number of carbon atoms therein is usually 2 to 14, preferably 2 to 10, and more preferably 1 to 6. Among these, an ethenyl group and a 2-propenyl group are particularly preferred. Specific examples of the optionally substituted cyclic alkenyl group include, but are not limited to, cyclopentenyl, cyclohexenyl, and the like. The number of carbon atoms is usually 4 to 14, preferably 5 to 10, and more preferably 5 to 6.
[0155] As described above, polysiloxane (A1) contains polyorganosiloxane (a1') and polyorganosiloxane (a2'), and the alkenyl group contained in polyorganosiloxane (a1') and the hydrogen atom (Si-H group) contained in polyorganosiloxane (a2') form a crosslinked structure by hydrosilylation reaction with platinum group metal catalyst (A2), and are cured. As a result, a cured film is formed.
[0156] The polyorganosiloxane (a1') contains one or more units selected from the group consisting of Q' units, M' units, D' units and T' units, and also contains at least one unit selected from the group consisting of M' units, D' units and T' units. As the polyorganosiloxane (a1'), a combination of two or more polyorganosiloxanes satisfying such conditions may be used.
[0157] Preferred combinations of two or more selected from the group consisting of Q' units, M' units, D' units and T' units include, but are not limited to, (Q' units and M' units), (D' units and M' units), (T' units and M' units) and (Q' units, T' units and M' units).
[0158] In addition, when the polyorganosiloxane (a1') contains two or more types of polyorganosiloxane, combinations of (Q' units and M' units) and (D' units and M' units), combinations of (T' units and M' units) and (D' units and M' units), and combinations of (Q' units, T' units and M' units) and (T' units and M' units) are preferred, but are not limited to these.
[0159] The polyorganosiloxane (a2') contains one or more units selected from the group consisting of Q" units, M" units, D" units, and T" units, and also contains at least one unit selected from the group consisting of M" units, D" units, and T" units. As the polyorganosiloxane (a2'), a combination of two or more polyorganosiloxanes satisfying such conditions may be used.
[0160] Preferred combinations of two or more selected from the group consisting of Q″ units, M″ units, D″ units and T″ units include, but are not limited to, (M″ units and D″ units), (Q″ units and M″ units), and (Q″ units, T″ units and M″ units).
[0161] The polyorganosiloxane (a1') is composed of siloxane units having alkyl and / or alkenyl groups bonded to the silicon atoms thereof. 1 '~R 6 The proportion of alkenyl groups in all the substituents represented by R 1 '~R 6 ' can be an alkyl group.
[0162] The polyorganosiloxane (a2') is composed of siloxane units in which an alkyl group and / or a hydrogen atom is bonded to the silicon atom. 1 ”~R 6 The proportion of hydrogen atoms in all the substituents and substituted atoms represented by R 1 ”~R6 " can be an alkyl group.
[0163] When the component (A) contains (a1) and (a2), in a preferred embodiment of the present invention, the molar ratio of the alkenyl groups contained in the polyorganosiloxane (a1) to the hydrogen atoms constituting the Si-H bonds contained in the polyorganosiloxane (a2) is in the range of 1.0:0.5 to 1.0:0.66.
[0164] The weight average molecular weight of polysiloxanes such as polyorganosiloxane (a1) and polyorganosiloxane (a2) is not particularly limited, but is usually 500 to 1,000,000, and preferably 5,000 to 50,000 from the viewpoint of achieving the effects of the present invention with good reproducibility. In the present invention, the weight average molecular weight, number average molecular weight and dispersity of polyorganosiloxane (excluding the above organosiloxane polymer) can be measured, for example, using a GPC apparatus (EcoSEC, HLC-8320GPC manufactured by Tosoh Corporation) and a GPC column (TSKgel SuperMultiporeHZ-N, TSKgel SuperMultiporeHZ-H manufactured by Tosoh Corporation), with a column temperature of 40°C, tetrahydrofuran as an eluent (elution solvent), a flow rate (flow rate) of 0.35 mL / min, and polystyrene (Shodex manufactured by Showa Denko K.K.) as a standard sample.
[0165] The viscosities of the polyorganosiloxane (a1) and the polyorganosiloxane (a2) are not particularly limited, but are usually 10 to 1,000,000 (mPa·s), and from the viewpoint of realizing the effects of the present invention with good reproducibility, are preferably 50 to 10,000 (mPa·s). The viscosities of the polyorganosiloxane (a1) and the polyorganosiloxane (a2) are values measured at 25°C using an E-type rotational viscometer.
[0166] Polyorganosiloxane (a1) and polyorganosiloxane (a2) react with each other to form a film by hydrosilylation, and therefore the mechanism of cure is different from that via, for example, silanol groups, and therefore neither siloxane needs to contain silanol groups or functional groups that form silanol groups upon hydrolysis, such as alkyloxy groups.
[0167] In a preferred embodiment of the present invention, the adhesive composition contains a platinum group metal catalyst (A2) together with the polyorganosiloxane component (A'). Such a platinum-based metal catalyst is a catalyst for promoting the hydrosilylation reaction between the alkenyl groups of the polyorganosiloxane (a1) and the Si-H groups of the polyorganosiloxane (a2).
[0168] Specific examples of platinum-based metal catalysts include platinum black, platinic chloride, chloroplatinic acid, a reaction product of chloroplatinic acid with a monohydric alcohol, a complex of chloroplatinic acid with an olefin, platinum bisacetoacetate, and other platinum-based catalysts, but are not limited to these. An example of a complex of platinum with an olefin is, but is not limited to, a complex of divinyltetramethyldisiloxane with platinum. The amount of the platinum group metal catalyst (A2) is not particularly limited, but is usually in the range of 1.0 to 50.0 ppm based on the total amount of the polyorganosiloxane (a1) and the polyorganosiloxane (a2).
[0169] The polyorganosiloxane component (A') may contain a polymerization inhibitor (A3) for the purpose of inhibiting the progress of the hydrosilylation reaction. The polymerization inhibitor is not particularly limited as long as it can inhibit the progress of the hydrosilylation reaction. Specific examples include alkynyl alcohols such as 1-ethynyl-1-cyclohexanol and 1,1-diphenyl-2-propion-1-ol. The amount of the polymerization inhibitor is not particularly limited, but is usually 1000.0 ppm or more based on the total amount of polyorganosiloxane (a1) and polyorganosiloxane (a2) from the viewpoint of obtaining the effect, and 10000.0 ppm or less from the viewpoint of preventing excessive inhibition of the hydrosilylation reaction.
[0170] An example of the adhesive composition used in the present invention may contain a component (B) that does not undergo a curing reaction to become a release agent component together with the curable component (A). By including such a component (B) in the adhesive composition, the resulting adhesive layer can be suitably peeled off with good reproducibility. Typically, such component (B) is a non-curable polyorganosiloxane, and specific examples thereof include, but are not limited to, epoxy group-containing polyorganosiloxane, methyl group-containing polyorganosiloxane, and phenyl group-containing polyorganosiloxane. In addition, the component (B) may be polydimethylsiloxane. The polydimethylsiloxane may be modified. Examples of the polydimethylsiloxane that may be modified include, but are not limited to, epoxy group-containing polydimethylsiloxane, unmodified polydimethylsiloxane, and phenyl group-containing polydimethylsiloxane.
[0171] Preferred examples of the polyorganosiloxane which is component (B) include, but are not limited to, epoxy group-containing polyorganosiloxanes, methyl group-containing polyorganosiloxanes, and phenyl group-containing polyorganosiloxanes.
[0172] The weight average molecular weight of the polyorganosiloxane, which is component (B), is not particularly limited, but is usually 100,000 to 2,000,000, and from the viewpoint of realizing the effects of the present invention with good reproducibility, it is preferably 200,000 to 1,200,000, and more preferably 300,000 to 900,000. The dispersity is not particularly limited, but is usually 1.0 to 10.0, and from the viewpoint of realizing suitable peeling with good reproducibility, it is preferably 1.5 to 5.0, and more preferably 2.0 to 3.0. The weight average molecular weight and dispersity can be measured by the above-mentioned method for polyorganosiloxane. The viscosity of the polyorganosiloxane, which is component (B), is not particularly limited, but is usually 1,000 to 2,000,000 mm 2 The viscosity value of the polyorganosiloxane, which is component (B), is expressed as a kinematic viscosity, and is expressed as centistokes (cSt) = mm 2 / s. Viscosity (mPa s) is density (g / cm 3 That is, the value can be calculated from the viscosity and density measured with an E-type rotational viscometer at 25°C, and the kinematic viscosity (mm 2 / s)=viscosity (mPa s) / density (g / cm 3 ) can be calculated from the formula:
[0173] Examples of epoxy group-containing polyorganosiloxanes include R 11 R 12 SiO 2 / 2 The siloxane unit (D 10 Examples include those containing the unit.
[0174] R 11 is a group bonded to a silicon atom and represents an alkyl group; R 12 is a group bonded to a silicon atom, and represents an epoxy group or an organic group containing an epoxy group. Specific examples of the alkyl group include those listed above. The epoxy group in the epoxy group-containing organic group may be an independent epoxy group that is not condensed with other rings, or may be an epoxy group that forms a condensed ring with other rings, such as a 1,2-epoxycyclohexyl group. Specific examples of organic groups containing an epoxy group include, but are not limited to, 3-glycidoxypropyl and 2-(3,4-epoxycyclohexyl)ethyl. In the present invention, a preferred example of the epoxy group-containing polyorganosiloxane is epoxy group-containing polydimethylsiloxane, but is not limited thereto.
[0175] The epoxy group-containing polyorganosiloxane is a polyorganosiloxane having the above-mentioned siloxane unit (D 10 D 10 In addition to units, Q units, M units and / or T units may be included. In a preferred embodiment of the present invention, specific examples of the epoxy group-containing polyorganosiloxane include 10 Polyorganosiloxane consisting of only units, D 10 Polyorganosiloxanes containing D units and Q units; 10 Polyorganosiloxanes containing D units and M units; 10 Polyorganosiloxanes containing D units and T units; 10 Polyorganosiloxanes containing units, Q units and M units, D 10 Polyorganosiloxanes containing units, M units and T units, D 10 and polyorganosiloxanes containing Q units, M units and T units.
[0176] The epoxy group-containing polyorganosiloxane is preferably an epoxy group-containing polydimethylsiloxane having an epoxy value of 0.1 to 5. In addition, the weight average molecular weight is not particularly limited, but is usually 1,500 to 500,000, and from the viewpoint of suppressing precipitation in the composition, is preferably 100,000 or less.
[0177] Specific examples of the epoxy group-containing polyorganosiloxane include those represented by formulas (E1) to (E3), but are not limited thereto.
[0178] [ka] (m1 and n1 each represent the number of repeating units and are positive integers.)
[0179] [ka] (m2 and n2 each represent the number of repeating units and are positive integers, and R represents an alkylene group having 1 to 10 carbon atoms.)
[0180] [ka] (m3, n3, and o3 each represent the number of repeating units and are positive integers, and R is an alkylene group having 1 to 10 carbon atoms.)
[0181] Examples of the methyl group-containing polyorganosiloxane include R 210 R 220 SiO 2 / 2 The siloxane unit (D 200 units), preferably R 21 R 21 SiO 2 / 2 The siloxane unit (D 20 Examples include those containing the unit.
[0182] R 210 and R 220 are groups bonded to a silicon atom, and each independently represents an alkyl group, with at least one being a methyl group. Specific examples of the alkyl group include those listed above. R 21 is a group bonded to a silicon atom, and represents an alkyl group. Specific examples of the alkyl group include those listed above. 21 As the alkyl group, a methyl group is preferable. In the present invention, a preferred example of the methyl group-containing polyorganosiloxane is polydimethylsiloxane, but is not limited thereto.
[0183] The methyl group-containing polyorganosiloxane is a polyorganosiloxane having the above-mentioned siloxane unit (D 200 Unit or D 20 D 200 Units and D 20 In addition to units, Q units, M units and / or T units may be included.
[0184] In one embodiment of the present invention, specific examples of the methyl group-containing polyorganosiloxane include D 200 Polyorganosiloxane consisting of only units, D 200 Polyorganosiloxanes containing D units and Q units; 200 Polyorganosiloxanes containing D units and M units; 200 Polyorganosiloxanes containing D units and T units; 200 Polyorganosiloxanes containing units, Q units and M units, D 200 Polyorganosiloxanes containing units, M units and T units, D 200 Examples of suitable polyorganosiloxanes include polyorganosiloxanes containing Q, M, and T units.
[0185] In a preferred embodiment of the present invention, specific examples of the methyl group-containing polyorganosiloxane include D 20 Polyorganosiloxane consisting of only units, D 20 Polyorganosiloxanes containing D units and Q units; 20 Polyorganosiloxanes containing D units and M units; 20 Polyorganosiloxanes containing D units and T units; 20 Polyorganosiloxanes containing units, Q units and M units, D 20 Polyorganosiloxanes containing units, M units and T units, D 20 Examples of suitable polyorganosiloxanes include polyorganosiloxanes containing Q, M, and T units.
[0186] Specific examples of methyl group-containing polyorganosiloxanes include, but are not limited to, those represented by formula (M1).
[0187] [ka] (n4 represents the number of repeating units and is a positive integer.)
[0188] Examples of the phenyl group-containing polyorganosiloxane include R 31 R 32 SiO 2 / 2 The siloxane unit (D 30 Examples include those containing the unit.
[0189] R 31 is a group bonded to a silicon atom and represents a phenyl group or an alkyl group; R 32 is a group bonded to a silicon atom and represents a phenyl group. Specific examples of the alkyl group include those listed above, with a methyl group being preferred.
[0190] The phenyl group-containing polyorganosiloxane is a polyorganosiloxane having the above-mentioned siloxane unit (D 30 D 30 In addition to units, Q units, M units and / or T units may be included.
[0191] In a preferred embodiment of the present invention, specific examples of the phenyl group-containing polyorganosiloxane include D 30 Polyorganosiloxane consisting of only units, D 30 Polyorganosiloxanes containing D units and Q units; 30 Polyorganosiloxanes containing D units and M units; 30 Polyorganosiloxanes containing D units and T units; 30 Polyorganosiloxanes containing units, Q units and M units, D 30 Polyorganosiloxanes containing units, M units and T units, D 30 Examples of suitable polyorganosiloxanes include polyorganosiloxanes containing Q, M, and T units.
[0192] Specific examples of the phenyl group-containing polyorganosiloxane include those represented by formula (P1) or (P2), but are not limited thereto.
[0193] [ka] (m5 and n5 each represent the number of repeating units and are positive integers.)
[0194] [ka] (m6 and n6 each represent the number of repeating units and are positive integers.)
[0195] The polyorganosiloxane which is the release agent component (B) may be a commercially available product or may be synthesized. Examples of commercially available polyorganosiloxanes include WACKERSILICONE FLUID AK series (AK50, AK 350, AK 1000, AK 10000, AK 1000000) and GENIOPLAST GUM, which are products of Wacker Chemical Co., Ltd.; dimethyl silicone oil (KF-96L, KF-96A, KF-96, KF-96H, KF-69, KF-965, KF-968), cyclic dimethyl silicone oil (KF-995), manufactured by Shin-Etsu Chemical Co., Ltd.; epoxy group-containing polyorganosiloxane (product name CMS-227, ECMS-327) manufactured by Gelest Co., Ltd.; epoxy group-containing polyorganosiloxane (KF-101, KF-1001, KF-1005, X-22-343) manufactured by Shin-Etsu Chemical Co., Ltd.; Epoxy group-containing polyorganosiloxane (BY16-839); phenyl group-containing polyorganosiloxanes (PMM-1043, PMM-1025, PDM-0421, PDM-0821) manufactured by Gelest, phenyl group-containing polyorganosiloxane (KF50-3000CS) manufactured by Shin-Etsu Chemical Co., Ltd., and phenyl group-containing polyorganosiloxanes (TSF431, TSF433) manufactured by Momentive, but are not limited to these.
[0196] In one embodiment, the adhesive composition used in the present invention contains a component (A) that cures and a component (B) that does not undergo a curing reaction, and in another embodiment, component (B) contains a polyorganosiloxane.
[0197] One example of the adhesive composition used in the present invention can contain component (A) and component (B) in any ratio. Taking into consideration the balance between adhesion and releasability, the ratio of component (A) to component (B) in terms of mass ratio [(A):(B)] is preferably 99.995:0.005 to 30:70, and more preferably 99.9:0.1 to 75:25. That is, when the composition contains a polyorganosiloxane component (A') that cures by a hydrosilylation reaction, the mass ratio of component (A') to component (B) [(A'):(B)] is preferably 99.995:0.005 to 30:70, and more preferably 99.9:0.1 to 75:25.
[0198] The viscosity of the adhesive composition used in the present invention is not particularly limited, but is usually 500 to 20,000 mPa·s, and preferably 1,000 to 1,0000 mPa·s at 25°C.
[0199] An example of an adhesive composition for use in the present invention can be prepared by mixing component (A) and, if used, component (B) and a solvent. The mixing order is not particularly limited, but examples of methods for easily and reproducibly producing an adhesive composition include, but are not limited to, a method of dissolving component (A) and component (B) in a solvent, or a method of dissolving a part of component (A) and component (B) in a solvent and the remaining part in a solvent, and mixing the obtained solutions. In addition, when preparing the adhesive composition, heating may be performed appropriately within a range that does not cause the components to decompose or change in quality. In the present invention, for the purpose of removing foreign matter, the solvent, solution, etc. used may be filtered using a filter during the production of the adhesive composition or after all of the components have been mixed.
[0200] The thickness of the adhesive layer in the laminate of the present invention is not particularly limited, but is usually 5 to 500 μm. From the viewpoint of maintaining film strength, it is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more, and from the viewpoint of avoiding non-uniformity due to a thick film, it is preferably 200 μm or less, more preferably 150 μm or less, even more preferably 120 μm or less, and even more preferably 70 μm or less.
[0201] A method for forming an adhesive layer from the adhesive composition will be described in detail below in the section describing an example of a method for producing a laminate in the first embodiment.
[0202] An example of the configuration of the laminate of the first embodiment will be described below with reference to the drawings. The laminate in FIG. 1 has a semiconductor substrate 1, an adhesive layer 2, a release agent layer 3, and a support substrate 4 in this order. The adhesive layer 2 and the release agent layer 3 are provided between the semiconductor substrate 1 and the support substrate 4. The adhesive layer 2 is in contact with the semiconductor substrate 1. The release agent layer 3 is in contact with the adhesive layer 2 and the support substrate 4.
[0203] <<An example of a method for producing the laminate in the first embodiment>> The method for producing the laminate will be described below by taking the laminate shown in FIG. 1 as an example among the laminates in the first embodiment. An example of the laminate of the present invention can be produced by a method including the following first to third steps. First step: A step of applying an adhesive composition onto a semiconductor substrate to form an adhesive coating layer. Second step: A step of applying a release agent composition onto a supporting substrate to form a release agent layer. The third step is to heat the adhesive layer while the adhesive layer and the release agent layer are in contact with each other, thereby forming an adhesive layer.
[0204] The method for applying the adhesive composition is not particularly limited, but is usually a spin coating method. Alternatively, a method may be adopted in which a coating film is formed by a separate spin coating method or the like to form a sheet-like coating film, and the sheet-like coating film is attached as an adhesive coating layer. The heating temperature of the applied adhesive composition cannot be generally specified because it varies depending on the type and amount of adhesive components contained in the adhesive composition, whether or not a solvent is contained, the boiling point of the solvent used, the desired thickness of the adhesive layer, etc., but is usually 80 to 150°C, and the heating time is usually 30 seconds to 5 minutes. When the adhesive composition contains a solvent, the applied adhesive composition is usually heated. The thickness of the adhesive coating layer obtained by applying the adhesive composition and heating it if necessary is usually about 5 to 500 μm, and is appropriately determined so that the final thickness of the adhesive layer falls within the above-mentioned range.
[0205] The method for applying the release agent composition is not particularly limited, but is usually a spin coating method. The heating temperature of the applied release agent composition cannot be generally specified because it varies depending on the type and amount of the release agent component contained in the release agent composition, the desired thickness of the release agent layer, etc., but from the viewpoint of realizing a suitable release agent layer with good reproducibility, it is 80°C or more and 300°C or less, and the heating time is appropriately determined usually within the range of 10 seconds to 10 minutes depending on the heating temperature. The heating temperature is preferably 100°C or more and 280°C or less, more preferably 150°C or more and 250°C or less. The heating time is preferably 30 seconds or more and 8 minutes or less, more preferably 1 minute or more and 5 minutes or less. Heating can be carried out using a hot plate, an oven, or the like. The thickness of the release agent film obtained by applying the release agent composition and heating it if necessary is usually about 5 nm to 100 μm.
[0206] In the present invention, such coating layers are placed together so as to be in contact with each other, and while performing heat treatment or reduced pressure treatment or both, a load is applied in the thickness direction of the semiconductor substrate and the support substrate to bring the two layers into close contact, and then a post-heat treatment is performed, thereby obtaining the laminate of the present invention. Note that the treatment conditions to be adopted, which are heat treatment, reduced pressure treatment, or a combination of both, are appropriately determined in consideration of various factors such as the type of adhesive composition, the specific composition of the release agent composition, the compatibility of the films obtained from the two compositions, the film thickness, and the desired adhesive strength.
[0207] The heat treatment temperature is usually appropriately determined within the range of 20 to 150° C. from the viewpoint of removing the solvent from the composition, softening the adhesive coating layer to realize suitable bonding with the release agent layer, etc. In particular, from the viewpoint of suppressing or avoiding excessive hardening or unnecessary deterioration of the adhesive component (A), it is preferably 130° C. or less, more preferably 90° C. or less, and the heating time is appropriately determined depending on the heating temperature and the type of adhesive, but from the viewpoint of reliably achieving suitable adhesion, it is usually 30 seconds or more, preferably 1 minute or more, and from the viewpoint of suppressing deterioration of the adhesive layer and other members, it is usually 10 minutes or less, preferably 5 minutes or less.
[0208] The reduced pressure treatment can be carried out by exposing the adhesive coating layer and the release agent layer, which are in contact with each other, to an atmospheric pressure of 10 to 10,000 Pa. The reduced pressure treatment time is usually 1 to 30 minutes.
[0209] From the viewpoint of reproducibly obtaining a laminate from which the substrates can be easily separated, the two layers that contact each other are preferably bonded together by a reduced pressure treatment, more preferably by a combination of a heat treatment and a reduced pressure treatment.
[0210] The load in the thickness direction of the semiconductor substrate and the supporting substrate is not particularly limited as long as it does not adversely affect the semiconductor substrate, the supporting substrate, and the two layers therebetween and can firmly adhere to them, but is usually within the range of 10 to 1000 N.
[0211] The post-heating temperature is preferably 120° C. or higher from the viewpoint of realizing a sufficient curing speed, and is preferably 260° C. or lower from the viewpoint of preventing deterioration of the substrate and each layer. The post-heating time is usually 1 minute or more, and preferably 5 minutes or more, from the viewpoint of achieving suitable bonding of the substrates and layers constituting the laminate, and is usually 180 minutes or less, and preferably 120 minutes or less, from the viewpoint of suppressing or avoiding adverse effects on each layer due to excessive heating. Heating can be performed using a hot plate, an oven, etc. When post-heating is performed using a hot plate, the laminate may be heated with either the semiconductor substrate or the support substrate facing down, but from the viewpoint of achieving suitable peeling with good reproducibility, post-heating is preferably performed with the semiconductor substrate facing down. One purpose of the post-heat treatment is to realize an adhesive layer and a release agent layer that are more suitable as self-supporting films, and in particular to realize favorable hardening by a hydrosilylation reaction.
[0212] An example of a method for producing the laminate of FIG. 1 will now be described with reference to FIGS. 2A to 2C. 2A to 2C are diagrams illustrating one embodiment of the production of a laminate. First, a laminate is prepared in which an adhesive coating layer 2a is formed on a semiconductor substrate 1 (FIG. 2A). This laminate can be obtained, for example, by coating an adhesive composition on the semiconductor substrate 1 and heating it. Separately, a laminate in which a release agent layer 3 is formed on a supporting substrate 4 is prepared (FIG. 2B). This laminate can be obtained, for example, by applying a release agent composition onto the supporting substrate 4 and heating it. 2A and 2B are bonded together so that the adhesive coating layer 2a contacts the release agent layer 3. Then, after applying a load in the thickness direction of the semiconductor substrate 1 and the support substrate 4 under reduced pressure, a heating device (hot plate, not shown) is placed on the surface of the semiconductor substrate 1 opposite to the surface where the adhesive coating layer 2a contacts, and the adhesive coating layer 2a is heated and hardened by the heating device to convert it into the adhesive layer 2 (FIG. 2C). A laminate is obtained by the steps shown in FIGS. 2A to 2C.
[0213] In FIG. 1, the laminate is laminated in the order of the semiconductor substrate 1, the adhesive layer 2, the release agent layer 3, and the support substrate 4, and therefore the above-mentioned manufacturing method is taken as an example. However, when manufacturing a laminate in the order of the semiconductor substrate 1, the release agent layer 3, the adhesive layer 2, and the support substrate 4, for example, the laminate can be manufactured by a method including a first step of applying a release agent composition to the surface of the semiconductor substrate and, if necessary, heating it to form a release agent layer, a second step of applying a release agent composition to the surface of the support substrate and, if necessary, heating it to form an adhesive coating layer, and a third step of bonding the release agent layer of the semiconductor substrate and the adhesive coating layer of the support substrate by applying a load in the thickness direction of the semiconductor substrate and the support substrate while carrying out at least one of a heat treatment and a decompression treatment, and then carrying out a post-heat treatment to form a laminate. As long as the effect of the present invention is not impaired, each composition may be applied and heated sequentially on either one of the substrates.
[0214] <Second embodiment> The laminate having the electronic device layer is used for processing the electronic device layer. During the processing of the electronic device layer, the electronic device layer is adhered to a supporting substrate. After processing of the electronic device layer, the electronic device layer is released from the supporting substrate after, for example, irradiating the release agent layer with light.
[0215] <<Electronic device layer>> The electronic device layer refers to a layer having an electronic device, and in the present invention, refers to a layer in which a plurality of semiconductor chip substrates are embedded in a sealing resin, that is, a layer consisting of a plurality of semiconductor chip substrates and a sealing resin disposed between the semiconductor chip substrates. Here, "electronic device" means a member constituting at least a part of an electronic component. The electronic device is not particularly limited, and may be one in which various mechanical structures or circuits are formed on the surface of a semiconductor substrate. The electronic device is preferably a composite of a member made of a metal or semiconductor and a resin that seals or insulates the member. The electronic device may be one in which a rewiring layer, which will be described later, and / or a semiconductor element or other element is sealed or insulated with a sealing material or an insulating material, and has a single-layer or multi-layer structure.
[0216] <<Support substrate>> Examples of the supporting substrate include those explained in the section "Supporting Substrate" of the first embodiment.
[0217] <<Release agent layer>> The release agent layer is formed using the release agent composition of the present invention described above. The release agent layer is described in detail in the section entitled "Release Agent Layer" in the above-mentioned "First Embodiment."
[0218] <<Adhesive layer>> The adhesive layer is formed using the adhesive composition described above. The detailed description of the adhesive layer is as explained in the section <<Adhesive Layer>> of the <First embodiment>> above.
[0219] An example of the configuration of the laminate of the second embodiment will be described below with reference to the drawings. FIG. 3 shows a schematic cross-sectional view of an example of the laminate of the second embodiment. The laminate in FIG. 3 has a support substrate 24, a release agent layer 23, an adhesive layer 22, and an electronic device layer 26, in that order. The electronic device layer 26 includes a plurality of semiconductor chip substrates 21 and sealing resin 25 that is a sealing material disposed between the semiconductor chip substrates 21 . The adhesive layer 22 and the release agent layer 23 are provided between the electronic device layer 26 and the support substrate 24. The adhesive layer 22 contacts the electronic device layer 26. The release agent layer 23 contacts the adhesive layer 22 and the support substrate 24. Another example of the configuration of the laminate of the second embodiment is shown in FIG. When the release agent layer according to the present invention is an adhesive release agent layer having both a release function and an adhesive function, the laminate may be formed of a single layer structure of a release agent layer having adhesive properties, rather than a two-layer structure of a release agent layer and an adhesive layer. FIG. 4 shows a schematic cross-sectional view of another example of the laminate. The laminate in FIG. 4 includes a support substrate 24, a release agent layer 27 having adhesive properties, and an electronic device layer 26, in that order. The release agent layer 27 having adhesive properties is provided between the support substrate 24 and the electronic device layer 26. The release agent layer 27 having adhesive properties can be prepared by mixing the components of a release agent composition that forms a release agent and the components of an adhesive composition that forms an adhesive layer.
[0220] <<An example of a method for producing a laminate in the second embodiment>> The method for producing the laminate will be described below by taking the laminate shown in FIG. 3 as an example among the laminates in the second embodiment. The laminate of the present invention can be produced, for example, by a method including the following first to fifth steps. First step: A step of applying a release agent composition to the surface of the support substrate to form a release agent coating layer (and, if necessary, further heating to form a release agent layer). The second step is to apply an adhesive composition to the release agent coating layer or to the surface of the release agent layer to form an adhesive coating layer (if necessary, further heat the composition to form an adhesive layer). A third step: placing a semiconductor chip substrate on the adhesive coating layer or adhesive layer, and bonding the semiconductor chip substrate to the adhesive coating layer or adhesive layer while performing at least one of a heat treatment and a decompression treatment. The fourth step is to cure the adhesive layer by post-heat treatment to form an adhesive layer. The fifth step is to seal the semiconductor chip substrate fixed on the adhesive layer with a sealing resin. The third step will be described in more detail below, for example, in the embodiment of step (i) below. (i) A semiconductor chip substrate is placed on the adhesive coating layer or adhesive layer, and while performing at least one of a heat treatment and a decompression treatment, a load is applied in the thickness direction of the semiconductor chip substrate and the support substrate to bring them into close contact, thereby bonding the semiconductor chip substrate to the adhesive coating layer or adhesive layer.
[0221] The fourth step may be performed after bonding the semiconductor chip substrate to the adhesive coating layer in the third step, or may be performed together with the third step. For example, the semiconductor chip substrate may be placed on the adhesive coating layer, and the adhesive coating layer may be heated and cured while applying a load in the thickness direction of the semiconductor chip substrate and the support substrate, thereby bonding the adhesive layer to the semiconductor chip substrate and the adhesive coating layer together and curing the adhesive coating layer to the adhesive layer. In addition, the fourth step may be performed before the third step, and the semiconductor chip substrate may be placed on the adhesive layer, and the adhesive layer and the semiconductor chip substrate may be bonded together while applying a load in the thickness direction of the semiconductor chip substrate and the support substrate.
[0222] The application method, the heating temperature of the applied release agent composition or adhesive composition, the heating means, and the like are as described in the above <<An example of the manufacturing method of the laminate in the first embodiment>> of the above <First embodiment>.
[0223] The procedure of the method for producing the laminate of the second embodiment will be described in more detail below with reference to the drawings. In this method, the laminate shown in FIG. 5A, a release agent coating layer 23' made of a release agent composition is formed on a supporting substrate 24. At that time, the release agent coating layer 23' may be heated to form the release agent layer 23. 5B, an adhesive coating layer 22' made of an adhesive composition is formed on the release agent coating layer 23' or the release agent layer 23. At that time, the adhesive coating layer 22' may be heated to form the adhesive layer 22. 5C, semiconductor chip substrate 21 is placed on adhesive layer 22 or adhesive coating layer 22', and while performing at least one of a heat treatment and a decompression treatment, a load is applied in the thickness direction of semiconductor chip substrate 21 and support substrate 24 to bring them into close contact, thereby bonding semiconductor chip substrate 21 to adhesive layer 22 or adhesive coating layer 22'. When semiconductor chip substrate 21 is bonded to adhesive coating layer 22', adhesive coating layer 22' is post-heat treated to harden it into adhesive layer 22, and semiconductor chip substrate 21 is fixed to adhesive layer 22. When the adhesive coating layer 22' is post-heat treated, the release agent coating layer 23' may also be post-heat treated at the same time, thereby forming the release agent layer 23. Next, as shown in Fig. 5D, the semiconductor chip substrate 21 fixed on the adhesive layer 22 is sealed with sealing resin 25. In Fig. 5D, the multiple semiconductor chip substrates 21 temporarily attached to the support substrate 24 via the adhesive layer 22 are sealed with sealing resin 25. An electronic device layer 26 having the semiconductor chip substrates 21 and the sealing resin 25 disposed between the semiconductor chip substrates 21 is formed on the adhesive layer 22. Thus, the electronic device layer 26 is a base layer in which the multiple semiconductor chip substrates are embedded in the sealing resin.
[0224] <<<Sealing process>>> The semiconductor chip substrate 21 is sealed using a sealing material. As a sealing material for sealing the semiconductor chip substrate 21, a material capable of insulating or sealing a member made of a metal or a semiconductor is used. In the present invention, for example, a resin composition (sealing resin) is used as the sealing material. The type of sealing resin is not particularly limited as long as it can seal and / or insulate metals or semiconductors, but it is preferable to use, for example, an epoxy resin or a silicone resin. The sealing material may contain other components such as a filler in addition to the resin component. Examples of the filler include spherical silica particles. In the sealing process, the sealing resin heated to, for example, 130 to 170° C. is supplied onto the adhesive layer 22 while maintaining a high viscosity so as to cover the semiconductor chip substrate 21, and is compression molded to form a layer made of the sealing resin 25 on the adhesive layer 22. At this time, the temperature condition is, for example, 130 to 170° C. The pressure applied to the semiconductor chip substrate 21 is, for example, 50 to 500 N / cm 2 It is.
[0225] (Method of Manufacturing Processed Semiconductor Substrate or Electronic Device Layer) The laminate according to the invention can be used to provide a method for producing a processed semiconductor substrate or a processed electronic device layer. The "method for producing a processed semiconductor substrate" uses the laminate described in the "First embodiment" section of the (Laminate) above. The "method for producing a processed electronic device layer" uses the laminate described in the "Second embodiment" section of the (Laminate) above. The "method for producing a processed semiconductor substrate" will be described in the <Third embodiment> below, and the "method for producing a processed electronic device layer" will be described in the <Fourth embodiment> below.
[0226] <Third embodiment> The method for producing a processed semiconductor substrate of the present invention includes the following step 5A and step 6A. The method for producing a processed electronic device layer may further include the following step 7A. Here, step 5A is a step of processing the semiconductor substrate in the laminate described in the above section <First embodiment>. Step 6A is a step of separating the semiconductor substrate processed in step 5A from the supporting substrate. Moreover, the 7A step is a step of cleaning the processed semiconductor substrate after the 6A step.
[0227] The processing performed on the semiconductor substrate in the 5A step is, for example, processing of the side opposite to the circuit surface of the wafer, and includes thinning the wafer by polishing the back surface of the wafer. After that, for example, through silicon vias (TSVs) are formed, and then the thinned wafer is peeled off from the support substrate to form a wafer stack, which is then three-dimensionally mounted. In addition, for example, before or after that, wafer back electrodes are formed. During the wafer thinning and TSV process, heat of about 250 to 350° C. is applied while the wafer is attached to the support substrate. The laminate of the present invention, including the adhesive layer, is usually heat-resistant to the load. The processing performed on the semiconductor substrate in step 5A may be a step of dicing (dividing) the semiconductor substrate. In addition, the processing is not limited to the above, and also includes, for example, the implementation of a mounting process for semiconductor components when a base material for mounting semiconductor components is temporarily bonded to a support substrate to support the base material.
[0228] In step 6A, the method of separating (peeling) the semiconductor substrate from the support substrate includes, but is not limited to, mechanical peeling using a tool having a sharp part after irradiating the release agent layer with light, or peeling between the support and the semiconductor wafer. By irradiating the release agent layer with light from the supporting substrate side, the release agent layer is altered (e.g., separated or decomposed) as described above, and then, for example, one of the substrates can be pulled up to easily separate the semiconductor substrate and the supporting substrate.
[0229] The light irradiation to the release agent layer does not necessarily have to be performed on the entire area of the release agent layer. Even if the light-irradiated area and the non-irradiated area are mixed, as long as the release ability of the release agent layer as a whole is sufficiently improved, the semiconductor substrate and the support substrate can be separated by a slight external force such as pulling up the support substrate. The ratio and positional relationship between the light-irradiated area and the non-irradiated area vary depending on the type and specific composition of the adhesive used, the thickness of the adhesive layer, the thickness of the adhesive layer, the thickness of the release agent layer, the intensity of the light irradiated, etc., but a person skilled in the art can set the conditions appropriately without requiring excessive testing. For these reasons, according to the manufacturing method of the processed semiconductor substrate of the present invention, for example, when the support substrate of the laminate used has light transparency, it is possible to shorten the light irradiation time when peeling by light irradiation from the support substrate side, and as a result, not only can the throughput be improved, but also the physical stress for peeling can be avoided, and the semiconductor substrate and the support substrate can be easily and efficiently separated only by light irradiation. Typically, the amount of light used for peeling is 50 to 3,000 mJ / cm 2 The irradiation time is appropriately determined depending on the wavelength and the amount of irradiation.
[0230] As described above, the wavelength of the light used for peeling is preferably, for example, 250 to 600 nm, more preferably 250 to 370 nm. More preferably, the wavelength is 308 nm, 343 nm, 355 nm, 365 nm, or 532 nm. The amount of light required for peeling is an amount that can cause suitable alteration, such as decomposition, of the novolac resin. The light used for the peeling may be laser light or non-laser light emitted from a light source such as an ultraviolet lamp.
[0231] The substrate can be cleaned by spraying the cleaning composition onto at least one of the surfaces of the separated semiconductor substrate and the supporting substrate, or by immersing the separated semiconductor substrate or the supporting substrate in the cleaning composition. In addition, the surface of the processed semiconductor substrate or the like may be cleaned using a removal tape or the like. As an example of cleaning the substrate, step 7A of cleaning the processed semiconductor substrate may be performed after step 6A. Examples of the detergent composition used for cleaning include the following.
[0232] The cleaning composition typically contains a salt and a solvent. A suitable example of the cleaning composition is a cleaning composition containing a quaternary ammonium salt and a solvent. The quaternary ammonium salt is composed of a quaternary ammonium cation and an anion, and is not particularly limited as long as it is used for this type of application. A typical example of such a quaternary ammonium cation is a tetra(hydrocarbon)ammonium cation. On the other hand, an anion paired with the quaternary ammonium cation is a hydroxide ion (OH - ); Fluorine ion (F - ), chloride ion (Cl - ), bromide ion (Br - ), iodine ion (I - ) and other halogen ions; tetrafluoroborate ion (BF4 - ); Hexafluorophosphate ion (PF6 - ) and the like, but are not limited to these.
[0233] The quaternary ammonium salt is preferably a halogen-containing quaternary ammonium salt, and more preferably a fluorine-containing quaternary ammonium salt. In the quaternary ammonium salt, the halogen atom may be contained in either the cation or the anion, but is preferably contained in the anion.
[0234] In a preferred embodiment, the fluorine-containing quaternary ammonium salt is a tetra(hydrocarbon)ammonium fluoride. Specific examples of the hydrocarbon group in the tetra(hydrocarbon)ammonium fluoride include an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an alkynyl group having 2 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms. In a more preferred embodiment, the tetra(hydrocarbon)ammonium fluoride comprises a tetraalkylammonium fluoride. Specific examples of tetraalkylammonium fluoride include, but are not limited to, tetramethylammonium fluoride, tetraethylammonium fluoride, tetrapropylammonium fluoride, tetrabutylammonium fluoride (also called tetrabutylammonium fluoride), etc. Among these, tetrabutylammonium fluoride is preferred.
[0235] The quaternary ammonium salts such as tetra(hydrocarbon)ammonium fluoride may be used in the form of a hydrate. The quaternary ammonium salts such as tetra(hydrocarbon)ammonium fluoride may be used alone or in combination of two or more. The amount of the quaternary ammonium salt is not particularly limited as long as it dissolves in the solvent contained in the cleaning composition, but is usually 0.1 to 30% by mass based on the cleaning composition.
[0236] The solvent contained in the cleaning composition is not particularly limited as long as it is used for this type of application and can dissolve salts such as quaternary ammonium salts. From the viewpoint of reproducibly obtaining a cleaning composition having excellent cleaning properties and obtaining a cleaning composition with excellent uniformity by satisfactorily dissolving salts such as quaternary ammonium salts, the cleaning composition preferably contains one or more amide solvents.
[0237] A suitable example of the amide solvent is an acid amide derivative represented by the formula (Z). [ka]
[0238] In the formula, R 0 R represents an ethyl group, a propyl group, or an isopropyl group, preferably an ethyl group or an isopropyl group, and more preferably an ethyl group. A and R Beach independently represents an alkyl group having 1 to 4 carbon atoms. The alkyl group having 1 to 4 carbon atoms may be linear, branched, or cyclic, and specific examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, a cyclopropyl group, an n-butyl group, an isobutyl group, an s-butyl group, a t-butyl group, and a cyclobutyl group. Of these, R A and R B As the alkyl group, a methyl group or an ethyl group is preferable, and it is more preferable that both are methyl groups or ethyl groups, and it is even more preferable that both are methyl groups.
[0239] Examples of the acid amide derivative represented by formula (Z) include N,N-dimethylpropionamide, N,N-diethylpropionamide, N-ethyl-N-methylpropionamide, N,N-dimethylbutyric acid amide, N,N-diethylbutyric acid amide, N-ethyl-N-methylbutyric acid amide, N,N-dimethylisobutyric acid amide, N,N-diethylisobutyric acid amide, N-ethyl-N-methylisobutyric acid amide, etc. Among these, N,N-dimethylpropionamide and N,N-dimethylisobutyric acid amide are particularly preferred, and N,N-dimethylpropionamide is more preferred.
[0240] The acid amide derivative represented by formula (Z) may be synthesized by a substitution reaction between a corresponding carboxylic acid ester and an amine, or a commercially available product may be used.
[0241] Another example of a preferred amide solvent is a lactam compound represented by the formula (Y). [ka]
[0242] In formula (Y), R 101 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; R 102represents an alkylene group having 1 to 6 carbon atoms. Specific examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an n-butyl group, and specific examples of the alkylene group having 1 to 6 carbon atoms include, but are not limited to, a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, and a hexamethylene group.
[0243] Specific examples of the lactam compound represented by formula (Y) include α-lactam compounds, β-lactam compounds, γ-lactam compounds, δ-lactam compounds, etc., which can be used alone or in combination of two or more.
[0244] In a preferred embodiment, the lactam compound represented by formula (Y) comprises 1-alkyl-2-pyrrolidone (N-alkyl-γ-butyrolactam), in a more preferred embodiment, N-methylpyrrolidone (NMP) or N-ethylpyrrolidone (NEP), and in an even more preferred embodiment, N-methylpyrrolidone (NMP).
[0245] The cleaning composition may contain one or more other organic solvents different from the above-mentioned amide compound. Such other organic solvents are not particularly limited as long as they are used for this type of application and are compatible with the above-mentioned amide compound. Preferred other solvents include, but are not limited to, alkylene glycol dialkyl ethers, aromatic hydrocarbon compounds, cyclic structure-containing ether compounds, and the like. The amount of the organic solvent other than the above-mentioned amide compound is appropriately determined so that the amount is usually 95 mass % or less of the solvent contained in the cleaning composition, as long as the quaternary ammonium salt contained in the cleaning composition does not precipitate or separate and is uniformly mixed with the above-mentioned amide compound. The cleaning composition may contain water as a solvent, but from the viewpoint of avoiding corrosion of the substrate, etc., usually, only an organic solvent is intentionally used as a solvent. In this case, it is not denied that the hydration water of the salt or a trace amount of water contained in the organic solvent may be contained in the cleaning composition. The water content of the cleaning composition is usually 5 mass% or less.
[0246] The constituent elements and methodological elements of the above-described steps of the method for producing a processed semiconductor substrate of the present invention may be modified in various ways without departing from the spirit and scope of the present invention. The method for producing a processed semiconductor substrate of the present invention may include steps other than those described above.
[0247] In the peeling method of the present invention, when the semiconductor substrate or the supporting substrate of the laminate of the present invention has optical transparency, the semiconductor substrate and the supporting substrate of the laminate are separated by irradiating the release agent layer with light from the semiconductor substrate side or the supporting substrate side. In one example of the laminate of the present invention, the semiconductor substrate and the support substrate are temporarily bonded by the adhesive layer and the release agent layer in a suitably peelable manner, so that, for example, when the support substrate has optical transparency, the semiconductor substrate and the support substrate can be easily separated by irradiating the release agent layer with light from the support substrate side of the laminate. Usually, the peeling is performed after the semiconductor substrate of the laminate has been processed.
[0248] An example of the third embodiment will be described with reference to Figures 6A to 6D. This example is an example of manufacturing a thinned semiconductor substrate. First, a laminate is prepared (FIG. 6A). This laminate is the same as the laminate shown in FIGS. 1 and 2C. Next, a polishing device (not shown) is used to polish the surface of the semiconductor substrate 1 opposite to the surface in contact with the adhesive layer 2, thereby thinning the semiconductor substrate 1 (FIG. 6B). Note that the thinned semiconductor substrate 1 may be subjected to formation of a through electrode or the like. Next, the release agent layer 3 is irradiated with light from the support substrate 4 side, and then a peeling device (not shown) is used to separate the thinned semiconductor substrate 1 from the support substrate 4 (FIG. 6C). A thinned semiconductor substrate 1 is then obtained (FIG. 6D). Here, residues of the adhesive layer 2 and the release agent layer 3 may remain on the thinned semiconductor substrate 1. Therefore, it is preferable to clean the thinned semiconductor substrate 1 with a cleaning agent composition to remove the residues of the adhesive layer 2 and the release agent layer 3 from the semiconductor substrate 1.
[0249] <Fourth embodiment> The method for producing a processed electronic device layer of the present invention includes the following step 5B and step 6B. The method for producing a processed electronic device layer may further include the following step 7B. Here, step 5B is a step of processing the electronic device layer in the laminate described in the section <Second embodiment> above. Step 6B is a step of separating the electronic device layer processed in step 5B from the supporting substrate. Step 7B is a step of cleaning the processed electronic device layer after step 6B. A specific example of the fourth embodiment will be described below with reference to FIGS. 7A to 7F.
[0250] Examples of the processing performed on the electronic device layer in the step 5B include a grinding step and a wiring layer forming step.
[0251] <<Grinding process>> The grinding step is a step of grinding away the resin portion of the layer of sealing resin 25 in electronic device layer 26 so that a part of semiconductor chip substrate 21 is exposed. Grinding of the sealing resin portion is performed, for example, as shown in Fig. 7B, by grinding the layer of sealing resin 25 of the laminate shown in Fig. 7A until it has a thickness substantially equal to that of the semiconductor chip substrate 21. The laminate shown in Fig. 7A is the same laminate as the laminate shown in Figs. 3 and 5D.
[0252] <<Wiring layer formation process>> The wiring layer forming step is a step of forming a wiring layer on the semiconductor chip substrate 21 exposed after the grinding step. In FIG. 7C, a wiring layer 28 is formed on an electronic device layer 26 made up of a semiconductor chip substrate 21 and a layer of sealing resin 25. In FIG. The wiring layer 28 is also called an RDL (Redistribution Layer), and is a thin-film wiring body that constitutes wiring connected to a substrate, and may have a single-layer or multi-layer structure. x The wiring may be formed by a conductor (for example, a metal such as aluminum, copper, titanium, nickel, gold, or silver, or an alloy such as a silver-tin alloy) between a metal layer (such as a photosensitive resin such as a photosensitive epoxy, or the like), but is not limited to this. The wiring layer 28 may be formed, for example, by the following method. First, silicon oxide (SiO x ) and a dielectric layer of photosensitive resin or the like is formed. The dielectric layer made of silicon oxide can be formed by, for example, a sputtering method, a vacuum deposition method, or the like. The dielectric layer made of photosensitive resin can be formed by applying the photosensitive resin onto the layer of sealing resin 25 by, for example, a method such as spin coating, dipping, roller blade, spray coating, or slit coating. Next, wiring is formed on the dielectric layer using a conductor such as a metal. As a method for forming the wiring, for example, a known semiconductor process such as a lithography process such as photolithography (resist lithography) or an etching process can be used. As such a lithography process, for example, a lithography process using a positive resist material and a lithography process using a negative resist material can be used. In the method for manufacturing a laminate according to the fourth embodiment, it is further possible to form bumps or mount elements on the wiring layer 28. Mounting elements on the wiring layer 28 can be performed using, for example, a chip mounter or the like. The laminate of the fourth embodiment may be a laminate produced in a process based on fan-out technology, in which terminals provided on a semiconductor chip substrate are mounted on a wiring layer that extends outside the chip area.
[0253] In step 6B, the method of separating (peeling) the electronic device layer from the support substrate may be, but is not limited to, mechanical peeling using a material having a sharp portion after irradiating the release agent layer with light, or peeling between the support and the electronic device layer. By irradiating the release agent layer with light from the supporting substrate side, the release agent layer is altered (e.g., separated or decomposed) as described above, and then, for example, one of the substrates can be pulled up to easily separate the electronic device layer from the supporting substrate.
[0254] 7D to 7E are schematic cross-sectional views for explaining a method for separating the laminate, and FIG. 7F is a schematic cross-sectional view for explaining a cleaning method after separation of the laminate. One embodiment of a method for manufacturing a semiconductor package (electronic component) can be explained with reference to FIG. 7D to FIG. 7F. The step of separating the laminate is a step of irradiating light (arrow) through support substrate 24 to release agent layer 23 to alter the properties of release agent layer 23, thereby separating electronic device layer 26 from support substrate 24, as shown in FIG. 7D. Release agent layer 23 is irradiated with light (arrow) to modify release agent layer 23, and then support substrate 24 is separated from electronic device layer 26 as shown in FIG. 7E. The conditions and method of irradiating the adhesive layer with light are as explained in the section of <Third embodiment> above.
[0255] The substrate can be cleaned by spraying the cleaning composition onto at least one of the surfaces of the separated electronic device layer and the supporting substrate, or by immersing the separated electronic device layer or the supporting substrate in the cleaning composition. In addition, the surface of the processed electronic device layer or the like may be cleaned using a removal tape or the like. For example, in Fig. 7E, after the separation step, adhesive layer 22 and release agent layer 23 are attached to electronic device layer 26, but adhesive layer 22 and release agent layer 23 can be removed by decomposing adhesive layer 22 and release agent layer 23 using a cleaning composition such as an acid or alkali. By removing the release agent layer and adhesive layer, a processed electronic device layer (electronic component) as shown in Fig. 7F can be suitably obtained.
[0256] Various modifications of the components and methodological elements of the above-described steps of the method for producing a processed electronic device layer of the present invention may be made without departing from the spirit and scope of the present invention. The method of producing a processed electronic device layer of the present invention may include steps other than those described above.
[0257] In the laminate of the present invention, since the electronic device layer and the support substrate are temporarily bonded by the adhesive layer in a suitably peelable manner, for example, when the support substrate has optical transparency, the electronic device layer and the support substrate can be easily separated by irradiating the release agent layer with light from the support substrate side of the laminate. Peeling is usually performed after processing the electronic device layer of the laminate. EXAMPLES
[0258] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples. The following apparatuses were used.
[0259] [Device] (1) Mixer: Thinky Planetary Mixer ARE-500 (2) Rheometer: Anton Paar Japan Co., Ltd. Viscoelasticity measuring device MCR302 (3) Vacuum bonding device: SUSS MicroTec, manual bonder (4) High-rigidity grinding machine: HRG300 manufactured by Tokyo Seimitsu Co., Ltd. (5) Laser irradiation device (Lambda SX, manufactured by Coherent, Inc.)
[0260] [Molecular weight measurement conditions] The weight average molecular weight was measured using a GPC apparatus (EcoSEC, HLC-8220GPC manufactured by Tosoh Corporation) and GPC columns (Shodex KF-803L, KF-802, and KF-801 manufactured by Showa Denko K.K., in this order), with a column temperature of 40° C., tetrahydrofuran (THF) as an eluent (elution solvent), a flow rate (flow velocity) of 1.00 mL / min, and polystyrene (manufactured by Sigma-Aldrich) as a standard sample.
[0261] [1] Preparation of adhesive composition [Preparation Example 1] In a 600 mL container for the stirrer, 80 g of MQ resin (manufactured by Wacker Chemical Industries, Ltd.) containing a polysiloxane skeleton and vinyl groups, 2.52 g of SiH group-containing linear polydimethylsiloxane (manufactured by Wacker Chemical Industries, Ltd.) with a viscosity of 100 mPa·s, 5.89 g of SiH group-containing linear polydimethylsiloxane (manufactured by Wacker Chemical Industries, Ltd.) with a viscosity of 70 mPa·s, and 0.22 g of 1-ethynyl-1-cyclohexanol (manufactured by Wacker Chemical Industries, Ltd.) were placed and stirred with the stirrer for 5 minutes. To the resulting mixture, 0.147 g of platinum catalyst (manufactured by Wacker Chemical Co.) and 5.81 g of vinyl-containing linear polydimethylsiloxane with a viscosity of 1,000 mPa s (manufactured by Wacker Chemical Co.) were stirred for 5 minutes using a stirrer, and 3.96 g of the mixture obtained separately was added and stirred for 5 minutes using a stirrer. Finally, the resulting mixture was filtered through a 300 mesh nylon filter to obtain an adhesive composition.
[0262] [2] Preparation of cleaning composition [Preparation Example 2] 5 g of tetrabutylammonium fluoride trihydrate (manufactured by Kanto Chemical Co., Ltd.) was mixed with 95 g of N-methyl-2-pyrrolidone and thoroughly stirred to obtain a cleaning composition.
[0263] [3] Synthesis of organic resin (novolac resin) [Synthesis Example 1] Into a flask were placed 56.02 g of N-phenyl-1-naphthylamine, 50.00 g of 1-pyrenecarboxaldehyde, 6.67 g of 4-(trifluoromethyl)benzaldehyde, and 2.46 g of methanesulfonic acid, and then 86.36 g of 1,4-dioxane and 86.36 g of toluene were added, and the mixture was refluxed and stirred under a nitrogen atmosphere for 18 hours. After cooling the reaction mixture, 96 g of tetrahydrofuran was added to dilute it, and the resulting diluted solution was dropped into methanol to obtain a precipitate. The resulting precipitate was collected by filtration, washed with methanol, and dried under reduced pressure at 60°C to obtain 72.12 g of novolac resin. The weight average molecular weight was measured by the above-mentioned method, and the weight average molecular weight of the polymer novolac resin was 1,100.
[0264] [4] Branched chain polysilane (polysilane) The polysilanes manufactured by Osaka Gas Chemicals Co., Ltd. (OGSOL SI-20-10 and OGSOL SI-20-14) are branched polysilanes represented by the formula (X-1). The weight average molecular weights of OGSOL SI-20-10 and OGSOL SI-20-14 were measured by the above-mentioned method, and the weight average molecular weights were 1,380 and 4,620, respectively. [ka] (Ph represents a phenyl group, R represents a terminal substituent, represents an atom or a group, and n represents the number of repeating units.)
[0265] [5] Preparation of stripping agent composition [Examples 1 to 18, Comparative Examples 1 to 3] The above Synthesis Example 1, crosslinking agent, curing catalyst, polysilane compound, antioxidant, and solvent were mixed in the ratio shown in Table 1, and filtered using a 0.2 μm polyethylene microfilter to obtain a release agent composition.
[0266] [Table 1]
[0267] The correspondence between the compounds abbreviated in Table 1 is as follows: PGME-BIP-A: Phenol, 4,4'-(1-methylethylidene)bis[2,6-bis[(2-methoxy-1-methylethoxy)methyl]]- ·TMOM-BP : 3,3',5,5'-Tetrakis(methoxymethyl)-[1,1'-biphenyl]-4,4'-diol PyPTS: Pyridinium-p-toluenesulfonate PyPSA: Pyridinium-p-hydroxybenzenesulfonic acid ·PGME: Propylene glycol monomethyl ether ·PGMEA: Propylene glycol monomethyl ether acetate The antioxidants in Table 1 are as follows:
[0268] [ka] TIFF2024135070000052.tif107167 [ka]
[0269] [Thermal stability test] The stripping agent compositions prepared in Examples 1 to 14 and Comparative Examples 1 and 2 were heated in solution at 90°C for 24 hours. 1 mL of the stripping agent composition before and after heating was diluted with 4 mL of THF, and the molecular weight was measured by GPC. The peaks of THF and the solvent appeared at known peak positions away from the stripping agent composition, so that the molecular weight of the components other than the solvent can be calculated below without being influenced by THF and the solvent. The weight average molecular weight was measured before and after heating, and the change in molecular weight was calculated by [(weight average molecular weight after heating) / (weight average molecular weight before heating)]×100. The results are shown in Table 2.
[0270] [Table 2]
[0271] As shown in Table 2, the stripping agent compositions containing an antioxidant in Examples 1 to 14 showed that the molecular weight change during heating was kept to 105% or less, demonstrating their stability during heating. On the other hand, in Comparative Examples 1 and 2 not containing an antioxidant, an increase in molecular weight was observed upon heating. From this, it was confirmed that a stripping agent composition with high thermal stability can be obtained by adding an antioxidant to a stripping agent composition containing an antioxidant.
[0272] [Qualitative storage test] The release agent compositions prepared in Examples 1 and 7 and Comparative Example 1 were stored at 35° C. for one month. The weight average molecular weights were measured before storage, after two weeks, and after one month, and the change in molecular weight was calculated by dividing the weight average molecular weight before and after storage by the weight average molecular weight before heating × 100. The results are shown in Table 3.
[0273] [Table 3]
[0274] As shown in Table 3, it was confirmed that the release agent composition containing the antioxidant had less change in molecular weight and higher storage stability than the release agent composition of Comparative Example 1 even after storage at 35°C for 2 weeks and 1 month.
[0275] [Production of laminate and confirmation of peelability by light irradiation and cleaning ability by detergent composition] The release agent composition prepared in Example 15 was spin-coated onto a 301 mm glass wafer (EAGLE-XG, Corning, thickness 700 μm) as a carrier-side substrate such that the film thickness in the final laminate was 200 nm, forming a release agent coating layer on the glass wafer as a supporting substrate. On the other hand, the adhesive composition obtained in Preparation Example 1 was spin-coated onto a 300 mm silicon wafer (thickness 775 μm) as the device side substrate so that the film thickness in the final laminate was 60 μm, forming an adhesive coating layer on the silicon wafer as the semiconductor substrate. Then, using a bonding device, the glass wafer and the silicon wafer were bonded together so as to sandwich the release agent coating layer and the adhesive coating layer, and then a post-heat treatment was performed at 200°C for 10 minutes to produce a laminate. The bonding was performed at a temperature of 23°C and a reduced pressure of 1,500 Pa.
[0276] The silicon wafer of the obtained laminate was thinned to 50 μm using a high-rigidity grinder, and the laminate was then placed in an oven and subjected to high-temperature treatment at 250° C. for 1 hour. The laminate was then allowed to cool, and attached and fixed to a dicing tape (DU-300, manufactured by Nitto Denko Corporation) with the thinned silicon wafer side facing down. Using a laser irradiation device, a laser with a wavelength of 308 nm was irradiated onto the peelable layer from the glass wafer side of the fixed laminate, and the lowest irradiation amount at which peeling occurred was determined as the optimal irradiation amount. Then, a laser with a wavelength of 308 nm was irradiated onto the entire surface of the peelable layer from the glass wafer side of the fixed laminate at the optimal irradiation amount, and the support substrate was manually lifted up to confirm whether peeling was possible. After the peeled and fixed semiconductor substrate was removed, the separated semiconductor wafer and glass wafer were each cut into 4 cm x 4 cm pieces, and the cut wafers were immersed in 7 mL of the cleaning composition obtained in Preparation Example 2 for 10 minutes, and the presence or absence of a residue such as a film remaining on the surface of the wafer was visually confirmed (cleaning property test). In addition, the cleaning composition after cleaning the wafer was collected, and the presence or absence of foreign matter remaining in the composition was visually confirmed (foreign matter confirmation).
[0277] Laminates were produced in the same manner as above, except that the release agent compositions prepared in Examples 16, 17, 18, and Comparative Example 3 were used instead of the release agent composition prepared in Example 15, and the release properties were confirmed, and a cleaning property test and foreign matter confirmation were performed.
[0278] [Table 4]
[0279] As described above, the semiconductor substrate and the support substrate of the laminate having the film obtained using the stripping composition of Examples 15 to 18 and Comparative Example 3 as a release layer were separated by irradiating the release layer with light. As shown in Table 4, in all Examples and Comparative Examples, the separated substrates were washed with the cleaning composition, and could be suitably washed without leaving any residue on the substrate. In addition, no foreign matter was found in each of the cleaning compositions used to wash each substrate. From this result, it was confirmed that the stripping composition containing the antioxidant of Examples 15 to 18 could obtain a film suitable as a release layer that exhibits good removability or solubility even after stripping, especially after stripping by light irradiation, similar to the stripping composition not containing the antioxidant of Comparative Example 3. From this, it was confirmed that the release agent composition containing the added antioxidant has good removability or solubility after the formation of the release layer, and also suppresses changes in molecular weight in the solution, resulting in excellent long-term storage stability. [Explanation of symbols]
[0280] 1. Semiconductor substrate 2 Adhesive layer 2a Adhesive coating layer 3 Release agent layer 4 Support substrate 21 Semiconductor chip substrate 22 Adhesive layer 23 Release agent layer 24 Support substrate 25 Sealing resin 26 Electronic Device Layer 27 Release agent layer with adhesive properties 28 wiring layer
Claims
1. A semiconductor substrate; A support substrate; A release agent composition for forming a release layer of a laminate having an adhesive layer and a release layer provided between the semiconductor substrate and the support substrate, comprising: A stripping agent composition comprising an organic resin, a branched polysilane, an antioxidant, and a solvent.
2. 2. The stripping agent composition according to claim 1, wherein the antioxidant is at least one selected from the group consisting of a phenol-based antioxidant, an amine-based antioxidant, a phosphoric acid-based antioxidant, and a sulfide-based antioxidant.
3. The stripping composition according to claim 2 , wherein the phenol-based antioxidant is a compound having a group represented by the following formula (1): [Formula 1] (In the formula, R 1 represents an alkyl group having 1 to 10 carbon atoms; R 2 ~R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and * represents a bond.
4. The stripping composition according to claim 2 , wherein the amine-based antioxidant is a compound having a group represented by the following formula (2): [chemical 2] (In the formula, R 5 represents a hydrogen atom, an oxy radical group, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms, and * represents a bond.
5. 3. The stripping agent composition according to claim 2, wherein the phosphoric acid-based antioxidant is a compound represented by the following formula (3) or (4), and the sulfide-based antioxidant is a compound represented by the following formula (5) or (6): [C3] (In the formula, R 6 ~R 8 represents an alkyl group having 1 to 12 carbon atoms, or an aryl group which may be substituted with an alkyl group. [C4] (In the formula, R 9 ~R 10 represents an alkyl group having 1 to 12 carbon atoms, or an aryl group which may be substituted with an alkyl group. [C5] (In the formula, R 11 ~R 12 represents an alkyl group having 1 to 12 carbon atoms. [C6] (In the formula, R 13 ~R 16 represents an alkyl group having 1 to 12 carbon atoms.
6. The stripping composition according to claim 1 , wherein the branched chain polysilane has a structure represented by the following formula (B): [C7] (In the formula, R B represents a hydrogen atom, a hydroxyl group, a silyl group, or an organic group.
7. The R B The stripping composition according to claim 6, wherein is a phenyl group.
8. 2. The stripping composition according to claim 1, wherein the organic resin is a novolak resin.
9. The release agent composition according to claim 8, wherein the novolak resin is a polymer containing one or more units selected from the group consisting of units represented by formula (C1-1), units represented by formula (C1-2), and units represented by formula (C1-3). [C8] (In the formula, C 1 represents a group derived from an aromatic compound containing a nitrogen atom, C 2 represents a group containing a tertiary carbon atom having at least one member selected from the group consisting of a secondary carbon atom, a quaternary carbon atom, and an aromatic ring in a side chain, 3 represents a group derived from an aliphatic polycyclic compound, C 4represents a group derived from phenol, a group derived from bisphenol, a group derived from naphthol, a group derived from biphenyl, or a group derived from biphenol.
10. The stripping composition according to claim 1, which contains a crosslinking agent.
11. a semiconductor substrate or electronic device layer; A support substrate; a release agent layer provided between the semiconductor substrate or the electronic device layer and the support substrate; A laminate, wherein the release agent layer is formed from the release agent composition according to any one of claims 1 to 10.
12. The laminate according to claim 11 , further comprising an adhesive layer provided between the semiconductor substrate or the electronic device layer and the support substrate.
13. 1. A method for producing a processed semiconductor substrate or electronic device layer, comprising the steps of: A step 5A in which the semiconductor substrate of the laminate according to claim 11 is processed, or a step 5B in which the electronic device layer of the laminate according to claim 11 is processed; a 6A step in which the semiconductor substrate processed in the 5A step is separated from the support substrate, or a 6B step in which the electronic device layer processed in the 5B step is separated from the support substrate; 2. A method for producing a processed semiconductor substrate or electronic device layer, comprising:
14. 14. The method for producing a processed semiconductor substrate or electronic device layer according to claim 13, wherein the support substrate is optically transparent, and step 6A or step 6B comprises irradiating the laminate with a laser from the support substrate side.
Citation Information
Patent Citations
Multilayer body, release agent composition, and method for producing processed semiconductor substrate
WO2022019211A1
Cited By
Composition for forming coating film for adhesive removal, laminate, method for producing laminate, and method for producing processed semiconductor substrate or electronic device layer
WO2026204966A1