Method for producing modified polylactic resin, modified polylactic resin, and polylactic resin foam sheet

A controlled extrusion process with temperature management and twin-screw extrusion suppresses gel fraction increase, producing high-quality polylactic acid resin foam sheets with improved appearance and foaming characteristics.

JP2024135082APending Publication Date: 2024-10-04SEKISUI PLASTICS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023045596
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

The gel fraction of modified polylactic acid resin affects the appearance of resulting polylactic acid resin foam sheets, leading to deterioration when it increases.

Method used

A method for producing modified polylactic acid resin involving a modification step in an extruder with controlled temperature zones and kneading sections, maintaining the gel fraction below 10% by mass, and using specific conditions to suppress its increase, along with a twin-screw extruder for uniform dispersion.

Benefits of technology

The method produces a modified polylactic acid resin with low gel fraction, ensuring excellent appearance and foaming properties in the resulting foam sheets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135082000001_ABST
    Figure 2024135082000001_ABST
Patent Text Reader

Abstract

To provide a method for producing a modified polylactic resin, which can suppress the increase of a gel fraction of the obtained modified polylactic resin, a modified polylactic resin of a limited gel fraction obtained by such a method, and a polylactic resin foam sheet having a good appearance and obtained from such a modified polylactic resin.SOLUTION: This method for producing the modified polylactic resin comprises a modification step of modifying a polylactic resin in an extruder. The extruder includes, sequentially from an upstream side to a downstream side, a feed part to which the polylactic resin is fed, a reaction part in which the polylactic resin is modified, and a mixing part that mixes a resin composition obtained in the reaction part. The set temperature of the feed part is 180°C or lower, and the gel fraction of the obtained modified polylactic resin less than 10% by mass.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a modified polylactic acid resin, a modified polylactic acid resin, and a polylactic acid resin foam sheet. [Background technology]

[0002] Resin foam sheets are lightweight, have excellent cushioning properties, and can be easily molded into a variety of shapes, so they are used as a raw material for various molded products, including packaging materials.

[0003] In recent years, resin foam sheets, which are used in large quantities and then discarded in large quantities, have placed a heavy burden on the environment and become a cause of various social problems such as global warming, resource depletion, waste disposal, etc. In response to this, a polylactic acid resin foam sheet has been proposed that uses polylactic acid resin, which is biodegradable, has a small environmental impact, and can be produced relatively inexpensively (for example, Patent Document 1).

[0004] As a method for producing a polylactic acid resin foam sheet having excellent foaming properties, a method for producing an extrusion foam sheet using a modified polylactic acid resin has been reported (Patent Document 2).

[0005] When further improvements were considered for the polylactic acid resin foam sheet using such a modified polylactic acid resin, it was found that the gel fraction of the modified polylactic acid resin has a large effect on the appearance of the resulting polylactic acid resin foam sheet, and that the appearance of the resulting polylactic acid resin foam sheet deteriorates as the gel fraction of the modified polylactic acid resin increases. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 6971947 [Patent Document 2] Patent No. 6968118 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention aims to provide a method for producing a modified polylactic acid resin that can suppress an increase in the gel fraction of the resulting modified polylactic acid resin. It also aims to provide a modified polylactic acid resin with a low gel fraction obtained by the method. It also aims to provide a polylactic acid resin foam sheet with excellent appearance obtained from the modified polylactic acid resin. [Means for solving the problem]

[0008] [1] A method for producing a modified polylactic acid resin according to an embodiment of the present invention includes a modification step of modifying a polylactic acid resin in an extruder, the extruder including, from upstream to downstream, a feed section to which the polylactic acid resin is supplied, a reaction section in which the polylactic acid resin is modified, and a kneading section in which the resin composition obtained in the reaction section is kneaded, the set temperature of the feed section being 180°C or less, and the resulting modified polylactic acid resin having a gel fraction of less than 10 mass%. [2] The method for producing a modified polylactic acid resin according to [1] above may be such that a modifier is supplied to the feed section. [3] The method for producing the modified polylactic acid resin according to [1] or [2] above may include a pelletizing step of pelletizing the kneaded mixture extruded from the extruder. [4] A modified polylactic acid resin according to an embodiment of the present invention is a modified polylactic acid resin having a gel fraction of less than 10 mass %, which is obtained by the manufacturing method described in any one of [1] to [3] above. [5] The modified polylactic acid resin described in [4] above may have an MFR of 5.0 g / 10 min or less at a temperature of 190° C. and a test load of 21.18 N, measured in accordance with Method B of JIS K 7210:1999. [6] The modified polylactic acid resin according to [4] or [5] above may have a melt tension of more than 18 cN at a temperature of 190°C. [7] The polylactic acid resin foam sheet according to the embodiment of the present invention is obtained by melt-kneading a polylactic acid resin (P) containing as a main component the modified polylactic acid resin described in any one of [4] to [6] above with a foaming agent in an extruder, followed by extrusion foaming. Effect of the Invention

[0009] According to an embodiment of the present invention, it is possible to provide a method for producing a modified polylactic acid resin, which can suppress an increase in the gel fraction of the resulting modified polylactic acid resin. It is also possible to provide a modified polylactic acid resin with a low gel fraction obtained by such a production method. Furthermore, it is also possible to provide a polylactic acid resin foam sheet with excellent appearance obtained from such a modified polylactic acid resin. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic diagram showing one preferred configuration of an extruder used in a method for producing a modified polylactic acid resin according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram showing one preferred configuration of a production apparatus in a method for producing a modified polylactic acid resin according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic diagram showing one preferred configuration of a production apparatus for producing a polylactic acid resin foam sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0012] In this specification, when the polylactic acid resin is not specifically described as "polylactic acid resin (P)", "modified polylactic acid resin", or "unmodified polylactic acid resin" but is simply described as "polylactic acid resin", it means unmodified polylactic acid resin. Here, "unmodified polylactic acid resin" refers to polylactic acid resin that has not been modified, typically a polylactic acid resin that is generally available, and is not a modified polylactic acid resin obtained by the manufacturing method for modified polylactic acid resin according to an embodiment of the present invention.

[0013] In this specification, "containing as a main component" means that the content ratio is preferably more than 50% by mass, more preferably 70% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably substantially 100% by mass.

[0014] In this specification, the term "substantially 100% by mass" means that the presence of a trace amount (for example, less than 1% by mass) of unintentionally mixed impurities may be ignored.

[0015] <<Method for producing modified polylactic acid resin>> A method for producing a modified polylactic acid resin according to an embodiment of the present invention includes a modification step of modifying a polylactic acid resin in an extruder, the extruder including, from upstream to downstream, a feed section to which the polylactic acid resin is supplied, a reaction section in which the polylactic acid resin is modified, and a kneading section in which the resin composition obtained in the reaction section is kneaded, the set temperature of the feed section being 180°C or lower, and the resulting modified polylactic acid resin having a gel fraction of less than 10% by mass.

[0016] The modified polylactic acid resin obtained by the manufacturing method according to the embodiment of the present invention has a gel fraction of preferably less than 10% by mass, more preferably less than 8% by mass, even more preferably less than 6% by mass, particularly preferably less than 4% by mass, and most preferably less than 2% by mass. If the gel fraction of the modified polylactic acid resin obtained by the manufacturing method according to the embodiment of the present invention is within the above range, the modified polylactic acid resin can be used to provide a polylactic acid resin foam sheet with excellent appearance.

[0017] The modified polylactic acid resin obtained by the manufacturing method according to the embodiment of the present invention has an MFR (melt mass flow rate) of preferably 5.0 g / 10 min or less, more preferably 0.2 g / 10 min to 5.0 g / 10 min, even more preferably 0.5 g / 10 min to 4.5 g / 10 min, particularly preferably 1.0 g / 10 min to 4.0 g / 10 min, and most preferably 1.0 g / 10 min to 3.5 g / 10 min. When the MFR (melt mass flow rate) of the modified polylactic acid resin obtained by the manufacturing method according to the embodiment of the present invention is within the above range, it can exhibit appropriate fluidity during thermal melting, and can be a modified polylactic acid resin useful for providing a polylactic acid resin foamed sheet with excellent foaming properties. The method for measuring the MFR (melt mass flow rate) will be described later.

[0018] The modified polylactic acid resin obtained by the manufacturing method according to the embodiment of the present invention has a melt tension of preferably 18 cN or more, more preferably 20 cN to 100 cN, even more preferably 30 cN to 80 cN, particularly preferably 40 cN to 70 cN, and most preferably more than 40 cN to 60 cN or less. When the melt tension of the modified polylactic acid resin obtained by the manufacturing method according to the embodiment of the present invention is within the above range, the modified polylactic acid resin can be useful for providing a polylactic acid resin foamed sheet with excellent foamability. The method for measuring the melt tension will be described later.

[0019] <Modification process> In the modification step, the polylactic acid resin is modified in an extruder. The polylactic acid resin as a raw material in the modification step preferably means an unmodified polylactic acid resin. The polylactic acid resin as a raw material in the modification step may be one type or two or more types.

[0020] As the extruder, any appropriate extruder may be used as long as the effects of the present invention are not impaired. In terms of being able to more effectively exhibit the effects of the present invention, the extruder is preferably a twin-screw extruder.

[0021] Fig. 1 is a schematic diagram showing one preferred configuration of an extruder used in a method for producing a modified polylactic acid resin according to an embodiment of the present invention. As shown in Fig. 1, an extruder 30 includes, from upstream to downstream, a feed section 31 to which a polylactic acid resin is supplied, a reaction section 32 in which the polylactic acid resin is modified, and a kneading section 33 in which the resin composition obtained in the reaction section is kneaded.

[0022] The extruder 30 includes, in order from the upstream side to the downstream side, a feed section 31 to which polylactic acid resin is supplied, a reaction section 32 in which the polylactic acid resin is modified, and a kneading section 33 in which the resin composition obtained in the reaction section is kneaded, and may have any other appropriate areas as long as the effects of the present invention are not impaired.

[0023] The feed section 31 typically has a supply port 31a through which a polylactic acid resin is supplied as a raw material. The raw material is supplied from the supply port 31a using, for example, a hopper.

[0024] The extruder 30 is typically equipped with a die 3 at its downstream end. Examples of the die include a strand die and a T-die, and a strand die is preferable.

[0025] The total length of the length L1 of the feed section 31, the length L2 of the reaction section 32, and the length L3 of the kneading section 33 is preferably 50% to 100% of the total length L of the extruder 30, more preferably 70% to 100%, even more preferably 90% to 100%, particularly preferably 95% to 100%, and most preferably 100%.

[0026] The length L1 of the feed section 31 is preferably 5% to 30%, more preferably 10% to 30%, and even more preferably 10% to 25% of the total length L of the extruder 30. If the length L1 of the feed section 31 is too short outside the above range, the dispersion of the modifier may become non-uniform, and the gel fraction may increase. If the length L1 of the feed section 31 is too long outside the above range, the load on the extruder may increase, making extrusion difficult.

[0027] The length L2 of the reaction section 32 is preferably 20% to 50%, more preferably 25% to 50%, and even more preferably 25% to 45% of the total length L of the extruder 30. If the length L2 of the reaction section 32 is too short outside the above range, the reaction may become non-uniform, the melt tension may decrease, and the gel fraction may increase. If the length L2 of the reaction section 32 is too long outside the above range, the resin may deteriorate and the melt tension may decrease.

[0028] The length L3 of the kneading section 33 is preferably 30% to 60%, more preferably 35% to 60%, and even more preferably 35% to 55% of the total length L of the extruder 30. If the length L3 of the kneading section 33 is too short outside the above range, a homogeneously modified polylactic acid resin may not be obtained, and quality may vary. If the length L3 of the kneading section 33 is too long outside the above range, resin deterioration may occur, resulting in a decrease in melt tension.

[0029] In the method for producing a modified polylactic acid resin according to an embodiment of the present invention, the set temperature of the feed section is 180°C or less, preferably 170°C or less, more preferably 160°C or less, even more preferably 155°C or less, and particularly preferably 150°C or less. The lower limit of the set temperature of the feed section is preferably 100°C or more, more preferably 110°C or more, even more preferably 120°C or more, and particularly preferably 130°C or more. By setting the set temperature of the feed section within the above range, an increase in the gel fraction of the modified polylactic acid resin obtained can be effectively suppressed. If the set temperature of the feed section is too high outside the above range, the gel fraction of the modified polylactic acid resin obtained may increase, and thus a polylactic acid resin foam sheet with excellent appearance can be provided from the modified polylactic acid resin obtained in this way. If the set temperature of the feed section is too low outside the above range, the resin does not soften, and the load of the extruder increases, making extrusion difficult.

[0030] The feed section may be composed of one zone or multiple zones. When composed of multiple zones, it is sufficient that the set temperature in each zone is adjusted within the set temperature range of the feed section.

[0031] The set temperature of the feed section is a temperature set by the means for setting the temperature of the feed section in the extruder. However, if the extruder is not provided with a means for setting the temperature of the feed section, the temperature of the mixture (typically, a mixture of polylactic acid resin and modifier) ​​present in the feed section shall be read as the set temperature of the feed section.

[0032] In the method for producing a modified polylactic acid resin according to an embodiment of the present invention, the set temperature of the reaction section may be any appropriate set temperature within a range that does not impair the effects of the present invention. In terms of being able to more effectively express the effects of the present invention, such a set temperature is preferably 280°C or less, more preferably 260°C or less, even more preferably 250°C or less, and particularly preferably 240°C or less. The lower limit of the set temperature of the reaction section is preferably 160°C or more, more preferably 170°C or more, even more preferably 180°C or more, and particularly preferably 190°C or more. By setting the set temperature of the reaction section within the above range, the modification reaction can be made to proceed homogeneously and sufficiently. If the set temperature of the reaction section is too high outside the above range, the reaction may proceed rapidly and the gel fraction may increase. If the set temperature of the reaction section is too low outside the above range, the reaction may not proceed sufficiently and the melt tension may decrease.

[0033] The reaction section may be composed of one zone or multiple zones. When composed of multiple zones, it is sufficient that the set temperature in each zone is adjusted within the set temperature range of the reaction section.

[0034] The set temperature of the reaction section is a temperature set by a means for setting the temperature of the reaction section in the extruder. However, if the extruder is not provided with a means for setting the temperature of the reaction section, the temperature of the mixture present in the reaction section (typically, a reaction mixture of polylactic acid resin and modifier) ​​shall be read as the set temperature of the reaction section.

[0035] In the method for producing a modified polylactic acid resin according to an embodiment of the present invention, the set temperature of the kneading section may be any appropriate set temperature within a range that does not impair the effects of the present invention. In terms of being able to more effectively exhibit the effects of the present invention, such a set temperature is preferably 240°C or less, more preferably 230°C or less, even more preferably 220°C or less, and particularly preferably 200°C or less. The lower limit of the set temperature of the kneading section is preferably 160°C or more, more preferably 170°C or more. By setting the set temperature of the kneading section within the above range, it is possible to suppress resin deterioration of the kneaded product, suppress the decrease in molecular weight and the decrease in melt tension of the obtained modified polylactic acid resin, and improve the foaming properties of the polylactic acid resin foam sheet obtained from the modified polylactic acid resin obtained in this way. If the set temperature of the kneading section is too high outside the above range, the resin of the kneaded product may deteriorate, the molecular weight and melt tension of the resulting modified polylactic acid resin may decrease, and the foaming properties of the polylactic acid resin foam sheet obtained from the modified polylactic acid resin may deteriorate. If the set temperature of the kneading section is too low outside the above range, the load on the extruder may increase, making extrusion difficult.

[0036] The kneading section may be composed of one zone or may be composed of multiple zones. When composed of multiple zones, it is sufficient that the set temperature in each zone is adjusted within the set temperature range of the kneading section.

[0037] The set temperature of the kneading section is a temperature set by a means for setting the temperature of the kneading section in the extruder. However, if the extruder is not provided with a means for setting the temperature of the kneading section, the temperature of the mixture present in the kneading section (typically, a reaction mixture of polylactic acid resin and modifier) ​​shall be read as the set temperature of the kneading section.

[0038] The rotation speed of the extruder may vary depending on the size of the extrusion, the discharge amount, etc., and any appropriate condition may be adopted within a range that does not impair the effects of the present invention. Such a rotation speed is, for example, preferably 20 rpm to 800 rpm.

[0039] The polylactic acid resin used as the raw material in the modification step is adjusted to have a moisture content of preferably 0.30% by mass or less, more preferably 0.25% by mass or less, more preferably 0.20% by mass or less, even more preferably 0.17% by mass or less, and particularly preferably 0.15% by mass or less. The lower limit of this moisture content is preferably as low as possible, and is ideally 0% by mass.

[0040] The polylactic acid resin may be a homopolymer of lactic acid or a copolymer of lactic acid and other monomers, such as aliphatic hydroxycarboxylic acids other than lactic acid, aliphatic polyhydric alcohols, aliphatic polycarboxylic acids, and polyfunctional polysaccharides.

[0041] The lactic acid constituting the polylactic acid resin may be either the L-form or the D-form, or may be both the L-form and the D-form. That is, the polylactic acid resin, which is a homopolymer of lactic acid, may be any of poly(L-lactic acid) resin, poly(D-lactic acid) resin, and poly(DL-lactic acid) resin.

[0042] Examples of hydroxycarboxylic acids other than lactic acid include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid.

[0043] Examples of the aliphatic polyhydric alcohol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, neopentyl glycol, tetramethylene glycol, and 1,4-cyclohexanedimethanol.

[0044] Examples of the aliphatic polycarboxylic acid include oxalic acid, succinic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, undecanedioic acid, and dodecanedioic acid. The aliphatic polycarboxylic acid may be an acid anhydride.

[0045] Examples of polyfunctional polysaccharides include cellulose, cellulose nitrate, methylcellulose, ethylcellulose, celluloid, viscose rayon, regenerated cellulose, cellophane, cupra, cuprammonium rayon, cuprophane, Bemberg, hemicellulol, starch, acropectin, dextrin, dextran, glycogen, pectin, chitin, chitosan, gum arabic, guar gum, locust bean gum, and acacia gum.

[0046] In the polylactic acid resin, the content of structural portions derived from lactic acid (L- and D-form) in the molecule is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and most preferably 90% by mass or more.

[0047] At least a part of the polylactic acid resin used as the raw material may be recycled.

[0048] In the modification step, a modifier is used to modify the polylactic acid resin by increasing the molecular weight of the polylactic acid resin or by providing a crosslinked structure or a long-chain branched structure in the molecular structure of the polylactic acid resin.

[0049] The modifier may be of only one type, or of two or more types.

[0050] To increase the molecular weight of polylactic acid resin, a chain extender such as carbodiimide can be used as a modifier. In the modification using a chain extender, a compound having one or more functional groups capable of undergoing a condensation reaction with a hydroxyl group or a carboxyl group present in the molecular structure of polylactic acid resin, such as an acrylic organic compound, an epoxy organic compound, or an isocyanate organic compound, can be used. That is, the molecular weight of polylactic acid resin can be increased by using a chain extender such as carbodiimide to bond an acrylic organic compound, an epoxy organic compound, an isocyanate organic compound, or the like to the polylactic acid resin.

[0051] In order to provide a crosslinked structure or a long-chain branched structure in the molecular structure of polylactic acid resin, for example, a radical initiator can be used as a modifier. In this case, polylactic acid resins are reacted with each other using a radical initiator having appropriate reactivity. When polylactic acid resins are reacted with each other using a radical initiator having appropriate reactivity, for example, the decomposition starting point of the polylactic acid resin in the extruder is attacked by the free radicals generated by the radical initiator, and the site becomes a crosslinked point (branching point) and can be stabilized. By performing such modification, the thermal stability of the polylactic acid resin is increased and the molecular weight is less likely to be reduced when passing through the extruder.

[0052] Examples of the radical initiator include organic peroxides, azo compounds, and halogen molecules, with organic peroxides being preferred.

[0053] Examples of organic peroxides include peroxy esters, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxydicarbonates, peroxyketals, and ketone peroxides.

[0054] Examples of peroxy esters include t-butylperoxy 2-ethylhexyl carbonate, t-hexylperoxy isopropyl monocarbonate, t-hexylperoxybenzoate, t-butylperoxybenzoate, t-butylperoxylaurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyacetate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and t-butylperoxyisopropyl monocarbonate.

[0055] Examples of hydroperoxides include permethane hydroperoxide, diisopropylbenzene hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide.

[0056] Examples of dialkyl peroxides include dicumyl peroxide, di-t-butyl peroxide, and 2,5-dimethyl-2,5-di(t-butylperoxy)-hexyne-3.

[0057] Examples of diacyl peroxides include dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, and di(3-methylbenzoyl) peroxide.

[0058] Examples of peroxydicarbonates include di(2-ethylhexyl) peroxydicarbonate and diisopropyl peroxydicarbonate.

[0059] Examples of peroxyketals include 1,1-di-t-butylperoxy-3,3,5-trimethylcyclohexane, 1,1-di-t-butylperoxycyclohexane, 2,2-di(t-butylperoxy)-butane, n-butyl 4,4-di-(t-butylperoxy)valerate, and 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane.

[0060] Examples of the ketone peroxide include methyl ethyl ketone peroxide and acetylacetone peroxide.

[0061] In the modification with organic peroxide, there is a risk that the modified polylactic acid resin may be mixed with components having an excessively large molecular weight that may gel when thermally melted, or that odor problems may occur due to decomposition residues of the organic peroxide. The organic peroxide is preferably a peroxyester, in that it can suppress the occurrence of such problems and can easily modify the polylactic acid resin to a state suitable for foaming. Among peroxyesters, peroxycarbonate-based organic peroxides such as peroxymonocarbonate and peroxydicarbonate are preferred. Furthermore, among peroxycarbonate-based organic peroxides, peroxymonocarbonate-based organic peroxides are preferred, and t-butylperoxyisopropylmonocarbonate is more preferred.

[0062] The amount of organic peroxide used depends on the molecular weight, etc., but in order to more effectively exhibit the effects of the present invention, it is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of polylactic acid resin. The upper limit of the amount of organic peroxide used is preferably 2.0 parts by mass or less, more preferably 1.5 parts by mass or less, and even more preferably 1.0 part by mass or less.

[0063] The raw material used in the modification step may contain any other appropriate components other than the polylactic acid resin and the modifier within a range that does not impair the effects of the present invention. The total content of the polylactic acid resin and the modifier in the raw material used in the modification step is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, even more preferably 90% by mass to 100% by mass, and particularly preferably 95% by mass to 100% by mass.

[0064] In the modification step, the feed section is supplied with the polylactic acid resin as a raw material, preferably with the polylactic acid resin and the modifier as raw materials. The polylactic acid resin as raw material, the modifier, and other components as necessary may be mixed in advance and then fed to the feed section. Examples of such a mixing method include a mixing method using a mixer such as a tumbler, ribbon blender, V blender, Henschel mixer, or Redige mixer.

[0065] <Optional other steps> The method for producing a modified polylactic acid resin according to an embodiment of the present invention may include any other appropriate steps other than the modification step, as long as the effects of the present invention are not impaired. Such steps may be one type only, or two or more types. Examples of such steps include a pelletizing step for pelletizing the kneaded material obtained in the modification step, a cooling step for cooling the kneaded material obtained in the modification step, and a drying step for drying the pellets obtained in the pelletizing step.

[0066] In one embodiment of the method for producing a modified polylactic acid resin according to the present invention, the modified polylactic acid resin is obtained as pellets. In this case, in one preferred embodiment of the method for producing a modified polylactic acid resin according to the present invention, as shown in Fig. 2, the raw material polylactic acid resin fed into a hopper 11 is modified in an extruder 30, and the strand-shaped kneaded material extruded from a die 3 is cooled in a cooling device 6, then pelletized by a pelletizer 4, and dried in a drying device 5 to obtain pellets of the modified polylactic acid resin.

[0067] <Cooling process> In one preferred embodiment of the modified polylactic acid resin according to the present invention, a cooling step of cooling the kneaded material extruded from the extruder may be included after the modification step.

[0068] The cooling method in the cooling step may be any appropriate method as long as it does not impair the effects of the present invention. Examples of such methods include a method using a cooling device, a representative example of which is a method of water-cooling the strand discharged from the strand die, specifically a method of water-cooling the strand discharged from the strand die by introducing it into a water tank.

[0069] The cooling temperature is preferably 70° C. or lower, more preferably 60° C. or lower, even more preferably 50° C. or lower, particularly preferably 40° C. or lower, and most preferably 35° C. or lower. There are no particular limitations on the lower limit of the cooling temperature, but in consideration of the cost required for cooling and the like, it is practically preferably 5° C. or higher, more preferably 10° C. or higher.

[0070] <Pelletizing process> In one preferred embodiment of the modified polylactic acid resin according to the present invention, after the modification step, a pelletizing step of pelletizing the kneaded material extruded from the extruder may be included.

[0071] As the pelletizing method in the pelletizing step, any suitable method can be adopted as long as the kneaded material extruded from the extruder in the modification step can be pelletized, as long as the effect of the present invention is not impaired. As a representative example of such a pelletizing method, the strand-shaped or sheet-shaped kneaded material extruded from the extruder in the modification step is cut with a pelletizer to prepare pellets. In order to efficiently proceed with the pelletizing step, the above-mentioned cooling step may be included after the modification step and before the pelletizing step.

[0072] As the pelletizer, any appropriate pelletizer can be adopted as long as it does not impair the effects of the present invention.

[0073] The extruder in the modification step may be equipped with a pelletizing die (hot cut die). In this case, the kneaded material is pelletized immediately after being extruded, and the pelletization in the pelletizing die can be the pelletizing step.

[0074] <Drying process> In one preferred embodiment of the modified polylactic acid resin according to the present invention, a drying step may be included in which the pellets obtained in the pelletizing step are dried.

[0075] As a method for drying the pellets in the drying step, any appropriate method may be adopted as long as it does not impair the effects of the present invention. Examples of such methods include a method of drying the pellets using a dryer such as a dehumidifying dryer, a vacuum dryer, or a hot air dryer. It is a preferred embodiment that the pellets sufficiently dried in the above-mentioned dryer or the like are directly introduced (without being exposed to a moisture-containing environment) into the next step. It is also a preferred embodiment that the pellets sufficiently dried in the above-mentioned dryer or the like are immediately sealed in an aluminum bag after drying, and the bag is opened just before being introduced into the next step.

[0076] <<Modified polylactic acid resin>> The modified polylactic acid resin according to the embodiment of the present invention can be obtained by the method for producing the modified polylactic acid resin according to the embodiment of the present invention.

[0077] <<Polylactic acid resin foam sheet>> The polylactic acid resin foam sheet according to an embodiment of the present invention is obtained by melt-kneading a polylactic acid resin (P) containing as a main component the modified polylactic acid resin obtained by the manufacturing method according to an embodiment of the present invention with a foaming agent in an extruder, and extruding and foaming the resulting mixture.

[0078] The polylactic acid resin (P) contains, as a main component, a modified polylactic acid resin obtained by the manufacturing method according to the embodiment of the present invention. For convenience, the following description will be given assuming that the content of the modified polylactic acid resin in the polylactic acid resin (P) is substantially 100% by mass.

[0079] The foaming agent may be of only one type, or of two or more types.

[0080] As the foaming agent, any appropriate foaming agent can be used within a range that does not impair the effects of the present invention. Examples of the foaming agent include a volatile foaming agent that becomes gas at room temperature (23°C) and normal pressure (1 atm) and a decomposition type foaming agent that generates gas by thermal decomposition, and a volatile foaming agent is preferred.

[0081] The volatile foaming agent is preferably an organic compound whose boiling point is equal to or lower than the softening point of polylactic acid resin and is in a gaseous or liquid state at normal pressure.Specific examples include aliphatic hydrocarbons such as propane, n-butane, isobutane, pentane (n-pentane, isopentane, neopentane), and n-hexane; alicyclic hydrocarbons such as cyclopentane and cyclopentadiene; ketones such as acetone and methyl ethyl ketone; alcohols such as methanol, ethanol, and isopropyl alcohol; low-boiling ether compounds such as dimethyl ether, diethyl ether, dipropyl ether, and methyl ethyl ether; halogen-containing hydrocarbons such as trichloromonofluoromethane and dichlorodifluoromethane.The volatile foaming agent may also be an inorganic gas such as carbon dioxide, nitrogen, or ammonia. Among these, in terms of further exerting the effects of the present invention, the volatile blowing agent is preferably at least one selected from n-butane, isobutane, n-pentane, isopentane, neopentane, cyclopentane, and cyclopentadiene, and more preferably at least one selected from n-butane, isobutane, n-pentane, and isopentane.

[0082] Decomposition type foaming agents include, for example, azodicarbonamide, dinitrosopentamethylenetetramine, sodium bicarbonate, or a mixture of an organic acid or its salt, such as citric acid, and a bicarbonate.

[0083] The amount of the foaming agent used can be appropriately set depending on the purpose. The amount of the foaming agent used is preferably 0.1 to 10.0 parts by mass, more preferably 0.3 to 7.0 parts by mass, still more preferably 0.5 to 5.0 parts by mass, and particularly preferably 0.8 to 3.0 parts by mass, based on 100 parts by mass of the polylactic acid resin (P).

[0084] The extruder may contain any other appropriate components other than the polylactic acid resin (P) and the foaming agent within a range that does not impair the effects of the present invention. The total content of the polylactic acid resin (P) and the foaming agent in the total amount of materials supplied to the extruder is preferably 50% by mass to 100% by mass, more preferably 70% by mass to 100% by mass, even more preferably 90% by mass to 100% by mass, and particularly preferably 95% by mass to 100% by mass.

[0085] The extruder may contain a foaming aid as another component. The foaming aid may be one type or two or more types. Examples of the foaming aid include diisobutyl adipate, toluene, cyclohexane, ethylbenzene, liquid paraffin, and coconut oil.

[0086] The extruder may contain a bubble regulator as another component. The bubble regulator may be one type only, or two or more types. Examples of the bubble regulator include higher fatty acid amides, partial esters of higher fatty acids and alcohols, talc, calcium carbonate, mica, citric acid, sodium bicarbonate, polytetrafluoroethylene, aluminum hydroxide, and silica. Examples of higher fatty acid amides include fatty acid monoamides such as oleic acid amide, stearic acid amide, and hydroxystearic acid amide; and fatty acid bisamides such as methylene bisstearic acid amide and ethylene bisstearic acid amide. Examples of higher fatty acids in the partial esters of higher fatty acids and alcohols include fatty acids having 15 or more carbon atoms, such as palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, and behenic acid. Examples of partial esters of higher fatty acids and alcohols include stearic acid monoglyceride and stearic acid diglyceride.

[0087] Examples of other components other than those mentioned above include other resins, pigments, radiant heat transfer suppressing components, crosslinking agents, plasticizers, stabilizers, fillers, lubricants, colorants, antioxidants, antistatic agents, spreading agents, weather resistance agents, flame retardants, ultraviolet absorbing agents, light stabilizers, antiaging agents, anti-fogging agents, fragrances, and antibacterial agents.

[0088] In producing a polylactic acid resin foam sheet, the polylactic acid resin (P), the cell regulator, and other components as necessary may be mixed in advance. Examples of such a mixing method include a mixing method using a mixer such as a tumbler, a ribbon blender, a V blender, a Henschel mixer, or a Redigay mixer.

[0089] As the extruder, any appropriate extruder may be used as long as the effects of the present invention are not impaired. In terms of being able to more effectively exhibit the effects of the present invention, a tandem extruder is preferably used as the extruder.

[0090] The tip of the tandem extruder is provided with any appropriate die so as to ultimately obtain a polylactic acid resin foam sheet, as long as the effects of the present invention are not impaired. Preferably, the extruder may further be provided with a cooling mandrel, a take-up roller for winding up the polylactic acid resin foam sheet into a raw roll, and the like.

[0091] The polylactic acid resin foam sheet according to the embodiment of the present invention can be produced using any appropriate production apparatus as long as the effects of the present invention are not impaired. In order to further exert the effects of the present invention, the polylactic acid resin foam sheet according to the embodiment of the present invention can be produced using, for example, an apparatus as shown in FIG.

[0092] The manufacturing apparatus shown in Fig. 3 includes a tandem extruder 10 and a circular die CD for discharging the polylactic acid resin composition melt-kneaded in the tandem extruder 10 into a cylindrical shape. The manufacturing apparatus further includes a cooling device CL for air-cooling the foamed sheet discharged from the circular die CD into a cylindrical shape, a mandrel MD for expanding the diameter of the cylindrical foamed sheet into a cylindrical shape of a predetermined size, a slitting device for slitting the foamed sheet after passing through the mandrel MD and dividing it into two sheets, and a take-up roller 22 for winding up the slit foamed sheet 1 after passing through a plurality of rollers 21. The extruder (hereinafter also referred to as "first extruder 10a") upstream of the tandem extruder 10 includes a hopper 11 for introducing the modified polylactic acid resin that is the raw material of the foamed sheet, and a gas introduction section 12 for supplying a foaming agent into the cylinder. An extruder (hereinafter also referred to as "second extruder 10b") is provided downstream of the first extruder 10a for melt-kneading a polylactic acid resin composition containing a modified polylactic acid resin and a foaming agent.

[0093] The temperature conditions of the melt kneading may vary depending on the size of the extrusion, the discharge amount, etc., and therefore any appropriate conditions may be adopted within a range that does not impair the effects of the present invention. For example, the temperature of the raw material feed section of the upstream extruder 10a is preferably set to 100°C to 200°C, more preferably 140°C to 200°C, the temperature after the upstream extruder 10a is preferably set to 120°C to 300°C, more preferably 140°C to 270°C, and the temperature of the downstream extruder 10b is preferably set to 100°C to 250°C, more preferably 120°C to 220°C.

[0094] The rotation speed of the extruder may vary depending on the size of the extrusion, the discharge amount, etc., and any appropriate condition may be adopted within a range that does not impair the effects of the present invention. For example, the rotation speed of the upstream extruder 10a is preferably 10 rpm to 300 rpm, and the rotation speed of the downstream extruder 10b is preferably 5 rpm to 200 rpm.

[0095] The thickness of the polylactic acid resin foam sheet obtained by the method for producing a polylactic acid resin foam sheet according to the embodiment of the present invention can be appropriately set depending on the purpose. The thickness of the polylactic acid resin foam sheet obtained by the method for producing a polylactic acid resin foam sheet according to the embodiment of the present invention is typically preferably 0.2 mm to 10 mm, more preferably 0.3 mm to 8.0 mm, even more preferably 0.4 mm to 5.0 mm, and particularly preferably 0.5 mm to 3.0 mm.

[0096] The open cell ratio of the polylactic acid resin foamed sheet obtained by the method for producing a polylactic acid resin foamed sheet according to the embodiment of the present invention is preferably 60% or less, more preferably 40% or less, even more preferably 30% or less, particularly preferably 20% or less, and most preferably less than 16%. The lower limit of the open cell ratio is preferably 0% or more. If the open cell ratio of the polylactic acid resin foamed sheet obtained by the method for producing a polylactic acid resin foamed sheet according to the embodiment of the present invention is within the above range, the polylactic acid resin foamed sheet is less likely to shrink and has excellent foaming properties. The method for measuring the open cell ratio will be described later. EXAMPLES

[0097] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating each property are as follows.

[0098] <Measurement of gel fraction> The gel fraction (mass %) was measured by the following method. Prepare about 0.5 g of a sample and precisely weigh the initial mass (m0 (g)) of this sample. Also, prepare a 200-mesh wire mesh (wire diameter 0.05 mm) for filtering the solution in which this sample is dissolved. Precisely weigh the initial mass (M0 (g)) of this wire mesh. Put the weighed measurement sample into a beaker (100 mL). Put 50 mL of chloroform as a solvent and a stir bar into the beaker, and cover it with aluminum foil. Stir for 2 hours with a stirrer and dissolve it at room temperature. After 2 hours, remove the aluminum foil and filter the dissolved matter in the beaker with the wire mesh. After filtration, let the wire mesh air-dry naturally in a draft for 12 hours or more. After natural drying, further dry this wire mesh in a constant-temperature dryer at 120 °C for 2 hours. Cool the dried wire mesh in a desiccator. After cooling, weigh the wire mesh with the resin insoluble matter attached, and calculate the gel fraction using the following formula. Gel fraction (mass %) = (m1 / m0) × 100 m0: Initial mass of the sample m1: Mass of the resin insoluble matter (M1 - M0) M0: Initial mass of the wire mesh M1: Total mass of the resin insoluble matter and the wire mesh

[0099] <Measurement of MFR (Melt Mass Flow Rate)> MFR was measured in accordance with the standard of JIS K 7210:1999. Specifically, it was measured by the method of "b) Measuring the time for the piston to move a predetermined distance" described in Method B of the same standard. MFR was measured using a melt flow index tester (automatic) 120-SAS (manufactured by Yasuda Seiki Seisakusho Co., Ltd.). As the sample, the one that was vacuum-dried at 70 °C for 5 hours and stored in a desiccator sealed until immediately before measurement was used. The number of measurements was 3 times, and the average was taken as the value of MFR (g / 10 min). The measurement conditions were as follows. Sample: 3 g to 8 g Preheating (1): 200 seconds Preheating (2): 30 seconds Test temperature: 190 °C Test load: 21.18 N Piston movement distance (interval): 25 mm

[0100] <Melt tension (MT) measurement> The melt tension was measured using a Capillograph 1D (manufactured by Toyo Seiki Seisakusho Co., Ltd.) and Rheotens 71.97 (manufactured by Gottfert) as measuring devices. The measurement sample was vacuum dried at 70°C for 5 hours in advance. First, the measurement sample was filled into a barrel with a diameter of 9.55 mm heated to a test temperature of 190°C, and then preheated for 5 minutes. The molten resin was extruded into a string-like shape from a capillary die (diameter 2.095 mm, length 8 mm, inlet angle 90 degrees (conical)) of the above-mentioned measuring device while maintaining a constant piston descending speed (20 mm / min). The string-like material was passed through a wheel (wheel interval: upper 0.6 mm to 0.8 mm, lower 1.0 mm) installed so that the distance from the outlet of the capillary die to the measurement section was 80 mm, and the initial speed was set to 6.92 mm / s, and the acceleration was set to 10 mm / s. 2 The Rheotens was passed through the wire while gradually increasing the tension, and the average of the maximum and minimum tension values ​​just before the point where the string-like object broke was taken as the melt tension (MT) of the measured sample. If the Rheotens could not be brought closer to 80 mm due to interference, measures were taken to avoid interference and set the Rheotens in a specified location. If there was only one maximum point on the tension chart, the maximum value was taken as the melt tension, and if the string-like object became thinner and the take-up was in an idle state, that point was taken as the break point, and the average of the maximum and minimum tension values ​​just before that was taken as the melt tension of the measured sample. [Measurement conditions for "Capillograph 1D"] Die: diameter 2.095mm, length 8mm, inlet angle 90 degrees (conical) Barrel diameter: 9.55mm Piston speed: 20mm / min Measurement temperature: 190℃ [Measurement conditions for "Rheotens 71.97"] Wheel spacing: Top 0.6mm~0.8mm, bottom 1.0mm Acceleration: 10mm / s 2 Pulling speed: Initial speed 6.92mm / s

[0101] <Measurement of open cell ratio> Cut out several sheet-like samples of 25 mm length and 25 mm width from the polylactic acid resin foam sheet, stack the cut samples without leaving any gaps to make a measurement sample of 25 mm thickness, measure the outer dimensions of this measurement sample to 1 / 100 mm using a "Digimatic Caliper" made by Mitutoyo Corporation, and calculate the apparent volume (cm 3 ) was sought. Next, the volume (cm) of the sample to be measured was measured using an air comparison type specific gravity meter Model 1000 (Tokyo Science Co., Ltd.) by the 1-1 / 2-1 atmospheric pressure method. 3 ) was sought. The open cell ratio (%) was calculated from these determined values ​​and the following formula, and the average value for five test pieces was calculated. The measurement was performed in a JIS K7100-1999, symbol 23 / 50, grade 2 environment after conditioning the measurement sample for 16 hours in the JIS K7100-1999, symbol 23 / 50, grade 2 environment. In addition, the air comparison type specific gravity meter was calibrated using standard bulbs (large 28.9cc, small 8.5cc). Open cell rate (%) = [(apparent volume - volume measured with air comparison type specific gravity meter) / apparent volume] x 100 (%)

[0102] <Measurement of foaming ratio> The expansion ratio of a polylactic acid resin foam sheet can be calculated by determining the apparent density (ρ1) of the polylactic acid resin foam sheet, determining the density (true density: ρ0) of the polylactic acid resin composition constituting the polylactic acid resin foam sheet, and dividing the true density (ρ0) by the apparent density (ρ1). Expansion ratio = true density (ρ0) / apparent density (ρ1) The density of the foamed sheet can be determined by the method described in JIS-K7222:1999 "Foamed plastics and rubber - Measurement of apparent density", and specifically, it was determined by the following method. (Density measurement method) From polylactic acid resin foam sheet, 100cm 3The above samples were cut without changing the original cell structure, and the samples were conditioned for 16 hours in a JIS K7100:1999, symbol 23 / 50, class 2 environment, after which the dimensions and mass were measured, and the density was calculated according to the following formula. Apparent density (kg / m 3 ) = mass of sample (kg) / volume of sample (m 3 ) The dimensions of the samples were measured using a "DIGIMATIC" CD-15 type manufactured by Mitutoyo Corporation. The density of the polylactic acid resin composition constituting the polylactic acid resin foam sheet was determined by measuring a sample of the polylactic acid resin foam sheet that had been made non-foamed by, for example, heat pressing, based on the Archimedes method (the liquid weighing method of JIS-K8807:2012 "Methods for determining density and specific gravity of solids").

[0103] <Appearance of polylactic acid resin foam sheet> The appearance of the polylactic acid resin foam sheet was evaluated according to the following criteria. ○: The foam is uniform and the appearance is beautiful. △: The foam is uniform, but some lumps are visible on the sheet surface. ×: Numerous blemishes are observed on the sheet surface.

[0104] [Example 1] (1) Preparation of modified polylactic acid resin Polylactic acid resin (Nature Works, "Biopolymer Ingeo 4032D", MFR = 4.4g / 10min, density = 1240kg / m 3 A mixture was obtained by stirring and mixing 100 parts by mass of 1,000g of tert-butylperoxyisopropyl monocarbonate (manufactured by Kayaku Nouryon, "Trigonox BPIC-75", 1-minute half-life temperature T1 = 158.8°C) using a ribbon blender. The obtained mixture was fed from the feed port of a twin-screw extruder (L / D=31.5) having a diameter of 57 mm. The twin-screw extruder had, from upstream to downstream, a feed section to which the above mixture was supplied, a reaction section in which the polylactic acid resin was modified, and a kneading section in which the resin composition obtained in the reaction section was kneaded.Of the total length of the extruder (100%), the length of the feed section was 20%, the length of the reaction section was 40%, and the length of the kneading section was 40%. The feed section was composed of one zone (C1), the reaction section was composed of four zones (C2 to C5), and the kneading section was composed of four zones (C6 to C9). The temperature setting for C1 in the feed section was 140°C, the temperatures for C2 to C5 in the reaction sections were 200°C, and the temperatures for C6 to C9 in the kneading sections were 185°C. The mixture was melt-kneaded in the twin-screw extruder at a rotation speed of 150 rpm, and the kneaded product was extruded in the form of strands at an output rate of 30 kg / h from a die with an orifice diameter of 3 mm and 18 holes attached to the tip of the twin-screw extruder. Next, the extruded strand-like kneaded product was passed through a 2 m long cooling water tank containing water at 30° C. to cool it. The cooled strand was cut with a pelletizer to obtain pellets of the modified polylactic acid resin (1). (2) Preparation of polylactic acid resin foam sheet 100 parts by mass of the resulting modified polylactic acid resin (1) and 1.0 part by mass of a cell regulator ("Crown Talc" manufactured by Matsumura Sangyo Co., Ltd.) were dry blended to prepare a mixture. In a tandem extruder equipped with a first extruder (upstream) with a diameter of φ50 mm and a second extruder (downstream) with a diameter of φ65 mm, the obtained mixture was supplied to the first extruder with a diameter of φ50 mm through a hopper and heated and melted at 220°C. Thereafter, butane (isobutane / normal butane=70% by mass / 30% by mass) as a foaming agent was pressure-fed into the first extruder and melt-mixed together with the above mixture. The molten mixture was then transferred to a second extruder with a 65 mm aperture and uniformly cooled to 170°C, after which it was extruded and foamed through a circular die with a φ70 mm aperture at a discharge rate of 30 kg / h to obtain a cylindrical foam. The obtained cylindrical foam was placed on a φ206 mm mandrel whose inside was cooled with water at about 20°C, and its outer surface was cooled and molded by blowing air onto it using an air ring larger than its diameter. It was then cut at one point on the circumference with a cutter to obtain a belt-shaped polylactic acid resin foam sheet (1). The results are shown in Table 1.

[0105] [Example 2] The same procedure as in Example 1 was carried out except that the set temperatures of the reaction sections C2 to C5 were set to 230°C and the set temperatures of the kneading sections C6 to C9 were set to 200°C, thereby obtaining modified polylactic acid resin pellets (2) and a polylactic acid resin foam sheet (2). The results are shown in Table 1.

[0106] [Example 3] As a polylactic acid resin, Nature Works' Biopolymer Ingeo 6202D (MFR = 10.1 g / 10 min, density = 1240 kg / m 3 The same procedure as in Example 1 was carried out except that a modified polylactic acid resin having a moisture content of 0.05% by mass was used, to obtain modified polylactic acid resin pellets (3) and a polylactic acid resin foam sheet (3). The results are shown in Table 1.

[0107] [Comparative Example 1] The same procedure as in Example 1 was carried out except that the set temperature of the feed section C1 was 185°C and the set temperatures of the reaction sections C2 to C5 were 230°C, thereby obtaining modified polylactic acid resin pellets (C1) and a polylactic acid resin foam sheet (C1). The results are shown in Table 1.

[0108] [Table 1] [Industrial Applicability]

[0109] The polylactic acid resin foam sheet obtained by the production method of the present invention has an excellent appearance and can be easily molded into a variety of shapes, and is therefore used as a raw material for various molded products, including packaging materials. [Explanation of symbols]

[0110] 1 Foam sheet 3 Die 4 Pelletizer 5 Drying equipment 6 Cooling device 10 Tandem Extruder 10a First Extruder 10b Second Extruder 11 Hopper 12 Gas inlet 21 Laura 22 Winding roller 30 Extruder 31 Feed section 31a Supply port 32 Reaction section 33 Mixing section

Claims

1. A method for producing a modified polylactic acid resin, comprising the steps of: The method includes a modification step of modifying a polylactic acid resin in an extruder, The extruder includes, in order from the upstream side to the downstream side, a feed section to which the polylactic acid resin is supplied, a reaction section in which the polylactic acid resin is modified, and a kneading section in which the resin composition obtained in the reaction section is kneaded; The set temperature of the feed section is 180° C. or less, The gel fraction of the resulting modified polylactic acid resin is less than 10% by mass. A method for producing a modified polylactic acid resin.

2. The method for producing a modified polylactic acid resin according to claim 1 , wherein a modifier is supplied to the feed section.

3. The method for producing the modified polylactic acid resin according to claim 1, further comprising a pelletizing step of pelletizing the kneaded material extruded from the extruder.

4. A modified polylactic acid resin having a gel fraction of less than 10% by mass, obtained by the method according to any one of claims 1 to 3.

5. The modified polylactic acid resin according to claim 4, which has an MFR of 5.0 g / 10 min or less at a temperature of 190° C. and a test load of 21.18 N, measured in accordance with Method B of JIS K 7210:1999.

6. The modified polylactic acid resin of claim 4, having a melt tension of greater than 18 cN at a temperature of 190°C.

7. A polylactic acid resin foamed sheet obtained by melt-kneading a polylactic acid resin (P) containing the modified polylactic acid resin according to claim 4 as a main component with a foaming agent in an extruder, followed by extrusion foaming.

Citation Information

Patent Citations

  • Regeneration treatment of coating film applied resin

    JP1996300352A

  • Method for producing cross-linked material made of polylactic acid and the cross-linked material made of polylactic acid

    JP2006249384A

  • Production method of polycarbonate resin composition

    JP2012072329A

  • Polylactic resin foam

    JP2019183097A

  • Method for producing modified polylactic resin

    JP2019183140A