Electrode structure and manufacturing method thereof, secondary battery and manufacturing method thereof, battery pack, vehicle, and stationary power source
The electrode structure with ionic liquid capsules addresses water electrolysis in secondary batteries, enhancing electromotive force and energy density by preventing water entry and hydrogen gas generation.
Patent Information
- Application Number
- JP2023045728
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Secondary batteries with aqueous electrolytes face challenges in preventing water electrolysis, which limits their electromotive force and hinders the development of high-performance batteries.
An electrode structure incorporating ionic liquid capsules with a wall containing first particles and an ionic liquid, which acts as a separator to prevent water molecules and hydrogen ions from entering the electrode, allowing for wider potential windows and higher electromotive force.
The electrode structure suppresses water electrolysis, enabling higher electromotive force and improved energy density and capacity in secondary batteries.
Smart Images

Figure 2024135177000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an electrode structure and a manufacturing method thereof, a secondary battery and a manufacturing method thereof, a battery pack, a vehicle, and a stationary power source. [Background technology]
[0002] In the case of secondary batteries with aqueous electrolytes, the electrolysis of water, mainly the generation of hydrogen gas at the negative electrode, is an issue. In order to prevent the electrolysis of water, it is desirable to charge and discharge the battery within the potential window of water. As a result, the electromotive force of the battery is also limited by the electrolysis of water, making it difficult to realize a secondary battery with an aqueous electrolyte that has a high electromotive force. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 4580801 [Non-patent literature]
[0004] [Non-Patent Document 1] H. Seki, K. Yoshima, Y. Yamashita, S. Matsuno, N. Takami, J. Power Sources, 482 (2021) 228950. [Non-Patent Document 2] JW Kim, JY Ko, JB Jun, IS Chang, HH Kang, KD Suh, Colloid Polym Sci. 281 (2003) 157. [Non-Patent Document 3] S. Kiyoyama, K. Shiomori, Y. Kawano, and Y. Hatate, J. Microencapsulatoin, 20, 4 (2003)497. Summary of the Invention [Problem to be solved by the invention]
[0005] The problem to be solved is to provide an electrode structure and a manufacturing method thereof, a secondary battery and a manufacturing method thereof, a battery pack, a vehicle, and a stationary power source, which are capable of suppressing electrolysis of water and improving electromotive force. [Means for solving the problem]
[0006] According to an embodiment, there is provided an electrode structure including an electrode and a layer in contact with the electrode, the layer including a capsule having a wall including a first particle and an ionic liquid contained within the capsule.
[0007] According to the embodiment, a secondary battery is provided that includes the electrode structure of the embodiment and an aqueous electrolyte.
[0008] According to the embodiment, a battery pack including the secondary battery of the embodiment is provided.
[0009] According to the embodiment, a vehicle including the battery pack of the embodiment is provided.
[0010] According to the embodiment, there is also provided a stationary power source including the battery pack of the embodiment.
[0011] Furthermore, according to an embodiment, there is provided a method for producing an electrode structure, the method including the steps of: producing capsules having a wall membrane containing the first particles and containing an ionic liquid therein by causing a polymerization reaction in an emulsion containing the first particles, an ionic liquid, and a wall membrane raw material; and forming a layer containing the capsules in an active material-containing layer.
[0012] According to the embodiment, there is provided a method for producing a secondary battery, the method including the steps of producing an electrode group including the electrode structure of the embodiment and a counter electrode, and causing the electrode group to retain an electrolyte solution. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view taken along a thickness direction (stacking direction) of an electrode structure according to an embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing an ionic liquid capsule of the electrode structure shown in FIG. 1. [Diagram 3] FIG. 4 is a schematic cross-sectional view of another example of an electrode structure according to an embodiment, taken along the thickness direction (stacking direction). [Figure 4] 5A to 5C are schematic diagrams showing an example of producing a single emulsion in a manufacturing method of an electrode structure according to an embodiment. [Diagram 5] FIG. 4 is a schematic diagram showing a primary emulsification of an example of double emulsion production in a manufacturing method of an electrode structure according to an embodiment. [Figure 6] FIG. 4 is a schematic diagram showing secondary emulsification of an example of double emulsion production in a manufacturing method of an electrode structure according to an embodiment. [Figure 7] 1 is a schematic cross-sectional view of an electrode group including an electrode structure according to an embodiment, taken along a thickness direction (stacking direction). [Figure 8] FIG. 4 is a schematic cross-sectional view along the thickness direction (stacking direction) of another example of an electrode group including the electrode structure of the embodiment. [Figure 9] FIG. 2 shows cyclic voltammograms of an ionic liquid for a positive electrode and an ionic liquid for a negative electrode. [Figure 10] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Figure 11] 11 is a schematic cross-sectional view taken along line XI-XI of the secondary battery shown in FIG. 10. [Figure 12] FIG. 4 is a partially cutaway perspective view illustrating a secondary battery according to another embodiment of the present invention. [Figure 13] 13 is an enlarged cross-sectional view of a portion E of the secondary battery shown in FIG. 12. [Figure 14] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 15] FIG. 13 is an exploded perspective view illustrating a battery pack according to another embodiment of the present invention. [Figure 16] FIG. 16 is a block diagram showing an example of an electrical circuit of the battery pack shown in FIG. [Figure 17]FIG. 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 18] FIG. 1 is a block diagram showing an example of a system including a stationary power supply according to an embodiment. [Figure 19] FIG. 4 is a schematic diagram showing a method for producing an ionic liquid capsule in Example 2. [Figure 20] FIG. 1 shows a reaction scheme of a polymerization reaction used in the preparation of ionic liquid capsules in Example 3. [Figure 21] FIG. 1 shows a reaction scheme of a polymerization reaction used in the preparation of ionic liquid capsules in Example 4. [Figure 22] FIG. 13 shows a reaction scheme of a polymerization reaction used in the preparation of the ionic liquid capsules of Example 5. [Figure 23] 3 is a graph showing charge / discharge curves of the secondary batteries of Example 1 and Comparative Example 1. [Figure 24] FIG. 3 is a cross-sectional view showing a schematic cross section of the ionic liquid capsule shown in FIG. 2 taken along a radial direction. [Diagram 25] FIG. 11 is a cross-sectional view showing a schematic cross section of another example of an ionic liquid capsule cut in a radial direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] (First embodiment) According to a first embodiment, an electrode structure is provided. The electrode structure includes an electrode and a layer (hereinafter referred to as a first layer) in contact with the electrode. The first layer includes a capsule having a wall membrane containing first particles, and an ionic liquid contained in the capsule. A capsule having a wall membrane containing first particles and containing an ionic liquid is hereinafter referred to as an ionic liquid capsule. The first layer has ion conductivity, but can electrically insulate the electrode from other members, and therefore can function as an insulating layer (e.g., a separator) having ion conductivity.
[0015] The multiblock structure consisting of the wall membrane, the first particle, and the ionic liquid is a water molecule (HO) and a hydrogen ion (H +Since the electrolyte prevents the intrusion of hydrogen into the electrode, the electrolysis of water on the electrode is suppressed, thereby suppressing the generation of hydrogen gas. This allows the battery to be charged and discharged within a potential window of an ionic liquid or the like that is wider than that of water, thereby providing an aqueous battery with a high electromotive force.
[0016] Ionic liquid capsules can freely deform in response to stress, and therefore have excellent elasticity, flexibility, and adhesion. Therefore, the electrode structure can improve the uniformity of in-plane contact within the secondary battery. By controlling the thickness, material, and structure of the wall of the ionic liquid capsule, the elasticity and flexibility of the first layer can be controlled.
[0017] In addition, since the ionic liquid capsules can be freely deformed, it is easy to increase the density of the first layer, for example by pressing, and a highly dense first layer can be obtained.
[0018] Furthermore, since the ionic liquid is encapsulated in a capsule, leakage of the ionic liquid can be prevented.
[0019] An example of the electrode structure will be described with reference to Figs. 1 to 3, 24 and 25. In Figs. 1 to 3, the direction parallel to the thickness direction or lamination direction of the electrode structure is the z-axis direction, the direction parallel to one side of a surface (referred to as a main surface) of the electrode structure that intersects perpendicularly to the z-axis direction is the x-axis direction, and the direction parallel to the other side that intersects perpendicularly to the one side of the main surface is the y-axis direction. When the main surface of the electrode structure is rectangular, for example, the x-axis direction is parallel to the long side or short side direction of the main surface. Fig. 24 is a cross-sectional view that typically shows a cut surface along the radial direction of the ionic liquid capsule shown in Fig. 2. Meanwhile, Fig. 25 is a cross-sectional view that typically shows a cut surface along the radial direction of another example of the ionic liquid capsule.
[0020] As shown in FIG. 1, the electrode structure 1 includes an electrode 500 and a first layer 502 including ionic liquid capsules 501. The electrode 500 includes a current collector 503 and an active material-containing layer 504 formed on one side of the current collector 503. The first layer 502 including the ionic liquid capsules 501 is on the main surface of the active material-containing layer 504. The first layer 502 including the ionic liquid capsules 501 is in contact with the main surface of the active material-containing layer 504 and is bonded to the main surface of the active material-containing layer 504. As shown in FIG. 2 and FIG. 24, the ionic liquid capsules 501 include a wall film 505, first particles 506 dispersed in the wall film 505, and an ionic liquid (IL) contained in a space defined by the wall film 505. A part of the first particles 506 is exposed to the surface of the wall film 505 or protrudes from above the wall film 505. FIG. 24 shows an example in which the first particles 506 are dispersed in the wall film 505, but the ionic liquid capsule 501 is not limited to this example. For example, as shown in FIG. 25, a part of the first particles 506 may be dispersed in the wall film 505, and another part of the first particles 506 may be dispersed in the ionic liquid (IL). A preferred form of the ionic liquid capsule 501 is a form in which the first particles 506 are dispersed in the wall film 505 but are not present in the ionic liquid (IL), as exemplified in FIG. 24. The first layer 502 is an aggregate of the ionic liquid capsules 501. The aggregate of the ionic liquid capsules 501 is formed by bonding the ionic liquid capsules 501 together, for example, by pressure bonding or by a first binder. In FIG. 1, the active material-containing layer 504 is laminated on one side of the current collector 503, but the active material-containing layer 504 may be laminated on both sides of the current collector 503. In this case, the first layer 502 is bonded to the major surfaces of both active material-containing layers 504 .
[0021] The multiblock structure consisting of the wall film 505, the first particles 506, and the ionic liquid (IL) forms water molecules (HO) and hydrogen ions (H + ) can be prevented from penetrating into the active material-containing layer 504, so that electrolysis of water on the electrode 500 can be suppressed, and the generation of hydrogen gas can be suppressed. In addition, since the first particles 506 are particles that are permeable to alkali metal ions, lithium ions (Li + ) can secure a path for the movement of metal ions (shown by arrows in Figure 2).
[0022] Further, for example, as shown in FIG. 3, at least a part of the first layer 502 containing the ionic liquid capsule 501 may be present so as to penetrate into the active material-containing layer 504. Therefore, in the electrode structure 1, at least a part of the boundary between the active material-containing layer 504 and the first layer 502 may be composed of a region R containing (mixed with) a part of the active material-containing layer (for example, active material particles) and the ionic liquid capsule 501. Thereby, since the adhesion between the first layer 502 and the active material-containing layer 504 can be increased, the in-plane contact uniformity between the first layer 502 and the active material-containing layer 504 can be improved.
[0023] Hereinafter, the electrode structure will be described in more detail.
[0024] <Electrode> The electrode includes a current collector and an active material-containing layer formed on at least one surface of the current collector. The electrode can be at least one of a positive electrode and a negative electrode. The case where the electrode is a positive electrode and the case where the electrode is a negative electrode will be described separately.
[0025] <Positive Electrode> <Positive Electrode Active Material-Containing Layer> The positive electrode active material-containing layer can contain a positive electrode active material, and optionally a conductive agent and a binder.
[0026] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain one kind of compound alone as the positive electrode active material, or may contain a combination of two or more kinds of compounds. Examples of the oxide and the sulfide include compounds into which Li or Li ions can be inserted and desorbed.
[0027] Such compounds include, for example, manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (for example, Li x Mn2O4 or Li x MnO2; 0 <x ≦ 1), lithium nickel composite oxide (for example, Li xNiO2; 0 < x ≤ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium phosphate having an olivine structure (e.g., Li x FePO4; 0 < x ≤ 1, Li x Fe 1-y Mn y PO4; 0 < x ≤ 1, 0 < y < 1, Li x CoPO4; 0 < x ≤ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) are included.
[0028] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≤ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni yO4; where 0 < x ≤ 1 and 0 < y < 2), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; where 0 < x ≤ 1 and 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; where 0 < x ≤ 1), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; where 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, and y + z < 1) are included. When these compounds are used as the positive electrode active material, the positive electrode potential can be increased.
[0029] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. The positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. The positive electrode active material with a primary particle size of 1 μm or less can allow the solid-state diffusion of lithium ions to proceed smoothly.
[0030] The specific surface area of the positive electrode active material is preferably 0.1 m 2 / g or more and 10 m 2 / g or less. The positive electrode active material with a specific surface area of 0.1 m 2 / g or more can sufficiently secure the Li-ion insertion / extraction sites. The positive electrode active material with a specific surface area of 10 m 2 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.
[0031] The binder (positive electrode binder) is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the positive electrode binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the positive electrode binder, or two or more may be combined and used as the positive electrode binder.
[0032] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanofiber, and carbon nanotube, and other carbonaceous materials. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0033] In the positive electrode active material-containing layer, the positive electrode active material and the positive electrode binder are preferably mixed in proportions of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.
[0034] By making the amount of the positive electrode binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the positive electrode binder can function as an insulator. Therefore, by making the amount of the positive electrode binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0035] When a conductive agent is added, the positive electrode active material, the positive electrode binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.
[0036] By setting the amount of the conductive agent to 3% by mass or more, the above-mentioned effects can be achieved. Also, by setting the amount of the conductive agent to 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0037] <Positive electrode current collector> Examples of the positive electrode current collector include a current collector containing a material that is electrochemically stable at a potential at which lithium (Li) is inserted into and extracted from the active material, a current collector containing a conductive resin that contains a polymer material and a conductive material, and a current collector containing at least one metal element selected from the group consisting of Pb, Bi, Zn, Sb, and Sn.
[0038] The current collector containing a material that is electrochemically stable at a potential at which lithium (Li) is inserted into and extracted from the active material may be an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si, a metal foil containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si, a nickel foil, a stainless steel foil, or an aluminum foil.
[0039] Examples of polymeric materials include materials containing at least one resin consisting of polyene, polyaniline, polypyrrole, polythiophene, polyacetylene, polyparaphenylene, polyphenylenevinylene, polyacrylonitrile, polyoxadiazole, polyethylene, polypropylene, polystyrene, polyethylene terephthalate, polyether nitrile, polyimide, polyamide, polyamideimide, polytetrafluoroethylene, styrene-butadiene rubber, and their analogues. The polymeric materials can be used alone or in combination of two or more. Examples of conductive materials (conductive fillers) include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbonaceous materials such as carbon nanofibers and carbon nanotubes, and metal particles. Examples of metals for the metal particles include gold, silver, copper, iron, aluminum, titanium, and nickel. The conductive materials can be one type or two or more types. The thickness of the positive electrode current collector can be, for example, not less than 5 μm and not more than 200 μm.
[0040] The current collector may include a portion on the surface of which no active material-containing layer is formed, and this portion may function as a current collecting tab or a current collecting lead.
[0041] <Negative electrode> <Negative electrode active material containing layer> The negative electrode active material-containing layer can contain a negative electrode active material, and optionally a conductive agent and a binder.
[0042] The negative electrode active material may be, for example, lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12, 0≦x≦3), monoclinic titanium dioxide (TiO2(B)), anatase titanium dioxide, rutile titanium dioxide, niobium pentoxide (Nb2O5), hollandite titanium composite oxide, orthorhombic titanium-containing composite oxide, and monoclinic niobium titanium composite oxide. The type of the negative electrode active material may be one or more types.
[0043] As an example of an orthorhombic titanium-containing composite oxide, Li 2+a M(I) 2-b Ti 6-c M(II) d O 14+σ Here, M(I) is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb, and K. M(II) is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).
[0044] As an example of monoclinic niobium titanium composite oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium composite oxides include Li x Examples include Nb2TiO7 (0≦x≦5).
[0045] Another example of monoclinic niobium titanium composite oxide is Li x Ti1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0046] The conductive agent is blended to improve the current collecting performance and to reduce the contact resistance between the active material and the current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanofibers, and carbonaceous materials such as carbon nanotubes. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coating or an electronically conductive inorganic material coating may be applied to the surface of the active material particles.
[0047] The binder (negative electrode binder) is blended to fill the gaps between the dispersed active materials and to bind the active materials and the negative electrode current collector. Examples of the negative electrode binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene-butadiene rubber (SBR), polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC), and salts of CMC. One of these may be used as the negative electrode binder, or two or more may be combined and used as the negative electrode binder.
[0048] The mixing ratio of the negative electrode active material, the conductive agent, and the negative electrode binder in the negative electrode active material-containing layer can be appropriately changed depending on the application of the negative electrode. For example, it is preferable to mix the negative electrode active material, the conductive agent, and the negative electrode binder at a ratio of 68% by mass or more and 96% by mass or less, 2% by mass or more and 30% by mass or less, and 2% by mass or more and 30% by mass or less, respectively. By making the amount of the conductive agent 2% by mass or more, the current collection performance of the negative electrode active material-containing layer can be improved. In addition, by making the amount of the negative electrode binder 2% by mass or more, the binding property between the negative electrode active material-containing layer and the current collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferable to make the conductive agent and the negative electrode binder 30% by mass or less, respectively, in order to increase the capacity.
[0049] <Negative electrode current collector> Examples of the negative electrode current collector include a current collector containing a material that is electrochemically stable at a potential at which lithium (Li) is inserted into and extracted from the active material, a current collector containing a conductive resin that contains a polymer material and a conductive material, and a current collector containing at least one metal element selected from the group consisting of Pb, Bi, Zn, Sb, and Sn. The current collector containing a material that is electrochemically stable at a potential at which lithium (Li) is inserted and extracted from the active material is preferably made of copper, nickel, stainless steel, aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si.
[0050] Examples of the current collector containing a conductive resin containing a polymer material and a conductive material, and the current collector containing at least one metal element selected from the group consisting of Pb, Bi, Zn, Sb, and Sn, can be similar to those described for the positive electrode.
[0051] The thickness of the negative electrode current collector can be, for example, not less than 5 μm and not more than 200 μm.
[0052] The current collector may include a portion on the surface of which no active material-containing layer is formed, and this portion may function as a current collecting tab or a current collecting lead.
[0053] <First layer containing ionic liquid capsules> The first layer containing ionic liquid capsules may be, for example, an aggregate of a plurality of ionic liquid capsules. In the aggregate of ionic liquid capsules, the ionic liquid capsules may be bonded together by pressure or with a binder (first binder). The ionic liquid capsule contains a wall membrane, a first particle contained in the wall membrane, and an ionic liquid contained in a space defined by the wall membrane.
[0054] The type of ionic liquid capsule may be one or more types. Therefore, the capsule may contain one type of ionic liquid, or the capsule may have the same type of wall membrane but different types of ionic liquid.
[0055] The wall membrane of the ionic liquid capsule is not particularly limited, but may include a matrix consisting of at least one selected from the group consisting of an amphiphilic molecular membrane, a polymer membrane, a carbon layer membrane, an organic material membrane, an inorganic material membrane, and a membrane containing an organic material and an inorganic material, and a first particle dispersed in the matrix. The matrix may be formed of a single material or a plurality of types. The carbon layer membrane can be formed by baking a material containing C. The amphiphilic molecular membrane includes crosslinked amphiphilic molecules.
[0056] The thickness of the wall film can be, for example, 10 μm or more.
[0057] The first particles may be, for example, particles that are permeable to alkali metal ions. This allows the lithium ions (Li +) can ensure a path for the movement (diffusion) of metal ions such as Li ions. Examples of materials that can transmit alkali metal ions include conductors of alkali metal ions such as Li ions and solid electrolytes. Specific examples of alkali metal ion conductors and solid electrolytes include lithium aluminum titanium phosphate (LAPT), MOFs (metal organic frameworks), lithium oxynitride phosphate (LiPON), LICGC (Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2), Al2O3, SiO2, Si3N4, Li2S-SiS2, Li2O-B2O3-P2O5, Li2O-B2O3-SiO2, Li2O-B2O3-SeO2, Li2S-GeS2-SiS2, n-Li2SiS3, oxide solid electrolytes with a garnet structure, and lithium phosphate solid electrolytes with a Nasicon structure (for example, Li 1.5 Al 0.5 Ti 1.5 (PO4)3(LATP) etc. The first particles may be formed of a single material or a plurality of types of materials.
[0058] The first particles may be one component constituting the wall film, and the arrangement thereof is not limited. For example, the first particles may be dispersed in the wall film, and a part of the first particles may be exposed on the surface of the wall film, a part of the first particles may protrude from the surface of the wall film, or a part of the first particles may be embedded in the wall film.
[0059] The size of the first particles contained in the wall membrane may be smaller than that of the ionic liquid capsule, and may have an average particle size in the range of 1 μm to 15 μm, for example. The first particles having an average particle size in this range can be uniformly dispersed on the capsule surface. A more preferable range is 1 μm to 2 μm.
[0060] The first layer may contain second particles that are not enclosed in either the wall or the capsule. The second particles may be similar to those described for the first particles.
[0061] The ionic liquid capsules may be of a size called a microcapsule. The average particle size of the ionic liquid capsules may be, for example, in the range of 20 μm to 300 μm. More preferably, the average particle size may be in the range of 20 μm to 100 μm.
[0062] Ionic liquids can be composed of cations (positive ions) and anions (negative ions). The types of ions constituting an ionic liquid can be one or more types.
[0063] The ionic liquid is preferably an ionic liquid that is impermeable to at least one of water and hydrogen ions. As the ionic liquid that is impermeable to at least one of water and hydrogen ions, it is preferable to use an aprotic ionic liquid or a hydrophobic ionic liquid. The ionic liquid that is impermeable to at least one of water and hydrogen ions will be described in detail below.
[0064] Representative cations include at least one selected from the group consisting of imidazolium ion, ammonium ion, phosphonium ion, pyridinium ion, pyridium ion, piperidinium ion, tetramethylammonium ion, trialkylsulfonium ion, alkylimidazolium ion, and quaternary ammonium ion, and an alkali metal ion.
[0065] The anions are halides, formate, nitrate, hydrogen sulfate, and trifluoromethanesulfonate (abbreviation: [TfO] - ), PF6 - ,BF4 ― , trifluoroacetate ion, bis(trifluoromethylsulfonyl)imide (abbreviation: [N(CF3SO2)2] - ) and [N(FSO2)2]- The anion preferably includes at least one selected from the group consisting of CF3SO3 - , [N(CF3SO2)2] - , and [N(FSO2)2] - The compound is one or more selected from the group consisting of:
[0066] The ionic liquid, which is composed of the above-mentioned cations and anions, is impermeable to at least one of water and hydrogen ions, and has a wide potential window, is non-volatile, has high thermal stability, a low melting point, and has high ionic conductivity.
[0067] Examples of the alkali metal ion as the cation include a lithium ion, a sodium ion, a potassium ion, etc. The alkali metal ion is preferably a lithium ion.
[0068] Lithium ions can be provided, for example, from a lithium salt. Examples of lithium salts include LiBF4, LiPF6, LiAsF6, LiClO4, LiCF3SO3, LiN(FSO2)2, LiN(CF3SO2)2, LiN(C2F5SO2)2, Li(CF3SO2)3C, LiB[(OCO)2]2, and the like. The type of lithium salt used can be one or more. The amount of lithium salt dissolved in the ionic liquid is preferably 0.1 mol / kg or more and 2 mol / kg or less.
[0069] The trialkylsulfonium ion has a skeleton represented by the following formula (1). Examples of the trialkylsulfonium ion include a triethylsulfonium ion, a trimethylsulfonium ion, and a methylethylpropylsulfonium ion. The triethylsulfonium ion and the methylethylpropylsulfonium ion, which have a low melting point and high ionic conductivity, are preferred.
[0070] [ka]
[0071] The alkylimidazolium ion and the quaternary ammonium cation each have a skeleton represented by formula (2).
[0072] [ka]
[0073] Examples of alkylimidazolium ions include dialkylimidazolium ions, trialkylimidazolium ions, and tetraalkylimidazolium ions. An example of a dialkylimidazolium ion is 1-methyl-3-ethylimidazolium ion (MEI + ), 1-methyl-3-propylimidazolium ion. An example of a trialkylimidazolium ion is 1,2-dimethyl-3-propylimidazolium ion (DMPI + Examples of tetraalkylimidazolium ions include the 1,2-diethyl-3,4(5)-dimethylimidazolium ion.
[0074] Examples of quaternary ammonium ions include tetraalkylammonium ions, cyclic ammonium ions, etc. Tetraalkylammonium ions are preferred. Examples of tetraalkylammonium ions include diethylmethylmethoxyethylammonium ion (DEME), dimethylethylmethoxyethylammonium ion, dimethylethylmethoxymethylammonium ion, dimethylethylethoxyethylammonium ion, and trimethylpropylammonium ion.
[0075] When the first layer containing ionic liquid capsules is joined to the negative electrode active material-containing layer, the self-discharge of the secondary battery can be suppressed by using an aprotic ionic liquid as the ionic liquid. Examples of aprotic ionic liquids include N-(2-Methoxyethyl)-N-methylpyrrolidinium tetrafluoroborate (abbreviation: MEMPBF4), N-(2-Methoxyethyl)-N-methylpyrrolidinium bis(trifluoromethanesulfonyl)imide (abbreviation: MEMPTFSI or MEMOTFSA), N,N-Diethyl-N-methyl-N-(2-methoxyethyl)ammonium tetrafluoroborate (abbreviation: DEMEBF4), N,N-Diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethanesulfonyl)imide (abbreviation: DEMEBF4), and N,N-Diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethanesulfonyl)imide (abbreviation: DEMEBF4). N-Diethyl-N-methyl-N-(2-methoxyethyl) ammonium bis(trifluoromethanesulfonyl)imide (abbreviation: DEMETFSI or DEMETFSA)), N,N,N-trimethyl-N-propylammonium bis(trifluoromethanesulfonyl)imide (N,N,N-Trimethyl-N-propylammonium bis(trifluoromethanesulfonyl)imide (abbreviation: TMPA TFSI)), N-Methyl-N-propylpiperidinium bis(trifluoromethanesulfonyl)imide (PP13 TFSI)), 1-Ethyl-3-methylimidazolium trifluoromethanesulfonate (abbreviation: [emim][Tf]), ethyl-3-methylimidazolium tetrafluoroborate (abbreviation: [emim][BF4]), ethyl-3-methylimidazolium chloride (abbreviation: [emim][Cl]), 1-Ethyl-3-methylimidazolium These include bis(trifluoromethylsulfonyl)imide (1-Ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide (abbreviation: EMIM TFSI)) and 1-Butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide (abbreviation: BMIMTFSI).
[0076] The ionic liquid may be in a gel state. This can stabilize the first layer. The gel state ionic liquid can be obtained, for example, by adding a low molecular weight organic gelling agent to the ionic liquid, heating them, and then cooling them. An example of the low molecular weight organic gelling agent is 12-hydroxystearic acid Cyclo(L-β-3,7-dimethyloctylas-paraginyl-L-phenylalanyl)Gelatin (LMOG). In addition, for example, gelatin, MOGs, or hydroxypropylmethylcellulose (HPMC) can be used as the gelling agent.
[0077] Ionic liquids can also be used in the form of polymerized ionic liquids by polymerizing or cross-linking.
[0078] The first layer containing the ionic liquid capsules may contain an ionic liquid (second ionic liquid) in addition to the ionic liquid capsules. The second ionic liquid can function as a plasticizer, and therefore can improve the elasticity and flexibility of the first layer. The second ionic liquid can be the same as that described for the ionic liquid (first ionic liquid) used in the ionic liquid capsules.
[0079] The first layer containing the ionic liquid capsules may contain a first binder. The first binder is not particularly limited as long as it is of the type used as the second binder (positive or negative electrode binder) in the active material-containing layer, but for example, CMC (Carboxymethyl cellulose) can be used. The content of the first binder in the layer containing the ionic liquid capsules can be 10 mass% or less.
[0080] The layer containing the ionic liquid capsules may include a support (carrier) having voids. The ionic liquid capsules can be fixed by being embedded in the voids of a porous support (carrier) or a retina-like support. In this case, no binder is required.
[0081] As a carrier for immobilizing the ionic liquid capsules, a carrier such as a porous membrane, a porous monolayer material, zeolite, a silica glass membrane, or a polymer can be used. When a polymer is used as a carrier for ionic liquid capsules, a polymer / ionic liquid composite material such as a polymer / ionic liquid capsule composite membrane or a polymer / ionic liquid capsule fiber can be produced by casting, electrospinning, or suction. Examples of polymers that can be used include poly(vinylidene difuoride) (PVDF) and poly(vinylidene difuoride)-hexafluoropropylene (PVDF-HFP). In addition, a polymer / ionic liquid capsule membrane can be created on the surface of the electrode by dissolving and mixing a polymer material and an ionic liquid capsule material in a solvent and spraying the mixture onto a porous electrode material. As a carrier material for preparing the ionic liquid capsule membrane, for example, a hydrophobic polymer material or a hydrophilic polymer material can be used. As a hydrophobic polymer material, for example, polyvinylidene fluoride (PVDF) can be used. As a hydrophilic polymer material, for example, polyethylene (PE), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA) can be used. Alternatively, a mixture of hydrophobic and hydrophilic polymer materials can be used. When a mixture is used, for example, PVDF and PTFE can be mixed and used. In addition to polymer materials, anodized alumina nanoporous membrane, porous TiO2, mesoporous carbon, etc. can also be used as a carrier material that enables the ionic liquid capsule to be used as a membrane.
[0082] The average particle size of the ionic liquid capsules, the average thickness of the wall film, and the average particle size of the first particles can be measured using a measuring device such as a high-sensitivity optical microscope, a scanning electron microscope (SEM), or a confocal microscope. The average particle size of the ionic liquid capsules, the average thickness of the wall film, and the average particle size of the first particles can be obtained based on optical images, SEM image photographs, and confocal microscope images of the capsules obtained using a high-sensitivity optical microscope, SEM, or confocal microscope. The thickness of the wall film of the ionic liquid capsule can be estimated from optical images, SEM image photographs, or confocal microscope images of the cross section of the ionic liquid capsule. An appropriate method is selected from the above methods depending on the size of the ionic liquid capsule or the measurement site.
[0083] When the electrode structure is incorporated in a secondary battery, the electrode structure is removed from the secondary battery by the following method, and then the above measurement is performed. The secondary battery is discharged, disassembled, and the electrode structure is removed. The removed electrode structure is washed with pure water for 30 minutes. Then, it is dried for 24 hours in a temperature environment of 40°C to 80°C. After drying, the temperature is returned to 25°C, and the electrode structure to be measured is obtained.
[0084] A method for manufacturing the electrode structure will be described below.
[0085] <Preparation of electrodes> First, a method for producing an electrode will be described. An active material, a conductive agent, and a second binder (positive electrode binder or negative electrode binder) are suspended in a solvent to prepare a slurry. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. Then, this laminate is pressed. In this manner, an electrode is produced. Alternatively, the electrode may be produced by the following method. First, an active material, a conductive agent, and a second binder are mixed to obtain a mixture. Next, this mixture is formed into pellets. Next, these pellets are placed on a current collector to obtain an electrode.
[0086] <Preparation of ionic liquid capsules> Next, the ionic liquid capsule is prepared by the following method. First, an intermediate containing the first particle, the ionic liquid, and the wall membrane raw material is prepared. Examples of the intermediate include an ionic liquid / water (IL / W) single emulsion, an ionic liquid / water / oil (IL / W / O) double emulsion, a vesicle, or an inverse vesicle. The intermediate can be prepared, for example, by a one-step emulsification method or a two-step emulsification method. The one-step emulsification method and the two-step emulsification method can be an existing method. For example, the one-step emulsification method described in Japanese Patent No. 4580801 (Patent Document 1) may be used. The two-step emulsification method is described, for example, in Non-Patent Document 2 and Non-Patent Document 3. The IL / W single emulsion is an emulsion containing an IL phase and a W phase, with the IL phase dispersed in the W phase. The first particles are preferably dispersed in the W phase. The wall membrane material is dispersed in at least one of the W phase or the IL phase. In the IL / W / O double emulsion, the first particles are dispersed in the continuous phase O. The first particles can be dispersed in either the IL or W phase, but are preferably dispersed in the W phase. The wall membrane material is dispersed in any of the O, W, or IL phases. In the case of vesicles and reverse vesicles, microcapsules can be made by photopolymerizing or crosslinking the amphiphilic molecules.
[0087] Examples of wall film raw materials include amphiphilic molecules, monomers, dimers, trimers, tetramers, dimers, polymers, organic materials, inorganic materials, and hybrid materials of organic and inorganic materials. For example, when urethane is used as the wall film raw material, it is possible to prevent the wall film raw material from remaining in the core (core) of the ionic liquid capsule. In addition, the ionic liquid contained in the core (core) of the ionic liquid capsule is hydrophobic. Therefore, when a hydrophilic wall film raw material such as urea is used, the wall film raw material does not dissolve in the ionic liquid, so it is possible to prevent the wall film raw material from remaining in the core (core) of the ionic liquid capsule.
[0088] Each of the above intermediates may contain an emulsifier.As the emulsifier, for example, lipids and boundary lipids, sphingolipids, fluorescent lipids, cationic surfactants, anionic surfactants, amphoteric surfactants, nonionic surfactants, ionic liquid surfactants, synthetic polymers, natural polymers such as proteins, etc. can be appropriately selected and used.In addition, when the first particle functions as an emulsifier, it is not necessary to use an emulsifier.
[0089] For the O phase (oil phase), for example, any of the following can be practically used: hydrocarbons such as hexane, octane, isooctane, decane, dodecane, hexadecane, cyclohexane, etc.; hydrophobic solvents such as chloroform and soybean oil, hydrophobic ionic liquids, aromatic hydrocarbons such as benzene and toluene, etc. These solvents can be used alone or in combination.
[0090] Next, ionic liquid capsules are synthesized from intermediates such as IL / W single emulsions, IL / W / O double emulsions, vesicles, or reverse vesicles by at least one polymerization method selected from condensation polymerization, radical polymerization, in-situ polymerization, photopolymerization, interfacial precipitation, interfacial polymerization, interfacial reaction, and hydrolysis-condensation polymerization. This process allows the fluid membrane of the intermediate to be converted into a non-fluid wall membrane by physical or chemical methods. After synthesis, washing and drying may be performed as necessary.
[0091] <Preparation of the first layer containing ionic liquid capsules> The first binder is added to the ionic liquid capsules. These are mixed in the presence of a solvent to obtain a slurry. The obtained slurry is applied onto the active material-containing layer of the electrode, and the slurry is dried to form a first layer on the active material-containing layer, thereby obtaining an electrode structure. The first binder may be of the type described above.
[0092] An example of a method for synthesizing ionic liquid capsules from an IL / W single emulsion will be described with reference to FIG.
[0093] A Pickering emulsion 507 is prepared in which an ionic liquid (IL) and first particles 506 are dispersed in an aqueous solution (W phase) in which hexamethylenediamine is dissolved as a wall membrane raw material. As an example of the ionic liquid (IL), an ionic liquid called 1-butyl-3-methylimidazolium hexafluorophosphate (bmim) (PF6) is used. The first particles 506 function as a surfactant. The IL phase emulsified by the first particles 506 contains hexamethylene diisocyanate. The hexamethylene diisocyanate is a wall membrane raw material of the ionic liquid capsule.
[0094] In Pickering emulsion 507, polyurea is synthesized by interfacial polymerization of hexamethylene diamine and hexamethylene diisocyanate, and wall film 505 is formed in which first particles 506 are dispersed in a polyurea matrix. After leaving it for a time sufficient for the formation of the wall film, the reaction product is washed, the ionic liquid capsules are separated from the reaction product, and the separated ionic liquid capsules are washed and dried to obtain ionic liquid capsules 501. The obtained ionic liquid capsules 501 may contain unreacted hexamethylene diisocyanate in addition to the ionic liquid (IL).
[0095] Next, an example of a method for synthesizing ionic liquid capsules from an IL / W / O double emulsion will be described with reference to Figures 5 and 6. Figure 5 is a schematic diagram showing the primary emulsification for producing an IL / W single emulsion, and Figure 6 is a schematic diagram showing the secondary emulsification for producing an IL / W / O double emulsion using an IL / W single emulsion. The emulsification method shown in Figures 5 and 6 is a two-stage emulsification method, and the produced double emulsion is a multiple internal phase type double emulsion having multiple internal phases (ionic liquid phases). Note that when a one-stage emulsification method (for example, Patent Document 1 (P2005-96550)) is used, a single internal phase type double emulsion can be produced.
[0096] In the primary emulsification illustrated in Fig. 5, the aqueous solvent W phase in which the emulsifier 508 and the first particles 506 are dispersed is stirred, and the ionic liquid IL and the first particles 506 are emulsified in the aqueous solvent W phase (continuous phase) by the emulsifier 508 to obtain an IL / W single emulsion 509. Next, in the secondary emulsification illustrated in Fig. 6, the IL / W single emulsion 509 is poured into the oil phase O in which the emulsifier 508 is dispersed, and secondary emulsification is caused by stirring with a weaker stirring force than in the first stage, and the W phase (aqueous phase) containing the ionic liquid IL and the first particles 506 is emulsified in the oil phase O to obtain an IL / W / O double emulsion 510. The IL / W / O double emulsion 510 is subjected to a polymerization reaction to synthesize ionic liquid capsules.
[0097] The electrode structure of the first embodiment described above includes a first layer in contact with the electrode. The first layer includes a capsule having a wall membrane containing the first particles, and an ionic liquid contained in the capsule. The structure consisting of the wall membrane, the first particles, and the ionic liquid is a structure in which water molecules (HO) and hydrogen ions (H + ) from penetrating into the electrode, thereby suppressing the electrolysis of water on the electrode and suppressing the generation of hydrogen gas. Therefore, by using the electrode structure in a secondary battery having an aqueous electrolyte, it is possible to increase the electromotive force of the secondary battery. In addition, the capsules containing the first particles and the ionic liquid can be freely deformed in response to stress, and therefore have excellent elasticity, flexibility, and adhesion. Therefore, the electrode structure can improve the uniformity of in-plane contact and increase the density of the first layer. Second Embodiment According to the second embodiment, a secondary battery including an electrode structure is provided. The electrode structure of the first embodiment can be used for the electrode structure. The secondary battery can be, for example, a lithium secondary battery. The secondary battery may further include a counter electrode for the electrode of the electrode structure and an aqueous electrolyte. The secondary battery may further include a second layer, an exterior member, a positive electrode terminal, and a negative electrode terminal. The counter electrode, the second layer, the aqueous electrolyte, the exterior member, the positive electrode terminal, and the negative electrode terminal will be described below. <Opposite> The counter electrode is provided so that the first layer is located between the electrode of the electrode structure.
[0098] When the electrode of the electrode structure is a positive electrode, a negative electrode is used as the counter electrode. When the electrode of the electrode structure is a negative electrode, a positive electrode is used as the counter electrode. The positive electrode and the negative electrode are the same as those described in the first embodiment.
[0099] Between the counter electrode and the electrode of the electrode structure, only the first layer may be located, or another layer (second layer) may be present between the first layer and the counter electrode. An example of the second layer is a second separator. When only the first layer is interposed between the counter electrode and the electrode of the electrode structure, the first layer may be a single layer, or multiple first layers may be interposed between the counter electrode and the electrode. <2nd layer> The second layer may be disposed between the first layer and the counter electrode of the electrode structure. The second layer may be in contact with or bonded to the first layer. The second layer may function as a second separator.
[0100] The second separator may be any material that can fulfill the role of a separator. For example, it may be made of a porous film containing polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. In addition, a separator made of a porous film coated with an inorganic compound or an organic compound may also be used. From the viewpoint of safety, it is preferable to use a porous film made of polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off the electric current.
[0101] Also, as the second separator, a membrane containing at least inorganic solid particles, an aggregate or sintered body of inorganic solid particles, a membrane containing inorganic solid particles and a polymer material, for example, a composite membrane of inorganic solid particles and a polymer material, or an ion exchange membrane can be used. The inorganic solid particles can be, for example, particles of a solid electrolyte, and the membrane can be a solid electrolyte membrane. The solid electrolyte membrane can be, for example, a solid electrolyte composite membrane formed by forming solid electrolyte particles into a membrane using a polymer material.
[0102] Examples of the inorganic solid particles include ceramics such as alumina, and particles of a solid material having Li-ion conductivity. Examples of the solid material having Li-ion conductivity include the same as those described for the first particles. The inorganic solid particles may be of a single type or a mixture of multiple types.
[0103] The polymeric material may be a polymer made of a single monomer unit, a copolymer made of multiple monomer units, or a mixture of these. The polymeric material preferably contains a monomer unit made of a hydrocarbon having a functional group containing one or more selected from the group consisting of oxygen (O), sulfur (S), nitrogen (N), and fluorine (F). As the polymeric material, a single type may be used, or multiple types may be mixed and used.
[0104] The second separator may contain a plasticizer and an electrolyte salt in addition to the inorganic solid particles and the polymer material. For example, when the second separator contains an electrolyte salt, the ionic conductivity of the second separator can be further increased. <Aqueous electrolyte> The solvent of the aqueous electrolyte is a solvent containing water, and may be composed of water alone or water and a solvent other than water. Examples of the solvent other than water include water-soluble organic solvents. Examples of the water-soluble organic solvents include γ-butyrolactone, acetonitrile, alcohols, N-methylpyrrolidone (NMP), dimethylacetamide, dimethylsulfoxide, and tetrahydrofuran. The type of solvent contained in the aqueous electrolyte solvent may be one or more types. In the aqueous electrolyte solvent, the content of the solvent other than water is desirably 20 mass % or less.
[0105] The presence of water in aqueous electrolytes can be confirmed by GC-MS (Gas Chromatography-Mass Spectrometry) measurements. In addition, the salt concentration and water content in aqueous electrolytes can be measured, for example, by ICP (Inductively Coupled Plasma) optical emission spectrometry. The molar concentration (mol / L) can be calculated by weighing a specified amount of aqueous electrolyte and calculating the salt concentration contained therein. In addition, the number of moles of solute and solvent can be calculated by measuring the specific gravity of the aqueous electrolyte.
[0106] The alkali metal salt contained in the aqueous electrolyte is, for example, one or more alkali metal salts selected from the group consisting of Li, Na, and K. Each of Li, Na, and K has excellent ionic conductivity, and therefore can increase the ionic conductivity of the aqueous electrolyte. The type of alkali metal salt in the aqueous electrolyte can be one or more types. By dissolving the alkali metal salt in the aqueous solvent, Li + is more preferably obtained as an alkali metal ion. For this reason, it is more preferable to use a lithium salt as the alkali metal salt of the aqueous electrolyte. In the aqueous electrolyte, the concentration of the alkali metal ion in the aqueous solvent is preferably 1 mol / L or more and 12 mol / L or less. By increasing the concentration of the alkali metal ion, the number of free water molecules in the aqueous electrolyte is reduced, and hydrogen generation can be suppressed. In addition, even within the above-mentioned range, the concentration of the alkali metal ion in the aqueous solvent is preferably 4 mol / L or more, and more preferably 5 mol / L or more. In addition, even within the above-mentioned range, the concentration of the alkali metal ion in the aqueous solvent is preferably 10 mol / L or less.
[0107] The alkali metal salt of the aqueous electrolyte is, for example, a lithium salt. Examples of the lithium salt include LiCl, LiBr, LiOH, Li2SO4, LiNO3, Li2C2O4, Li2CO3, Li[(FSO2)2N], Li[(CF3SO2)2N], and LiB[(OCO)2]2. The type of lithium salt used can be one or more. The lithium salt used is preferably a lithium salt containing LiCl, LiOH, Li[(FSO2)2N], or Li[(CF3SO2)2N].
[0108] The anion of the alkali metal salt of the aqueous electrolyte is, for example, Cl. - , Br - , O.H. - , SO4 2- , NO3 - , C2O4 2- , CO3 2- , [(FSO2)2N] - , [(CF3SO2)2N] - and B[(OCO)2] 2- In particular, the anion is selected from the group consisting of Cl - , O.H. - , [(FSO2)2N] - and [(CF3SO2)2N] -It is preferable that the battery contains one or more ions selected from the group consisting of. This makes it possible to increase the concentration of alkali metal ions, thereby suppressing hydrogen generation at the negative electrode. This increases the charge / discharge efficiency (Coulomb efficiency) of the battery, and significantly improves the storage performance and cycle life performance.
[0109] The aqueous electrolyte may be a gel electrolyte containing a complex of the above-mentioned alkali metal salt and polymer material. When the aqueous electrolyte is a gel electrolyte, the diffusion of water molecules from the aqueous electrolyte to the negative electrode can be suppressed, and hydrogen generation at the negative electrode can be significantly suppressed. This can significantly improve the cycle life performance and storage performance of the battery. The complex is, for example, a gel electrolyte obtained by compositing an aqueous solution in which the above-mentioned alkali metal salt is dissolved in an aqueous solvent with a polymer material to form a gel. Examples of the polymer material to be composited with the alkali metal salt include polyacrylates (e.g., lithium polyacrylate, potassium polyacrylate, etc.), polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), and polyethylene oxide (PEO). The type of polymer material can be one or more types. The form of the polymer material can be, for example, granular or fibrous. The content of the polymer material in the electrolyte can be in the range of 0.5% by mass to 10% by mass. <Exterior materials> At least one of the electrode structure, the counter electrode, the separator, and the aqueous electrolyte is housed in the exterior member. As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0110] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0111] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0112] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0113] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content is preferably 100 mass ppm or less. A battery equipped with such a metal container can dramatically improve long-term reliability and heat dissipation in a high-temperature environment.
[0114] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, button, sheet, laminated, or the like. The exterior member can be appropriately selected according to the battery dimensions and the use of the battery. For example, the exterior member may be an exterior member for a small battery mounted on a portable electronic device or the like. In addition, the exterior member may be an exterior member for a large battery mounted on a vehicle such as a two-wheeled or four-wheeled automobile. (Negative terminal) The negative electrode terminal has a potential range of 0.8 V to 3 V with respect to the redox potential of lithium (vs. Li / Li +) and can be formed from a material that is electrically stable and conductive. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector. (Positive terminal) The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.
[0115] The structure of the secondary battery will be described with reference to Fig. 7 to Fig. 8. In Fig. 7 to Fig. 8, the same members as those in Fig. 1 to Fig. 3 are denoted by the same reference numerals, and description thereof will be omitted. In Fig. 7 to Fig. 8, the direction parallel to the thickness direction or lamination direction of the electrode structure is defined as the z-axis direction, the direction parallel to one side of a surface (referred to as a main surface) of the electrode structure that intersects perpendicularly to the z-axis direction is defined as the x-axis direction, and the direction parallel to the other side that intersects perpendicularly to the one side of the main surface is defined as the y-axis direction. When the main surface of the electrode structure is, for example, rectangular, the x-axis direction is parallel to the long side or short side direction of the main surface.
[0116] The secondary battery may include an electrode structure and a counter electrode. A structure including the electrode structure and the counter electrode is called an electrode group. As shown in FIG. 7, the electrode group 2 includes an electrode structure 1 and a counter electrode 511. The counter electrode 511 includes a counter electrode current collector 512 and a counter electrode active material-containing layer 513 laminated on one side of the counter electrode current collector 512. The surface of the counter electrode active material-containing layer 513 along the xy axis is in contact with the surface of the first layer 502 of the electrode structure 1 along the xy axis. The counter electrode active material-containing layer 513 may be bonded to the first layer 502 by compression or with a binder (first binder or second binder). The first layer 502 functions as a separator. According to the electrode group shown in FIG. 7, the first layer 502 is formed by mixing water molecules (H2O) and hydrogen ions (H + 7 prevents hydrogen from penetrating into both the electrode 500 and the counter electrode 511, thereby suppressing the electrolysis of water in the electrode 500 and the counter electrode 511 and suppressing the generation of hydrogen gas. Therefore, the secondary battery having the electrode group and aqueous electrolyte shown in FIG. 7 can increase the electromotive force.
[0117] The electrode group may include a second layer 514 between the counter electrode active material-containing layer 513 and the first layer 502. An example of this is shown in FIG. 8. The second layer 514 may be a second separator. According to the electrode group having the structure shown in FIG. 8, the second layer 514 can reinforce the first layer 502. Therefore, electrical insulation between the electrode 500 and the counter electrode 511 can be maintained for a long period of time.
[0118] Instead of the second layer 514, another first layer may be provided between the first layer 502 and the counter electrode active material-containing layer 513. The other first layer is preferably joined to the counter electrode active material-containing layer 513. Since the ionic liquid is unlikely to leak out of the ionic liquid capsules in the first layer, even if the type of ionic liquid contained in the first layer 502 and the type of ionic liquid contained in the other first layer are different, it is possible to prevent the ionic liquids from mixing with each other. Therefore, the types of ionic liquid for the positive electrode and the ionic liquid for the negative electrode can be different, so that the battery can be charged and discharged within the potential window of the ionic liquid, which has a potential window wider than that of water. Therefore, it is possible to provide a water-based battery having a high electromotive force. FIG. 9 shows cyclic voltammograms of the ionic liquid for the positive electrode and the ionic liquid for the negative electrode. In FIG. 9, the horizontal axis is the potential (V vs. Ag / AgCl) and the vertical axis is the current density (Acm -2 As shown in cyclic voltammogram 515 of the positive electrode ionic liquid and cyclic voltammogram 516 of the negative electrode ionic liquid, the electromotive force of the battery can be improved by using a different type of ionic liquid for the positive electrode from that for the negative electrode.
[0119] 7 and 8, the active material-containing layers 504, 513 are formed on one side of the current collectors 503, 512, respectively, but the active material-containing layers 504, 513 may be formed on both sides of the current collectors 503, 512, respectively. In this case, the first layer 502 may be provided on both sides of the active material-containing layers 504, 513, respectively.
[0120] The secondary battery of the embodiment can be manufactured by a method including, for example, a step of preparing an electrode group including the electrode structure of the embodiment and a counter electrode, and a step of holding an electrolytic solution in the electrode group by, for example, injection or impregnation. A liquid aqueous electrolyte can be used as the electrolytic solution.
[0121] The secondary battery of the embodiment will be described with reference to FIGS.
[0122] As shown in FIG. 10, the electrode group 2 is housed in an exterior member 20 made of a rectangular cylindrical metal container. The electrode group 2 includes a negative electrode 3, a separator 4 made of a first layer, and a positive electrode 5. The electrode group 2 has a structure in which the separator 4 is interposed between the positive electrode 5 and the negative electrode 3 and wound in a spiral shape to form a flat shape. The separator 4 made of the first layer is bonded to one of the electrodes, the negative electrode 3 or the positive electrode 5. Therefore, the electrode group 2 includes the electrode structure of the embodiment. The aqueous electrolyte (not shown) may be held as a counter electrode to the electrode structure in the electrode group 2. As shown in FIG. 10, a strip-shaped negative electrode lead 16 is electrically connected to each of a plurality of points on the end of the negative electrode 3 located on the end face of the electrode group 2. In addition, a strip-shaped positive electrode lead 17 is electrically connected to each of a plurality of points on the end of the positive electrode 5 located on this end face. The plurality of negative electrode leads 16 are connected to the negative electrode terminal 6 in a bundled state as shown in FIG. 11. Although not shown, the positive electrode leads 17 are also similarly bundled together and electrically connected to the positive electrode terminal 7 .
[0123] The metal sealing plate 21 is fixed to an opening of the metal exterior member 20 by welding or the like. The negative electrode terminal 6 and the positive electrode terminal 7 are each drawn out to the outside through an extraction hole provided in the sealing plate 21. A negative electrode gasket 8 and a positive electrode gasket 9 are disposed on the inner circumferential surface of each extraction hole of the sealing plate 21 to prevent a short circuit due to contact with the negative electrode terminal 6 and the positive electrode terminal 7, respectively. By disposing the negative electrode gasket 8 and the positive electrode gasket 9, the airtightness of the secondary battery 100 can be maintained.
[0124] A control valve 22 (safety valve) is disposed on the sealing plate 21. When the internal pressure of the battery cell increases due to gas generated in the exterior member 20, the generated gas can be released to the outside from the control valve 22. The control valve 22 may be of a reset type that operates when the internal pressure exceeds a set value and functions as a sealing plug when the internal pressure decreases. Alternatively, a non-reset type control valve that does not recover its function as a sealing plug once it is activated may be used. In FIG. 10, the control valve 22 is disposed in the center of the sealing plate 21, but the control valve 22 may be located at the end of the sealing plate 21. The control valve 22 may be omitted.
[0125] Further, the sealing plate 21 is provided with a liquid inlet 23. The electrolyte can be injected through this liquid inlet 23. After the electrolyte is injected, the liquid inlet 23 can be closed by a sealing plug 24. The liquid inlet 23 and the sealing plug 24 may be omitted.
[0126] Another example of the secondary battery will be described with reference to Figures 12 and 13. Figures 12 and 13 show an example of a secondary battery 100 that uses an exterior member made of a laminate film as a container.
[0127] The secondary battery 100 shown in Figures 12 and 13 includes an electrode group 2 shown in Figures 12 and 13, an exterior member 20 shown in Figure 12, and an electrolyte (not shown). The electrode group 2 and the electrolyte are housed in the exterior member 20. The electrolyte is held in the electrode group 2.
[0128] The exterior member 20 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0129] The electrode group 2 is a laminated electrode group as shown in Fig. 12. The laminated electrode group 2 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with a separator 4 made of a first layer interposed therebetween. The separator 4 made of the first layer is bonded to one of the negative electrodes 3 and the positive electrodes 5. Therefore, the electrode group 2 includes the electrode structure of the embodiment. An aqueous electrolyte (not shown) may be held in the electrode group 2 as a counter electrode to the electrode structure.
[0130] The electrode group 2 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 2 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0131] The negative electrode current collector 3a of each negative electrode 3 includes a portion 3c on one side of which the negative electrode active material-containing layer 3b is not supported on any surface. This portion 3c serves as a negative electrode current collector tab. As shown in FIG. 13, the portion 3c serving as the negative electrode current collector tab does not overlap with the positive electrode 5. The multiple negative electrode current collector tabs (portions 3c) are electrically connected to a strip-shaped negative electrode terminal 6. The tip of the strip-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 20.
[0132] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is located on the opposite side of the electrode group 2 to the negative electrode current collector tab (portion 3c). The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side to the negative electrode terminal 6, and is drawn out to the outside of the exterior member 20.
[0133] The secondary battery of the embodiment described above includes the electrode structure of the embodiment. According to the secondary battery of the embodiment, it is possible to suppress the electrolysis of water when using an aqueous electrolyte, thereby suppressing the generation of hydrogen gas. Furthermore, according to the secondary battery of the embodiment, it is possible to increase the electromotive force. Furthermore, it is possible to improve the uniformity of the in-plane contact in the secondary battery. Therefore, according to the secondary battery of the embodiment, it is possible to improve the energy density and capacity.
[0134] Third embodiment According to a third embodiment, there is provided a battery pack including a plurality of secondary batteries according to the embodiment.
[0135] In the battery pack according to this embodiment, the individual cells may be electrically connected in series or in parallel, or may be connected in a combination of series and parallel.
[0136] Next, an example of a battery pack will be described with reference to the drawings.
[0137] 14 includes five cells 100a to 100e, four bus bars 201, a positive electrode lead 207, and a negative electrode lead 206. Each of the five cells 100a to 100e is a secondary battery according to the embodiment.
[0138] The bus bar 201 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 201. That is, the battery pack 200 in FIG. 14 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.
[0139] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 207 for external connection. In addition, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 206 for external connection.
[0140] The battery pack according to the embodiment includes the battery according to the embodiment. Therefore, the battery pack can suppress the electrolysis of water when using an aqueous electrolyte, thereby suppressing the generation of hydrogen gas. Furthermore, the battery pack according to the embodiment can increase the electromotive force. Furthermore, the uniformity of the in-plane contact within the battery can be improved. Therefore, the battery pack according to the embodiment can improve the energy density and capacity.
[0141] [Fourth embodiment] According to a fourth embodiment, a battery pack including a secondary battery according to the embodiment is provided. The battery pack may include the battery assembly according to the embodiment. The battery pack may include a single battery instead of the battery assembly according to the embodiment.
[0142] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0143] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0144] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0145] The battery pack 300 shown in Figs. 15 and 16 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0146] 15 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0147] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 207, a negative electrode lead 206, and an adhesive tape .
[0148] At least one of the plurality of unit cells 100 is a secondary battery according to the embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 16. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0149] The adhesive tape 36 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 36. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0150] One end of the positive electrode lead 207 is connected to the battery pack 200. One end of the positive electrode lead 207 is electrically connected to the positive electrode of one or more of the cells 100. One end of the negative electrode lead 206 is connected to the battery pack 200. One end of the negative electrode lead 206 is electrically connected to the negative electrode of one or more of the cells 100.
[0151] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0152] The other end 207a of the positive electrode lead 207 is electrically connected to the positive electrode connector 342. The other end 206a of the negative electrode lead 206 is electrically connected to the negative electrode connector 343.
[0153] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0154] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0155] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0156] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0157] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0158] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0159] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0160] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0161] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 207 and the negative electrode lead 206 may be used as the positive and negative terminals of the external terminals for current supply, respectively.
[0162] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0163] The battery pack according to the fourth embodiment includes the battery according to the embodiment or the battery pack according to the embodiment. Therefore, the battery pack can suppress the electrolysis of water when using an aqueous electrolyte, thereby suppressing the generation of hydrogen gas. Furthermore, the battery pack according to the embodiment can increase the electromotive force. Furthermore, the uniformity of the in-plane contact within the battery can be improved. Therefore, the battery pack according to the embodiment can improve the energy density and capacity.
[0164] [Fifth embodiment] According to a fifth embodiment, a vehicle including a battery pack according to an embodiment is provided.
[0165] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0166] Examples of vehicles according to the embodiment include two-wheeled to four-wheeled hybrid electric vehicles, two-wheeled to four-wheeled electric vehicles, power-assisted bicycles, and rail vehicles.
[0167] The mounting position of the battery pack in the vehicle according to the embodiment is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0168] The vehicle according to the embodiment may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected by a combination of series and parallel connections.
[0169] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0170] A vehicle 400 shown in Fig. 17 includes a vehicle body 40 and a battery pack 300 according to an embodiment. In the example shown in Fig. 17, the vehicle 400 is a four-wheeled automobile.
[0171] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0172] 17 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0173] The vehicle according to the fifth embodiment is equipped with the battery pack according to the embodiment, and therefore the vehicle can exhibit high performance and is highly reliable.
[0174] [Sixth embodiment] According to a sixth embodiment, there is provided a stationary power source including a battery pack according to an embodiment.
[0175] Such a stationary power source may be equipped with a battery pack according to an embodiment or a battery according to an embodiment instead of the battery pack according to an embodiment. Such a stationary power source can exhibit a long life.
[0176] FIG. 18 is a diagram showing an application example to stationary power sources 112 and 123 as an example of use of the battery packs 300A and 300B according to the embodiment. In the example shown in FIG. 18, a system 110 in which the stationary power sources 112 and 123 are used is shown. The system 110 includes a power plant 111, a stationary power source 112, a consumer-side power system 113, and an energy management system (EMS) 115. A power grid 116 and a communication network 117 are also formed in the system 110, and the power plant 111, the stationary power source 112, the consumer-side power system 113, and the EMS 115 are connected via the power grid 116 and the communication network 117. The EMS 115 utilizes the power grid 116 and the communication network 117 to perform control to stabilize the entire system 110.
[0177] The power plant 111 generates a large amount of power using fuel sources such as thermal power and atomic power. Power is supplied from the power plant 111 through a power grid 116 or the like. A battery pack 300A is mounted on the stationary power source 112. The battery pack 300A can store the power supplied from the power plant 111. The stationary power source 112 can supply the power stored in the battery pack 300A through the power grid 116 or the like. The system 110 is provided with a power conversion device 118. The power conversion device 118 includes a converter, an inverter, a transformer, and the like. Thus, the power conversion device 118 can perform conversion between direct current and alternating current, conversion between alternating currents having different frequencies, and voltage transformation (boosting and bucking), and the like. Thus, the power conversion device 118 can convert the power from the power plant 111 into power that can be stored in the battery pack 300A.
[0178] The consumer-side power system 113 includes a power system for a factory, a power system for a building, a power system for a home, etc. The consumer-side power system 113 includes a consumer-side EMS 121, a power conversion device 122, and a stationary power source 123. The stationary power source 123 is equipped with a battery pack 300B. The consumer-side EMS 121 performs control to stabilize the consumer-side power system 113.
[0179] The consumer-side power system 113 is supplied with power from the power plant 111 and power from the battery pack 300A through the power grid 116. The battery pack 300B can store the power supplied to the consumer-side power system 113. Similarly to the power conversion device 118, the power conversion device 122 includes a converter, an inverter, a transformer, and the like. Therefore, the power conversion device 122 can perform conversion between DC and AC, conversion between ACs with different frequencies, and voltage transformation (boost and step-down), etc. Therefore, the power conversion device 122 can convert the power supplied to the consumer-side power system 113 into power that can be stored in the battery pack 300B.
[0180] The power stored in the battery pack 300B can be used, for example, to charge a vehicle such as an electric car. The system 110 may also be provided with a natural energy source. In this case, the natural energy source generates power using natural energy such as wind power and solar power. Power is supplied from the natural energy source in addition to the power plant 111 through the power grid 116. EXAMPLES
[0181] The above embodiment will be specifically described below using examples, but the present invention is not limited to the following examples as long as they do not deviate from the gist of the present invention.
[0182] Example 1 A secondary battery was fabricated according to the following procedure.
[0183] <Preparation of positive electrode> The positive electrode active material is LiNi with an average primary particle size of 2 μm. 0.5 Co 0.2 Mn 0.3A slurry for forming an active material-containing layer was prepared by blending 90% by mass of O2 oxide, 5% by mass of graphite powder as a conductive agent, and 5% by mass of polyvinylidene fluoride (PVdF) as a positive electrode binder in an N-methyl-2-pyrrolidone (NMP) solvent. The blending amounts are the masses relative to the mass of the positive electrode active material-containing layer. The prepared slurry was applied to both sides of an aluminum alloy foil (purity 99.3%) with a thickness of 15 μm. The slurry coating was dried to obtain a laminate. The laminate was pressed to prepare a positive electrode.
[0184] <Preparation of negative electrode> The active material has an average particle size of 0.6 μm and a specific surface area of 10 m 2 / g Li4Ti5O 12 Particles were prepared. The active material particles, graphite powder with an average particle diameter of 6 μm as a conductive agent, and PVdF as a negative electrode binder were mixed in a mass ratio of 95:3:2 and dispersed in an NMP solvent. The dispersion was stirred to prepare a slurry. The obtained slurry was applied to both sides of an aluminum alloy foil (purity 99.3%) with a thickness of 15 μm, the coating was dried, and a negative electrode was produced by passing through a hot pressing process.
[0185] <Preparation of the first layer containing ionic liquid capsules> Preparation of LATP-IL capsules The first particle is LATP (Li 1.5 Al 0.5 Ti 1.5 (PO4)3) particles were used. First, the aqueous phase was prepared by dissolving a sodium carbonate solution (1M, 0.010mL) in an LATP solution (1gL -1 The ionic liquid phase was then prepared by mixing [bmim][PF6] (0.2 mL) with hexamethylene diisocyanate (0.042 mL). The aqueous phase (1 mL) and the ionic liquid phase were mixed in a vial, and the two phases were emulsified by alternately stirring with a magnetic stirrer (10 seconds) and ultrasonic treatment (10 seconds) three times in a cycle to prepare an emulsion solution. Then, an aqueous hexamethylenediamine solution (0.14 M, 0.25 mL) was dropped into the emulsion solution, and the vial was gently swirled by hand. The mixture was left for 72 hours without stirring, and then ammonium hydroxide (1 M, 7 mL) was added to remove unreacted isocyanate functional groups. The LATP-IL capsules obtained by the above method were collected by gravity filtration and further washed with pure water until the pH was neutral. The LATP-IL capsules were then dried at 60 °C for 3 hours to obtain LATP-IL capsules, which are ionic liquid capsules.
[0186] The obtained ionic liquid capsules had an average particle size of 100 μm, a wall thickness of 10 μm, and an average particle size of the first particles of 2 μm.
[0187] 95% by mass of the ionic liquid capsules and 5% by mass of CMC as a first binder were mixed in the presence of an aqueous solvent to prepare a slurry. The obtained slurry was applied onto the negative electrode active material layer and left to dry overnight at 80°C to bond the first layer onto the negative electrode active material layer, thereby obtaining an electrode structure.
[0188] <Preparation of aqueous electrolyte> An aqueous electrolyte consisting of a 12 mol / L LiCl solution was prepared.
[0189] <Preparation of secondary battery> The negative electrode, the positive electrode, and the first layer were stacked so that the active material-containing layer of the negative electrode and the active material-containing layer of the positive electrode faced each other with the first layer in between to form an electrode group, and the resulting electrode group was then housed in an exterior member. A container made of a 0.1 mm-thick laminate film having a three-layer structure of a nylon layer / aluminum layer / polyethylene layer was prepared as the exterior member.
[0190] Next, a liquid aqueous electrolyte was poured into the exterior member. After the electrolyte was poured, the exterior member was sealed. Through the above process, a secondary battery with a design capacity of 3 Ah was produced.
[0191] Example 2 A secondary battery was produced in the same manner as in Example 1, except that the first layer was produced by the method described below.
[0192] As an emulsifier, 1-tetradecyl-3-methylimidazolium ([C 14 mim]Br) and the nonionic surfactant octylphenol ethoxylate (molecular formula: C 14 H 22 O(C2H4O) n ) mixed surfactant (mixing ratio 2:1) was used. The first particle was LATP (Li 1.5 Al 0.5 Ti 1.5 (PO4)3) particles were used. [Bmim]PF6 was used as the ionic liquid (IL). The mixture was added to an aqueous solution containing the above-mentioned mixed surfactant and ionic liquid ([Bmim]PF6). The water content of the above-mentioned mixture was 60 wt%, and the ratio of the amount of the mixed surfactant to the ionic liquid was 1:10. The aqueous phase contained a mixture (1:1) of urethane and diol (20 to 50 mol % of the aqueous solution) and the first fine particles. The above mixture was stirred to obtain an IL / W emulsion.
[0193] Next, n-hexane was used as the oil phase O. 0.1M sorbitan monooleate was dispersed in the O phase as an emulsifier. The IL / W emulsion was poured into this, and the rotation speed was slowed down from the previous step to perform stirring, thereby obtaining the IL / W / O double emulsion shown in FIG. 19. Furthermore, the IL / W / O double emulsion 510 was used as a mold, and photopolymerization of urethane was caused by irradiating it with gamma rays of 3 to 50 Mrad, thereby producing an ionic liquid capsule 501 having a wall membrane 505 in which first particles 506 were dispersed in polyurethane. The ionic liquid capsule 501 was separated from the oil phase O, and the separated ionic liquid capsule 501 was dried. The stirring force can be controlled by controlling the rotation speed of the stirring device or homogenizer. In addition, the emulsification using a pressure homogenizer can also have the same effect by adjusting the pressure.
[0194] The obtained ionic liquid capsules had an average particle size of 200 μm, a wall thickness of 20 μm, and an average particle size of the first particles of 10 μm.
[0195] An electrode structure was produced in the same manner as in Example 1 using the obtained ionic liquid capsules.
[0196] Example 3 A secondary battery was produced in the same manner as in Example 1, except that the first layer was produced by the method described below.
[0197] In Example 3, an IL / W / O double emulsion was prepared by the same method as in Example 2, and ionic liquid capsules were prepared using the IL / W / O double emulsion as a template. In the case of Example 3, when preparing IL / W, the aqueous phase (W) as the continuous phase was a solution in which an appropriate amount of ethylene glycol and terephthalic acid were dissolved in an alkaline aqueous solution. A nonionic surfactant, Polyoxyethylene-23-lauryl ether, was used as an emulsifier. In addition, MEMPTFS was used as the ionic liquid as the dispersed phase. Alternatively, the continuous phase (O) of the IL / W / O double emulsion was the ionic liquid [Bmim]PF6. The surfactant dispersed in the continuous phase (O) was also Polyoxyethylene-23-lauryl ether. The above IL / W / O double emulsion was heated to cause condensation polymerization, producing ionic liquid capsules with walls made of polyethylene terephthalate. The first particles were dispersed in the walls. The ionic liquid capsules were separated from the oil phase, and the separated ionic liquid capsules were dried under reduced pressure.
[0198] The obtained ionic liquid capsules had an average particle size of 100 μm, a wall thickness of 10 μm, and an average particle size of the first particles of 7 μm.
[0199] An electrode structure was produced in the same manner as in Example 1 using the obtained ionic liquid capsules.
[0200] The reaction formula for synthesizing polyethylene terephthalate from ethylene glycol and terephthalic acid is shown in Figure 20.
[0201] Example 4 A secondary battery was produced in the same manner as in Example 1, except that the first layer was produced by the method described below. As an emulsifier, the anionic surfactant lithium dodecyl sulfate (abbreviation: LDS) (molecular formula: CH3(CH2) 11 The first particles were LATP (AlO3Li) with an average particle size of 2 to 3 μm. 0.3 Li 1.3 Ti 1.7(PO4)3) particles were used. MEMPTFSI was used as the ionic liquid (IL). The above anionic surfactant and ionic liquid were added to an aqueous solution containing urea, H2SO4 (0.45M) and the first fine particles, and the mixture was stirred to obtain an IL / W emulsion.
[0202] Next, the IL / W emulsion was dispersed in an oil phase (MEMPTFSI or soybean oil) containing LDS and stirred to obtain an IL / W / O double emulsion. After that, a mixture of formaldehyde and ethanol was added to the IL / W / O double emulsion and stirred. The formaldehyde dissolved in the water phase (W) and underwent condensation polymerization with the urea in the water phase (W) to produce ionic liquid capsules with a urea resin wall membrane. The reaction scheme is shown in Figure 21. The first particles were dispersed in the wall membrane. The ionic liquid capsules were separated from the oil phase and dried after separation.
[0203] The obtained ionic liquid capsules had an average particle size of 100 μm, a wall thickness of 10 μm, and an average particle size of the first particles of 2 to 3 μm.
[0204] An electrode structure was produced in the same manner as in Example 1 using the obtained ionic liquid capsules.
[0205] Example 5 A secondary battery was produced in the same manner as in Example 1, except that the first layer was produced by the method described below.
[0206] An IL / W emulsion was prepared by the same method as in Example 4. EMIM TFSI was used as the ionic liquid (IL). Next, the IL / W emulsion was dispersed in an oil phase (MEMPTFSI or soybean oil) containing LDS, and an IL / W / O double emulsion was obtained by stirring. A mixture of tetraethoxysilane (TEOS), acetic acid, and ethyl acetate was then added to the IL / W / O double emulsion, and the hydrolysis reaction and condensation polymerization reaction of TEOS shown in Figure 22 occurred in the W phase while stirring, producing ionic liquid capsules with silica wall membranes. The first particles were dispersed in the wall membrane. The ionic liquid capsules were separated from the oil phase, and the separated ionic liquid capsules were dried at 65°C for 24 hours to obtain ionic capsules with dry gel wall membranes. The obtained ionic capsules were further sintered at around 400°C to obtain ionic liquid capsules with silica wall membranes.
[0207] The obtained ionic liquid capsules had an average particle size of 100 μm, a wall thickness of 10 μm, and the first particle LATP (Li 1.5 Al 0.5 Ti 1.5 The average particle size of (PO4)3) was 5 μm.
[0208] An electrode structure was produced in the same manner as in Example 1 using the obtained ionic liquid capsules.
[0209] An electrode structure was produced in the same manner as in Example 1 using the obtained ionic liquid capsules.
[0210] Example 6 A secondary battery was produced in the same manner as in Example 1, except that the first layer was produced by the method described below.
[0211] In Example 6, an IL / W emulsion was prepared by the same method as in Example 4. The difference from Example 4 was that a mixed surfactant of sorbitan monooleate and polyoxyethylene sorbitan monooleate was used as the emulsifier, and a sodium silicate solution (4M) was used as the continuous phase (W). Next, the IL / W emulsion was dispersed in an oil phase (soybean oil) containing a mixed surfactant of sorbitan monooleate and polyoxyethylene sorbitan monooleate, and an IL / W / O double emulsion was obtained by stirring. After that, ammonium chloride (NH4Cl) was added as a precipitating agent to the IL / W / O double emulsion, and ionic liquid capsules with a silica gel wall membrane were produced by the interfacial reaction method while stirring. The first particles were dispersed in the wall membrane. The ionic liquid capsules were separated from the oil phase, and the separated ionic liquid capsules were dried at 65°C for 24 hours to obtain ionic capsules with a silica wall membrane.
[0212] The obtained ionic liquid capsules had an average particle size of 200 μm, a wall thickness of 10 μm, and an average particle size of the first particles of 5 μm.
[0213] An electrode structure was produced in the same manner as in Example 1 using the obtained ionic liquid capsules.
[0214] Example 7 A secondary battery was produced in the same manner as in Example 1, except that the first layer was produced by the method described below.
[0215] As a specific preparation method, for example, Gly-PCDA and PC-DIYNE were used as photopolymerizable emulsifiers. Reverse vesicles were prepared using a one-step or two-step emulsification method. Next, the reverse vesicles were irradiated with ultraviolet light (UV light) with a wavelength of 254 nm to cause photopolymerization of the emulsifier, thereby producing microcapsules from the reverse vesicles that encapsulate ionic liquid and have solid particles dispersed in the wall membrane.
[0216] An electrode structure was produced in the same manner as in Example 1 using the obtained ionic liquid capsules.
[0217] Comparative Example 1 A secondary battery was manufactured in the same manner as in Example 1, except that a separator made of a polyethylene porous film was prepared instead of the first layer containing the ionic liquid capsule. Specifically, the negative electrode, the positive electrode, and the separator were stacked so that the active material-containing layer of the negative electrode and the active material-containing layer of the positive electrode faced each other across the separator to form an electrode group, and then the obtained electrode group was housed in an exterior member. Next, a liquid aqueous electrolyte was poured into the exterior member. After the electrolyte was poured, the exterior member was sealed. Through the above process, a secondary battery with a design capacity of 3 Ah was manufactured.
[0218] The charge / discharge curve of the obtained secondary battery at 25°C was measured, and the results are shown in Figure 23. In Figure 23, the horizontal axis is charge / discharge capacity (mAh / g), and the vertical axis is voltage (V). The charge / discharge conditions are described below. After constant current charging at 1C up to 2.7V, constant voltage charging at 2.7V was performed. Charging was performed until the capacity reached 175mAh / g. Next, discharging was performed at 25°C at 1C until the voltage reached 2.2V. Figure 23 shows the results of Example 1 and Comparative Example 1.
[0219] As is clear from FIG. 23, the charge voltage of the secondary battery of Example 1 was 2.5V or more, which was higher than the charge voltage of the secondary battery of Comparative Example 1. The discharge capacity of the secondary battery of Example 1 was also higher than the discharge capacity of the secondary battery of Comparative Example 1. Although not shown in detail in FIG. 23, both the charge voltage and the discharge capacity of Examples 2-7 were also superior to those of Comparative Example 1. As shown by the above results, the secondary batteries of Examples 1-7 can obtain a high electromotive force, and can realize a higher energy density and a higher capacity.
[0220] According to at least one of these embodiments or examples, the electrode structure includes a first layer in contact with the electrode. The first layer includes a capsule having a wall membrane containing first particles, and an ionic liquid contained in the capsule. The structure consisting of the wall membrane, the first particles, and the ionic liquid is a water molecule (HO) and a hydrogen ion (H +Since the electrode structure prevents the intrusion of hydrogen gas into the electrode, the electrolysis of water on the electrode is suppressed, thereby suppressing the generation of hydrogen gas. Therefore, by using the electrode structure in a secondary battery having a water-based electrolyte, it is possible to increase the electromotive force of the secondary battery.
[0221] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims.
[0222] The following describes the embodiments of the invention. <1> An electrode structure including an electrode and a layer in contact with the electrode, The layer includes a capsule having a wall containing a first particle, and an ionic liquid contained within the capsule. <2> The first particles are permeable to alkali metal ions; <1> The electrode structure according to claim 1. <3> The ionic liquid is impermeable to at least one of water and hydrogen ions. <1> or <2> The electrode structure according to claim 1. <4> The ionic liquid is in a gel state. <1> from <3> 13. The electrode structure according to claim 12 . <5> The wall membrane of the capsule includes at least one selected from the group consisting of an amphiphilic molecular membrane, a polymer membrane, a carbon layer membrane, an organic material membrane, an inorganic material membrane, and a membrane containing an organic material and an inorganic material; <1> from <4> 13. The electrode structure according to claim 12 . <6> The amphiphilic molecule membrane comprises cross-linked amphiphilic molecules. <5> The electrode structure according to claim 1. <7> The layer further comprises a plasticizer consisting of an ionic liquid. <1> from <6> 13. The electrode structure according to claim 12 . <8> The layer further comprises second particles. <1> from <7> 13. The electrode structure according to claim 12 . <9> The electrode is at least one of a positive electrode or a negative electrode. <1> from <8> 13. The electrode structure according to claim 12 . <10> the electrode includes an active material-containing layer, and at least a part of the boundary between the layer and the active material-containing layer is configured with a region including a part of the active material-containing layer and the capsule; <1> from <9> 13. The electrode structure according to claim 12 . <11> <1> from <10> The electrode structure according to any one of claims 1 to 5, Aqueous electrolytes and A secondary battery comprising: <12> <11> A battery pack comprising the secondary battery according to claim 1. <13> Further including an external terminal for current supply and a protection circuit. <12> The battery pack according to claim 1 . <14> The battery includes a plurality of the secondary batteries, the secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel. <12> or <13> The battery pack according to claim 1 . <15> <12> from <14> A vehicle equipped with the battery pack according to any one of claims 1 to 5. <16> A mechanism for converting the kinetic energy of the vehicle into regenerative energy. <15> A vehicle as described in. <17> <12> from <14> A stationary power source comprising the battery pack according to any one of claims 1 to 5. <18> a step of producing a capsule having a wall membrane containing the first particles and containing the ionic liquid therein by causing a polymerization reaction in an emulsion containing the first particles, the ionic liquid, and a wall membrane raw material; forming a layer including the capsules in an active material-containing layer; A method for manufacturing an electrode structure comprising the steps of: <19> The emulsion further comprises an aqueous phase, the ionic liquid phase being dispersed in the aqueous phase, and the first particles being present in the ionic liquid phase. <18> A method for producing the electrode structure according to claim 1. <20> The step of forming a layer including the capsules in the active material-containing layer includes applying a slurry including the capsules and a binder to the active material-containing layer. <18> or <19> A method for producing the electrode structure according to claim 1. <21> The polymerization reaction is at least one reaction selected from the group consisting of condensation polymerization, radical polymerization, in-situ polymerization, photopolymerization, interfacial precipitation, interfacial polymerization, interfacial reaction, and hydrolysis-condensation polymerization. <18> from <20> 13. A method for producing the electrode structure according to claim 12. <22> <1> from <10> preparing an electrode group including the electrode structure according to any one of the above and a counter electrode; a step of retaining an electrolyte in the electrode group; A method for manufacturing a secondary battery comprising the steps of: [Explanation of symbols]
[0223] 1...electrode structure, 2...electrode group, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material-containing layer (negative electrode active material-containing layer), 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer (positive electrode active material-containing layer), 6...negative electrode terminal, 7...positive electrode terminal, 8...negative electrode gasket, 9...positive electrode gasket, 16...negative electrode lead, 17...positive electrode lead, 20...exterior member, 21...sealing plate, 22...control valve, 23...filling port, 24...sealing plug, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 36...adhesive tape, 40...vehicle body, 100...secondary battery, 110...system, 111...power plant, 112...stationary power source, 113...consumer-side power system, 115...energy management system, 116...power grid, 117...communication network, 118...power conversion device, 121...consumer-side EMS, 122...power conversion device, 123...stationary power source, 200...battery pack, 201...bus bar, 206...negative electrode lead, 207...positive electrode lead, 300...power battery pack, 300A... battery pack, 300B... battery pack, 310... housing, 320... opening, 332... output positive terminal, 333... output negative terminal, 342... positive connector, 342a... wiring, 343... negative connector, 343a... wiring, 345... thermistor, 346... protection circuit, 348a... positive wiring, 348b... negative wiring, 350... external terminal for energization, 352... positive terminal, 353... negative terminal, 400... vehicle, 500... electrode, 501... ionic liquid Capsule, 502...first layer, 503...current collector, 504...active material-containing layer, 505...wall film, 506...first particle, 507...Pickering emulsion, 508...emulsifier, 509...single emulsion, 510...double emulsion, 511...counter electrode, 512...counter electrode current collector, 513...counter electrode active material-containing layer, 514...second layer, 515...cyclic voltammogram of ionic liquid for positive electrode, 516...cyclic voltammogram of ionic liquid for negative electrode, 517...urethane.
Claims
1. An electrode structure including an electrode and a layer in contact with the electrode, The layer includes a capsule having a wall containing a first particle, and an ionic liquid contained within the capsule.
2. 2. The electrode structure of claim 1, wherein said first particles are permeable to alkali metal ions.
3. The electrode structure according to claim 1 , wherein the ionic liquid is impermeable to at least one of water and hydrogen ions.
4. 2. The electrode structure according to claim 1, wherein the wall membrane of the capsule includes at least one selected from the group consisting of an amphiphilic molecular membrane, a polymer membrane, a carbonaceous layer membrane, an organic material membrane, an inorganic material membrane, and a membrane containing an organic material and an inorganic material.
5. The electrode structure according to claim 1 , wherein the electrode is at least one of a positive electrode or a negative electrode.
6. 2. The electrode structure according to claim 1, wherein the electrode includes an active material-containing layer, and at least a portion of a boundary between the layer and the active material-containing layer is constituted by a region including a portion of the active material-containing layer and the capsule.
7. The electrode structure according to any one of claims 1 to 6, Aqueous electrolytes and A secondary battery comprising:
8. A battery pack comprising the secondary battery according to claim 7.
9. 9. The battery pack according to claim 8, further comprising an external terminal for current flow and a protection circuit.
10. 10. The battery pack according to claim 9, comprising a plurality of the secondary batteries, the secondary batteries being electrically connected in series, in parallel, or in a combination of series and parallel.
11. A vehicle comprising the battery pack according to claim 8.
12. The vehicle of claim 11 including a mechanism for converting kinetic energy of the vehicle into regenerative energy.
13. A stationary power source comprising the battery pack according to claim 8.
14. a step of producing a capsule having a wall membrane containing the first particles and containing the ionic liquid therein by causing a polymerization reaction in an emulsion containing first particles, an ionic liquid, and a wall membrane raw material; forming a layer including the capsules in an active material-containing layer; A method for manufacturing an electrode structure comprising the steps of:
15. A step of preparing an electrode group including the electrode structure according to any one of claims 1 to 6 and a counter electrode; a step of retaining an electrolyte in the electrode group; A method for manufacturing a secondary battery comprising the steps of:
Citation Information
Patent Citations
Electrolyte for lithium ion battery and preparation method thereof
CN115566270A
Ion gel with coating film and method for producing the same
JP2011126975A
Cell separator, ion conductor and battery and manufacturing method thereof
JP2012124125A
Ionic liquid involving granule and manufacturing method thereof
JP2012200632A
Ionic liquid involving granule with film and manufacturing method thereof
JP2012200633A
Cited By
Pore-forming agent for lithium ion battery as well as preparation method and application of pore-forming agent
CN122000357A
Pore-forming agent for lithium ion battery and preparation method and application thereof
CN122000357B