Laminated film and film laminate
The laminated film with a metal and resin layer structure enhances brightness by optimizing light reflection and transmission, addressing reflectance loss in reflective films.
Patent Information
- Application Number
- JP2023045873
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing reflective films experience a decrease in reflectance due to light passing through multiple layers, which is undesirable for high-luminance applications.
A laminated film structure with a metal layer on one side and a resin layer on the other, utilizing a specific resin composition and structure to enhance brightness by optimizing light reflection and transmission.
The laminated film effectively suppresses reflectance loss, achieving high brightness and luminance suitable for reflective sheets and displays.
Smart Images

Figure 2024135269000002 
Figure 2024135269000003 
Figure 2024135269000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate film and a film laminate. [Background technology]
[0002] Laminated films, which have a resin layer on at least one side of a base film, are used in various fields such as industrial materials, optical materials, electronic component materials, battery packaging materials, etc. Polyethylene terephthalate (PET) films, which are representative polyester films, and biaxially oriented PET films in particular, are widely used as the base film for laminated films because of their excellent transparency, mechanical strength, heat resistance, flexibility, etc.
[0003] Conventionally, there has been known a reflective material having a structure in which a reflective film having a metal layer made of an aluminum thin film layer, a silver thin film layer, or the like on a plastic film and a support made of a metal plate such as an aluminum plate or a stainless steel plate are laminated via an adhesive layer. Patent Document 1 discloses a reflective film in which an anchor layer, a silver vapor deposition layer, and a corrosion prevention layer made of a resin are formed on one side of a base material made of a plastic film, and further a resin layer having an ultraviolet absorbing function is provided on the opposite side of the base material made of a plastic film. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-122717 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the reflective film disclosed in Patent Document 1, when the reflective surface is the resin layer side, the light incident from the outside passes through a substrate made of a resin film having a relatively large thickness, usually a thickness of about 25 μm or more, and then passes through the anchor layer and is reflected by the silver vapor deposition layer, which is the reflective layer. After that, the reflected light passes through the anchor layer and the substrate made of a resin film once more in order, so the reflectance of the reflected light tends to be lower than when the corrosion prevention layer side is the reflective surface. In recent years, there has been a demand for a higher brightness type of reflective member for displays, and there has been a demand for further improvement in the reflective characteristics.
[0006] Therefore, in order to solve the above problems, an objective of the present invention is to provide a laminated film that can suppress the decrease in reflectance and achieve high brightness, even in cases where the film structure is used in a way that tends to result in a decrease in reflectance. [Means for solving the problem]
[0007] As a result of intensive research, the inventors have discovered that the above-mentioned problems can be solved by using a laminated film in which a resin layer is formed by applying a resin composition of a specific composition to one side of a base film, and have completed the present invention described below. That is, the present invention provides the following [1] to
[19] . [1] A substrate film with a metal layer on one side and a resin layer on the other side. The reflectance L of the resin layer surface measured by the SCE method * A laminated film having a (D65) value of 13.0 or more. [2] The laminate film according to the above [1], wherein the base film is a polyester film. [3] The laminate film according to [2] above, wherein the polyester film has a three-layer structure. [4] The laminate film according to the above [3], wherein the polyester layer in contact with the resin layer of the polyester film having at least a three-layer structure is substantially free of particles. [5] The laminate film according to the above [3] or [4], wherein the polyester layer on the side of the polyester film having at least three layers on which the metal layer is to be provided is substantially free of particles. [6] The laminated film according to any one of the above [2] to [4], wherein the polyester film contains titanium element. [7] The laminate film according to any one of the above [1] to [6], wherein the resin layer contains one or more kinds of (A) crosslinking agents selected from the group consisting of melamine, oxazoline, epoxy, and isocyanate. [8] The laminate film according to any one of the above [1] to [7], wherein the resin layer contains one or more kinds of binder resin (B) selected from polyester resins, acrylic resins, and urethane resins. [9] The laminate film according to any one of the above [1] to [8], wherein the resin layer has a thickness of 10 to 200 nm.
[10] The laminate film according to any one of the above [1] to [9], wherein the thickness of the base film is 9 to 75 μm.
[11] The laminate film according to any one of [1] to
[10] , wherein the metal layer is provided by any one of vapor deposition, sputtering, or plating.
[12] The laminate film according to any one of the above [1] to
[11] , wherein the metal layer contains silver or a silver alloy containing silver as a main component.
[13] The laminate film according to any one of the above [1] to
[12] , further comprising an anchor layer between the base film and the metal layer.
[14] The laminate film according to any one of the above [1] to
[13] , further comprising a protective layer on the metal layer.
[15] A film laminate, comprising the laminate film according to any one of [1] to
[14] and another resin film bonded to the metal layer side of the laminate film via an adhesive layer.
[16] The film laminate according to the above
[15] , wherein the other resin film is a white film.
[17] The film laminate according to the above
[15] or
[16] , wherein the thickness of the other resin film is 9 to 75 μm.
[18] The laminate film according to any one of the above [1] to
[14] , which is for use as a reflective sheet.
[19] The film laminate according to any one of the above
[15] to
[17] , which is for use as a reflective sheet. Effect of the Invention
[0008] According to the present invention, it is possible to provide a laminated film capable of suppressing a decrease in reflectance and realizing high brightness. [Brief description of the drawings]
[0009] [Figure 1] 1 is a configuration example of a metal laminate film showing an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing how light is incident and reflected based on the structure of a metal laminated film. [Diagram 3] 1 is a configuration example of a film laminate showing an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Next, an example of an embodiment of the present invention will be described. However, the present invention is not limited to the embodiment described below.
[0011] The laminated film of the present invention has a configuration in which a metal layer is provided on one side of a base film and a resin layer is provided on the other side. The resin layer is formed by applying a resin composition for forming the resin layer, followed by drying and curing. Hereinafter, the present invention will be described with reference to an embodiment of a laminated film having a metal layer on one side and a resin layer formed by curing the resin composition provided on the other side of the base film.
[0012] <Laminated film> The laminated film of the present invention has a structure in which a metal layer is provided on one side of a base film and a resin layer is provided on the other side. Each member will be described in more detail below, but first the members constituting the laminated film will be described in more detail.
[0013] [Base film] The material of the base film constituting the laminated film is not particularly limited as long as it has a film shape. For example, it may be made of paper, resin, metal, etc. Among these, it is preferable to use a resin from the viewpoint of mechanical strength and flexibility.
[0014] Examples of the resin substrate film include resin films formed from polymers such as polyethylene, polypropylene, cycloolefin polymer (COP), polyester, polystyrene, acrylic resin, polycarbonate, polyurethane, triacetyl cellulose (TAC), polyvinyl chloride, polyethersulfone, polyamide, polyimide, polyamideimide, etc. Furthermore, as long as it is possible to form a film, it may be a mixture of these materials (polymer blend) or a composite of the structural units (copolymer).
[0015] Among the above-mentioned films, polyester films are particularly preferred because they have excellent physical properties such as heat resistance, flatness, optical properties, and strength. The polyester films may be single-layered or multi-layered films (i.e., laminated films) having two or more layers with different properties. The polyester film is a film containing polyester as a main resin component. The polyester film may be a non-stretched film (sheet) or a stretched film. Of these, a stretched film stretched in a uniaxial or biaxial direction is preferable. Of these, a biaxially stretched film is more preferable from the viewpoint of balance of mechanical properties and flatness. Therefore, a biaxially stretched polyester film is even more preferable.
[0016] The polyester, which is the main component resin of the polyester film, may be a homopolyester or a copolymer polyester. The main component resin means the resin having the largest mass ratio among the resins constituting the polyester film, and may account for 50 mass% or more, 75 mass% or more, 90 mass% or more, or 100 mass% of the resins constituting the polyester film.
[0017] The homopolyester is preferably one obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid, and terephthalic acid is preferred. Examples of the aliphatic glycol include ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,4-cyclohexanedimethanol, and ethylene glycol is preferred. Representative examples of homopolyester include polyethylene terephthalate (PET) and polybutylene terephthalate (PBT).
[0018] On the other hand, when the polyester is a copolymer polyester, it is preferable that the polyester is a copolymer containing 30 mol % or less of a third component. Examples of the dicarboxylic acid component of the copolymer polyester include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, etc., and examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, etc. It is preferable that the copolymer polyester contains terephthalic acid as the dicarboxylic acid, contains ethylene glycol as the glycol component, and has a third component other than these. Among these, the base material in the present release film is preferably polyethylene terephthalate, which contains 60 mol % or more, and preferably 80 mol % or more, of ethylene terephthalate units.
[0019] Particles can be blended into the base film in the present laminated film mainly for the purpose of imparting easy slippage and preventing scratches in each process. When particles are blended, the type of particles to be blended is not particularly limited as long as they are particles that can impart easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, in the case of polyester film, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester manufacturing process can also be used.
[0020] On the other hand, the shape of the particles to be used is not particularly limited, and any of spherical, blocky, rod-like, flat, etc. may be used. In addition, there is no particular limit to the hardness, specific gravity, color, etc. Two or more kinds of these particles may be used in combination as necessary. The average particle size of the particles used is preferably 5 μm or less, more preferably in the range of 0.1 to 3 μm. By using particles with an average particle size in the above range, an appropriate surface roughness can be imparted to the film, and good slipperiness and smoothness can be ensured. When particles are blended, for example, it is preferable to provide a surface layer and an intermediate layer and to incorporate the particles in the surface layer. In this case, it is more preferable to form a multi-layer structure having a surface layer containing particles, an intermediate layer, and a surface layer containing particles in this order.
[0021] Furthermore, the content of particles in the base film is preferably 5% by mass or less, more preferably in the range of 0.0003 to 3% by mass. By setting the content of particles within the above range, the transparency of the base film is ensured, while the slipperiness of the base film is easily imparted. However, the base film does not have to substantially contain particles. In this specification, "substantially free of particles" means that particles are not intentionally contained, and specifically means that the particle content (particle mass concentration) is 200 ppm or less, more preferably 150 ppm or less, relative to the member or layer (here, the base film). Similar terms shown below have the same meaning. In addition, when the substrate film does not substantially contain particles or the content is small, the substrate film has high transparency, and the film has a good appearance, and the smoothness of the resin layer surface tends to be high. On the other hand, the slipperiness of the laminated film may be insufficient. Therefore, in such a case, the slipperiness may be improved by blending particles in the resin layer, or the slipperiness may be improved by providing a slippery layer having particles as described later.
[0022] The laminated film of the present invention preferably has at least three layers, for example, three polyester layers. As for particles, the polyester layer in contact with the resin layer described in detail later is preferably substantially free of particles. By substantially not containing particles, the straightness of transmitted light is improved, and the effect of improving brightness can be expected. It is also preferred that the polyester layer on the side opposite to the resin layer, on which the metal layer is to be provided, does not substantially contain particles, which is expected to have an effect of improving the brightness of the base film. As described above, it is important to control the particle content in both surface layers of the laminate film from the viewpoints of smoothness and brightness improvement, and it is preferable to adjust the particle content according to the specifications.
[0023] <Polyester polycondensation catalyst> Examples of the polycondensation catalyst used in polycondensing the polyester include antimony compounds, germanium compounds, aluminum compounds, titanium compounds, etc. Among these, at least one of antimony compounds and titanium compounds is preferred, and it is particularly preferred to use a polyester obtained by using a titanium compound. Therefore, the polyester film preferably contains at least one of an antimony compound and a titanium compound, and more preferably contains a titanium compound. By using the titanium compound, when the light traveling through the laminated film is reflected by the metal layer and returns, the color of the light is whitish and bright, which is expected to contribute to further improvement of brightness. In terms of the brightness of light, when an antimony compound is used, the light transmitted through the film tends to be dull and often dark.
[0024] In the case of the present polyester film, it is preferred that at least one layer, and more preferably all layers, contain a titanium compound. The content of titanium element derived from the titanium compound contained in the polyester film is preferably 3 ppm or more and 300 ppm or less, and more preferably 5 ppm or more and 200 ppm or less. Within the above range, it is possible to contribute to further improving the brightness of the film without reducing the production efficiency of the polyester.
[0025] The thickness of the base film is preferably 12 to 75 μm, more preferably 20 to 60 μm. When the thickness of the base film is within the above range, it can be suitably used in various fields such as industrial materials, optical parts, electronic parts, and battery packaging materials.
[0026] (Layer structure of this film) When the present film has a laminated structure having two or more layers, preferred are a three-layer structure of B / A / C consisting of a base layer A, a surface layer B, and a surface layer C, and a B / A / B consisting of a base layer A and a surface layer B. When the present film has a laminated structure having two or more layers, the main component resin constituting each layer is preferably polyester as described above.
[0027] In the three-layer structure of B / A / C and B / A / B, the surface layer B and the surface layer C may contain the minimum amount of particles necessary to ensure handling properties. Preferably, they do not substantially contain particles.
[0028] In the above-mentioned three-layer structures of B / A / C and B / A / B, it is particularly preferable that the surface layer B and the surface layer C each contain particles having a narrow particle size distribution and a substantially uniform average particle size (so-called monodispersity).
[0029] Surface layer B contains particles having an average particle size of, for example, 0.1 to 3 μm, and preferably 0.1 to 0.5 μm. Surface layer C contains particles having an average particle size of, for example, 0.1 to 3 μm, and preferably 0.05 to 0.2 μm, and more preferably 0.05 to 0.1 μm.
[0030] The average particle size of particles can be determined by measuring the diameters of 10 or more particles using a scanning electron microscope (SEM) and taking the average value. In this case, in the case of non-spherical particles, the average value of the longest and shortest diameters is taken as the diameter of each particle.
[0031] The film contains the particles at a mass ratio of, for example, 900 ppm or more, preferably 2000 to 10000 ppm, more preferably 2500 ppm to 9500 ppm, and even more preferably 3000 ppm to 9000 ppm. The mass ratio here refers to the ratio of particles in each surface layer.
[0032] Moreover, it is particularly preferable that the surface layer C contains the particles in a mass ratio of 900 ppm or more and 6000 ppm or less. When the surface layer C contains particles in this range, the handling properties of the film can be improved.
[0033] Moreover, it is particularly preferable that the surface layer B contains the particles in a mass ratio of less than 5000 ppm, and it is most preferable that the surface layer B contains the particles in a mass ratio of 2000 ppm or more and 4000 ppm or less.
[0034] The base layer A preferably functions as the thickest main layer, and in order to reduce costs, it preferably does not substantially contain particles or contains particles at a lower concentration than the surface layer B. In this embodiment, the surface layer B is preferably the surface layer on the metal layer side.
[0035] <Resin layer> The resin layer is formed by curing a resin composition and is provided on the substrate film. The resin layer may be provided on only one side of the substrate film, or on both sides. The resin layer has a function of improving the optical properties of the base film. The resin composition can further improve the total light transmittance while keeping the film haze small by combining a binder resin, a crosslinking agent, and particles. When the resin layer is provided on both sides, it may be possible to further improve the light transmittance while also imparting an effect of improving the adhesion to the metal layer. The thickness of the resin layer is preferably from 0.01 to 2 μm, more preferably from 0.03 to 1.5 μm, and further preferably from 0.03 to 1.0 μm. When the thickness of the resin layer is equal to or greater than the lower limit, it is advantageous in that a uniform resin layer can be easily formed, whereas when the thickness is equal to or less than the upper limit, it is advantageous in that curability can be improved. Note that the thickness of the resin layer is the thickness after drying.
[0036] The resin layer in the laminate film of the present invention preferably contains a crosslinking agent, which improves the strength, heat resistance, etc. of the resin layer. (A) Crosslinking agent As the crosslinking agent, various known crosslinking agents can be used, for example, oxazoline compounds, melamine compounds, epoxy compounds, isocyanate compounds, carbodiimide compounds, silane coupling compounds, etc. The oxazoline compound may be an acrylic polymer having an oxazoline group. Among these, melamine compounds, oxazoline compounds, and epoxy compounds are preferred. These crosslinking agents may be used alone or in combination of two or more. The content of the crosslinking agent in the resin composition is, for example, 5 to 50 mass %, preferably 10 to 40 mass %, based on the solid content.
[0037] The resin layer in the laminate film of the present invention preferably contains a binder resin, which improves the strength, heat resistance, etc. of the resin layer. (B) Binder resin Examples of the binder resin include polyester resin, acrylic resin, urethane resin, polyvinyl resin such as polyvinyl alcohol, polyalkylene glycol, polyalkyleneimine, methyl cellulose, hydroxycellulose, starch, etc. Among these, from the viewpoint of film forming properties, it is preferable to use polyester resin, acrylic resin, and urethane resin, and more preferably polyester resin and acrylic resin. These binder resins may be used alone or in combination of two or more. In the resin composition, the content of the binder resin is, for example, 20 to 90 mass %, preferably 30 to 80 mass %, based on the solid content.
[0038] The resin composition may contain particles for the purpose of improving blocking resistance and slippage. As the particles, those shown in the easy-slip layer described later can be used appropriately. However, it is preferable that the resin composition does not substantially contain particles. By substantially not containing particles, the smoothness of the resin layer surface can be increased. The resin composition may also contain a component for promoting crosslinking, such as a crosslinking catalyst, etc. Furthermore, it is also possible to use in combination an antifoaming agent, a coating property improving agent, a thickener, an organic lubricant, an antistatic agent, an ultraviolet absorber, an antioxidant, a foaming agent, a dye, a pigment, etc.
[0039] Generally, the resin composition is preferably diluted with water, an organic solvent, or a mixture thereof, and the resin layer may be formed by coating the diluted resin composition as a coating liquid on the surface of the substrate film and drying it. The coating may be performed by a conventionally known method. The thickness of the resin layer is usually in the range of 10 to 200 nm, preferably 10 to 150 nm, and more preferably 20 to 100 nm. By satisfying the above range, it becomes easy to take in light from the outside, and the total light transmittance is further improved by combining with the resin layer constituent material.
[0040] <Method of forming resin layer> As described above, the resin layer can be obtained by applying a resin composition to the surface of a substrate film, drying the composition to form a coating layer, and curing the coating layer. Examples of a method for applying the resin composition include air doctor coating, blade coating, rod coating, bar coating, knife coating, squeeze coating, impregnation coating, reverse roll coating, transfer roll coating, gravure coating, kiss roll coating, cast coating, spray coating, curtain coating, calendar coating, and extrusion coating. The drying conditions are not particularly limited, and the drying may be performed at about room temperature or by heating, for example, at about 25 to 120° C., preferably 50 to 100° C., and more preferably 60 to 90° C. The drying time is not particularly limited as long as the solvent can be sufficiently evaporated, and is, for example, about 10 seconds to 30 minutes, and preferably about 15 seconds to 10 minutes.
[0041] <Physical properties of polyester film> (Film Haze) It is preferable that the film haze value is 1.3% or less. By making the film haze value equal to or less than the upper limit, for example, it becomes possible to apply the film to applications requiring visibility. The film haze value is preferably 1.0% or less, more preferably 0.8% or less.
[0042] (Total light transmittance) The total light transmittance is preferably 89% or more, and more preferably 90% or more. By making the total light transmittance equal to or more than the lower limit, the film can be applied to, for example, display applications that require a high level of brightness.
[0043] <Physical properties of laminated film (with metal layer)> (Reflection L of the resin layer surface by the SCE method * (D65) Reflection L by SCE method * (D65) must be 13.0 or more, preferably 15.0 or more, more preferably 17.0 or more, and particularly preferably 19.0 or more. By satisfying the above range, the film is suitable for applications requiring a high level of brightness, such as a reflective sheet for a display. In the present invention, in order to reproduce the state close to that when a person sees an object, a method of measuring using only diffuse light (SCE method) is adopted, excluding specular reflected light. Furthermore, the reflected L when using a D65 light source is * The inventors have found that the value has a good correlation with the luminance, and have completed the present invention.
[0044] Specifically, the measurement is performed by taking in light from outside as shown in Figure 2. When light passes through to the metal layer (arrow A), absorption of the light occurs in the resin layer, base film, and anchor layer, and the amount of light tends to attenuate before it reaches the metal layer. The light then reflects off the surface of the metal layer and travels outward in the opposite direction to the route it took (arrow B in Figure 2). As a result, the amount of light remains attenuated by the time it reaches the surface of the resin layer, so in order to further improve the brightness, it was necessary to somehow increase the amount of light taken in from outside. Therefore, the inventors have found that a resin layer of a specific configuration has a different effect of increasing the amount of light taken in from the outside, acting as a so-called "brightness improving layer", and have completed the present invention. By comparing the examples and the comparative examples, it is found that there is a difference in the total light transmittance depending on whether or not the resin layer is present, and the resin layer allows more light to be taken in and transmitted. As a result, in a film configuration with a metal layer on the back side, even if the amount of light is attenuated to the same extent, more light is reflected back, so it is presumed that the brightness is further improved.
[0045] <Metal layer> The metal layer is preferably provided directly or via an anchor layer on the surface of the substrate film on which the resin layer is not provided. As for the type of metal, it is preferable that the silver alloy contains silver or a silver alloy containing silver as a main component. Here, "containing silver as a main component" means that the silver content in the silver alloy is 50% by mass or more. The silver content in the silver alloy is more preferably 70% by mass or more, and even more preferably 90% by mass or more.
[0046] When forming a silver alloy, the type of other metal is not particularly limited. Conventionally known materials can be used. Specific examples include copper, bismuth, gold, platinum, zinc, tin, titanium, nickel, magnesium, and lead. The ratio of other metals contained in the silver alloy is preferably 0.1 to 10 (unit: atomic %).
[0047] The thickness of the metal layer is usually 40 to 300 nm, preferably 60 to 200 nm, and more preferably 80 to 150 nm. By satisfying the above range, for example, when used for reflection purposes, good reflection characteristics can be obtained.
[0048] The metal layer can be formed by a conventional method such as a "dry coating method" such as vacuum deposition, sputtering, EB deposition, CVD deposition, or ion plating.
[0049] <Protective layer> A protective layer may be provided on the metal layer to protect the surface of the metal layer from scratches or corrosion. The protective layer may be a single layer or a laminated structure of two or more layers, and can be appropriately selected depending on the application or required properties of the laminate film.
[0050] As the composition constituting the protective layer, a conventionally known resin can be used. Examples of the resin include polyester resins, acrylic resins, melamine resins, epoxy resins, polyamide resins, vinyl chloride resins, vinyl chloride-vinyl acetate copolymer resins, etc. These may be used alone or in combination of two or more kinds.
[0051] Furthermore, for the purpose of protecting the metal layer from scratches or corrosion, "another resin film" may be laminated via an adhesive layer in place of or in addition to the protective layer. The "other resin film" may be the same as the resin film used for the base film. Among them, the "other resin film" is preferably a white film from the viewpoint of improving the reflection characteristics. The thickness of the "other resin film" is preferably 9 to 75 μm, more preferably 12 to 50 μm, from the viewpoint of minimizing the thickness in consideration of mounting in a limited space such as a display member.
[0052] The laminated film of the present invention can be used in various fields such as industrial materials, optical parts, electronic parts, and battery packaging materials, and is also suitable for optical applications such as various displays, lenses, mirrors, and window glass. As described above, the laminated film of the present invention maintains a low haze value, so that even if it is used in optical components, the performance of the optical components is not deteriorated. In particular, it is suitable as a reflective sheet among display peripheral members.
[0053] <Explanation of terms, etc.> In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES
[0054] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to the examples described below.
[0055] <Evaluation method> The methods for measuring and evaluating various physical properties and characteristics are as follows.
[0056] (1) Intrinsic viscosity (IV) 1 g of polyester was precisely weighed, dissolved in 100 ml of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and measured at 30°C.
[0057] (2) Average particle size The powder was observed using a scanning electron microscope (HITACHI, "S3400N"). The size of each particle was measured from the obtained image data, and the average value of 10 points was taken as the average particle size.
[0058] (3) Film haze, total light transmittance The film haze of each laminated film was measured using a haze meter HM-150 manufactured by Murakami Color Research Laboratory in accordance with JIS K 7136. The total light transmittance was measured in accordance with JIS K 7361 using the same device as above.
[0059] (4) Reflection L by SCE method * (D65) Using a Konica Minolta spectrophotometer (model: CM25-cG), a laminated film consisting of a metal layer, a base film, and a resin layer was used to measure the reflectance L of the resin layer surface by the SCE method. * (D65) value, a * (D65) value, and b * The L (D65) was also measured for the laminated film (base film / resin layer) before the metal layer was deposited. * Value, a * value, and b * was measured.
[0060] The raw materials of the laminated films in the respective Examples and Comparative Examples are as follows. (Base film) <Polyester (A)> 100 mol% dimethyl terephthalate, 100 mol% ethylene glycol, and 0.07 parts by mass of calcium acetate monohydrate were placed in a reactor, and the mixture was heated to a higher temperature while distilling off methanol to carry out an ester exchange reaction. After the reaction started, the temperature was raised to 230°C in about 4.5 hours, and the ester exchange reaction was essentially completed. Next, 0.04 parts by mass of phosphoric acid and 0.035 parts by mass of antimony trioxide were added, and polymerization was carried out according to a conventional method. The reaction temperature was gradually increased to a final temperature of 280°C, while the pressure was gradually reduced to a final temperature of 0.05 mmHg. After 4 hours, the reaction was terminated, and the mixture was chipped according to a conventional method to obtain polyester (A). The resulting intrinsic viscosity was 0.63. <Polyester (B)> Silica particles having an average particle size of 2 μm were added to the polyester (A) to obtain polyester (B) containing 0.2% by mass of silica particles. The intrinsic viscosity was 0.65.
[0061] [Example 1] A mixed raw material obtained by mixing polyesters (A) and (B) in a ratio of 90% by mass and 10% by mass, respectively, was used as the raw material for the outermost layer (surface layer), and polyester (A) alone was used as the raw material for the middle layer. These were fed into two extruders, melted at 285°C, and then co-extruded onto a cooling roll set at 40°C in a layer structure of two types and three layers (surface layer / middle layer / surface layer = extrusion volume (mass ratio) of 1 / 8 / 1), and cooled and solidified to obtain an unstretched sheet. Next, the film was stretched 3.4 times in the longitudinal direction at a film temperature of 85°C using the difference in roll peripheral speed, and then a coating solution of the resin layer composition described below was applied to one side of this longitudinally stretched film, which was then introduced into a tenter and stretched 4.3 times in the transverse direction at 110°C. After heat treatment at 235°C, the film was relaxed by 2% in the transverse direction to obtain a 23 μm thick polyester film (substrate film) having a resin layer with a thickness (after drying) of 30 nm.
[0062] (Formulation conditions of resin composition) The following compounds were mixed in a ratio of A1:B1=90:10 (mass % of solid content). (B1) Aqueous dispersion of acrylic resin polymerized with the following composition Emulsion polymer of ethyl acrylate / n-butyl acrylate / methyl methacrylate / N-methylolacrylamide / acrylic acid = 65 / 21 / 10 / 2 / 2 (mass%) (emulsifier: anionic surfactant) (A1) Melamine compound: Hexamethoxymethylolmelamine
[0063] (Formation of metal layer) A metal layer was formed on the surface of the polyester film obtained above opposite to the resin layer by depositing silver (purity 99.999%: manufactured by Kojundo Chemical Laboratory) by electron beam (EB) vacuum deposition. The laminated film thus obtained was evaluated by the above-mentioned methods, and the results are shown in Table 1.
[0064] [Example 2] A laminated film was obtained in the same manner as in Example 1, except that the resin layer composition and the resin layer thickness were changed in Example 1. The evaluation results are shown in Table 1. The following compounds were mixed in a ratio of A1:A2=60:40. The thickness of the resin layer after drying and stretching was 100 nm. (A1) Melamine compound: Hexamethoxymethylolmelamine (A2) Oxazoline compound: an acrylic polymer having an oxazoline group and a polyalkylene oxide chain
[0065] [Example 3] A laminated film was obtained in the same manner as in Example 1, except that the resin layer composition and the resin layer thickness were changed in Example 1. The evaluation results are shown in Table 1. The following compositions were mixed in a ratio of B2:B1:A1:A2:A3=40:30:10:10:10. The resin layer thickness after drying and stretching was 100 nm. (B2) Aqueous dispersion of polyester resin copolymerized with the following composition Monomer composition: (acid component) 2,6-naphthalenedicarboxylic acid / 5-sodium sulfoisophthalic acid / (diol component) ethylene glycol / diethylene glycol = 92 / 8 / / 80 / 20 (mol%) (B1) Aqueous dispersion of acrylic resin polymerized with the following composition Emulsion polymer of ethyl acrylate / n-butyl acrylate / methyl methacrylate / N-methylolacrylamide / acrylic acid = 65 / 21 / 10 / 2 / 2 (weight%) (emulsifier: anionic surfactant) (A1) Melamine compound: Hexamethoxymethylolmelamine (A2) Oxazoline compound: an acrylic polymer having an oxazoline group and a polyalkylene oxide chain (A3) Epoxy compound: Polyglycerol polyglycidyl ether
[0066] [Example 4] A laminated film was obtained in the same manner as in Example 1, except that the resin layer composition and the resin layer thickness were changed in Example 1. The evaluation results are shown in Table 1. The following B1:A2 ratio was 90:10, and the resin layer thickness after drying and stretching was 30 nm. (B1) Aqueous dispersion of acrylic resin polymerized with the following composition Emulsion polymer of ethyl acrylate / n-butyl acrylate / methyl methacrylate / N-methylolacrylamide / acrylic acid = 65 / 21 / 10 / 2 / 2 (weight%) (emulsifier: anionic surfactant) (A2) Oxazoline compound: an acrylic polymer having an oxazoline group and a polyalkylene oxide chain
[0067] [Comparative Example 1] A laminated film was obtained in the same manner as in Example 1, except that the resin layer was not provided. The evaluation results are shown in Table 1.
[0068] [Table 1]
[0069] (Consideration) In comparison with Comparative Example 1, Examples 1 to 4 show the reflectance L of the resin layer surface in the SCE method after deposition processing. * The (D65) values were all large and good. There is also a correlation with the total light transmittance of the polyester film before deposition. In general, the reflectance L after deposition is higher for films that capture a large amount of light from the outside. * (D65) values also tended to be large. The total light transmittance of the polyester film before deposition is only 1-3% lower than that of the comparative example, which is a level that is easily overlooked. However, the reflected light (L) measured by the SCE method was used as a substitute for the brightness. * Looking at the (D65) values, it was found that there were large differences between the samples (Examples 1 to 4). By appropriately combining the materials that make up the resin layer and the thickness of the resin layer (after drying), it is possible to achieve a more reflective L than ever before. * We also found that the (D65) value could be increased. [Explanation of symbols]
[0070] 1 Resin layer 2. Base film 3 Anchor Layer 4 metal layer 5 Protective layer 6 Other resin films A Incident light B Reflected light
Claims
1. The substrate film has a metal layer on one side and a resin layer on the other side. The reflectance L of the resin layer surface measured by the SCE method is * A laminated film having a D65 value of 13.0 or more.
2. The laminate film according to claim 1 , wherein the base film is a polyester film.
3. The laminate film according to claim 2 , wherein the polyester film has at least three layers.
4. 4. The laminate film according to claim 3, wherein the polyester layer in contact with the resin layer of the polyester film having at least three layers is substantially free of particles.
5. 4. The laminate film according to claim 3, wherein the polyester layer on the side of the polyester film having at least three layers on which the metal layer is to be formed is substantially free of particles.
6. The laminated film according to claim 2 , wherein the polyester film contains titanium element.
7. The laminate film according to claim 1 , wherein the resin layer contains one or more crosslinking agents (A) selected from the group consisting of melamine, oxazoline, epoxy, and isocyanate.
8. The laminate film according to claim 1 , wherein the resin layer contains one or more kinds of binder resins (B) selected from the group consisting of polyester resins, acrylic resins, and urethane resins.
9. The laminate film according to claim 1, wherein the resin layer has a thickness of 10 to 200 nm.
10. The laminate film according to claim 1, wherein the thickness of the base film is 9 to 75 μm.
11. The laminated film according to claim 1 , wherein the metal layer is provided by any one of vapor deposition, sputtering, and plating.
12. The laminate film according to claim 1 , wherein the metal layer comprises silver or a silver alloy containing silver as a main component.
13. The laminate film according to claim 1 , further comprising an anchor layer between the base film and the metal layer.
14. The laminate film according to claim 1 , further comprising a protective layer on the metal layer.
15. A film laminate, comprising the laminate film according to any one of claims 1 to 14 and another resin film bonded to the metal layer side of the laminate film via an adhesive layer.
16. The film laminate according to claim 15 , wherein the other resin film is a white film.
17. The film laminate according to claim 15, wherein the thickness of the other resin film is 9 to 75 μm.
18. The laminate film according to any one of claims 1 to 14, which is used as a reflective sheet.
19. The film laminate according to claim 15, which is used for a reflective sheet.
Citation Information
Patent Citations
Durable reflection film
JP2002122717A