Method for producing coil

The method of manufacturing winding wire with a thermoplastic polyimide coating addresses recycling and performance issues by ensuring excellent electrical properties and heat resistance, suitable for high voltage and compact motor applications.

JP2024135340APending Publication Date: 2024-10-04MITSUI CHEMICALS INC

Patent Information

Application Number
JP2023045969
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing winding wire technologies face challenges in recycling thermosetting resin components and do not adequately address the issues of partial discharge and heat resistance, which are exacerbated by high voltage applications and compact motor designs.

Method used

A method for manufacturing winding wire using a thermoplastic polyimide coating that directly covers the conductor, involving preparation, pulverization, and extrusion coating of thermoplastic polyimide material to create a film with excellent electrical properties and heat resistance.

Benefits of technology

The method enables the reuse of resin materials, providing a winding wire with a coating that maintains excellent electrical properties and heat resistance, suitable for high voltage and compact motor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135340000018
    Figure 2024135340000018
  • Figure 2024135340000001
    Figure 2024135340000001
  • Figure 2024135340000002
    Figure 2024135340000002
Patent Text Reader

Abstract

To provide a method for producing coils capable of producing coils provided with a resin coating excellent in electric characteristics and heat resistance by recycling a resin.SOLUTION: The disclosed method for producing a coil is a method for producing the coil including a conductor and a thermoplastic polyimide coating directly covering the conductor. The producing method of the present disclosure includes: providing a thermoplastic polyimide material separated from an object containing the thermoplastic polyimide; and extrusion coating a thermoplastic polyimide composition containing the thermoplastic polyimide material directly onto the conductor to produce the thermoplastic polyimide coating.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for manufacturing a winding. [Background technology]

[0002] Windings are widely used in electrical equipment (e.g., electric motors, transformers, etc.). "Windings" refers to wires for winding coils that create a magnetic field. "Wire" refers to conductors with insulating coating or insulation paint.

[0003] Patent Document 1 discloses an insulated electric wire (hereinafter also referred to as "winding wire"). The winding wire disclosed in Patent Document 1 has two or more multilayer insulating layers that cover a conductor. The innermost insulating layer of the multilayer insulating layers is an insulating layer formed of a specific crystalline thermoplastic resin. The outer insulating layers other than the innermost insulating layer include insulating layers formed of a specific crystalline thermoplastic resin. Specifically, polyether ether ketone (hereinafter also referred to as "PEEK"), modified PEEK, or thermoplastic polyimide are disclosed as materials for the innermost insulating layer, and nylon 66, polyphenylene sulfide, PEEK, or modified PEEK are disclosed as materials for the outer insulating layers.

[0004] Patent Document 2 discloses an insulated wire (hereinafter also referred to as a "winding wire"). The winding wire disclosed in Patent Document 2 has a specific thermosetting resin layer on the outer periphery of a conductor, and a specific thermoplastic resin layer on the outer periphery of the thermosetting resin layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2014 / 084063 [Patent Document 2] International Publication No. 2018 / 016498 Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, recycling has been attracting attention for the purpose of reducing the environmental load. For example, in the field of electric vehicles, the conductors of the windings included in electric motors are reused, and there is also an increasing need to recycle resins other than the conductors. However, Patent Document 1 and Patent Document 2 do not disclose anything about recycling the resin components used in the windings. In general, thermosetting resin layers may be difficult to thermally decompose. Therefore, it may be difficult to recycle the resin components of the windings disclosed in Patent Document 2.

[0007] Meanwhile, in recent years, in the field of electric vehicles, various proposals have been made for the purpose of increasing the output and miniaturizing the motor from the viewpoint of improving the power performance and fuel efficiency. As a measure for increasing the output of the motor, the motor is driven at a high voltage. However, when a high voltage is applied to an electrically insulating resin coating (hereinafter also referred to as a "resin coating") of the winding included in the motor, partial discharge may occur on the surface of the resin coating. The occurrence of partial discharge may cause the resin coating to be eroded early. As a result, the resin coating may be generated. That is, the life of the motor may be shortened. In addition, when the motor is miniaturized, the winding may not be able to dissipate heat easily. That is, the resin coating included in the winding may be exposed to a high-temperature environment (e.g., 200°C).

[0008] Therefore, there is a demand for a method for manufacturing a winding that can reuse resin and produce a winding having a resin coating that has excellent electrical properties (i.e., a partial discharge inception voltage of 1000 V or more) and excellent heat resistance (i.e., a glass transition temperature of 200° C. or more).

[0009] In view of the above circumstances, an object of the present disclosure is to provide a manufacturing method for a winding that can reuse resin and manufacture a winding having an insulating coating that has excellent electrical properties and heat resistance. [Means for solving the problem]

[0010] Means for solving the above problems include the following aspects.

[0011] <1> 1. A method for manufacturing a winding comprising a conductor and a coating of thermoplastic polyimide directly covering the conductor, comprising the steps of: providing a thermoplastic polyimide material that is separated from the thermoplastic polyimide-containing object; extrusion coating a thermoplastic polyimide composition comprising the thermoplastic polyimide material directly onto the conductor to produce the coating; A method for manufacturing a winding, comprising: <2> The thermoplastic polyimide contains a structural unit represented by the following formula (1): <1> A method for manufacturing the winding wire according to claim 1. [ka] In the above formula (1), X is a direct bond, -SO2-, -CO-, -C(CH3)2-, -C(CF3)2-, or -S-; R1, R2, R3, and R4 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a halogenated alkyl group, a halogenated alkoxy group, or a halogen atom; and Y is a group selected from the group consisting of four groups represented by the following formula (2). [ka] <3> The thermoplastic polyimide contains a structural unit represented by the following formula (1): <1> or <2> A method for manufacturing the winding wire according to claim 1. [ka] <4> and pulverizing the thermoplastic polyimide material to produce a thermoplastic polyimide pulverized material. The thermoplastic polyimide composition includes the thermoplastic polyimide pulverized material. <1> ~ <3> 13. A method for manufacturing a winding according to any one of claims 1 to 12. <5> The object includes a winding having a coating made of the thermoplastic polyimide. <1> ~ <4> 13. A method for manufacturing a winding according to any one of claims 1 to 12. <6> In preparing the thermoplastic polyimide material, the coating is peeled off from the winding having the coating to prepare the thermoplastic polyimide material. <5> A method for manufacturing the winding wire according to claim 1. <7> stripping the coating with a blade to remove the coating from the winding on which it is carried; <6> A method for manufacturing the winding wire according to claim 1. <8> The winding having the thermoplastic polyimide coating includes a winding separated from a motor. <5> ~ <7> 13. A method for manufacturing a winding according to any one of claims 1 to 12. Effect of the Invention

[0012] According to the present disclosure, it is possible to provide a method for manufacturing a winding that can reuse resin and produce a winding having a resin coating that has excellent electrical properties and heat resistance. [Brief description of the drawings]

[0013] [Figure 1] 1 is a cross-sectional view of an example of a winding manufactured by the winding manufacturing method of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In the present disclosure, the use of "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower limit and upper limit. In the present disclosure, in the ranges described stepwise, the upper or lower limit value described in one range may be replaced with the upper or lower limit value of another range described stepwise. In the ranges described in the present disclosure, the upper or lower limit value of the range may be replaced with the value shown in the examples. In this disclosure, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, it means the total amount of multiple substances present in the composition, unless otherwise specified.

[0015] (1) Winding manufacturing method The winding manufacturing method of the present disclosure is a method for manufacturing a winding (hereinafter also referred to as a "recycled winding") that includes a conductor and a coating of thermoplastic polyimide that directly coats the conductor. The winding manufacturing method includes preparing a thermoplastic polyimide material separated from an object containing the thermoplastic polyimide (hereinafter also referred to as a "used object") (hereinafter also referred to as a "preparation step (A)"), and extrusion coating a thermoplastic polyimide composition containing the thermoplastic polyimide material directly onto the conductor to produce the coating (hereinafter also referred to as a "coating step (C)"). The preparation step (A) and the coating step (C) are performed in this order.

[0016] "Thermoplastic polyimide" refers to a polyimide resin having thermoplastic properties. The thermoplastic polyimide is preferably a polyimide resin having a deflection temperature under load of 200°C or higher. The method for measuring the deflection temperature under load is in accordance with ASTM D648, and the load is 1.82 MPa. The higher the measured value of the deflection temperature under load, the better the deflection strength. "Directly covering the conductor" means that no other resin layer, different from the thermoplastic polyimide coating, is interposed between the conductor and the thermoplastic polyimide coating. The term "thermoplastic polyimide coating" refers to a coating that contains thermoplastic polyimide as a main component and has electrical insulation properties. The phrase "containing thermoplastic polyimide as a main component" means that the content of thermoplastic polyimide is 60% by mass or more, and preferably 100% by mass, based on the total amount of the thermoplastic polyimide coating. "Having electrical insulation" means that the electrical resistance is 10 10 Indicates that the resistance is Ω·m or more. The term "thermoplastic polyimide material" refers to a material containing thermoplastic polyimide as a main component. The term "thermoplastic polyimide composition" refers to a composition containing thermoplastic polyimide as a main component. The thermoplastic polyimide content in the thermoplastic polyimide coating, the thermoplastic polyimide content in the thermoplastic polyimide material, and the thermoplastic polyimide content in the thermoplastic polyimide composition may be the same or different.

[0017] The winding manufacturing method of the present disclosure has the above-mentioned configuration, and therefore can reuse resin to manufacture a winding having a resin coating that has excellent electrical properties and heat resistance. This effect is believed to be due to, but not limited to, the following reasons. In the present disclosure, the resin coating is a thermoplastic polyimide coating, which is mainly composed of thermoplastic polyimide. Thermoplastic polyimide is not a thermosetting resin and is therefore reusable. The glass transition temperature of thermoplastic polyimide is high (e.g., 240°C or higher). Therefore, the physical properties of the thermoplastic polyimide coating tend to be stable until the glass transition temperature of the thermoplastic polyimide is exceeded. In other words, the heat resistance of the resin coating of recycled winding wires is excellent. The partial discharge inception voltage of the thermoplastic polyimide coating is high (for example, 1000 V or more), so the electrical properties of the resin coating of the recycled winding wire are excellent. From the above, it is presumed that the winding manufacturing method of the present disclosure can reuse resin and manufacture a winding having a resin coating that has excellent electrical properties and heat resistance.

[0018] (1.1) Recycled windings The recycled winding includes a conductor and a coating of thermoplastic polyimide (hereinafter, also referred to as a "thermoplastic polyimide coating"). The thermoplastic polyimide coating directly covers the conductor.

[0019] A cross-sectional view of an example of a recycled winding is shown in Fig. 1. As shown in Fig. 1, the recycled winding 10 includes a conductor 11 and a thermoplastic polyimide coating 12. The thermoplastic polyimide coating 12 directly coats the conductor 11.

[0020] (1.1.1) Conductor A conductor has the function of carrying electric current.

[0021] The cross-sectional shape of the conductor when cut at a plane perpendicular to the axial direction of the recycled winding (hereinafter simply referred to as "cross-sectional shape") is not particularly limited, and examples include a rectangle (e.g., a square, a rectangle, etc.), a polygon (but excluding a rectangle), a circle, an ellipse, etc. Among these, it is preferable that the cross-sectional shape of the conductor is rectangular. Hereinafter, a conductor having a rectangular cross-sectional shape is also referred to as a "rectangular conductor".

[0022] From the viewpoint of suppressing the occurrence of partial discharge, the cross-sectional shape of the rectangular conductor is preferably one in which the four corners are chamfered (with a radius of curvature) as shown in Fig. 1. The radius of curvature is not particularly limited and is appropriately selected depending on the application of the recycled winding wire, and is preferably 0.6 mm or less, more preferably 0.2 mm to 0.4 mm.

[0023] The size of the conductor is not particularly limited. In the cross section of the rectangular conductor when cut at a plane perpendicular to the axial direction of the recycled winding, the lengths of the long and short sides of the rectangular conductor are not particularly limited and are appropriately selected depending on the application of the recycled winding, and are preferably within the following ranges. The length of the long side of the rectangular conductor is preferably 1.0 mm to 5.0 mm, more preferably 1.4 mm to 4.0 mm. The length of the short side of the rectangular conductor is preferably 0.4 mm to 3.0 mm, more preferably 0.5 mm to 2.5 mm. The ratio of the length of the long side of the rectangular conductor to the length of the short side of the rectangular conductor (length of the long side of the rectangular conductor / length of the short side of the rectangular conductor) is preferably 1 to 4. When the cross-sectional shape of the conductor is circular, the diameter of the conductor is preferably 0.3 mm to 3.0 mm, and more preferably 0.4 mm to 2.7 mm.

[0024] The material of the conductor may be a metal. The metal is not particularly limited, and examples thereof include copper, iron, nickel, gold, silver, platinum, cobalt, zinc, lead, tin, titanium, chromium, aluminum, magnesium, manganese, and alloys thereof (stainless steel, brass, phosphor bronze, etc.). The copper may be low-oxygen copper or oxygen-free copper. The oxygen content of the low-oxygen copper is 30 ppm or less, preferably 20 ppm or less.

[0025] (1.1.2) Thermoplastic polyimide coating The thermoplastic polyimide coating has a function of insulating the conductor.

[0026] The thickness of the thermoplastic polyimide coating is not particularly limited and may be appropriately selected depending on the application of the recycled winding wire, and is preferably 30 μm to 300 μm, and more preferably 40 μm to 250 μm.

[0027] Details of the composition of the thermoplastic polyimide coating will be described later.

[0028] (1.1.3) Other layers The recycled winding may have another layer different from the thermoplastic polyimide coating provided on the outer periphery of the thermoplastic polyimide coating depending on the application of the recycled winding, etc. Examples of the other layer include an electrical insulating layer and an adhesive layer.

[0029] (1.1.4) Purpose The use of the recycled winding wire is not particularly limited, and examples of the use include windings of electric devices (for example, electric motors, transformers, etc.) In particular, it is preferable that the recycled winding wire is used as a winding included in an electric motor.

[0030] (1.2) Preparation process (A) The method for producing a winding wire according to the present disclosure includes a preparation step (A).

[0031] In the preparation step (A), a thermoplastic polyimide material separated from a used object is prepared.

[0032] (1.2.1) Used objects The used object is not particularly limited as long as it is an object containing a thermoplastic polyimide, and examples thereof include a winding having a coating made of a thermoplastic polyimide (hereinafter also referred to as a "used winding"), a film, a tube, a semiconductor manufacturing device, a wire plate covering, an office automation device (e.g., a heat insulating bush, a gear, etc.), an electric / electronic part (e.g., a socket, a connector, etc.), a structural member (e.g., an aircraft, an automobile, an industrial device, etc.), a seal, a washer, an industrial device part, a hard disk part, an electric / electronic manufacturing device part, a sealant, etc. Examples of the used winding include a winding separated from an electric motor, a winding separated from a transformer, etc.

[0033] The used object preferably includes a winding having a coating made of a thermoplastic polyimide, and more preferably is a winding having a coating made of a thermoplastic polyimide. This makes it possible for the manufacturing method of the winding disclosed herein to more efficiently manufacture recycled windings suitable for use as windings in electric motors (hereinafter also referred to as "electric motor windings") than when the used object does not include used windings.

[0034] The term "coating made of thermoplastic polyimide" means that the content of thermoplastic polyimide is 60% by mass or more, and preferably 100% by mass, based on the total amount of the coating.

[0035] When the used object includes a winding having a coating made of thermoplastic polyimide, the winding having a coating made of thermoplastic polyimide preferably includes a winding separated from an electric motor, and more preferably is a winding separated from an electric motor, whereby the manufacturing method of the winding disclosed herein can more efficiently manufacture recycled windings suitable for electric motor windings than when the used windings do not include electric motor windings.

[0036] (1.2.2) Preparation method The method for preparing the thermoplastic polyimide material is not particularly limited, and examples thereof include a method in which the thermoplastic polyimide material is separated from a used object, and a method in which a commercially available thermoplastic polyimide material is purchased.

[0037] The method for separating the thermoplastic polyimide material from the used object is appropriately selected depending on the type of the used object, and may be a known method. In detail, examples of the separation method include a method using a known peeling device, a method of heating the used object to soften or melt the thermoplastic polyimide (hereinafter also referred to as a "heating separation method"), and a method of separating the used object based on the difference in material properties (e.g., difference in specific gravity, difference between resistance to wind and weight of the material, difference in electrical properties, etc.) after crushing the used object. For example, the used object may be cooled to a low temperature to embrittle the material, and the thermoplastic polyimide material may be separated from the used object. When the thermoplastic polyimide material is separated from the used winding using a peeling device, a peeling tool (e.g., a blade, etc.) is inserted into the coating to peel off the coating, thereby obtaining the thermoplastic polyimide material. The thermoplastic polyimide material separated from the used object may be washed by a known method. By washing the thermoplastic polyimide material separated from the used object, impurities are easily removed from the thermoplastic polyimide material.

[0038] When the used object is a used winding, it is preferable to prepare a thermoplastic polyimide material by peeling off the coating from the winding having the coating in the preparation step (A). This makes it possible for the manufacturing method of the winding disclosed herein to more efficiently manufacture recycled windings suitable for windings for electric motors than when the coating of the used winding is not peeled off.

[0039] When removing the coating from the used winding, it is more preferable to peel the coating with a blade to remove the coating from the winding that includes the coating. This allows the manufacturing method of the winding disclosed herein to more efficiently separate the thermoplastic polyimide material from the used winding than the above-mentioned heat separation method. A known stripping device may be used for this purpose.

[0040] (1.2.3) Thermoplastic polyimide materials The thermoplastic polyimide material contains thermoplastic polyimide as a main component. The thermoplastic polyimide material may contain a component derived from a used object, or may consist only of thermoplastic polyimide.

[0041] The shape of the thermoplastic polyimide material is not particularly limited. The size of the thermoplastic polyimide material is not particularly limited, but is preferably small from the viewpoint of making the thermoplastic polyimide material easily melted in the covering step (C) described later.

[0042] The content of the thermoplastic polyimide is preferably 60% by mass to 100% by mass based on the total amount of the thermoplastic polyimide material. From the viewpoint of improving the electrical properties and heat resistance of the thermoplastic polyimide coating, the content of the thermoplastic polyimide is preferably as high as possible, and more preferably 100% by mass.

[0043] (1.3) Grinding process (B) The manufacturing method of the winding wire of the present disclosure may further include pulverizing the thermoplastic polyimide material to prepare a pulverized thermoplastic polyimide material (hereinafter also referred to as "pulverizing step (B)"). The pulverizing step (B) is performed after the preparation step (A) and before the covering step (C).

[0044] The term "thermoplastic polyimide pulverized material" refers to a material that is primarily composed of thermoplastic polyimide and has a size smaller than that of the thermoplastic polyimide material.

[0045] The method for producing a winding according to the present disclosure further includes pulverizing the thermoplastic polyimide material to produce a thermoplastic polyimide pulverized material, and the thermoplastic polyimide composition preferably includes the thermoplastic polyimide pulverized material. The size of one thermoplastic polyimide pulverized material is likely to be smaller than the size of one thermoplastic polyimide material. This makes it easier for the thermoplastic polyimide composition to melt in the covering step (C) described below than when the pulverizing step (B) is not performed. As a result, the method for producing a winding according to the present disclosure can produce recycled windings more efficiently.

[0046] The method for crushing the thermoplastic polyimide material is not particularly limited, and may be any known method, such as a method using a crusher. The crusher may be a dry type or a wet type. Examples of the crusher include a rod mill, a ball mill, a vibration mill, a planetary mill, a centrifugal mill, a stirring mill, a jet mill, and a roller mill. The crusher may be a freeze crusher that cools and crushes the thermoplastic polyimide material. These crushers may be used alone or in combination of two or more types.

[0047] The shape of the thermoplastic polyimide pulverized material is not particularly limited. The size of the thermoplastic polyimide material is preferably equal to or smaller than the general size of pellets fed into an extruder, from the viewpoint of making the thermoplastic polyimide material easier to melt in the coating step (C) described below.

[0048] (1.4) Covering process (C) The method for producing a winding wire according to the present disclosure includes a covering step (C).

[0049] In the coating step (C), a thermoplastic polyimide composition containing the thermoplastic polyimide material is extrusion coated directly onto the conductor to produce the thermoplastic polyimide coating, thereby obtaining a recycled winding.

[0050] (1.4.1) Thermoplastic polyimide composition The thermoplastic polyimide composition includes a thermoplastic polyimide material. If the grinding step (B) is performed, the thermoplastic polyimide composition includes a thermoplastic polyimide ground material. The thermoplastic polyimide composition may consist of only a thermoplastic polyimide material or a thermoplastic polyimide ground material.

[0051] The thermoplastic polyimide composition may or may not contain additives depending on the application of the recycled winding wire. Examples of additives include the same additives as those described below as additives that can be contained in the thermoplastic polyimide coating. When the thermoplastic polyimide coating contains an additive, the additive contained in the thermoplastic polyimide composition is, in principle, the same as the additive contained in the thermoplastic polyimide coating. Furthermore, when the thermoplastic polyimide coating contains an additive, the content of the additive contained in the thermoplastic polyimide composition is, in principle, the same as the content of the additive contained in the thermoplastic polyimide coating. The method of adding additives to the thermoplastic polyimide composition may be any known method.

[0052] (1.4.2) Covering method The method for extrusion coating the thermoplastic polyimide composition directly onto the conductor may be a known method, such as a method using an extruder equipped with a die. The extruder may be a known extruder. The shape of the die hole is similar to the cross-sectional shape of the conductor. The thickness of the thermoplastic polyimide coating can be adjusted by adjusting the size of the shape of the die hole.

[0053] The heating temperature of the extruder is not particularly limited, but is preferably 380°C to 420°C.

[0054] When the thermoplastic polyimide composition is extrusion coated onto the conductor, the conductor is preferably preheated. By preheating the conductor, the adhesion between the thermoplastic polyimide composition and the conductor can be improved. The preheating temperature of the conductor is not particularly limited, and is preferably 100°C to 250°C, more preferably 180°C to 220°C.

[0055] (1.5) Thermoplastic polyimide coating The thermoplastic polyimide coating will be described in more detail below.

[0056] (1.5.1) Thermoplastic polyimide resin The thermoplastic polyimide coating contains thermoplastic polyimide as a main component, and may be made of only thermoplastic polyimide.

[0057] (1.5.1.1) Composition Examples of the thermoplastic polyimide resin include a thermoplastic polyimide resin (a1) having a structural unit represented by the following chemical formula (1), a thermoplastic polyimide resin (a2) having a structural unit represented by the following chemical formula (3), a thermoplastic polyimide copolymer resin (a3) ​​having structural units represented by the following chemical formulas (4) and (5), and a thermoplastic polyimide resin (a4) having a structural unit represented by the following chemical formula (6).

[0058] [ka]

[0059] In chemical formula (1), X is a direct bond, -SO2-, -CO-, -C(CH3)2-, -C(CF3)2-, or -S-; R1, R2, R3, and R4 each independently represent a hydrogen atom, an alkyl group, an alkoxy group, a halogenated alkyl group, a halogenated alkoxy group, or a halogen atom; and Y is a tetravalent aromatic group selected from the following group of linking groups (2).

[0060] [ka]

[0061] [ka]

[0062] [ka]

[0063] [ka]

[0064] Here, m in chemical formula (4) and n in chemical formula (5) represent the copolymerization ratio of the polyimide copolymer, and m / n is in the range of 4 to 99 (mol % / mol %).

[0065] [ka]

[0066] The four types of thermoplastic polyimide resins (a1) to (a4) can be produced by reacting an aromatic diamine compound and an aromatic tetracarboxylic dianhydride, which form the structural units represented by each chemical formula, with each other in the presence or absence of an organic solvent, and imidizing the resulting polyamic acid. The production can be carried out under conditions of a known method for producing polyimides. At least one of the aromatic diamine compound and the aromatic tetracarboxylic dianhydride may be a biomass-derived compound, at least a part of which is derived from biomass. That is, the thermoplastic polyimide may be a biomass-derived thermoplastic polyimide.

[0067] To explain the thermoplastic polyimide resin (a2) having a structural unit represented by chemical formula (1) in more detail, an aromatic diamine compound represented by the following chemical formula (7) and an aromatic tetracarboxylic dianhydride represented by the following chemical formula (8) are used as raw materials.

[0068] [ka]

[0069] In the chemical formula (7), X and R1 to R4 are the same as X and R1 to R4 in the chemical formula (2).

[0070] [ka]

[0071] In chemical formula (8), Y is the same as Y in chemical formula (1).

[0072] In chemical formulas (1) and (7), specific examples of R1, R2, R3, and R4 include a hydrogen atom, an alkyl group such as a methyl group, an ethyl group, and the like; an alkoxy group such as a methoxy group, an ethoxy group, and the like; a halogenated alkyl group such as a fluoromethyl group, a trifluoromethyl group, and the like; a halogenated alkoxy group such as a fluoromethoxy group, and the like; and a halogen atom such as a chlorine atom, a fluorine atom, and the like; and is preferably a hydrogen atom.

[0073] In the chemical formulas (1) and (8), Y is a tetravalent aromatic group selected from the above-mentioned linking group group (2), preferably a benzene ring. In this case, the aromatic tetracarboxylic acid dianhydride of the chemical formula (8) is pyromellitic dianhydride.

[0074] The thermoplastic polyimide resin is preferably a thermoplastic polyimide resin (a1), a thermoplastic polyimide resin (a2), a thermoplastic polyimide copolymer resin (a3), or a thermoplastic polyimide resin (A4).

[0075] The thermoplastic polyimide more preferably contains a structural unit represented by the above chemical formula (1), and further preferably consists of the structural unit represented by the above chemical formula (1) (i.e., the thermoplastic polyimide is a thermoplastic polyimide resin (a1)). When the thermoplastic polyimide contains a structural unit represented by the above chemical formula (1), the electrical properties and heat resistance of the thermoplastic polyimide coating are more excellent.

[0076] The thermoplastic polyimide more preferably contains a structural unit represented by the above chemical formula (3), and further preferably consists of the structural unit represented by the above chemical formula (3) (i.e., the thermoplastic polyimide is a thermoplastic polyimide resin (a2)). When the thermoplastic polyimide contains a structural unit represented by the above chemical formula (3), the electrical properties and heat resistance of the thermoplastic polyimide coating are more excellent.

[0077] When producing a thermoplastic polyimide resin, other aromatic diamine compounds or aromatic tetracarboxylic dianhydrides as raw materials can be used alone or in combination to be copolymerized, as long as the object of the present disclosure is not impaired.

[0078] The thermoplastic polyimide resins preferably used in the present disclosure may be blended together, or other polyimide resins may be blended in any manner within the scope of the present disclosure without impairing the object of the present disclosure.

[0079] (1.5.1.2) Melt Index The melt index (hereinafter, also referred to as "MI") of the thermoplastic polyimide resin is not particularly limited, but is preferably 2 g / 10 min to 30 g / 10 min, more preferably 4 g / 10 min to 20 g / 10 min. The method for measuring the MI of the thermoplastic polyimide resin is the same as the method described in the Examples.

[0080] (1.5.1.3) Logarithmic Viscosity The logarithmic viscosity of the thermoplastic polyimide resin is not particularly limited, but is preferably 0.1 dl / g to 3.0 dl / g, more preferably 0.2 dl / g to 2.0 dl / g, further preferably 0.3 dl / g to 1.5 dl / g, and particularly preferably 0.4 dl / g to 1.0 dl / g. If the logarithmic viscosity is 0.1 dl / g to 3.0 dl / g, the molecular weight of the thermoplastic polyimide resin is appropriate. Therefore, the mechanical strength of the thermoplastic polyimide coating is excellent, and the flowability of the thermoplastic polyimide resin for producing the thermoplastic polyimide coating by injection molding or extrusion molding is excellent.

[0081] Logarithmic viscosity is measured by heating the mixture of parachlorophenol / phenol (90 / 10 weight ratio) at a concentration of 0.5g / 100ml to 200°C, then cooling to 35°C. The definition of logarithmic viscosity is given in the 1995 first edition of the "Polymer Handbook" published by Asakura Shoten and published by the Japan Society for Analytical Chemistry, p.58.

[0082] (1.5.1.4) Glass transition temperature Tg The glass transition temperature Tg of the thermoplastic polyimide resin is not particularly limited, and from the viewpoint of heat resistance, is preferably 200° C. or higher, more preferably 210° C. or higher, and even more preferably 220° C. or higher. The glass transition temperature Tg of the thermoplastic polyimide resin is not particularly limited, and is preferably 300° C. or lower, more preferably 290° C. or lower, and even more preferably 280° C. or lower. The glass transition temperature Tg is measured in the same manner as described in the Examples.

[0083] (1.5.1.5) Melting point The melting point of the thermoplastic polyimide resin is not particularly limited, and from the viewpoint of heat resistance, it is preferably 340° C. or higher, more preferably 350° C. or higher, and even more preferably 360° C. or higher. The melting point of the thermoplastic polyimide resin is not particularly limited, and from the viewpoint of moldability, it is preferably 420° C. or lower, more preferably 410° C. or lower, and even more preferably 400° C. or lower. The melting point was measured in the same manner as described in the Examples.

[0084] (1.5.1.6) How to obtain An example of a commercially available thermoplastic polyimide resin having the repeating structural unit of the above chemical formula (1) is AURUM (registered trademark, manufactured by Mitsui Chemicals, Inc., glass transition temperature 250° C., melting point 388° C.).

[0085] The thermoplastic polyimide resin may be a commercially available product as described above, but it can also be synthesized by the following method. In detail, a diamine represented by the following formula (9) and a tetracarboxylic dianhydride represented by the following formula (10) are co-condensed with each other through dehydration to obtain a thermoplastic polyimide resin.

[0086] [ka]

[0087] [ka]

[0088] The thermoplastic polyimide resin can be produced by a known imidization reaction. The amount of the raw material compound used is usually 0.90 to 0.99 equivalents of tetracarboxylic dianhydride per equivalent of diamine. The amount of the raw material compound used is preferably 0.93 to 0.985 equivalents, more preferably 0.95 to 0.98 equivalents. If the amount of the raw material compound used is 0.90 to 0.99 equivalents, the molecular weight of the thermoplastic polyimide resin is sufficiently high, so that the mechanical properties of the thermoplastic polyimide coating are excellent and the flowability of the thermoplastic polyimide resin is excellent.

[0089] In the synthesis of a thermoplastic polyimide resin, it is preferable to cap the reactive ends of the molecule with phthalic anhydride, etc. By capping the reactive ends, the thermal stability of the thermoplastic polyimide resin is significantly improved.

[0090] The reaction is particularly preferably carried out in an organic solvent. Examples of the organic solvent include N,N-dimethylformamide, N,N-diethylacetamide, N,N-dimethoxyacetamide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, 1,2-dimethoxyethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, bis[2-(2-methoxyethoxy)ethyl]ether, tetrahydrofuran, 1,3-dioxane, 1,4-dioxane, pyrroline, picoline, dimethyl sulfoxide, dimethyl sulfone, tetramethylurea hexamethylphosphoramide, phenol, o-cresol, m-cresol, p-cresol, p-chlorophenol, anisole, benzene, toluene, and xylene. The organic solvent may be used alone or in combination of two or more kinds.

[0091] The reaction temperature is usually room temperature to 250°C, preferably 140°C to 200°C. The reaction pressure is not particularly limited, and normal pressure is sufficient. The reaction time varies depending on the type of solvent and the reaction temperature, but is usually 4 hours to 24 hours. As for the imidization method, the precursor polyamic acid is heated to 100°C to 300°C for imidization, or an imidization agent such as acetic anhydride is used to chemically imidize the precursor to obtain the desired polyimide resin.

[0092] (1.5.2) Additives The thermoplastic polyimide coating may or may not contain additives depending on the application of the recycled winding wire.

[0093] The additive may contain at least one type selected from the group consisting of carbon fiber, glass fiber, potassium titanate fiber, aluminum borate fiber, metal fiber, ceramic fiber, boron fiber, silicon carbide fiber, asbestos fiber, rock wool fiber, and aramid fiber, within a range that does not impair the properties of the thermoplastic polyimide resin.

[0094] The additives may contain at least one type of filler such as mica, synthetic mica, wollastonite, talc, silicone oil, fluorine-based oil, glass beads, molybdenum disulfide, clay, silica, alumina, diatomaceous earth, hydrated alumina, shirasu balloons, carbon nanotubes, calcium carbonate, hydrotalcite, fluorine, graphite (e.g., artificial graphite, natural graphite (e.g., flake graphite, scaly graphite, earthy graphite), etc.), lubricant, release agent, stabilizer, colorant, crystal nucleating agent, etc., as necessary, within the range that does not impair the properties of the thermoplastic polyimide resin.

[0095] The additive may contain at least one of various liquid crystal polymers, thermoplastic resins (e.g., fluororesin, polyetherimide, polyethernitrile, polyetherketone, polyetheretherketone, polyetherketoneketone, polyetherketoneetherketoneketone, polyamideimide, polyethersulfone, polysulfone, polyarylate and / or polyphenylene sulfide), and thermosetting resins (e.g., epoxy resin, polybenzimidazole resin, polyimide resin, etc.) as long as the properties of the thermoplastic polyimide resin are not impaired.

[0096] When the thermoplastic polyimide coating contains an additive, the content of the additive and the content of the thermoplastic polyimide resin are not particularly limited and are appropriately selected depending on the type of additive, etc., and are preferably within the following ranges. The content of the additive is preferably from 0% by mass to 40% by mass or less based on the total amount of the thermoplastic polyimide coating. The content of the thermoplastic polyimide resin is preferably 60% by mass to 100% by mass based on the total amount of the thermoplastic polyimide coating. EXAMPLES

[0097] Hereinafter, the present disclosure will be specifically described with reference to examples. However, the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure.

[0098] [1] Examples and Comparative Examples [1.1] Example 1 [1.1.1] Preparation process (A) Thermoplastic polyimide (a2) containing the structural unit represented by the above chemical formula (3) was synthesized according to the following procedure. A vessel equipped with a stirrer, a reflux condenser, a water separator, and a nitrogen inlet tube was prepared. 3.312 kg (9.0 mol) of 4,4'-bis(3-aminophenoxy)biphenyl, 0.2 kg (1.0 mol) of 4,4'-diaminodiphenyl ether, 2.071 kg (9.5 mol) of pyromellitic dianhydride, 0.148 kg (1.0 mol) of phthalic anhydride, and 21.53 kg of cresylic acid were added to the vessel. Then, the mixture was heated to 145°C while stirring under a nitrogen atmosphere. During this time, about 350 ml of water was confirmed to be distilled out. The reaction was further carried out at 145°C for 4 hours. Then, the mixture was cooled to room temperature, and 10.8 kg of methyl ethyl ketone was added. Then, the mixture was filtered to obtain a yellow polyimide powder. The polyimide powder was washed with methyl ethyl ketone and then dried at 180°C for 24 hours to obtain 5.26 kg (98% yield) of polyimide powder (thermoplastic polyimide). The polyimide powder was extruded at 400°C using a Takayasu 25 mmΦ extruder to obtain pellets (1). The glass transition temperature of the thermoplastic polyimide (a2) was 245°C.

[0099] A rectangular conductor (material: copper with an oxygen content of 15 ppm) was prepared as the conductor. The length of the long side of the rectangular cross section of the rectangular conductor was 3.2 mm. The length of the short side of the rectangular cross section of the rectangular conductor was 2.4 mm. The radius of curvature of the chamfers at the four corners of the rectangular cross section of the rectangular conductor was 0.3 mm.

[0100] [1.1.1.1] Covering process (A1) An extruder equipped with a die (screw: full flight, diameter 20 mm, L / D = 24, compression ratio: 3.0) was prepared. The heating temperature in the cylinder part of the extruder was controlled by dividing it into three zones, C1, C2, and C3, in order from the material input side. The heating temperatures were set to 380°C in the C1 zone, 410°C in the C2 and C3 zones, and 420°C in the head part behind the cylinder of the extruder and the die at the tip of the head part. The shape of the hole in the die was similar to the cross-sectional shape of the rectangular conductor mentioned above. The pellets (1) were put into an extruder, and the molten pellets (1) were directly coated onto the outer circumference of a conductor preheated to a temperature of 200°C, and then allowed to cool. In this way, a winding (10) was obtained. The winding (10) comprises a conductor and a thermoplastic polyimide coating (11) that directly covers the conductor. The thermoplastic polyimide coating (11) is made of thermoplastic polyimide (a2). The cross-sectional outer shape of the winding (10) was similar to the shape of the conductor. The coating (11) had a thickness of 100 μm.

[0101] [1.1.1.2] Peeling process (A1) The coating (11) covering the conductor was cut with a cutter or blade to make a cut only in the coating, and only the coating portion was peeled off from the conductor to obtain a thermoplastic polyimide material (12).

[0102] [1.1.1.3] Grinding process (A1) The thermoplastic polyimide material (12) obtained in the peeling step was passed through a pulverizer to obtain pulverized thermoplastic polyimide material (13). A screen with a diameter of 8 mm was used to make the pulverized material uniform in size.

[0103] [1.1.1.4] Covering process (A2) A winding (20) was obtained in the same manner as in the covering step (A1), except that pulverized thermoplastic polyimide material (13) was used instead of the pellets (1). The winding (20) includes a conductor and a thermoplastic polyimide coating (21) that directly covers the conductor. The thermoplastic polyimide coating (21) is made of a thermoplastic polyimide (a2).

[0104] [1.1.1.5] Peeling process (A2) A thermoplastic polyimide material (22) was obtained in the same manner as in the peeling step (A1), except that the winding (20) was used instead of the winding (10).

[0105] [1.1.1.6] Grinding process (A2) A thermoplastic polyimide pulverized material (23) was obtained in the same manner as in the pulverizing step (A1), except that a thermoplastic polyimide material (22) was used instead of the thermoplastic polyimide material (12).

[0106] [1.1.1.7] Covering process (A3) A winding (30) was obtained in the same manner as in the covering step (A1), except that pulverized thermoplastic polyimide material (23) was used instead of the pellets (1). The winding (30) includes a conductor and a thermoplastic polyimide coating (31) that directly covers the conductor. The thermoplastic polyimide coating (31) is made of a thermoplastic polyimide (a2).

[0107] In this way, the winding (30) was prepared.

[0108] [1.1.2] Peeling process (B) A thermoplastic polyimide material (32) was obtained in the same manner as in the peeling step (A1), except that the winding (30) was used instead of the winding (10).

[0109] [1.1.3] Grinding process (C) A thermoplastic polyimide pulverized material (33) was obtained in the same manner as in the pulverizing step (A1), except that a thermoplastic polyimide material (32) was used instead of the thermoplastic polyimide material (12).

[0110] [1.1.4] Covering process (D) A recycled winding (40) was obtained in the same manner as in the covering step (A1), except that pulverized thermoplastic polyimide material (33) was used instead of the pellets (1). The recycled winding (40) includes a conductor and a thermoplastic polyimide coating (41) that directly covers the conductor. The thermoplastic polyimide coating (41) is made of thermoplastic polyimide (a2). The cross-sectional outer shape of the recycled winding (40) was similar to the shape of the conductor. The thickness of the thermoplastic polyimide coating (41) was 100 μm.

[0111] [1.2] Example 2 Except for changing the die, a recycled winding wire (40) was obtained in the same manner as in Example 1. The thickness of the thermoplastic polyimide coating (41) was 80 μm.

[0112] [1.3] Example 3 A recycled winding wire (40) was obtained in the same manner as in Example 1, except that the pellet (2) was used instead of the pellet (1).

[0113] The pellet (2) is made of a thermoplastic polyimide (a3) ​​containing structural units represented by the above formula (4) and formula (5) by the following procedure. The thermoplastic polyimide (a3) ​​was synthesized by the following procedure. Into a vessel similar to that of Example 1, 3.680 kg (10 mol) of 4,4'-bis(3-aminophenoxy)biphenyl, 2.071 kg (9.5 mol) of pyromellitic dianhydride, 0.148 kg (1.0 mol) of phthalic anhydride, and 21.53 kg of cresylic acid were charged. Except for this, the procedure was the same as in Example 1 to obtain 5.46 kg of yellow polyimide powder (yield 98.5%). The polyimide powder was extruded at 400°C using a Takayasu 25 mmΦ extruder to obtain pellets (2). The glass transition temperature of the thermoplastic polyimide (a3) ​​was 253°C.

[0114] [1.4] Example 4 Except for changing the die, a recycled winding wire (40) was obtained in the same manner as in Example 3. The thickness of the thermoplastic polyimide coating (40) was 80 μm.

[0115] [1.5] Comparative Example 1 A recycled winding (40) was obtained in the same manner as in Example 1, except that the pellet (3) was used instead of the pellet (1) and the extrusion temperature in the covering process and the preheating temperature of the conductor were changed as follows.

[0116] As the pellets (3), polyether ether ketone (PEEK) (manufactured by Solvay Specialty Polymers, product name: "KetaSpire KT-851NL", glass transition temperature: 150°C) was used.

[0117] The extrusion temperatures were changed to 300°C in the C1 zone, 380°C in the C2 and C3 zones, 390°C in the head behind the extruder cylinder, and 400°C in the die at the end of the head. The conductor preheat temperature was changed to 180°C.

[0118] [1.6] Comparative Example 2 Except for changing the die, a recycled winding wire (40) was obtained in the same manner as in Comparative Example 1. The thickness of the thermoplastic polyimide coating (41) was 200 μm.

[0119] [1.7] Comparative Example 3 The rectangular conductor was prepared as above. Polyamideimide varnish (product name: "HI-406", Hitachi Chemical Co., Ltd., NMP solution containing 32% by mass of resin component, dielectric constant: 3.9) was prepared. A die having a similar shape to the cross-sectional shape of the conductor was prepared.

[0120] The polyamideimide varnish was repeatedly applied to the surface of the conductor using a die to obtain a conductor with polyamideimide varnish. The conductor with polyamideimide varnish was transported into a baking furnace and passed through at a predetermined speed. The temperature inside the furnace was set to 550°C. The length of the baking furnace was 8 m. The conductor with polyamideimide varnish passed through the baking furnace for 15 seconds. In this way, a winding (50) was obtained. The winding (50) includes a conductor and a polyamideimide coating (51) that directly coats the conductor. The thickness of the polyamideimide coating (51) was 100 μm.

[0121] [1.8] Comparative Example 4 A winding (60) was obtained in the same manner as in Comparative Example 3, except that the number of times the polyamideimide varnish was applied was changed. The winding (60) includes a conductor and a polyamideimide coating (61) that directly covers the conductor. The thickness of the polyamideimide coating (61) was 80 μm.

[0122] [1.9] Comparative Example 5 A winding (70) was obtained in the same manner as in Comparative Example 3, except that the following polyimide varnish was used instead of the polyamideimide varnish. The winding (70) includes a conductor and a polyimide coating (71) that directly covers the conductor. The polyimide coating (71) had a thickness of 100 μm.

[0123] As the polyimide varnish, a polyimide varnish (product name: "U-imide", manufactured by Unitika Ltd., NMP solution containing 25% by mass of PI resin component, dielectric constant: 3.2) was used.

[0124] [1.10] Comparative Example 6 A winding (80) was obtained in the same manner as in Comparative Example 5, except that the number of times the polyimide varnish was applied was changed. The winding (80) includes a conductor and a polyimide coating (81) that directly covers the conductor. The thickness of the polyimide coating (81) was 80 μm.

[0125] [2]Measurement method The methods for measuring the partial discharge inception voltage (25° C.) and the like in Examples 1 to 4 and Comparative Examples 1 to 6 are as follows. The measurement results are shown in Table 1.

[0126] [2.1] Partial discharge inception voltage (25℃) A partial discharge tester (Kikusui Electronics Co., Ltd., product name: "KPD 2050") was used to measure the partial discharge inception voltage of the winding. A sample was made by closely contacting two windings. In the sample, the flat surfaces of the outer circumferential surfaces of the two windings were closely contacted with each other without any gap over a length of 150 mm. The "flat surface" refers to the surface formed by the long side of the longitudinal section of the rectangular winding in the axial direction. An electrode was connected between the two conductors of this sample, and the measurement temperature was 25°C. A 50Hz AC voltage was applied and the voltage was continuously increased. The peak voltage (Vp) was read at the point when a partial discharge of 10 pC occurred. The peak voltage (Vp) read was the partial discharge inception voltage (25°C) (hereinafter also referred to as "Vp (25°C)"). The allowable Vp (25°C) is 1000Vp or more.

[0127] [2.2] Partial discharge inception voltage (200℃) Except for changing the measurement temperature to 200°C, the voltage at the time when a partial discharge of 10 pC occurred was read as the peak voltage (Vp) in the same manner as for the partial discharge inception voltage (25°C). The peak voltage (Vp) that was read was taken as the partial discharge inception voltage (200°C) (hereinafter also referred to as "Vp(200°C)"). The allowable Vp(200°C) is 1000Vp or more.

[0128] [2.3] Heat resistance The heat resistance of the windings was quantitatively evaluated using the reduction rate of the partial discharge inception voltage. The reduction rate of the partial discharge inception voltage is expressed by the following formula (1). The allowable reduction rate of the partial discharge inception voltage is 3% or less. Equation (1): Reduction rate of partial discharge inception voltage = ((Vp(25℃)-Vp(200℃)) / Vp(25℃)) × 100

[0129] [2.4] Vp(25℃) reduction rate For Examples 1 to 4 and Comparative Examples 1 and 2, the Vp(25°C) reduction rate was calculated using the Vp(25°C) of the winding (10) and the Vp(25°C) of the winding (40). The Vp(25°C) reduction rate is expressed by the following formula (2). Equation (2): Vp(25℃) reduction rate = (([Vp(25℃) of winding (10)]-[Vp(25℃) of winding (40)]) / [Vp(25℃) of winding (10)]) × 100

[0130] [2.5] Vp(200℃) reduction rate For Examples 1 to 4 and Comparative Examples 1 and 2, the Vp(200°C) reduction rate was calculated using the Vp(200°C) of the winding (10) and the Vp(200°C) of the winding (40). The Vp(200°C) reduction rate is expressed by the following formula (3). Equation (3): Vp(200°C) reduction rate = (([Vp(200°C) of winding (10)] - [Vp(200°C) of winding (40)]) / [Vp(200°C) of winding (10)]) x 100

[0131] [2.6] Adhesion The adhesion of the winding was evaluated by the bending workability test described below. The winding was cut to obtain a straight test piece with a length of 300 mm. A scratch (incision) of about 5 μm depth and 2 μm length was made in the center of the coating on the edge surface of this straight test piece in both the longitudinal and vertical directions using a special tool. At this time, the coating and the conductor were in close contact and did not peel off. The "edge surface" refers to the surface formed by the short side in the axial direction in the cross section of the rectangular winding. The straight test piece was bent 180° (in a U-shape) with the scratch as the apex and the rectangular conductor as the axis, and this state was maintained for 5 minutes. The progress of peeling between the conductor and the coating occurring near the apex of the straight test piece was visually observed. The adhesion of the winding was evaluated according to the following evaluation criteria. The acceptable adhesion of the winding is evaluated as "A".

[0132] [2.6.1] Evaluation Criteria A: None of the scratches formed in the coating expanded, and the coating did not peel off from the conductor. B: At least one of the scratches formed in the coating expanded, and the entire coating peeled off from the conductor, etc.

[0133] [2.7] Melt index The melt index was measured using a melt indexer (manufactured by Toyo Seiki Seisakusho Co., Ltd., model number: A-371401705). The measurement was performed in accordance with JIS K7210, with a cylinder temperature of 400° C. and a load of 1.05 kg. The unit is g / 10 min.

[0134] [2.8] Glass transition temperature The glass transition temperature was measured using a differential scanning calorimeter (DSC220C, manufactured by Seiko Instruments Inc.). Specifically, about 5 mg of the material was sealed in an aluminum pan for measurement and set in the differential scanning calorimeter. Then, it was heated from room temperature to 450°C at 10°C / min. In order to completely melt the resin, it was held at 450°C for 5 minutes and then cooled to 30°C at 10°C / min. After being left at 30°C for 5 minutes, it was heated a second time to 450°C at 10°C / min. The transition point corresponding to the glass transition was taken as the glass transition temperature (Tg). The acceptable glass transition temperature is 200°C.

[0135] [Table 1]

[0136] In Table 1, "winding (new)" refers to the winding (10) in Examples 1 to 4 and Comparative Examples 1 and 2, the winding (50) in Comparative Example 3, the winding (60) in Comparative Example 4, the winding (70) in Comparative Example 5, and the winding (80) in Comparative Example 6. "Recycled winding" refers to the winding (40) in Examples 1 to 4 and Comparative Examples 1 and 2. "Tg" refers to the glass transition temperature. "TPI (a2)" refers to the thermoplastic polyimide resin (a2). "TPI (a3)" refers to the thermoplastic polyimide resin (a3). "PEEK" refers to polyether ether ketone. "PI" refers to polyimide. "PAI" refers to polyamideimide. In "MI", "coating process", and "recycled winding" in Comparative Examples 3 to 6, "-" indicates that the process was not possible.

[0137] In the winding manufacturing methods of Comparative Examples 1 and 2, polyether ether ketone was prepared instead of a thermoplastic resin polyimide material. As a result, the glass transition temperatures of the resin coatings of the recycled windings of Comparative Examples 1 and 2 were not 200°C or higher. In other words, the heat resistance of the resin coatings of the recycled windings of Comparative Examples 1 and 2 was not excellent. From the above, it was found that the winding manufacturing methods of Comparative Examples 1 and 2 are not methods for manufacturing windings that can reuse resin and produce windings with resin coatings that are excellent in electrical properties and heat resistance.

[0138] In the winding manufacturing methods of Comparative Example 3 to Comparative Example 6, a thermosetting resin (polyamideimide or polyimide) was prepared instead of a thermoplastic resin polyimide material. Therefore, it was not possible to reuse the resin coatings of the windings (50) to (80). From the above, it was found that the winding manufacturing methods of Comparative Example 3 to Comparative Example 6 are not methods for manufacturing windings that can reuse resin and produce windings with resin coatings that are excellent in electrical properties and heat resistance.

[0139] The manufacturing methods of the windings of Examples 1 to 4 are methods for manufacturing windings including a conductor and a thermoplastic polyimide coating that directly covers the conductor, and include a preparation step and a coating step. Therefore, the glass transition temperatures of the resin coatings of the recycled windings of Examples 1 to 4 were 200°C or higher. Furthermore, the Vp (25°C) and Vp (200°C) of the recycled windings of Examples 1 to 4 were each 1000V or higher. From the above, it was found that the manufacturing methods of the windings of Examples 1 to 4 are capable of manufacturing windings including a resin coating that is excellent in electrical properties and heat resistance by reusing resin. [Explanation of symbols]

[0140] 10 Windings 11 Conductor 12 Thermoplastic polyimide coating

Claims

1. 1. A method for manufacturing a winding comprising a conductor and a coating of thermoplastic polyimide directly covering the conductor, comprising the steps of: providing a thermoplastic polyimide material that is separated from the thermoplastic polyimide-containing object; extrusion coating a thermoplastic polyimide composition comprising the thermoplastic polyimide material directly onto the conductor to produce the coating; A method for manufacturing a winding, comprising:

2. 2. The method for producing a winding wire according to claim 1, wherein the thermoplastic polyimide contains a structural unit represented by the following formula (1): 【Chemistry 1】 In the formula (1), X is a direct bond, -SO 2 -, -CO-, -C(CH 3 ) 2 -, -C(CF 3 ) 2 - or -S-, R1, R2, R3, and R4 each independently represent a hydrogen atom, an alkyl group, an alkoxy group, a halogenated alkyl group, a halogenated alkoxy group, or a halogen atom, and Y is a group selected from the group consisting of four groups represented by the following formula (2): 【Chemistry 2】

3. 2. The method for producing a winding wire according to claim 1, wherein the thermoplastic polyimide contains a structural unit represented by the following formula (3): 【Chemistry 3】

4. and pulverizing the thermoplastic polyimide material to produce a thermoplastic polyimide pulverized material. The method for producing a winding according to claim 1 or 2, wherein the thermoplastic polyimide composition contains the ground thermoplastic polyimide material.

5. The method for manufacturing a winding according to claim 1 or 2, wherein the object includes a winding having a coating made of the thermoplastic polyimide.

6. The method for manufacturing a winding according to claim 5 , wherein in preparing the thermoplastic polyimide material, the coating is peeled off from a winding having the coating to prepare the thermoplastic polyimide material.

7. The method of claim 6, wherein the coating is stripped from the winding with the coating by stripping the coating with a blade.

8. The method for manufacturing a winding according to claim 5 , wherein the winding having the coating made of thermoplastic polyimide includes a winding separated from an electric motor.

Citation Information

Patent Citations

  • Method and device for separating core conductor and cladding material of electric wire

    JP1997055135A

  • Preprocessing method of regeneration for waste electric wire coated with sheath material and its device

    JP2001351450A

  • Thermally curable polyimide oligomer, molding method therefor, molded article thereby, and cured product obtained by heat treatment of molded article

    JP2003105083A

  • Piston ring made of melt-moldable thermoplastic polyimide resin

    JP2007192242A

  • Insulated electric wire

    JP2012015038A

Cited By

  • Insulated wire, coil, and motor

    WO2026204443A1