Coated paper and paper cushioning body
The coated paper with a gas barrier and heat seal layer addresses air leakage and heat-sealing issues, offering durable and effective cushioning performance.
Patent Information
- Application Number
- JP2023046096
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing paper-based cushioning materials suffer from air leakage and poor heat-sealing strength, making them impractical for long-term storage and impact resistance.
A coated paper with a gas barrier layer and a heat seal layer on a paper base material, where the gas barrier layer contains an acrylic resin with limited pigment content and a specific coating amount, and the heat seal layer is composed of styrene-acrylic copolymer, ensuring high air permeability resistance and heat-sealability.
The coated paper effectively retains air over time and withstands impacts without tearing, providing a practical cushioning solution.
Smart Images

Figure 2024135424000001 
Figure 2024135424000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a coated paper and a paper cushioning material made from this coated paper. [Background technology]
[0002] Air cushions, which are made by forming a bag out of flexible plastic film and sealing air inside, are used, for example, to protect products from impacts during transportation. Air cushions are lightweight and inexpensive, and after use, they can be significantly reduced in volume by drilling holes to release the air, which helps reduce disposal costs, so they are widely used. On the other hand, in recent years, environmental problems such as plastic waste and global warming have led to a growing trend to move away from petroleum and plastic, and it is desirable to reduce the amount of resin materials derived from fossil resources and non-biodegradable resin materials used in industrial products as much as possible. Paper has therefore been attracting attention as an alternative material to plastic.
[0003] As a paper-based cushioning material, Patent Document 1 proposes a laminated paper for cushioning material in which a water-soluble polyvinyl alcohol layer is laminated on one side of a paper base material. The laminated paper for cushioning material in Patent Document 1 is highly recyclable and biodegradable, but it is prone to air leakage, so air needs to be sealed in just before use, and it is prone to tearing when subjected to impact due to its poor heat seal strength. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-262935 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a coated paper that can be used as a practical cushioning material, and a paper cushioning body made from this coated paper. [Means for solving the problem]
[0006] The means for solving the problems of the present invention are as follows. 1. A gas barrier layer and a heat seal layer are provided on a paper substrate in this order. The hysteresis 2HB of the paper base material in the MD direction according to the KES method is 0.001 g cm / cm or more and 0.5 g cm / cm or less, The gas barrier layer contains an acrylic resin, the blending amount of a pigment is 20 parts by weight or less per 100 parts by weight of the acrylic resin, and the coating amount is 3 g / m 2 That's all. A coated paper characterized in that the overall Oken air resistance is 100,000 seconds or more. 2. The coated paper according to 1, wherein the gas barrier layer contains a styrene-acrylic copolymer. 3. The coated paper according to 1 or 2, wherein the heat seal layer contains a styrene-acrylic copolymer. 4. The coated paper according to any one of 1. to 3., wherein the gas barrier layer and the heat seal layer each contain a pigment in an amount of 1% by weight or less based on the total weight of the paper. 5. A paper cushioning material comprising the coated paper according to any one of 1. to 4. and containing a gas therein. Effect of the Invention
[0007] The coated paper of the present invention shows only a small decrease in barrier properties when bent, and therefore the paper cushioning of the present invention made of this coated paper is less prone to air leakage and can be stored for long periods of time. The coated paper of the present invention has excellent heat seal strength, and therefore the paper cushioning of the present invention made of this coated paper is resistant to tearing even when subjected to impact, making it suitable for practical use as a cushioning material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Coated paper The coated paper of the present invention has a gas barrier layer and a heat seal layer in this order on a paper base material, The bending hysteresis 2HB in the MD direction of the paper base material as measured by the KES method is 0.001 g cm / cm or more and 0.5 g cm / cm or less. The gas barrier layer contains an acrylic resin, the pigment content is 20 parts by weight or less per 100 parts by weight of the acrylic resin, and the coating amount is 3 g / m 2 That's all. The overall Oken air resistance is 100,000 seconds or more.
[0009] The KES method is an abbreviation for Kawabata Evaluation System, and is one of the methods for measuring the physical properties of flexible materials such as nonwoven fabrics and woven fabrics, and can objectively evaluate tensile properties, bending properties, and shear properties. The bending hysteresis 2HB according to the KES method can be measured, for example, by an automated pure bending tester KES-FB2-S manufactured by Kato Tech Co., Ltd. The bending hysteresis 2HB, which is a bending property, can be calculated from the relationship between the bending moment (M) and the curvature (K) during bending deformation. The bending hysteresis 2HB represents the difference in bending moment when bending and returning, and is calculated from the difference in the MK curve when going back and forth. The bending stiffness B, which is a bending property, is calculated from the increase in bending moment (M) relative to the increase in curvature (K), that is, the slope of the MK curve.
[0010] (Paper base material) The paper base material of the present invention has a hysteresis 2HB of 0.001 g·cm / cm or more and 0.5 g·cm / cm or less in bending in the MD direction according to the KES method. The smaller the hysteresis 2HB value, the easier it is to return to the original state after bending. A paper base material having a hysteresis 2HB of 0.001 g·cm / cm or more and 0.5 g·cm / cm or less has excellent processability and is less likely to have a barrier layer that is less likely to crack during processing or when subjected to impact, so that the barrier properties are less likely to decrease. In the paper base material of the present invention, the hysteresis 2HB is preferably 0.002 g·cm / cm or more, more preferably 0.004 g·cm / cm or more, even more preferably 0.006 g·cm / cm or more, even more preferably 0.008 g·cm / cm or more, and preferably 0.46 g·cm / cm or less, more preferably 0.42 g·cm / cm or less, and even more preferably 0.38 g·cm / cm or less.
[0011] The paper substrate has a bending stiffness B of 0.2 g cm in the MD direction according to the KES method. 2 / cm or more 1.5g·cm 2 / cm or less. The smaller the value of bending stiffness B, the softer the material. This bending stiffness B is preferably 0.2 g cm 2 / cm or more 1.5g·cm 2 When the thickness is 1 / cm or less, the paper base material has a good balance between flexibility and strength, is excellent in processability and air sealing property, and is less likely to deteriorate in barrier property. The paper base material has a basis weight of 20 g / m 2 More than 80g / m 2 It is preferable that the bending hysteresis 2HB is equal to or less than this value, since this makes it easier to adjust the bending hysteresis 2HB within the range of the present invention. The paper substrate preferably has a thickness of 15 μm or more and 60 μm or less, since this makes it easier to adjust the bending hysteresis 2HB within the range of the present invention.
[0012] In the present invention, the paper base material is not particularly limited except that the bending hysteresis 2HB in the MD direction measured by the KES method described above is 0.001 g cm / cm or more and 0.5 g cm / cm or less, and can be obtained by a known method using known materials. However, since it is easy to obtain a flexible paper base material, it is preferable that the paper base material contains 50% by weight or more of hardwood pulp as papermaking fiber.
[0013] (Gas barrier layer) The gas barrier layer is a layer that imparts gas barrier properties and prevents air from escaping when the coated paper of the present invention is made into a bag-shaped paper cushioning material. In the present invention, the gas barrier layer contains an acrylic resin, the blending amount of pigment is 20 parts by weight or less per 100 parts by weight of the acrylic resin, and the coating amount (dry weight) per one side is 3 g / m 2 The gas barrier layer and the heat seal layer described below are formed by coating, but the coating layer and the laminate layer can be distinguished by observing the cross section with a microscope or the like.
[0014] The acrylic resin is a resin in which the copolymerization ratio of an acrylic monomer is 50 mol % or more. Examples of the acrylic monomer include acrylic acid, methacrylic acid, and (meth)acrylic acid esters. The acrylic resin may be a polymer consisting of only an acrylic monomer, or a copolymer containing other monomers. Examples of the copolymer include a styrene-acrylic copolymer and an ethylene-acrylic copolymer.
[0015] The gas barrier layer may contain, on a dry weight basis, 20 parts by weight or less of a pigment per 100 parts by weight of the acrylic resin. The pigment is optional, and may not be contained. As the pigment, inorganic pigments such as kaolin, clay, engineered kaolin, delaminated clay, heavy calcium carbonate, light calcium carbonate, mica, talc, titanium dioxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicate salts, colloidal silica, satin white, and organic pigments such as solid, hollow, and core-shell types can be used alone or in combination of two or more. Among these, from the viewpoint of gas barrier properties, flat pigments having an average particle size of 3 μm or more and an aspect ratio of 10 or more are preferable, and flat pigments having an average particle size of 5 μm or more and an aspect ratio of 30 or more are more preferable. In this specification, the average particle size means the volume 50% average particle size (D50).
[0016] The greater the amount of pigment blended, the better the gas barrier properties, but the lower the flex resistance, making the barrier layer more susceptible to cracking during processing, etc. Therefore, the amount of pigment blended in the gas barrier layer is preferably 16 parts by weight or less, more preferably 12 parts by weight or less, even more preferably 8 parts by weight or less, even more preferably 4 parts by weight or less, even more preferably 2 parts by weight or less, and even more preferably 1 part by weight or less, based on 100 parts by weight of the acrylic resin, on a dry weight basis. The pigment is optional, and may not be included. In addition to the acrylic resin and pigment, the gas barrier layer may contain various commonly used auxiliary agents such as a crosslinking agent, a surfactant, a dispersant, a thickener, a water retention agent, an antifoaming agent, a water resistance agent, a dye, and a fluorescent dye.
[0017] The gas barrier layer may contain other gas barrier resins other than acrylic resins, within the range that does not impair the effects of the present invention. Examples of other gas barrier resins include polyvinyl alcohol resins such as fully saponified polyvinyl alcohol, partially saponified polyvinyl alcohol, and ethylene copolymerized polyvinyl alcohol; proteins such as casein, soybean protein, and synthetic protein; starches such as oxidized starch, cationic starch, urea phosphate esterified starch, and hydroxyethyl etherified starch; cellulose derivatives such as carboxymethyl cellulose, hydroxymethyl cellulose, and hydroxyethyl cellulose; polyvinylpyrrolidone; and sodium alginate. However, in the present invention, the gas barrier layer preferably contains 60% by weight or more of acrylic resins, more preferably 80% by weight or more, even more preferably 90% by weight or more, even more preferably 95% by weight or more, even more preferably 98% by weight or more, and even more preferably 99% by weight or more of the total gas barrier resin.
[0018] The coating weight of the gas barrier layer is 3 g / m per side in dry weight. 2 The coating weight of the gas barrier layer is 3 g / m 2 If it is less than this, the gas barrier properties will be insufficient and the injected air will easily escape over time. The dry weight of the gas barrier layer on one side should be 5 g / m 2 More than 7g / m is preferable. 2 Although there is no particular upper limit to the coating amount per side in terms of dry weight of the gas barrier layer, the gas barrier property is not improved beyond this limit and reaches saturation, and the cost becomes high. 2 The gas barrier layer may be a single layer or may be configured as a multi-layer of two or more layers. By configuring the gas barrier layer as a multi-layer of two or more layers, defects such as coating unevenness can be reduced compared to the case of a single layer. When the gas barrier layer is configured as a multi-layer of two or more layers, it is preferable that the total dry weight of all the gas barrier layers is in the above range, and the coating amount of the dry weight of a single layer is 2 g / m2 or less. 2 More preferably, it is equal to or greater than this.
[0019] (Heat seal layer) The heat seal layer is a layer that imparts heat sealability, specifically, a layer that can be bonded to an object by applying heat and pressure. The coated paper of the present invention has heat-sealing suitability, which allows it to be processed into bag-shaped paper cushioning materials and makes it easy to ensure airtightness.
[0020] The heat seal layer is provided on the gas barrier layer by coating. The thermoplastic resin contained in the heat seal layer is not particularly limited, and thermoplastic resins used for heat seal applications such as styrene-acrylic copolymers, acrylic resins, ethylene-acrylic copolymers, ethylene-vinyl acetate resins, polyolefin resins (polyethylene, polypropylene, etc.), polyester resins (polyethylene terephthalate, polyethylene succinate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyvinyl alcohol resins, polyvinyl acetate resins, and polylactic acid resins can be used without any particular limitations. Among these, styrene-acrylic copolymers, acrylic resins, and ethylene-acrylic copolymers are preferred because they have excellent adhesion to the gas barrier layer to which the heat seal layer is applied, and styrene-acrylic copolymers are more preferred. Also, biodegradable resins such as polyvinyl alcohol, polylactic acid, and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (PHBH) are preferred from the viewpoint of reducing the environmental load when the resin is discharged as waste.
[0021] The heat seal layer may contain additives such as an antiblocking agent, a silane coupling agent, etc. As the antiblocking agent, pigments, waxes, metal soaps, etc. may be used without any particular limitation. However, in the flexible packaging paper of the present invention, it is preferable that the heat seal layer does not contain additives from the viewpoint of cost.
[0022] The coating weight of the heat seal layer is 3g / m per side in dry weight. 2 More than 20g / m2 It is preferable that the dry weight is 3 g / m or less. 2 If the dry weight is less than 20 g / m, the heat sealability may be insufficient. 2 If the thickness exceeds this range, there is almost no improvement in heat sealability and the cost increases. The heat seal layer may be a single layer, or may be configured as two or more layers. By configuring the heat seal layer as two or more layers, defects such as coating unevenness can be reduced compared to the case of a single layer. When the heat seal layer is configured as two or more layers, it is preferable that the total dry weight of all the heat seal layers is within the above range, and the coating amount of the dry weight of a single layer is 2 g / m2. 2 More preferably, it is equal to or greater than this.
[0023] The method for coating the gas barrier layer and the heat seal layer is not particularly limited, and they can be coated using a known coating device and coating system, such as a blade coater, a bar coater, an air knife coater, a curtain coater, a spray coater, a roll coater, a reverse roll coater, a size press coater, a gate roll coater, etc. The coating system may be either aqueous coating using a solvent such as water or solvent-based coating using a solvent such as an organic solvent, but aqueous coating is preferred from the viewpoint of safety and hygiene. When aqueous coating is used, the acrylic resin contained in the gas barrier layer and the thermoplastic resin contained in the heat seal layer are preferably water-dispersible resins or water-soluble resins.
[0024] The coated paper of the present invention has a gas barrier layer and a heat seal layer in this order on a paper base material. The coated paper of the present invention may have other layers, such as a sealing layer, an ink-receiving layer, a water-resistant layer, an oil-resistant layer, or a water vapor barrier layer, between the paper base material and the gas barrier layer, and between the gas barrier layer and the heat seal layer.
[0025] Paper cushioning The coated paper of the present invention can be made into a paper cushioning body by heat-sealing the periphery to form a bag and sealing air in it. The shape of the paper cushioning body can be any of the known bag-shaped packaging shapes, such as vertical pillow packaging bags, horizontal pillow packaging bags, side-sealed bags, two-sided sealed bags, three-sided sealed bags, and four-sided sealed bags. EXAMPLES
[0026] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, parts and % are by weight, respectively, unless otherwise specified. The resulting coated paper and paper cushioning were subjected to tests based on the evaluation methods described below. The results are shown in Table 1.
[0027] (Evaluation method) ·2HB, B by KES method Using a KES type pure bending tester (KES-FB2-S) manufactured by Kato Tech Co., Ltd., a sample with a length of 100 mm x 100 mm was held with a clamp width of 1.0 cm and bent at a speed of 0.5 cm. -1 / sec, maximum curvature 2.5cm -1 The measurements were performed under the following conditions. The difference in bending moment during reciprocation was measured at two locations, one with a curvature of 1.0 (front bending) and one with a curvature of -1.0 (reverse bending), and the average value was taken as the bending hysteresis 2HB. The MK curves were measured at two locations with curvatures ranging from 0.5 to 1.5 (front bending) and from -0.5 to -1.5 (reverse bending), and the average value was taken as the bending rigidity B in the MD direction.
[0028] ·Basis weight, coating amount The basis weight was measured in accordance with JIS P 8124. In addition, the basis weight was measured before and after coating, and the coating amount (g / m 2 ) was calculated. ·Air permeability (Oken air permeability resistance) The air permeability (Oken air resistance) of the prepared coated paper was measured using an Oken air permeability and smoothness tester (manufactured by Asahi Seiko Co., Ltd.) according to JAPAN TAPPI No. 5.
[0029] -Heat sealability Two square test pieces with sides of 100 mm were cut from the resulting coated paper, and the coating layers were placed in contact with each other and pressed at a pressure of 130°C and 2 kgf / cm. 2 The heat-sealed test piece was cut to a width of 15 mm and peeled at a tensile speed of 200 mm / min using a tensile tester, and the maximum load was recorded as the heat seal strength. Regarding peelability, the heat-sealed test piece was peeled by hand, and the peeled portion was visually observed, and the heat-sealability was evaluated according to the following criteria: ◯ or △ indicates no problem in practical use. [Evaluation Criteria] ◯: Peeling occurs within the paper base (paper base is destroyed). Δ: Most of the peeling occurs within the paper base (paper base is destroyed). ×: Peeling occurs between the coating layers.
[0030] Load testing A pressure strength test jig manufactured by our company was used to apply a load and evaluate the air escape. This pressure strength test jig is fixed so that the metal plate can only be moved in the vertical direction, and a specified load can be applied depending on the weight and number of metal plates. The cushion was placed flat and a 150g metal plate was placed on top of it. The height of the metal plate was measured every 24 hours and the number of days until the height fell to 30% or less compared to the start of the test was measured.
[0031] Recyclability Samples measuring 40 mm on a side were cut from the resulting coated paper, and the degree of disintegration of each sample was evaluated when the sample was disintegrated using a TAPPI disintegrator at a concentration of 2.5% by weight, in 40° C. water, for 10 minutes at 3,000 rpm. [Evaluation Criteria] Good: Pulp fibers are dispersed and disintegration is good. ×: Lumps or bundles of pulp fibers remain, and disintegrability is poor.
[0032] [Example 1] Paper base material (Nippon Paper Industries Co., Ltd., basis weight 38.5 g / m 2 Styrene-acrylic copolymer emulsion 1 (manufactured by Toyochem Co., Ltd., product name: FILLHARMO GS411, coating concentration: 38%) was applied to one side of a 100% LBKP sheet, with the target coating weight being 8.0 g / m2 in solid content. 2 Then, a styrene-acrylic copolymer emulsion 2 (manufactured by Daiichi Toryo Co., Ltd., product name: Harvil HS-1, coating concentration: 40%) was applied on the gas barrier layer to a target coating amount of 10.0 g / m2 in solid content. 2 The mixture was then air-dried to form a heat seal layer, thereby obtaining a coated paper. A square test piece with sides of 200 mm was cut out from the resulting coated paper and folded in half (200 mm x 100 mm) so that the coated side was on the inside. The three open sides were pressed at a temperature of 130°C and a pressure of 2 kgf / cm, leaving about 5 mm on the folded short sides. 2 The paper was heat-sealed at a width of 5 mm with a pressure application time of 0.5 seconds. 300 mL of air was injected through the non-heat-sealed gap, and the gap was then sealed with a soldering iron to obtain a paper cushioning body.
[0033] [Example 2] The target coating weight for the gas barrier layer is 6.0 g / m2 in solids. 2 A coated paper and a paper cushioning were obtained in the same manner as in Example 1, except that the coating was performed so that the coated paper and the paper cushioning were [Example 3] The target coating weight for the gas barrier layer is 4.0 g / m2 in solids. 2 A coated paper and a paper cushioning were obtained in the same manner as in Example 1, except that the coating was performed so that the coated paper and the paper cushioning were [Comparative Example 1] The target coating weight for the gas barrier layer is 2.0 g / m2 in solids. 2 A coated paper and a paper cushioning were obtained in the same manner as in Example 1, except that the coating was performed so that the coated paper and the paper cushioning were [Comparative Example 2] No gas barrier layer is formed (coating amount 0g / m 2 ) Coated paper and paper cushioning were obtained in the same manner as in Example 1.
[0034] [Example 4] Paper base material (manufactured by Nippon Paper Industries Co., Ltd., basis weight 48g / m 2 A coated paper and a paper cushioning were obtained in the same manner as in Example 1, except that 100% LBKP was used. [Comparative Example 3] Paper base material (basis weight 63g / m 2 A coated paper and a paper cushioning were obtained in the same manner as in Example 1, except that a 100% LBKP (manufactured by Nippon Paper Industries Co., Ltd.) was used.
[0035] [Example 5] Coated paper and paper cushioning were obtained in the same manner as in Example 1, except that the paint forming the gas barrier layer was mixed with 15 parts by dry weight of kaolin (manufactured by Shiraishi Kogyo Co., Ltd., average particle size 3.6 μm, aspect ratio 10-15) per 100 parts by weight of styrene-acrylic copolymer. [Comparative Example 4] Coated paper and paper cushioning were obtained in the same manner as in Example 5, except that 25 parts by dry weight of kaolin was added to 100 parts by weight of styrene-acrylic copolymer in the paint forming the gas barrier layer. [Comparative Example 5] Coated paper and paper cushioning were obtained in the same manner as in Example 5, except that 50 parts by dry weight of kaolin was added to 100 parts by weight of styrene-acrylic copolymer in the paint forming the gas barrier layer.
[0036] [Comparative Example 6] A coated paper and a paper cushioning body were obtained in the same manner as in Example 1, except that a PVA resin 1 (manufactured by Nippon Vinyl Acetate & Poval Co., Ltd., product name: JP-05) was used for the gas barrier layer. [Comparative Example 7] A coated paper and a paper cushioning were obtained in the same manner as in Example 1, except that a PVA-based resin 2 (manufactured by Kuraray Co., Ltd., product name: 5-95) was used for the gas barrier layer. [Reference example] A commercially available PE film air cushioning material (product name: ACF100, manufactured by Aswill Co., Ltd.) was used. Note that no evaluation of heat sealability was performed for this reference example.
[0037] [Table 1]
[0038] [Table 2]
[0039] The results of Examples 1 to 3 and Comparative Examples 1 and 2 confirmed that the greater the coating weight of the gas barrier layer, the less likely air is to escape, and the results of Examples 1 and 4 and Comparative Example 3 confirmed that air is less likely to escape when the bending hysteresis 2HB of the paper base material is between 0.001 g cm / cm and 0.5 g cm / cm. From the results of Examples 1 and 5 and Comparative Examples 4 and 5, it was confirmed that the more pigment the paper contained, the more likely the gas barrier properties would be improved, but when the paper was used as a paper cushioning material, air was more likely to escape. This is thought to be because the gas barrier layer is more likely to crack when folded or otherwise processed when the amount of pigment is high. From Example 1 and Comparative Examples 6 and 7, it was found that the gas barrier layer containing an acrylic resin was less susceptible to air leakage and also had excellent heat sealing suitability.
Claims
1. A gas barrier layer and a heat seal layer are provided on a paper substrate in this order. The hysteresis 2HB of the paper base material in the MD direction according to the KES method is 0.001 g cm / cm or more and 0.5 g cm / cm or less; The gas barrier layer contains an acrylic resin, and the blending amount of a pigment is 20 parts by weight or less per 100 parts by weight of the acrylic resin, and the coating amount is 3 g / m 2 That's all. A coated paper characterized in that the overall Oken air resistance is 100,000 seconds or more.
2. 2. The coated paper according to claim 1, wherein the gas barrier layer contains a styrene-acrylic copolymer.
3. 2. The coated paper according to claim 1, wherein the heat seal layer contains a styrene-acrylic copolymer.
4. 2. The coated paper according to claim 1, wherein the gas barrier layer and the heat seal layer each contain a pigment in an amount of 1% by weight or less based on the total weight of the layer.
5. A paper cushioning body comprising the coated paper according to any one of claims 1 to 4 and containing a gas therein.
Citation Information
Patent Citations
Laminated paper for buffer member
JP1997262935A
Barrier laminate
JP2020189489A
Barrier laminate
JP2021046626A
Food packaging paper
JP2021075827A
Coated paper
JP2021195717A