Expandable styrene resin particle, pre-expanded styrene resin particle, and styrene resin expanded molding

By controlling the amount of impregnated materials on expandable styrenic resin particles and pre-expanding them, the issues of decreased whiteness and moldability in styrenic resin foam molded products are addressed, resulting in high whiteness and improved moldability.

JP2024135585APending Publication Date: 2024-10-04SEKISUI PLASTICS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023046353
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Styrenic resin foam molded products face issues with decreased whiteness and appearance due to surface additives and dispersion stabilizers, leading to poor moldability and mechanical strength.

Method used

Expandable styrenic resin particles with a controlled amount of impregnated materials, such as resin powder, dispersant, and surface additives, are produced by washing with water and adjusting the impregnated material content to 0.003 to 0.080 parts by mass, followed by pre-expansion to achieve high whiteness and moldability.

Benefits of technology

The solution maintains high whiteness and beautiful appearance while enhancing moldability and mechanical strength of styrenic resin foam molded articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135585000001_ABST
    Figure 2024135585000001_ABST
Patent Text Reader

Abstract

To provide an expandable styrene resin particle capable of giving high whiteness and beautiful appearance to styrene resin expanded molding obtained therefrom, and capable of suppressing reduction of moldability to a styrene resin expanded molding, a pre-expanded styrene resin particle constituted by pre-expanding such expandable styrene resin particle, and a styrene resin expanded molding molded from such expandable styrene resin particle and pre-expanded styrene resin particle.SOLUTION: An expandable styrene resin particle by an embodiment of the present invention is an expandable styrene resin particle having an impregnated substance on a surface, where the amount of the impregnated substance to 100 pts.mass of the expandable styrene resin particle is 0.003-0.080 pts.mass.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to expandable styrene-based resin particles, pre-expanded styrene-based resin particles, and a styrene-based resin foamed article. [Background technology]

[0002] Styrene-based resin foam molded products are lightweight and have excellent heat insulation and mechanical strength, and therefore are widely used as heat insulation materials for houses and automobiles, heat retaining materials for building materials, embankment materials for polystyrene foam civil engineering, transport packaging materials for fish boxes and food containers, shock absorbing materials, cushioning fillers, etc. Among them, as styrene-based resin foam molded products, in-mold foam molded products manufactured from expandable particles (representatively, expandable styrene-based resin particles or pre-expanded styrene-based resin particles obtained by pre-expanding them) are widely used because of the advantage that the desired shape can be easily obtained. Such styrene-based resin foam molded products are composed of a plurality of expandable particles fused to each other.

[0003] Styrene resin foam molded articles are often required to have high whiteness and beautiful appearance due to the intended use, etc.

[0004] In general, in order to promote fusion of styrene-based resin foam molded products, a surface additive is attached to the surface of the expandable styrene-based resin particles, which are the raw material (Patent Documents 1 and 2). However, the surface additive often excessively plasticizes the surface due to the heat during foaming and molding. For this reason, when a surface additive is attached to the surface of the expandable styrene-based resin particles, which are the raw material, problems occur such as a decrease in whiteness of the styrene-based resin foam molded product and a deterioration in the appearance of the styrene-based resin foam molded product.

[0005] On the other hand, if the amount of surface additive added to the surface of the raw material, expandable polystyrene resin particles, is reduced in an attempt to solve the problems of decreased whiteness and deteriorated appearance of the styrene resin foamed molded body, problems arise in that fusion becomes difficult in the styrene resin foamed molded body and that mechanical strength and moldability are reduced.

[0006] In addition, when producing expandable styrene resin particles, which are the raw material for styrene resin foamed molded articles, a dispersion stabilizer is generally used. Therefore, the dispersion stabilizer may remain and be attached to the surface of the expandable styrene resin particles, and the attached dispersion stabilizer may also be a factor in reducing the whiteness and deteriorating the appearance of the styrene resin foamed molded article.

[0007] Furthermore, resin powder derived from various resins, such as styrene-based resins, used in producing expandable styrene-based resin particles, which are the raw material for styrene-based resin foamed molded articles, may remain on the surface of the expandable styrene-based resin particles and be attached thereto. Such attached resin powder may also be a factor in reducing the whiteness and deteriorating the appearance of the styrene-based resin foamed molded articles. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 6223097 [Patent Document 2] JP 2014-70150 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide expandable styrene-based resin particles that can impart high whiteness and beautiful appearance to the styrene-based resin foam molded article obtained therefrom and can suppress the deterioration of moldability into the styrene-based resin foam molded article. Also, the present invention is to provide pre-expanded styrene-based resin particles obtained by pre-expanding such expandable styrene-based resin particles, and a styrene-based resin foam molded article molded from such expandable styrene-based resin particles or pre-expanded styrene-based resin particles. [Means for solving the problem]

[0010] [1] The expandable styrene resin particles according to an embodiment of the present invention are expandable styrene resin particles having an attachment on the surface, and the amount of the attachment is 0.003 to 0.080 parts by mass relative to 100 parts by mass of the expandable styrene resin particles. The amount of the attachment was measured as follows. 500 g of the expandable styrene resin particles were placed in a 2 L polybeaker equipped with a discharge part capable of collecting overflowing liquid, and an aqueous solution obtained by mixing sodium dodecylbenzenesulfonate in 10 L of water to a concentration of 0.005% by mass was added to the polybeaker at a rate of 0.2 L per minute while stirring at 270 rpm with a stirring device. The liquid level rose from the center to the periphery due to the stirring, and the liquid overflowed from the lower end of the discharge part was passed through a wire mesh with a mesh size of 0.3 mm, and 6 L of the passed liquid was collected. The collected permeate was filtered by suction using a GLASS FIBER FILTER (product name: Glass filter paper GA-200, size: 125 mm) manufactured by Advantec Toyo Co., Ltd., and the substance remaining on the filter paper was used as the attachment. This attachment was dried in a constant temperature environment of 60°C for 24 hours, and the mass was measured. [2] In the expandable styrene-based resin particles described in [1] above, the additive may include at least one selected from the group consisting of resin powder, dispersing agents, and surface additives. [3] In the expandable styrene-based resin particles described in [1] or [2] above, the expandable styrene-based resin particles may be obtained by impregnating a styrene-based resin with a blowing agent to obtain expandable particles, and washing the resulting particles with water. [4] The pre-expanded styrene-based resin particles according to an embodiment of the present invention are pre-expanded styrene-based resin particles obtained by pre-expanding the expandable styrene-based resin particles described in any one of [1] to [3] above, and the bulk expansion ratio of the pre-expanded particles is 2 to 150 times. [5] A styrene-based resin foamed molded article according to one embodiment of the present invention is molded from the expandable styrene-based resin particles described in any one of [1] to [3] above. [6] A styrene-based resin foamed molded article according to one embodiment of the present invention is molded from the pre-expanded styrene-based resin particles described in [4] above. Effect of the Invention

[0011] According to the present invention, it is possible to provide expandable styrene-based resin particles which can impart high whiteness and beautiful appearance to the styrene-based resin foam molded article obtained therefrom and can suppress a decrease in moldability into the styrene-based resin foam molded article. It is also possible to provide pre-expanded styrene-based resin particles obtained by pre-expanding such expandable styrene-based resin particles, and a styrene-based resin foam molded article molded from such expandable styrene-based resin particles or pre-expanded styrene-based resin particles. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 is a schematic diagram illustrating a method for measuring the amount of an attached substance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0014] In this specification, "(meth)acrylic" means acrylic and / or methacrylic, and "(meth)acrylate" means acrylate and / or methacrylate. In this specification, "mass" has the same meaning as "mass" in the SI unit system, and may be read as "mass".

[0015] <<A. Expandable styrene resin particles>> The expandable styrene-based resin particles according to an embodiment of the present invention are expandable styrene-based resin particles having an attachment on the surface thereof.

[0016] The "adherent" in the present invention refers to a substance that is attached to the surface of the expandable styrene-based resin particles according to an embodiment of the present invention, and more specifically, refers to a substance that remains on the filter paper when the amount of the attached substance is measured using the method for measuring the amount of the attached substance described below. Therefore, in this specification, the substance that remains on the filter paper when the amount of the attached substance is measured using the method for measuring the amount of the attached substance described below is referred to as the "adherent" in the present invention.

[0017] The "attachment" in the present invention preferably includes at least one selected from the group consisting of a resin powder, a dispersant, and a surface additive. The resin powder may be of only one type or of two or more types. The dispersant may be of only one type or of two or more types. The surface additive may be of only one type or of two or more types.

[0018] Examples of resin powders that can serve as an attachment include resin powders derived from various resins used in producing expandable styrene-based resin particles, as described below, and a representative example is a powder of a styrene-based resin, as described below.

[0019] Examples of dispersants that can serve as the attachment include dispersants used in producing expandable styrene-based resin particles, as described below.

[0020] Examples of surface additives that can be attached include surface additives used in the surface modification that may be carried out when producing expandable styrene-based resin particles, as described below.

[0021] In the expandable styrene-based resin particles according to an embodiment of the present invention, the amount of the attachment relative to 100 parts by mass of the expandable styrene-based resin particles is 0.003 parts by mass to 0.080 parts by mass, preferably 0.003 parts by mass to 0.060 parts by mass, more preferably 0.003 parts by mass to 0.040 parts by mass, particularly preferably 0.003 parts by mass to 0.030 parts by mass, and most preferably 0.003 parts by mass to 0.023 parts by mass.

[0022] The expandable styrene resin particles according to the embodiment of the present invention can impart high whiteness and beautiful appearance to the styrene resin foam molded body obtained therefrom by strictly adjusting the amount of the additive to the expandable styrene resin particles within the above-mentioned specific narrow range, and can suppress the deterioration of the moldability to the styrene resin foam molded body. That is, as mentioned in the background art, it was difficult to achieve high whiteness, beautiful appearance, and excellent moldability in the styrene resin foam molded body in the past, but in the present invention, by the technical means of strictly adjusting the amount of the additive to the expandable styrene resin particles within a specific narrow range, it has become possible to achieve high whiteness, beautiful appearance, and excellent moldability in the styrene resin foam molded body. In addition, the amount of the additive to the expandable styrene resin particles can be measured by a very simple method as described below, so that the amount of the additive can be easily adjusted.

[0023] The expandable styrene resin particles according to the embodiment of the present invention have a particle shape as a whole. The specific shape of the expandable styrene resin particles according to the embodiment of the present invention can be any suitable shape within the range that does not impair the effects of the present invention. Examples of such shapes include spherical, approximately spherical, elliptical (egg-shaped), cylindrical, approximately cylindrical, etc.

[0024] The expandable styrene-based resin particles according to the embodiment of the present invention preferably have an average particle size of 0.3 mm to 3.0 mm, and more preferably 0.3 mm to 1.7 mm.

[0025] <<B. Method for producing expandable styrene-based resin particles>> The expandable styrene-based resin particles according to the embodiment of the present invention can be produced by any suitable method as long as the effects of the present invention are not impaired. In terms of being able to more effectively exhibit the effects of the present invention, such a production method is preferably a method of impregnating a styrene-based resin with a blowing agent and washing the resulting expandable particles with water. That is, the expandable styrene-based resin particles according to the embodiment of the present invention are preferably obtained by impregnating a styrene-based resin with a blowing agent and washing the resulting expandable particles with water.

[0026] <B-1. Expandable particles> The expandable particles are obtained by impregnating a styrene-based resin with a blowing agent.

[0027] The styrene-based resin is obtained by polymerizing a monomer component containing a styrene-based monomer.

[0028] The styrene monomer includes styrene or a styrene derivative. Examples of the styrene derivative include α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene. The styrene monomer may be one type or two or more types. The styrene monomer preferably contains at least styrene. The content ratio of styrene to the total amount of the styrene monomer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0029] The monomer component may contain other monomers as long as it contains a styrene monomer as the main component. In this specification, the "main component" means that the content of the component in all components is preferably 50 mass% or more, more preferably 70 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more.

[0030] A representative example of the other monomer is a vinyl monomer.

[0031] Examples of the vinyl monomer include a polyfunctional monomer, a (meth)acrylic acid ester monomer, a maleic acid ester monomer, and a fumaric acid ester monomer. The vinyl monomer may be one type or two or more types.

[0032] Specific examples of the polyfunctional monomer include divinylbenzenes such as o-divinylbenzene, m-divinylbenzene, and p-divinylbenzene; and alkylene glycol di(meth)acrylates such as ethylene glycol di(meth)acrylate and polyethylene glycol di(meth)acrylate. By using a polyfunctional monomer, a branched structure can be imparted to the styrene-based resin. The content of the polyfunctional monomer in the monomer components constituting the styrene-based resin is preferably 0% by mass to 0.1% by mass, and more preferably 0.005% by mass to 0.05% by mass.

[0033] Specific examples of the (meth)acrylic acid ester monomer include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and hexyl (meth)acrylate. Among these (meth)acrylic acid ester monomers, butyl acrylate, 2-ethylhexyl acrylate, and ethyl acrylate are preferred, and butyl acrylate is more preferred. By using the (meth)acrylic acid ester monomer, the glass transition temperature (Tg) of the styrene-based resin can be lowered. The content of the acrylate monomer in the monomer component constituting the styrene-based resin is preferably 0% by mass to 4.0% by mass, and more preferably 0.1% by mass to 3.0% by mass.

[0034] An example of the maleate monomer is dimethyl maleate.

[0035] Examples of the fumarate monomer include dimethyl fumarate, diethyl fumarate, and ethyl fumarate.

[0036] The styrene resin may be a styrene resin that is not a recycled raw material, such as general-purpose styrene resin (GPPS), a commercially available styrene resin, or a styrene resin newly prepared by a method such as a suspension polymerization method, or may be a styrene resin that is a recycled raw material. The recycled raw material may typically be a used styrene resin foamed molded body. The recycled raw material may be a product obtained by recovering food packaging trays, fish boxes, cushioning materials for home appliances, etc., and regenerating them by a limonene dissolution method or a heat reduction method. The recycled raw material may be a product obtained by crushing non-foamed styrene resin molded bodies that have been separated and recovered from home appliances (e.g., televisions, refrigerators, washing machines, air conditioners, etc.) and office equipment (e.g., copiers, facsimiles, printers, etc.), melt-kneading them, and repelletizing them.

[0037] The styrene resin may be a composite resin of a styrene resin and an olefin resin. The content ratio of the styrene resin to the olefin resin in the composite resin (styrene resin / olefin resin: mass ratio) is preferably 50 / 50 to 90 / 10, more preferably 60 / 40 to 85 / 15. If the content of the styrene resin is too low, the foamability and / or moldability may be insufficient. If the content of the styrene resin is too high, the impact resistance and / or flexibility may be insufficient.

[0038] As the olefin resin, any appropriate olefin resin can be adopted as long as it does not impair the effects of the present invention. The olefin resin may be one type or two or more types. Specific examples include polyethylene resins such as branched low density polyethylene, linear low density polyethylene, medium density polyethylene, high density polyethylene, ethylene-vinyl acetate copolymer, ethylene-methyl methacrylate copolymer, and crosslinked bodies of these polymers; and polypropylene resins such as propylene homopolymer, propylene-vinyl acetate copolymer, ethylene-propylene random copolymer, propylene-1-butene copolymer, and ethylene-propylene-butene random copolymer. Among these olefin resins, preferred are ethylene-vinyl acetate copolymer, high density polyethylene, linear low density polyethylene, and mixtures thereof. The low density is preferably 0.91 g / cm. 3 ~0.94g / cm 3 and more preferably 0.91 g / cm 3 ~0.93g / cm 3 The high density is preferably 0.95 g / cm 3 ~0.97g / cm 3 and more preferably 0.95 g / cm 3 ~0.96g / cm 3 Medium density is a density between low and high density.

[0039] The foaming agent may be of only one type, or of two or more types.

[0040] Any suitable foaming agent can be used as long as it does not impair the effects of the present invention. The foaming agent is preferably an organic compound whose boiling point is equal to or lower than the softening point of the styrene resin and is in a gaseous or liquid state at normal pressure. Specific examples include aliphatic hydrocarbons such as propane, n-butane, isobutane, pentane (n-pentane, isopentane or neopentane), and n-hexane; alicyclic hydrocarbons such as cyclopentane and cyclopentadiene; ketones such as acetone and methyl ethyl ketone; alcohols such as methanol, ethanol, and isopropyl alcohol; low-boiling ether compounds such as dimethyl ether, diethyl ether, dipropyl ether, and methyl ethyl ether; and halogen-containing hydrocarbons such as trichloromonofluoromethane and dichlorodifluoromethane. Inorganic gases such as carbon dioxide, nitrogen, and ammonia may be used as the foaming agent. Among these, aliphatic hydrocarbons are preferred as the foaming agent. This is because they can prevent the destruction of the ozone layer and can be quickly replaced with air, thereby suppressing the deterioration of the styrene resin foamed molded body over time. More preferred blowing agents are propane, n-butane, isobutane, n-pentane, isopentane, and combinations thereof.

[0041] The content of the foaming agent can be appropriately set depending on the purpose as long as it is an amount sufficient to form pre-expanded styrene resin particles and a styrene resin foamed molded article. The content of the foaming agent is preferably 2 to 16 parts by mass, more preferably 3 to 8 parts by mass, based on 100 parts by mass of the styrene resin.

[0042] Methods for impregnating styrene resin with a foaming agent include: (i) A method in which a monomer component is continuously or intermittently supplied to an aqueous medium, suspension polymerized in the presence of a polymerization initiator, and a blowing agent is added during and / or after the completion of the polymerization to cause impregnation (one-stage method); (ii) A method in which, without adding a blowing agent, the particles obtained by polymerizing the monomer components are sieved to obtain only particles having a required particle size range, the particles, water, and a dispersing agent are supplied to a reaction vessel, the temperature is raised to prepare a dispersion, and the blowing agent is added to the dispersion to impregnate the particles with the blowing agent (two-stage method); (iii) A method (seed polymerization method) in which small styrene-based resin particles (seed particles), water, and a dispersant are supplied to a reaction vessel and the temperature is raised to prepare a dispersion, to which a monomer component having a polymerization initiator dissolved therein is continuously supplied, and further monomer components are continuously supplied as necessary, thereby carrying out polymerization, and a blowing agent is added during and / or after the completion of polymerization to impregnate the particles and grow them to the desired particle size, etc.

[0043] As the polymerization initiator, any suitable polymerization initiator can be used as long as it does not impair the effects of the present invention. Examples of such polymerization initiators include organic peroxides such as benzoyl peroxide, t-butylperoxy-2-ethylhexanoate, t-butylperoxybenzoate, t-butylperoxy-2-ethylhexyl monocarbonate, dicumyl peroxide, t-butylperoxypivalate, t-butylperoxyisopropyl carbonate, 2,2-t-butylperoxybutane, t-butylperoxy-3,3,5-trimethylhexanoate, and di-t-butylperoxyhexahydroterephthalate; and azo compounds such as azobisdimethylvaleronitrile. These polymerization initiators may be used alone or in combination of two or more kinds.

[0044] As the polymerization initiator, in order to adjust the molecular weight and reduce the amount of residual monomer, a polymerization initiator having a decomposition temperature in the range of 50°C to 80°C to obtain a half-life of 10 hours and a polymerization initiator having a decomposition temperature in the range of 80°C to 120°C to obtain a half-life of 10 hours may be used in combination. The polymerization initiator is preferably added as a liquid since it is necessary to uniformly absorb it into the seed particles. If the polymerization initiator is added directly to the dispersion liquid, it is difficult to uniformly absorb it into the seed particles. Therefore, it is preferable to add the polymerization initiator in a suspended or emulsified state in an aqueous medium, or to dissolve it in a small amount of styrene-based monomer, add a dispersant, and add it as an aqueous suspension.

[0045] The amount of the polymerization initiator used may be any appropriate amount within the range that does not impair the effects of the present invention. The amount used is preferably 0.1% by mass to 1.0% by mass, more preferably 0.1% by mass to 0.8% by mass, based on the monomer component.

[0046] The polymerization initiator is preferably added after being dissolved in a monomer component containing a styrene-based monomer or in a solvent. Examples of the solvent include aromatic hydrocarbons such as ethylbenzene and toluene; and aliphatic hydrocarbons such as heptane and octane. When a solvent is used, it is usually used in an amount of 10% by mass or less based on the monomer component.

[0047] As the dispersant, any suitable dispersant can be adopted as long as it does not impair the effects of the present invention. Examples of such dispersants include suspension stabilizers and anionic surfactants. These may be used alone or in combination of two or more kinds.

[0048] Examples of the suspension stabilizer include water-soluble polymers such as polyvinyl alcohol, methyl cellulose, polyacrylamide, and polyvinylpyrrolidone; and poorly soluble inorganic metal salts such as calcium triphosphate, magnesium pyrophosphate, and magnesium oxide. When poorly soluble inorganic metal salts are used, an anionic surfactant is usually used in combination.

[0049] Examples of anionic surfactants include alkyl sulfates such as sodium lauryl sulfate; alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate; higher fatty acid salts such as sodium oleate; and β-tetrahydroxynaphthalene sulfonates.

[0050] The reaction liquid (typically a suspension) containing a styrene-based monomer may further contain an additive. Examples of the additive include a radiation heat transfer suppressing component, a resin other than a styrene-based resin, a crosslinking agent, a plasticizer, a filler, a colorant, a bubble adjusting agent, a weathering agent, an antiaging agent, an antifogging agent, and a fragrance. The type, number, combination, content, and the like of the additives may be appropriately set according to the purpose. The additive may be one type only or two or more types.

[0051] When producing expandable particles, a foaming assistant may be included together with the foaming agent. Examples of the foaming assistant include diisobutyl adipate, toluene, cyclohexane, ethylbenzene, liquid paraffin, and coconut oil. The foaming assistant may be one type or two or more types.

[0052] When producing expandable particles, a flame retardant or a flame retardant assistant may be included together with the blowing agent. Examples of the flame retardant include tetrabromocyclooctane, hexabromocyclododecane, hexabromocyclohexane, trisdibromopropyl phosphate, tetrabromobisphenol A, tetrabromobisphenol F, tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tetrabromobisphenol A-diglycidyl ether, and 2,2-bis[4'(2'',3''-dibromoalkoxy)-3',5'-dibromophenyl]-propane. Examples of the flame retardant assistant include cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, 2,3-dimethyl-2,3-diphenylbutane, and 3,4-dimethyl-3,4-diphenylhexane. The flame retardant may be of only one kind or of two or more kinds. The flame retardant auxiliary may be of only one kind or of two or more kinds.

[0053] The expandable particles may be produced by a melt extrusion method. In the melt extrusion method, styrene resin pellets are supplied to a resin supplying device, a blowing agent is injected and kneaded into the styrene resin melted in the resin supplying device, and the molten resin containing the blowing agent is extruded from a small hole in a die attached to the tip of the resin supplying device, and then cooled to obtain expandable styrene resin particles. A method in which the resin is directly extruded from a small hole in the die into a cooling liquid, the extrudate is cut with a rotary blade immediately after extrusion, and the cut particles are cooled in the cooling liquid is called a hot cut method. A method in which the resin is once extruded into the air in the form of a strand from a small hole in the die, introduced into a cooling water tank before the strand foams, the strand is cooled in the cooling water tank, and then cut into cylindrical particles is called a strand cut method (cold cut method). Expandable styrene resin particles can be produced by either the hot cut method or the strand cut method (cold cut method).

[0054] <B-2. Cleaning process> The expandable styrene-based resin particles according to the embodiment of the present invention are preferably obtained by impregnating a styrene-based resin with a blowing agent and washing the resulting expandable particles with water. This washing step is referred to as the "washing step."

[0055] In the washing step, the temperature of the water is preferably adjusted to a specific temperature range so that the effects of the present invention can be more effectively exhibited. The temperature range is preferably from 1° C. to 37° C., more preferably from 3° C. to 35° C., even more preferably from 5° C. to 33° C., particularly preferably from 6° C. to 31° C., and most preferably from 7° C. to 30° C. By washing the expandable particles with water in such a temperature range, it is possible to provide expandable styrene-based resin particles that can impart high whiteness and beautiful appearance to the styrene-based resin foam molded article obtained therefrom and can suppress a decrease in moldability into a styrene-based resin foam molded article.

[0056] In the washing step, the amount of water relative to 100 parts by mass of the expandable particles is preferably adjusted to a specific range in order to further exhibit the effects of the present invention. The range is preferably 31 parts by mass to 390 parts by mass, more preferably 40 parts by mass to 300 parts by mass, even more preferably 50 parts by mass to 200 parts by mass, particularly preferably 60 parts by mass to 150 parts by mass, and most preferably 65 parts by mass to 120 parts by mass. By washing the expandable particles with water in such a range, it is possible to provide expandable styrene-based resin particles that can impart high whiteness and beautiful appearance to the styrene-based resin foam molded article obtained therefrom and can suppress the deterioration of moldability into a styrene-based resin foam molded article.

[0057] The washing time in the washing step can be set to any appropriate time within a range that does not impair the effects of the present invention. Taking into consideration production costs, etc., the washing time is preferably 90 minutes or less, more preferably 60 minutes or less.

[0058] ≪B-3. Drying process≫ The expandable styrene-based resin particles according to the embodiment of the present invention are preferably obtained by drying the particles obtained through the above-mentioned washing step. This drying step is referred to as the "drying step". As the drying conditions, any appropriate drying conditions can be set within a range that does not impair the effects of the present invention.

[0059] <B-4. Surface modification process> The expandable styrene-based resin particles according to the embodiment of the present invention may have their surfaces modified with a surface additive. The process of performing this modification is referred to as the "surface modification process."

[0060] In the surface modification step, a surface additive is added (typically applied) to the surface of the expandable styrene-based resin particles. The surface additive may be of only one type, or of two or more types.

[0061] By applying the surface additive to the surface of the expandable styrene-based resin particles, the surface properties of the expandable styrene-based resin particles can be appropriately modified depending on the purpose.

[0062] The amount of the surface additive may be any appropriate amount within the range that does not impair the effects of the present invention. The amount is typically preferably 0.05 to 3.0 parts by mass, more preferably 0.05 to 2.0 parts by mass, and even more preferably 0.1 to 1.6 parts by mass, relative to 100 parts by mass of the expandable styrene-based resin particles.

[0063] Surface additives include, for example, spreading agents, antistatic agents, antibinding agents, adhesion promoters, and lubricants.

[0064] Examples of surface additives include polyethylene glycol (typically functions as a spreading agent and antistatic agent); aliphatic compounds that are liquid at 5°C, such as medium-chain fatty acid triglycerides (glycerides of linear or branched fatty acids having 5 to 12 carbon atoms) (typically functions as a fusion promoter); metal salts of higher fatty acids, such as zinc stearate and magnesium stearate (typically functions as an anti-binding agent); stearic acid triglyceride (typically functions as a fusion promoter) and stearate monostearate (typically functions as an antistatic agent); and silicone oil (typically functions as a lubricant).

[0065] <<C. Pre-expanded styrene resin particles>> The pre-expanded styrene-based resin particles are prepared by pre-expanding expandable styrene-based resin particles.

[0066] That is, the pre-expanded styrene-based resin particles according to the embodiment of the present invention are obtained by pre-expanding the expandable styrene-based resin particles according to the embodiment of the present invention. The pre-expanding includes expanding the expandable styrene-based resin particles to a desired bulk expansion ratio (bulk density) using water vapor or the like. The bulk expansion ratio of the pre-expanded styrene-based resin particles is preferably 2 to 150 times, more preferably 5 to 100 times. The bulk density is the reciprocal of the bulk expansion ratio. The bulk expansion ratio and bulk density are determined, for example, as follows. By having the bulk expansion ratio of the pre-expanded styrene-based resin particles within the above range, it is possible to provide pre-expanded styrene-based resin particles that can better prevent blocking during expansion and molding, and further, can exhibit better fusion properties and surface properties while further suppressing electrostatic charge during expansion and molding, and can mold a styrene-based resin foam molded article with less static electricity.

[0067] A measurement sample of W (g) of expandable styrene resin particles is collected. This measurement sample is allowed to fall naturally into a measuring cylinder, and the volume of the measurement sample that fell into the measuring cylinder, V (cm 3) is measured using an apparent density measuring device conforming to JIS K 6911. From the mass and volume of the measurement sample, the bulk expansion ratio and bulk density can be calculated according to the following formula. Bulk foaming ratio (times = cm 3 / g) = volume of measurement sample (V) / mass of measurement sample (W) Bulk density (g / cm 3 ) = mass of measurement sample (W) / volume of measurement sample (V)

[0068] In one representative embodiment, the pre-expanded styrene-based resin particles can be used for forming a styrene-based resin foamed molded article. In another embodiment, the pre-expanded styrene-based resin particles can be used as they are as a buffer material, a heat insulating material, etc. When the pre-expanded styrene-based resin particles are used as they are, the pre-expanded styrene-based resin particles can be preferably used as a packed body in which a large number of the pre-expanded styrene-based resin particles are filled in a bag.

[0069] D. Styrene-based resin foam molding The styrene-based resin foam molded product according to one embodiment of the present invention is a styrene-based resin foam molded product molded from the expandable styrene-based resin particles according to an embodiment of the present invention. The styrene-based resin foam molded product according to another embodiment of the present invention is a styrene-based resin foam molded product molded from the pre-expanded styrene-based resin particles according to an embodiment of the present invention.

[0070] A styrene-based resin foamed molded article typically contains expanded styrene-based resin particles (hereinafter sometimes simply referred to as "expanded particles") obtained by further expanding pre-expanded styrene-based resin particles.

[0071] A styrene-based resin foamed molded article is typically composed of a plurality of foamed particles fused to one another.

[0072] The styrene-based resin foam molded article can be typically produced by charging pre-expanded styrene-based resin particles into a mold having a predetermined shape according to the purpose and performing in-mold foam molding. More specifically, the in-mold foam molding includes (i) filling the pre-expanded styrene-based resin particles into a closed mold having a large number of small holes, (ii) heating and foaming the pre-expanded styrene-based resin particles with a heat medium (e.g., pressurized steam, etc.) to obtain foamed particles, and (iii) filling the voids between the foamed particles by the heating and foaming, and fusing the foamed particles to each other to integrate them. The density of the styrene-based resin foam molded article can be appropriately set according to the purpose. The density of the styrene-based resin foam molded article can be adjusted, for example, by previously adjusting the bulk expansion ratio of the pre-expanded styrene-based resin particles to be filled in the mold, or by adjusting the amount of pre-expanded styrene-based resin particles to be filled in the mold.

[0073] The heat-foaming temperature (substantially the temperature of the heat transfer medium) is preferably 90°C to 150°C, more preferably 110°C to 130°C. The heat-foaming time is preferably 5 seconds to 50 seconds, more preferably 10 seconds to 50 seconds. The molding vapor pressure of the heat-foaming (gauge pressure of the heat transfer medium blowing in) is preferably 0.04 MPa to 0.1 MPa, more preferably 0.06 MPa to 0.08 MPa. If the heat-foaming is performed under such conditions, the expanded particles can be well fused to each other.

[0074] If necessary, the pre-expanded styrene resin particles may be aged before molding into a styrene resin foamed molded article. The aging temperature of the pre-expanded styrene resin particles is preferably 20°C to 60°C. If the aging temperature is too low, an excessively long aging time may be required. If the aging temperature is too high, the blowing agent in the pre-expanded styrene resin particles may dissipate, resulting in a decrease in moldability.

[0075] The bulk expansion ratio of the expanded beads in the styrene-based resin expansion molded product is preferably 2 to 150 times, and more preferably 5 to 100 times.

[0076] The styrene-based resin foamed molded article according to the embodiment of the present invention is molded from the expandable styrene-based resin particles according to the embodiment of the present invention, or from the pre-expanded styrene-based resin particles according to the embodiment of the present invention, and therefore exhibits high whiteness and beautiful appearance, and has excellent moldability.

[0077] The styrene-based resin foam molded article according to the embodiment of the present invention has a whiteness of preferably 90 or more, more preferably 93 or more, even more preferably 95 or more, particularly preferably 97 or more, and most preferably 98 or more. The method for measuring the whiteness will be described later.

[0078] The fusion rate of the styrene-based resin foam molded article according to the embodiment of the present invention is preferably 80% or more, more preferably 85% or more, even more preferably 88% or more, particularly preferably 90% or more, and most preferably 92% or more. The method for measuring the fusion rate will be described later. EXAMPLES

[0079] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating each property are as follows.

[0080] <Measurement of the amount of additives on the surface of expandable styrene resin particles> As shown in Fig. 1, 500 g of the expandable styrene resin particles (10) were placed in a 2 L polybeaker (100) equipped with a discharge part (150) capable of collecting overflowing liquid, and an aqueous solution (A) obtained by mixing sodium dodecylbenzenesulfonate in 10 L of water to a concentration of 0.005% by mass was added to the polybeaker at a rate of 0.2 L per minute while stirring at 270 rpm with a stirring device (200). The liquid level (500) rose from the center to the periphery due to the stirring, and the liquid overflowed from the lower end (a) of the discharge part (150) was passed through a wire mesh (300) with a mesh size of 0.3 mm, and 6 L of the passed liquid (B) was collected. The collected passed liquid (B) was suction filtered using a GLASS FIBER FILTER (trade name "Glass filter paper GA-200", size: 125 mm) manufactured by Advantec Toyo Co., Ltd., and the substance remaining on the filter paper was used as the attachment. This attachment was dried in a constant temperature environment of 60° C. for 24 hours, the mass was measured, and the amount of attachment per 100 parts by mass of the expandable styrene-based resin particles was calculated.

[0081] <Measurement of whiteness of styrene resin foam molded products> Evaluation was performed by color difference measurement based on JIS Z8729-2004 "Method of displaying color - L*a*b* color system." For the measurement, a color difference meter (Konica Minolta, model: CR-400) and a standard white calibration plate (Y: 94.3, x: 0.3144, y: 0.3208) were used for standardization. Measurements were performed at 20 arbitrary points on the surface of a flat styrene resin foam molded product using the calibrated color difference meter, and the average value of the lightness L* value was taken as the whiteness. The evaluation criteria were as follows: ◎:96 or above. ○: 93 or more but less than 96. △: Between 90 and 93. ×: Less than 90

[0082] <Evaluation of the Appearance of Styrene-Based Resin Foam Molded Products> The appearance of the styrene-based resin foam molded article was evaluated visually. ◯: The boundary portions where the foamed particles on the surface of the styrene-based resin foamed molded article are joined are smooth and have a uniform appearance. ×: The surface of the styrene resin foam molded article has irregularities at the boundaries where the foam particles are joined, making it less smooth and mottled in appearance.

[0083] <Measurement of fusion rate of styrene resin foam molded body> On the surface of a flat styrene resin foam molded body having a width of 300 mm, a length of 400 mm, and a thickness of 30 mm, a cut line of about 2 mm depth was made with a cutter knife along a straight line connecting the centers of a pair of long sides, and the styrene resin foam molded body was divided into two parts by hand along the cut line, and the number of particles broken within the particles (a) and the number of particles broken at the interface between the particles (b) were counted for any range of 100 to 150 foam particles on the fracture surface, and the value obtained by substituting the formula [(a) / ((a) + (b))] × 100 was taken as the fusion rate (%). The evaluation criteria were as follows. ◎: 90% or more ○: 85% or more but less than 90% △: 80% or more but less than 85% ×: Less than 80%

[0084] [Example 1] <Production of Expandable Styrene-Based Resin Particles> In a polymerization vessel equipped with a stirrer having a capacity of 100 liters, 40,000 parts by mass of water, 100 parts by mass of tricalcium phosphate as a suspension stabilizer, and 3.2 parts by mass of sodium dodecylbenzenesulfonate as an anionic surfactant were supplied, and while stirring, 40,000 parts by mass of styrene, 102 parts by mass of benzoyl peroxide as a polymerization initiator, and 24 parts by mass of t-butylperoxy-2-ethylhexyl monocarbonate were added, and the temperature was raised to 90°C for polymerization. The mixture was kept at this temperature for 6 hours, and then heated to 125°C and cooled after 2 hours to obtain styrene-based resin particles. The obtained styrene-based resin particles were sieved to obtain styrene-based resin particles having a particle diameter of 0.5 mm to 0.71 mm as seed particles. The rotation speed of the stirrer was adjusted so that the above particle diameter was obtained. Next, seed particles: 2150 parts by mass, water: 7520 parts by mass, magnesium pyrophosphate: 30 parts by mass, sodium dodecylbenzenesulfonate: 1.0 parts by mass were supplied to a polymerization vessel with an internal volume of 25 liters and equipped with a stirrer, and the mixture was heated to 72 ° C. while stirring to prepare a dispersion. Next, a solution was prepared in which benzoyl peroxide: 31 parts by mass, t-butylperoxy-2-ethylhexyl monocarbonate: 8 parts by mass, didodecyl 3,3'-thiodipropionate: 0.7 parts by mass as a cell regulator was dissolved in a monomer mixture of styrene: 786 parts by mass, and butyl acrylate: 137 parts by mass, and all of this was supplied to the above dispersion while stirring. Then, after the above solution was supplied to the dispersion, the temperature was maintained at 72 ° C. for 60 minutes. Next, 2,346 parts by mass of styrene was constantly fed while increasing the temperature to 87°C over 1 hour, and then, while maintaining the temperature at 87°C for 1 hour and 30 minutes, a monomer mixture having 3,744 parts by mass of styrene and 2.7 parts by mass of divinylbenzene dissolved therein was constantly fed, and this was maintained for a further 30 minutes. Next, the temperature was raised to 125°C and maintained for 30 minutes to react the unreacted monomers. Next, the temperature was cooled to 100°C, and 92 parts by mass of cyclohexane, 82 parts by mass of diisobutyl adipate, 45 parts by mass of styrene, and 640 parts by mass of mixed butane were injected into the polymerization vessel, and the vessel was maintained for 2 hours, and then the inside of the polymerization vessel was cooled to 25°C. Thereafter, the reaction liquid was separated from the expandable styrene-based resin particles, and only the reaction liquid was removed. Then, 50 parts by mass of washing water that had been adjusted to 2°C in advance per 100 parts by mass of the expandable styrene-based resin particles was added, followed by washing for 10 minutes and dehydration. After dehydration and drying, the resulting expandable styrene resin particles were coated with 0.1 part by mass of zinc stearate as an anti-blocking agent and 0.08 part by mass of 12-hydroxystearic acid triglyceride as a fusion promoter. After coating, the expandable styrene resin particles were left for 5 days in a thermostatic chamber at 13° C. Completion of aging was confirmed, and expandable styrene resin particles (1) were obtained. The amount of matter attached to the surface of the resulting expandable styrene-based resin particles (1) was measured. <Preparation of pre-expanded styrene resin particles> The resulting expandable styrene-based resin particles (1) were heated to a bulk density of 0.0166 g / cm 3 The resulting pre-expanded styrene-based resin particles (1) were aged at 20° C. for 24 hours. <Preparation of styrene-based resin foam molded body> The matured pre-expanded styrene resin particles (1) were left for 24 hours under room temperature atmosphere, and then foamed in a mold to obtain a plate-shaped styrene resin foamed molded product (1) of 400 mm x 300 mm x 30 mm size. The foaming in the mold was performed using an ACE-3SP molding machine manufactured by Sekisui Kogyo Co., Ltd. The heating time was one-sided heating time 8 seconds, reverse one-sided heating time 2 seconds, double-sided heating time 5 seconds, and the molding pressure (steam injection gauge pressure) was 0.06 MPa. The resulting styrene resin foam molded article (1) was subjected to measurement of whiteness, evaluation of appearance, and measurement of fusion rate. The results are shown in Table 1.

[0085] [Examples 2 to 30] The same procedures as in Example 1 were carried out except that the temperature and amount of washing water were changed as shown in Table 1, to obtain expandable styrene-based resin particles (2) to (30), pre-expanded styrene-based resin particles (2) to (30), and styrene-based resin foamed molded articles (2) to (30). The results are shown in Table 1.

[0086] [Comparative Example 1] The same procedure as in Example 1 was repeated, except that the temperature of the washing water was 0.5°C and the amount of washing water was 30 parts by mass per 100 parts by mass of the expandable styrene-based resin particles, to obtain expandable styrene-based resin particles (C1), pre-expanded styrene-based resin particles (C1), and styrene-based resin foamed molded products (C1). The results are shown in Table 2.

[0087] [Comparative Examples 2 to 24] Except for changing the temperature and amount of washing water as shown in Table 2, the same procedure as in Comparative Example 1 was performed to obtain expandable styrene-based resin particles (C2) to (C24), pre-expanded styrene-based resin particles (C2) to (C24), and styrene-based resin expansion molded articles (C2) to (C24). The results are shown in Table 2.

[0088] [Table 1]

[0089] [Table 2] [Industrial Applicability]

[0090] The expandable styrene resin particles, pre-expanded styrene resin particles, and styrene resin foam molded body according to the embodiment of the present invention are preferably used as heat insulating materials for houses and automobiles, heat retaining materials for building materials, transport packaging materials such as fish boxes and food containers, cushioning materials, etc. More specifically, the expandable styrene resin particles, pre-expanded styrene resin particles, and styrene resin foam molded body according to the embodiment of the present invention are preferably used as wall insulation materials, floor insulation materials, roof insulation materials, automobile insulation materials, heat retaining materials for hot water tanks, heat retaining materials for piping, heat retaining materials for solar systems, heat retaining materials for water heaters, containers for food and industrial products (e.g., food containers such as fish boxes, commuting boxes), cushioning materials, floats, blocks, packaging materials for fish and agricultural products, embankment materials (embankment molded bodies, embankment blocks, etc.), core materials for tatami mats, core materials for cushions, aggregates for concrete, etc. [Explanation of symbols]

[0091] 10 Expandable styrene resin particles 100 2L Poly Beakers 150 Discharge section 200 Mixing device 300 Wire Mesh 500 liquid level a Bottom end of the discharge section A aqueous solution B Passage liquid

Claims

1. Expandable styrene-based resin particles having an attachment on the surface thereof, the amount of the attachment is 0.003 parts by mass to 0.080 parts by mass per 100 parts by mass of the expandable styrene-based resin particles; Expandable styrene resin particles. The amount of the above-mentioned attached matter was measured as follows. 500 g of the above-mentioned expandable styrene-based resin particles were placed in a 2 L polybeaker equipped with a discharge part capable of collecting the overflowing liquid, and an aqueous solution obtained by mixing sodium dodecylbenzenesulfonate with 10 L of water to a concentration of 0.005 mass % was added to the above-mentioned polybeaker at a rate of 0.2 L per minute while stirring at 270 rpm with a stirring device. The stirring caused the liquid level to rise from the center toward the periphery, and the liquid overflowed from the bottom end of the discharge part was passed through a wire mesh with 0.3 mm openings, and 6 L of the passed liquid was collected. The collected permeate was filtered by suction using a GLASS FIBER FILTER (product name: Glass filter paper GA-200, size: 125 mm) manufactured by Advantec Toyo Co., Ltd., and the substance remaining on the filter paper was used as the attachment. This attachment was dried in a constant temperature environment of 60° C. for 24 hours, and the mass was measured.

2. 2. The expandable styrene-based resin particles according to claim 1, wherein the additive comprises at least one selected from the group consisting of resin powder, a dispersant, and a surface additive.

3. The expandable styrene-based resin particles according to claim 1 , which are obtained by impregnating a styrene-based resin with a blowing agent to obtain expandable particles, and washing the resulting particles with water.

4. A pre-expanded styrene-based resin particle obtained by pre-expanding the expandable styrene-based resin particle according to any one of claims 1 to 3, The bulk expansion ratio of the pre-expanded foam is 2 to 150 times. Pre-expanded styrene-based resin particles.

5. A styrene-based resin foamed article produced from the expandable styrene-based resin particles according to any one of claims 1 to 3.

6. A styrene-based resin foamed article produced from the pre-expanded styrene-based resin particles according to claim 4.

Citation Information

Patent Citations

  • Voice recognition equipment

    JP1987023097A

  • Polystyrene-based foamed molding, production method thereof, and foamed resin-made container

    JP2014070150A