Thermosetting resin compound
A thermosetting resin compound with a bismaleimide composition and additives achieves high glass transition temperature and heat resistance, addressing strength and durability issues in inductor sealing, particularly for inductor exteriors and coils.
Patent Information
- Application Number
- JP2023046482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Thermosetting resins used for sealing electronic components like inductors suffer from a significant decrease in strength due to phase transition above the glass transition temperature, necessitating materials with higher glass transition temperatures for improved thermal durability and resistance to magnetic material deterioration.
A thermosetting resin compound comprising a bismaleimide composition, a curing agent, a catalyst, a mold release agent, a coupling agent, and a soft magnetic powder, which results in a cured product with a glass transition temperature of 250°C or higher.
The resin compound achieves high glass transition temperature and heat resistance, suitable for sealing inductor exteriors and coils, maintaining strength and magnetic properties even in high-temperature environments.
Smart Images

Figure 2024135680000001 
Figure 2024135680000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin compound. [Background technology]
[0002] For example, in electronic components such as inductors, coils are sealed with thermosetting resin to protect them from the external environment. However, although thermosetting resins have excellent heat resistance, they undergo a phase transition from the glass region to the rubber region in environments where the glass transition temperature is exceeded, resulting in a significant decrease in strength. Therefore, in terms of the thermal durability of inductors, materials that exhibit a high glass transition temperature are required.
[0003] A possible solution to the above problems is to use a resin with high heat resistance. An example of such a resin with high heat resistance is a bismaleimide compound available on the market. Patent Document 1 discloses that a bismaleimide compound is dissolved in a solvent and used. Patent Document 1 describes that both solvent solubility and solution stability are improved by melting a resin mixture containing a bismaleimide compound at 150°C or higher and 210°C or lower.
[0004] In addition, magnetic materials are sometimes added to electronic components such as inductors. Patent Document 2 discloses a magnetic material that has excellent long-term heat resistance in a high-temperature environment. There is a relationship between the long-term heat resistance and the glass transition temperature in a cured product of a thermosetting resin, and it is said that when the cured product contains a magnetic material, the magnetic material is likely to deteriorate in a temperature environment above the glass transition temperature of the cured product. From the viewpoint of preventing such deterioration of the magnetic material, a material with a higher glass transition temperature is desired.
[0005] Patent Document 3 discloses a resin composition for printed wiring boards obtained by melting a resin mixture containing (A) a bismaleimide compound, (B) benzoxazine, (C) an epoxy resin, and (D) a coumarone resin. Patent Document 3 aims to provide a resin composition that has high heat resistance and low dielectric properties (low relative dielectric constant, low dielectric tangent) and is used as a laminate, printed wiring board, adhesive, sealant, paint, molded product, etc. in electronic and electric parts. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent Publication No. 2020-26509 [Patent Document 2] Patent No. 7133114 [Patent Document 3] Patent No. 6946578 Summary of the Invention [Problem to be solved by the invention]
[0007] In view of the above circumstances, the present inventors have conducted intensive research and found that the use of a thermosetting resin compound having a specific composition results in a cured product having a high glass transition temperature. An object of the present invention is to provide a thermosetting resin compound that provides a cured product having a high glass transition temperature and high heat resistance. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to solve the above problems, and have found that a thermosetting resin compound obtained by melt-mixing a bismaleimide composition, a curing agent, a catalyst, a release agent, a coupling agent, and a soft magnetic powder exhibits a high glass transition temperature.
[0009] [1] A thermosetting resin compound comprising: The thermosetting resin compound comprises a bismaleimide composition, a curing agent, a catalyst, a release agent, a coupling agent and a soft magnetic powder, and a cured product of the thermosetting resin compound has a glass transition temperature of 250°C or higher as measured by a TMA method. [2] The thermosetting resin compound according to [1], wherein the curing agent comprises a phenolic resin. [3] The thermosetting resin compound according to [1] or [2], wherein the soft magnetic powder is a metal powder whose main component is iron. [4] The thermosetting resin compound according to any one of [1] to [3], which is a thermosetting resin compound for sealing an inductor exterior. [5] The thermosetting resin compound according to any one of [1] to [4], which is used as an exterior material for a coil in an inductor. Effect of the Invention
[0010] The thermosetting resin compound of the present invention has a high glass transition temperature and high heat resistance when cured. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The thermosetting resin compound of the present invention will now be described.
[0012] The thermosetting resin compound of the present invention comprises: The present invention includes a bismaleimide composition, a curing agent, a catalyst, a release agent, a coupling agent, and a soft magnetic powder. The thermosetting resin compound has a cured product having a glass transition temperature of 250° C. or higher as measured by a TMA method.
[0013] (hardening agent) The curing agent is not particularly limited, but from the viewpoints of heat resistance and easy availability on the market, a phenolic resin is preferable, and a phenolic novolac resin is particularly preferable. As such a phenolic resin, any resin that is used as a curing agent for an epoxy resin molding material can be used as long as it is classified as a general phenolic resin.
[0014] The content of the curing agent in the entire thermosetting resin compound excluding the soft magnetic powder is not particularly limited, but is preferably 3 to 35% by weight, more preferably 5 to 25% by weight, and most preferably 10 to 15% by weight.
[0015] (catalyst) In the thermosetting resin compound of the present invention, by blending a catalyst (curing accelerator), the reaction during heating of the resin compound can be accelerated, and the molding time can be shortened. The catalyst is not particularly limited, but includes imidazoles, amines, metal salts, ureas such as diureas, and phosphorus-based catalysts. Among these, ureas are preferred from the viewpoint of storage stability at room temperature, and 3-(3,4-dichlorophenyl)-1,1-dimethylurea and diureas are particularly preferred.
[0016] The content of the catalyst in the entire thermosetting resin compound excluding the soft magnetic powder is not particularly limited, but is preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and most preferably 1 to 3% by weight. By keeping the catalyst content within the above range, it is possible to promote curing while suppressing the effect on the glass transition temperature.
[0017] (Release agent) The release agent is not particularly limited, and those generally used in epoxy resin compositions can be used. Representative examples of the release agent include carnauba wax such as carnauba wax; esters of higher fatty acids such as montanic acid and stearic acid; partially saponified products of the above-mentioned esters of higher fatty acids; metal salts of higher fatty acids such as magnesium stearate, barium stearate, and aluminum stearate; and metal soaps such as zinc stearate. These may be used alone or in combination. Among the above-mentioned release agents, it is preferable to use partially saponified wax of montanic acid ester, carnauba wax, or a mixture thereof.
[0018] The content of the release agent in the entire thermosetting resin compound excluding the soft magnetic powder is not particularly limited, but is preferably 1 to 15% by weight, more preferably 2 to 10% by weight, and most preferably 3 to 7% by weight.
[0019] (Coupling Agent) Examples of coupling agents include vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and N-2-(aminoethyl)-3-aminopropyltrimethoxysilane. These coupling agents can be used alone or in combination of two or more. Among the above coupling agents, it is preferable to use 3-glycidoxypropyltrimethoxysilane.
[0020] The content of the coupling agent in the entire thermosetting resin compound excluding the soft magnetic powder is not particularly limited, but is preferably 0.1 to 10% by weight, more preferably 0.5 to 5% by weight, and most preferably 1 to 3% by weight. By keeping the content of the coupling agent within the above range, it is possible to improve the adhesion between the resin component and the soft magnetic powder while suppressing the effect on the glass transition temperature.
[0021] (Soft magnetic powder) The soft magnetic powder is a component that imparts magnetism to the thermosetting resin compound and also functions as a filler. The soft magnetic powder is not particularly limited, but may be a metal powder mainly composed of iron. The soft magnetic powder may contain other elements such as C, Si, Cr, Fe, Cu, B, Nb, As, and O. The particle size of the soft magnetic powder is not particularly limited, but may be a median diameter of 1 to 100 μm. In order to improve the packing rate of the compound by closest packing, a combination of soft magnetic powders having different particle sizes may be used.
[0022] The soft magnetic powder can be mixed in an amount of preferably 100 to 5000 parts by weight, more preferably 1000 to 3000 parts by weight, per 100 parts by weight of the components of the thermosetting resin compound excluding the soft magnetic powder. The content of the soft magnetic powder in the entire thermosetting resin compound is not particularly limited, but is preferably 60 to 99% by weight, more preferably 75 to 97% by weight, and most preferably 90 to 95% by weight. From the viewpoint of improving the magnetic properties, it is preferable that the content of the soft magnetic powder is as high as possible, but it is also desirable to consider the fluidity during molding. By having the content of the soft magnetic powder within the above numerical range, it is easy to balance the magnetic properties and the fluidity during molding, and this balance is particularly easy to achieve when the content is 90 to 95% by weight.
[0023] (Other ingredients) The thermosetting resin compound may also contain other components, such as colorants, stress relief agents, etc., either singly or in combination.
[0024] (Melt Viscosity) The melt viscosity of the thermosetting resin compound is not particularly limited, but is preferably 300 Pa·s or less, more preferably 200 Pa·s or less, and most preferably 150 Pa·s or less. The melt viscosity of the thermosetting resin compound can also be 5 Pa·s or more, 10 Pa·s or more, or 15 Pa·s or more. The above numerical ranges of the melt viscosity of the thermosetting resin compound can be combined in any combination. If the melt viscosity of the thermosetting resin compound is 300 Pa·s or less, it will flow easily in the mold, reducing the rate of unfilled parts in the mold. The melt viscosity of the thermosetting resin compound can be measured according to the conditions, procedures and methods described in <Evaluation of Thermosetting Resin Compound> in the [Examples] below.
[0025] (glass transition temperature) The glass transition temperature of the cured product of the thermosetting resin compound as measured by the TMA method is 250° C. or higher, preferably 260° C. or higher, more preferably 270° C. or higher, and most preferably 280° C. or higher. The glass transition temperature of the cured product of the thermosetting resin compound as measured by the TMA method can also be 500° C. or lower, 400° C. or lower, or 300° C. or lower. The above numerical ranges of the glass transition temperature of the thermosetting resin compound as measured by the TMA method can be combined in any desired manner. Since the thermosetting resin compound has a glass transition temperature of 250°C or higher as measured by the TMA method, the cured product has high heat resistance. The glass transition temperature of the thermosetting resin compound by the TMA method can be measured according to the conditions, procedures, and methods described in <Evaluation of Thermosetting Resin Compound> in [Examples] below. The glass transition temperature of the thermosetting resin compound by the TMA method can be the glass transition temperature of the "molded product after additional curing" described in <Evaluation of Thermosetting Resin Compound> in [Examples] below.
[0026] (Method of manufacturing thermosetting resin compound) A thermosetting resin compound can be produced by further adding a curing agent, a catalyst, a release agent, a coupling agent and a soft magnetic powder to the bismaleimide composition, mixing and stirring the mixture, and molding the mixture into a predetermined shape such as granules. The equipment such as a mixer used to mix the components and the mixing conditions are not particularly limited, and the same equipment and conditions as those used in the production of conventional thermosetting resin compounds can be used.
[0027] (Application) The thermosetting resin compound is preferably a thermosetting resin compound for sealing an inductor exterior, and is particularly preferably used as an exterior material for a coil in an inductor. In the case of exterior sealing of coils contained in inductors, etc., a method of molding a solvent-free thermosetting resin composition by compression molding or transfer molding has been preferably used from the viewpoint of productivity. The thermosetting resin compound of the present invention can be used in compression molding or transfer molding like conventional thermosetting resin compositions, and is suitable as a thermosetting resin compound having a high glass transition temperature and suitable for magnetic-related parts such as inductors containing soft magnetic powder. EXAMPLES
[0028] The present invention will be experimentally described by the following examples, but the following description is not intended to limit the scope of the present invention to the following examples.
[0029] The commercially available products used in the practice of the present invention are listed below. <Bismaleimide composition> Bismaleimide resin: HR-3070 (manufactured by Printec Co., Ltd.) <Epoxy resin> Bisphenol A epoxy resin: jER-1001 (manufactured by Mitsubishi Chemical Corporation) Triphenylmethane type epoxy resin: TECHMORE VG3101L (manufactured by Printec Co., Ltd.) -Tetrafunctional epoxy resin (softening point: 89°C): HP-4700 (DIC Corporation)
[0030] <Hardening agent> Phenol novolac resin: H-1 (UBE Corporation) <Catalyst> Diurea catalyst: U-CAT 3512T (manufactured by San-Apro Co., Ltd.) <Release agent> Partially saponified wax of montanic acid ester: RICOWAX (registered trademark) OP (manufactured by Clariant Japan Co., Ltd.) Carnauba wax: Carnauba Special No.1 (manufactured by Kato Yoko Co., Ltd.) <Coupling Agent> 3-Glycidoxypropyltrimethoxysilane: KBM-403 (Shin-Etsu Chemical Co., Ltd.) <Soft magnetic powder> Amorphous magnetic powder (coarse powder): KUAMET6B2 -53μm (Epson Atmix Corporation) Amorphous magnetic powder (fine powder): AW2-08 PF-8F (manufactured by Epson Atmix Corporation)
[0031] <Preparation of Thermosetting Resin Compounds of Example 1 and Comparative Examples 1 to 3> The bismaleimide composition (Example 1) or each epoxy resin (Comparative Examples 1 to 3) shown in Table 1, as well as the above-mentioned catalyst, release agent, coupling agent, and soft magnetic powder (filler) were charged into a Henschel mixer and uniformly dispersed to obtain a dispersion, so that the weight parts of each component were as shown in Table 1 below. In the obtained dispersion, each component was physically dispersed without being melted. The dispersion obtained as described above was mixed for 1 minute at 120°C and 130 rpm using a Labo Plastomill (manufactured by Toyo Seiki Seisakusho Co., Ltd.) to obtain a kneaded product. The kneaded product (high temperature clay-like) was collected in a tray, cooled to room temperature, and then pulverized into granules using an impact pulverizer (manufactured by Dalton Co., Ltd.) to obtain the thermosetting resin compounds of Example 1 and Comparative Examples 1 to 3.
[0032] Then, the content (wt %) of the soft magnetic powder (corresponding to the filler) relative to the total amount of the thermosetting resin compound was calculated for Example 1 and Comparative Examples 1 to 3. The results are shown in Table 1. Furthermore, the content (wt %) of each component relative to the total amount of the components other than the soft magnetic powder in the thermosetting resin compound was calculated for Example 1 and Comparative Examples 1 to 3. The results are shown in Table 2.
[0033] <Evaluation of Thermosetting Resin Compounds> The following evaluations 1. and 2. were carried out for each of the thermosetting resin compounds of Example 1 and Comparative Examples 1 to 3. The results are shown in Table 1.
[0034] 1. Melt Viscosity For each thermosetting resin compound, the melt viscosity (Pa s) was measured using a flow tester (CFT-500EX, Shimadzu Corporation) under the following conditions: temperature 180°C, test load 50 kgf, die hole diameter 1 mm × depth 1 mm, and preheating for 20 seconds. A thermosetting resin compound with a low melt viscosity is preferred because it flows easily in a mold and reduces the rate of unfilled parts in the mold.
[0035] 2. Glass transition temperature <Creating molded objects> 7 g of each thermosetting resin compound was taken and compressed in a compression molding machine at a temperature of 180°C and a gauge pressure of 60 kg / cm. 2 The mixture was then held at room temperature for 4 minutes to obtain a square prism-shaped cured product (height: 80 mm, bottom surface (cross section): 10 mm x 4 mm). This cured product is referred to as the "molded product before additional curing." The square prism-shaped cured product obtained in the same manner as above was further cured at 250°C for 3 hours in a hot air dryer to obtain a molded product, which is referred to as the "molded product after additional curing." <Evaluation of heat resistance> The molded product before and after the additional curing was cut to a desired size, and the glass transition temperature was measured by the TMA method using DL-9600 manufactured by Advance Riko Co., Ltd. A molded product with a high glass transition temperature is preferred because it has excellent heat resistance.
[0036] [Table 1]
[0037] [Table 2]
[0038] Example 1 relates to a thermosetting resin compound containing a bismaleimide composition, a curing agent, a catalyst, a release agent, a coupling agent, and a soft magnetic powder, while Comparative Examples 1 to 3 relate to thermosetting resin compounds containing an epoxy resin, a curing agent, a catalyst, a release agent, a coupling agent, and a soft magnetic powder but not a bismaleimide composition.
[0039] As shown in Table 1, it was found that the molded product of Example 1 after additional curing had a higher glass transition temperature and higher heat resistance than the molded products based on the epoxy resins of Comparative Examples 1 to 3. Furthermore, the thermosetting resin compound of Example 1 did not show a significant change in resin fluidity (melt viscosity) when compared with the thermosetting resin compounds of Comparative Examples 1 to 3, and was found to have properties at a practical level.
[0040] From the above, the thermosetting resin compound of the present invention, which contains the bismaleimide composition, curing agent, catalyst, release agent, coupling agent and soft magnetic powder, has a cured product with a high glass transition temperature and high heat resistance. [Industrial Applicability]
[0041] The thermosetting resin compound of the present invention can be used in electronic and electric parts as a sealing molding compound for the exterior parts of electronic parts such as inductors, by compression molding or transfer molding.
Claims
1. A thermosetting resin compound, comprising: The present invention includes a bismaleimide composition, a curing agent, a catalyst, a release agent, a coupling agent, and a soft magnetic powder. The thermosetting resin compound, wherein a cured product of the thermosetting resin compound has a glass transition temperature of 250° C. or higher as measured by a TMA method.
2. The thermosetting resin compound of claim 1 , wherein the curing agent comprises a phenolic resin.
3. 3. The thermosetting resin compound according to claim 1, wherein the soft magnetic powder is a metal powder containing iron as a main component.
4. 3. The thermosetting resin compound according to claim 1, which is a thermosetting resin compound for sealing an inductor exterior.
5. 3. The thermosetting resin compound according to claim 1, which is used as an exterior material for a coil in an inductor.
Citation Information
Patent Citations
Resin composition and method for producing the same
JP2020026509A
Resin composition and method for producing same
JP6946578B2
Magnetic materials and magnetic elements
JP7133114B1