Laminate film
A laminated film with a 4-methyl-1-pentene polymer base layer and a specific resin composition sealant layer addresses the challenges of high heat-sealing temperatures and low gas permeability, providing enhanced adhesive strength, transparency, and reduced content adhesion.
Patent Information
- Application Number
- JP2023046513
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
4-methyl-1-pentene polymers have high heat resistance, leading to high heat-sealable temperature requirements in laminated films, while using other polymers for lower temperatures results in low gas permeability, and there are issues with adhesive strength and transparency between layers, as well as content adhesion to the inside of packaging bags.
A laminated film structure comprising a base layer made of 4-methyl-1-pentene polymer and a sealant layer containing a specific blend of 4-methyl-1-pentene polymer and copolymer, optimized for intrinsic viscosity, melting point, density, and critical surface tension, ensuring high gas permeability, transparency, and mold releasability.
The laminated film achieves heat sealing performance, high gas permeability, transparency, and mold releasability, with improved adhesive strength and reduced content adhesion, making it suitable for various packaging applications.
Smart Images

Figure 2024135701000001 
Figure 2024135701000002 
Figure 2024135701000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated film. [Background technology]
[0002] 4-methyl-1-pentene polymers have bulky functional groups and therefore have a lower density than other polyolefins. Therefore, films containing 4-methyl-1-pentene polymers have high gas permeability for oxygen, carbon dioxide, and the like, and have been developed as non-porous gas permeable films for packaging plants, fresh foods, and the like. For example, Patent Document 1 proposes a packaging bag for bulbs obtained by molding a resin composition containing a 4-methyl-1-pentene polymer and a butene-1 polymer.
[0003] On the other hand, 4-methyl-1-pentene polymers are known to have a high melting point and good releasability, and a film mainly composed of 4-methyl-1-pentene polymers (hereinafter sometimes referred to as "4-methyl-1-pentene polymer film") requires a high heat seal temperature and has low heat seal strength. Therefore, as a method for improving the heat sealability of 4-methyl-1-pentene polymer films, a method of laminating a film composed of another thermoplastic resin such as a polyolefin polymer (hereinafter sometimes referred to as a "polyolefin polymer film") onto the 4-methyl-1-pentene polymer film has been investigated (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-301691 [Patent Document 2] JP 2000-189051 A Summary of the Invention [Problem to be solved by the invention]
[0005] As described above, 4-methyl-1-pentene polymers have high heat resistance. However, due to the high heat resistance, when a film containing a 4-methyl-1-pentene polymer is used as a heat-sealable laminate film, particularly as a sealant layer of the laminate film, there is a problem that the heat-sealable temperature range becomes a relatively high temperature range. On the other hand, when a resin film other than a 4-methyl-1-pentene polymer is used as a sealant layer to expand the heat-sealable temperature range to a lower temperature side, the gas permeability of the resin film tends to be low, and there is also a problem that it is difficult to obtain a heat-sealable laminate film that makes use of the excellent gas permeability of the 4-methyl-1-pentene polymer.
[0006] Although the film and packaging bag described in Patent Document 2 allow for some adjustment of the gas permeability characteristic of the 4-methyl-1-pentene polymer film, depending on the application, the adhesive strength between the 4-methyl-1-pentene polymer film and the polyethylene polymer film or polypropylene polymer film laminated thereon may be insufficient. In addition, since the packaging bag has a polyethylene polymer film or polypropylene laminated on the inside, depending on the application, improvement in the transparency of the package may be required. Furthermore, in the packaging bag described in Patent Document 2, when the contents are filled in the packaging bag, the contents tend to adhere to the inside of the packaging bag, so there is room for improvement in this respect.
[0007] One method for preventing the contents from adhering to the inside of a packaging bag is, for example, embossing the surface of a film that will be on the inside of the packaging bag during molding. However, the surface of an embossed film generally has an uneven shape and is therefore less smooth, and the transparency of the film tends to be reduced due to light scattering.
[0008] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a laminated film that combines heat sealability, high gas permeability, transparency, and releasability. [Means for solving the problem]
[0009] Means for solving the above-mentioned problems relate to, for example, the following items [1] to [3].
[0010] [1] A laminated film having a base layer (X) and a sealant layer (Y) laminated on one side of the base layer (X), The base layer (X) contains a 4-methyl-1-pentene polymer (A) that satisfies the following requirements (Aa) to (Ad), The sealant layer (Y) is a laminated film made of a resin composition (Z) containing 5 to 25 parts by mass of the 4-methyl-1-pentene polymer (A) and 75 to 95 parts by mass of a 4-methyl-1-pentene copolymer (B) satisfying the following requirements (Ba) to (Bd) (the total of the 4-methyl-1-pentene polymer (A) and the 4-methyl-1-pentene copolymer (B) being 100 parts by mass). Requirement (Aa): The amount of structural units (i) derived from 4-methyl-1-pentene is 90 to 100 mol %, and the total amount of structural units (ii) derived from α-olefins having 5 to 20 carbon atoms (excluding 4-methyl-1-pentene) is 0 to 10 mol % (with the sum of structural units (i) and structural units (ii) being 100 mol %). Requirement (Ab): The intrinsic viscosity [η] measured in decalin at 135°C is in the range of 0.5 to 5.0 dl / g. Requirement (Ac): The melting point (Tm) measured by differential scanning calorimetry (DSC) is in the range of 200 to 250°C. Requirement (Ad): Density 820-860kg / m 3 is in the range. Requirement (Ba): The amount of structural units (iii) derived from 4-methyl-1-pentene is 60 to 90 mol %, and the total amount of structural units (iv) derived from an α-olefin having 2 to 4 carbon atoms is 10 to 40 mol % (provided that the total of structural units (iii) and structural units (iv) is 100 mol %). Requirement (Bb): The intrinsic viscosity [η] measured in decalin at 135°C is in the range of 0.5 to 5.0 dl / g. Requirement (Bc): The melting point (Tm) measured by differential scanning calorimetry (DSC) is not observed or is in the range of less than 160°C. Requirement (Bd): Density is 820-860kg / m 3 is in the range.
[0011] [2] The laminate film according to [1], wherein when the sealant layers (Y) are heat-sealed together under conditions of a temperature of 200°C, a pressure of 0.2 MPa, and a sealing time of 2 seconds, the peel strength of the sealant layer (Y) is 2.0 N / 15 mm or more.
[0012] [3] The laminated film according to [1] or [2], wherein the critical surface tension of the sealant layer (Y) at a temperature of 23° C. is 20 to 26 mN / m. Effect of the Invention
[0013] According to the present invention, a laminated film having excellent heat sealability, high gas permeability, transparency, and releasability can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Specific embodiments of the present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be implemented with appropriate modifications within the scope of the present invention.
[0015] In this specification, a range of numerical values expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. In this specification, when referring to the amount of each component in a composition, if multiple substances corresponding to each component are present in the composition, the amount means the total amount of multiple substances present in the composition, unless otherwise specified.
[0016] <Laminated film> The laminated film of the present invention has a base layer (X) and a sealant layer (Y) laminated on one side of the base layer (X). The base layer (X) contains a specific 4-methyl-1-pentene polymer (A). The sealant layer (Y) is made of a resin composition (Z) containing the 4-methyl-1-pentene polymer (A) and a specific 4-methyl-1-pentene copolymer (B).
[0017] <4-methyl-1-pentene polymer (A)> The 4-methyl-1-pentene polymer (A) (hereinafter sometimes abbreviated as "polymer (A)") is included in the base layer (X) of the laminate film of the present invention, and is also included in the sealant layer (Y) of the laminate film of the present invention. The polymer (A) satisfies the following requirements (Aa) to (Ad), and preferably satisfies one or more of the requirements (Ae) and (Af) in addition to the requirements (Aa) to (Ad).
[0018] [Requirements (Aa)] The amount of structural unit (i) derived from 4-methyl-1-pentene in polymer (A) is 90 to 100 mol %, preferably 91.0 to 99.5 mol %, and more preferably 92.0 to 99.0 mol % (wherein the total of structural unit (i) and structural unit (ii) is 100 mol %). Furthermore, the total amount of structural units (ii) derived from an α-olefin having 5 to 20 carbon atoms (excluding 4-methyl-1-pentene) in polymer (A) is 0 to 10 mol %, preferably 0.5 to 9.0 mol %, and more preferably 1.0 to 8.0 mol % (wherein the total of structural units (i) and structural units (ii) is 100 mol %).
[0019] When the content of the structural unit (i) in the polymer (A) is 90 mol% or more, the gas permeability of the base layer (X) containing the polymer (A) is high, and the transparency of the base layer (X) is also high. Furthermore, since the polymer (A) is also contained in the resin composition (Z) used to form the sealant layer (Y), when the content of the structural unit (i) contained in the polymer (A) is 90 mol% or more, the sealant layer (Y) also tends to be excellent in both gas permeability and transparency. As a result, when the content of the structural unit (i) contained in the polymer (A) is 90 mol% or more, the entire laminate film in which the base layer (X) and the sealant layer (Y) are laminated tends to be excellent in both gas permeability and transparency.
[0020] The 4-methyl-1-pentene from which the structural unit (i) is derived may be solely 4-methyl-1-pentene obtained from a biomass-derived raw material, or may be a mixture of 4-methyl-1-pentene obtained from a biomass-derived raw material and 4-methyl-1-pentene derived from a fossil fuel, or may be solely 4-methyl-1-pentene derived from a fossil fuel.
[0021] Examples of the α-olefin having 5 to 20 carbon atoms other than 4-methyl-1-pentene that forms the structural unit (ii) include 1-hexene, 1-heptene, 1-octene, 1-decene, 1-tetradecene, 1-hexadecene, 1-heptadecene, 1-octadecene, and 1-eicosene, etc. The α-olefin having 5 to 20 carbon atoms may be only α-olefins obtained from a biomass-derived raw material, may be a mixture of α-olefins obtained from a biomass-derived raw material and α-olefins derived from a fossil fuel, or may be only α-olefins derived from a fossil fuel.
[0022] As the α-olefin forming the structural unit (ii), from the viewpoint of exhibiting high gas permeability and transparency in the base layer (X) and sealant layer (Y) containing the polymer (A), an α-olefin having 8 to 18 carbon atoms (for example, 1-octene, 1-decene, 1-tetradecene, 1-hexadecene, 1-heptadecene, and 1-octadecene) is preferred. These can be used alone or in combination of two or more.
[0023] The polymer (A) may contain other structural units other than the structural unit (i) derived from 4-methyl-1-pentene and the structural unit (ii) derived from an α-olefin other than 4-methyl-1-pentene, within a range that does not impair the effects of the present invention. The content of the other structural units is, for example, 0 to 10 mol% (wherein the total content of the structural units (i) and (ii) is 100 mol%).
[0024] The content (mol%) of the structural unit in the polymer (A) was determined by carbon-13 nuclear magnetic resonance (hereinafter, 13 The value is calculated by a measurement method using 1H-C NMR. The specific measurement method is as described in the Examples below.
[0025] [Requirements (Ab)] The polymer (A) has an intrinsic viscosity [η] measured in decalin solvent at 135°C in the range of 0.5 to 5.0 dl / g, preferably 0.6 to 4.0 dl / g, more preferably 0.8 to 3.0 dl / g. When the intrinsic viscosity [η] of the polymer (A) is in the above-mentioned range, the amount of low molecular weight components is small, so that both the base layer (X) and the sealant layer (Y) containing the polymer (A) tend to be less sticky and easier to mold. As a result, the laminated film according to the present invention having the base layer (X) and the sealant layer (Y) also tends to be less sticky and easier to mold. The specific method for measuring the intrinsic viscosity [η] is as described in the Examples below.
[0026] [Requirements (Ac)] The polymer (A) has a melting point (Tm) measured by a differential scanning calorimeter (DSC) in the range of 200 to 250°C, preferably 205 to 245°C, more preferably 210 to 240°C. If the melting point of the polymer (A) is within the above range, both the base layer (X) and the sealant layer (Y) containing the polymer (A) tend to be easily molded, and as a result, the laminated film according to the present invention is easily molded. Furthermore, if the melting point of the polymer (A) is within the above range, both the base layer (X) and the sealant layer (Y) containing the polymer (A) have relatively high heat resistance, so that the laminated film has appropriate heat resistance. The method for measuring the melting point is as described in the Examples below.
[0027] The melting point of the polymer (A) varies depending on the stereoregularity of the polymer (A) and the α-olefin from which the copolymerized structural unit (ii) is derived. The melting point can be adjusted by using an olefin polymerization catalyst described below and further adjusting the composition of the polymer (A) to the desired range.
[0028] [Requirements (Ad)] The polymer (A) has a density of 820 to 860 kg / m 3 , preferably 825 to 855 kg / m 3 , more preferably 830 to 850 kg / m 3 When the density of the polymer (A) is within the above range, the gas permeability is good in both the base layer (X) and the sealant layer (Y) containing the polymer (A), and as a result, the laminate film according to the present invention containing the base layer (X) and the sealant layer (Y) is expected to have high gas permeability. The method for measuring the density of the polymer (A) is as described in the Examples below.
[0029] [Requirements (Ae)] The melt flow rate (MFR) of the polymer (A) measured according to ASTM D1238 under conditions of a temperature of 260°C and a load of 5.0 kgf is not particularly limited, but is preferably 0.1 to 100 g / 10 min, more preferably 0.5 to 50 g / 10 min, and even more preferably 1.0 to 40 g / 10 min, from the viewpoint of fluidity during molding of the base layer (X) and the sealant layer (Y) containing the polymer (A). In addition, when the melt flow rate of the polymer (A) is within the above range, the thickness of the base layer (X) and the sealant layer (Y) containing the polymer (A) can be easily maintained uniform during molding, and as a result, a laminated film having a uniform thickness can be easily molded. In addition, when the MFR of the polymer (A) is within the above range, the 4-methyl-1-pentene copolymer (B) described below and the polymer (A) can be easily mixed by melt kneading, and the resin composition (Z) obtained by mixing can be easily molded.
[0030] Requirements In the film formed from the polymer (A), the critical surface tension at 23° C. obtained using the Zisman plot is preferably 20 to 26 mN / m, more preferably 21 to 25 mN / m. The forming conditions for the polymer (A) are arbitrary, but for example, the same conditions as those for producing the laminated film described below can be used.
[0031] Here, in the method of calculating the critical surface tension of a solid by the Zisman plot, the contact angle of the solid with respect to various liquids with different surface tensions is measured, and a graph is drawn with the surface tension of each liquid on the horizontal axis and the measured contact angle (cosθ) of the solid on the vertical axis. Since the graph obtained can be approximated to a straight line, the line obtained by approximation is extrapolated to cosθ=1.0, which is considered to be a completely wet state, and the value of the surface tension when cosθ=1.0 on the straight line (i.e., the value on the horizontal axis at the point where cosθ=1.0 on the straight line) is taken as the critical surface tension (mN / m) of the solid. Details of the measurement conditions, etc. are as described in the examples below.
[0032] The critical surface tension of other general polyolefins at 23°C is, for example, 31 to 35 mN / m for polypropylene and 28 to 32 mN / m for polyethylene, so the polymer (A) has a lower critical surface tension than other general polyolefins. The critical surface tension is an index of the degree of releasability, and the smaller the critical surface tension, the higher the releasability tends to be. Therefore, when the critical surface tension of the film formed from the polymer (A) is within the above range, the releasability of the base layer (X) and the sealant layer (Y) containing the polymer (A) tends to be good. Incidentally, when a packaging bag is produced from a laminated film having a base layer (X) and a sealant layer (Y) by heat sealing, the sealant layer (Y) is often on the inside of the packaging bag and in contact with the contents. In addition, since substances are less likely to adhere to the surface of a film with excellent releasability, a laminated film having a sealant layer (Y) produced using a polymer (A) having a critical surface tension (23°C) of 20 to 26 mN / m can be used to produce a packaging bag in which the contents are less likely to adhere to the inside of the packaging bag and the contents are less likely to remain when the contents are discharged (so-called good releasability).
[0033] <Method for producing polymer (A)> The polymer (A) may be produced by polymerizing 4-methyl-1-pentene and, if necessary, an α-olefin having 5 to 20 carbon atoms (excluding 4-methyl-1-pentene), or by pyrolyzing a high molecular weight 4-methyl-1-pentene polymer. The polymer (A) may be purified by a method such as solvent fractionation, which separates the polymer based on the difference in solubility in a solvent, or molecular distillation, which separates the polymer based on the difference in boiling point.
[0034] The 4-methyl-1-pentene polymer used as the polymer (A) can be obtained by polymerizing 4-methyl-1-pentene and, if necessary, an α-olefin having 5 to 20 carbon atoms (excluding 4-methyl-1-pentene) using a conventionally known olefin polymerization catalyst, for example, a vanadium-based catalyst, a titanium-based catalyst, a magnesium-supported titanium-based catalyst, or a metallocene catalyst described in WO 01 / 53369, WO 01 / 27124, WO 2006 / 054613, JP-A 3-193796, or JP-A 2-41303.
[0035] Also, a commercially available 4-methyl-1-pentene polymer can be used as the polymer (A). An example of a commercially available product that can be used as the polymer (A) is TPX (registered trademark) manufactured by Mitsui Chemicals, Inc. Note that when producing the polymer (A) by pyrolyzing a high molecular weight 4-methyl-1-pentene polymer, a commercially available product may be used as the high molecular weight 4-methyl-1-pentene polymer that is the raw material.
[0036] <4-Methyl-1-pentene-α-olefin polymer (B)> The resin composition (Z) constituting the sealant layer (Y) of the laminated film of the present invention contains the polymer (A) and a 4-methyl-1-pentene copolymer (B) (hereinafter, sometimes abbreviated as "copolymer (B)"). The copolymer (B) is a copolymer of 4-methyl-1-pentene and an α-olefin, and satisfies the following requirements (Ba) to (Bd). Preferably, the copolymer (B) satisfies one or more of the requirements (Be) to (Bh) in addition to the following requirements (Ba) to (Bd).
[0037] [Requirements (Ba)] The amount of the structural unit (iii) derived from 4-methyl-1-pentene in the copolymer (B) is 60 to 90 mol %, preferably 65 to 89 mol %, more preferably 68 to 88 mol %, and even more preferably 70 to 87 mol % (wherein the total of the structural units (iii) and (iv) is 100 mol %). Furthermore, the total amount of structural units (iv) derived from an α-olefin having 2 to 4 carbon atoms in copolymer (B) is 10 to 40 mol %, preferably 11 to 35 mol %, more preferably 12 to 32 mol %, and even more preferably 13 to 30 mol % (wherein the total of structural units (iii) and structural units (iv) is 100 mol %).
[0038] When the content of the structural unit (iii) in the copolymer (B) is 90 mol % or less (i.e., the content of the structural unit (iv) is 10 mol % or more), the adhesive strength of the sealant layer (Y) containing the copolymer (B) is relatively high, and as a result, in the laminated film of the present invention, an adhesive strength sufficient to prevent layer peeling between the base layer (X) and the sealant layer (Y) is obtained, which is preferable. Furthermore, when the content of the structural unit (iii) in the copolymer (B) is 60 mol % or more, the releasability of the resin composition (Z) containing the copolymer (B) is good, and as a result, the laminated film can exhibit releasability.
[0039] Furthermore, when the content of the structural unit (iv) in the copolymer (B) is 10 mol % or more, good compatibility is obtained between the polymer (A) and the copolymer (B) used in the resin composition (Z).
[0040] Examples of the α-olefin having 2 to 4 carbon atoms forming the structural unit (iv) include ethylene, propylene, and 1-butene. These can be used alone or in combination of two or more types within the scope of the present invention. Propylene is preferred as the α-olefin having 2 to 4 carbon atoms forming the structural unit (iv) because it has good compatibility with the polymer (A) used in the resin composition (Z).
[0041] The 4-methyl-1-pentene from which the structural unit (iii) in the copolymer (B) is derived may be solely 4-methyl-1-pentene obtained from a biomass-derived raw material, may be a mixture of 4-methyl-1-pentene obtained from a biomass-derived raw material and 4-methyl-1-pentene derived from a fossil fuel, or may be solely 4-methyl-1-pentene derived from a fossil fuel. Similarly, the α-olefin having 2 to 4 carbon atoms from which the structural unit (iv) in the copolymer (B) is derived may be an α-olefin obtained from a biomass-derived raw material, or may be a mixture of an α-olefin obtained from a biomass-derived raw material and an α-olefin derived from a fossil fuel, or may be solely an α-olefin derived from a fossil fuel.
[0042] Copolymer (B) may contain other structural units besides the structural unit (iii) derived from 4-methyl-1-pentene and the structural unit (iv) derived from an α-olefin having 2 to 4 carbon atoms, as long as the effects of the present invention are not impaired. The content of the other structural units is, for example, 0 to 10 mol % (wherein the total content of the structural unit (iii) and the structural unit (iv) is 100 mol %).
[0043] The content (mol%) of the structural units in the copolymer (B) was measured by carbon-13 nuclear magnetic resonance (hereinafter, 13 The molecular weight distribution is calculated by a measurement method using C-NMR. The specific measurement method is as described later in the Examples section, similar to the case of the polymer (A).
[0044] [Requirements (Bb)] The copolymer (B) has an intrinsic viscosity [η] measured in decalin solvent at 135°C in the range of 0.5 to 5.0 dl / g, preferably 0.6 to 4.0 dl / g, more preferably 0.8 to 3.0 dl / g. When the intrinsic viscosity [η] of the copolymer (B) is in the above-mentioned range, the low molecular weight components in the copolymer (B) are small, so that the stickiness of the resin composition (Z) containing the copolymer (B) is easily reduced, and the molding of the sealant layer (Y) using the resin composition (Z) tends to be easy. As a result, the stickiness is also reduced in the laminated film according to the present invention having the sealant layer (Y), which is preferable because the molding of the laminated film is easy. The specific method for measuring the intrinsic viscosity [η] is as described in the Examples below, similar to the polymer (A). Since objects are less likely to adhere to the surface of a film with reduced stickiness, when the stickiness of the sealant layer (Y) is reduced, the contents are less likely to adhere to the inside of a packaging bag manufactured with the sealant layer (Y) on the inside, and as a result, the contents tend not to remain when discharged (so-called good release function). For this reason, a laminate film having a sealant layer (Y) as the outermost layer manufactured using the copolymer (B) having an intrinsic viscosity [η] within the above range can be used to manufacture a packaging bag in which the contents are less likely to remain when discharged.
[0045] [Requirements (Bc)] The copolymer (B) has a melting point (Tm) measured by a differential scanning calorimeter (DSC) that is not observed or is in a range of less than 160° C. When the copolymer (B) has a melting point, the upper limit is preferably 150° C. or less, more preferably 145° C. or less, and even more preferably 140° C. or less.
[0046] The melting point value of copolymer (B) varies depending on the stereoregularity of copolymer (B) and the α-olefin from which the copolymerized structural unit (iv) is derived. The above melting point value can be adjusted by using an olefin polymerization catalyst described later and further adjusting the composition of copolymer (B) to a desired range. The measurement method is the same as that of polymer (A) and is described in the examples described later.
[0047] [Requirements (Bd)] The copolymer (B) has a density of 820 to 860 kg / m 3 , preferably 825 to 855 kg / m 3 , more preferably 830 to 850 kg / m 3 The density of the copolymer (B) is preferably within the above range, since the sealant layer (Y) containing the copolymer (B) is likely to have high gas permeability, and a laminated film having high gas permeability is likely to be obtained. The density is measured in the same manner as the polymer (A) as described in the Examples below.
[0048] [Requirements (Be)] The molecular weight distribution (Mw / Mn) of the copolymer (B), which is the ratio of the weight average molecular weight (Mw) in terms of polystyrene to the number average molecular weight (Mn) in terms of polystyrene measured by gel permeation chromatography (GPC), is not particularly limited, but is preferably in the range of 1.0 to 4.0, more preferably 1.2 to 3.5, and even more preferably 1.5 to 3.0. When the molecular weight distribution (Mw / Mn) is 4.0 or less, the influence of low molecular weight and low stereoregularity polymers derived from the composition distribution is small, which is advantageous for the transparency of the sealant layer (Y) obtained from the resin composition (Z) containing the copolymer (B). The method for measuring the weight average molecular weight (Mw) and the number average molecular weight (Mn) is as described in the Examples below.
[0049] [Requirements (Bf)] The weight average molecular weight (Mw) of the copolymer (B) measured by gel permeation chromatography (GPC) is preferably 500 to 10,000,000, more preferably 1,000 to 5,000,000, and even more preferably 5,000 to 2,500,000, in terms of polystyrene. When the weight average molecular weight (Mw) is within the above range, the rigidity of the sealant layer (Y) obtained from the resin composition (Z) containing the copolymer (B) tends to be within a range suitable for the application of the laminate film of the present invention.
[0050] [Requirements (Bg)] The melt flow rate (MFR) of copolymer (B) measured according to ASTM D1238 under conditions of a temperature of 230°C and a load of 2.16 kgf is not particularly limited, but is preferably 0.1 to 100 g / 10 min, more preferably 0.5 to 50 g / 10 min, and even more preferably 1.0 to 30 g / 10 min, from the viewpoint of fluidity during molding of the sealant layer (Y) containing copolymer (B). In addition, when the melt flow rate of copolymer (B) is within the above range, it is easy to keep the thickness of the sealant layer (Y) containing copolymer (B) uniform during the production of a laminated film, and as a result, it is easy to mold a laminated film having a uniform thickness. In addition, when the MFR of copolymer (B) is within the above range, it is easy to mix copolymer (B) and polymer (A) by melt kneading during the production of resin composition (Z).
[0051] [Requirements (Bh)] In the film formed from the copolymer (B), the critical surface tension at 23° C. obtained using the Zisman plot is preferably 20 to 26 mN / m, more preferably 21 to 25 mN / m. The forming conditions for the polymer (B) are arbitrary, but for example, the same conditions as those for producing the laminated film described later can be used.
[0052] Since the copolymer (B) has a lower critical surface tension than other common polyolefins, when the critical surface tension of a film formed from the copolymer (B) is within the above range, the release properties of the sealant layer (Y) containing the copolymer (B) tend to be good. Since objects are less likely to adhere to the surface of a film with excellent releasability, when the sealant layer (Y) has good releasability, the contents are less likely to adhere to the inside of a packaging bag manufactured so that the sealant layer (Y) faces the inside. As a result, in a packaging bag manufactured so that the sealant layer (Y) obtained using the copolymer (B) having a critical surface tension within the above range faces the inside, the contents tend not to remain when the contents are discharged (so-called, the bag has good releasability).
[0053] <Method for producing copolymer (B)> The method for producing the copolymer (B) is not particularly limited. For example, the copolymer (B) can be produced by polymerizing 4-methyl-1-pentene and the above-mentioned α-olefin having 2 to 4 carbon atoms in the presence of a suitable polymerization catalyst such as a magnesium-supported titanium catalyst or a metallocene catalyst.
[0054] Here, examples of polymerization catalysts that can be used include conventionally known catalysts, such as magnesium-supported titanium catalysts, metallocene catalysts described in International Publication No. 01 / 53369, International Publication No. 01 / 27124, JP-A-3-193796, or JP-A-2-41303, International Publication No. 2011 / 055803, International Publication No. 2014 / 050817, etc. Polymerization can be carried out by appropriately selecting from liquid phase polymerization methods including solution polymerization and suspension polymerization, and gas phase polymerization methods.
[0055] In the liquid phase polymerization method, an inert hydrocarbon solvent can be used as the solvent that constitutes the liquid phase.Examples of the inert hydrocarbon include aliphatic hydrocarbons including propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, alicyclic hydrocarbons including cyclopentane, cyclohexane, methylcyclopentane, and methylcyclohexane, aromatic hydrocarbons including benzene, toluene, and xylene, and halogenated hydrocarbons including ethylene chloride, chlorobenzene, dichloromethane, trichloromethane, and tetrachloromethane, and mixtures thereof.
[0056] In addition, in the liquid phase polymerization method, bulk polymerization can also be performed using the monomer corresponding to the structural unit (iii) derived from the aforementioned 4-methyl-1-pentene (i.e., 4-methyl-1-pentene) or the monomer corresponding to the structural unit (iv) derived from the aforementioned α-olefin having 2 to 4 carbon atoms (i.e., the aforementioned α-olefin having 2 to 4 carbon atoms) itself as a solvent.
[0057] By stepwise copolymerizing the above-mentioned 4-methyl-1-pentene with the above-mentioned α-olefin having 2 to 4 carbon atoms, it is also possible to appropriately adjust the composition distribution of the 4-methyl-1-pentene structural units (iii) constituting the copolymer (B) and the α-olefin structural units (iv) having 2 to 4 carbon atoms.
[0058] The polymerization temperature when polymerizing the copolymer (B) is preferably −50 to 200° C., more preferably 0 to 100° C., and further preferably 20 to 100° C. The polymerization pressure when polymerizing the copolymer (B) is preferably normal pressure to 10 MPa gauge pressure, and more preferably normal pressure to 5 MPa gauge pressure.
[0059] During polymerization of the copolymer (B), hydrogen may be added for the purpose of controlling the molecular weight and polymerization activity of the resulting polymer. The amount of hydrogen to be added is appropriately about 0.001 to 100 NL per 1 kg of the total amount of the 4-methyl-1-pentene and the α-olefin having 2 to 4 carbon atoms.
[0060] <Resin composition (Z)> The resin composition (Z) constituting the sealant layer (Y) contains 5 to 25 parts by mass, preferably 6 to 22 parts by mass, more preferably 7 to 20 parts by mass, and even more preferably 8 to 18 parts by mass of a 4-methyl-1-pentene polymer (A) satisfying the above-mentioned requirements (Aa) to (Ad), and 75 to 95 parts by mass, preferably 78 to 94 parts by mass, more preferably 80 to 93 parts by mass, and even more preferably 82 to 92 parts by mass of a 4-methyl-1-pentene·α-olefin copolymer (B) satisfying the above-mentioned requirements (Ba) to (Bd) (the total of the polymer (A) and the copolymer (B) is 100 parts by mass).
[0061] When the blending amount of the copolymer (B) in the resin composition (Z) is less than the above range, good heat sealability cannot be obtained in the sealant layer (Y).When the blending amount of the copolymer (B) in the resin composition (Z) is more than the above range, it becomes difficult to maintain practical heat resistance in the sealant layer (Y).
[0062] In addition, since the polymer (A) and the copolymer (B) are resins having similar polarities, the polymer (A) can be uniformly and favorably dispersed in the copolymer (B). Although the polymer (A) has a substantially sea-island structure, the dispersed phase size of the polymer (A) is extremely small. Therefore, the film of the sealant layer (Y) is very little affected by the surface irregularities caused by the sea-island structure, and is considered to have smoothness and excellent transparency.
[0063] The resin composition (Z) is obtained by mixing the polymer (A) and the copolymer (B) in the specific ratio. The resin composition (Z) can be prepared by various known methods, for example, a method of dry blending the above-mentioned components using a Henschel mixer, a tumbler blender, a V-blender or the like, a method of dry blending and then melt kneading using a single screw extruder, a twin screw extruder, a Banbury mixer or the like, and a method of stirring and mixing in the presence of a solvent.
[0064] Resin composition (Z) may contain an antioxidant as necessary within a range that does not impair the effects of the present invention. Known antioxidants can be used as the antioxidant. Specifically, hindered phenol compounds, sulfur-based antioxidants, lactone-based antioxidants, organic phosphite compounds, organic phosphonite compounds, or combinations of several of these can be used, such as phenol-based (2,6-di-t-butyl-4-methylphenol, etc.), polycyclic phenol-based (2,2'-methylenebis(4-methyl-6-t-butylphenol) etc.), phosphorus-based (tetrakis(2,4-di-t-butylphenyl)-4,4-biphenylenediphosphonate, etc.), and amine-based (N,N-diisopropyl-p-phenylenediamine, etc.).
[0065] The resin composition (Z) may contain various additives known in the art, such as a heat stabilizer, a weather stabilizer, an ultraviolet absorber, an antistatic agent, a surfactant, an antislip agent, an antiblocking agent, a crystal nucleating agent, a lubricant, a pigment, a dye, an antioxidant, a hydrochloric acid absorber, an inorganic or organic filler, a crosslinking agent, a crosslinking assistant, a softener, and a flame retardant, within the scope of not impairing the effects of the present invention.
[0066] Examples of the ultraviolet absorbing agent include benzotriazole-based, benzophenone-based, salicylic acid-based, and acrylate-based ultraviolet absorbing agents. Antibacterial agents include quaternary ammonium salts, pyridine compounds, organic acids, organic acid esters, halogenated phenols, and organic iodines.
[0067] Examples of the antistatic agent include surfactants, fatty acid esters, polymeric antistatic agents, etc., which will be described later. Examples of the fatty acid esters include esters of stearic acid and oleic acid, and examples of the polymeric antistatic agents include polyether ester amides.
[0068] Examples of the surfactant include nonionic, anionic, cationic, or amphoteric surfactants. Examples of the nonionic surfactant include polyethylene glycol-type nonionic surfactants such as higher alcohol ethylene oxide adducts, fatty acid ethylene oxide adducts, higher alkylamine ethylene oxide adducts, and polypropylene glycol ethylene oxide adducts; polyhydric alcohol-type nonionic surfactants such as polyethylene oxide, fatty acid esters of glycerin, fatty acid esters of pentaerythritol, fatty acid esters of sorbitol or sorbitan, alkyl ethers of polyhydric alcohols, and fatty amides of alkanolamines; examples of the anionic surfactant include sulfate ester salts such as alkali metal salts of higher fatty acids; sulfonates such as alkylbenzene sulfonates, alkyl sulfonates, and paraffin sulfonates; and phosphate ester salts such as higher alcohol phosphate ester salts; examples of the cationic surfactant include quaternary ammonium salts such as alkyltrimethylammonium salts. Examples of the amphoteric surfactant include amino acid-type amphoteric surfactants such as higher alkylaminopropionates; and betaine-type amphoteric surfactants such as higher alkyldimethyl betaines and higher alkyldihydroxyethyl betaines.
[0069] Examples of slip agents include waxes (such as carnauba wax), higher fatty acids (such as stearic acid), higher fatty acid salts (such as calcium stearate), higher alcohols (such as stearyl alcohol), and higher fatty acid amides (such as stearamide, erucic acid amide, and oleic acid amide).
[0070] Examples of the softener include known softeners including process oil, lubricating oil, paraffin, liquid paraffin, polyethylene wax, polypropylene wax, petroleum-based substances including petroleum asphalt and Vaseline, coal tars including coal tar and coal tar pitch, fatty oils including castor oil, linseed oil, rapeseed oil, soybean oil and coconut oil, tall oil, beeswax, carnauba wax and lanolin, fatty acids or metal salts thereof including ricinoleic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, montanic acid, oleic acid and erucic acid, synthetic polymers including petroleum resin, coumarone-indene resin and atactic polypropylene, ester-based plasticizers, microcrystalline wax, liquid polybutadiene or modified or hydrogenated products thereof, and liquid thiokol.
[0071] Examples of the ester-based plasticizer include aromatic carboxylates (dibutyl phthalate, dioctyl phthalate, etc.), aliphatic carboxylates (methyl acetylricinoleate, etc.), aliphatic dicarboxylates (dioctyl adipate, dioctyl sebacate, adipic acid-propylene glycol polyesters, etc.), aliphatic tricarboxylates (triethyl citrate, etc.), phosphate triesters (triphenyl phosphate, etc.), and epoxy fatty acid esters (epoxybutyl stearate, etc.).
[0072] The content of the above-mentioned antioxidant and various additives is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, per 100 parts by mass of the total of the polymer (A) and the copolymer (B) in the resin composition (Z).
[0073] Furthermore, the resin composition (Z) may contain a resin other than the polymer (A) and the copolymer (B) within a range that does not impair the effects of the present invention. In this case, the content of the resin other than the polymer (A) and the copolymer (B) is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, based on 100 parts by mass of the total of the polymer (A) and the copolymer (B).
[0074] <Laminated film manufacturing method> The method for producing the laminated film of the present invention is not particularly limited, and any known method such as extrusion cast molding, extrusion lamination molding, or dry lamination molding can be used. An example of a method for producing the laminated film of the present invention will be described. The laminated film of the present invention can be produced, for example, by the following method. However, the method for producing the laminated film of the present invention is not limited thereto. First, a co-extrusion molding machine connected to a T-die is used, and the resin material used for the base layer (X) is charged into the hopper of one extruder of the co-extrusion molding machine, and the resin composition (Z) constituting the sealant layer (Y) is charged into the hopper of the other extruder of the co-extrusion molding machine. Then, the cylinder temperature is set to 160 to 280°C, and the die temperature is set to 200 to 280°C to melt the resin. The molten resin of the base layer (X) and the molten resin of the resin composition (Z) constituting the sealant layer (Y) are co-extruded from a T-die, and then cooled and solidified at a cast roll temperature of 20 to 100°C, thereby obtaining a film in which the base layer (X) and the sealant layer (Y) are laminated.
[0075] The layer structure of the laminated film is not particularly limited and can be appropriately set depending on the application. For example, the layer structure is preferably a base layer (X) / sealant layer (Y) structure, but the laminated film may contain at least one of the base layer (X) or the sealant layer (Y) in multiples. In addition, it is preferable that the sealant layer (Y) is in direct contact with the base layer (X). Furthermore, the thickness ratio of each layer of the laminated film is not particularly limited and can be appropriately set depending on the application. The laminated film of the present invention has a base layer (X) and a sealant layer (Y) provided on one side of the base layer (X), and the sealant layer (Y) in the laminated film is preferably one layer so that the laminated film can be reliably sealed by heat sealing. From the viewpoint of being able to select a wide range of sealing temperature ranges for heat sealing, the sealant layer (Y) is preferably the outermost layer of the laminated film.
[0076] The thickness of the laminated film of the present invention is not particularly limited, but can be appropriately determined as desired. Usually, the thickness of the base layer (X) is in the range of 18 to 350 μm, preferably 24 to 260 μm, more preferably 30 to 180 μm, and the thickness of the sealant layer (Y) is in the range of 2 to 50 μm, preferably 4 to 40 μm, more preferably 5 to 20 μm. The total thickness of the laminated film is in the range of 20 to 400 μm, preferably 28 to 300 μm, and more preferably 35 to 200 μm. When the total thickness of the laminate film is 20 μm or more, it is easy to handle and is not easily torn when peeled off. Furthermore, when the total thickness of the laminate film is 400 μm or less, it is easy to reduce the weight of the laminate film and to control the gas permeability.
[0077] <Physical properties of laminated film> When the laminated film of the present invention is heat-sealed under conditions of a temperature of 200°C, a pressure of 0.2 MPa, and a sealing time of 2 seconds with the surfaces of the sealant layers (Y) facing each other, the peel strength between the laminated films (hereinafter sometimes referred to as "heat seal strength") is preferably 2.0 N / 15 mm or more, more preferably 2.5 N / 15 mm or more, and even more preferably 3.0 N / 15 mm or more. When the heat seal strength of the above laminated film is 2.0 N / 15 mm or more, when the film is used to package an object to be packaged to form a package, peeling between the sealant layers during storage or transportation of the package is easily prevented. The upper limit of the heat seal strength of the laminated film is not particularly limited, but is usually 25 N / 15 mm or less. The specific method for measuring the heat seal strength is as described in the Examples below.
[0078] The sealant layer (Y) of the laminated film of the present invention preferably has a peel strength of 0.1 to 3.0 N / 25 mm, more preferably 0.2 to 2.0 N / 25 mm, when an adhesive tape layer (an adhesive tape coated with an acrylic adhesive, such as Nitto Denko Corporation's Adhesive Tape No. 31B) is peeled off from the sealant layer (Y) under the measurement conditions described in the following Examples. The lower the peel strength when the sealant layer (Y) is peeled off from the adhesive tape, the more excellent the releasability of the sealant layer (Y) of the laminated film of the present invention tends to be.
[0079] The critical surface tension of the sealant layer (Y) of the laminated film of the present invention is preferably 20 to 26 mN / m, more preferably 21 to 26 mN / m, and particularly preferably 22 to 25 mN / m. The critical surface tension value is a value that indicates the releasability of the film surface. The smaller the critical surface tension value, the better the releasability tends to be. When the critical surface tension of the sealant layer (Y) is 20 to 26 mN / m, the laminate film of the present invention has excellent releasability, and therefore exhibits a releasability function when the laminate film is made into a packaging bag and the packaged item is filled into the packaging bag (i.e., the contents are less likely to adhere to the inner layer surface of the packaging bag, and when the contents are discharged from the packaging bag, the contents are less likely to remain adhered to the inner surface of the packaging bag).
[0080] The gas permeability of the laminated film of the present invention is not particularly limited, but can be, for example, oxygen permeability (oxygen permeability coefficient, unit: cm 3 mm / (m 2 ·24hr.·atm)] and carbon dioxide permeability (carbon dioxide permeability coefficient, unit: cm 3 mm / (m 2 ·24hr.·atm) can be evaluated in accordance with JIS K7126-1, differential pressure method. In addition, water vapor permeability (water vapor permeability coefficient, unit: g mm / (m 2 ·24 hr.) can be evaluated in accordance with JIS K7129-2, infrared sensor method (MOCON method). The specific measurement method is as described in the examples below. The larger the oxygen permeability coefficient and carbon dioxide permeability coefficient, the better the gas permeability. Also, the larger the water vapor permeability coefficient, the better the gas permeability (moisture permeability).
[0081] The total haze of the laminated film of the present invention (when the film has a thickness of 50 μm) is not particularly limited, but is preferably 50% or less, more preferably 40% or less, even more preferably 30% or less, and particularly preferably 20% or less. When the total haze of the laminated film of the present invention is 50% or less, the laminated film becomes transparent. The method for measuring the total haze is as described in the Examples below. The lower the total haze value, the more transparent the laminate film is.
[0082] <Applications of laminated film> The laminated film of the present invention is widely used, for example, as tapes, masking films, masking tapes, temporary adhesive films, freshness-preserving packaging films, plastic envelopes, easy-open packaging bags, automatic packaging films, shopping bags, standing packs, liquid film packaging bags, transparent packaging sheets, construction material films, laminating films, agricultural films, food packaging materials, fruit packaging materials, plant packaging materials, flower bouquet packaging materials, electronic component packaging materials, machine component packaging materials, grain packaging materials, seafood and other marine product packaging materials, medical films, medical sheets, medical tapes, cell culture bags, and the like. The laminated film of the present invention has both heat sealing properties and high gas permeability, and is therefore suitable for use as a packaging material. In particular, since it exhibits high gas permeability despite being a non-porous film, it can prevent the intrusion of bacteria and the like, and is therefore highly useful as a packaging material for food and medical use. In addition, since it has excellent releasability, it is suitable for use as a packaging material with a releasable function when the contents are filled into a film packaging bag. EXAMPLES
[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring the physical properties of resins, the resins used, the methods for preparing test pieces, and the evaluation methods in the following examples and comparative examples are as follows.
[0084] <Method of measuring physical properties of polymer> <Content of structural units> The amount of the structural unit derived from 4-methyl-1-pentene and the amount of the structural unit derived from α-olefin contained in the polymer (A) and the copolymer (B) were measured using the following apparatus and conditions. 13 The amount of structural units derived from α-olefins in this measurement does not include the amount of structural units derived from 4-methyl-1-pentene. A nuclear magnetic resonance spectrometer (JEOL ECP500 type) was used, and the mixture solvent was o-dichlorobenzene / deuterated benzene (80 / 20% by volume), the sample concentration was 55 mg / 0.6 mL, the measurement temperature was 120°C, and the observed nuclei were 13 The measurements were performed using C (125 MHz), a sequence of single pulse proton decoupling, a pulse width of 4.7 μs (45° pulse), a repetition time of 5.5 s, and an accumulation count of 10,000 or more, with 27.50 ppm as the reference value for the chemical shift. 13 The compositions of the polymer (A) and the copolymer (B) were quantified by C-NMR spectroscopy.
[0085] <Intrinsic viscosity> The intrinsic viscosity was determined in decalin solvent at 135°C using an Ubbelohde viscometer. About 20 mg of sample was taken for each of the polymer (A) and copolymer (B). Here, the sample may be in the form of a polymer powder, pellet, or resin block. The sample was dissolved in 15 mL of decalin, and the specific viscosity ηsp was measured in an oil bath heated to 135°C. After diluting the decalin solution by adding 5 mL of decalin solvent, the specific viscosity ηsp was measured in the same manner. This dilution procedure was repeated two more times, and the value of ηsp / C when the concentration (C) was extrapolated to zero was calculated as the intrinsic viscosity (see the formula below). [η]=lim(ηsp / C) (C→0)
[0086] <Weight average molecular weight (Mw), number average molecular weight (Mn), molecular weight distribution (Mw / Mn value)> The molecular weight was measured by gel permeation chromatography (GPC). Specifically, a Waters ALC / GPC150-Cplus type (integrated with differential refractometer detector) was used as a liquid chromatograph, two Tosoh GMH6-HT columns and two GMH6-HTL columns connected in series were used as separation columns, o-dichlorobenzene was used as a mobile phase medium, and 0.025% by mass dibutylhydroxytoluene (Takeda Pharmaceutical Co., Ltd.) was used as an antioxidant, the mobile phase medium was moved at 1.0 mL / min, the sample concentration was 15 mg / 10 mL, the sample injection amount was 500 μL, and a differential refractometer was used as a detector. As standard polystyrene, standard polystyrene manufactured by Tosoh with a weight average molecular weight (Mw) of 1,000 or more and 4,000,000 or less was used. The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn value) were calculated by preparing a calibration curve using a standard polystyrene sample and analyzing the obtained chromatogram by a known method. The measurement time per sample was 60 minutes.
[0087] <Melt flow rate (MFR)> In accordance with ASTM D1238, the MFR of the polymer (A) was measured at a temperature of 260° C. and a load of 5.0 kgf, and the MFR of the copolymer (B) was measured at a temperature of 230° C. and a load of 2.16 kgf.
[0088] <Melting point> In accordance with JIS K7121, a differential scanning calorimeter (DSC220C manufactured by Seiko Instruments Inc.) was used, and about 5 mg of the sample was placed in an aluminum pan for measurement, and the temperature was raised to 200°C at a heating rate of 10°C / min. The temperature of the highest melting peak among the melting peaks measured was taken as the melting point. When no melting peak was observed, it was evaluated that the melting point was not observed.
[0089] <density> The densities of the polymer (A) and the copolymer (B) were measured using a density gradient tube in accordance with JIS K7112.
[0090] <Polymer synthesis> <Synthesis Example 1: Synthesis of Polymer (A-1)> According to the method described in WO 2006 / 054613, the ratio of 4-methyl-1-pentene, 1-hexadecene, 1-octadecene, and hydrogen was adjusted to obtain polymer (A-1). The measurement results of each physical property of polymer (A-1) are shown in Table 1.
[0091] Next, 2000 ppm of tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionic acid]pentaerythritol as a heat stabilizer and 2000 ppm of tris(2,4-di-t-butylphenyl)phosphate as a secondary antioxidant were blended with 100 parts by mass of the above polymer (A-1), and strands were extruded using a twin-screw extruder (TEX25αIII, manufactured by The Japan Steel Works, Ltd., screw diameter 25 mm, L / D=52) under conditions of a cylinder setting temperature of 270°C, an extrusion rate of 5 kg / hour, and a screw rotation speed of 100 rpm. The strands were then immersed in a water tank and guided to a pelletizer (KM-100, manufactured by Katsumik Co., Ltd.) for granulation.
[0092] <Synthesis of Copolymer (B)> As copolymer (B), two types of copolymers were prepared, which differ in the amount of structural units derived from 4-methyl-1-pentene and the amount of structural units derived from α-olefins having 2 to 4 carbon atoms. These are distinguished as copolymer (B-1) and copolymer (B-2). The synthesis methods for each are as described below.
[0093] <Synthesis Example 2: Synthesis of Copolymer (B-1)> A 1.5 L stainless steel autoclave equipped with an agitator and thoroughly purged with nitrogen was charged with 300 ml of n-hexane (dried over activated alumina under a dry nitrogen atmosphere) and 450 ml of 4-methyl-1-pentene at 23° C. 0.75 ml of a 1.0 mmol / ml toluene solution of triisobutylaluminum (TIBAL) was charged into the autoclave and stirred.
[0094] Next, the autoclave was heated to an internal temperature of 60°C and pressurized with propylene so that the total pressure (gauge pressure) was 0.40 MPa. Then, 0.34 ml of a toluene solution containing 1 mmol of methylaluminoxane and 0.01 mmol of diphenylmethylene (1-ethyl-3-t-butyl-cyclopentadienyl) (2,7-di-t-butyl-fluorenyl) zirconium dichloride, which had been prepared in advance, was pressed into the autoclave with nitrogen to start the polymerization reaction. During the polymerization reaction, the temperature was adjusted so that the internal temperature of the autoclave was 60°C. 60 minutes after the start of polymerization, 5 ml of methanol was pressed into the autoclave with nitrogen to stop the polymerization reaction, and the inside of the autoclave was depressurized to atmospheric pressure. After depressurization, acetone was added to the reaction solution and stirred.
[0095] The obtained powdery copolymer containing the solvent was dried at 100°C under reduced pressure for 12 hours. The weight of the product copolymer (B-1) was 36.9 g. In the copolymer (B-1), the amount of structural units derived from 4-methyl-1-pentene was 72.4 mol%, and the amount of structural units derived from propylene was 27.6 mol%. When a DSC measurement was performed, no melting point was observed. The measurement results of each physical property of the copolymer (B-1) are shown in Table 1.
[0096] Next, 100 parts by mass of the above copolymer (B-1) was mixed with 2000 ppm of tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionic acid]pentaerythritol as a heat stabilizer and 2000 ppm of tris(2,4-di-t-butylphenyl)phosphate as a secondary antioxidant, and the strand was extruded using a twin-screw extruder (TEX25αIII, manufactured by The Japan Steel Works, Ltd., screw diameter 25 mm, L / D=52) under conditions of a cylinder setting temperature of 200°C, an extrusion rate of 5 kg / hour, and a screw rotation speed of 100 rpm. The strand was then guided to a pelletizer (KM-100, manufactured by Katsumik Co., Ltd.) while immersed in a water tank, and granulated.
[0097] <Synthesis Example 3: Synthesis of Copolymer (B-2)> A 1.5 L stainless steel autoclave equipped with an agitator and thoroughly purged with nitrogen was charged with 300 ml of n-hexane (dried over activated alumina under a dry nitrogen atmosphere) and 450 ml of 4-methyl-1-pentene at 23° C. 0.75 ml of a 1.0 mmol / ml toluene solution of triisobutylaluminum (TIBAL) was charged into the autoclave and stirred.
[0098] Next, the autoclave was heated to an internal temperature of 60°C, and pressurized with propylene so that the total pressure (gauge pressure) was 0.19MPa. Then, 0.34ml of a toluene solution containing 1mmol of methylaluminoxane and 0.01mmol of diphenylmethylene (1-ethyl-3-t-butyl-cyclopentadienyl) (2,7-di-t-butyl-fluorenyl) zirconium dichloride, which had been prepared in advance, was pressed into the autoclave with nitrogen to start the polymerization reaction. During the polymerization reaction, the temperature was adjusted so that the internal temperature of the autoclave was 60°C. 60 minutes after the start of polymerization, 5ml of methanol was pressed into the autoclave with nitrogen to stop the polymerization reaction, and then the inside of the autoclave was depressurized to atmospheric pressure. After depressurization, acetone was added to the reaction solution while stirring.
[0099] The obtained powdery polymer containing the solvent was dried at 130°C under reduced pressure for 12 hours. The weight of the product, copolymer (B-2), was 44.0 g. In copolymer (B-2), the amount of structural units derived from 4-methyl-1-pentene was 84.1 mol%, and the amount of structural units derived from propylene was 15.9 mol%. When DSC measurement was performed, the melting point was 130°C. The measurement results of each physical property of copolymer (B-2) are shown in Table 1.
[0100] Next, 100 parts by mass of the above copolymer (B-2) was mixed with 2000 ppm of tetrakis[3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionic acid]pentaerythritol as a heat stabilizer and 2000 ppm of tris(2,4-di-t-butylphenyl)phosphate as a secondary antioxidant, and the strand was extruded using a twin-screw extruder (TEX25αIII, manufactured by The Japan Steel Works, Ltd., screw diameter 25 mm, L / D=52) under conditions of a cylinder setting temperature of 200°C, an extrusion rate of 5 kg / hour, and a screw rotation speed of 100 rpm. The strand was then guided to a pelletizer (KM-100, manufactured by Katsumik Co., Ltd.) while immersed in a water tank, and granulated.
[0101] [Table 1]
[0102] <Example 1> [Preparation Example 1: Resin composition (preparation of Z-1)] The resin composition (Z-1) which is a component of the sealant layer (Y) was prepared by mixing (dry blending) 10 parts by mass of the polymer (A-1) and 90 parts by mass of the copolymer (B-1) using a tumbler blender.
[0103] [Making laminated film] Next, pellets of the polymer (A-1) for forming the base layer (X-1) and the resin composition (Z-1) which is a component of the sealant layer (Y-1) were respectively put into each extruder hopper of a multi-layer co-extrusion molding machine (screw diameter 20 mm, L / D = 28, T-die width 300 mm, lip opening 1 mm) equipped with a T-die. The cylinder temperature was set to 160 to 280 ° C., and the die temperature was set to 280 ° C., and the molten resin was co-extruded from the T-die, while the casting roll temperature was set to 80 ° C. and the take-up speed was set to 2.0 m / min., and a two-kind two-layer cast film was molded so that the thickness of the base layer (X-1) was 40 μm and the thickness of the sealant layer (Y-1) was 10 μm, to obtain a laminated film with a total thickness of 50 μm.
[0104] [Heat seal strength] The obtained laminated film having a total thickness of 50 μm was cut into a rectangular shape having a width of 150 mm and a length of 50 mm, and two pieces were prepared as test pieces. Next, the two prepared test pieces were overlapped so that the sealant layers (Y-1) faced each other, and then heat-sealed using a heat seal tester (Tester Sangyo Co., Ltd., thermal gradient heat seal tester TP-701-G) under the conditions of upper temperature 160 to 220 ° C, lower temperature 120 ° C, seal width 5 mm, seal pressure 0.2 MPa, and seal time 2 seconds. Next, the heat-sealed laminated film was taken out of the heat seal tester and cut to a width of 15 mm. The heat-sealed laminated film of 15 mm width was pulled in a direction of 180° with respect to the heat-sealed surfaces of the laminated films at a test speed of 300 mm / min and an atmospheric temperature of 23°C using a tensile tester (Shimadzu Corporation, AGS-X) to peel the laminated films from each other, and the maximum peel strength was measured. The maximum value was taken as the heat seal strength (unit: N / 15 mm). At that time, when the laminated film was fully stretched without peeling, the maximum value of the observed tensile strength was taken as the heat seal strength. The heat seal strength was measured for five test pieces, and the average value was calculated.
[0105] [Heat seal peeling pattern] After the heat-sealed portion was peeled off, the laminated film was observed for its peeling state, and the results were classified according to the following criteria. (Classification criteria) P: Peeling occurred at the heat-sealed surface of the sealant layer (Y), and the surface was not damaged during peeling. In addition, no peeling occurred between the sealant layer (Y) and the base layer (X). T: The edge of the seal portion (welded surface) of the sealant layer (Y) was broken, but no peeling occurred between the sealant layer (Y) and the base layer (X). D: Peeling was unlikely to occur on the heat-sealed surface of the sealant layer (Y), and peeling occurred at least partially between the sealant layer (Y) and the base layer (X).
[0106] [Critical surface tension] In order to evaluate the critical surface tension of the sealant layer (Y-1) of the obtained laminated film, a mixture for wetting tension test of ethylene glycol monoethyl ether / formamide mixture (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) with the surface tension of the liquid adjusted to 31 mN / m, 34 mN / m, 37 mN / m, and 40 mN / m, respectively, was dropped onto the surface of the sealant layer (Y-1) under an atmosphere of 23°C temperature and 50% relative humidity. Then, the contact angle was measured using an image processing type solid-liquid interface analysis system (DropMaster500, manufactured by Kyowa Interface Science Co., Ltd.). By the Zisman plot method, the surface tension value of each mixture was plotted on the horizontal axis and the measured value of the contact angle (the angle was converted to radian units and expressed as cosθ) on the vertical axis, and a linear linear function was obtained according to the least squares method. The graph of the linear function was extrapolated up to cosθ=1.0, which is considered to be a completely wet state, and the surface tension at which cosθ=1.0 on the graph (i.e., the value on the horizontal axis at the point where cosθ=1.0 on the graph) was determined to be the critical surface tension (mN / m).
[0107] [Peel strength with adhesive tape] Under a constant environment of 23°C temperature and 50% relative humidity, an adhesive tape coated with an acrylic adhesive [Nitto Denko Corporation adhesive tape No. 31B (tape width 25 mm)] was applied to the sealant layer (Y-1) of the laminated film by rolling it back and forth twice using a rubber roller capable of applying a constant load of 2.0 kgf, and then cut to a width of 25 mm and a length of 150 mm to prepare a test specimen. The test piece was aged for one day in a constant environment of 23°C and 50% relative humidity, and then the peel strength (N / 25 mm) was measured when the adhesive tape layer and the sealant layer (Y) were peeled off in a 180° direction at a test speed of 300 mm / min using a tensile testing machine (Intesco 201X).
[0108] [Oxygen permeability and carbon dioxide permeability] The gas permeability of the laminated film is expressed as oxygen permeability (oxygen permeability coefficient, unit: cm 3 mm / (m 2 ·24hr.·atm)] and carbon dioxide permeability (carbon dioxide permeability coefficient, unit: cm 3 mm / (m 2 ·24 hr.·atm) was measured by the following method. A laminated film with a total thickness of 50 μm was cut into a size of 30 mm wide x 30 mm long and used as a test piece. The oxygen permeability and carbon dioxide permeability were measured in accordance with JIS K7126-1 using a differential pressure gas permeability measuring device (CT1 manufactured by Toyo Seiki Co., Ltd.) at a test temperature of 23°C and a relative humidity of 0%. The measurement area of the laminated film was 5 cm2. 2 The measurement area of the laminated film was adjusted by preparing two aluminum masks with adhesive (manufactured by Modern Kotrol Co., Ltd.) with two holes of 25 mm diameter in the center, and overlapping these two masks so that the laminated film to be measured was sandwiched between them.
[0109] [Water vapor permeability coefficient] Water vapor permeability of laminated film (water vapor permeability coefficient, unit: g mm / (m 224hr.) was measured in accordance with JIS K7129-2, infrared sensor method (MOCON method), using a water vapor transmission rate measuring device (Hitachi High-Tech, PERMATRAN-W3 / 34G) at a test temperature of 40°C and a relative humidity of 90% on a laminated film measuring area of 50cm. 2 and measurements were taken.
[0110] [All Haze] The obtained laminated film was cut into a square with a side length of 50 mm to prepare a test piece, which was aged for 3 days in a constant environment of a temperature of 23° C. and a relative humidity of 50%. The test piece was measured at 5 arbitrary points using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., NDH4000) in accordance with JIS K7136, and the average value was taken as the total haze (%). The results of the physical property evaluation are shown in Table 2. Note that hereinafter, Table 2-1 and Table 2-2 are collectively referred to as Table 2.
[0111] <Example 2> As the resin composition (Z-2) forming the sealant layer (Y-2), 10 parts by mass of the polymer (A-1) and 90 parts by mass of the copolymer (B-2) were dry-blended. Except for using the obtained resin composition (Z-2), a laminated film was obtained in the same manner as in Example 1, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0112] <Example 3> As the resin composition (Z-3) forming the sealant layer (Y-3), 10 parts by mass of the polymer (A-1), 45 parts by mass of the copolymer (B-1), and 45 parts by mass of the copolymer (B-2) were dry-blended. Except for using the obtained resin composition (Z-3), a laminated film was obtained in the same manner as in Example 1, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0113] <Example 4> In the resin composition (Z-4) forming the sealant layer (Y-4), the blending ratio of the polymer (A-1) and the copolymer (B-1) was changed as shown in Table 2. Except for using the obtained resin composition (Z-4), a laminated film was obtained in the same manner as in Example 1, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0114] <Example 5> In the resin composition (Z-5) forming the sealant layer (Y-5), the blending ratio of the polymer (A-1) and the copolymer (B-1) was changed as shown in Table 2. Except for using the obtained resin composition (Z-5), a laminated film was obtained in the same manner as in Example 2, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0115] <Comparative Example 1> The resin composition (CZ-1) used to form the sealant layer (CY-1) was changed to 100 parts by mass of the polymer (A-1). Except for using the resin composition (CZ-1) instead of the resin composition (Z-1), a laminated film was obtained in the same manner as in Example 1, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0116] <Comparative Example 2> In the resin composition (CZ-2) forming the sealant layer (CY-2), the blending ratio of the polymer (A-1) and the copolymer (B-1) was changed as shown in Table 2. Except for using the resin composition (CZ-2) instead of the resin composition (Z-1), a laminated film was obtained in the same manner as in Example 1, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0117] <Comparative Example 3> In the resin composition (CZ-3) forming the sealant layer (CY-3), the blending ratio of the polymer (A-1) and the copolymer (B-1) was changed as shown in Table 2. Except for using the resin composition (CZ-3) instead of the resin composition (Z-1), a laminated film was obtained in the same manner as in Example 1, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0118] <Comparative Example 4> The resin composition (CZ-4) used to form the sealant layer (CY-4) was changed to 100 parts by mass of propylene polymer (C) [homogenous propylene F107BV manufactured by Prime Polymer Co., Ltd.: MFR = 7g / 10 min (230°C, load 2.16 kgf), melting point (Tm) 162°C]. Except for using resin composition (CZ-4) instead of resin composition (Z-1), a laminated film was obtained in the same manner as in Example 1, and various test pieces were prepared and the physical properties were evaluated. The results are shown in Table 2.
[0119] [Table 2-1]
[0120] [Table 2-2]
[0121] As shown in Table 2, in Examples 1 to 5, when the sealant layers (Y) were heat sealed together under conditions of a temperature of 200° C., a pressure of 2.0 MPa, and a sealing time of 2 seconds, the heat seal strength was 2.0 N / mm or more, and the heat seal performance was sufficient. In addition, laminated films were obtained that had high gas permeability (oxygen permeability, carbon dioxide permeability, water vapor permeability), transparency, and releasability.
[0122] On the other hand, although Comparative Examples 1 to 3 were relatively excellent in gas permeability, transparency, and releasability, sufficient heat seal strength was not obtained between the sealant layers (CY). In Comparative Example 4, when the sealant layers (CY) were heat sealed together, peeling occurred between the base layer (X) and the sealant layer (CY), and sufficient adhesive strength was not obtained even when heat sealed under conditions of a temperature of 200°C, a pressure of 2.0 MPa, and a sealing time of 2 seconds (heat seal performance was not good). [Industrial Applicability]
[0123] The laminated film of the present invention is a film and laminated film that combines heat sealing performance, high gas permeability, transparency, and releasability, and is widely used for various purposes such as masking film, masking tape, temporary adhesive film, freshness-preserving packaging film, plastic envelopes, easy-open packaging bags, automatic packaging film, standing packs, liquid film packaging bags, transparent packaging sheets, construction material films, lamination films, agricultural films, food packaging materials, fruit packaging materials, plant packaging materials, electronic component packaging materials, machine component packaging materials, grain packaging materials, seafood and other marine product packaging materials, medical films, medical sheets and tapes, and cell culture bags.
Claims
1. A laminated film having a base layer (X) and a sealant layer (Y) laminated on one side of the base layer (X), The base layer (X) contains a 4-methyl-1-pentene polymer (A) that satisfies the following requirements (A-a) to (A-d), a laminated film comprising a resin composition (Z) in which the sealant layer (Y) contains 5 to 25 parts by mass of the 4-methyl-1-pentene polymer (A) and 75 to 95 parts by mass of a 4-methyl-1-pentene copolymer (B) satisfying the following requirements (Ba) to (B-d) (the total of the 4-methyl-1-pentene polymer (A) and the 4-methyl-1-pentene copolymer (B) being taken as 100 parts by mass); Requirement (A-a) The amount of structural units (i) derived from 4-methyl-1-pentene is 90 to 100 mol %, and the total amount of structural units (ii) derived from an α-olefin having 5 to 20 carbon atoms (excluding 4-methyl-1-pentene) is 0 to 10 mol % (with the proviso that the sum of structural units (i) and structural units (ii) is 100 mol %); Requirement (A-b) The intrinsic viscosity [η] measured in decalin at 135° C. is in the range of 0.5 to 5.0 dl / g; Requirement (Ac) The melting point (Tm) measured by differential scanning calorimetry (DSC) is in the range of 200 to 250°C; Requirement (A-d) Density is 820 to 860 kg / m 3 in the range of; Requirement (Ba-a) The amount of structural units (iii) derived from 4-methyl-1-pentene is 60 to 90 mol %, and the total amount of structural units (iv) derived from an α-olefin having 2 to 4 carbon atoms is 10 to 40 mol % (with the proviso that the total of structural units (iii) and structural units (iv) is 100 mol %); Requirement (B-b): The intrinsic viscosity [η] measured in decalin at 135° C. is in the range of 0.5 to 5.0 dl / g; Requirement (B-c) The melting point (Tm) measured by differential scanning calorimetry (DSC) is not observed or is in the range of less than 160°C; Requirement (B-d): Density is 820 to 860 kg / m 3 is in the range.
2. 2. The laminate film according to claim 1, wherein when the sealant layers (Y) are heat-sealed together under conditions of a temperature of 200° C., a pressure of 0.2 MPa, and a sealing time of 2 seconds, the peel strength of the sealant layer (Y) is 2.0 N / 15 mm or more.
3. 3. The laminated film according to claim 1, wherein the critical surface tension of the sealant layer (Y) at a temperature of 23° C. is 20 to 26 mN / m.
Citation Information
Patent Citations
Bulb packaging bag
JP1999301691A
Self-standing packaging bag for vegetable and fruit
JP2000189051A